Method for activating lithium secondary batteries

The method addresses gas removal inefficiencies in lithium secondary batteries by sequencing initial charging, degassing, and aging processes, enhancing gas evacuation and SEI film stability without pressurization, thus preventing lithium precipitation and maintaining battery performance.

JP2024540729AActive Publication Date: 2024-11-01LG ENERGY SOLUTION LTD
View PDF 13 Cites 0 Cited by

Patent Information

Application Number
JP2024525847
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-08-17
Filing Date
2023-08-21
Publication Date
2024-11-01
Estimated Expiration
2043-08-21

AI Technical Summary

Technical Problem

Conventional activation methods for lithium secondary batteries, particularly those with stack-and-fold electrode assemblies, fail to efficiently remove internal gas generated during the activation process, leading to lithium precipitation and reduced capacity and life characteristics due to gas trapping.

Method used

A method involving an initial charging process followed by a degassing process to remove internal gas, followed by an aging process to stabilize the SEI film, without requiring pressurization, specifically for batteries that cannot be compressed.

Benefits of technology

This method effectively minimizes lithium precipitation and maintains battery capacity and life characteristics by promptly removing generated gas, ensuring stable SEI film formation and efficient electrolyte adhesion.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024540729000001_ABST
    Figure 2024540729000001_ABST
Patent Text Reader

Abstract

The method for activating a lithium secondary battery according to the present invention includes: (a) a process for preparing a spare lithium secondary battery in which an electrode assembly including a positive electrode, a negative electrode, and a separator is housed in a battery case together with an electrolyte; (b) an initial charging process for charging the spare lithium secondary battery until a predetermined voltage is reached; (c) a degassing process for removing gas generated in the initial charging process from inside the spare lithium secondary battery and sealing it; and (d) an aging process for aging the spare lithium secondary battery, the above processes (a) to (d) being performed sequentially.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] This application claims the benefit of priority from Korean Patent Application No. 10-2022-0105424 filed on August 23, 2022 and Korean Patent Application No. 10-2023-0107553 filed on August 17, 2023.

[0002] The present invention relates to a method for activating a lithium secondary battery. [Background technology]

[0003] In general, as the depletion of fossil fuels leads to rising energy prices and concerns over environmental pollution, the demand for environmentally friendly alternative energy sources is becoming an essential factor for future life. Therefore, research into various power generation technologies such as atomic, solar, wind, and tidal power is ongoing, and there is also great interest in power storage devices to use the energy produced in this way more efficiently.

[0004] In particular, as technological development and demand for mobile devices increases, the demand for batteries as an energy source is rapidly increasing, and accordingly, much research is being conducted on batteries that can meet various demands.

[0005] Typically, in terms of battery shape, there is high demand for square-type secondary batteries and pouch-type secondary batteries that are thin and can be applied to products such as mobile phones, and in terms of materials, there is high demand for lithium secondary batteries such as lithium ion batteries and lithium ion polymer batteries that have advantages such as high energy density, discharge voltage, and output stability.

[0006] In addition, secondary batteries may be classified according to the structure of the electrode assembly in which a positive electrode, a negative electrode, and a separator interposed between the positive and negative electrodes are stacked. Representative examples include a jelly roll type (wound type) electrode assembly in which long sheet-like positive and negative electrodes are wound with a separator interposed therebetween, and a stack type (lamination type) electrode assembly in which a number of positive and negative electrodes cut into a predetermined size are stacked sequentially with a separator interposed therebetween. Recently, in order to solve the problems of the jelly roll type electrode assembly and the stack type electrode assembly, a stack-and-fold type electrode assembly has been developed as an electrode assembly with an advanced structure that is a combination of the jelly roll type and the stack type, in which unit cells in which a predetermined unit of positive and negative electrodes are stacked with a separator interposed therebetween are positioned on a separator film and then wound sequentially.

[0007] Meanwhile, secondary batteries, due to their characteristics, must undergo an activation process during the first cycle to activate the positive electrode active material and form a stable surface film (SEI, Solid Electrolyte Interface) on the negative electrode, and conventionally, it has been common to sequentially perform an initial charging process in which the secondary battery is charged to a certain voltage range, an aging process to stabilize the SEI film formed by the initial charging, and a degassing process. The degassing process is a process in which a large amount of gas generated inside the secondary battery due to the activation process is discharged to the outside of the secondary battery.

[0008] If the gas generated inside the battery cell during the activation process is not efficiently removed, the gas occupies a certain space inside the battery cell, causing the center of the battery case to swell and resulting in deformation of the battery, and the internal gas creates uncharged areas, which adversely affect the battery performance, such as lithium deposition, capacity, and output, as well as the battery life.

[0009] In particular, in the case of a stack-and-fold type electrode assembly, due to its structural characteristics, internal gas generated during the activation process is trapped in the folded portion of the separator, and there is a problem that the gas cannot be sufficiently discharged in the conventional activation process.

[0010] In addition, in the conventional activation process, the secondary battery is charged to a predetermined voltage range in order to form an SEI film on the negative electrode, and the SEI film is uniformly formed during initial charging, and the secondary battery is generally pressurized with a pressure jig during charging in order to prevent gas generated during initial charging from being trapped in the electrode assembly, which is called zig formation. It is known that such zig formation has the effect of reducing the risk of lithium deposition. However, depending on the specifications of the secondary battery, zig formation, in which the battery is pressurized during initial charging, may not be performed. Therefore, there is a need for technological development of an activation method that can reduce the risk of lithium deposition when zig formation is not performed. Summary of the Invention [Problem to be solved by the invention]

[0011] The present invention provides an activation method that reduces the risk of lithium deposition in a lithium secondary battery to which a stack-and-fold type electrode assembly is applied and / or a lithium secondary battery in which pressure cannot be applied during initial charging in an activation process, and has an excellent effect of removing gas generated during the activation process. [Means for solving the problem]

[0012] The method for activating a lithium secondary battery according to the present invention includes: (a) a process for preparing a spare lithium secondary battery in which an electrode assembly including a positive electrode, a negative electrode, and a separator is housed in a battery case together with an electrolyte; (b) an initial charging process for charging the spare lithium secondary battery until a predetermined voltage is reached; (c) a degassing process for removing gas generated in the initial charging process from inside the spare lithium secondary battery and sealing it; and (d) an aging process for aging the spare lithium secondary battery, the above processes (a) to (d) being performed sequentially.

[0013] In one embodiment of the present invention, the electrode assembly may be a stack-and-folding type electrode assembly.

[0014] In one embodiment of the present invention, the stack-and-fold type electrode assembly may have a structure in which a plurality of unit electrode assemblies, in which electrodes and separators are alternately stacked, are arranged on a first surface of a folding separator sheet and then folded one by one to form a stack of a plurality of unit electrode assemblies.

[0015] In one embodiment of the present invention, the initial charging process may not include a process of pressurizing the lithium secondary battery.

[0016] In one embodiment of the present invention, the end-of-charge voltage of the initial charging process can be set within a range of 30% to 80% (SOC 30% to SOC 80%) of the secondary battery design capacity, preferably within a range of 60% to 80% (SOC 60% to SOC 80%).

[0017] In an embodiment of the present invention, the spare lithium secondary battery may be a battery case including a resin layer and a metal layer, and an outer periphery of the battery case may be sealed by heat sealing in a state where the electrode assembly is housed in the battery case.

[0018] In one embodiment of the present invention, the aging process may include (d-1) a high-temperature aging process of aging the spare lithium secondary battery at a temperature range of 50 to 80 degrees Celsius for 10 to 40 hours.

[0019] In one embodiment of the present invention, the aging process may further include (d-2) a room temperature aging process of aging the spare lithium secondary battery at a temperature range of 18 to 27 degrees Celsius for 24 to 80 hours.

[0020] In one embodiment of the present invention, after the aging process, (e) a charging and discharging process of charging and discharging the spare lithium secondary battery may be further included.

[0021] In one embodiment of the present invention, the method may further include, after the initial charging step, (f) rolling the spare lithium secondary battery.

[0022] In one embodiment of the present invention, the spare lithium secondary battery can be roll pressed at a linear pressure of 1 kgf / mm to 10 kgf / mm.

[0023] In one embodiment of the present invention, the roll pressing step may be performed before the degassing step.

[0024] In an embodiment of the present invention, in the roll pressing process, the spare lithium secondary battery may be roll pressed in a direction parallel to a first direction that is a direction in which the electrode leads are drawn out.

[0025] In one embodiment of the present invention, the degassing process may be performed once.

[0026] In an embodiment of the present invention, the process of preparing the spare lithium secondary battery may include a pre-aging process of aging the spare lithium secondary battery for 12 to 48 hours to impregnate the electrode assembly with an electrolyte. Effect of the Invention

[0027] In cases where jig pressurization cannot be performed during initial charging due to battery specifications or where a stack-and-fold type electrode assembly is used, the risk of lithium deposition is minimized without a decrease in capacity and life characteristics compared to conventional activation methods, and the method has an excellent gas discharge effect by removing internal gas immediately after the initial charging process, which is the process in which the amount of gas generated is the largest during the activation process. [Brief description of the drawings]

[0028] [Figure 1] 2 is a flowchart of a method for activating a lithium secondary battery according to an embodiment of the present invention. [Diagram 2] 1 is a schematic diagram of a lithium secondary battery to which the activation method of the present invention is applied. [Diagram 3] 2 is a flowchart of a method for activating a lithium secondary battery according to an embodiment of the present invention. [Figure 4] 4 is a flowchart of an activation method of a lithium secondary battery according to another embodiment of the present invention. [Diagram 5] FIG. 2 is a perspective view of a pressure roller that may be used in the roll pressing process of the present invention. [Figure 6] FIG. 2 is a top view of a pressure roller that may be used in the roll pressing process of the present invention. [Figure 7] FIG. 1 is a schematic diagram of a stack-and-fold type electrode assembly. [Figure 8] 1 is a schematic diagram showing a pressing method in a roll pressing process according to the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0029] Hereinafter, a preferred embodiment of the present invention will be described in detail with reference to the attached drawings. Before that, the terms and words used in the specification and claims should not be interpreted as being limited to their ordinary or dictionary meanings, but should be interpreted as meanings and concepts that are consistent with the technical idea of ​​the present invention, based on the principle that the inventor can appropriately define the concept of the term to best describe his own invention.

[0030] Therefore, the embodiment described in this specification and the configurations illustrated in the drawings are merely the most preferred embodiment of the present invention and do not represent the entire technical idea of ​​the present invention, and it can be understood that there are various equivalents and modifications that can replace them at the time of this application.

[0031] Fig. 1 is a flow chart of a method for activating a lithium secondary battery according to an embodiment of the present invention. Referring to Fig. 1, the method for activating a lithium secondary battery according to the present invention includes (a) a process of preparing a spare lithium secondary battery in which an electrode assembly including a positive electrode, a negative electrode, and a separator is housed in a battery case together with an electrolyte, (b) an initial charging process of charging the spare lithium secondary battery until it reaches a predetermined voltage, (c) a degassing process of removing gas generated in the initial charging process from inside the spare lithium secondary battery and sealing it, and (d) an aging process of aging the spare lithium secondary battery, and the above processes (a) to (d) are performed sequentially.

[0032] In the conventional activation method, an initial charging process in which a spare lithium secondary battery is charged until a predetermined voltage is reached, an aging process in which the spare lithium secondary battery is aged, and a degassing process in which gas inside the spare lithium secondary battery is removed and sealed have been sequentially performed. When a spare lithium secondary battery is subjected to an initial charging process, an SEI film is formed on the surface of the negative electrode, and in order to stabilize the thus formed SEI film, it is considered advantageous to perform an aging process immediately after the initial charging process. Since gas is generated during a series of activation processes including the aging process performed after the initial charging process, it has been a conventional technical practice to perform the degassing process after the aging process or after the interruption of the activation process.

[0033] The inventors of the present invention noticed that the amount of gas generated is the largest during the initial charging process among the multiple-step activation process of a secondary battery, and changed the order of the degassing process to be after the initial charging process. As a result, not only is there no deterioration in the long-term cycle performance of the battery due to instability in the formation of the SEI film, which was a concern when the degassing process was performed before the aging process, but it was also found that there is a better gas discharge effect because the degassing process can be performed before the electrolyte wet adhesion force is generated between the separator and the electrode, which led to the present invention.

[0034] The activation method of the present invention has an effect of preventing lithium deposition and improving capacity and life characteristics, particularly when applied to a lithium secondary battery using a stack-and-fold type electrode assembly in which internal gas was not sufficiently discharged in the conventional activation method, and a model of a lithium secondary battery in which pressure cannot be applied to the battery during initial charging.

[0035] FIG. 7 is a side view of a stack-and-folding type electrode assembly to which the activation method of the present invention is applied. Referring to FIG. 7, the stack-and-folding type electrode assembly E according to one embodiment may have a structure in which a plurality of unit electrode assemblies 10; 10A-10E, in which electrodes 11, 13 and separators 12 are alternately stacked, are arranged on a first surface 21 of a folding separator sheet 20, and folded one by one to stack a plurality of unit electrode assemblies 10. The ends of the electrodes 11, 13 and separator 12 constituting the stack-and-folding type electrode assembly E are wrapped by the folding separator sheet 20, and therefore, compared to the stack-type electrode assembly, the structure is disadvantageous in terms of gas discharge. Here, the stack-type electrode assembly may be an electrode assembly in which electrodes and separators are alternately stacked and the separator sheet wrapping them is eliminated.

[0036] The lithium secondary battery to which the activation method of the present invention is applied will be described below.

[0037] The lithium secondary battery of the present invention may be one in which an electrode assembly is housed in a battery case including a resin layer and a metal layer, and the outer periphery of the battery case is sealed by heat fusion.

[0038] The materials of the positive electrode, negative electrode, and separator included in the electrode assembly are not particularly limited, and any positive electrode, negative electrode, and separator known in the art may be used without particular limitation.

[0039] For example, the negative electrode may be formed by coating a negative electrode current collector made of copper, nickel, aluminum, or an alloy containing at least one of them with a negative electrode active material such as lithium metal, a lithium alloy, carbon, petroleum coke, activated carbon, graphite, a silicone compound, a tin compound, a titanium compound, or an alloy thereof.

[0040] The positive electrode may be formed by coating a positive electrode current collector made of, for example, aluminum, nickel, copper, or an alloy containing at least one of these with a positive electrode active material such as lithium manganese oxide, lithium cobalt oxide, lithium nickel oxide, lithium iron phosphate, or a compound or mixture containing at least one of these.

[0041] In addition, the electrode active material may be coated on both sides of the current collector, or may be coated on only one side of the current collector to form a non-coated portion, etc. In addition, the thickness of the positive electrode and the negative electrode is not particularly limited. That is, the thickness may be set in consideration of the purpose of use, such as focusing on output or energy, or focusing on ion conductivity.

[0042] The separator may be a conventional porous polymer film, such as a porous polymer film made of a polyolefin polymer, such as an ethylene homopolymer, a propylene homopolymer, an ethylene / butene copolymer, an ethylene / hexene copolymer, or an ethylene / methacrylate copolymer, either alone or in a laminated state, or a conventional porous nonwoven fabric, such as a nonwoven fabric of a high melting point glass fiber, a polyethylene terephthalate fiber, etc., but is not limited thereto. The method of applying the separator to a battery may include, in addition to the general method of winding, lamination or stacking of the separator and the electrode, or folding.

[0043] The electrolytic solution may contain a lithium salt as an electrolyte and an organic solvent.

[0044] The lithium salt may be any one that is commonly used in electrolytes for lithium secondary batteries without limitation. + X - It can be expressed as:

[0045] The anion of such a lithium salt is not particularly limited, but may be F - , Cl - , Br - , I - , NO3 - , N(CN)2 - , BF4 - , ClO4 - , PF6 - , (CF3)2PF4 - , (CF3)3PF3 - , (CF3)4PF2 - , (CF3)5PF - , (CF3)6P - , CF3SO3 - , CF3CF2SO3 - , (CF3SO2)2N - , (FSO2)2N - , CF3CF2(CF3)2CO - , (CF3SO2)2CH - , (SF5)3C - , (CF3SO2)3C - , CF3(CF2)7SO3 - , CF3CO2 - , CH3CO2 - , SCN - , and (CF3CF2SO2)2N - Examples include:

[0046] The organic solvent may be any organic solvent commonly used in electrolytes for lithium secondary batteries without any limitations. Representative examples include any one selected from the group consisting of propylene carbonate (PC), ethylene carbonate (EC), diethyl carbonate (DEC), dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), methyl propyl carbonate, dipropyl carbonate, dimethyl sulfoxide, acetonitrile, dimethoxyethane, diethoxyethane, vinylene carbonate, sulfolane, gamma-butyrolactone, propylene sulfite, and tetrahydrofuran, or a mixture of two or more of these organic solvents.

[0047] Hereinafter, a method for activating a lithium secondary battery according to an embodiment of the present invention will be described in more detail.

[0048] (a) Preparation process for spare lithium secondary batteries (a) The process for preparing a spare lithium secondary battery may be a process for manufacturing a spare lithium secondary battery by housing an electrode assembly including a positive electrode, a negative electrode, and a separator together with an electrolyte in a battery case. The spare lithium secondary battery manufactured by the above-mentioned preparation process may be a battery case in which the electrode assembly is housed in a battery case including a resin layer and a metal layer, and an outer circumferential surface of the electrode assembly housing is sealed by heat sealing.

[0049] Specifically, as shown in FIG. 2, the spare lithium secondary battery may include an electrode assembly (not shown), electrode tabs (not shown) provided on the electrode assembly, electrode leads 111, 112 coupled to the electrode tabs, and a battery case 120 housing the electrode assembly.

[0050] The electrode assembly may have a stack type or stack-and-fold type structure in which a positive electrode and a negative electrode are sequentially stacked with a separator interposed therebetween. The electrode tabs may include a positive electrode tab provided on the positive electrode of the electrode assembly and a negative electrode tab provided on the negative electrode, and the electrode leads may include a positive electrode lead 111 coupled to the positive electrode and a negative electrode lead 112 coupled to the negative electrode tab.

[0051] Here, the electrode tab and the electrode lead are electrically connected by being joined by welding, and the electrode leads 111 and 112 are pulled out to the outside of the battery case 120 and a portion thereof is exposed. In addition, an insulating film (not shown) may be attached to a portion of the upper and lower surfaces of the electrode leads 111 and 112 to ensure sealing with the battery case and electrical insulation.

[0052] The battery case 120 may include a case body having a recessed receiving portion in which an electrode assembly can be seated, and a cover integrally connected to the case body and sealing the receiving portion. That is, the battery case may be configured to receive an electrode assembly and an electrolyte in the receiving portion of the case body, and then to closely contact the case body and the cover and seal edges of the case body and the cover.

[0053] Meanwhile, the battery case 120 may have an aluminum laminate structure of a resin outer layer / a metal layer with barrier properties / a heat-meltable resin sealant layer, and thus, the resin sealant layers may be fused to each other by applying heat and pressure to both sides and the upper end of the cover and the body that are in contact with each other, thereby forming a sealed excess portion.

[0054] Meanwhile, since the upper and lower battery cases are in direct contact with the same resin sealant layer at the upper end, uniform sealing can be achieved by melting. Meanwhile, since the electrode leads 111, 112 protrude from the both sides, the electrode leads 111, 112 can be heat-sealed with an insulating film interposed between the battery case and the electrode leads 111, 112 to improve sealing performance by taking into consideration the thickness of the electrode leads 111, 112 and the heterogeneity of the material of the battery case 120.

[0055] In one specific example, the (a) spare lithium secondary battery preparation process may include a pre-aging process of aging the spare lithium secondary battery for 12 to 48 hours to allow the electrolyte to be impregnated into the electrode assembly.

[0056] In order for the electrode reaction to proceed by initial charging after the electrode assembly and electrolyte are housed in the battery case, the electrolyte must be sufficiently impregnated into the positive electrode, negative electrode, and separator that constitute the electrode assembly in advance. If the initial charging process is performed without the electrolyte being impregnated, uncharged areas may occur, which may prevent the SEI film from being formed uniformly, resulting in a decrease in battery performance.

[0057] Such a pre-aging process may involve aging the lithium secondary battery for 12 to 48 hours at a temperature range of 18 to 27 degrees Celsius, and the temperature range may be 18 to 27 degrees Celsius, preferably 19 to 26 degrees Celsius, and more preferably 20 to 25 degrees Celsius. The time for carrying out the pre-aging process may be 12 to 48 hours, and preferably 18 to 36 hours.

[0058] The pre-aging process may include a high-temperature pre-aging process to improve the impregnation efficiency of the electrolyte. Such a high-temperature pre-aging process may be a process of aging the spare lithium secondary battery at a temperature of 40°C to 55°C for 12 to 24 hours.

[0059] In the pre-aging process, when such a high-temperature pre-aging process is performed, the impregnation of the electrolyte is improved, the SEI film can be formed more uniformly during the initial charging process, and the occurrence of uncharged areas is reduced, thereby preventing the risk of lithium precipitation.

[0060] (b) Initial charging process The initial charging process according to an embodiment of the present invention may be a process of charging the spare lithium secondary battery prepared as described above until a predetermined voltage is reached.

[0061] Lithium secondary batteries are activated by initial charging during the manufacturing process. During this initial charging, lithium ions released from the positive electrode move to and are inserted into the negative electrode, forming a solid electrolyte interface (SEI) film on the surface of the negative electrode.

[0062] Once the SEI film is formed, it acts as an ion tunnel and allows only lithium ions to pass through. The effect of the ion tunnel is to solvate the lithium ions, and prevents organic solvent molecules with large molecular weights that move with the lithium ions in the electrolyte, such as lithium salts, EC, DMC, or DEC, from being inserted into the graphite anode and causing the structure of the anode to collapse. Once the SEI film is formed, the lithium ions do not react again with the graphite anode or other materials, and the charge consumed in the formation of the SEI film has the property of not reacting reversibly during discharge, which is an irreversible capacity. Therefore, no further decomposition of the electrolyte occurs, and the amount of lithium ions in the electrolyte is reversibly maintained, so that stable charging and discharging can be maintained.

[0063] In conclusion, once the SEI film is formed, the amount of lithium ions can be reversibly maintained, and the life characteristics of the battery are also improved.

[0064] Among the activation processes, the initial charging process is the process in which the largest amount of gas is generated due to the reaction between the positive electrode, the negative electrode, and the electrolyte. Since the activation method according to the present invention performs a degassing process after the initial charging process, it is preferable to induce maximum gas generation through the initial charging process.

[0065] In one specific example, the charge cut-off voltage in the initial charging process may be set within a range of 30% (SOC 30%) to 80% (SOC 80%) of the lithium secondary battery capacity (SOC 100%), or within a range of SOC 40% to SOC 80%, or within a range of SOC 50% to SOC 80%, or within a range of SOC 60% to SOC 80%, or within a range of SOC 60% to SOC 75%. When the charge cut-off voltage in the initial charging process is set within the above SOC range, it is preferable because it is possible to minimize the collapse or instability of the SEI film formed through the initial charging during the degassing process while inducing maximum gas generation during the initial charging process.

[0066] Specifically, when the positive electrode contains a lithium nickel cobalt manganese oxide (NCM)-based positive electrode active material, the end-of-charge voltage may be preferably 3.4V to 4.1V, and more preferably 3.5V to 4.0V.

[0067] The charging conditions in the initial charging process may be according to conditions known in the art. Specifically, the charging method may be a constant current charging method until the charge end voltage is reached. At this time, the charging rate (c-rate) may be 0.01C to 2C, 0.1C to 1.5C, or 0.2C to 1C, but is not necessarily limited thereto, and may be suitably changed according to the material properties of the positive and negative electrodes.

[0068] The initial charging process may be performed at a temperature condition of 18°C ​​to 28°C, specifically 19°C to 27°C, and more specifically 20°C to 26°C.

[0069] In one embodiment, the initial charging process may not include a process of pressurizing the lithium secondary battery.

[0070] In the case of a pouch-type battery, the battery case is flexible, and the initial charging process can be performed while the battery is pressurized. For example, the pouch-type battery can be initially charged while being pressurized using a pressurizing jig configured to be capable of surface pressurization, and such a pressurizing process can prevent the trapping of gas during the charging process.

[0071] However, it is not suitable to charge a cylindrical or prismatic battery in a pressurized state during the initial charging process. This is because the battery case constituting a cylindrical or prismatic battery has a hard outer shape compared to the battery case of a pouch-type battery, and pressurizing the battery may cause damage to the battery. Therefore, due to the characteristics of the battery, a cylindrical or prismatic battery cannot proceed with a pressurization process during initial charging, and therefore, in a cylindrical or prismatic battery, gas generated during initial charging is more likely to be trapped inside the electrode assembly compared to a pouch-type battery manufactured by performing an initial charging process in a pressurized state. When the degassing process is performed between the initial charging process and the aging process according to the present invention, the internal gas can be effectively removed, so the activation method according to the present invention may be useful when activating a cylindrical or prismatic battery.

[0072] (c) Degassing process The degassing process according to an embodiment of the present invention may include a process of removing and sealing gas from an initially charged spare lithium secondary battery. The present invention performs a degassing process on an initially charged spare lithium secondary battery before performing an aging process. A significant amount of gas generated during a series of activation processes is generated during the initial charging process, and if a high-temperature aging process is performed without performing a degassing process, the electrodes and the separator may adhere to each other, and the gas generated during the initial charging process may be trapped between them. To prevent this, the activation method according to the present invention performs a degassing process after the initial charging process, more specifically, before the high-temperature aging process.

[0073] In the activation method of the present invention, the degassing process is a process for discharging gas generated inside the battery during the activation process to the outside of the battery, and the internal gas can be sufficiently removed by performing only one degassing process during the activation process, i.e., there is no need to perform an additional degassing process after the aging process described below.

[0074] Such a degassing process may employ various degassing techniques known at the time of filing of the present invention. For example, the degassing process may be performed by cutting open a part of the gas pocket GP of the spare lithium secondary battery shown in Fig. 2, discharging the gas inside the secondary battery to the outside of the secondary battery through the cut portion, and then resealing the cut portion. However, such degassing techniques are widely known to those skilled in the art, and therefore a detailed description thereof will be omitted.

[0075] (d) Aging process The aging process according to an embodiment of the present invention may be a process of aging a spare lithium secondary battery to stabilize the SEI film formed through the initial charging process.

[0076] In one specific example, the aging process may include (d-1) a high-temperature aging process of aging the spare lithium secondary battery for 10 to 40 hours at a temperature range of 50 to 80 degrees C. When the high-temperature aging process is performed, the stabilization of the SEI film formed during the initial charging process is further accelerated.

[0077] The temperature range of the high-temperature aging process may be 50 to 80 degrees Celsius, preferably 55 to 80 degrees Celsius, and more preferably 60 to 75 degrees Celsius. The aging time of the high-temperature aging process may be 10 to 40 hours, 12 to 36 hours, or 18 to 30 hours.

[0078] If the set temperature during high-temperature aging is too high or the time period during which the high-temperature aging process is performed is too long, the durability of the SEI coating may be reduced, which is undesirable. Conversely, if the set temperature during high-temperature aging is too low or the time period during which the high-temperature aging process is performed is too short, the life characteristics of the lithium secondary battery may be reduced.

[0079] In one specific example, the aging process may further include (d-2) a room temperature aging process of aging the spare lithium secondary battery at a temperature range of 18 to 27 degrees Celsius for 24 to 80 hours.

[0080] The temperature range of the room temperature aging process may be 18 to 27 degrees Celsius, preferably 19 to 26 degrees Celsius, and more preferably 20 to 25 degrees Celsius. The aging time of the room temperature aging process may be 24 to 80 hours, preferably 30 to 72 hours, and more preferably 16 to 60 hours.

[0081] If the room temperature aging process is performed at an excessively low temperature range outside the above range or for an excessively short period of time, the spare lithium secondary battery may not be sufficiently activated, and thus the electrical performance may be degraded. Conversely, if the room temperature aging process is performed at an excessively high temperature or for an excessively long period of time, swelling may occur or the durability of the SEI coating may be degraded.

[0082] On the other hand, the order of the high-temperature aging process and the room-temperature aging process is not particularly limited, but it is more preferable to perform the room-temperature aging process after the high-temperature aging process in terms of stabilizing the SEI film.

[0083] 3 is a flow chart of a method for activating a lithium secondary battery according to an embodiment of the present invention. Referring to FIG. 3, the method for activating a lithium secondary battery according to an embodiment of the present invention may further include, after the aging process (d), (e) a charge / discharge process of charging and discharging a spare lithium secondary battery. In one specific example, the charge / discharge process may be a full discharge and full charge process of fully discharging the spare lithium secondary battery to near SOC0, and then charging the discharged secondary battery to 95% (SOC95%) or more of its design capacity, and the full discharge and full charge processes may be performed once or repeatedly two or more times.

[0084] In one specific example, the method for activating a secondary battery according to the present invention may further include an additional aging process after the (e) additional charge / discharge process. The additional aging process may be performed at room temperature or at a high temperature to stabilize the secondary battery, specifically for 1 to 21 days. The additional aging process may include a monitoring (OCV tracking) process including a process of measuring the open circuit voltage (OCV) of the battery at regular time intervals in order to screen low-voltage defective batteries in which a voltage drop occurs beyond the self-discharge of the battery.

[0085] 4 is a flow chart of a method for activating a lithium secondary battery according to another embodiment of the present invention. Referring to FIG. 4, the method for activating a lithium secondary battery according to another embodiment of the present invention may further include, after the initial charging process, (f) a process of roll pressing the spare lithium secondary battery.

[0086] Among the activation processes of a lithium secondary battery, the initial charging process (b) is the process that generates the most gas, so if the roll pressing process is performed after the initial charging process, the gas present in the interface between the electrode of the electrode assembly and the separator may be removed by physical force. In addition, since the roll pressing can directionally pressurize the battery from one side to the other, the internal gas that may be present in the electrode assembly can be pushed out along the roll pressing direction and moved to the outside of the electrode assembly. Here, the outside of the electrode assembly may be the space between the electrode assembly and the battery case.

[0087] Therefore, the roll pressing process has the effect of minimizing the trapping of gas generated during the initial charging process inside the electrode assembly and maximizing the amount of gas discharged from inside the secondary battery.

[0088] 5 and 6 show an embodiment of a pressure roller for performing the roll pressing process. Referring to these drawings, the roll pressing process of the present invention may be to pressurize a spare lithium secondary battery 100 while passing the battery between opposing upper and lower pressure rollers 1a and 1b.

[0089] Roll pressing using such a pressure roller can induce a linear pressure on the spare lithium secondary battery, and in one specific example, the roll pressing process can pressurize the spare lithium secondary battery with a linear pressure of 1kgf / mm to 10kgf / mm (9.8N / mm to 98N / mm), preferably 2kgf / mm to 9kgf / mm (20N / mm to 88N / mm), and more preferably 2.5kgf / mm to 7.5kgf / mm (25N / mm to 74N / mm).

[0090] The roll pressing process may be performed once or may be performed 2 to 5 times. The number of times of roll pressing may be suitably determined depending on the thickness of the lithium secondary battery, the material properties of the battery, and the like.

[0091] Fig. 8 is a diagram showing a schematic diagram of the roll pressing process of the present invention. Referring to Fig. 8, the direction of roll pressing in one embodiment may be a direction parallel to a first direction (y-axis direction) which is a direction in which the electrode leads 111, 112 are pulled out. However, the present invention is not limited thereto, and roll pressing may be performed in a direction parallel to a second direction (x-axis direction) perpendicular to the direction in which the electrode leads 111, 112 are pulled out, or roll pressing may be performed in a direction parallel to the first direction and then in a direction parallel to the second direction.

[0092] When performing roll pressing in a direction parallel to the first direction, in order to enhance the effect of gas removal, as shown in FIG. 8, roll pressing may be performed first from one side to the other side in the first direction, and then from the other side to one side in the first direction.

[0093] Meanwhile, when a stack-and-folding type electrode assembly is housed inside the spare lithium secondary battery, it is preferable to roll-press the spare lithium secondary battery in a direction parallel to the first direction, which is the direction in which the electrode leads are drawn out.

[0094] 7 and 8, the folding separator sheet 20 constituting the stack-and-fold type electrode assembly E encases the unit electrode assemblies 10A-10E, but encases the portions other than the edge ends from which the electrode leads are drawn. That is, the electrode leads are drawn along a first direction (y-axis direction), and the folding separator sheet 20 encases the electrode surface along a second direction (x-axis direction). If the roll pressing direction is parallel to the second direction, internal gas may collect in the surplus space between the end of the electrode assembly and the folding portion of the folding separator sheet 20. Therefore, in order to prevent gas generated during the initial charging process from collecting in the folding portion of the folding separator sheet 20, it is preferable that the roll pressing direction is parallel to the electrode lead drawing direction.

[0095] The roll pressing process may be performed at any stage after the initial charging process, and is preferably performed before the degassing process, because the gas inside the electrode assembly is pushed out to the outside of the electrode assembly through the roll pressing process, and the degassing process is performed in such a state that the gas inside the battery can be discharged to the outside of the battery to the maximum extent.

[0096] When the activation method and the manufacturing method of the lithium secondary battery of the present invention are applied to a lithium secondary battery including a stack-and-fold type electrode assembly or a battery in which jig pressurization cannot be performed during initial charging due to battery specifications, the activation method and the manufacturing method of the lithium secondary battery of the present invention minimize the risk of lithium deposition without decreasing capacity and life characteristics compared to conventional activation methods, and have an excellent gas discharge effect by removing internal gas immediately after the initial charging process in which the amount of gas generated is the largest during the activation process.

[0097] The present invention will be described in more detail with reference to the following examples. However, the configurations described in the examples described in this specification are merely examples of the present invention and do not represent all of the technical ideas of the present invention, so it is understood that there may be various equivalents and modifications that can replace them at the time of filing this application.

[0098] <Preparation Example 1: Preparation of spare lithium secondary battery including stack-and-fold type electrode assembly> LiNi as the positive electrode active material 0.8 Co 0.1 Mn 0.1 95.9 parts by weight of O2, 1.6 parts by weight of PVDF as a binder, and 2.5 parts by weight of carbon black as a conductive material were weighed and mixed in N-methylpyrrolidone (NMP) solvent to prepare a positive electrode mixture layer slurry. The mixture layer slurry was applied to an aluminum foil, dried, and then rolled to form a positive electrode having a positive electrode mixture layer (average thickness: 130 μm).

[0099] A negative electrode mixture layer slurry was prepared by mixing 85 parts by weight of natural graphite as a carbon-based active material, 5 parts by weight of SiO (silicon oxide) as a silicone-based active material, 6 parts by weight of carbon black as a conductive material, and 4 parts by weight of PVDF as a binder in an N-methylpyrrolidone solvent, and the slurry was applied to a copper foil to prepare a negative electrode having a negative electrode mixture layer (average thickness: 180 μm).

[0100] A stack-and-fold type electrode assembly was prepared by interposing a separator (thickness: about 16 μm) made of a porous polyethylene (PE) film between each of the prepared positive and negative electrodes. The electrode assembly was placed inside a pouch-type battery case made of an aluminum laminate sheet, and an electrolyte was injected into the case. The case was then left at room temperature for 3 days (pre-aging) to allow the electrolyte to be fully impregnated, thereby preparing a preliminary lithium secondary battery. The electrolyte was prepared by injecting 1MLiPF6 dissolved in an organic solvent in which ethylene carbonate (EC) and ethyl methyl carbonate (EMC) were mixed in a ratio of 3:7 (volume ratio) to prepare a battery.

[0101] <Example 1> A spare lithium secondary battery of the above manufacturing example was prepared and initially charged to SOC 30%, and then a degassing process was performed by opening a portion of the pouch-type battery case to release the gas inside the battery to the outside of the battery and re-sealing the opened portion. Then, the battery was subjected to high-temperature aging at a temperature of 60°C for 24 hours and room temperature aging at a temperature of 23°C for 72 hours, and then discharged to SOC 0 for the first time. Then, the process of charging to SOC 100 and discharging to SOC 0 was repeated two more times to complete the activation process.

[0102] <Example 2> A spare lithium secondary battery of the above manufacturing example was prepared and initially charged to SOC 30%, and then roll pressed at a linear pressure of 3 kgf / mm using the pressure roller shown in FIG. 5. Then, a part of the pouch-type battery case was opened to discharge the gas inside the battery to the outside of the battery, and the opened part was re-sealed to perform a degassing process. Then, the battery was subjected to high-temperature aging at a temperature of 60° C. for 24 hours and room temperature aging at a temperature of 23° C. for 72 hours, and then discharged to SOC 0 for the first time. Then, the process of charging to SOC 100 and discharging to SOC 0 was repeated two more times to complete the activation process.

[0103] <Example 3> The activation process was performed in the same manner as in Example 1, except that the end-of-charge voltage during the initial charge was set to SOC 60%.

[0104] <Comparative Example> A spare lithium secondary battery of the above manufacturing example was prepared and initially charged to SOC 30%, followed by high temperature aging at 60°C for 24 hours and room temperature aging at 23°C for 72 hours. A degassing process was then performed by opening a portion of the pouch-type battery case to remove the gas inside the battery by discharging it to the outside of the battery and resealing it, followed by a primary discharge to SOC 0. The process of charging to SOC 100 and discharging to SOC 0 was then repeated two more times to complete the activation process.

[0105] <Experimental Example 1: Evaluation of room temperature cycle characteristics> Each of the lithium secondary batteries prepared in the above Examples and Comparative Examples was charged to 4.35V at a rate of 0.8C at a temperature of 25°C, and then discharged to 3.0V at a rate of 0.5C after constant current / constant voltage charging with a 0.05C cutoff. This cycle was repeated 100 times. The capacity retention rate was calculated from the measured discharge capacity using the following formula, and the results are shown in Table 1.

[0106] [Mathematical formula] Capacity retention rate (%) = (discharge capacity for 100 cycles) x 100 / (discharge capacity of the first cycle)

[0107] <Experimental Example 2: Observation of lithium deposition> Each of the lithium secondary batteries manufactured in the above Examples and Comparative Examples was charged to 4.35 V at a rate of 0.8 C, and then discharged to 3.0 V at 0.5 C by constant current / constant voltage charging with a 0.05 C cut-off. This cycle was repeated 300 times. The batteries were then disassembled to observe whether lithium deposition occurred, and the results are shown in Table 1.

[0108] <Experimental Example 3: Evaluation of gas generation amount> Each of the lithium secondary batteries manufactured in the above Examples and Comparative Examples was charged to 4.35V at a rate of 0.8C at a temperature condition of 25°C, and then discharged to 3.0V at 0.5C after constant current / constant voltage charging with a 0.05C cut-off. This cycle was repeated 10 times, and the amount of gas generated after discharge was measured and the results are shown in Table 1. Table 1 below shows the relative amount of gas generated when the amount of gas generated in Example 1 is set to 100.

[0109] [Table 1]

[0110] Referring to Table 1 above, it was shown that the lithium secondary batteries manufactured according to the embodiments of the present invention did not exhibit lithium precipitation, had excellent capacity retention, and generated less gas than the lithium secondary batteries of the comparative examples.

[0111] Therefore, in a lithium secondary battery including a stack-and-fold type electrode assembly, it can be seen that an activation method in which a degassing process is performed after an initial charge has a more advantageous effect on gas emission than an activation method in which a degassing process is performed after an aging process. [Explanation of symbols]

[0112] 100: Lithium secondary battery 111, 112: electrode lead 120: Battery case GP: Gas pocket 1: Pressure roller 1a: upper pressure roller, 1b: lower pressure roller E: Stack and fold type electrode assembly 10A to 10E: Unit electrode assembly 11: Positive electrode 12: Separation membrane 20: Separation membrane sheet for folding

Claims

1. (a) preparing a spare lithium secondary battery having a structure in which an electrode assembly including a positive electrode, a negative electrode, and a separator is housed in a battery case together with an electrolyte; (b) an initial charging step of charging the spare lithium secondary battery until it reaches a predetermined voltage; (c) a degassing process for removing gas generated in the spare lithium secondary battery during an initial charging process and sealing the spare lithium secondary battery; (d) an aging process for aging the spare lithium secondary battery; The method for activating a lithium secondary battery comprises the steps (a) to (d) being carried out sequentially.

2. 2. The method of activating a lithium secondary battery according to claim 1, wherein the electrode assembly is a stack-and-fold type electrode assembly.

3. The stack-and-fold type electrode assembly is 3. The method of activating a lithium secondary battery according to claim 2, wherein a plurality of unit electrode assemblies, each having an electrode and a separator stacked alternately, are arranged on a first surface of a folding separator sheet and folded one by one to form a stack of a plurality of unit electrode assemblies.

4. 2. The method of claim 1, wherein the initial charging step does not include a step of pressurizing the lithium secondary battery.

5. 2. The method for activating a lithium secondary battery according to claim 1, wherein the end-of-charge voltage of the initial charging process is set within a range of 30% to 80% (SOC 30% to SOC 80%) of the secondary battery design capacity.

6. 2. The method for activating a lithium secondary battery according to claim 1, wherein the initial charging step sets an end-of-charge voltage within a range of 60% to 80% (SOC 60% to SOC 80%) of a design capacity of the secondary battery.

7. The aging process includes: The method for activating a lithium secondary battery according to claim 1, further comprising: (d-1) a high-temperature aging process for aging the spare lithium secondary battery at a temperature in the range of 50 to 80 degrees Celsius for 10 to 40 hours.

8. The aging process includes: The method for activating a lithium secondary battery according to claim 7, further comprising (d-2) a room temperature aging process of aging the spare lithium secondary battery at a temperature range of 18 to 27 degrees Celsius for 24 to 80 hours.

9. 2. The method for activating a lithium secondary battery according to claim 1, further comprising, after the aging process, (e) a charge-discharge process of charging and discharging the spare lithium secondary battery.

10. 2. The method for activating a lithium secondary battery according to claim 1, further comprising the step of: (f) rolling the spare lithium secondary battery after the initial charging step.

11. 11. The method for activating a lithium secondary battery according to claim 10, wherein in the roll pressing step, the spare lithium secondary battery is roll pressed at a linear pressure of 1 kgf / mm to 10 kgf / mm (9.8 N / mm to 98 N / mm).

12. The method of claim 10, wherein the roll pressing step is performed before the degassing step.

13. 11. The method of claim 10, wherein in the roll pressing, the spare lithium secondary battery is roll pressed in a direction parallel to a first direction, which is a direction in which electrode leads are drawn out.

14. 2. The method for activating a lithium secondary battery according to claim 1, wherein the degassing process is performed once.

15. 2. The method of activating a lithium secondary battery according to claim 1, wherein the step of preparing the spare lithium secondary battery includes a pre-aging step of aging the spare lithium secondary battery for 12 to 48 hours to allow an electrolyte to be impregnated into an electrode assembly.

Citation Information

Patent Citations

  • Battery cell for evaluating lithium precipitation behavior, and method for manufacturing same

    EP4024559A1

  • Manufacture of nonaqueous solvent type secondary battery

    JP1999102729A

  • Bipolar type secondary battery

    JP2008097940A

  • Manufacturing method of lithium secondary batteries

    JP2010528404A

  • Method for manufacturing nonaqueous electrolyte secondary battery

    JP2016119276A