Method for producing positive electrode active material

The method of dual firing and coating with a specific nickel compound enhances the electrochemical performance of high-nickel positive electrode active materials, improving initial capacity and life characteristics in lithium secondary batteries.

JP2024541893AActive Publication Date: 2024-11-13LG CHEM LTD
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
JP2024523971
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2022-05-10
Filing Date
2023-04-04
Publication Date
2024-11-13
Estimated Expiration
2043-04-04

AI Technical Summary

Technical Problem

High nickel content in positive electrode active materials for lithium secondary batteries leads to rapid deterioration of electrochemical performance, increased discharge resistance, and reduced life characteristics.

Method used

A method involving primary and secondary firing of a positive electrode active material precursor with a nickel compound added in a specific range (0.01-0.15 mol%) to produce a lithium transition metal oxide, followed by coating with a coating element to form a uniform layer.

Benefits of technology

Improves both initial capacity and life characteristics of the battery by reducing charge transfer resistance and maintaining performance over multiple cycles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024541893000001
    Figure 2024541893000001
  • Figure 2024541893000002
    Figure 2024541893000002
  • Figure 2024541893000003
    Figure 2024541893000003
Patent Text Reader

Abstract

The present invention relates to a method for producing a positive electrode active material capable of realizing a battery having both excellent initial capacity and life characteristics, and includes the steps of (A) mixing a positive electrode active material precursor containing 80 mol % or more of nickel (Ni) among all metals with a lithium-containing raw material, and then performing primary firing to produce a primary fired product, and (B) mixing the primary fired product with a nickel compound, and then performing secondary firing to produce a lithium transition metal oxide, wherein the nickel compound is added so that the mole % of nickel contained in the nickel compound is more than 0.01 mol % and less than 0.15 mol % with respect to the number of moles of all metals contained in the positive electrode active material precursor.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] This application claims the benefit of priority based on Korean Patent Application No. 10-2022-0057424, filed May 10, 2022, the entire contents of which are incorporated herein by reference.

[0002] The present invention relates to a method for producing a positive electrode active material. [Background technology]

[0003] Among the positive electrode active materials used in lithium secondary batteries, the performance of positive electrode active materials having a layered structure is being improved day by day for application in EVs (Electric Vehicles) such as electric automobiles.

[0004] The higher the electrochemical capacity that a positive electrode active material can exhibit, the higher the energy density, and battery manufacturers around the world are striving to be first to develop positive electrode active materials with high energy density. As a result, positive electrode active materials with a layered structure and high nickel content are becoming the hottest topic.

[0005] However, the higher the nickel content, the more rapidly the electrochemical performance of the positive electrode active material deteriorates after repeated charge and discharge. That is, if the nickel content of all metals other than lithium is increased to 80 mol % or more in order to increase the energy density, the charge and discharge capacity increases, but the discharge resistance increase rate increases, causing a rapid deterioration in life characteristics (capacity retention rate, gas generation amount, etc.). Summary of the Invention [Problem to be solved by the invention]

[0006] The present invention has been made to solve the above problems, and an object of the present invention is to provide a method for manufacturing a positive electrode active material that can realize a battery having both excellent initial capacity and life characteristics. [Means for solving the problem]

[0007] In order to solve the above problems, the present invention provides a method for producing a positive electrode active material.

[0008] (1) The present invention provides a method for producing a positive electrode active material, the method comprising the steps of: (A) mixing a positive electrode active material precursor containing 80 mol % or more of nickel (Ni) among all metals with a lithium-containing raw material, followed by primary firing to produce a primary fired product; and (B) mixing the primary fired product with a nickel compound, followed by secondary firing to produce a lithium transition metal oxide, wherein the nickel compound is added such that the mole % of nickel contained in the nickel compound is more than 0.01 mol % and less than 0.15 mol % with respect to the number of moles of all metals contained in the positive electrode active material precursor.

[0009] (2) The present invention provides a method for producing a positive electrode active material according to the above (1), wherein the positive electrode active material precursor has a composition represented by the following chemical formula 1-1 or 1-2: [Chemical formula 1-1] Ni a1 Co b1 Mn c1 M 1 d1 (OH)2 [Chemical formula 1-2] Ni a1 Co b1 Mn c1 M 1 d1 O.H. In the above Chemical Formula 1-1 and Chemical Formula 1-2, M 1 is one or more selected from Al, Zr, B, W, Mg, Ce, Hf, Ta, La, Ti, Sr, Ba, Ce, Hf, F, P, S, Y, and La, 0.80≦a1<1.0, 0 <b1≦0.20、0<c1≦0.20、0≦d1≦0.10、a1+b1+c1+d1=1である。

[0010] (3) In the present invention, in the above (1) or (2), the nickel compound has an average particle size (D 50The present invention provides a method for producing a positive electrode active material having a grain size of less than 3 μm.

[0011] (4) The present invention provides a method for producing a positive electrode active material according to any one of (1) to (3), wherein the nickel compound is one or more selected from Ni(OH)2, NiO, NiCO3, NiSO4, NiF2, NiCl2, NiBr2, NiI2, 2Ni(OH)2·4H2O, NiC2O4·2H2O, Ni(NO3)2·6H2O and NiSO4·6H2O.

[0012] (5) The present invention provides the method for producing a positive electrode active material according to any one of the above (1) to (4), wherein the nickel compound is added so that a molar percentage of nickel contained in the nickel compound is more than 0.01 mol % and not more than 0.14 mol % with respect to the total moles of metals contained in the positive electrode active material precursor.

[0013] (6) The present invention provides a method for producing a positive electrode active material according to any one of the above (1) to (5), wherein the nickel compound is added so that a molar percentage of nickel contained in the nickel compound is 0.02 mol % to 0.10 mol % with respect to the total moles of metals contained in the positive electrode active material precursor.

[0014] (7) The present invention provides the method for producing a positive electrode active material according to any one of the above (1) to (6), wherein the primary firing is carried out at a temperature of 600°C to 750°C.

[0015] (8) The present invention provides the method for producing a positive electrode active material according to any one of the above (1) to (7), wherein the secondary baking is carried out at a temperature of 750°C to 900°C.

[0016] (9) The present invention provides the method for producing a positive electrode active material according to any one of the above (1) to (8), wherein the secondary firing is carried out at a temperature higher than that of the primary firing.

[0017] (10) The present invention provides a method for producing a positive electrode active material according to any one of (1) to (9), further comprising the step of (C) mixing the lithium transition metal oxide with a coating element-containing raw material, and heat-treating the mixture to form a coating layer. Effect of the Invention

[0018] According to the present invention, when a specific amount of nickel compound is added to the primary sintered product and then secondary sintered, the initial characteristics and life characteristics of a battery using the positive electrode active material produced therefrom can both be improved. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0019] The terms and words used in this specification and the claims should not be interpreted in a limited manner to their ordinary or dictionary meanings, but should be interpreted in a manner that is consistent with the technical idea of ​​the present invention, based on the principle that the inventors can appropriately define the concepts of terms in order to best describe their invention.

[0020] In this specification, the terms "comprise", "comprise", "have" and the like are intended to specify the presence of embodied features, numbers, steps, components, or combinations thereof, but are not intended to preclude the presence or additional possibility of one or more different features, numbers, steps, components, or combinations thereof.

[0021] The present invention will now be described in further detail.

[0022] Method for producing positive electrode active material The present inventors have discovered that when a positive electrode active material having a high nickel content is produced by calcining a positive electrode active material precursor and a lithium-containing raw material twice (first calcination and second calcination) and adding a specific amount of a nickel compound before the second calcination, the performance of a battery using the produced positive electrode active material is improved, and have completed the present invention.

[0023] The method for producing a positive electrode active material according to the present invention includes the steps of (A) mixing a positive electrode active material precursor containing 80 mol % or more of nickel (Ni) among all metals with a lithium-containing raw material, followed by primary firing to produce a primary fired product, and (B) mixing the primary fired product with a nickel compound, followed by secondary firing to produce a lithium transition metal oxide, wherein the nickel compound is added such that the mole % of nickel contained in the nickel compound is more than 0.01 mol % and less than 0.15 mol % with respect to the moles of all metals contained in the positive electrode active material precursor.

[0024] The method for preparing a positive electrode active material according to the present invention may further include the step of (C) mixing the lithium transition metal oxide with a coating element-containing raw material, followed by heat treatment to form a coating layer.

[0025] The method for producing the positive electrode active material will be specifically described below.

[0026] (A) Step and (B) Step The method for producing a positive electrode active material according to the present invention includes the steps of (A) mixing a positive electrode active material precursor containing 80 mol % or more of nickel (Ni) among all metals with a lithium-containing raw material, followed by primary firing to produce a primary fired product, and (B) mixing the primary fired product with a nickel compound, followed by secondary firing to produce a lithium transition metal oxide, where the nickel compound is added such that the mole % of nickel contained in the nickel compound is more than 0.01 mol % and less than 0.15 mol % with respect to the moles of all metals contained in the positive electrode active material precursor.

[0027] The positive electrode active material produced by the production method of the present invention has a surface coated with an appropriate amount of nickel that exhibits high capacity performance. When applied to a lithium secondary battery, this improves the initial capacity of the battery and reduces the charge transfer resistance on the surface of the positive electrode active material, thereby resulting in an improvement in life characteristics, in particular, a significant reduction in the rate of increase in resistance.

[0028] According to the present invention, the nickel compound may be added so that the mole percent of nickel contained in the nickel compound is more than 0.01 mole percent and less than 0.15 mole percent with respect to the total moles of metal contained in the positive electrode active material precursor, specifically, more than 0.01 mole percent, 0.02 mole percent or more, 0.04 mole percent or more, 0.06 mole percent or more, 0.08 mole percent or more, 0.10 mole percent or less, 0.12 mole percent or less, 0.14 mole percent or less, and less than 0.15 mole percent. In this case, an appropriate amount of nickel is coated on the surface of the positive electrode active material, improving the charge / discharge capacity and preventing the side effect of deterioration of the lifespan.

[0029] When the nickel compound is added such that the mole % of nickel contained in the nickel compound is 0.01 mol % or less with respect to the total moles of metal contained in the positive electrode active material precursor, the amount of nickel coating is insufficient to completely cover the surface of the positive electrode active material, which may result in a problem of poor coating effect.

[0030] When the nickel compound is added such that the mole % of nickel contained in the nickel compound is 0.15 mol % or more with respect to the total moles of metal contained in the positive electrode active material precursor, an uneven coating film having some parts intertwined therein may be formed due to excessive nickel coating, which may significantly deteriorate the life characteristics of the positive electrode active material.

[0031] According to the present invention, the positive electrode active material precursor may have a composition represented by the following Formula 1-1 or 1-2.

[0032] [Chemical formula 1-1] Ni a1 Co b1 Mn c1 M 1 d1 (OH)2

[0033] [Chemical formula 1-2] Ni a1 Co b1 Mn c1 M1 d1 O.H.

[0034] In the above Chemical Formula 1-1 and Chemical Formula 1-2, M 1 is one or more selected from Zr, B, W, Mg, Ce, Hf, Ta, La, Ti, Sr, Ba, Ce, Hf, F, P, S, Y and La, 0.80≦a1<1.0, 0 <b1≦0.20、0<c1≦0.20、0≦d1≦0.10、a1+b1+c1+d1=1である。

[0035] The a1 means the atomic fraction of nickel among the metal elements in the precursor, and may be 0.80 or more, 0.85 or more, 0.95 or less, 0.98 or less, or less than 1.0.

[0036] The b1 means the atomic fraction of cobalt among the metal elements in the precursor, and may be greater than 0, 0.01 or more, 0.02 or more, 0.05 or less, 0.10 or less, or 0.20 or less.

[0037] The c1 means the atomic fraction of manganese among the metal elements in the precursor, and may be greater than 0, 0.01 or more, 0.02 or more, 0.05 or more, 0.10 or less, or 0.20 or less.

[0038] The d1 is the metal element M in the precursor. 1 It means the element fraction of an element, and can be 0 or more, 0.01 or more, 0.02 or less, 0.05 or less, or 0.10 or less.

[0039] The lithium-containing raw material may be, for example, at least one selected from the group consisting of lithium carbonate (Li2CO3), lithium hydroxide (LiOH), LiNO3, CH3COOLi, and Li2(COO)2, and may be preferably lithium carbonate (Li2CO3), lithium hydroxide (LiOH), or a combination thereof.

[0040] When preparing the positive electrode active material, the positive electrode active material precursor and the lithium-containing raw material may be mixed in a molar ratio of 1:1 to 1:1.625 or 1:1 to 1:1.15. If the lithium-containing raw material is mixed in an amount less than this range, the capacity of the prepared positive electrode active material may decrease, and if the lithium-containing raw material is mixed in an amount exceeding this range, unreacted Li may remain as a by-product, resulting in a decrease in capacity and separation of the positive electrode active material particles after firing (inducing an entanglement phenomenon of the positive electrode active material).

[0041] When the positive electrode active material precursor and the lithium-containing raw material are mixed, a doping element-containing raw material may be further mixed. The metal element contained in the doping element-containing raw material may be Al, Zr, B, W, Mo, Cr, Nb, Mg, Hf, Ta, La, Ti, Sr, Ba, Ce, F, P, S, and Y. The doping element-containing raw material may be acetate, nitrate, sulfate, halide, sulfide, hydroxide, oxide, or oxyhydroxide containing the metal element. For example, when the metal element is Al, aluminum hydroxide (Al(OH)3) may be used, and when the metal element is Zr, zirconium oxide (ZrO2) may be used.

[0042] According to the present invention, the nickel compound has an average particle size (D 50 Specifically, the nickel compound may have an average particle size (D 50 The maximum particle size (D) of the nickel compound may be more than 0.01 μm and less than 3 μm, more specifically more than 0.05 μm and less than 2.5 μm. max In this case, the particle size is similar to or smaller than the particle size of the positive active material, and therefore, during coating, uniform coating is possible in terms of atomic diffusion onto the surface of the positive active material, and the properties of the positive active material produced may be uniform.

[0043] According to the present invention, the nickel compound may be nickel hydroxide, oxide, carbonate, acetate, nitrate, sulfate, halide, sulfide, or hydrates thereof, and specifically may be one or more selected from Ni(OH)2, NiO, NiCO3, NiSO4, NiF2, NiCl2, NiBr2, NiI2, 2Ni(OH)2·4H2O, NiC2O4·2H2O, Ni(NO3)2·6H2O, and NiSO4·6H2O. Specifically, the nickel compound may have a melting point or decomposition temperature of 700° C. or less.

[0044] According to the present invention, the primary firing may be performed at a temperature of 600°C to 750°C. Specifically, the primary firing may be performed at 600°C or more, 650°C or more, 700°C or more, 730°C or less, 740°C or less, or 750°C or less. The primary firing is a step of mixing and reacting a positive electrode active material precursor with a lithium raw material, and the strength of the primary fired product can be adjusted to be low by firing at a relatively low temperature of 600°C to 750°C. This is because the strength of the fired product is weaker as the lithium by-product on the surface of the particles is fired at a relatively low temperature.

[0045] According to the present invention, the secondary firing may be performed at a temperature of 750°C to 900°C. Also, the secondary firing may be performed at a temperature higher than that of the primary firing. Specifically, the primary firing may be performed at 750°C or higher, 760°C or higher, 770°C or higher, 800°C or lower, 850°C or lower, or 900°C or lower. The secondary firing is a step in which a small amount of residual lithium that is unreacted in the primary firing reacts, and the secondary firing is performed at a relatively higher temperature than the primary firing temperature, which can help in effective crystal growth.

[0046] In step (B), after the secondary firing, a commonly performed water washing, filtering and drying process may be performed to remove residual lithium that may be present on the surface of the lithium transition metal oxide.

[0047] The water washing process may be performed using a washing solution such as deionized water, distilled water, ethanol, etc., and the content of the washing solution may be 50 parts by weight to 150 parts by weight based on 100 parts by weight of the secondary fired product. The water washing may be performed at a temperature of 5° C. to 40° C. for 1 minute to 30 minutes. In this case, residual ions on the surface of the positive electrode active material can be effectively removed, and surface deterioration of the positive electrode active material that occurs during the water washing process can be minimized.

[0048] The filtering and drying steps are steps for removing moisture from the positive electrode active material that has been washed with water. The filtering can be performed using a filter press, and the drying can be performed at a temperature of 100° C. to 150° C. in a vacuum state.

[0049] (C) Step The method for preparing a positive electrode active material according to the present invention may further include a step of mixing the lithium transition metal oxide with a coating element-containing raw material and heat-treating the mixture to form a coating layer.

[0050] The metal element contained in the coating element-containing raw material may be Zr, B, W, Mo, Cr, Nb, Mg, Hf, Ta, La, Ti, Sr, Ba, Ce, F, P, S, and Y. The coating element-containing raw material may be acetate, nitrate, sulfate, halide, sulfide, hydroxide, oxide, or oxyhydroxide containing the metal element. For example, when the metal element is B, boric acid (H3BO3) may be used.

[0051] The coating element-containing raw material may be included in an amount of 200 ppm to 2000 ppm by weight based on the lithium transition metal oxide. When the content of the coating element-containing raw material is within this range, the capacity of the battery may be improved, and the resulting coating layer may suppress a direct reaction between the electrolyte and the lithium transition metal oxide, thereby improving the long-term performance characteristics of the battery.

[0052] The heat treatment in step (C) may be performed at a temperature of 200°C to 400°C. When the heat treatment temperature is within the above range, a coating layer can be formed while maintaining the structural stability of the transition metal oxide. The heat treatment may be performed for 1 hour to 10 hours. When the heat treatment time is within the above range, a proper coating layer can be formed and production efficiency can be improved.

[0053] positive electrode The present invention also provides a positive electrode for a lithium secondary battery, which contains the positive electrode active material produced by the above-mentioned method.

[0054] Specifically, the positive electrode includes a positive electrode current collector and a positive electrode active material layer located on at least one surface of the positive electrode current collector and including the positive electrode active material produced by the above-mentioned method.

[0055] The positive electrode current collector is not particularly limited as long as it does not cause a chemical change in the battery and has conductivity, and for example, stainless steel, aluminum, nickel, titanium, baked carbon, or aluminum or stainless steel surface treated with carbon, nickel, titanium, silver, etc. can be used. In addition, the positive electrode current collector can usually have a thickness of 3 μm to 500 μm, and fine irregularities can be formed on the surface of the current collector to increase the adhesive force of the positive electrode active material. For example, it can be used in various forms such as a film, sheet, foil, net, porous body, foam, nonwoven fabric, etc.

[0056] The positive electrode active material layer may contain a conductive material and a binder in addition to the positive electrode active material.

[0057] In this case, the positive electrode active material may be included in an amount of 80 wt% to 99 wt%, more specifically, 85 wt% to 98 wt%, based on the total weight of the positive electrode active material layer. When included in the above content range, excellent capacity characteristics can be exhibited.

[0058] In this case, the conductive material is used to impart conductivity to the electrode, and can be used without any particular limitation as long as it does not cause a chemical change in the battery to be constructed and has electronic conductivity. Specific examples include graphite such as natural graphite and artificial graphite; carbon-based materials such as carbon black, acetylene black, ketjen black, channel black, furnace black, lamp black, thermal black, and carbon fibers; metal powders or metal fibers such as copper, nickel, aluminum, and silver; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; and conductive polymers such as polyphenylene derivatives, and one or more of these can be used alone or in combination. The conductive material can be included in an amount of 1% by weight to 30% by weight based on the total weight of the positive electrode active material layer.

[0059] The binder serves to improve the adhesion between the positive electrode active material particles and the adhesive strength between the positive electrode active material and the current collector. Specific examples include polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol, polyacrylonitrile, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene polymer (EPDM), sulfonated-EPDM, styrene-butadiene rubber (SBR), fluororubber, and various copolymers thereof, and one or more of these may be used alone or in combination. The binder may be included in an amount of 1 wt% to 30 wt% based on the total weight of the positive electrode active material layer.

[0060] The positive electrode may be manufactured by a conventional method for manufacturing a positive electrode, except for using the positive electrode active material. Specifically, the positive electrode may be manufactured by applying a positive electrode mixture prepared by dissolving or dispersing the positive electrode active material and, optionally, a binder and a conductive material in a solvent onto a positive electrode current collector, followed by drying and rolling. Here, the types and contents of the positive electrode active material, binder, and conductive material are as described above. Alternatively, the positive electrode may be manufactured by casting the positive electrode mixture onto another support, peeling it off from the support, and laminating the resulting film onto the positive electrode current collector.

[0061] The solvent may be a solvent commonly used in the art, such as dimethyl sulfoxide (DMSO), isopropyl alcohol, N-methylpyrrolidone (NMP), acetone, or water, and may be used alone or in combination of two or more of these. The amount of the solvent used is sufficient to dissolve or disperse the positive electrode active material, conductive material, and binder, and to provide a viscosity that allows excellent thickness uniformity during subsequent coating for the manufacture of a positive electrode, taking into consideration the coating thickness of the slurry and the manufacturing yield.

[0062] Lithium secondary battery In addition, the present invention can provide an electrochemical device including the positive electrode. The electrochemical device can be, for example, a battery or a capacitor, and more specifically, a lithium secondary battery.

[0063] Specifically, the lithium secondary battery includes a positive electrode, a negative electrode facing the positive electrode, a separator interposed between the positive electrode and the negative electrode, and an electrolyte. Since the positive electrode is as described above, a detailed description thereof will be omitted, and only the remaining components will be described in detail below.

[0064] Also, the lithium secondary battery may optionally further include a battery container that houses an electrode assembly of the positive electrode, the negative electrode, and the separator, and a sealing member that seals the battery container.

[0065] In the lithium secondary battery, the negative electrode includes a negative electrode current collector and a negative electrode active material layer located on the negative electrode current collector.

[0066] The negative electrode current collector is not particularly limited as long as it does not cause a chemical change in the battery and has high conductivity, and may be, for example, copper, stainless steel, aluminum, nickel, titanium, calcined carbon, copper or stainless steel surface treated with carbon, nickel, titanium, silver, or aluminum-cadmium alloy. The negative electrode current collector may have a thickness of usually 3 μm to 500 μm, and like the positive electrode current collector, the surface of the current collector may be formed with fine irregularities to strengthen the binding force of the negative electrode active material. For example, it may be used in various forms such as a film, sheet, foil, net, porous body, foam, nonwoven fabric, etc.

[0067] The negative electrode active material layer includes a negative electrode active material, and optionally a binder and a conductive material.

[0068] The negative electrode active material may be a compound capable of reversible intercalation and deintercalation of lithium. Specific examples of the negative electrode active material include carbonaceous materials such as artificial graphite, natural graphite, graphitized carbon fiber, and amorphous carbon; metallic compounds capable of alloying with lithium such as Si, Al, Sn, Pb, Zn, Bi, In, Mg, Ga, Cd, Si alloys, Sn alloys, and Al alloys; SiO β(0<β<2), metal oxides capable of doping and dedoping lithium, such as SnO2, vanadium oxide, and lithium vanadium oxide; or composites containing the metallic compounds and carbonaceous materials, such as Si-C composites or Sn-C composites, and any one or a mixture of two or more of these may be used. In addition, a thin film of metallic lithium may be used as the negative electrode active material. In addition, the carbon material may be either low-crystalline carbon or high-crystalline carbon. Representative examples of low crystalline carbon include soft carbon and hard carbon, and representative examples of high crystalline carbon include amorphous, plate-like, flake-like, spherical or fibrous natural or artificial graphite, kish graphite, pyrolytic carbon, mesophase pitch based carbon fiber, meso-carbon microbeads, mesophase pitches, and high-temperature fired carbon such as petroleum or coal tar pitch derived cokes.

[0069] The negative electrode active material may be included in an amount of 80% by weight to 99% by weight based on the total weight of the negative electrode active material layer.

[0070] The binder is a component that facilitates bonding between the conductive material, the active material, and the current collector, and can be added in an amount of 0.1% by weight to 10% by weight based on the total weight of the negative electrode active material layer. Examples of such binders include polyvinylidene fluoride (PVDF), polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene polymer (EPDM), sulfonated-EPDM, styrene-butadiene rubber, nitrile-butadiene rubber, fluororubber, and various copolymers thereof.

[0071] The conductive material is a component for further improving the conductivity of the negative electrode active material, and may be added in an amount of 10% by weight or less, specifically 5% by weight or less, based on the total weight of the negative electrode active material layer. Such a conductive material is not particularly limited as long as it does not cause a chemical change in the battery and has conductivity, and examples of such conductive materials include graphite such as natural graphite and artificial graphite; carbon black such as acetylene black, ketjen black, channel black, furnace black, lamp black, and thermal black; conductive fibers such as carbon fibers and metal fibers; metal powders such as carbon fluoride, aluminum, and nickel powder; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; and conductive materials such as polyphenylene derivatives.

[0072] The negative electrode active material layer can be produced by applying a negative electrode mixture, which is prepared by dissolving or dispersing a negative electrode active material, and optionally a binder and a conductive material, in a solvent, onto a negative electrode current collector and drying the applied mixture. Alternatively, the negative electrode mixture can be cast onto a separate support, and then peeled off from the support to obtain a film, which can be laminated onto the negative electrode current collector.

[0073] Meanwhile, in the lithium secondary battery, the separator separates the negative electrode and the positive electrode and provides a path for lithium ions to move. Any separator that is generally used as a separator in a lithium secondary battery can be used without any particular limitation. In particular, a separator that has low resistance to ion movement of the electrolyte and has excellent humidification ability of the electrolyte solution is preferable. Specifically, a porous polymer film, for example, a porous polymer film made of a polyolefin-based polymer such as an ethylene homopolymer, a propylene homopolymer, an ethylene / butene copolymer, an ethylene / hexene copolymer, and an ethylene / methacrylate copolymer, or a laminate structure of two or more layers thereof can be used. In addition, a conventional porous nonwoven fabric, for example, a nonwoven fabric made of a high-melting point glass fiber, a polyethylene terephthalate fiber, etc., can be used. In addition, a coated separator containing a ceramic component or a polymeric material can be used to ensure heat resistance or mechanical strength, and can be selectively used as a single layer or a multilayer structure.

[0074] In addition, examples of the electrolyte used in the present invention include organic liquid electrolytes, inorganic liquid electrolytes, solid polymer electrolytes, gel-type polymer electrolytes, solid inorganic electrolytes, and molten inorganic electrolytes that can be used in the production of lithium secondary batteries, but are not limited to these.

[0075] Specifically, the electrolyte may include an organic solvent and a lithium salt.

[0076] The organic solvent can be used without any particular limitation as long as it serves as a medium through which ions involved in the electrochemical reaction of the battery can move. Specifically, the organic solvent can be an ester solvent such as methyl acetate, ethyl acetate, γ-butyrolactone, or ε-caprolactone; an ether solvent such as dibutyl ether or tetrahydrofuran; a ketone solvent such as cyclohexanone; an aromatic hydrocarbon solvent such as benzene or fluorobenzene; dimethylcarbonate (DMC), diethylcarbonate (DEC), ethylmethylcarbonate (EMC), ethylene carbonate (EC), or propylene carbonate (propylene carbonate). Examples of the solvents that can be used include carbonate-based solvents such as ethylene carbonate (PC), alcohol-based solvents such as ethanol and isopropyl alcohol, nitriles such as R-CN (R is a straight-chain, branched or cyclic hydrocarbon group having 2 to 20 carbon atoms, which may contain a double bond aromatic ring or an ether bond), amides such as dimethylformamide, dioxolanes such as 1,3-dioxolane, and sulfolanes. Among these, carbonate-based solvents are preferred, and a mixture of a cyclic carbonate (e.g., ethylene carbonate or propylene carbonate) having high ionic conductivity and high dielectric constant that can enhance the charge / discharge performance of the battery and a low-viscosity linear carbonate compound (e.g., ethyl methyl carbonate, dimethyl carbonate or diethyl carbonate) is more preferred. In this case, the cyclic carbonate and the linear carbonate are mixed in a volume ratio of about 1:1 to about 1:9, so that the electrolyte can exhibit excellent performance.

[0077] The lithium salt can be used without any particular limitation as long as it is a compound capable of providing lithium ions used in a lithium secondary battery. Specifically, the lithium salt may be LiPF6, LiClO4, LiAsF6, LiBF4, LiSbF6, LiAlO4, LiAlCl4, LiCF3SO3, LiC4F9SO3, LiN(C2F5SO3)2, LiN(C2F5SO2)2, LiN(CF3SO2)2, LiCl, LiI, or LiB(C2O4)2. The concentration of the lithium salt is preferably within the range of 0.1M to 2.0M. When the concentration of the lithium salt is within the above range, the electrolyte has appropriate conductivity and viscosity, so that it can exhibit excellent electrolyte performance and lithium ions can move effectively.

[0078] In addition to the electrolyte components, the electrolyte may further contain one or more additives such as haloalkylene carbonate compounds such as difluoroethylene carbonate, pyridine, triethyl phosphite, triethanolamine, cyclic ethers, ethylenediamine, n-glyme, hexamethylphosphoric triamide, nitrobenzene derivatives, sulfur, quinoneimine dyes, N-substituted oxazolidinones, N,N-substituted imidazolidines, ethylene glycol dialkyl ethers, ammonium salts, pyrrole, 2-methoxyethanol, or aluminum trichloride, in order to improve the life characteristics of the battery, suppress the decrease in the capacity of the battery, and improve the discharge capacity of the battery. In this case, the additives may be contained in an amount of 0.1% by weight to 5% by weight based on the total weight of the electrolyte.

[0079] As described above, the lithium secondary battery including the positive electrode active material according to the present invention stably exhibits excellent discharge capacity, output characteristics and life characteristics, and is therefore useful in portable devices such as mobile phones, notebook computers and digital cameras, and electric vehicles such as hybrid electric vehicles (HEVs).

[0080] Therefore, according to another embodiment of the present invention, there is provided a battery module including the lithium secondary battery as a unit cell, and a battery pack including the same.

[0081] The battery module or battery pack may be used as a power source for one or more medium- to large-sized devices, such as a power tool; an electric vehicle (EV), a hybrid electric vehicle, and a plug-in hybrid electric vehicle (PHEV); or a power storage system.

[0082] The external shape of the lithium secondary battery of the present invention is not particularly limited, and may be a cylindrical shape using a can, a square shape, a pouch shape, a coin shape, or the like.

[0083] The lithium secondary battery according to the present invention can be used not only as a battery cell used as a power source for a small device, but also preferably as a unit battery in a medium- to large-sized battery module including a large number of battery cells.

[0084] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS The present invention may, however, be embodied in many different forms and should not be construed as limited to the embodiments set forth herein.

[0085] Examples and Comparative Examples Example 1 Ni 0.89 Co 0.04 Mn 0.07 A small amount of Al(OH)3 was added to the positive electrode active material precursor having a composition represented by (OH)2, and the lithium source material LiOH·H2O was added so that the molar ratio of Li / Metal(Ni+Co+Mn+Al) became 1.05, and then these were mixed to produce a mixture. The mixture was placed in an alumina crucible and primarily fired at 720℃ in an oxygen atmosphere for 5 hours to produce a primarily fired product.

[0086] The primary fired product was mixed with Ni(OH)2 such that the mole percent of nickel contained was 0.02 mole percent based on the total moles of metals contained in the positive active material precursor, and then secondary fired at 790°C in an oxygen atmosphere for 5 hours. The mixture was washed with deionized water, filtered using a filter press, and dried in a vacuum oven at 130°C to produce a lithium transition metal oxide.

[0087] Then, the lithium transition metal oxide was mixed with 1000 ppm of boric acid (H3BO3) and heat-treated at 295°C for 5 hours in an air atmosphere to produce a lithium transition metal oxide (cathode active material A) having a coating layer containing boron.

[0088] Example 2 Positive electrode active material B was prepared in the same manner as in Example 1, except that Ni(OH)2 was mixed so that the mole percent of nickel contained in Ni(OH)2 was 0.06 mole percent based on the total moles of metals contained in the positive electrode active material precursor.

[0089] Example 3 Positive electrode active material C was prepared in the same manner as in Example 1, except that Ni(OH)2 was mixed so that the mole percent of nickel contained in Ni(OH)2 was 0.1 mole percent based on the total moles of metals contained in the positive electrode active material precursor.

[0090] Example 4 A positive electrode active material D was produced in the same manner as in Example 1, except that the secondary baking was carried out at 800° C. in an oxygen atmosphere (oxygen 90% by volume or more).

[0091] Example 5 Positive electrode active material E was produced in the same manner as in Example 1, except that Ni(OH)2 was mixed so that the mole percentage of nickel contained in Ni(OH)2 was 0.06 mole percent relative to the total moles of metals contained in the positive electrode active material precursor, and secondary firing was performed at 800° C. in an oxygen atmosphere (oxygen 90% by volume or more).

[0092] Example 6 Positive electrode active material F was produced in the same manner as in Example 1, except that Ni(OH)2 was mixed so that the mole percentage of nickel contained in Ni(OH)2 was 0.1 mole percent relative to the total moles of metals contained in the positive electrode active material precursor, and secondary firing was performed at 800°C in an oxygen atmosphere (oxygen 90% by volume or more).

[0093] Example 7 A positive electrode active material G was produced in the same manner as in Example 1, except that the secondary baking was carried out at 810° C. in an oxygen atmosphere (oxygen 90% by volume or more).

[0094] Example 8 Positive electrode active material H was produced in the same manner as in Example 1, except that Ni(OH)2 was mixed so that the mole percentage of nickel contained in Ni(OH)2 was 0.06 mole percent relative to the total moles of metals contained in the positive electrode active material precursor, and secondary firing was performed at 810° C. in an oxygen atmosphere (oxygen 90% by volume or more).

[0095] Example 9 Positive electrode active material I was produced in the same manner as in Example 1, except that Ni(OH)2 was mixed so that the mole percentage of nickel contained in Ni(OH)2 was 0.1 mole percent relative to the total moles of metals contained in the positive electrode active material precursor, and secondary firing was performed in an oxygen atmosphere (oxygen 90 volume % or more) at 810°C.

[0096] Comparative Example 1 Ni 0.89 Co 0.04 Mn 0.07 A small amount of Al(OH)3 was added to the positive electrode active material precursor having a composition represented by (OH)2, and the lithium source material LiOH·H2O was added so that the molar ratio of Li / Metal(Ni+Co+Mn+Al) became 1.05, and then these were mixed to produce a mixture. The mixture was placed in an alumina crucible and primarily fired at 720℃ in an oxygen atmosphere for 5 hours to produce a primarily fired product.

[0097] The primary fired product was subjected to secondary firing at 790° C. in an oxygen atmosphere for 5 hours, washed with deionized water, filtered using a filter press, and dried in a vacuum oven at 130° C. to produce a lithium transition metal oxide.

[0098] Then, the lithium transition metal oxide was mixed with 1000 ppm of boric acid (H3BO3) and heat-treated at 295°C for 5 hours in an air atmosphere to produce a lithium transition metal oxide (cathode active material J) having a coating layer containing boron.

[0099] Comparative Example 2 Positive electrode active material K was prepared in the same manner as in Example 1, except that Ni(OH)2 was mixed so that the mole percent of nickel contained in Ni(OH)2 was 0.01 mole percent based on the total moles of metals contained in the positive electrode active material precursor.

[0100] Comparative Example 3 Positive electrode active material L was prepared in the same manner as in Example 1, except that Ni(OH)2 was mixed so that the mole percent of nickel contained in Ni(OH)2 was 0.15 mole percent based on the total moles of metals contained in the positive electrode active material precursor.

[0101] The primary firing temperature, secondary firing temperature, and amount of Ni(OH)2 added in Examples 1 to 9 and Comparative Examples 1 to 3 are summarized in Table 1 below.

[0102] [Table 1]

[0103] Experimental Example Experimental example 1: Coin cell characterization Lithium secondary batteries were manufactured using the positive electrode active materials manufactured in the Examples and Comparative Examples, and the initial charge / discharge capacity, charge / discharge efficiency, and discharge resistance after 30 cycles were evaluated for each of the lithium secondary batteries.

[0104] Specifically, the positive electrode active materials prepared in the examples and comparative examples were mixed with FX35 conductive material, KF9709 binder, and BM740H binder in a weight ratio of 97.5:1.0:1.4:0.1 in NMP solvent to prepare a positive electrode slurry. The positive electrode slurry was applied to one side of an aluminum current collector, dried at 130°C, and rolled to prepare a positive electrode. Meanwhile, a Li metal disk was used as the negative electrode active material. An electrode assembly was prepared by interposing a separator between the positive electrode and negative electrode prepared as above, and the electrode assembly was placed inside a battery case, and an electrolyte was injected into the case to prepare a lithium secondary battery. Here, an electrolyte obtained by dissolving 1M LiPF6 in an organic solvent of EC / EMC / DMC (30 / 30 / 40, vol%) was injected to prepare a lithium secondary battery.

[0105] The lithium secondary battery manufactured as described above was charged in CC / CV mode at 25° C. at a constant current of 0.1 C to 4.25 V (final current 0.05 C), and then discharged in CC mode to 3.0 V to obtain the initial charge capacity, initial discharge capacity, and charge / discharge efficiency (shown in Table 2 below). The battery was then subjected to 30 charge / discharge cycles at a constant current of 0.33 C in the range of 3.0 V to 4.25 V at 45° C. Here, the voltage drop for 60 seconds after the start of discharge in the 30th charge / discharge cycle was measured, and the voltage drop was divided by the applied current value to calculate the discharge resistance, which is shown in Table 2 below as a value representative of the life characteristics. Meanwhile, the voltage was set to 1 C=200 mA / g throughout the entire process.

[0106] [Table 2]

[0107] Referring to Table 2, it can be seen that the batteries including the positive electrode active materials prepared in Examples 1 to 9 have excellent initial charge / discharge capacity and charge / discharge efficiency, and have significantly better life characteristics than the batteries including the positive electrode active materials prepared in Comparative Examples 1 to 3.

[0108] As a result, when a positive electrode active material having a high nickel content is manufactured as in the method for manufacturing a positive electrode active material according to the present invention, a positive electrode active material precursor and a lithium-containing raw material are calcined twice, and a specific amount of a nickel compound is added before the secondary calcination to manufacture the positive electrode active material, it is found that a battery using the positive electrode active material not only has excellent initial characteristics, but also has significantly improved life characteristics.

Claims

1. (A) mixing a positive electrode active material precursor containing 80 mol % or more of nickel (Ni) among all metals with a lithium-containing raw material, and then performing primary firing to produce a primary fired product; (B) mixing the primary fired product with a nickel compound and then secondary firing to produce a lithium transition metal oxide; the nickel compound is added so that a mole percentage of nickel contained in the nickel compound is more than 0.01 mol % and less than 0.15 mol % with respect to the total moles of metals contained in the positive electrode active material precursor.

2. The method for producing a positive electrode active material according to claim 1, wherein the positive electrode active material precursor has a composition represented by the following Chemical Formula 1-1 or Chemical Formula 1-2: [Chemical formula 1-1] Ni a1 Co b1 Mn c1 M 1 d1 (OH) 2 [Chemical formula 1-2] Ni a1 Co b1 Mn c1 M 1 d1 O・OH In the above Chemical Formula 1-1 and Chemical Formula 1-2, M 1 is one or more selected from Al, Zr, B, W, Mg, Ce, Hf, Ta, La, Ti, Sr, Ba, Ce, Hf, F, P, S, Y, and La; 0.80≦a1<1.0, 0<b1≦0.20, 0<c1≦0.20, 0≦d1≦0.10, and a1+b1+c1+d1=1.

3. The nickel compound has an average particle size (D 50 2. The method for producing a positive electrode active material according to claim 1, wherein the average particle diameter is less than 3 μm.

4. The nickel compound is Ni(OH). 2 , NiO, NiCO 3 , NiSO 4 , NiF 2 , NiCl 2 , NiBr 2 , NiI 2 , 2Ni(OH) 2 ・4H 2 O,NiC 2 O 4 ・2H 2 O, Ni(NO 3 ) 2 ・6H 2 O and NiSO 4 ・6H 2 2. The method for producing a positive electrode active material according to claim 1, wherein the first metal oxide is one or more selected from the group consisting of fluorine, fluorine, arsenic, fluorine ...

5. 2. The method for producing a positive electrode active material according to claim 1, wherein the nickel compound is added so that a mole percentage of nickel contained in the nickel compound is more than 0.01 mol % and not more than 0.14 mol % with respect to a mole number of all metals contained in the positive electrode active material precursor.

6. 2. The method for producing a positive electrode active material according to claim 1, wherein the nickel compound is added so that a mole percentage of nickel contained in the nickel compound is 0.02 mol % to 0.10 mol % with respect to a mole number of all metals contained in the positive electrode active material precursor.

7. The method for producing a positive electrode active material according to claim 1, wherein the primary baking is carried out at a temperature of 600°C to 750°C.

8. The method for producing a positive electrode active material according to claim 1, wherein the secondary baking is carried out at a temperature of 750°C to 900°C.

9. The method for producing a positive electrode active material according to claim 1 , wherein the secondary firing is performed at a temperature higher than that of the primary firing.

10. The method for producing a positive electrode active material according to claim 1 , further comprising the step of: (C) mixing the lithium transition metal oxide with a coating element-containing raw material, and heat-treating the mixture to form a coating layer.

Citation Information

Patent Citations

  • Method for preparing high-nickel positive electrode material and high-nickel positive electrode material obtained by using same

    CN109428077A

  • Single crystal high-capacity nickel-cobalt lithium manganate positive electrode material and preparation method thereof

    CN110061225A

  • Positive electrode material, preparation method thereof, positive electrode comprising positive electrode material and lithium ion battery

    CN113764638A

  • Nonaqueous electrolyte secondary battery and manufacture of its positive pole active material

    JP1995037576A

  • Manufacture of positive active material and non-aqueous secondary battery

    JP1997320601A