Graphite-based negative electrode material and its manufacturing method

A graphite-based negative electrode material with a graphite oxide and low crystalline carbon coating addresses volume expansion and contraction issues, enhancing electrode stability and battery performance through high tap density and low specific surface area, thus improving cycle characteristics and lifespan.

JP2024541356AActive Publication Date: 2024-11-08POSCO FUTURE M CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2024527805
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-11-24
Filing Date
2022-10-20
Publication Date
2024-11-08
Estimated Expiration
2042-10-20

AI Technical Summary

Technical Problem

Existing graphite-based negative electrode materials face issues with volume expansion and contraction during battery charging and discharging processes, leading to non-uniformity and decreased battery performance, due to their irregular shape and exposure of edges, which cause irreversible reactions and electrolyte decomposition.

Method used

A graphite-based negative electrode material is developed by oxidizing the surface of graphite to form graphite oxide and applying a graphite coating with low crystalline carbon, maintaining a ratio of 1/9 to 1/3, resulting in a material with high tap density and low specific surface area to suppress volume changes and improve manufacturing uniformity.

Benefits of technology

The solution effectively suppresses volume expansion and contraction, enhances electrode stability, and improves battery performance by maintaining high tap density and low specific surface area, resulting in improved cycle characteristics and lifespan.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024541356000001_ABST
    Figure 2024541356000001_ABST
Patent Text Reader

Abstract

The present embodiment relates to a graphite-based negative electrode material, a manufacturing method thereof, a negative electrode including the same, and a lithium secondary battery including the same. The graphite-based negative electrode material according to one embodiment includes a graphite oxide obtained by oxidizing the surface of a first graphite; and a graphite coating including a second graphite and low-crystalline carbon located on the surface of the second graphite, and the ratio of the graphite coating to the graphite oxide is 1 / 9 to 1 / 3.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present embodiment relates to a lithium secondary battery, and more particularly to a graphite-based negative electrode material and a method for producing the same. [Background technology]

[0002] As social interest in the depletion of fossil fuels and the environmental pollution caused by the use of fossil fuels grows, attention is being paid to environmentally friendly energy sources as a means of solving these problems. Among environmentally friendly energy sources, electrical energy has been attracting attention, and lithium secondary batteries in particular have been attracting attention.

[0003] The range of applications of lithium secondary batteries is expanding from small electronic devices and portable IT devices to electric vehicles and energy storage systems. As the range of applications for lithium secondary batteries expands, the development of new materials for high capacity and high output is becoming important. Among the components of lithium secondary batteries, the negative electrode material plays the role of storing lithium ions, and is a factor related to the capacity and lifespan of lithium secondary batteries.

[0004] Various types of carbonaceous materials, including artificial graphite, natural graphite, and hard carbon, which are capable of inserting and extracting lithium, have been used as anode materials. Graphite has a lower discharge voltage of 0.2V compared to lithium, and batteries using graphite as the anode active material show a high discharge voltage of 3.6V, providing an advantage in terms of energy density for lithium secondary batteries. In addition, its excellent reversibility ensures the long life of lithium secondary batteries, making it the most widely used.

[0005] Natural graphite has the advantage of being inexpensive and exhibiting similar electrochemical properties to artificial graphite, making it highly useful as an anode material. However, natural graphite has a plate-like shape with a large surface area and exposed edges, which can cause electrolyte penetration and decomposition reactions when used as an anode active material. As a result, the edges peel off or break, causing major irreversible reactions. When this is manufactured into an electrode plate, the graphitized material is pressed flat and oriented on the current collector, making it difficult to impregnate the electrolyte and reducing charge / discharge characteristics.

[0006] To solve this problem, efforts are being made to transform natural graphite into a smooth surface shape through post-processing such as a spheroidizing process in order to reduce irreversible reactions and improve the processability of the electrode.

[0007] Graphite, which has been commercialized as an anode material, shows excellent life characteristics and high theoretical capacity because oxidation and reduction reactions occur continuously with little change in crystal structure during the insertion and desorption of lithium ions. However, graphite can only accommodate one lithium ion per six carbon atoms, so it can only secure a limited theoretical capacity, for example, about 372mAh / g, and there are limitations to the requirements for high output and high capacity.

[0008] Research into new anode materials to overcome the limitations of graphite is ongoing, with particular interest in silicon-based anode materials. Silicon is not only abundant worldwide, but also has a high theoretical capacity of about 4,200 mAh / g compared to graphite, and has the advantage of being an environmentally friendly material with a low reaction potential with lithium.

[0009] However, silicon-based negative electrode materials have irregular shapes because bulk silicon is mechanically crushed. The irregular shapes induce irregular volume expansion and contraction during the charge and discharge process of silicon, resulting in reduced battery performance, and may also result in non-uniform electrodes being manufactured, resulting in reduced battery performance. Summary of the Invention [Problem to be solved by the invention]

[0010] The technical problem to be solved by the present invention is to provide a carbon-based negative electrode material, which can suppress volume expansion and contraction that occurs during charging and discharging of a battery, and can suppress non-uniformity during electrode manufacturing, thereby preventing a decrease in battery performance.

[0011] Another technical problem to be solved by the present invention is to provide a method for producing a graphite-based negative electrode material having the above-mentioned advantages. [Means for solving the problem]

[0012] According to one embodiment of the present invention, the graphite-based negative electrode material includes a graphite oxide obtained by oxidizing the surface of a first graphite, and a graphite coating including a second graphite and low-crystalline carbon located on the surface of the second graphite, and the ratio of the graphite coating to the graphite oxide is 1 / 9 to 1 / 3. In one embodiment, the graphite-based negative electrode material may have a D50 in the range of 17.5 μm to 19.5 μm.

[0013] In one embodiment, the graphite-based negative electrode material has a tap density of 0.80 g / cm 3 ~0.86g / cm 3 In one embodiment, the specific surface area of ​​the graphite-based negative electrode material is in the range of 4.57 m 2 / g~5.50m 2 In one embodiment, the oil absorption of the graphite-based negative electrode material may be in the range of 51 ml / 100 g to 56 ml / 100 g.

[0014] According to another embodiment of the present invention, the negative electrode for a lithium secondary battery can include 96 to 99 wt % of the above-mentioned graphite-based negative electrode material, 0.5 to 1.5 wt % of a thickener, and the balance of a binder. In one embodiment, the electrode density of the negative electrode for a lithium secondary battery is 1.2 g / m 3 ~1.8g / m 3 may be also possible.

[0015] According to yet another embodiment of the present invention, a lithium secondary battery may include the above-mentioned negative electrode for lithium secondary batteries, a positive electrode including a positive electrode active material, and an electrolyte, and the electrolyte may have an ethylene methyl carbonate (EMC) to ethylene carbonate (EC) ratio of 7 / 3 to 6 / 4.

[0016] According to yet another embodiment of the present invention, a method for producing a graphite-based negative electrode material includes the steps of oxidizing a surface of a first graphite to produce a graphite oxide, mixing a second graphite with low crystalline carbon to produce a graphite coating material, and mixing the graphite coating material with respect to the graphite oxide in a ratio of 1 / 9 to 1 / 3. In one embodiment, the step of producing the graphite oxide includes heating the first graphite at a temperature in the range of 550°C to 650°C.

[0017] In one embodiment, preparing the graphite coating may include mixing the low crystalline carbon with the second graphite in a ratio of 3 / 100 to 4 / 100 to prepare a homogeneous mixture. In another embodiment, firing the homogeneous mixture at a temperature of 1,100° C. or more. In one embodiment, the method for preparing the graphite-based negative electrode material may include providing the graphite-based negative electrode material with an oil absorption in the range of 51 ml / 100 g to 56 ml / 100 g. Effect of the Invention

[0018] According to one embodiment, the negative electrode material includes a graphite oxide obtained by oxidizing a surface of a first graphite, a second graphite, and a graphite coating obtained by disposing low-crystalline carbon on a surface of the second graphite, and the graphite coating is 1 / 9 to 1 / 3 of the graphite oxide. This provides a carbon-based negative electrode material with a small specific surface area and high tap density, thereby suppressing volume expansion and contraction that occurs during the charging and discharging process of a battery and suppressing non-uniformity during the manufacturing of the electrode, thereby preventing a decrease in battery performance. [Brief description of the drawings]

[0019] [Figure 1A]1 is a structure photograph of graphite oxide showing the configuration of a graphite-based negative electrode material according to one embodiment of the present invention. [Figure 1B] 1 is a structure photograph of a graphite coating of a graphite-based negative electrode material according to an embodiment of the present invention; [Diagram 2] 1 is a flowchart illustrating a method for manufacturing a graphite-based negative electrode material according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0020] Terms such as first, second and third are used to describe various parts, components, regions, layers and / or sections, but are not limited thereto. These terms are used only to distinguish one part, component, region, layer or section from another part, component, region, layer or section. Thus, the first part, component, region, layer or section described below may be referred to as a second part, component, region, layer or section without departing from the scope of the present invention.

[0021] The terminology used herein is merely for the purpose of referring to particular embodiments and is not intended to limit the present invention. As used herein, the singular form includes the plural form unless the language clearly indicates otherwise. The meaning of "comprising" as used in the specification embodies certain features, regions, integers, steps, operations, elements and / or components and does not exclude the presence or addition of other features, regions, integers, steps, operations, elements and / or components.

[0022] When we refer to an item as being "on" another item, this means that it is exactly on top of the other item, or there may be other items between them. In contrast, when we refer to an item as being "directly on" another item, there are no other items between them.

[0023] Unless otherwise defined, all terms, including technical and scientific terms, used herein have the same meaning as commonly understood by a person of ordinary skill in the art to which the present invention belongs. Terms defined in commonly used dictionaries are additionally interpreted to have a meaning consistent with the relevant technical literature and the presently disclosed content, and are not interpreted in an ideal or very formal sense unless otherwise defined.

[0024] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS Hereinafter, preferred embodiments of the present invention will be described in detail by way of example only, and are not intended to limit the present invention, which is defined only by the scope of the following claims.

[0025] 1A and 1B are structural photographs of graphite oxide and graphite coating, respectively, showing the structure of a graphite-based negative electrode material according to one embodiment of the present invention.

[0026] 1A and 1B, FIG. 1A is a scanning electron microscope (SEM) photograph showing the state of graphite oxide particles, and FIG. 1B is a SEM photograph of graphite coating particles. The graphite-based negative electrode material may include graphite oxide and graphite coating. The graphite oxide may be obtained by oxidizing the surface of a first graphite, and the graphite coating may include a graphite coating in which a second graphite and low-crystalline carbon are mixed.

[0027] In one embodiment, the first graphite and the second graphite may be natural graphite, as a non-limiting example. The natural graphite may be, for example, spherical natural graphite. The natural graphite is plate-shaped and highly oriented, which may make it difficult to apply it to a battery, such as causing a decrease in output in an electrode plate, and the first graphite and the second graphite of the present invention may be spherical graphite.

[0028] In one embodiment, the graphite oxide may be obtained by oxidizing graphite. The first graphite is oxidized in an oxidizing atmosphere, whereby carbon (C) on the surface of the first graphite reacts with oxygen (O2) to produce and emit carbon dioxide (CO2).

[0029] In one embodiment, the graphite oxide may have an average particle size (D50) of 12 μm to 20 μm, specifically 15 μm to 18 μm. The D50 is defined as a cumulative median diameter, and is a part of the volume cumulative particle size distribution. The volume cumulative particle size distribution is obtained by assuming a collection of one powder, and when a cumulative curve is obtained with the total volume of the powder collection as 100% in the particle size distribution, the particle sizes at the points where the cumulative curve is 10%, 50%, and 0% are represented as the 10% diameter, 50% diameter, and 90% diameter (μm), respectively.

[0030] In one embodiment, when the graphite oxide is within the above range, a stable anode material can be produced during electrode production, a high density electrode can be produced using the anode material, and the life and safety of the battery can be improved. However, this is a non-limiting example, and it is clear that the graphite oxide can be appropriately classified as necessary.

[0031] In one embodiment, the graphite coating may include a second graphite and a low-crystalline carbon located on a surface of the second graphite. The second graphite may be, for example, a spherical natural graphite, and the low-crystalline carbon material may be a petroleum pitch, a coal pitch, a mesophase pitch carbide, a low molecular weight heavy oil, polyvinyl alcohol (PVA), polyvinyl chloride (PVC), sucrose, a calcined coke, or a combination thereof, and may specifically be a softening point 250 pitch.

[0032] In one embodiment, the graphite coating may be a mixture of the low crystalline carbon and the second graphite at a ratio of 3 / 100 to 4 / 100. Specifically, the second graphite and the low crystalline carbon material may be mixed at a weight ratio of 100:3 to 100:4, specifically 94:6 to 98:2, and more specifically 95:5 to 97:3. By mixing the low crystalline carbon material at a weight ratio within this range, a coating layer that is uniformly coated on the surface of the spherical graphite may be formed.

[0033] In one embodiment, the average particle size (D50) of the graphite coating material may be 17.5 to 19.5 μm, specifically 18 μm to 19 μm. Within this range, a stable negative electrode material can be produced during electrode production, and a high-density electrode can be produced using the negative electrode material, improving the life and safety of the battery. However, this is a non-limiting example, and it is clear that the graphite coating material can be appropriately classified as necessary.

[0034] In one embodiment, the graphite coating material is 1 / 9 to 1 / 3 relative to the graphite oxide. Specifically, the graphite oxide and the graphite coating material may be in a weight ratio of 90:10 to 75:25. By utilizing a graphite-based negative electrode material mixed in this weight ratio range, a secondary battery having excellent initial capacity, efficiency, and life characteristics can be manufactured. More specifically, the graphite oxide and the graphite coating material may be in a weight ratio range of 85:15 to 80:20. In this weight ratio range, a content ratio having high tap density, low specific surface area, and excellent cycle characteristics can be obtained.

[0035] As the ratio of the graphite coating material increases, the specific surface area decreases, the tap density increases, the electrical conductivity of the lithium secondary battery decreases, the impregnation of the electrolyte decreases, and the cycle characteristics decrease.As the ratio of the graphite oxide increases, the specific surface area increases, the tap density decreases, the electrical conductivity of the lithium secondary battery increases, the impregnation of the electrolyte increases, and the cycle characteristics increase.

[0036] If the ratio of the graphite oxide is too high, the tap density becomes too low, which causes a decrease in packing density and may cause a limit in rolling the electrode. Therefore, when the graphite coating material is mixed with the graphite oxide in the graphite-based negative electrode material in a ratio of 1 / 9 to 1 / 3, specifically 3 / 17 to 1 / 4, a graphite-based negative electrode material having advantages of high tap density, low specific surface area, and excellent cycle characteristics can be provided.

[0037] In one embodiment, the graphite-based negative electrode material may have a D50 in the range of 18.5 μm to 20.5 μm. Specifically, the graphite-based negative electrode material may have a D50 in the range of 18.5 μm to 19 μm.

[0038] In one embodiment, the graphite-based negative electrode material has a tap density of 0.80 g / cm 3 ~0.90g / cm 3 The tap density of the graphite-based negative electrode material may be specifically in the range of 0.82 g / cm 3 ~0.86g / cm 3 If the tap density of the graphite-based negative electrode material is greater than the lower limit, the ratio of oxide is increased, and pores formed on the outer surface of the oxide cause excessive viscosity during slurry preparation, ultimately resulting in a decrease in the absolute value of the active material disposed on the current collector, resulting in a decrease in packing density. If the tap density of the graphite-based negative electrode material is greater than the upper limit, the particle size is varied, resulting in relatively small particle voids that impede the permeation of the electrolyte, resulting in a decrease in ion conductivity, resulting in a decrease in processability during electrode preparation and cycle characteristics of the lithium secondary battery.

[0039] In one embodiment, the graphite-based negative electrode material has a specific surface area of ​​4.57 m 2 / g~5.50m 2 The specific surface area of ​​the graphite-based negative electrode material may be in the range of 4.60 m 2 / g~5.10m 2The specific surface area of ​​the graphite-based negative electrode material decreases as the ratio of the graphite coating increases, and the graphite coating contains about 3% amorphous carbon, so the irreversible capacity is greater than that of graphite oxide.

[0040] If the specific surface area is greater than the lower limit, there is a problem that the irreversible capacity may increase, whereas if the specific surface area is greater than the upper limit, there is a problem that the oxidation of the oxidized product is insufficient, and therefore channels cannot be formed well on the surface of the graphite-based negative electrode material, resulting in a low oil absorption and a low impregnation of the electrolyte.

[0041] In one embodiment, the oil absorption of the graphite-based negative electrode material may be in the range of 51 ml / 100 g or more. Specifically, the oil absorption of the graphite-based negative electrode material may be in the range of 51.0 ml / 100 g to 56.0 ml / 100 g. More specifically, the oil absorption of the graphite-based negative electrode material may be in the range of 51.5 ml / 100 g to 55.0 ml / 100 g. The oil absorption may be, for example, the oil absorption of linseed oil. When the oil absorption of the graphite-based negative electrode material exceeds the upper limit, the viscosity may increase and the slurry characteristics may decrease. When the oil absorption of the graphite-based negative electrode material exceeds the lower limit, the impregnation of the electrolyte and the lithium ion conductivity decrease, resulting in a problem of a decrease in the capacity and cycle characteristics of the lithium secondary battery.

[0042] When the oil absorption of the graphite-based negative electrode material satisfies the range of 51 ml / 100 g or more, it has the advantage of increasing the impregnation of the electrolyte and lithium ion conductivity, thereby improving cycle characteristics. When the oil absorption of the graphite-based negative electrode material exceeds the upper limit of the range, the surface of the graphite oxide in the graphite-based negative electrode material becomes rough and there are many voids, which causes a problem of agglomeration during the manufacture of an electrode using the graphite-based negative electrode material.

[0043] In one embodiment, the viscosity of the graphite-based negative electrode material may be in the range of 11,750 to 13,500 cP. Specifically, the viscosity may be in the range of 12,000 to 13,000 cP. If the viscosity exceeds the upper limit, the slurry becomes too thick, and when used in the manufacture of an electrode, a phenomenon of solidification occurs, resulting in a problem of deterioration of the slurry and electrode properties. If the viscosity exceeds the lower limit, there is a problem of deterioration of electrical conductivity during the manufacture of an electrode.

[0044] In one embodiment, the graphite-based negative electrode material has an electrical conductivity of 276.0 S / cm or more. Specifically, the electrical conductivity may be 280.0 S / cm or more. The electrical conductivity may be 700 kgf / cm or more. 2 The higher the electrical conductivity, the higher the ionic conductivity, since electrons must flow in order for ions to be conducted.

[0045] In one embodiment, a negative electrode for a lithium secondary battery may be provided, the negative electrode for a lithium secondary battery comprising the graphite-based negative electrode material. The negative electrode for a lithium secondary battery may comprise the graphite-based negative electrode material, a thickener, and a binder. The graphite-based negative electrode material may refer to the graphite-based negative electrode material described above to the extent that it is not inconsistent.

[0046] The thickener is an additive for increasing the viscosity of the negative electrode material, and may include, for example, at least one of carboxymethyl cellulose (CMC), guar gum, non-crosslinked polyacrylic acid, uncrosslinked polyacrylic acid, and polyvinyl alcohol.

[0047] The binder can effectively bond particles constituting the negative electrode material to each other and facilitate adhesion of the negative electrode material to a current collector, and can include, for example, at least one of polyvinylidene fluoride, ethylene-propylene-diene terpolymer, styrene butadiene rubber (SBR), acrylonitrile-butadiene rubber, fluororubber, polyvinyl acetate, polymethylmethacrylate, polyethylene, and cellulose nitrate.

[0048] In one embodiment, the negative electrode for a lithium secondary battery can include 96 to 99 wt % of a graphite-based negative electrode material, 0.5 to 1.5 wt % of a thickener, and the balance of a binder. In one embodiment, the negative electrode for a lithium secondary battery has an electrode density of 1.2 g / m 3 ~1.8g / m 3 In the above-mentioned electrode density range, the initial capacity, efficiency, and life characteristics of the lithium secondary battery can be improved when the electrode is manufactured in the future.

[0049] In one embodiment, a lithium secondary battery including the graphite-based negative electrode material can be provided. In one embodiment, the lithium secondary battery can include a negative electrode including the graphite-based negative electrode material, a positive electrode including a positive electrode active material, and an electrolyte. The graphite-based negative electrode material and the negative electrode are the same as those described above, and the positive electrode can refer to a positive electrode used in a typical lithium secondary battery. In one embodiment, the electrolyte may have ethylene methyl carbonate (EMC) with respect to ethylene carbonate (EC) in a ratio of 7 / 3 to 6 / 4. Specifically, the electrolyte may include the ethylene carbonate and the ethylene methyl carbonate in a weight ratio of 30:70 to 40:60. By including the graphite-based negative electrode material, the lithium secondary battery can have physical properties of an initial capacity of 360 mAh / g or more, specifically 363 mAh / g or more, an efficiency of 93.0% or more, specifically 94.0% or more, and a life characteristic of 88% or more, specifically 91% or more.

[0050] FIG. 2 is a flow chart of a method for producing a graphite-based negative electrode material according to one embodiment of the present invention.

[0051] 2, a method for manufacturing a graphite-based negative electrode material according to an embodiment of the present invention may include step S100 of oxidizing a surface of a first graphite to manufacture a graphite oxide, step S200 of mixing a second graphite with low crystalline carbon to manufacture a graphite coating, and step S300 of mixing the graphite coating with respect to the graphite oxide in a ratio of 1 / 9 to 1 / 3. For a detailed description of the first graphite, the second graphite, the graphite oxide, the low crystalline carbon, and the graphite coating, please refer to FIG. 1.

[0052] The step S100 of preparing graphite oxide by oxidizing the surface of the first graphite may be performed under gaseous or solid oxidation conditions containing a material capable of oxidizing the first graphite. Under the oxidation conditions, the graphite oxide oxidizes the first graphite, for example, spheroidal graphite, and removes some or all of defects in the crystal structure of the spheroidal graphite. The gaseous or solid state may contain, for example, oxygen. As a result, carbon element (C) in the spheroidal graphite, for example, on the surface, reacts with oxygen element (O2) to produce and emit carbon dioxide (CO2).

[0053] In one embodiment, the step of preparing the graphite oxide may include heating the first graphite at a temperature in the range of 550° C. to 700° C. The graphite oxide is prepared by heat treatment in an atmosphere at a temperature of 500° C. to 700° C., specifically, 550° C. to 650° C. As a result, the graphite oxide can have side reaction-inducing organic substances removed from the surface thereof, and voids, e.g., channels, generated by removing the side reaction-inducing organic substances are increased, facilitating the movement of lithium ions.

[0054] The step S200 of preparing a graphite coating material by mixing the second graphite and the low crystalline carbon may include mixing and stirring the second graphite and the low crystalline carbon. The step of preparing the graphite coating material may include mixing the second graphite and the low crystalline carbon in a weight ratio of 3 / 97 to 2 / 98. Specifically, the step may include mixing the second graphite and the low crystalline carbon in a weight ratio of 97:3 to 98:2 to prepare a uniform mixture.

[0055] In one embodiment, the mixing and stirring is performed by a mechanical mixing process, which is performed after spheroidizing the second graphite by selecting any one of ball milling, mechanofusion milling, shaker milling, planetary milling, attritor milling, disk milling, shape milling, nauta milling, nobilta milling, or a combination thereof.

[0056] In one embodiment, the mechanical mixing treatment can be performed at a rotation speed of 300 to 2000 rpm. In another embodiment, the mechanical mixing treatment can be performed in a two-stage treatment. Specifically, the two-stage treatment can include a first stage rotation at a rotation speed of 300 to 1000 rpm, followed by a second stage rotation at a rotation speed of 1000 rpm to 2000 rpm. By performing the two-stage treatment, the second graphite and the low crystalline carbon can be uniformly mixed and stirred.

[0057] In one embodiment, preparing the homogeneous mixture may further include calcining the homogeneous mixture at a temperature of 1,100° C. or more. In one embodiment, the calcining is performed in a gas atmosphere. The gas atmosphere may be nitrogen (N2), argon (Ar), helium (He), hydrogen (H2), or a mixture thereof. The calcining may produce a graphite coating in which low crystalline carbon is uniformly applied to a surface of the second graphite. In one embodiment, preparing the homogeneous mixture may further include classifying the homogeneous mixture through a 45 μm sieve.

[0058] In step S300 of mixing the graphite oxide and the graphite coating material in a ratio of 1 / 9 to 1 / 3, the graphite oxide and the graphite coating material may be mixed in a weight ratio of 95:5 to 75:25. By mixing in this range, a graphite-based negative electrode material having a low tap density and a high specific surface area can be manufactured. Thus, by including the graphite-based negative electrode material, a lithium secondary battery having excellent initial capacity, high efficiency, and excellent life characteristics can be manufactured. EXAMPLES

[0059] Examples of the present invention and comparative examples are shown in Figures 1 and 2. The following examples and comparative examples are merely examples of the present invention, and the present invention is not limited to the following examples.

[0060] To measure the tap density of the following examples and comparative examples, 15g of powder was filled into a 50ml cylinder and tapped and rotated 3,000 times simultaneously, using a tap density measuring device (Quantachrome's Autotap) etc. To measure the oil absorption, 30g of powder was put into the mixing unit of an oil absorption measuring device (ASAHI SOUKEN's S-500), and linseed oil was added and rotated simultaneously to measure the oil absorption per 100g of sample.

[0061] <Example 1> 1. Method for producing graphite oxide Spherical natural graphite with an average particle size of 18 μm was oxidized in an air atmosphere at 600° C. for 3 hours in a continuous rotary kiln. The physical properties of the oxidized natural graphite were measured, and the average particle size was 18.5 μm and the tap density was 0.78 g / cm. 3 , specific surface area is 5.4m 2 The oil absorption of linseed oil is 58.3 ml / 100 g. The natural graphite oxide is classified using a 45 μm sieve.

[0062] 2. Manufacturing method of graphite coating Spherical natural graphite with an average particle size of 17.5 μm and pitch were mixed in a weight ratio of 96:4 and mechanically mixed for 10 minutes at 1,500 rpm using a high-speed stirrer to prepare a homogeneous mixture. The homogeneous mixture was sintered in a nitrogen atmosphere at 1,200°C for 12 hours to produce a natural graphite-low crystalline carbon composite. The physical properties of the oxidized natural graphite were measured to find that it had an average diameter of 17.9 μm and a tap density of 1.09 g / cm. 3 , specific surface area is 2.7m 2 / g, and the oil absorption of linseed oil is 42.7 ml / 100 g.

[0063] 3. Manufacturing method of graphite-based negative electrode material The natural graphite oxide and the natural graphite coating were mixed in a weight ratio of 90:10.

[0064] 4. Manufacturing method of negative electrode The composite for the negative electrode material was mixed with carboxymethyl cellulose (CMC) as a thickener and styrene butadiene rubber (SBR) as a binder in a mass ratio of 98:1:1, and then dispersed in deionized distilled water to prepare a negative electrode active material layer composition. The mixture was applied to copper foil, dried, and rolled to obtain an electrode with a density of 1.4 g / m. 3 The negative electrode was manufactured so that

[0065] 5. Manufacturing method of lithium secondary battery The negative electrode and the counter electrode were made of lithium metal, and a polypropylene separator was placed between the negative electrode and the counter electrode in a battery container, and an electrolyte was injected to manufacture a lithium secondary battery. The electrolyte used was a mixture of ethylene carbonate (EC):ethylene methyl carbonate (EMC) in a ratio of 3:7, and 0.5 wt% vinylidene carbonate (VC), in which 1M LiPF6 was dissolved.

[0066] <Example 2> The same procedure as in Example 1 was repeated, except that the graphite oxide was used in an amount of 85 wt % and the graphite coating material was used in an amount of 15 wt %.

[0067] <Example 3> The same procedure as in Example 1 was repeated, except that the graphite oxide was used in an amount of 80 wt % and the graphite coating material was used in an amount of 20 wt %.

[0068] <Example 4> The same procedure as in Example 1 was repeated, except that the graphite oxide was used in an amount of 75 wt % and the graphite coating material was used in an amount of 25 wt %.

[0069] <Comparative Examples 1 to 5> Comparative Example 1 used 70 wt % of the graphite oxide and 30 wt % of the graphite coating material, Comparative Example 2 used 65 wt % of the graphite oxide and 35 wt % of the graphite coating material, Comparative Example 3 used 60 wt % of the graphite oxide and 40 wt % of the graphite coating material, Comparative Example 4 used 55 wt % of the graphite oxide and 45 wt % of the graphite coating material, and Comparative Example 5 used 50 wt % of the graphite oxide and 50 wt % of the graphite coating material.

[0070] <Comparative Examples 6 to 8> Comparative Example 6 was carried out in the same manner as Example 1, except that 100% of the raw material was used, 100% of the graphite oxide was used, and 100% of the graphite coating was used. Comparative Example 7 was carried out in the same manner as Example 1, except that 100% of the graphite oxide was used, and 100% of the graphite coating was used.

[0071] The physical properties of Examples 1 to 4 and Comparative Examples 1 to 8 can be confirmed from Table 1 below.

[0072] [Table 1]

[0073] As can be seen from Table 1, the ratio of the graphite coating to the graphite oxide is 1 / 9 to 1 / 3, and specifically, the graphite oxide and the graphite coating have a low tap density, a high specific surface area, a high viscosity, and a high electrical conductivity in a weight ratio range of 90:10 to 75:25. Specifically, it can be seen that the graphite-based negative electrode materials according to Examples 1 to 4 and Comparative Examples 1 to 5 have a lower tap density value as the ratio of the mixed graphite oxide increases, and the tap density value increases as the ratio of the graphite coating increases. In addition, it can be seen that the graphite-based negative electrode materials according to Examples 1 to 4 and Comparative Examples 1 to 5 have an improved oil absorption value as the ratio of the mixed graphite oxide increases, and the oil absorption value increases as the ratio of the graphite coating decreases.

[0074] It can be seen that in the graphite-based anode materials of Comparative Examples 6 and 7, the oxidation of the graphite surface increases the oil absorption, and in the graphite-based anode materials of Comparative Examples 7 and 8, the low crystalline carbon coating reduces the oil absorption. This confirms that the graphite-based anode materials in which the graphite coating and the graphite oxide are mixed are used as a negative electrode material, and that the secondary battery has excellent initial capacity, efficiency, and life characteristics.

[0075] The present invention is not limited to the above-mentioned embodiments, and can be manufactured in various different forms, and a person skilled in the art to which the present invention pertains will understand that the present invention can be embodied in other specific forms without changing the technical idea or essential features of the present invention. Therefore, it should be understood that the above-mentioned embodiments are illustrative in all respects and are not limiting.

Claims

1. A graphite oxide obtained by oxidizing the surface of the first graphite; and a graphite coating including a second graphite and low crystalline carbon located on a surface of the second graphite; The graphite-based negative electrode material has a graphite coating ratio of 1 / 9 to 1 / 3 to the graphite oxide.

2. The graphite-based negative electrode material according to claim 1, wherein the graphite-based negative electrode material has a D50 in the range of 17.5 to 19.5 μm.

3. The tap density of the graphite-based negative electrode material is 0.80 g / cm 3 ~0.86g / cm 3 The graphite-based negative electrode material according to claim 1, wherein the graphite-based negative electrode material has a molecular weight of 1000 or more.

4. The specific surface area of ​​the graphite-based negative electrode material is 4.57 m 2 / g to 5.50 m 2 The graphite-based negative electrode material according to claim 1, wherein the carbon black content is in the range of 0.1 to 0.5 wt %.

5. 2. The graphite-based negative electrode material according to claim 1, wherein the graphite-based negative electrode material has an oil absorption in the range of 51 ml / 100 g to 56 ml / 100 g.

6. 6. A negative electrode for a lithium secondary battery comprising 96 to 99 wt % of the graphite-based negative electrode material according to claim 1, 0.5 to 1.5 wt % of a thickener, and the balance being a binder.

7. Electrode density is 1.2 g / m 3 ~1.8g / m 3 The negative electrode for a lithium secondary battery according to claim 6 ,

8. The negative electrode for a lithium secondary battery according to any one of claims 6 and 7; a positive electrode comprising a positive electrode active material; and Contains electrolytes, The electrolyte of the lithium secondary battery is ethylene methyl carbonate (EMC) with respect to ethylene carbonate (EC) in a ratio of 7 / 3 to 6 / 4.

9. oxidizing the surface of the first graphite to produce graphite oxide; mixing the second graphite with low crystalline carbon to produce a graphite coating; and The graphite coating material is mixed with the graphite oxide in a ratio of 1 / 9 to 1 / 3.

10. The method of claim 9, wherein the step of producing the graphite oxide comprises heating the first graphite at a temperature in the range of 550° C. to 650° C.

11. 10. The method of claim 9, wherein the graphite coating comprises mixing the second graphite and the low crystalline carbon in a ratio of 3 / 100 to 4 / 100 to prepare a uniform mixture.

12. The method for producing a graphite-based negative electrode material according to claim 11, further comprising a step of firing the homogeneous mixture at a temperature of 1,100° C. or higher.

13. The method for producing a graphite-based negative electrode material according to claim 9, wherein the graphite-based negative electrode material has an oil absorption in the range of 51 ml / 100 g to 56 ml / 100 g.

Citation Information

Patent Citations

  • Negative electrode active material for rechargeable lithium battery, method of preparing the same, and rechargeable lithium battery including the same

    KR1020150089209A