Composite material for lithium-ion secondary battery and its preparation method and application
The composite material with vapor-deposited nanosilicon in porous carbon addresses the dispersion and expansion issues, enhancing lithium-ion battery performance through uniform dispersion and structural stability.
Patent Information
- Application Number
- JP2024532907
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-12-22
- Filing Date
- 2022-06-23
- Publication Date
- 2024-11-14
- Estimated Expiration
- 2042-06-23
AI Technical Summary
Existing methods for preparing silicon-carbon composites for lithium-ion batteries fail to uniformly disperse nanosilicon particles in carbon materials, leading to structural damage due to silicon expansion and poor electrical contact, which affects the battery's capacity and performance.
A composite material is prepared by vapor phase deposition of nanosilicon and gaseous compounds containing C, N, B, or P within the pores of a spherical porous carbon matrix, which limits silicon expansion and ensures uniform dispersion, maintaining the structural integrity and enhancing electrochemical properties.
The composite material achieves improved specific capacity, cycling properties, and rate properties of lithium-ion batteries by minimizing silicon expansion and maintaining electrical contact, suitable for use in various electrolyte types.
Smart Images

Figure 2024542323000001_ABST
Abstract
Description
[Technical field]
[0001] [Cross reference] This application claims priority to a Chinese patent application filed with the China Patent Office on December 22, 2021, bearing application number 202111582639.1 and entitled "Composite material for lithium-ion secondary batteries and its preparation method and application."
[0002] [Technical field] The present invention relates to the technical field of materials, in particular to a composite material for lithium-ion secondary batteries and its preparation method and application. [Background technology]
[0003] Silicon is used as an ideal anode material for high-capacity lithium-ion batteries because its theoretical specific capacity is 4200mAh / g, which is one order of magnitude higher than the 372mAh / g of conventional graphite anodes. However, the high capacity of lithium-ion batteries is accompanied by the volume expansion (300%) of the silicon anode during the lithium insertion process, which leads to mass destruction of the electrode and a decrease in battery capacity.
[0004] At present, the effect of volume expansion can be effectively alleviated by preparing silicon-carbon composite materials. For example, in Chinese Patent Application No. 201510448316.1, silicon and different carbon materials are mechanically mixed twice, spray-dried, and then coated with a carbon shell on the outermost layer by vapor deposition, which alleviates the silicon expansion problem to a certain extent. However, at present, the mainstream method is to perform the compounding by mechanical mixing or simple coating, which cannot uniformly disperse nano silicon particles in the carbon material, and cannot fully exert the advantages of silicon-carbon composite materials. At the same time, such a method cannot effectively solve the destruction of materials caused by the large volume expansion of silicon. Summary of the Invention [Problem to be solved by the invention]
[0005] The embodiment of the present invention provides a composite material for lithium-ion secondary batteries and its preparation method and application. The nanosilicon in the composite material and one or more gaseous compounds containing any of the elements C, N, B, and P are uniformly dispersed in the pores of spherical porous carbon by vapor deposition. The porous structure limits the size and uniform dispersion of the nanosilicon after deposition, suppresses the effect of volume expansion, and avoids the problem of poor electrical contact caused by silicon pulverization, while the large hole in the center provides a large buffer space for the expansion of the silicon material, making it difficult for the structure of the entire composite material to be destroyed by expansion. Therefore, when the lithium insertion and extraction reaction is sufficiently performed on the silicon, the structure of the composite material can be kept intact, and the electrochemical properties of the battery can be further improved. And in the case of multi-element composite, C and N are beneficial to improve the cycle characteristics of the material, and B and P are beneficial to improve the rate characteristics of the material. [Means for solving the problem]
[0006] In a first aspect, an embodiment of the present invention provides a composite material for a lithium-ion secondary battery, the composite material being a spherical porous non-graphitizable carbon material having internal hollow pores, in which products (including silicon nanoparticles) are deposited by decomposition of a silicon-containing gas and one or more gaseous compounds containing any of the elements C, N, B, and P, and the products are deposited inside the pores; Here, the porous non-graphitizable carbon material is obtained by preparing a non-graphitizable carbon matrix by hardening it using a double emulsion method, and then carbonizing it.
[0007] Preferably, the silicon content in the composite material is 1 wt % to 70 wt %.
[0008] Preferably, the particle size range of the composite material is 1 μm to 100 μm, the average pore size is 0.1 nm to 10 nm, and the diameter of the hollow pores is 0.5 μm to 80 μm.
[0009] Preferably, the non-graphitizable carbon matrix of the spherical porous non-graphitizable carbon material is one or a combination of a phenolic resin, an epoxy resin, a furfural resin, or a polybutadiene resin; The silicon-containing gas is a silane compound and includes one or a combination of monosilane, trisilane, dichlorosilane, trichlorosilane, and tetrachlorosilane; The gaseous compound containing a C element includes one or more of acetylene, methane, propylene, ethylene, propane, and gaseous ethanol; The gaseous compound containing the N element includes at least one of nitrogen, ammonia, urea, and melamine, The gaseous compound containing the B element includes one or more of diborane, trimethyl borate, tripropyl borate, and boron tribromide; The gaseous compound containing the P element includes phosphine and / or phosphorus oxychloride.
[0010] In a second aspect, an embodiment of the present invention provides a method for preparing a composite material for a lithium-ion secondary battery according to the first aspect, the method comprising the steps of: Step 1: Using pure oil as the first liquid phase, dissolving resin in the corresponding solvent, adding non-ionic surfactant and curing agent to prepare the second liquid phase, and using oil containing surfactant as the third liquid phase, slowly adding the first liquid phase to the second liquid phase, stirring for 0.5-1 hour, then adding the stirred mixture to the third liquid phase, stirring to obtain the desired emulsion, heating to 80-130°C while continuing to stir, and keeping warm for 1-24 hours until the resin is cured, forming resin hollow microspheres, then centrifuging, washing and drying; Step 2: Put the dried sample into a reactor, heat the temperature to 800°C to 1300°C, and keep the temperature at 800°C to 1300°C for 0.5 hours to 15 hours to perform high-temperature carbonization treatment, thereby obtaining a non-graphitizable carbon matrix having a particle size in the range of 1 μm to 100 μm; Step 3: continuously introducing a pore-forming gas source into the obtained non-graphitizable carbon matrix at 600°C to 1000°C for 1 hour to 10 hours to subject the non-graphitizable carbon matrix to a pore-forming treatment to obtain a porous non-graphitizable carbon matrix material, in which the pore-forming gas source is one or a combination of two of oxygen, carbon dioxide and water vapor, and the gas flow rate of the pore-forming gas source is 2L / min to 20L / min; Step 4: performing vapor deposition on the obtained porous non-graphitizable carbon matrix material to obtain a composite material for a lithium ion secondary battery, the gas source for the vapor deposition including a silicon-containing gas and one or more gaseous compounds including any one of C, N, B, and P elements; Includes.
[0011] Preferably, the protective gas for the vapor deposition is one of nitrogen gas or argon gas or a combination thereof, the flow rate is 1-5 L / min, the gas flow rate of the gaseous compound is 0.5-10 L / min, the flow rate of the silicon-containing gas is 0.5-10 L / min, the deposition temperature is 500-1500° C., and the deposition time is 1-20 hours.
[0012] Preferably, the resin comprises one or more combinations of a phenolic resin, an epoxy resin, a furfural resin, or a polybutadiene resin; The solvent comprises one or a combination of ethanol, acetone, and toluene; The oils include one or more combinations of vegetable oil, paraffin oil, mineral oil, etc. The nonionic surfactant comprises one or more combinations of alkylglucosides, fatty acid glycerides, sorbitan fatty acid esters, and polysorbates; The curing agent includes one or a combination of trimethylhexamethylenediamine, ethylenediamine, and metaxylenediamine; The surfactant may include one or more of the following: stearic acid, sodium dodecylbenzenesulfonate, lecithin, etc. The silicon-containing gas is a silane compound and includes one or a combination of monosilane, trisilane, dichlorosilane, trichlorosilane, and tetrachlorosilane; The gaseous compound containing a C element includes one or more of acetylene, methane, propylene, ethylene, propane, and gaseous ethanol; The gaseous compound containing the N element includes at least one of nitrogen, ammonia, urea, and melamine, The gaseous compound containing the B element includes one or more of diborane, trimethyl borate, tripropyl borate, and boron tribromide; The gaseous compound containing the P element includes phosphine and / or phosphorus oxychloride.
[0013] Preferably, the mass fraction of the first liquid phase: the second liquid phase: the third liquid phase = (0, 30%]: (0, 30%]: (0, 50%], In the second liquid phase, the mass fraction is resin:solvent:hardener:nonionic surfactant=(0, 80%]:(0, 90%]:[0, 30%]:(0, 20%], In the third liquid phase, the mass fraction of oil:surfactant is (0, 90%):(0, 30%).
[0014] In a third aspect, an embodiment of the present invention provides an anode material for a lithium battery comprising the composite material for a lithium ion secondary battery according to the first aspect above.
[0015] In a fourth aspect, an embodiment of the present invention provides a lithium-ion battery comprising the composite material for a lithium-ion secondary battery according to the first aspect above. Effect of the Invention
[0016] Nanosilicon in the composite material for lithium ion secondary batteries according to the embodiment of the present invention and one or more gaseous compounds containing any of C, N, B, and P elements are uniformly dispersed in the pores of spherical porous carbon by vapor deposition. The porous structure limits the size and uniform dispersion of nanosilicon after deposition, suppresses the effect of volume expansion, and avoids the problem of poor electrical contact due to pulverization of silicone, while having a large hole in the center provides a large buffer space due to the expansion of the silicon material, making it difficult for the structure of the entire composite material to be destroyed by expansion. Therefore, when lithium insertion and extraction reactions are sufficiently performed on silicon, the structure of the composite material can be kept intact, and the electrochemical properties of the battery are further improved. In the case of multi-element composite, C and N are beneficial for improving the cycle characteristics of the material, and B and P are beneficial for improving the rate characteristics of the material. The composite material for lithium ion batteries provided by the present invention can be used in lithium ion batteries with liquid, semi-solid, quasi-solid, and all-solid electrolytes. [Brief description of the drawings]
[0017] Hereinafter, the technical solutions in the embodiments of the present invention will be described in more detail with reference to the drawings and examples.
[0018] [Figure 1] 1 is a flowchart showing a method for preparing a composite material for a lithium ion secondary battery according to an embodiment of the present invention. [Diagram 2] 1 is a scanning electron microscope (SEM) image of a cross section of the composite material for lithium ion secondary batteries prepared in Example 1 of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0019] The present invention will be further described below with reference to the drawings and specific examples. However, it should be understood that these examples are merely for the purpose of explaining the present invention in more detail and are not intended to limit the present invention in any manner, i.e., they are not intended to limit the scope of protection of the present invention.
[0020] The present invention proposes a composite material for lithium ion secondary batteries, which is a spherical porous non-graphitizable carbon material having hollow holes inside, in which products (including silicon nanoparticles) are deposited inside the pores by decomposition of a silicon-containing gas and one or more gaseous compounds containing any of the elements C, N, B, and P, Here, the porous non-graphitizable carbon material is obtained by preparing a non-graphitizable carbon matrix by hardening it using a double emulsion method, and then carbonizing it.
[0021] The silicon content in the composite material is 1 wt% to 70 wt%.
[0022] The particle size range of the composite material is 1 μm to 100 μm, the average pore size is 0.1 nm to 10 nm, and the diameter of the internal hollow pores is 0.5 μm to 80 μm.
[0023] The flow of the manufacturing method of the above-mentioned composite material for lithium batteries having hollow holes is shown in FIG. 1, and includes the following steps: In step 1, pure oils are used as the first liquid phase, resin is dissolved in the corresponding solvent, and nonionic surfactant and curing agent are added to prepare the second liquid phase, and oils containing surfactant are used as the third liquid phase, the first liquid phase is slowly added to the second liquid phase, and after stirring for 0.5-1 hour, the stirred mixture is added to the third liquid phase, and stirred to obtain the desired emulsion, and the mixture is heated to 80°C-130°C while continuing to stir, and kept warm for 1-24 hours until the resin is cured, and then the resin hollow microspheres are formed, which are then centrifuged, washed and dried; The resin comprises one or more combinations of a phenolic resin, an epoxy resin, a furfural resin, or a polybutadiene resin, and the solvent comprises one or more combinations of ethanol, acetone, and toluene; The oils include one or more combinations of vegetable oils, paraffin oils, mineral oils, etc., the nonionic surfactants include one or more combinations of alkyl glucosides, fatty acid glycerides, sorbitan fatty acid esters, polysorbates, the hardeners include one or more combinations of trimethylhexamethylenediamine, ethylenediamine, metaxylenediamine, and the surfactants include one or more combinations of stearic acid, sodium dodecylbenzenesulfonate, lecithin, etc.
[0024] The mass fraction of the first liquid phase: the second liquid phase: the third liquid phase = (0, 30%]:(0, 30%]:(0, 50%], In the second liquid phase, the mass fraction is resin:solvent:hardener:nonionic surfactant=(0, 80%]:(0, 90%]:[0, 30%]:(0, 20%], In the third liquid phase, the mass fraction of oil:surfactant is (0, 90%):(0, 30%).
[0025] In step 2, the dried sample is placed in a reactor, the temperature is raised to 800°C to 1300°C, and the sample is kept at 800°C to 1300°C for 0.5 to 15 hours for high-temperature carbonization to obtain a non-graphitizable carbon matrix with a particle size in the range of 1 μm to 100 μm. Here, as the reaction device, specifically, a general reaction device such as a high-temperature reaction furnace is selected.
[0026] In step 3, a pore-forming gas source is continuously introduced into the obtained non-graphitizable carbon matrix at 600°C to 1000°C for 1 hour to 10 hours to subject the non-graphitizable carbon matrix to a pore-forming treatment, thereby obtaining a porous non-graphitizable carbon matrix material, Here, the hole-forming gas source is one or a combination of oxygen, carbon dioxide, and water vapor, and the gas flow rate of the hole-forming gas source is 2 L / min to 20 L / min.
[0027] In step 4, vapor deposition is performed on the obtained porous non-graphitizable carbon matrix material to obtain a composite material for a lithium-ion secondary battery; Here, the gas source for vapor phase deposition includes a silicon-containing gas and one or more gaseous compounds containing any of the elements C, N, B, and P.
[0028] The protective gas for vapor deposition is one of nitrogen gas or argon gas or a combination thereof, the flow rate is 1-5 L / min, the gas flow rate of the gaseous compound is 0.5-10 L / min, the flow rate of the silicon-containing gas is 0.5-10 L / min, the deposition temperature is 500-1500°C, and the deposition time is 1-20 hours.
[0029] The silicon-containing gas is a silane compound and includes one or a combination of monosilane, trisilane, dichlorosilane, trichlorosilane, and tetrachlorosilane; The gaseous compound containing a C element includes one or more of acetylene, methane, propylene, ethylene, propane, and gaseous ethanol; The gaseous compound containing an N element includes at least one of nitrogen, ammonia, urea, and melamine, The gaseous compound containing the B element includes one or more of diborane, trimethyl borate, tripropyl borate, and boron tribromide; The gaseous compound containing the element P includes phosphine and / or phosphorus oxychloride.
[0030] The composite material for lithium ion secondary batteries prepared in the present invention can be used as a negative electrode material for lithium ion batteries.
[0031] In order to better understand the technical solution of the present invention, several specific examples are given below to describe the specific process of preparing a composite material for lithium ion secondary batteries using the method according to the above embodiment of the present invention, and the application method and battery characteristics thereof in lithium ion secondary batteries.
[0032] [Example 1] This embodiment provides a method for preparing a composite material for a lithium-ion secondary battery, which includes the following steps: In step 1, vegetable oil is used as the first liquid phase, phenolic resin is dissolved in alcohol, alkyl glucoside and ethylenediamine are added to prepare the second liquid phase, and oils containing stearic acid are used as the third liquid phase. The first liquid phase is slowly added to the second liquid phase, and after stirring for 1 hour, the stirred mixture is added to the third liquid phase and stirred to obtain the desired emulsion, which is heated to 130°C while continuing to stir, and kept warm for 1 hour until the resin hardens, forming hollow resin microspheres, which are then centrifuged, washed and dried. In step 2, the dried sample is placed in a reactor, the temperature is raised to 800° C., and the temperature is maintained for 0.5 hours, so that the dried sample is subjected to high-temperature carbonization treatment to obtain a non-graphitizable carbon matrix having a particle size of 10.8 μm. In step 3, the non-graphitizable carbon matrix obtained in step 2 is subjected to a pore-forming treatment, the gas source used is oxygen, the flow rate is 2 L / min, the pore-forming temperature is 600°C, and the time is 10 hours. In step 4, nitrogen gas is used as a protective gas and / or carrier gas at a flow rate of 1 L / min, the porous carbon obtained in step 3 is used as a matrix, and monosilane, a silicon-containing gas, is used as a silicon source. The gas is introduced into a reaction vessel together with methane, a compound containing C element, in the form of gas to perform vapor phase deposition, the monosilane gas flow rate is 0.5 L / min, and the methane gas flow rate is 0.5 L / min. The deposition temperature is 500°C, and the deposition time is 20 hours, to obtain a composite material for lithium-ion secondary batteries.
[0033] 2 is a SEM image of the cross section of the composite material for lithium ion secondary batteries prepared in Example 1 of the present invention. The SEM image of the cross section shows that there is a large cavity in the central region inside the material, which provides a large buffer space for the expansion of silicon while providing an abundance of pores.
[0034] The resulting material was used as the negative electrode material.
[0035] The obtained negative electrode material, carbon black as a conductive additive, and adhesive (1:1 sodium cellulose and styrene butadiene rubber) are weighed in a ratio of 95:2:3. A slurry is prepared in a beater at room temperature. The prepared slurry is evenly applied onto copper foil. After drying for 2 hours in a blower dryer at a temperature of 50°C, it is cut into pole pieces of 8 x 8 mm and dried for 10 hours in a vacuum dryer at a temperature of 100°C under vacuum. The dried pole pieces are immediately transferred into a glove box and prepared for battery assembly.
[0036] The assembly of the simulated battery was carried out in a glove box containing a high-purity Ar atmosphere, with lithium metal as the counter electrode and 1 mol / L LiPF 6 The battery was assembled using an ethylene carbonate (EC) / dimethyl carbonate (DMC) solution containing the above as the electrolyte. A constant current charge / discharge mode test was performed using a charger / discharger, with the discharge end voltage being 0.005 V and the charge end voltage being 1.5 V, and the charge / discharge test was performed at a current density of C / 10. The results are shown in Table 1.
[0037] [Example 2] This embodiment provides a method for preparing a composite material for a lithium-ion secondary battery, comprising the following steps: In step 1, vegetable oil is used as the first liquid phase, phenolic resin is dissolved in alcohol, alkyl glucoside and ethylenediamine are added to prepare the second liquid phase, and oils containing stearic acid are used as the third liquid phase. The first liquid phase is slowly added to the second liquid phase, and after stirring for 1 hour, the stirred mixture is added to the third liquid phase and stirred to obtain the desired emulsion, which is heated to 80°C while continuing to stir, and kept warm for 24 hours until the resin hardens, forming hollow resin microspheres, which are then centrifuged, washed and dried. In step 2, the dried sample is placed in a reactor, the temperature is raised to 1300°C, and the temperature is maintained for 0.5 hours, so that the dried sample is subjected to high-temperature carbonization treatment to obtain a non-graphitizable carbon matrix having a particle size of 12.1 μm. In step 3, the non-graphitizable carbon matrix obtained in step 2 is subjected to a pore-forming treatment, the gas source used is a combination of carbon dioxide and water vapor, the flow rate is 20 L / min, the pore-forming temperature is 1000°C, and the time is 1 hour. In step 4, argon gas is used as a protective gas and / or carrier gas, the flow rate is 1.5 L / min, the porous carbon obtained in step 3 is used as a matrix, trisilane, a silicon-containing gas, is used as a silicon source, and is introduced into a reaction vessel in gas form together with ammonia, a compound containing an N element, to perform vapor phase deposition, the flow rate of trisilane is 0.8 L / min, and the flow rate of the ammonia-containing gas is 0.8 L / min. The deposition temperature is 600° C., and the deposition time is 12.5 hours.
[0038] The button battery was assembled according to the method of Example 1 above, and the electrochemical properties were measured and evaluated under the same test conditions. The results are shown in Table 1.
[0039] [Example 3] This embodiment provides a method for preparing a composite material for a lithium-ion secondary battery, which includes the following steps: In step 1, mineral oil is used as the first liquid phase, phenolic resin is dissolved in alcohol, alkyl glucoside and metaxylenediamine are added to prepare the second liquid phase, and oils containing stearic acid are used as the third liquid phase. The first liquid phase is slowly added to the second liquid phase and stirred for 3 hours, after which the stirred mixture is added to the third liquid phase and stirred to obtain the desired emulsion. The mixture is heated to 100°C while continuing to stir, and kept warm for 4 hours until the resin hardens, forming hollow resin microspheres, which are then centrifuged, washed and dried. In step 2, the dried sample is placed in a reactor, the temperature is raised to 800°C, and the temperature is maintained for 5 hours to subject the dried sample to high-temperature carbonization treatment, thereby obtaining a non-graphitizable carbon matrix with a particle size of 13.5 μm. In step 3, the non-graphitizable carbon matrix obtained in step 2 is subjected to a pore-forming treatment, the gas source used is water vapor, the flow rate is 2 L / min, the pore-forming temperature is 1000°C, and the time is 10 hours. In step 4, nitrogen gas is used as a protective gas and / or carrier gas, the flow rate is 2 L / min, the porous carbon obtained in step 3 is used as a matrix, dichlorosilane, a silicon-containing gas, is used as a silicon source, and is introduced into a reaction vessel in gas form together with tripropyl borate, a compound containing B element, to perform vapor phase deposition, the gas flow rate of dichlorosilane is 1 L / min, and the gas flow rate of tripropyl borate is 1 L / min. The deposition temperature is 700° C., and the deposition time is 10 hours.
[0040] A button battery was assembled according to the method of Example 1 above, and its electrochemical properties were measured and evaluated under the same test conditions. The results are shown in Table 1.
[0041] [Example 4] This embodiment provides a method for preparing a composite material for a lithium-ion secondary battery, which includes the following steps: In step 1, vegetable oil is used as the first liquid phase, phenolic resin is dissolved in alcohol, alkyl glucoside and ethylenediamine are added to prepare the second liquid phase, and oils containing stearic acid are used as the third liquid phase. The first liquid phase is slowly added to the second liquid phase, and after stirring for 1 hour, the stirred mixture is added to the third liquid phase and stirred to obtain the desired emulsion, which is heated to 130°C while continuing to stir, and kept warm for 5 hours until the resin hardens, forming hollow resin microspheres, which are then centrifuged, washed and dried. In step 2, the dried sample is placed in a reactor, the temperature is raised to 1000°C, and the temperature is maintained for 6 hours to subject the dried sample to high-temperature carbonization treatment, thereby obtaining a non-graphitizable carbon matrix with a particle size of 9.2 μm. In step 3, the non-graphitizable carbon matrix obtained in step 2 is subjected to a pore-forming treatment, the gas source used is carbon dioxide, the flow rate is 2 L / min, the pore-forming temperature is 950° C., and the time is 6 hours. In step 4, argon gas is used as a protective gas and / or carrier gas, the flow rate is 2.5 L / min, the porous carbon obtained in step 3 is used as a matrix, trichlorosilane, a silicon-containing gas, is used as a silicon source, and is introduced into a reaction vessel in gas form together with phosphorus oxychloride, a compound containing P element, to perform vapor phase deposition, the gas flow rate of trichlorosilane is 1.25 L / min, and the gas flow rate of phosphorus oxychloride gaseous compound is 1.25 L / min. The deposition temperature is 800°C, and the deposition time is 8 hours.
[0042] A button battery was assembled according to the method of Example 1 above, and its electrochemical properties were measured and evaluated under the same test conditions. The results are shown in Table 1.
[0043] [Example 5] This embodiment provides a method for preparing a composite material for a lithium-ion secondary battery, which includes the following steps: In step 1, paraffin oil is used as the first liquid phase, phenolic resin is dissolved in alcohol, alkyl glucoside and ethylenediamine are added to prepare the second liquid phase, and oils containing stearic acid are used as the third liquid phase. The first liquid phase is slowly added to the second liquid phase and stirred for 1 hour, and the stirred mixture is added to the third liquid phase and stirred to obtain the desired emulsion. The mixture is heated to 130°C while continuing to stir, and kept warm for 10 hours until the resin hardens, forming hollow resin microspheres, which are then centrifuged, washed and dried. In step 2, the dried sample is placed in a reactor, the temperature is raised to 800°C, and the temperature is maintained for 2 hours, so that the dried sample is subjected to high-temperature carbonization treatment to obtain a non-graphitizable carbon matrix having a particle size of 15.1 μm. In step 3, the non-graphitizable carbon matrix obtained in step 2 is subjected to a pore-forming treatment, the gas source used is carbon dioxide, the flow rate is 5 L / min, the pore-forming temperature is 800° C., and the time is 2 hours. In step 4, nitrogen gas is used as a protective gas and / or carrier gas, the flow rate is 3L / min, the porous carbon obtained in step 3 is used as a matrix, and silicon-containing gas tetrachlorosilane is used as a silicon source, which is introduced into a reaction vessel in gas form together with gaseous compounds containing C, N, B and P elements, methane, ammonia, trimethyl borate and phosphorus oxychloride, to perform vapor phase deposition, the gas flow rate of tetrachlorosilane is 2L / min, and the flow rates of methane, ammonia, trimethyl borate and phosphorus oxychloride gaseous compounds are all 0.5L / min. The deposition temperature is 900°C, and the deposition time is 5 hours.
[0044] A button battery was assembled according to the method of Example 1 above, and its electrochemical properties were measured and evaluated under the same test conditions. The results are shown in Table 1.
[0045] [Example 6] This embodiment provides a method for preparing a composite material for a lithium-ion secondary battery, which includes the following steps: In step 1, vegetable oil is used as the first liquid phase, phenolic resin is dissolved in alcohol, alkyl glucoside and ethylenediamine are added to prepare the second liquid phase, and oils containing stearic acid are used as the third liquid phase. The first liquid phase is slowly added to the second liquid phase and stirred for 1 hour, and the stirred mixture is added to the third liquid phase and stirred to obtain the desired emulsion. While continuing to stir, the mixture is heated to 130°C and kept at this temperature for 14 hours until the resin hardens, forming hollow resin microspheres, which are then centrifuged, washed and dried. In step 2, the dried sample is placed in a reactor, the temperature is raised to 1300°C, and the temperature is kept for 2 hours to subject the dried sample to high-temperature carbonization treatment, thereby obtaining a non-graphitizable carbon matrix with a particle size of 8.5 μm. In step 3, the non-graphitizable carbon matrix obtained in step 2 is subjected to a pore-forming treatment, the gas source used is oxygen, the flow rate is 2 L / min, the pore-forming temperature is 900° C., and the time is 2 hours. In step 4, argon gas is used as a protective gas and / or carrier gas, the flow rate is 3.5 L / min, the porous carbon obtained in step 3 is used as a matrix, monosilane and trisilane, which are silicon-containing gases, are used as silicon sources, and are introduced into a reaction vessel in gas form together with propylene, urea, tripropyl borate, and phosphine, which are gaseous compounds containing C, N, B, and P elements, to perform vapor phase deposition, the gas flow rates of monosilane and trisilane are 1.25 L / min, and the gas flow rates of propylene, urea, tripropyl borate, and phosphine gaseous compounds are all 0.6 L / min. The deposition temperature is 1000° C., and the deposition time is 4 hours.
[0046] A button battery was assembled according to the method of Example 1 above, and its electrochemical properties were measured and evaluated under the same test conditions. The results are shown in Table 1.
[0047] [Example 7] This embodiment provides a method for preparing a composite material for a lithium-ion secondary battery, which includes the following steps: In step 1, vegetable oil is used as the first liquid phase, phenolic resin is dissolved in alcohol, polysorbate and metaxylenediamine are added to prepare the second liquid phase, and oils containing stearic acid are used as the third liquid phase. The first liquid phase is slowly added to the second liquid phase and stirred for 1 hour, and the stirred mixture is added to the third liquid phase and stirred to obtain the desired emulsion. The mixture is heated to 130°C while continuing to stir, and kept warm for 5 hours until the resin hardens, forming hollow resin microspheres, which are then centrifuged, washed and dried. In step 2, the dried sample is placed in a reactor, the temperature is raised to 900°C, and the temperature is kept for 2 hours to subject the dried sample to high-temperature carbonization treatment, thereby obtaining a non-graphitizable carbon matrix with a particle size of 13.8 μm. In step 3, the non-graphitizable carbon matrix obtained in step 2 is subjected to a pore-forming treatment, the gas source used is one or a combination of two of oxygen, carbon dioxide and water vapor, the pore-forming temperature is 1000°C, and the time is 5 hours. In step 4, nitrogen gas is used as a protective gas and / or carrier gas, the flow rate is 4 L / min, the porous carbon obtained in step 3 is used as a matrix, and silicon-containing gases monosilane, trisilane and dichlorosilane are used as silicon sources, which are introduced into a reaction vessel in gas form together with propane, hydrazine, diborane and phosphine, which are compounds containing C, N, B and P elements, to perform vapor phase deposition, the gas flow rates of monosilane, trisilane and dichlorosilane are all 1.3 L / min, and the gas flow rates of propane, hydrazine, diborane and phosphine are all 0.5 L / min. The deposition temperature is 1100° C., and the deposition time is 2.5 hours.
[0048] A button battery was assembled according to the method of Example 1 above, and its electrochemical properties were measured and evaluated under the same test conditions. The results are shown in Table 1.
[0049] [Example 8] This embodiment provides a method for preparing a composite material for a lithium-ion secondary battery, which includes the following steps: In step 1, vegetable oil is used as the first liquid phase, phenolic resin is dissolved in alcohol, fatty acid glyceride and ethylenediamine are added to prepare the second liquid phase, and oils containing stearic acid are used as the third liquid phase. The first liquid phase is slowly added to the second liquid phase, and after stirring for 1 hour, the stirred mixture is added to the third liquid phase and stirred to obtain the desired emulsion. While continuing to stir, the mixture is heated to 80°C to 130°C, and kept warm for 12 hours until the resin hardens, forming hollow resin microspheres, which are then centrifuged, washed and dried. In step 2, the dried sample is placed in a reactor, the temperature is raised to 1200°C, and the temperature is kept for 5 hours to subject the dried sample to high-temperature carbonization treatment, thereby obtaining a non-graphitizable carbon matrix with a particle size of 15.8 μm. In step 3, the non-graphitizable carbon matrix obtained in step 2 is subjected to a pore-forming treatment, the gas source used is water vapor, the flow rate is 5 L / min, the pore-forming temperature is 1000°C, and the time is 1.5 hours. In step 4, argon gas is used as a protective gas and / or carrier gas, the flow rate is 4.5L / min, the porous carbon obtained in step 3 is used as a matrix, and silicon-containing gases monosilane, trisilane and trichlorosilane are used as silicon sources, which are introduced into a reaction vessel in gas form together with ethanol, nitrogen, trimethyl borate and phosphorus oxychloride, which are compounds containing C, N, B and P elements, to perform vapor phase deposition, the gas flow rates of monosilane, trisilane and trichlorosilane are all 1.7L / min, and the gas flow rates of ethanol, nitrogen, trimethyl borate and phosphorus oxychloride gaseous compounds are 1.25L / min. The deposition temperature is 1200°C, and the deposition time is 2 hours.
[0050] A button battery was assembled according to the method of Example 1 above, and its electrochemical properties were measured and evaluated under the same test conditions. The results are shown in Table 1.
[0051] [Example 9] This example provides a method for preparing a composite material for a lithium-ion secondary battery, comprising the following steps: Includes In step 1, vegetable oil is used as the first liquid phase, phenolic resin is dissolved in alcohol, alkyl glucoside and trimethylhexamethylenediamine are added to prepare the second liquid phase, oils containing sodium dodecylbenzenesulfonate are used as the third liquid phase, the first liquid phase is slowly added to the second liquid phase, and after stirring for 1 hour, the stirred mixture is added to the third liquid phase and stirred to obtain the desired emulsion, which is heated to 100°C while continuing to stir, and kept warm for 6 hours until the resin hardens, forming hollow resin microspheres, which are then centrifuged, washed and dried. In step 2, the dried sample is placed in a reactor, the temperature is raised to 900°C, and the temperature is maintained for 6 hours, so that the dried sample is subjected to high-temperature carbonization treatment to obtain a non-graphitizable carbon matrix with a particle size of 14.5 μm. In step 3, the non-graphitizable carbon matrix obtained in step 2 is subjected to a pore-forming treatment, the gas source used is carbon dioxide, the flow rate is 10 L / min, the pore-forming temperature is 1000°C, and the time is 1 hour. In step 4, nitrogen gas is used as a protective gas and / or carrier gas, the flow rate is 5L / min, the porous carbon obtained in step 3 is used as a matrix, and silicon-containing gases trisilane, dichlorosilane and trichlorosilane are used as silicon sources, which are introduced into a reaction vessel in gas form together with ethylene, propane, urea, melamine, tripropyl borate, boron tribromide, phosphine and phosphorus oxychloride, which are compounds containing C, N, B and P elements, to perform vapor phase deposition, the gas flow rates of trisilane, dichlorosilane and trichlorosilane are all 2.7L / min, and the gas flow rates of ethylene, propane, urea, melamine, tripropyl borate, boron tribromide, phosphine and phosphorus oxychloride gaseous compounds are all 1L / min. The deposition temperature is 1400°C, and the deposition time is 1.25 hours.
[0052] A button battery was assembled according to the method of Example 1 above, and its electrochemical properties were measured and evaluated under the same test conditions. The results are shown in Table 1.
[0053] [Example 10] This embodiment provides a method for preparing a composite material for a lithium-ion secondary battery, which includes the following steps: In step 1, vegetable oil is used as the first liquid phase, phenolic resin is dissolved in alcohol, alkyl glucoside and ethylenediamine are added to prepare the second liquid phase, and oils containing stearic acid are used as the third liquid phase. The first liquid phase is slowly added to the second liquid phase, and after stirring for 1 hour, the stirred mixture is added to the third liquid phase and stirred to obtain the desired emulsion, which is heated to 130°C while continuing to stir, and kept warm for 2 hours until the resin hardens, forming hollow resin microspheres, which are then centrifuged, washed and dried. In step 2, the dried sample is placed in a reactor, the temperature is raised to 900°C, and the temperature is kept at 1000°C for 6 hours, so that the dried sample is subjected to high-temperature carbonization treatment to obtain a non-graphitizable carbon matrix with a particle size of 16.2 μm. In step 3, the non-graphitizable carbon matrix obtained in step 2 is subjected to a pore-forming treatment, the gas source used is one or a combination of two of oxygen, carbon dioxide and water vapor, the pore-forming temperature is 800°C, and the time is 5 hours. Step 4: Argon gas is used as a protective gas and / or carrier gas, the flow rate is 5L / min, the porous carbon obtained in step 3 is used as a matrix, silicon-containing gases dichlorosilane, trichlorosilane and tetrachlorosilane are used as silicon sources, and are introduced into a reaction vessel in gas form together with acetylene, propane, ammonia, hydrazine, tripropyl borate, boron tribromide, phosphine and phosphorus oxychloride, which are compounds containing C, N, B and P elements, to perform vapor phase deposition, the gas flow rates of dichlorosilane, trichlorosilane and tetrachlorosilane are all 3.3L / min, and the gas flow rates of acetylene, propane, ammonia, hydrazine, tripropyl borate, boron tribromide, phosphine and phosphorus oxychloride gaseous compounds are all 1.3L / min. The deposition temperature is 1500°C, and the deposition time is 1 hour.
[0054] A button battery was assembled according to the method of Example 1 above, and its electrochemical properties were measured and evaluated under the same test conditions. The results are shown in Table 1.
[0055] For easier comparison, comparative samples were prepared according to the following method.
[0056] [Comparative Example 1] This comparative example provides a method for preparing a silicon-carbon composite material based on the prior art, which includes the following steps: (1) Silicon particles, polyvinylpyrrolidone as a precursor of the carbon source, graphite, and citric acid as an antioxidant are added to an ethanol system, and ground in a mass ratio of 1:1:1:0.1 to obtain a dispersion. (2) The dispersion is spray-dried to obtain silicon-carbon powder. (3) The powder is then vapor-coated to finally obtain a silicon-carbon composite material.
[0057] A button battery was assembled according to the method of Example 1 above, and its electrochemical properties were measured and evaluated under the same test conditions. The results are shown in Table 1.
[0058] [Table 1]
[0059] From the comparison between the comparative examples and the examples, it can be seen that the silicon-containing porous hollow non-graphitizable carbon composite material provided by the present invention has higher specific capacity and first cycle Coulombic efficiency. At the same time, the present invention can further improve the first cycle Coulombic efficiency of the material by adjusting the deposition time, temperature and gas flow rate. The present invention scientifically sets the gas flow rate and temperature during preparation to avoid the gas flow rate and temperature being too high, which causes the silane to decompose too quickly and deposit directly on the surface of the carbon matrix, affecting the performance of the battery. At the same time, it also avoids the temperature being too low, which causes the silane to decompose incompletely, affecting the capacity of the battery.
[0060] Nanosilicon in the composite material for lithium ion secondary batteries according to the embodiment of the present invention and one or more gaseous compounds containing any of C, N, B, and P elements are uniformly dispersed in the pores of the spherical porous carbon by vapor deposition. The porous structure limits the size and uniform dispersion of nanosilicon after deposition, suppresses the effect of volume expansion, and avoids the problem of poor electrical contact due to pulverization of silicone, while having a large hole in the center provides a large buffer space due to the expansion of the silicon material, making it difficult for the structure of the entire composite material to be destroyed by expansion. Therefore, when lithium insertion and extraction reactions are sufficiently performed with respect to silicon, the structure of the composite material can be kept intact, and the electrochemical properties of the battery are further improved. In the case of multi-element composite, C and N are beneficial for improving the cycle characteristics of the material, and B and P are beneficial for improving the rate characteristics of the material. The composite material for lithium ion batteries provided by the present invention can be used in lithium ion batteries with liquid, semi-solid, quasi-solid, and all-solid electrolytes. In addition, the multi-element composite further improves the specific capacity and the coulombic efficiency of the first cycle.
[0061] The above specific embodiments further describe the objectives, technical solutions and beneficial effects of the present invention. The above are only specific embodiments of the present invention, and are not intended to limit the protection scope of the present invention. Any modifications, equivalent replacements, improvements, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
[0062] (Additional Note) (Appendix 1) A composite material for a lithium ion secondary battery, comprising: The composite material is a spherical porous non-graphitizable carbon material having hollow pores therein, and a product (including silicon nanoparticles) formed by decomposition of a silicon-containing gas and one or more gaseous compounds containing any one of C, N, B, and P elements is deposited inside the pores, The porous non-graphitizable carbon material is prepared by hardening a non-graphitizable carbon matrix by a double emulsion method, and then carbonizing the hardened non-graphitizable carbon matrix. A composite material comprising:
[0063] (Appendix 2) The silicon content in the composite material is 1 wt% to 70 wt%; 2. The composite material according to claim 1 .
[0064] (Appendix 3) The particle size range of the composite material is 1 μm to 100 μm, the average pore size is 0.1 nm to 10 nm, and the diameter of the hollow pores is 0.5 μm to 80 μm. 2. The composite material according to claim 1 .
[0065] (Appendix 4) The non-graphitizable carbon matrix of the spherical porous non-graphitizable carbon material is one or a combination of a phenolic resin, an epoxy resin, a furfural resin, or a polybutadiene resin; The silicon-containing gas is a silane compound and includes one or a combination of monosilane, trisilane, dichlorosilane, trichlorosilane, and tetrachlorosilane; The gaseous compound containing a C element includes one or more of acetylene, methane, propylene, ethylene, propane, and gaseous ethanol; The gaseous compound containing the N element includes at least one of nitrogen, ammonia, urea, and melamine, The gaseous compound containing the B element includes one or more of diborane, trimethyl borate, tripropyl borate, and boron tribromide; The gaseous compound containing the P element includes phosphine and / or phosphorus oxychloride. 2. The composite material according to claim 1 .
[0066] (Appendix 5) A method for preparing a composite material for a lithium ion secondary battery according to any one of claims 1 to 4, comprising the steps of: Step 1: Using pure oil as the first liquid phase, dissolving resin in the corresponding solvent, adding non-ionic surfactant and curing agent to prepare the second liquid phase, and using oil containing surfactant as the third liquid phase, slowly adding the first liquid phase to the second liquid phase, stirring for 0.5-1 hour, then adding the stirred mixture to the third liquid phase, stirring to obtain the desired emulsion, heating to 80-130°C while continuing to stir, and keeping warm for 1-24 hours until the resin is cured, forming resin hollow microspheres, then centrifuging, washing and drying; Step 2: Put the dried sample into a reactor, heat the temperature to 800°C to 1300°C, and keep the temperature at 800°C to 1300°C for 0.5 hours to 15 hours to perform high-temperature carbonization treatment, thereby obtaining a non-graphitizable carbon matrix having a particle size in the range of 1 μm to 100 μm; Step 3: continuously introducing a pore-forming gas source into the obtained non-graphitizable carbon matrix at 600°C to 1000°C for 1 hour to 10 hours to subject the non-graphitizable carbon matrix to a pore-forming treatment to obtain a porous non-graphitizable carbon matrix material, in which the pore-forming gas source is one or a combination of two of oxygen, carbon dioxide and water vapor, and the gas flow rate of the pore-forming gas source is 2L / min to 20L / min; Step 4: performing vapor deposition on the obtained porous non-graphitizable carbon matrix material to obtain a composite material for a lithium ion secondary battery, the gas source for the vapor deposition including a silicon-containing gas and one or more gaseous compounds including any one of C, N, B, and P elements; Including, A preparation method comprising the steps of:
[0067] (Appendix 6) The protective gas for the vapor deposition is one of nitrogen gas or argon gas or a combination thereof, and the flow rate is 1-5 L / min, the gas flow rate of the gaseous compound is 0.5-10 L / min, the flow rate of the silicon-containing gas is 0.5-10 L / min, the deposition temperature is 500-1500°C, and the deposition time is 1-20 hours; The preparation method according to claim 5,
[0068] (Appendix 7) The resin comprises one or a combination of a phenolic resin, an epoxy resin, a furfural resin, or a polybutadiene resin; The solvent comprises one or a combination of ethanol, acetone, and toluene; The oils include one or more combinations of vegetable oil, paraffin oil, mineral oil, etc. The nonionic surfactant comprises one or more combinations of alkylglucosides, fatty acid glycerides, sorbitan fatty acid esters, and polysorbates; The curing agent includes one or a combination of trimethylhexamethylenediamine, ethylenediamine, and metaxylenediamine; The surfactant may include one or more of the following: stearic acid, sodium dodecylbenzenesulfonate, lecithin, etc. The silicon-containing gas is a silane compound and includes one or a combination of monosilane, trisilane, dichlorosilane, trichlorosilane, and tetrachlorosilane; The gaseous compound containing a C element includes one or more of acetylene, methane, propylene, ethylene, propane, and gaseous ethanol; The gaseous compound containing the N element includes at least one of nitrogen, ammonia, urea, and melamine, The gaseous compound containing the B element includes one or more of diborane, trimethyl borate, tripropyl borate, and boron tribromide; The gaseous compound containing the P element includes phosphine and / or phosphorus oxychloride. The preparation method according to claim 5,
[0069] (Appendix 8) The mass fraction of the first liquid phase: the second liquid phase: the third liquid phase = (0, 30%]:(0, 30%]:(0, 50%], In the second liquid phase, the mass fraction is resin:solvent:hardener:nonionic surfactant=(0, 80%]:(0, 90%]:[0, 30%]:(0, 20%], In the third liquid phase, the mass fraction of oil:surfactant is (0, 90%]: (0, 30%]. The preparation method according to claim 5,
[0070] (Appendix 9) The composite material for a lithium ion secondary battery according to any one of claims 1 to 4 is included. A negative electrode material for a lithium-ion battery.
[0071] (Appendix 10) The composite material for a lithium ion secondary battery according to any one of claims 1 to 4 is included. A lithium-ion battery characterized by:
Claims
1. A composite material for a lithium ion secondary battery, comprising: The composite material is a spherical porous non-graphitizable carbon material having hollow pores therein, and a product (including silicon nanoparticles) formed by decomposition of a silicon-containing gas and one or more gaseous compounds containing any one of C, N, B, and P elements is deposited inside the pores; The porous non-graphitizable carbon material is prepared by hardening a non-graphitizable carbon matrix by a double emulsion method, and then carbonizing the hardened non-graphitizable carbon matrix. A composite material comprising:
2. The silicon content in the composite material is 1 wt % to 70 wt %; 2. The composite material of claim 1 .
3. The particle size range of the composite material is 1 μm to 100 μm, the average pore size is 0.1 nm to 10 nm, and the diameter of the hollow pores is 0.5 μm to 80 μm.
2. The composite material of claim 1 .
4. The non-graphitizable carbon matrix of the spherical porous non-graphitizable carbon material is one or a combination of a phenolic resin, an epoxy resin, a furfural resin, or a polybutadiene resin; The silicon-containing gas is a silane compound and includes one or a combination of a plurality of monosilane, trisilane, dichlorosilane, trichlorosilane, and tetrachlorosilane; The gaseous compound containing a C element includes one or more of acetylene, methane, propylene, ethylene, propane, and gaseous ethanol; The gaseous compound containing the N element includes at least one of nitrogen, ammonia, urea, and melamine, The gaseous compound containing the B element includes one or more of diborane, trimethyl borate, tripropyl borate, and boron tribromide; The gaseous compound containing the P element includes phosphine and / or phosphorus oxychloride.
2. The composite material of claim 1 .
5. A method for preparing the composite material for a lithium ion secondary battery according to any one of claims 1 to 4, comprising the steps of: Step 1: using pure oil as the first liquid phase, dissolving resin in a corresponding solvent, adding non-ionic surfactant and curing agent to prepare a second liquid phase, and using oil containing surfactant as the third liquid phase; slowly adding the first liquid phase to the second liquid phase, stirring for 0.5-1 hour, then adding the stirred mixture to the third liquid phase, stirring to obtain a desired emulsion, heating to 80-130°C while continuing to stir, and keeping warm for 1-24 hours until the resin is cured, forming hollow resin microspheres, which are then centrifuged, washed and dried; Step 2: Put the dried sample into a reactor, heat the sample to 800°C to 1300°C, and hold the sample at 800°C to 1300°C for 0.5 to 15 hours to perform high-temperature carbonization treatment to obtain a non-graphitizable carbon matrix having a particle size in the range of 1 μm to 100 μm; Step 3: continuously introducing a pore-forming gas source into the obtained non-graphitizable carbon matrix at 600°C to 1000°C for 1 hour to 10 hours to subject the non-graphitizable carbon matrix to a pore-forming treatment to obtain a porous non-graphitizable carbon matrix material, in which the pore-forming gas source is one or a combination of two of oxygen, carbon dioxide and water vapor, and the gas flow rate of the pore-forming gas source is 2L / min to 20L / min; Step 4: performing vapor deposition on the obtained porous non-graphitizable carbon matrix material to obtain a composite material for a lithium ion secondary battery, the gas source for the vapor deposition including a silicon-containing gas and one or more gaseous compounds including any one of C, N, B, and P elements; Including, A preparation method comprising the steps of:
6. The protective gas for the vapor deposition is one of nitrogen gas or argon gas or a combination thereof, and the flow rate is 1-5 L / min, the gas flow rate of the gaseous compound is 0.5-10 L / min, the flow rate of the silicon-containing gas is 0.5-10 L / min, the deposition temperature is 500-1500° C., and the deposition time is 1-20 hours; 6. The method according to claim 5 .
7. The resin comprises one or a combination of a phenolic resin, an epoxy resin, a furfural resin, or a polybutadiene resin; The solvent comprises one or a combination of ethanol, acetone, and toluene; The oils include one or more combinations of vegetable oil, paraffin oil, mineral oil, etc. The non-ionic surfactant comprises one or more combinations of alkylglucosides, fatty acid glycerides, sorbitan fatty acid esters, and polysorbates; The curing agent includes one or a combination of two or more of trimethylhexamethylenediamine, ethylenediamine, and metaxylenediamine, The surfactant may include one or more combinations of stearic acid, sodium dodecylbenzenesulfonate, lecithin, etc. The silicon-containing gas is a silane compound and includes one or a combination of a plurality of monosilane, trisilane, dichlorosilane, trichlorosilane, and tetrachlorosilane; The gaseous compound containing a C element includes one or more of acetylene, methane, propylene, ethylene, propane, and gaseous ethanol; The gaseous compound containing the N element includes at least one of nitrogen, ammonia, urea, and melamine, The gaseous compound containing the B element includes one or more of diborane, trimethyl borate, tripropyl borate, and boron tribromide; The gaseous compound containing the P element includes phosphine and / or phosphorus oxychloride.
6. The method according to claim 5 .
8. The mass fraction of the first liquid phase: the second liquid phase: the third liquid phase = (0, 30%]: (0, 30%]: (0, 50%], In the second liquid phase, the mass fraction is resin:solvent:hardener:nonionic surfactant=(0,80%]:(0,90%]:[0,30%]:(0,20%], In the third liquid phase, the mass fraction of oil:surfactant is (0, 90%]: (0, 30%).
6. The method according to claim 5 .
9. The composite material for lithium ion secondary batteries according to any one of claims 1 to 4 is included. A negative electrode material for a lithium-ion battery.
10. The composite material for lithium ion secondary batteries according to any one of claims 1 to 4 is included. A lithium-ion battery characterized by:
Citation Information
Patent Citations
Three-dimensional porous silicon-carbon composite material and preparation method and application thereof
CN113078318A
Negative electrode for secondary battery, copper foil for electrode, secondary battery, and process for producing the negative electrode for secondary battery
JP2010282959A
Silicon-carbon composite anode material
WO2020099589A1
Electroactive materials for metal-ion batteries
WO2020128495A1