Recycling of Plastics by Solvent Targeted Recovery and Precipitation ("STRAP")

The STRAP process effectively recycles multilayer plastic films by selectively dissolving and precipitating individual polymer components, addressing the chemical incompatibility issue and achieving efficient waste reduction.

JP2024541759APending Publication Date: 2024-11-12WISCONSIN ALUMNI RES FOUND
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
JP2024529945
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-11-18
Filing Date
2022-11-18
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Current recycling technologies are inadequate for multilayer plastic films due to chemical incompatibility of layers, leading to significant post-industrial and post-consumer waste accumulation, which cannot be efficiently recycled using traditional methods.

Method used

A method called Solvent Targeted Recovery and Precipitation (STRAP) that selectively dissolves individual polymer components in multilayer plastic films using computer-aided solvent selection and temperature control, followed by mechanical filtration and precipitation, allowing for the recovery of pure polymer streams.

Benefits of technology

The STRAP process achieves nearly complete separation and recovery of individual polymers from multilayer plastic films, making them suitable for reuse, with a cost comparable to virgin materials, and reducing waste accumulation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024541759000001_ABST
    Figure 2024541759000001_ABST
Patent Text Reader

Abstract

A method for recovering constituent polymers in a multi-layer plastic film or mixed plastic waste is disclosed herein. The method involves selectively dissolving certain polymers in a solvent at a temperature that dissolves some polymers but not other polymers in the multi-layer plastic film or mixed plastic waste. The solubilized polymers are then separated from the multi-layer plastic film or mixed plastic waste by mechanical filtration and precipitated by changing the temperature and / or adding a co-solvent. The process is repeated for each polymer component, resulting in multiple separated streams that can be recycled. Computational tools are used to select solvent systems and temperatures that selectively dissolve various polymers among all the components.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] [CROSS REFERENCE TO RELATED APPLICATIONS] Priority is claimed to Provisional Application No. 63 / 280,669, filed November 18, 2021, which is incorporated herein by reference.

[0002] [Federal Funding Statement] This invention was made with government support under DE-EE0009285 awarded by the U.S. Department of Energy. The Government has certain rights in this invention. [Background technology]

[0003] Multilayer plastic films are ubiquitous in the flexible and rigid plastic packaging industry (LK Massey, Permeability Properties of Plastics and Elastomers: A Guide to Packaging and Barrier Materials. William Andrew, Norwich, NY, 2003). These composites are composed of different layers of heteropolymers such as polyolefins and polyesters, with each layer selected to provide property benefits corresponding to the bulk material depending on the application (OG Piringer, AL Baner, Plastic Packaging: Interactions with Food and Pharmaceuticals. Wiley-VCH Verlag GmbH & Co. KGaA, Weinheim, 2008).

[0004] The versatility and affordability of multilayer plastic films have created a lot of demand. As a result, the world produces more than 100 million tons of multilayer thermoplastics every year (D. Lithner et al., Environmental and health hazard ranking and assessment of plastic polymers based on chemical composition. Sci. Total Environ. 409, 3309-3324 (2011)). However, up to 40% of the multilayer films produced are not used in final packaging applications due to inefficiencies in the packaging manufacturing process, such as cutting the film into template shapes (R. Coles, MJ Kirwan, Food and Beverage Packaging Technology. Blackwell Publishing Ltd, 2011). These unused fractions are a large source of post-industrial waste (PIW) that is not contaminated with food or other impurities and can be easily recovered and reintroduced into multilayer film manufacturing equipment. However, multilayer packaging materials cannot be recycled by traditional plastic recycling techniques (e.g., mechanical recycling) because the different layers are chemically incompatible. To fit into existing recycling infrastructure, multi-layer plastic waste must first be partially or completely broken down into its component resins, which are then fed into a processor to produce a reconstituted multi-layer film (JM Garcia, ML Robertson, The future of plastics recycling. Science 358, 870-872 (2017)). Currently, no commercially viable technologies exist. Similar issues exist for multi-layer plastics present in post-consumer municipal waste streams.That is, while technologies exist for recycling monocomponent plastics based on mechanical or chemically assisted methods (NA Rorrer et al., Combining reclaimed PET with bio-based monomers enables plastics upcycling. Joule 3, 1006-1027 (2019)), there are no strategies to process multi-layer films in a closed-loop primary recycling scheme (O. Horodytska, FJ Valdes, A. Fullana, Plastic flexible films waste management - A state of art review. Waste Manag. 77, 413-425 (2018); P. Lacy, J. Rutqvist, Waste to Wealth: The Circular Economy Advantage. Palgrave Macmillan, New York, NY, 2016). Moreover, in contrast to PIW, these post-consumer waste streams are contaminated with food and other impurities, making cleaning a challenge. Together, these technology gaps represent a key aspect of the ongoing human and environmental health crisis characterized by the accumulation of plastic waste in the oceans, decaying human habitats, and the death of marine life (CM Rochman et al., Policy: Classify plastic waste as hazardous. Nature 494, 169-171 (2013)).

[0005] One approach to recover individual polymer components from mixed plastic waste is to selectively dissolve the polymer of interest in a solvent system (G. Pappa et al., The selective dissolution / precipitation technique for polymer recycling: A pilot unit application. Resour. Conserv. Recycl. 34, 33-44 (2001); DS Achilias et al., Chemical recycling of plastic wastes made from polyethylene (LDPE and HDPE) and polypropylene (PP). J. Hazard. Mater. 149, 536-542 (2007)). Technologies based on this strategy have been investigated and are currently being implemented by a number of companies. For example, APK's Newcycling process is based on preferential dissolution of polyethylene (PE) or polypropylene from multi-layer plastics in a solvent system consisting of alkanes, isooctane, or cycloalkanes (I. Vollmer et al., Beyond mechanical recycling: Giving new life to plastic waste. Angew. Chem. Int. Ed. 59, 15402-15423 (2020)); the dissolved polymer is recovered from the solution and pelletized by extrusion (M. Niaounakis, Recycling of Flexible Plastic Packaging. Plastics Design Library, William Andrew, 2020; K. Wohnig, in GPCA PlastiCon, 2018). The CreaSolv process is based on selective dissolution of polyolefins using a solvent selected from the group of aliphatic hydrocarbons. An antisolvent consisting of a mono / polyhydroxy hydrocarbon, such as 1-propanol or 1,3-propanediol, is then used to precipitate the polyolefin from the mixture (US Pat. No. 8,138,232).The PureCycle process contacts plastic waste with a proprietary solvent at high temperature and pressure to obtain purified polypropylene (PP). Solvay's VinyLoop® process separates polyvinyl chloride (PVC) from its polymer coating and involves both mechanical and selective dissolution steps using a proprietary solvent. The above examples show that selective dissolution is a promising approach to recycle complex plastic waste. However, while these technologies process large amounts of waste plastic, only one or two polymer components can be recovered in pure form.

[0006] Several chemical depolymerization processes have been developed to convert polyesters into monomer units, such as Eastman's methanolysis process (P. Muhs et al., Recycling PET bottles by depolymerization. Kunstst. Ger. Plast. 82, 289-292 (1992)), IBM's Volcat process (K. Fukushima et al., Advanced chemical recycling of poly (ethylene terephthalate) through organocatalytic aminolysis. Polym. Chem. 4, 1610-1616 (2013)), and Ioniqa's catalytic PET process (U.S. Pat. No. 10,266,479). These techniques are likely to be more costly to operate, as they require the reconstitution of virgin polymers from their corresponding monomers, necessitating more separation steps. Other fundamental research efforts in waste plastics recycling aim to replace multilayer film components with polymers that are more easily depolymerized or biodegraded. However, these efforts represent long-term approaches that are far from commercialization (B. Fan et al., Polyglyoxylates: A versatile class of triggerable self-immolative polymers from readily accessible monomers. J. Am. Chem. Soc. 136, 10116-10123 (2014); EKY Chen et al., Self-immolative polymers containing rapidly cyclizing spacers: Toward rapid depolymerization rates. Macromolecules 45, 7364-7374 (2012)).

[0007] The diversity of these examples illustrates the timeliness of the issues surrounding the recycling of complex, multi-layered plastics. These multi-layered packaging materials are increasingly coming from post-industrial and post-consumer waste, and therefore require further technological development for more efficient collection, sorting, separation and recycling. Summary of the Invention

[0008] Disclosed herein is a method for recovering constituent polymers in a multi-layer plastic film or mixed plastic waste, the method comprising the steps of: (a) selectively dissolving a polymer in a solvent at a temperature to obtain a solubilized polymer, the polymer dissolving but not other polymers in the multi-layer plastic film or mixed plastic waste; (b) separating the solubilized polymer from the multi-layer plastic film or mixed plastic waste by mechanical filtration; (c) precipitating the solubilized polymer from the solvent; and (d) repeating steps (a), (b), and (c) for each different polymer in the multi-layer plastic film or mixed plastic waste using a solvent and temperature that selectively dissolves each different polymer. Includes.

[0009] The method further includes using a computational tool to select a solvent and temperature that selectively dissolves a polymer from among all of the components present in the multi-layer plastic film or mixed plastic waste, the computational tool including calculating Hansen solubility parameters (HSP), molecular dynamics (MD) simulation, and combined quantum chemistry and statistical mechanics modeling.

[0010] The method further comprises a deinking step prior to step (a) to remove ink from the multilayer plastic film or mixed plastic waste. In some embodiments, the deinking step is carried out by treating the multilayer plastic film or mixed plastic waste in tetrahydrofuran (THF) and N,N-dimethylformamide (DMF). Alternatively, the deinking step can be omitted entirely or carried out only on the polymer fraction separated with PET. It has been found that most inks used on polymers are separated into the PET fraction.

[0011] The method further comprises, prior to step (a), separating the multi-layer plastic film or mixed plastic waste into a volume of 1 cm 2 In one version, the method further comprises, prior to step (a), shredding the multi-layer plastic film or mixed plastic waste into strips of 5 mm or less, 4 mm or less, 3 mm or less, or 2 mm or less.

[0012] In some embodiments, in step (c), the solubilized polymer is precipitated from the solvent by addition of an antisolvent. In some embodiments, in step (c), the solubilized polymer is precipitated from the solvent by changing the temperature of the solvent.

[0013] In one version of this method, the multilayer plastic film consists essentially of polyethylene (PE), ethylene vinyl alcohol (EVOH) and polyethylene terephthalate (PET). In step (a), PE is selectively dissolved in toluene at about 110° C. and EVOH is selectively dissolved in dimethyl sulfoxide (DMSO) at about 95° C. In step (c), the solubilized PE is precipitated by adding acetone and the solubilized EVOH is precipitated by adding water.

[0014] Alternatively, in step (a), PE is reacted with toluene or C6-C 12The EVOH is selectively dissolved in an alkane, and the EVOH is selectively dissolved in a solvent comprising DMSO and water at about 95° C. In step (c), the solubilized PE is precipitated by lowering the temperature of the toluene to about 35° C., and the solubilized EVOH is precipitated by lowering the temperature of the DMSO and water to about 35° C.

[0015] In one version of this method, the multilayer plastic film further comprises a tie layer comprising ethylene vinyl acetate (EVA). The EVA is dissolved in toluene at about 110° C. in step (a) and precipitated with PE in step (c) by adding acetone, and the EVA is separated from the PE after step (c) by selectively dissolving the EVA in N-methylpyrrolidone (NMP). Alternatively, the EVA is dissolved in toluene with PE in step (a) at about 110° C., and the EVA is separated from the PE in step (c) by reducing the temperature of the toluene to about 35° C. to precipitate the PE.

[0016] In one version of this method, a multilayer plastic film consists essentially of polyethylene terephthalate (PETG), PE, EVOH, and PET. In step (a), PETG is selectively dissolved in a solvent comprising DMF and THF at about 87° C., PE is dissolved in toluene at about 110° C., and EVOH is dissolved in a solvent comprising DMSO and water at about 95° C. In step (c), the solubilized PETG is precipitated by adding 1-propanol, the solubilized PE is precipitated by reducing the temperature of the toluene to about 35° C., and the solubilized EVOH is precipitated by reducing the temperature of the DMSO and water to about 35° C.

[0017] In another version of this method, the mixed plastic waste consists essentially of PE, polypropylene (PP), polyvinyl chloride (PVC), PET and polyamide (PA). In step (a), PE is dissolved in dodecane at about 100° C. and PP is dissolved in toluene at about 110° C. In step (c), the solubilized PE is precipitated by reducing the temperature of the dodecane to about 35° C. and the solubilized PP is precipitated by reducing the temperature of the toluene to about 35° C.

[0018] In yet another version of this method, the multilayer plastic film consists essentially of PE, EVOH, and nylon. In step (a), PE is selectively dissolved in toluene at about 110° C., and EVOH is selectively dissolved in a solvent comprising DMSO and water at about 85° C. In step (c), the solubilized PE is precipitated by reducing the temperature of the toluene to about 35° C., and the solubilized EVOH is precipitated by reducing the temperature of the DMSO and water to about 35° C.

[0019] In a further version of this method, the mixed plastic waste consists essentially of PVC, low density polyethylene (LDPE), PP, high density polyethylene (HDPE), PET, nylon 6,6,6, nylon 6, and nylon 6,6. In step (a), PVC is selectively dissolved in THF at about 68° C., LDPE is selectively dissolved in toluene or a C6-C12 alkane at about 85° C., PP is selectively dissolved in tetrahydropyran (THP) at about 90° C., HDPE is selectively dissolved in toluene at about 110° C., PET is selectively dissolved in gamma valerolactone (GVL) at about 160° C., nylon 6,6,6 is dissolved in 1,2-propanediol at about 135° C., nylon 6 is selectively dissolved in DMSO at about 145° C., and nylon 6,6 is dissolved in formic acid at about 65° C. In step (c), the solubilized PVC is precipitated by the addition of water, the solubilized LDPE is precipitated by reducing the temperature of the toluene to about 35° C., the solubilized PP is precipitated by reducing the temperature of the THP to about 35° C., the solubilized PP is precipitated by reducing the temperature of the THP to about 35° C., the solubilized HDPE is precipitated by reducing the temperature of the toluene to about 35° C., the solubilized PET is precipitated by reducing the temperature of the GVL to about 35° C., the solubilized nylon 6,6,6 is precipitated by reducing the temperature of the 1,2-propanediol to about 35° C., the solubilized nylon 6 is precipitated by reducing the temperature of the DMSO to about 35° C., and the solubilized nylon 6,6 is precipitated by the addition of water.

[0020] The objects and advantages of the present disclosure will become more fully apparent from the following detailed description of preferred embodiments thereof taken in conjunction with the accompanying drawings. [Brief description of the drawings]

[0021] [Figure 1] Overview of the Solvent Targeted Recovery and Precipitation (STRAP) Process. Schematic diagram of a multilayer plastic film composed of three common polymer resins and the key steps of the STRAP process for separating these constituent resins into pure recyclable streams using a series of solvent washes. [Diagram 2] FIG. 1 is a flow chart using a computational tool to select a solvent system and temperature to selectively dissolve a single polymer component from among all components present in a multi-layer plastic film or mixed plastic waste. [Figure 3A] Computational tools used to guide solvent selection for the STRAP process. A process for selecting solvents using a combination of HSP, classical MD simulations, and COSMO-RS calculations. The solubility of PE, EVOH, and PET was estimated using HSP for 22 common solvents. Calculations were then performed using solvents selective for each polymer. Classical MD simulations were performed to provide input oligomer configurations for COSMO-RS, and first-principles calculations were used to calculate the screening charge density for each molecule. The COSMO-RS calculations then determine thermodynamic properties such as solubility. [Figure 3B] Computational tools used to guide solvent selection for the STRAP process. PE-selective solvents, EVOH-selective solvents, and PET-selective solvents and antisolvents (do not dissolve any polymer) determined from HSP calculations. DMSO dimethylsulfoxide; DMF N,N-dimethylformamide; THFA tetrahydrofurfuryl alcohol; THF tetrahydrofuran; NMP N-methylpyrrolidinone; GVL y-valerolactone; IPA isopropyl alcohol. [Figure 3C] Computational tools used to guide solvent selection for the STRAP process. Predicted solubility of PE, EVOH, and PET in pure toluene (PE selective) and DMSO (EVOH selective) versus temperature, calculated using COSMO-RS. The dashed black lines in the figure are the temperatures and mass ratios selected for the STRAP process. [Figure 3D] Computational tools used to guide solvent selection for the STRAP process. Predicted solubility of PE (top) and EVOH (bottom) versus solvent-antisolvent mass ratio. Acetone and water were used as antisolvents for dissolving PE and EVOH, respectively. The black dashed lines in the figure are the temperatures and mass ratios selected for the STRAP process. [Figure 4A] The STRAP process separates PE, EVOH, and PET blends. Schematic of the process for breaking down commercial Amcor multilayer film (Amcor, Zurich, Switzerland) into its constituent resins using the STRAP process. [Figure 4B] The STRAP process separates PE, EVOH, and PET mixtures. Photograph of mixed plastic resin beads consisting of 7:2:2 PE, EVOH, and PET and the resin recovered using the same procedure as shown in Figure 4A. The mass balance for this process is 99.40 wt% with an SE of ±0.19 wt% relative to the initial mass of the physical mixture. Photo by Theodore W. Walker, University of Wisconsin-Madison. [Figure 4C] The STRAP process separates PE, EVOH, and PET blends. Photograph of commercial Amcor film and resin recovered using the STRAP process in Figure 4A. The mass balance for this process was 100.44 wt% relative to the initial mass of the commercial film, with an SE of ±1.39 wt%. Photo by Theodore W. Walker, University of Wisconsin-Madison. [Diagram 5] ATR-FTIR spectra of a) HDPE, b) EVOH, and c) PET. ATR-FTIR spectra are shown for virgin resin beads (top), solids recovered from a physical mixture of resin beads in the STRAP process (middle), and solids recovered from an actual Amcor commercial multilayer film in the STRAP process (bottom). [Figure 6] ATR-FTIR spectrum of HDPE after NMP washing. ATR-FTIR spectrum of PE. The subspectra in each figure correspond to either virgin resin (for reference) or the solids recovered from the STRAP process. The subspectra are labelled accordingly. [Figure 7]Total capital investment and MSP (both as a function of Amcor commercial film supply capacity (tonnes / year)) for the combined recycled PE, EVOH, and PET streams derived from Amcor commercial multilayer film using the STRAP process (circles MSP; boxes capital investment). The market price for virgin PET (2022) is shown as a dotted line for reference. [Figure 8] Example molecular structures of EVOH oligomer (top) and PETG oligomer (bottom) and the corresponding COSMO-RS screening charge densities. [Figure 9] Schematic diagram of the STRAP-A process for separating and recovering polymer components in Amcor multilayer film A1. [Figure 10] COSMO-RS solubility prediction of EVOH in DMSO-water mixed solvent. Two EVOH recovery processes are indicated by arrows. The STRAP-A process dissolves EVOH in pure DMSO at 95°C (predicted solubility 22.77 wt%) and precipitates EVOH in 81.5% water at 48°C (predicted solubility 1.23 wt%). The STRAP-B process dissolves EVOH in 40% water at 95°C (predicted solubility 10.45 wt%) and precipitates EVOH by lowering the temperature to 35°C (predicted solubility 1.72 wt%). [Figure 11] STRAP-B process schematic for the separation and recovery of polymer components in Amcor multilayer film A1. [Figure 12A] ATR-FTIR spectra of virgin resin and polymer recovered from multilayer film A1 by STRAP-A and STRAP-B. PE. [Figure 12B] ATR-FTIR spectra of virgin resin and polymer recovered from multilayer film A1 by STRAP-A and STRAP-B. EVOH. [Figure 12C] ATR-FTIR spectra of virgin resin and polymer recovered from multilayer film A1 by STRAP-A and STRAP-B. PET. [Figure 13]ATR-FTIR spectra: (a) EVA virgin resin, (b) EVA recovered from multilayer film A1 by STRAP-B, (c) PE recovered from multilayer film A1 by STRAP-A, (d) PE recovered from multilayer film A1 by STRAP-B. [Figure 14] STRAP-C process schematic for the separation and recovery of polymer components in Amcor multilayer film A2. [Figure 15A] ATR-FTIR spectra of virgin resin and polymer recovered from multilayer film A2 by STRAP-C. PETG. [Figure 15B] ATR-FTIR spectra of virgin resin and polymer recovered from multilayer film A2 by STRAP-C. PE. [Figure 15C] ATR-FTIR spectra of virgin resin and polymer recovered from multilayer film A2 by STRAP-C. EVOH. [Figure 15D] ATR-FTIR spectra of virgin resin and polymer recovered from multilayer film A2 by STRAP-C. EVA. [Figure 15E] ATR-FTIR spectra of virgin resin and polymer recovered from multilayer film A2 by STRAP-C. PET. [Figure 16] Breakdown of MSPs and revenue destinations for STRAP-A, STRAP-B, and STRAP-C. [Figure 17] Total capital expenditures and MSP as a function of process feed capacity for (A, top) STRAP-B and (B, bottom) STRAP-C processes. [Figure 18] Internal rate of profit as a function of polymer selling price for three different feed capacities of the STRAP-C process. [Figure 19] Sensitivity analysis (±30%) of the parameters of the STRAP-C process. [Figure 20] STRAP process schematic for separation and recovery of polymer components in printed multilayer films with a deinking step. [Figure 21]ATR-FTIR spectra of virgin resin and polymer recovered from multilayer film by STRAP process with deinking step shown in Figure 20. (a) = PE virgin resin (top) and PE STRAP printed film (bottom); (b) = EVOH virgin resin (top) and EVOH STRAP printed film (bottom); (c) = PET virgin resin (top) and PET STRAP printed film (bottom). [Figure 22] STRAP process schematic for separation and recovery of polymer components in printed multilayer films by chopping the film into strips of 2 mm or less size. [Figure 23] ATR-FTIR spectra of virgin resin and polymer recovered from multilayer film by STRAP process applied to strips with size less than 2 mm as shown in Figure 22. (a) = PE virgin resin (top), PE STRAP printed film 803 (middle), PE STRAP printed film 802 (bottom); (b) = EVOH virgin resin (top), EVOH STRAP printed film 803 (middle), EVOH STRAP printed film 802 (bottom); (c) = PET virgin resin (top), PET STRAP printed film 803 (middle), PET STRAP printed film 802 (bottom). [Figure 24] Schematic diagram of the STRAP process for separating and recovering PE and PP from mixed plastic waste. [Diagram 25] Schematic of the STRAP process for separating and recovering polymer components from nylon-based multilayer plastic films. [Figure 26] ATR-FTIR spectra of virgin resin and polymer recovered from nylon-based multilayer plastic film by the STRAP process shown in Figure 25. Left panel = nylon fraction (top) and pure nylon 6 (bottom), center panel = PE fraction (top) and pure LDPE (bottom), right panel = EVOH fraction (top) and pure EVOH (bottom). [Figure 27]STRAP process schematic for the separation and recovery of polymer components from mixed plastic waste consisting of several PEs (LDPE and HDPE), nylons (nylon 6,6,6, nylon 6,6, and nylon 6), PP, PET, and PVC. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0022] Definitions and Abbreviations ATR-FTIR = Attenuated Total Reflectance Fourier Transform Infrared Spectroscopy. COSMO / COSMO-RS = Conductor-Like Screening Model for Realistic Solvents. CPE = Chlorinated Polyethylene. DMF = N,N-Dimethylformamide. DMSO = Dimethylsulfoxide. EVA = Ethylene Vinyl Acetate. EVOH = Ethylene Vinyl Alcohol. GVL = Gamma Valerolactone. HDPE = High Density Polyethylene. HDXLPE = High Density Crosslinked Polyethylene. HMWPE = High Molecular Weight Polyethylene. HSP = Hansen Solubility Parameter. IPA = Isopropyl Alcohol. LDPE = Low Density Polyethylene. LLDPE = Linear Low Density Polyethylene. MD = Molecular Dynamics. NMP = N-Methylpyrrolidinone. PA = Polyamide. PC = Polycarbonate. PE = Polyethylene. PEI = Polyetherimide. PES = Polyethersulfone. PET = Polyethylene terephthalate. PETG = Polyethylene terephthalate. PEX = Crosslinked Polyethylene. PIW = Post-industrial waste. POM = polyoxymethylene. PP = polypropylene. PPO = polyphenylene oxide. PPS = polyphenylene sulfide. PS = polystyrene. PTFE = polytetrafluoroethylene. PVC = polyvinyl chloride. PVDF = polyvinylidene fluoride. SAN = styrene acrylonitrile. SMA = styrene maleic anhydride. STRAP = solvent targeted recovery and precipitation. THF = tetrahydrofuran. THP = tetrahydropyran. UHMWPE = ultra high molecular weight polyethylene. ULMWPE = ultra low molecular weight polyethylene. VLDPE = very low density polyethylene.

[0023] As used herein, the term "about" refers to ±10% of the referenced variable.

[0024] Numeric ranges used herein are intended to include all values ​​and subsets of values ​​contained within the range, whether or not specifically disclosed. Moreover, these numerical ranges should be construed as providing support for a claim directed to any value or subset of values ​​within the range. For example, a disclosure of 1 to 10 should be construed as supporting ranges from 2 to 8, 3 to 7, 5 to 6, 1 to 9, 3.6 to 4.6, 3.5 to 9.9, etc.

[0025] As used herein, the singular forms "a," "an," and "the" include plural referents unless the context clearly dictates otherwise.

[0026] As used herein, the term "or" is an inclusive "or" operator and is equivalent to the term "and / or," unless the context clearly dictates otherwise.

[0027] The elements and method steps described herein, whether explicitly described or not, can be used in any combination unless otherwise specified or clearly implied to the contrary by the context in which the referenced combination is made.

[0028] All combinations of method steps used herein can be performed in any order unless otherwise specified or unless the contrary is clearly implied by the context in which the referenced combination is made.

[0029] The systems disclosed herein comprise, consist of, or consist essentially of the various steps and elements disclosed herein.

[0030] It is understood that the disclosure is not limited to the particular elements and method steps illustrated and described herein, but encompasses such modifications as fall within the scope of the claims.

[0031] Solvent Targeted Recovery and Precipitation (STRAP) Disclosed herein is an approach we call Solvent Targeted Recovery and Precipitation (STRAP) to break down multi-layer plastic films or mixed plastic waste with three or more polymeric components into their constituent resins through a series of solvent washes. As shown by way of example in FIG. 1, the general principle underlying the STRAP process is to selectively dissolve a single polymeric component in a solvent system that dissolves the targeted polymeric component but not the other polymeric components. The solubilized polymeric component is then separated from the multi-layer plastic film or mixed plastic waste by mechanical filtration and precipitated by changing the temperature and / or adding a co-solvent (i.e., anti-solvent) that insolubilizes the dissolved polymer. The solvent and anti-solvent are distilled and reused in the process, and the targeted polymeric component is recovered as a dry pure solid. This process can be repeated for each of the polymeric components in the multi-layer plastic film or mixed plastic waste to obtain multiple fractionated streams that can then be recycled.

[0032] The methods disclosed herein can be used to separate and recover polymer components in multi-layer plastic films or mixed plastic waste having three or more polymer components, including, but not limited to, polyethylene (PE), ethylene vinyl alcohol (EVOH), polyethylene terephthalate (PET), polypropene (PP), polyvinyl chloride (PVC), polyamide (PA), polyethylene terephthalate glycol (PETG), polystyrene (PS), polycarbonate (PC), polyethersulfone (PES), polyoxymethylene (POM), polyetherimide (PEI), polyphenylene oxide (PPO), polyphenylene sulfide (PPS), polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), nylon, styrene maleic anhydride (SMA), and styrene acrylonitrile (SAN). Of these polymers, PE is often classified by its density and branching and includes ultra-high molecular weight polyethylene (UHMWPE), ultra-low molecular weight polyethylene (ULMWPE or PE-WAX), high molecular weight polyethylene (HMWPE), high density polyethylene (HDPE), high density cross-linked polyethylene (HDXLPE), cross-linked polyethylene (PEX or XLPE), medium density polyethylene (MDPE), linear low density polyethylene (LLDPE), low density polyethylene (LDPE), very low density polyethylene (VLDPE), and chlorinated polyethylene (CPE). All of these types of polyethylene are included within the simple definition of the word polyethylene ("PE") as used herein.

[0033] The multilayer plastic film may further include any number of tie layers (also known as adhesive films), such as ethylene vinyl acetate (EVA), wet bond adhesives, and additives (such as TiO) that may be present in small amounts relative to the major resin fraction (typically less than 1 wt% of the total composition).

[0034] The selective solvent used in the present method can be any common industrial solvent, including, but not limited to, toluene, dodecane, o-xylene, p-xylene, benzene, cyclohexane, n-butanol, dimethylformamide (DMF), tetrahydrofurfuryl alcohol, dimethylsulfoxide (DMSO), tetrahydrofuran (THF), tetrahydropyran (THP), N-methyl-2-pyrrolidone (NMP), gamma-valerolactone (GVL), acetone, 1-propanol, 1,2-propanediol, isopropyl alcohol (IPA), methanol, water, formic acid, furfural, acetonitrile, 1,4-dioxane, silane, and dihydropyran.

[0035] The key to the successful implementation of the STRAP process is the preselection of a solvent system and temperature that can selectively dissolve a single polymer component among all the components present in the multi-layer plastic film or mixed plastic waste. The complexity of multi-layer plastic films and mixed plastic waste, often consisting of more than 10 components, and the large variety of industrial solvents and solvent blends available make the selection of a solvent difficult by experimental screening alone. The aforementioned tie layers and additives present in real multi-layer plastic films, which are present in dilute amounts (<1 wt%) and are often unclear, further complicate the problem of identifying an appropriate sequence of solvent-mediated steps to break down the bulk material into a manageable series of separated streams.

[0036] Therefore, we disclose herein a guided approach for the rational selection of solvents using calculations of Hansen solubility parameters (HSPs), molecular dynamics (MD) simulations, and a combined quantum chemistry and statistical mechanics modeling approach named the conductor-like screening model for realistic solvents, as summarized in Figure 2.

[0037] The solubility of a polymer depends on the dispersion interactions between the solvent and the polymer molecules (δ D ), dipole-dipole interaction (δ P), and hydrogen bond interactions (δ H Solubility of a polymer can be characterized by three HSPs that quantify the strength of its interaction with the solvent. These three parameters are used as coordinates to locate the compound in the HSP space. Each polymer also has a radius parameter, R0, which defines a sphere in the HSP space. HSPs (and values ​​of R0) for a wide range of pure solvents and polymers have been tabulated to obtain self-consistent values ​​based on empirical measurements (S. Abbott, C. M. Hansen, Hansen Solubility Parameters in Practice (2008); Hansen-Solubility.com). Solvents' HSPs are estimated as a function of their measured enthalpy of vaporization. The HSP of a polymer is determined by experimentally quantifying the solubility of the polymer in reference solvent systems that span the HSP space and identifying a spherical subspace centered on the polymer's HSP such that the solvents that promote the polymer's dissolution fall within the sphere. Thus, R0 depends on the solubility of the polymer in the reference solvent system.

[0038] "Good" solvents (solvents that promote the dissolution of the polymer at the desired concentration) not included in the reference set are identified by δ using Eq. D -δ P -δ H The geometric distance (R a ) can be determined by calculating

number

[0039] A good solvent is one that is within the solubility range of the corresponding polymer (see Figure 3A for an example), or equivalently, R a / R0 ratio is defined as a solvent with a ratio of less than 1 (1). In this way, in HSP calculations, a good solvent (R a / R0<1) and poor solvent (R a / R0>1). Antisolvents can also be identified as solvents that do not readily dissolve any of the polymer layers.

[0040] MD simulation and COSMO-RS are further used for quantitative solubility prediction. MD simulation provides detailed calculation of polymer structure and conformation. COSMO-RS can predict the solubility of polymer as a function of both temperature and liquid phase composition using the conformation obtained from MD. COSMO-RS combines single molecule density functional theory calculations and statistical thermodynamic methods to take into account molecular interactions, and can predict the solubility of polymer in solvent mixtures a priori as a function of both temperature and liquid phase composition (A. Klamt, Conductor-like screening model for real solvents: A new approach to the quantitative calculation of solvation phenomena. J. Phys. Chem. 99, 2224-2235 (1995); A. Klamt et al., Refinement and parametrization of COSMO-RS. J. Phys. Chem. A 102, 5074-5085 (1998)). See Examples 1 and 2 for exemplary methods of performing MD simulations and COSMO-RS.

[0041] In one version, the method further comprises a deinking step to remove ink from the printed plastic before dissolving the polymeric components. Methods for removing ink from printed plastic have been previously reported, such as using a mixture of surfactants in water (U.S. Pat. No. 9,616,595) and a cleaning agent comprising a non-ionic surfactant, an organic solvent, and an aqueous mineral base (European Patent Publication No. 1419829). It is contemplated that any reagent and method effective for removing ink from printed plastic is useful in the methods disclosed herein. In a preferred embodiment, the deinking step is carried out by treating the multilayer plastic film or mixed plastic waste in a solvent comprising THF and DMF at 83° C.

[0042] The temperature and dissolution time of the solvent for dissolving the polymer can be optimized to improve the efficiency of the STRAP process. The size of the plastic to be processed is one of the factors that affect the dissolution time. Shredding the plastic into smaller particles helps to reduce the dissolution time of the polymer components. Preferably, the multi-layer plastic film or mixed plastic waste is cut into 1 cm 2 More preferably, the multi-layer plastic film or mixed plastic waste is shredded into strips of ≦5 mm, ≦4 mm, ≦3 mm, or ≦2 mm. In one embodiment, the multi-layer plastic film or mixed plastic waste is shredded into strips of ≦2 mm. At a size of ≦2 mm, the dissolution time of the plastic can be reduced to less than 5 minutes.

[0043] Also disclosed herein are exemplary embodiments of the method, which are applied to recover constituent polymers from various multi-layer plastic films and mixed plastic waste. The exemplary embodiments are described in detail in the Examples. The exemplary embodiments are not intended to limit the scope of the present disclosure.

[0044] 1. A method for recovering constituent polymers in a multi-layer plastic film consisting essentially of PE, EVOH, and PET (see Example 1). The method comprises: (i) selectively dissolving PE in toluene at about 110° C., separating the solubilized PE from the EVOH and PET by mechanical filtration, and precipitating the solubilized PE by adding acetone; and (ii) selectively dissolving the EVOH in DMSO at about 95° C., separating the solubilized EVOH from the PET by mechanical filtration, and precipitating the solubilized EVOH by adding water; Includes.

[0045] 2. A method for recovering constituent polymers in a multi-layer plastic film consisting essentially of PE, EVOH, and PET (see Example 2). The method comprises: (i) selectively dissolving PE in toluene at about 110° C., separating the solubilized PE from the EVOH and PET by mechanical filtration, and precipitating the solubilized PE by reducing the temperature of the toluene to about 35° C.; and (ii) selectively dissolving the EVOH in a solvent comprising DMSO and water at about 95° C., separating the solubilized EVOH from the PET by mechanical filtration, and precipitating the solubilized EVOH by lowering the temperature of the DMSO and water to about 35° C. Includes.

[0046] 3. A method for recovering constituent polymers in a multi-layer plastic film consisting essentially of PE, EVOH, PET, and a tie layer of EVA (see Example 1). The method comprises: (i) selectively dissolving PE and EVA in toluene at about 110° C., separating the solubilized PE and EVA from EVOH and PET by mechanical filtration, and precipitating the solubilized PE and EVA by adding acetone; (ii) selectively dissolving EVA in NMP at about 170° C., separating the solubilized EVA from PE by mechanical filtration, and precipitating the solubilized EVA by adding acetone; and (iii) selectively dissolving the EVOH in DMSO at about 95° C., separating the solubilized EVOH from the PET by mechanical filtration, and precipitating the solubilized EVOH by adding water. Includes.

[0047] 4. A method for recovering constituent polymers in a multi-layer plastic film consisting essentially of PE, EVOH, PET, and a tie layer of EVA (see Example 2). The method comprises: (i) selectively dissolving PE and EVA in toluene at about 110° C., separating the solubilized PE and EVA from the EVOH and PET by mechanical filtration, and precipitating the solubilized PE by reducing the temperature of toluene to about 35° C.; (ii) separating the solubilized EVA from the precipitated PE by mechanical filtration and precipitating the solubilized EVA by adding acetone; and (iii) selectively dissolving the EVOH in a solvent comprising DMSO and water at about 95° C., separating the solubilized EVOH from the PET by mechanical filtration, and precipitating the solubilized EVOH by lowering the temperature of the DMSO and water to about 35° C. Includes.

[0048] 5. A method for recovering constituent polymers in a multi-layer plastic film consisting essentially of PETG, PE, EVOH, and PET (see Example 2). The method comprises: (i) selectively dissolving PETG in a solvent comprising DMF and THF at about 87° C., separating the solubilized PETG from PE, EVOH and PET by mechanical filtration, and precipitating the solubilized PETG by adding 1-propanol; (ii) selectively dissolving the PE in toluene at about 110° C., separating the solubilized PE from the EVOH and PET by mechanical filtration, and precipitating the solubilized PE by reducing the temperature of the toluene to about 35° C.; and (iii) selectively dissolving the EVOH in a solvent comprising DMSO and water at about 95° C., separating the solubilized EVOH from the PET by mechanical filtration, and precipitating the solubilized EVOH by lowering the temperature of the DMSO and water to about 35° C. Includes.

[0049] 6. A method for recovering constituent polymers in a multi-layer plastic film consisting essentially of PE, EVOH, and PET, involving a deinking step (see Example 3). The method comprises: (i) treating the multi-layer plastic film in a solvent comprising THF and DMF at about 83° C. to remove the ink from the multi-layer plastic film; and (ii) recovering the polymer as described in exemplary embodiment 1 or 2. Includes.

[0050] 7. A method for recovering PE and PP from mixed plastic waste consisting essentially of PE, PP, PVC, PET, and PA (see Example 5). The method comprises: (i) selectively dissolving PE in dodecane at about 100° C., separating the solubilized PE from PP, PVC, PET and PA by mechanical filtration, and precipitating the solubilized PE by reducing the temperature of the dodecane to about 35° C.; and (ii) selectively dissolving the PP in toluene at about 110° C., separating the solubilized PP from the PVC, PET and PA by mechanical filtration, and precipitating the solubilized PP by reducing the temperature of the toluene to about 35° C. Includes.

[0051] 8. A method for recovering the constituent polymers of a multi-layer plastic film consisting essentially of PE, EVOH, and nylon (see Example 6). The method comprises: (i) selectively dissolving PE in toluene at about 110° C., separating the solubilized PE from the EVOH and nylon by mechanical filtration, and precipitating the solubilized PE by reducing the temperature of the toluene to about 35° C.; and (ii) selectively dissolving the EVOH in a solvent comprising DMSO and water at about 85° C., separating the solubilized EVOH from the nylon by mechanical filtration, and precipitating the solubilized EVOH by reducing the temperature of the DMSO and water to about 35° C. Includes.

[0052] 9. A method for recovering constituent polymers in mixed plastic waste consisting essentially of PVC, LDPE, PP, HDPE, PET, nylon 6,6,6, nylon 6, nylon 6,6 (see Example 6). The method comprises: (i) selectively dissolving PVC in THF at about 68° C., separating the solubilized PVC from the remaining mixed plastic waste by mechanical filtration, and adding water to precipitate the solubilized polyvinyl chloride; (ii) selectively dissolving the LDPE in toluene at about 85°C, separating the solubilized LDPE from the remaining mixed plastic waste by mechanical filtration, and precipitating the solubilized LDPE by reducing the temperature of the toluene to about 35°C; (iii) selectively dissolving the PP in THP at about 90° C., separating the solubilized PP from the remaining mixed plastic waste by mechanical filtration, and precipitating the solubilized PP by reducing the temperature of the THP to about 35° C.; (iv) selectively dissolving the HDPE in toluene at about 110°C, separating the solubilized HDPE from the remaining mixed plastic waste by mechanical filtration, and precipitating the solubilized HDPE by reducing the temperature of the toluene to about 35°C; (v) selectively dissolving the PET in the GVL at about 160°C, separating the solubilized PET from the remaining mixed plastic waste by mechanical filtration, and precipitating the solubilized PET by reducing the temperature of the GVL to about 35°C; (vi) selectively dissolving the nylon 6,6,6 in 1,2-propanediol at about 135° C., separating the solubilized nylon 6,6,6 from the remaining mixed plastic waste by mechanical filtration, and precipitating the solubilized nylon 6,6,6 by reducing the temperature of the 1,2-propanediol to about 35° C.; (vii) selectively dissolving nylon 6 in DMSO at about 145° C., separating the solubilized nylon 6 from the remaining mixed plastic waste by mechanical filtration, and precipitating the solubilized nylon 6 by reducing the temperature of the DMSO to about 35° C.; and (viii) selectively dissolving the nylon 6,6 in formic acid at about 65° C., separating the solubilized nylon 6,6 from the remaining mixed plastic waste by mechanical filtration, and precipitating the solubilized nylon 6,6 by adding water. Includes.

[0053] While particular embodiments disclosed herein have been shown and described in detail to illustrate the application of the principles described above, it will be understood that the disclosure may be embodied in other manners without departing from such principles. EXAMPLES

[0054] Example 1. Recycling of multi-layer plastic packaging materials by solvent targeted recovery and precipitation In this example, we demonstrate the STRAP process by isolating three representative polymer resins - PE, EVOH, and PET - from an actual post-industrial multilayer film (manufactured by Amcor Flexibles) that consists primarily of these three components. By sequentially solubilizing each component in a solvent system identified by molecular modeling of temperature-dependent polymer solubility, we succeeded in separating these three components with nearly 100% material efficiency and recovering the individual resins in chemically pure form. A detailed techno-economic analysis demonstrated that in a post-industrial operating environment characterized by a minimum volume of 5400 tons per year and a nearly constant film composition, the STRAP process is capable of recycling Amcor multilayer films into their pure corresponding resins at a cost comparable to virgin materials. Thus, the STRAP process is a realistic and near-future approach to design solvent systems for recycling multilayer plastics. See Walker et al.

[33] , published November 20, 2020, which is incorporated herein by reference in its entirety.

[0055] Materials and Methods Materials: Model resins were obtained from vendors and used as received: Soarnol EVOH (Mitsubishi Chemical, 32 mol% ethylene), high density PE (ExxonMobil Chemical; molecular weight 7845.30 Da), Array 9921M PET (DAK Americas). Solvents and anti-solvents were obtained from vendors and used as received: acetone (Fisher Scientific, histology grade), water (Alfa Acer, high performance liquid chromatography grade), toluene (Sigma-Aldrich, >99.5%), DMSO (Sigma-Aldrich, American Chemical Society reagent grade). Model multilayer films were obtained from Amcor Flexibles (commercial film, proprietary formulation).

[0056] ATR-FTIR spectroscopy: ATR-FTIR spectroscopy was performed using a Bruker Optics Vertex system equipped with a diamond germanium ATR single reflection crystal. Samples were dried overnight in a vacuum oven to remove moisture before analysis and pressed uniformly onto the diamond surface using a spring-loaded anvil. Sample spectra were captured using a 2 cm -1 with a spectral resolution of 400 and 4000 cm -1 The images were acquired in triplicate with an average of 128 scans over the range between 0.01 and 0.05. Air was used as background.

[0057] Differential Scanning Calorimetry: The glass transition temperatures of PET and EVOH samples were determined by differential scanning calorimetry using a TA Instruments Q100 calorimeter equipped with a liquid nitrogen cooled refrigeration unit. The temperature ramp was calibrated with an empty pan reference cell. The heating rate was 5 °C min -1 A 20 mg sample was used for each experiment. The glass transition temperature was determined by determining the maximum apparent heat capacity of the sample in the observed temperature range according to standard methods using analysis software provided by TA Instruments.

[0058] Headspace Gas Chromatography-Flame Ionization Detector Testing: 1 g of each sample was sealed in a 20 ml headspace vial. The vials were heated to 130°C for 5 min using a Teledyne Tekmar "Versa" headspace autosampler and sent to an Agilent 7890 GC equipped with an Rtx-1701 column. The resulting peaks were compared to external standards containing 1 mg of each solvent in 1 ml of high boiling glycol ether (where 1 mg corresponds to 100 ppm in 1 g).

[0059] Computer and techno-economic modeling methods: Techno-economic modeling was performed using the Aspen Plus software package. HSP(δ D , δ P , and δ H The values ​​of ) and Ro were taken from [1]. COSMO-RS calculations were performed using COSMOtherm 19 software with the parameterization file BP_TZVPD_FINE_18[2,3]. All density functional theory calculations were performed using TURBOMOLE 7.3 software[4]. All classical MD simulations used to generate polymer conformations in the COSMO-RS calculations were performed using GROMACS 2016[5]. The polymer and solvent molecules were parameterized using Antechamber and the Generalized AMBER force fields[6,7].

[0060] The MSP of recycled polymers obtained from the separation of PE, EVOH, and PET components of Amcor commercial films using the STRAP process was estimated using a process model developed in Aspen Plus (V1 1.0, Aspen Technology). For this purpose, the STRAP process was divided into two sections: (i) the PE separation process section and (ii) the EVOH / PET separation process section. Process models of the polymer dissolution unit (stirred tank), polymer precipitation unit (settler), and solvent / antisolvent separation unit (distillation column) were developed in the Aspen Plus modeling suite, and the corresponding performance indicators were set based on the experimental data reported herein. Process models of feed processing units such as shredders, floating tanks, friction washers, dewaterers, and thermal dryers were adapted and appropriately scaled from previous studies [8].

[0061] result A computational tool used in solvent selection for the STRAP process. We tabulated the HSPs of 22 common industrial solvents from [1] and compared them with the HSPs of PE, EVOH, and PET to determine which solvents were suitable for selective dissolution of each resin among the three physical mixtures (Figure 3B). The HSPs of some of the solvents considered are shown in Table 1. Considering these calculations and the design criteria regarding cost, solvent and antisolvent miscibility, and toxicity limits, we selected toluene / acetone and dimethyl sulfoxide (DMSO) / water mixtures as the solvent / antisolvent systems to selectively dissolve / recover PE and EVOH resins, respectively. The HSP analysis predicted that PET would not dissolve readily in any of the solvents.

[0062] [Table 1]

[0063] Next, we performed COSMO-RS calculations to estimate process conditions (temperature and specific mixture composition) for efficient material recovery. We performed classical MD simulations of single oligomers in solution to consider various polymer configurations. The lowest energy configurations were input into COSMO-RS to calculate the solubility of the three polymers in the same 22 solvents for which the HSP was calculated. The good solvents identified by COSMO-RS (solvents with high polymer solubility) overlapped closely with the solvents selected based on HSP, indicating that both methods select similar solvents. Toluene and DMSO were ranked as top candidate solvents for selectively dissolving PE and EVOH, respectively, based on both methods. Both methods indicate that tetrahydrofuran (THF) may selectively dissolve PET, but the COSMO-RS calculations suggested that its solubility at room temperature was still low.

[0064] Next, we calculated the solubilities of all three polymers in toluene and DMSO at temperatures from room temperature to the boiling point of each solvent to determine the temperature required to promote the desired separation (Figure 3C). In toluene, the solubility of PE increases more rapidly with temperature than PET and EVOH, and the solubilities of PET and EVOH never exceed a few weight percent in the temperature range examined. Therefore, we chose the boiling point of toluene (110 °C) for the separation of PE. In DMSO, the solubility of EVOH is much higher than that of PET and PE, but the solubility of PE begins to increase around 100 °C. Therefore, we decided to separate EVOH at 95 °C in DMSO. Finally, we calculated the solubilities of PE in toluene-acetone mixed solvents and EVOH in DMSO-water mixed solvents by varying the mass ratio of solvent to antisolvent (Figure 3D). Both solubilities decreased as the proportion of antisolvent increased. We used a DMSO:water mass ratio of 1:4, which is close to the lowest mass ratio we have calculated.

[0065] Table 1 shows the normalized HSP interaction radius (R a / Ro ), COSMORS predicted solubilities, and experimentally determined solubility limits are shown. As expected, the highest experimentally determined solubilities were obtained for the solvent systems selected from the simulations, and the discrepancy between the predicted and experimental solubilities is attributed to the uncertainty in the crystallinity of the polymer samples. The results in Table 1, taken together with Figures 3A-3D, demonstrate the feasibility of three steps for separating a mixture consisting of PE, EVOH, and PET into pure resins: 1) selectively dissolving the PE fraction in toluene at 110° C., followed by separation of the solubilized fraction from the EVOH and PET by mechanical filtration; 2) selectively dissolving the EVOH fraction in DMSO at 95° C., followed by separating the solubilized fraction from the remaining PET by mechanical filtration; and 3) It is the basis of a process consisting of recovering the solubilized PE and EVOH fractions by lowering the temperature of the corresponding solution to 25 °C and adding 4 parts by weight of acetone or water, respectively, to precipitate the polymer resin as a solid (Figure 4A). The recovered PE and EVOH are separated from the toluene-acetone or DMSO-water mixture by filtration. The solvents used in this process can then be separated by distillation and reused.

[0066] STRAP process used to separate PE, EVOH and PET To demonstrate the STRAP process using the protocol above, we first attempted separation of a physical mixture of resin beads consisting of a 7:2:2 ratio by weight of PET:EVOH:PE. As shown in Figure 4B, nearly quantitative yields of the original polymers were recovered (98.5 wt% recovery of PE, 95.7 wt% recovery of EVOH, and 100.7 wt% recovery of PET). The solid fractions isolated from this process were essentially pure in the individual PE, EVOH, or PET components as represented by Fourier transform infrared (FTIR) spectra (Figure 5).

[0067] Next, we attempted to decompose an actual post-industrial rigid multi-layer film manufactured by Amcor Flexibles. This multi-layer film is composed of PET as the main component, PE and EVOH. This film was cut into 1×1 cm 2 The resin was cut into strips and stirred in a solvent system consisting of toluene at 110 °C, followed by DMSO at 95 °C, with a solid-liquid ratio of 1:4 by mass, respectively. After vacuum filtration at 95 °C, the filtered solution was combined with a room temperature antisolvent consisting of 4% acetone or water by mass relative to toluene or DMSO, and the resulting mixture was cooled to room temperature before filtering off the precipitated solid. All three solid fractions obtained were washed with water and dried overnight at 85 °C in a vacuum oven to remove residual solvent. Near quantitative recovery of pure resin was achieved, with an overall mass balance of 100.4 wt % and an SE of ±1.39 wt % between three replicate experiments (Figure 4C).

[0068] Characterization of solids from the STRAP process. Figure 5 shows the attenuated total reflectance (ATR)-FTIR spectra corresponding to representative solid materials recovered from the above-mentioned experiments. As represented by their ATR-FTIR spectra, the PET, EVOH, and PE recovered from the physical mixtures are indistinguishable from the same corresponding virgin resins. These results demonstrate that the STRAP process is capable of separating physical mixtures of PET, EVOH, and PE into three solid fractions that are essentially pure in their individual resin components. Similarly, the virgin PET and the PET-rich solids recovered from the Amcor multilayer film were indistinguishable from each other, indicating complete separation of the PET from the multilayer film. Similar results were obtained for the EVOH fraction recovered from the multilayer film.

[0069] The toluene solubles recovered from Amcor's multilayer film contained primarily PE with some EVA impurity (Figure 5). The presence of this EVA component (copolymer tie layer) was not known a priori, and its removal is not necessary to recycle PE in Amcor's equipment. Nevertheless, a third solvent-mediated separation step was performed to complete the separation of these two components by dissolving the EVA component in N-methylpyrrolidone (NMP), in which PE is immiscible. The resulting solids (Figure 6) showed a noticeable reduction in EVA contamination, as represented by the reduction of the corresponding spectral features in the FTIR signature.

[0070] Having demonstrated nearly complete separation of the three polymeric components representative of a multilayer film, we tested the physical properties of the recovered solids and evaluated their suitability for reuse in standard industrial processing equipment such as a blown film extruder. The glass transition temperatures (T g ) are shown in Table 2. g These tests were not performed in this example because they are difficult to measure. The Tg of the EVOH fraction recovered from the physical mixture and the actual multilayer film was unchanged from the virgin resin and similar to literature values ​​[9-11]. The Tg of the PE recovered from the multilayer film was slightly lower than that of the PE recovered from the physical mixture. However, the Tg of the PET fraction recovered from the physical mixture was unchanged compared to the virgin resin and similar to reported values ​​[12, 13]. These results suggest that the Tg of PET is slightly modified during the process used to make the multilayer film, but not during the STRAP process. We believe that under the conditions studied in this example, the average molecular weights of the PE, EVOH, and PET resins do not change during the dissolution / recrystallization process. Although not performed in this example, this behavior can be confirmed by gel permeation chromatography coupled with multi-angle laser light scattering.

[0071] [Table 2]

[0072] Finally, headspace gas chromatography-flame ionization detector testing was performed to determine the presence of entrained solvents in the recovered polymer fractions (Table 3). The results showed that for all materials shown in Table 1, less than 1000 parts per million (ppm) of residual solvent was present in the recovered resin. These levels of solvent retention make the recovered polymers suitable for use in most multilayer films, as long as the solvent does not impair the mechanical properties of the final reconstituted product.

[0073] [Table 3]

[0074] Although a detailed analysis is beyond the scope of this Example, additional concerns in this context include how the toxicity, odor, or other properties of the retained solvent affect the suitability of the recovered polymer for applications such as food packaging. A number of solutions are possible on a case-by-case basis to address such issues. For example, if solvent retention is an issue in a food packaging application, the recycled resin could be used to produce a multi-layer film (i.e., an inner layer of the film) in which the recycled fraction does not come into contact with the food. However, for any application, the viability of the STRAP process ultimately depends on the ability to produce recycled resin suitable for use while efficiently recovering and reusing the solvent so that the production of recycled polymer resin is cost-competitive with the production of virgin material.

[0075] Techno-economic analysis of the STRAP process. Following the requirement that recycled polymers must be produced at costs comparable to the prices of the corresponding virgin resins, we performed a techno-economic analysis of the STRAP process based on the experimental data reported here. Figure 7 shows the total capital investments and the minimum selling prices (MSPs) of the recycled polymer components as a function of supply capacity.

[0076] Our calculations suggest that the STRAP process can separate Amcor commercial film at an MSP of $1.19 / kg of combined recycled resins for a 3000 ton / year feed rate of Amcor commercial film. If the feed rate increases to 15,000 ton / year, the MSP decreases to $0.6 / kg. The distillation column and heat required to separate the solvent and antisolvent are the primary cost drivers of the process, accounting for 33.6% of the total capital investment and 79.3% of the variable operating costs, respectively. At a feed rate of 3800 ton / year, less than half the throughput at APK's Newcycling plant in Germany

[14] , the MSP of the recovered polymer is comparable to the average market price for virgin PET ($1.1 / kg)[15,16]. It should be noted that Amcor commercial film is composed of 90.2 wt% PET.

[0077] The energy required for the separation of the multi-layer film is 79.13 MJ / kg, approximately 37% less than the energy required for the production of virgin PET resin (125 MJ / kg). For comparison, the energy generated from the incineration of waste plastics (the most realistic non-landfill disposal of plastic film today) is 6.09 MJ / kg of multi-layer film [17, 18], but incineration emits 950 kg of CO2 per tonne of plastic waste

[19] . These analyses, together with examples of comparable solvent-based technologies [14, 20-22], show that the STRAP process can be deployed at a large scale to fully recycle realistic waste streams generated from multi-layer plastic film plants.

[0078] Consideration The method described here has been demonstrated to be capable of completely degrading multi-layer plastic waste of realistic complexity. Although we have not performed a detailed analysis of the dilute but non-zero levels of tie layers (e.g., EVA; Figure 6), wet-bond adhesives, and other additives present in realistic multi-layer films, we believe that these layers are chemically compatible and therefore can be recycled together with the main resin fraction. However, highly cross-linked polymers (e.g., cross-linked polybutadiene) may not be readily soluble in any available solvent and may be impossible to completely separate from the desired resin. As mentioned above, the impact of these impurities, as well as entrained solvents (Table 3), on the suitability of the recovered polymer for use will depend on the application of the final reconstituted multi-layer film, and a detailed analysis of these impurities is necessary to fully de-risk the STRAP process in a given operating environment.

[0079] In conclusion, we have demonstrated that the STRAP process can efficiently degrade commercial PIW films into their three constituent resins with near 100% yield. The process uses successive solubilization steps in solvents selected based on computer modeling of the polymer solubility. We propose that the STRAP process can be rapidly implemented at large scale to target post-industrial multi-layer plastic waste streams because they originate from point sources (manufacturing plants), have known and nearly constant composition, and are substantially large volumes (~100 billion pounds per year globally). These characteristics allow for the treatment and recycling of large volumes of post-industrial multi-layer plastic waste using existing equipment in combination with the STRAP technology. A detailed economic analysis of the STRAP process assuming an annual feed rate of 3800 tons shows that the STRAP process can completely degrade multi-layer plastic waste streams consisting of PE, EVOH, and PET into their corresponding resins at a cost comparable to the corresponding virgin resins.

[0080] Our rigorous molecular modeling framework, leveraging a fundamental understanding of the thermodynamics of polymer-solvent interactions, is broadly applicable and will enable the rational design of new solvent systems to process complex multilayer plastics of almost any composition in the future. As the compositions of multilayer films are constantly being redesigned to meet changing needs, requiring flexible technologies to successfully recycle them, this rapidly adaptable aspect of the STRAP process represents an important advancement for addressing the problem of complex plastic waste accumulating in the environment. Finally, because the STRAP process is based on simple unit operations such as stirred tanks, filters, and distillation columns, it can be considered a platform technology that can mitigate risks in well-defined post-industrial operating environments and can be adapted to post-consumer waste treatment to treat more complex post-consumer waste streams. Taken together, these features make the STRAP process a promising strategy for the near-term reduction of post-industrial and post-consumer plastic waste, as well as for addressing the ongoing environmental crisis associated with the infiltration of these wastes into human and animal habitats at all scales.

[0081] Example 2: Reducing anti-solvent usage in the STRAP process by enabling temperature-controlled polymer dissolution and precipitation for recycling of multi-layer plastic films The objective of this example is to identify operating conditions that reduce the amount of antisolvent used in the STRAP process and to demonstrate how STRAP can be applied to a more complex industrial multilayer film (provided by Amcor). We combine thermodynamic computational tools, polymer characterization methods, and modern process design tools to develop a realistic near-term approach to design solvent systems for recycling multilayer plastics. To utilize these solvents efficiently, processes are required that allow the solvent to be recovered and reused while minimizing the amount of solvent left as waste. Approaches to reduce antisolvent use include the use of solvents or solvent mixtures that allow for temperature-controlled dissolution and precipitation of the target polymer in the multilayer film. The use of solvent combinations has been explored as an option in the dissolution / precipitation process for certain polymers. In some trials, the solvent mixture is used only to dissolve the target plastic, and the antisolvent is added later for precipitation. Hadi et al. studied a method to dissolve polyolefins using a turpentine / petroleum ether (PetE) mixture, followed by precipitation using n-hexane and PetE

[23] . Weeden et al. used a heptane / dichloromethane mixed solvent to dissolve e-waste components

[24] ; however, they recovered the polymer by evaporating the solvent. Pure solvents or combinations of solvents have also been used to dissolve different polymers at different temperatures, reducing the number of solvents required to recover each polymer. Some patents disclosing this technique rely on evaporating the solvent to obtain the final solid polymer [25, 26]. A method to precipitate the polymer by changing the temperature of the solvent instead of evaporating the solvent or adding an antisolvent may make the dissolution / precipitation method more feasible

[27] .

[0082] In this example, we evaluate and compare the STRAP technique using two different polymer precipitation techniques: precipitation by addition of antisolvent (STRAP-A) and precipitation by reduction of solvent temperature (STRAP-B). Two post-industrial rigid multilayer films (A1 and A2) from Amcor were used to demonstrate the STRAP process. Multilayer film A1 was composed of PE, EVOH, and PET with a small amount of EVA. Film A2 was the same polymer with the addition of glycol-modified polyethylene terephthalate (PETG). Thermodynamic tools were used for the selection of the solvent, and experimental results were used in a process model that allowed for the estimation of process costs. See Sanchez-Rivera et al.

[44] , published August 10, 2021, which is incorporated herein by reference.

[0083] Materials and Methods Computational modeling for solvent screening: We computationally assessed the solubility of polymers to guide solvent selection for the STRAP process. Our approach used a combination of HSP, MD simulations, and COSMO-RS, following Example 1. In this example, HSP was taken from the HSP Handbook

[28] and was used for preliminary solvent selection, even though it does not provide a quantitative prediction of solubility.

[0084] MD simulations and COSMO-RS are used for further quantitative solubility predictions utilizing an updated protocol compared to Example 1. Atomistic MD simulations of the oligomers were performed to obtain the input structures for COSMO-RS. MD simulations were first performed in an isothermal-isobaric ensemble for a single oligomer in dilute solution. Each MD simulation contained one oligomer molecule (EVOH or PETG) and 216 solvent molecules. EVOH was simulated in water, and PETG in toluene. The EVOH oligomer molecule contained four vinyl alcohol repeat units and two ethylene repeat units. The PETG oligomer contained four ethylene glycol repeat units and two 1,4-cyclohexanedimethanol repeat units. The radius of gyration (Rg) and solvent accessible surface area (SASA) of the oligomers were then calculated as a function of simulation time from the MD trajectories to characterize the distribution of conformations of the oligomers. Representative oligomer conformations spanning the Rg-SASA space were extracted from the MD trajectories and used as input for the COSMO-RS workflow detailed below. A total of 22 conformers were extracted from the EVOH trajectory and 18 from the PETG trajectory. MD simulations were performed using GROMACS 2016 [5]. All compounds were parameterized using Antechamber and the Generalized AMBER force fields [6,7].

[0085] COSMO-RS predicts the equilibrium properties of multicomponent systems based on quantum mechanical calculations and statistical thermodynamic methods

[29] . COSMO-RS represents each molecule based on the screening charge density that arises on the molecular surface due to the polarization of the medium. The screening charge density is obtained from density functional theory (DFT) calculations and is histogrammed to generate a σ-profile. We approximated the σ-profile of a polymer by generating σ-profiles for oligomer structures with deactivated end groups

[30] . The screening charge density and the resulting σ-profile depend on the specific molecular conformation; consequently, we generated a set of oligomer conformations using MD (described above) to span the range of possible σ-profiles. Figure 8 shows an example of two conformers of a different oligomer and the results of DFT calculations of their screening charge distributions. The chemical potential of the polymer is calculated based on the σ-profile, and the solubility of the polymer can be predicted by solid-liquid equilibrium calculations. DFT calculations of the screening charge distribution were performed using Gaussian 16 at the BVP86 / TZVP / DGA1 level of theory

[31] . COSMO-RS solubility calculations were performed with COSMOtherm 19 using BP_TZVP_19 as a parameter [29,32].

[0086] Experimental procedure with multilayer Al: The primary objective of the STRAP process is to separate the constituent polymers in a multilayer plastic film using a series of solvent washes. To develop and demonstrate the experimental procedure, a model film manufactured by Amcor was used. The plastic film was an Al film with a base of PE, PET, EVA, and EVOH. Prior to a typical STRAP experiment, the multilayer film was washed with 1 × 1 cm 2The multilayer film pieces were cut into strips of 1000 μm. A 250 mL round-bottom flask connected to a reflux condenser with a cold water supply line was used. The round-bottom flask containing the corresponding solvent and a 40 g batch of multilayer film pieces was partially immersed in a 1500 mL dish containing silicone oil as a heat transfer fluid. The system was heated to the desired dissolution temperature with an electric heat plate equipped with a magnetic stirring drive, and the stirring speed was adjusted to provide constant mixing. Based on the computational analysis for the solvent selection, we experimentally evaluated the recovery of each polymer in the multilayer film Al by performing three processing steps: (1) selectively dissolving the PE fraction in toluene at 110 °C for 4 h, then separating the solubilized fraction from the EVOH and PET by mechanical filtration; (2) selectively dissolving the EVOH fraction in DMSO at 95 °C for 30 min, then separating the solubilized fraction from the remaining PET by mechanical filtration; (3) precipitating the solubilized PE and EVOH fractions by adding acetone or water, respectively. The precipitated PE and EVOH were then separated from the toluene-acetone and DMSO-water mixtures by filtration. The resulting solid fraction was dried overnight at 65 °C in a vacuum oven to remove residual solvent. This method was identified as STRAP-A and requires the addition of an anti-solvent to precipitate the desired polymer.

[0087] Another method to precipitate the dissolved polymer was explored. It consisted of lowering the temperature of the solvent and dissolved polymer to 35 °C. In this method, named STRAP-B, a solvent mixture was explored to dissolve the target polymer at a higher temperature and to precipitate the polymer at a lower temperature, reducing the need to add a large amount of antisolvent after dissolution to precipitate the polymer. Toluene-acetone and DMSO-water mixtures were tested for the recovery of PE and EVOH, respectively.

[0088] Experimental procedure with multilayer film A2: The same experimental setup was used for multilayer film A2, which consisted of PETG, PE, EVOH, PET, and EVA. As with Al, the multilayer film was cut into 1 × 1 cm 2The inventors experimentally evaluated the recovery rate of each polymer in the multilayer film A2 by carrying out four processing steps: (1) selectively dissolving the PETG fraction in a mixed solvent of 60% DMF-40% THF (v / v) at 87°C for 4 hours, then separating the solubilized fraction from PE, EVOH, PET, and EVA by mechanical filtration; (2) selectively dissolving the PE and EVA fractions in toluene at 110°C for 2 hours, then separating the solubilized fraction from EVOH and PET by mechanical filtration; (3) dissolving the EVOH fraction in a mixed solvent of 60% DMSO-40% water (v / v) at 95°C for 30 minutes, then separating the solubilized fraction from the remaining PET by mechanical filtration; (4) precipitating the solubilized PETG by adding 1-propanol as an antisolvent, and precipitating the PE and EVOH fractions by lowering the temperature of the solvent containing the dissolved polymers to 35°C. The precipitated PETG, PE, and EVOH solids were then separated from the corresponding solvents by filtration. EVA was recovered by adding acetone as an antisolvent to toluene after removing the PE solids. The five resulting solid fractions were dried overnight at 65°C in a vacuum oven to remove residual solvent. The process with multilayer film A2 was named STRAP-C.

[0089] Characterization of solids from the STRAP process: ATR-FTIR spectroscopy was used to characterize the polymer fractions isolated from the STRAP process and compare the spectra with virgin resin. The instrument was a Bruker Vertex 70 equipped with a liquid nitrogen cooled mercury-cadmium-telluride (MCT) detector. The ATR cell used was a MIRacle single reflection cell equipped with a diamond crystal (Pike Technologies). A typical measurement averaged 128 scans with a resolution of 4 cm. -1 , measuring range is 4000~400cm -1 It was.

[0090] Results and Discussion STRAP-A using multilayer Al The STRAP-A process was carried out in the same manner as in Example 1 and was used as a benchmark for comparison with the alternative processes in this example. Table 4 shows that for the recovery of PE, PET, and EVOH from multilayer film Al, the overall average mass balance was 102.58 wt% with a standard deviation of ±0.96 wt%. The overall mass balance was greater than 100 wt% due to solvent entrapment. Drying conditions need to be adjusted to minimize entrained solvent. The values ​​reported in Table 4 are consistent with Example 1. Figure 9 shows the solvent, antisolvent, temperature, and dissolution time used in each process step of STRAP-A. Acetone and water were used as antisolvents for PE and EVOH precipitation, respectively.

[0091] [Table 4]

[0092] The use of large amounts of poor solvents is of concern at large scale, as it can lead to high costs and environmental and safety risks. The energy required to separate each solvent and antisolvent used in STRAP-A was found to account for 33.6% of the total capital costs and 79.3% of the total operating costs

[33] . The distillation column in STRAP-A was the main cost driver of the process. An alternative to using an antisolvent to precipitate the polymer is to cool the solvent containing the dissolved polymer to induce precipitation. To this end, a mixed solvent was considered that dissolves the desired polymer at high temperatures and readily precipitates the polymer when the temperature is reduced. In this way, we can have a constant solvent composition throughout the process to target specific polymer components in the multilayer film. Thermodynamic and computational tools allowed us to rapidly screen potential solvent compositions for recovering EVOH and PE using this approach.

[0093] Computer modeling results COSMO-RS predictions were used to identify potential solvent compositions for EVOH recovery, leveraging the method's ability to capture temperature-dependent solubility. Figure 10 shows the COSMO-RS predictions of EVOH solubility as a function of temperature and DMSO-water composition. For comparison, the predicted EVOH solubility in pure DMSO at 95 °C is 22.77 wt%, which is similar to the experimentally measured solubility of 24.02 wt%. This comparison supports the validity of COSMO-RS to predict EVOH solubility. In the STRAP-A process, EVOH is dissolved in pure DMSO at 95 °C. Water is then added as an anti-solvent to reduce the solubility of EVOH and induce precipitation, ultimately achieving a 20% DMSO-80% water (v / v) mixture at low temperature. These steps are indicated by the labeled white arrows in Figure 10. This first process exploits the large solubility difference between the two states (predicted by COSMO-RS and measured experimentally) to achieve high EVOH recovery.

[0094] Figure 10 shows that the STRAP-B process can achieve the same solubility reduction to precipitate the polymer by lowering the temperature without changing the solvent composition. COSMO-RS solubility calculations indicate that EVOH recovery should be possible in pure DMSO, which is consistent with pure DMSO being unable to dissolve EVOH at room temperature. However, experiments showed low EVOH recovery upon cooling. Therefore, different mixture compositions were tested. A 60% DMSO-40% water mixture (v / v) was selected for EVOH recovery, as it was predicted to show satisfactory solubility at 95 °C (10.45 wt%) and low solubility at 35 °C (1.72 wt%). The latter value is comparable to the EVOH solubility predicted for the final step of the STRAP-A process. Experimental values ​​showed a solubility of 7.17 wt% at 95 °C and 0.01 wt% at 35 °C, leading to high EVOH recovery. We find that COSMO-RS over-predicts the experimental solubilities, but gets the general trends right.

[0095] Similar COSMO-RS solubility predictions were calculated for PE in various toluene-acetone mixtures to see if there were suitable mixtures for recovery. The experimental solubility of PE in pure toluene (14.56 wt% at 110 °C) was used as a reference input for the COSMO-RS calculations. The calculated solubility of PE in 90% toluene-10% acetone (v / v) was 0.02 wt% at 55 °C. This result suggests that the addition of a small amount of acetone to toluene makes PE insoluble in the mixture even at high temperatures; similar results were obtained with other volume fractions of acetone. This low solubility was also confirmed experimentally, where none of the toluene-acetone mixtures tested were able to dissolve PE. Therefore, pure toluene was still used to ensure initial PE dissolution. Pure toluene was able to cause PE precipitation with decreasing temperature.

[0096] STRAP-B using multi-layered Al film Using the thermodynamic insights from the previous section, the STRAP-B process was completed using a solvent composition that allows for temperature-induced precipitation of EVOH and PE polymers. Table 5 shows that similar polymer yields as STRAP-A were obtained for PE, EVOH, and PET in STRAP-B, demonstrating that temperature-controlled dissolution and precipitation for polymer recovery is a promising approach that could reduce costs and make solvent-based recycling processes more attractive.

[0097] [Table 5]

[0098] One of the major differences between the STRAP processes was the PE yield achieved. The PE yield was higher in STRAP-A, which used acetone as an antisolvent to precipitate the polymer. This difference in yield is due to the presence of ethylene vinyl acetate (EVA), a minor component of the multilayer film Al; EVA is soluble in toluene and precipitates with PE when acetone is added. An N-methylpyrrolidinone (NMP) step was previously explored to remove EVA from PE, but we found that this separation could be easily accomplished by lowering the temperature of the toluene to precipitate the PE, since the EVA still remains in the solvent. The EVA can then be precipitated by adding acetone as an antisolvent. Figure 11 shows the solvents, temperatures, and dissolution times used in each process step of STRAP-B.

[0099] ATR-FTIR characterization of polymers recovered by STRAP-A and STRAP-B The Fourier transform (FT) IR spectral results of Example 1 showed that PE, EVOH, and PET recovered from a physical mixture of these components and from multilayer film A1 using the STRAP-A process were indistinguishable from the corresponding virgin resins. The FTIR spectra of PE, EVOH, and PET recovered by STRAP-A and STRAP-B were similar for the most part, indicating that pure polymers were obtained using either precipitation method after selective dissolution (Figures 12A-12C). The polymer recovered by STRAP-A contained peaks at 1736, 1240, 1097, and 1018 cm. -1In the spectrum of PE recovered from STRAP-B, the EVA peaks were observed to be less prominent, confirming that the EVA polymer could be separated from the PE by this process. To further remove the EVA from the solvent, acetone had to be added as an anti-solvent. When the solid recovered from this additional step was characterized, the spectrum showed mainly EVA peaks (Figure 13, panel (b)). For PET recovered from STRAP-A and B, the EVA peaks were less prominent at 3000 cm -1 A low intensity peak was observed near the PE residue in the PET (Figure 12C). The purification of PET may be improved by changing the amount of solvent or dissolving time of other polymers. Quantitative measurement of the amount of PE in PET can help determine whether PE is significant enough to affect the properties of PET.

[0100] STRAP-C using multi-layer film A2 Solvent screening of the PETG component in multilayer film A2: The A2 multilayer film from Amcor was used to demonstrate the STRAP process for a more complex feed composition. This film contained PETG as an additional polymer component. When the same STRAP process developed for film Al was applied to film A2, both PETG and PE were dissolved in toluene. We therefore used a computational approach to identify alternative solvents that could dissolve PETG in order to develop a new STRAP process (called STRAP-C). We first obtained the HSPs of 850 solvents and then calculated the distance (R) of the HSP of PETG in the HSP space of each solvent. a ) was calculated. And each R a The value of was normalized by the radius of the solubility sphere of PETG (R0). a Only solvents with a value of / R0 less than 1 are expected to dissolve PETG. Table 6 shows the HSP values ​​of some common and readily available solvents. Toluene, cyclohexanone, 1,4-dioxane, and triethylamine have R aThe R values ​​are less than 0.7 and are considered to be good candidates. On the other hand, THF, 1,1-dichloroethane and ethyl acetate are R a The R0 values ​​are between 0.9 and 1, indicating a high probability of solubility. DMF and ethanol have R0 values ​​greater than 2. a A2 is identified as a poor solvent with a molar ratio of EG / CHDM. However, PETG is a copolymer commonly synthesized from terephthalic acid (TPA), ethylene glycol (EG), and 1,4-cyclohexanedimethanol (CHDM), and the ratio of EG / CHDM influences its properties

[34] . Unfortunately, the available HSP values ​​for PETG do not provide any information about its composition

[28] ; therefore, we also performed COSMO-RS solubility calculations that consider both the structure and composition of this copolymer to identify solvents that can dissolve PETG. In this case, PETG was modeled as a random copolymer with a molar ratio of EG / CHDM of 2:1 based on the known information about the PETG components in film A2. Table 6 shows that for toluene, cyclohexanone, 1,4-dioxane, THF, and ethanol, the HSP and COSMO-RS results are in agreement with each other; these solvents have high COSMO-RS predicted solubility and low R a The results show that the PETG solubility is excellent with a 0.01% / R0 value. However, the COSMO-RS results also identify DMF as a potential good solvent. From these results, toluene, cyclohexanone, dioxane, DMF, and THF are all potentially suitable solvents for dissolving PETG. Toluene was excluded as a possible solvent for PETG because it also dissolves PE. We also excluded dioxane because it may be a health hazard, and cyclohexanone because the ketone may be unstable. Thus, we selected THF and DMF as possible solvents for further experimental investigation.

[0101] [Table 6]

[0102] After solvent selection for the PETG component, the STRAP-C process was experimentally applied to the A2 multilayer film. Dissolution of PETG was performed with THF for 4 hours at 65 °C before any other polymer components. It was difficult to completely separate PETG from the film using THF, and some polymer remained after the end of the dissolution time. This was not improved by different polymer / solvent ratios or longer dissolution times. This poor separation efficiency is probably due to the glueing of the film strips by the presence of THF. This behavior was not observed when DMF was used for PETG separation. DMF also dissolves the EVOH component, so THF was used as a poor solvent for EVOH (R a With a solubility of 1.34 and a COSMO-RS predicted solubility of 1.78 wt%, various THF / DMF mixtures were experimentally tested. A 40% THF-60% DMF (v / v) mixed solvent was confirmed to selectively dissolve PETG and not EVOH. When this mixed solvent was used for an actual film, the PETG yield was improved from 15.28 to 20.83 wt%. 1-propanol was selected as the anti-solvent for precipitating PETG because of its low solubility in PETG and the ease of solvent recycling after PETG recovery. In the future, it is also possible to explore the solvent composition for dissolving the PETG components and precipitating the PETG components without the addition of an anti-solvent. The results of STRAP-C are shown in Table 7. For the remaining polymer components (PE, EVOH, PET, and EVA), the process of STRAP-B was used, as shown in Figure 14.

[0103] [Table 7]

[0104] ATR-FTIR characterization of polymers recovered by STRAP-C The FTIR spectra of PETG, EVOH, EVA, and PET recovered using STRAP-C were nearly identical to the corresponding virgin resins (Figures 15A-15E). The spectrum of PE contained peaks at 1740, 1370, 1240, and 1020 cm.-1 Some notable differences were observed, such as additional peaks near . These may be due to remnants of PETG that were not separated in the initial dissolution step. Quantitative measurements are needed to determine if the amount of PETG in PE affects its properties. Further adjustments to the dissolution time and solvent volume can improve the purity of PE and remove more PETG.

[0105] Techno-economic analysis A techno-economic analysis (TEA) was performed to determine whether it was possible to produce recycled polymers at prices comparable to virgin resins using any of the STRAP processes examined. Minimum selling prices (MSP) for recycled resins were calculated for a process operating continuously for 20 years with a discount rate of 10% and free input flow of multilayer film (using discounted cash flow analysis). We developed a STRAP process model in Aspen Plus (V11 Aspen Technology) based on our reported experimental mass balances. We estimated the size and cost of equipment required for three different STRAP processes using multilayer films Al and A2. Equipment purchase prices and variable operating costs for distillation columns, pumps, and heat exchangers were estimated using Aspen Process Economic Analyzer (V11 Aspen Technology), and other equipment prices were estimated using engineering methods such as proportional equations and power laws based on cost data from our previous work

[33] .

[0106] We calculated the MSPs of the STRAP-A, STRAP-B, and STRAP-C processes based on the material balance and economic parameters shown in

[44] . The total capital investment (in millions of dollars) was $25.65 for STRAP-A, $22.42 for STRAP-B, and $31.78 for STRAP-C. The MSPs of the STRAP-A and STRAP-B processes using multi-layered Al were calculated to be $2.05 kg 1 and $1.62 kg 1, respectively, at a feed rate of 3000 tonnes per year, as shown in Figure 16. According to our calculations, the MSP of the STRAP-B process was 21.0% lower than that of the STRAP-A process. This is because STRAP-B produced similar polymer yields to STRAP-A, but did not separate the solvent and antisolvent by distillation. Even with the addition of an EVA recovery step in STRAP-B, the MSP is still lower than that of STRAP-A. In addition, the MSP of STRAP-A is higher than that of the previously reported STRAP process

[33] because the STRAP process proposed in this study includes an extruder for each recycled polymer, which accounts for 55.22% of the total equipment purchase cost of STRAP-A.

[0107] The STRAP-C process was estimated to have an MSP of $2.18 kg 1 at a 3000 ton / year feed rate using multilayer film A2. The higher MSP is explained by the fact that STRAP-C recovers an additional polymer, PETG, and that DMF / THF and 1-propanol are used as solvent / antisolvent pairs, requiring a distillation step to recover and recycle the solvent. In general, the selection and minimization of usage of low boiling point solvents can reduce the energy costs of the required distillation column. As a result, STRAP-C can be operated with lower variable operating costs, despite requiring higher capital investments.

[0108] In addition, to evaluate the effect of economies of scale, a sensitivity analysis of the supply volume of the STRAP-B and STRAP-C processes was performed. The results showed that, as shown in Figure 17, the MSP begins to plateau while the capital investment increases between 1,000 and 30,000 tons per year of supply. The MSP of the STRAP-C process is lower than that of the STRAP-A process as the supply capacity increases, especially after about 7,000 tons per year of supply

[33] . This is because, at 3,000 tons per year, the annual capital investment of the STRAP-C process is 62.58% of the total required cost, while the annual capital investment of the STRAP-A process is 53.81% of the total required cost. For example, at 7,000 tons per year of supply, the MSP of the STRAP-A and STRAP-C processes is $1.43 kg 1 and $1.40 kg 1, respectively. As scale increases, especially above 15,000 tonnes per year, the MSPs of the recycled polymers (STRAP-A: $1.07 kg 1, STRAP-B: $0.78 kg 1, and STRAP-C: $0.95 kg 1) are comparable to the average market price of virgin resins (around $0.9–$1.2 kg 1) [20, 42, 43]. These calculations indicate that the STRAP process can be implemented on a large scale to recover and recycle components of a variety of post-industrial multilayer films.

[0109] Economic analysis of recycled polymer from the STRAP-C process was carried out varying the polymer selling price from 0.8 to $3.0 kg 1 for three different supply capacities as shown in Figure 18. As expected, the internal rate of return (IRR) of the STRAP-C process increased with increasing selling price. For a polymer selling price of $3.0 kg 1, the IRR of the STRAP-C process is estimated to be 16.63, 32.51, and 40.99% for 3000, 9000, and 15000 tons per year, respectively. It shows that the economic feasibility of the STRAP process improves with increasing supply capacity due to the effect of economies of scale. Furthermore, to investigate the parameters that affect the economics of the STRAP-C process, we conducted a sensitivity analysis varying the selected parameters by ±30% (Figure 19). The MSP of STRAP-C is sensitive to the extruder equipment cost and project life. This is because the cost structure of the STRAP process is dominated by capital investment. It was also observed that the amount of solvent relative to the polymer affects the MSP, as the amount of solvent affects the size of the equipment. Overall, the TEA results for STRAP-B and STRAP-C indicate that the STRAP process is economically viable, even with increasing plastic feed complexity. The use of solvents that allow for temperature-controlled dissolution and precipitation can significantly reduce capital costs by reducing the number of separation units required for solvent recovery.

[0110] conclusion In this example, we demonstrate the Solvent Targeted Recovery and Precipitation (STRAP) technique to separate and recover constituent polymers in two rigid post-industrial multilayer plastic films manufactured by Amcor. Thermodynamic computational techniques allow for early prediction of polymer solubility in different solvents and solvent mixtures, reducing the number of experiments required. The main cost driver in the STRAP process was already found to be the distillation step required for recycling the solvent and antisolvent. We show in this example that reducing the use of antisolvents and replacing them with solvents and solvent mixtures that allow temperature control of polymer dissolution and precipitation can increase the economic competitiveness of STRAP. This was observed in our STRAP-B process, which showed similar yields and was more efficient in separating polymers than STRAP-A, while using a smaller amount of antisolvent. In addition to this, we demonstrated that the STRAP process can remain economically competitive even if the plastic supply becomes more complex, as demonstrated in STRAP-C with multilayer film A2. Solvent mixtures are crucial in solvent-based recycling systems, and tuning the solvent composition is a valuable parameter to obtain the desired polymer yield. Further development of computational tools to predict the solubility of polymers in various solvents with different compositions will be useful in introducing this approach to the recycling of multilayer plastic films. The dissolution time and the amount of solvent can be further adjusted to improve the purity of the polymers recovered with STRAP. Quantitative measurements can also be performed to evaluate whether impurities in the recovered polymers affect their properties. In the future, we will also focus on using STRAP to process multilayer films of polymers not reported in this example, such as polyamide, polystyrene, polypropylene, and polyvinyl chloride. Ideally, this would be to find a solvent or combination of solvents that promotes the thermal dissolution and precipitation of each polymer. In addition, we will consider the removal of additives, such as adhesives and inks, that may also be present in the plastic film.Our computational modeling framework provides us with an understanding of thermodynamic polymer-solvent properties, enabling the design of solvent systems that can be used to efficiently separate and recover polymer components in a variety of multilayer plastic films.

[0111] Example 3: STRAP with printed multilayer film (PE / EVOH / PET) In this example, we separated and recovered polymer components from a printed multilayer film consisting essentially of PE, EVOH and PET. 2 The EVOH fraction was cut into strips of 0.01 mm diameter. An initial deinking step was performed by treating the strips in 50% THF-50% DMF (v / v) at 83° C. for 60 min. Subsequent steps followed the STRAP-A process described in Examples 1 and 2, except that the PE fraction was dissolved in toluene at 110° C. for 180 min and the EVOH fraction was dissolved in DMSO at 95° C. for 45 min (dissolution times were different). Figure 20 shows the structure, solvent, sparing solubility, temperature and dissolution time of the printed multilayer film used in each process step.

[0112] The process resulted in an overall mass balance of 91.47 wt% (Figure 20). ATR-FTIR spectra corresponding to the solid material recovered from the process showed that the PE, EVOH and PET recovered from the film were indistinguishable from the same, corresponding virgin resins (Figure 21). These results indicate that a deinking step can be used in conjunction with the STRAP process to remove ink from printed plastics without significantly impacting the yield or quality of the recovered polymer resin.

[0113] Example 4: Dissolution times can be significantly reduced using film strips sized 2 mm or less In this example, we attempted to reduce the dissolution time of the STRAP process by chopping the multilayer film into strips 2 mm or smaller in size. The multilayer film is a printed film consisting essentially of PE, EVOH and PET. The chopped strips were first treated with 50% THF-50% DMF (v / v) at 83° C. for 5 minutes to remove the ink. Subsequent steps followed the STRAP-B process described in Example 2, except that the dissolution time for the PE and EVOH fractions was 5 minutes instead of 4 hours or 30 minutes. Figure 22 shows the solvents, temperatures and dissolution times used at each process step.

[0114] The process achieved an overall mass balance of 86.02 wt% (Figure 22). The yield was measured using a 1 x 1 cm 2 This is relatively lower than the longer dissolution times used in experiments with films of 1 × 1 cm. However, the dissolution time can be further optimized to maximize yield. Nevertheless, the dissolution time required to dissolve strips of 2 mm or less in size is about 1 × 1 cm. 2 The PET, EVOH and PE recovered from the films are indistinguishable from the same corresponding virgin resins, as shown by the ATR-FTIR spectra in Figure 23, although one PET sample shows a 3000 cm peak that appears to be derived from undissolved PE. -1 The results showed a peak near the STRAP time (Figure 23, panel (c)). These results indicate that chopping the multilayer film into strips of smaller size (e.g., ≦2 mm) can effectively reduce the dissolution time required in the STRAP process.

[0115] Example 5: STRAP with mixed plastic waste In this example, we experimented with mixed plastic waste consisting essentially of PE, PP, PVC, PET and PA, and found a solvent system (dodecane / toluene) that can separate PE and PP from the mixture of polymers. PP has historically been a very difficult polymer to separate. The process involves dissolving PE in dodecane at 100°C for 90 minutes, then dissolving PP in toluene at 110°C for 90 minutes. Figure 24 shows the solvents, temperatures and dissolution times used for each process step. The solubilized PE and PP can be precipitated by lowering the temperature of the solvent to about 35°C.

[0116] Example 6: STRAP using nylon-based multilayer plastic film and mixed plastic waste In this example, we separated and recovered polymer components from a nylon-based multilayer plastic film consisting essentially of PE, EVOH and nylon, and a mixed plastic waste consisting essentially of several types of PE (LDPE and HDPE), nylon (nylon 6,6,6, nylon 6,6, nylon 6), PP, PET, and PVC. Various solvent and temperature combinations were tried until the appropriate polymer was targeted.

[0117] The process for recovering the polymer components from nylon-based multilayer plastic films involves dissolving the PE in toluene at 110°C, then dissolving the EVOH in a solvent containing DMSO and water at 85°C. The solubilized PE and EVOH were precipitated by lowering the temperature of the solvent. The remaining solid is nylon. Figure 25 shows the solvent, temperature, and dissolution time used for each process. The PE, EVOH, and nylon recovered from the films are indistinguishable from the same, corresponding pure resins, as shown by the ATR-FTIR spectra in Figure 26. The slight difference in the EVOH peaks is believed to be due to additives or contamination in the film. The process achieved an overall mass balance of 96.66%, as shown in Table 8.

[0118] [Table 8]

[0119] The process for recovering polymer components from mixed plastic waste involves, sequentially, dissolving PVC in THF at 68°C, LDPE in toluene at 85°C, PP in THP at 90°C, HDPE in toluene at 110°C, PET in GVL at 160°C, Nylon 6,6,6 in 1,2-propanediol at 135°C, Nylon 6 in DMSO at 145°C, and Nylon 6,6 in formic acid at 65°C. Precipitation of the solubilized polymers was mostly accomplished by lowering the temperature of the solvent, except for PVC and Nylon 6,6, which were precipitated by adding the antisolvent water. Figure 27 shows the solvents, temperatures, and dissolution times used at each process step. The residue includes aluminum, cardboard, and residual polymer that was not completely dissolved. The process achieved an overall mass balance of 95.83%, as shown in Table 9.

[0120] [Table 9]

[0121] References TIFF2024541759000012.tif221152 TIFF2024541759000013.tif228152 TIFF2024541759000014.tif180152

Claims

1. 1. A method for recovering constituent polymers in a multi-layer plastic film or mixed plastic waste, comprising: (a) selectively dissolving a polymer in a solvent at a temperature to obtain a solubilized polymer, the polymer dissolving but not other polymers in the multi-layer plastic film or mixed plastic waste; (b) separating the solubilized polymer from the multi-layer plastic film or mixed plastic waste by mechanical filtration; (c) precipitating the solubilized polymer from the solvent; and (d) repeating steps (a), (b), and (c) for each different polymer in the multi-layer plastic film or mixed plastic waste using a solvent and temperature that selectively dissolves each different polymer. The method includes:

2. 10. The method of claim 1, further comprising using a computer tool to select a solvent and a temperature that selectively dissolves a polymer from among all of the components present in the multi-layer plastic film or mixed plastic waste.

3. 3. The method of claim 2, wherein the computational tools include calculating Hansen solubility parameters (HSP), molecular dynamics (MD) simulations, and combined quantum chemistry and statistical mechanics modeling.

4. 2. The method of claim 1, further comprising a deinking step prior to step (a) for removing ink from said multi-layer plastic film or mixed plastic waste.

5. 5. The method of claim 4, wherein the deinking step is carried out by treating the multi-layer plastic film or mixed plastic waste in tetrahydrofuran (THF) and N,N-dimethylformamide (DMF).

6. Prior to step (a), the multi-layer plastic film or mixed plastic waste is cut into 1 cm 2 2. The method of claim 1, further comprising the step of: cutting into strips:

7. 2. The method of claim 1, further comprising the step of shredding the multi-layer plastic film or mixed plastic waste into strips of 5 mm or less, 4 mm or less, 3 mm or less, or 2 mm or less prior to step (a).

8. 2. The method of claim 1, wherein in step (c) the solubilized polymer is precipitated from the solvent by addition of an antisolvent.

9. 2. The method of claim 1, wherein in step (c), the solubilized polymer is precipitated from the solvent by changing the temperature of the solvent.

10. 2. The method of claim 1, wherein the multi-layer plastic film consists essentially of polyethylene (PE), ethylene vinyl alcohol (EVOH) and polyethylene terephthalate (PET).

11. 11. The method of claim 10, wherein in step (a), PE is selectively dissolved in toluene at about 110°C, and EVOH is selectively dissolved in dimethylsulfoxide (DMSO) at about 95°C.

12. 12. The method of claim 11, wherein in step (c), the solubilized PE is precipitated by adding acetone and the solubilized EVOH is precipitated by adding water.

13. In step (a), PE is dissolved in toluene or C at about 110° C. 6 ~C 12 11. The method of claim 10, wherein the EVOH is selectively dissolved in an alkane and the EVOH is selectively dissolved in a solvent comprising DMSO and water at about 95°C.

14. 14. The method of claim 13, wherein in step (c), the solubilized PE is precipitated by reducing the temperature of the toluene to about 35°C, and the solubilized EVOH is precipitated by reducing the temperature of the DMSO and water to about 35°C.

15. 11. The method of claim 10, wherein the multi-layer plastic film further comprises a tie layer comprising ethylene vinyl acetate (EVA).

16. 16. The method of claim 15, wherein EVA is dissolved in toluene at about 110° C. in step (a) and precipitated together with PE by adding acetone in step (c), and EVA is separated from PE after step (c) by selectively dissolving EVA in N-methylpyrrolidone (NMP).

17. 16. The method of claim 15, wherein the EVA is dissolved together with the PE in toluene at about 110° C. in step (a), and the EVA is separated from the PE in step (c) by reducing the temperature of the toluene to about 35° C. to precipitate the PE.

18. 2. The method of claim 1, wherein the multilayer plastic film consists essentially of polyethylene terephthalate (PETG), PE, EVOH and PET.

19. 20. The method of claim 18, wherein in step (a), PETG is selectively dissolved in a solvent comprising DMF and THF at about 87°C, PE is dissolved in toluene at about 110°C, and EVOH is dissolved in a solvent comprising DMSO and water at about 95°C.

20. 20. The method of claim 19, wherein in step (c), the solubilized PETG is precipitated by adding 1-propanol, the solubilized PE is precipitated by reducing the temperature of the toluene to about 35°C, and the solubilized EVOH is precipitated by reducing the temperature of the DMSO and water to about 35°C.

21. 2. The method of claim 1, wherein the mixed plastic waste consists essentially of PE, polypropylene (PP), polyvinyl chloride (PVC), PET and polyamide (PA).

22. 22. The method of claim 21, wherein in step (a), PE is dissolved in dodecane at about 100°C and PP is dissolved in toluene at about 110°C.

23. 23. The method of claim 22, wherein in step (c), the solubilized PE is precipitated by reducing the temperature of the dodecane to about 35°C, and the solubilized PP is precipitated by reducing the temperature of the toluene to about 35°C.

24. 2. The method of claim 1, wherein the multi-layer plastic film consists essentially of PE, EVOH and nylon.

25. 25. The method of claim 24, wherein in step (a), PE is selectively dissolved in toluene at about 110°C, and EVOH is selectively dissolved in a solvent comprising DMSO and water at about 85°C.

26. 26. The method of claim 25, wherein in step (c), the solubilized PE is precipitated by reducing the temperature of the toluene to about 35°C, and the solubilized EVOH is precipitated by reducing the temperature of the DMSO and water to about 35°C.

27. 2. The method of claim 1, wherein the mixed plastic waste consists essentially of PVC, low density polyethylene (LDPE), PP, high density polyethylene (HDPE), PET, nylon 6,6,6, nylon 6, and nylon 6,6.

28. 28. The method of claim 27, wherein in step (a), PVC is selectively dissolved in THF at about 68°C, LDPE is selectively dissolved in toluene or a C6-C12 alkane at about 85°C, PP is selectively dissolved in tetrahydropyran (THP) at about 90°C, HDPE is selectively dissolved in toluene at about 110°C, PET is selectively dissolved in gamma valerolactone (GVL) at about 160°C, nylon 6,6,6 is dissolved in 1,2-propanediol at about 135°C, nylon 6 is selectively dissolved in DMSO at about 145°C, and nylon 6,6 is dissolved in formic acid at about 65°C.

29. 29. The method of claim 28, wherein in step (c), the solubilized PVC is precipitated by the addition of water, the solubilized LDPE is precipitated by reducing the temperature of the toluene to about 35° C., the solubilized PP is precipitated by reducing the temperature of the THP to about 35° C., the solubilized PP is precipitated by reducing the temperature of the THP to about 35° C., the solubilized HDPE is precipitated by reducing the temperature of the toluene to about 35° C., the solubilized PET is precipitated by reducing the temperature of the GVL to about 35° C., the solubilized nylon 6,6,6 is precipitated by reducing the temperature of the 1,2-propanediol to about 35° C., the solubilized nylon 6 is precipitated by reducing the temperature of the DMSO to about 35° C., and the solubilized nylon 6,6 is precipitated by the addition of water.

Citation Information

Cited By

  • Method for dissolving and precipitating polymer compound, method for recovering good solvent phase and poor solvent phase, and method for purifying polymer compound

    WO2026159985A1