Secondary batteries and electrical appliances

The secondary battery design addresses lithium loss in lithium iron phosphate batteries by optimizing CB/PD ratios and particle sizes, improving cycle and shelf life through lithium balance and reduced energy loss.

JP2024542342AActive Publication Date: 2024-11-15SUNWODA MOBILITY ENERGY TECHNOLOGY CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2023581039
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2022-10-27
Filing Date
2022-12-30
Publication Date
2024-11-15
Estimated Expiration
2042-12-30

AI Technical Summary

Technical Problem

Lithium iron phosphate batteries face challenges in achieving a service life of 20-30 years due to lithium loss and SEI film degradation, leading to shortened lifespan, and existing lithium replenishment methods are costly and risky.

Method used

A secondary battery design optimizing the ratio of negative electrode capacity to positive electrode capacity (CB/PD) within specific ranges, combined with controlled particle sizes and additives in the electrolyte, to maintain lithium balance and improve cycle and shelf life.

Benefits of technology

The optimized battery design enhances cycle life and energy efficiency by maintaining active lithium levels, reducing energy loss, and preventing lithium precipitation, thereby extending battery life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024542342000001
    Figure 2024542342000001
  • Figure 2024542342000002
    Figure 2024542342000002
  • Figure 2024542342000003
    Figure 2024542342000003
Patent Text Reader

Abstract

This application discloses a secondary battery and an electrical appliance. The secondary battery includes a positive electrode sheet and a negative electrode sheet, and the secondary battery satisfies 0.258≦CB / PD≦0.700. This application appropriately controls the ranges of the CB value and the PD value to improve the cycle life and storage life of the secondary battery, improve the energy efficiency of the secondary battery, and reduce the energy loss during charging and discharging.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] This application claims priority to a Chinese patent application bearing application number 202211328888.2 and entitled "Secondary Battery and Electrical Appliance" filed with the China Patent Office on October 27, 2022, the entire contents of which are incorporated herein by reference.

[0002] The present application relates to the field of battery technology, and in particular to secondary batteries and electrical appliances. [Background technology]

[0003] Although lithium-ion batteries have great advantages in the field of energy storage, there are still some problems in their practical application. Take lithium iron phosphate batteries as an example. The service life of a lithium iron phosphate single battery is 4,000-6,000 times, which makes it difficult to meet the 20-30 year service life (more than 10,000 cycles) required for energy storage projects with high life requirements. The loss of active lithium is the cause of the life decay of energy storage lithium-ion batteries. During the cycle in which the battery absorbs and desorbs lithium, the expansion and contraction of graphite, the elution of positive electrode transition metals, etc., cause the breakage and formation of the SEI (solid electrolyte interphase), which increases the area and thickness of the SEI film, consuming the limited active lithium in the battery system, and ultimately shortening the service life of the battery. How to reduce and replenish the consumption of active lithium during the battery decay process is an important issue for improving the life of lithium iron phosphate batteries.

[0004] To solve these problems, a method of "lithium replenishment" is generally used for the negative electrode, and the method of lithium replenishment can be divided into physical lithium replenishment and electrochemical lithium replenishment. However, physical lithium replenishment is prone to lithium deposition in the battery during subsequent cycles, which can lead to short circuiting of the battery and pose a safety hazard. Although electrochemical lithium replenishment can compensate for the shortcomings of physical lithium replenishment, the current method has no significant effect, is not simple in process, is expensive, and is not suitable for practical production.

[0005] Therefore, there is a demand for the development of a secondary battery that has a long cycle life, excellent electrochemical properties, is easy to process and manufacture, and is inexpensive to use. Summary of the Invention [Problem to be solved by the invention]

[0006] An object of the present application is to provide a secondary battery having improved cycle life and storage life by adjusting the relationship between the CB value of the battery and the compressed density of the positive electrode sheet. [Means for solving the problem]

[0007] In a first aspect, an embodiment of the present application provides a secondary battery, the secondary battery including a positive electrode sheet and a negative electrode sheet, the secondary battery satisfying 0.258≦CB / PD≦0.700, where CB is a ratio of the capacity of the negative electrode sheet per unit area to the capacity of the positive electrode sheet per unit area, and PD is the compression density of the positive electrode sheet, expressed in g / cm. 3 It is.

[0008] In some embodiments, 0.275≦CB / PD≦0.55.

[0009] In some embodiments, 0.31≦CB / PD≦0.48.

[0010] In some embodiments, 0.8≦CB≦1.1.

[0011] In some embodiments, 0.8≦CB≦1.05.

[0012] In some embodiments, the compressed density PD of the positive electrode sheet is 1.5≦PD≦3.1 (g / cm 3 ) is satisfied.

[0013] The positive electrode sheet includes a positive electrode active material layer, the positive electrode active material layer includes a positive electrode active material material, the negative electrode sheet includes a negative electrode active material layer, the negative electrode active material layer includes a negative electrode active material material, and the positive electrode active material and the negative electrode active material satisfy 2≦Dv50′ / Dv50≦25, where Dv50′ is a particle size, in μm, corresponding to when a cumulative volume percentage of the negative electrode active material reaches 50%, and Dv50 is a particle size, in μm, corresponding to when a cumulative volume percentage of the positive electrode active material reaches 50%.

[0014] In some embodiments, the particle size of the negative electrode active material satisfies 5≦Dv50′≦25.

[0015] In some embodiments, the particle size of the positive electrode active material satisfies 0.3≦Dv50≦3.5.

[0016] In some embodiments, the particle size of the negative electrode active material satisfies 0.5≦Dv10′≦10, 2.5≦Dv90′≦45, Dv99′≦50, Dn10′≦4, 0.5≦Dn50′≦10.5, 1.5≦Dn90′≦25, Dn99′≦40, and the unit of particle size is μm.

[0017] In some embodiments, the particle size of the positive electrode active material satisfies 0.1≦Dv10≦1, 0.5≦Dv90≦6.5, 3.5≦Dv99≦20, 0.05≦Dn10≦1, 0.1≦Dn50≦2.5, 0.5≦Dn90≦3.5, or 1.5≦Dn99≦10, and the unit of particle size is μm.

[0018] In some embodiments, the positive electrode active material layer and the negative electrode active material layer satisfy 0≦(H1-H2) / H2≦0.9, where H1 is the thickness of the positive electrode active material layer on one side, the unit is μm, and H2 is the thickness of the negative electrode active material layer on one side, the unit is μm.

[0019] In some embodiments, 40≦H1≦160 and 30≦H2≦120 are satisfied.

[0020] In some embodiments, the chemical formula of the positive electrode active material is Li y A x Fe (1-x) PO4, where 0.8≦y≦1.2, 0<x<1, and the element A includes at least one of Ni, Co, Mn, Mg, Ca, Ba, Ti, and V.

[0021] In some embodiments, the element A accounts for 0% to 36% of the weight of the positive electrode active material.

[0022] The secondary battery includes an electrolyte, the electrolyte includes a first additive, and the first additive includes at least one of vinylene carbonate and vinyl ethylene carbonate.

[0023] The electrolyte includes a second additive, and the second additive includes at least one of LiFSI, LiODFB, LiPO2F2, LiBF4, and LiBOB.

[0024] In some embodiments, the first additive accounts for a% of the total weight of the electrolyte, where a, CB, and PD satisfy 0.2≦a×CB / PD≦3.

[0025] In some embodiments, the second additive accounts for b% of the total weight of the electrolyte. a and b satisfy at least one of the following characteristics. (I) 0.1≦a + b≦5; (II) 0.1≦a / b≦10.

[0026] In some embodiments, the secondary battery satisfies 1.1≦CB′≦1.3, where CB′ is the ratio of the reversible capacity of the negative electrode sheet per unit area to the actual capacity of the positive electrode sheet per unit area.

[0027] In a second aspect, the present invention further provides an electrical appliance including a secondary battery, the secondary battery being used as a power supply for the electrical appliance. Effect of the Invention

[0028] Compared with the prior art, the secondary battery of the present application includes a positive electrode sheet and a negative electrode sheet, and the secondary battery satisfies 0.258≦CB / PD≦0.700. By controlling the ratio of the battery design CB value and the positive electrode sheet PD value of the present application, the cycle and storage life of the secondary battery are improved, the energy efficiency of the secondary battery is improved, and the energy loss during the charging and discharging process is reduced. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0029] The present application provides a secondary battery and an electric appliance, and in order to make the purpose, technical solution and technical effects of the present application clearer and more specific, the present application will be described in more detail below with reference to examples. It should be understood that the specific examples described in the present specification are only for the purpose of illustrating the present application, and are not intended to limit the present application.

[0030] secondary battery

[0031] The present application provides a secondary battery, which includes a positive electrode sheet and a negative electrode sheet, and satisfies 0.258≦CB / PD≦0.700, where CB is the ratio of the capacity of the negative electrode sheet per unit area to the capacity of the positive electrode sheet per unit area, and PD is the compression density (g / cm) of the positive electrode sheet. 3 ).

[0032] In order to calculate the CB value, the unit area of ​​the positive and negative electrode sheets must be kept equal, and the CB value is the reversible capacity of the negative electrode sheet of the battery / the reversible capacity of the positive electrode sheet of the battery. The present application limits the value of the CB / PD ratio to balance the lithium ion desorption rate of the positive and negative electrode materials and improves the cycle and storage life of the secondary battery.

[0033] In some examples, the CB value is obtained by the following test method:

[0034] The capacity of the negative electrode sheet per unit area is obtained by the following method: leave one side of the active material on a unit area of ​​the negative electrode sheet, combine it with lithium pieces, a separator, and an electrolyte to form a button battery, discharge it at 0.1C to 0.005V, discharge it at 0.05mA to 0.005V, discharge it at 0.02mA to 0.005V, and charge it at 0.1C to 2V, and the resulting charge capacity is the capacity of the negative electrode sheet per unit area.

[0035] The capacity of the positive electrode sheet per unit area is obtained by the following method: leave one side of the active material on a unit area of ​​the positive electrode sheet, combine it with lithium pieces, a separator, and an electrolyte to form a button battery, charge it to 3.7 V at 0.1 C, keep the voltage constant to 50 μA, and discharge it to 2.0 V at 0.1 C, and the resulting discharge capacity is the capacity of the positive electrode sheet per unit area.

[0036] In some embodiments, the compressed density is calculated according to the following formula:

[0037] Compressed density = areal density / (thickness of sheet after rolling - thickness of current collector), unit is g / cm 3 It is.

[0038] In some embodiments, the compressed density of the positive electrode sheet can be calculated according to the following formula:

[0039] Compression density of positive electrode sheet = areal density of positive electrode sheet / (thickness of positive electrode sheet after rolling - thickness of positive electrode current collector), unit is g / cm 3 It is.

[0040] In some embodiments, the compressed density is tested by a compressed density meter, and the test process can refer to the international standard GB / T24533-2019.

[0041] In some embodiments, the value of CB / PD may be any one of the following values, or a range consisting of any two of the following values: 0.258, 0.28, 0.30, 0.32, 0.33, 0.341, 0.35, 0.353, 0.36, 0.367, 0.37, 0.38, 0.383, 0.39, 0.40, 0.41, 0.43, 0.45, 0.458, 0.47, 0.48, 0.50, 0.52, 0.54, 0.55, 0.57, 0.59, 0.60, 0.62, 0.64, 0.65, 0.67, 0.69, 0.70.

[0042] In some embodiments, the value of CB may be any one of the following values, or a range consisting of any two of the following values: 0.8, 0.81, 0.82, 0.821, 0.83, 0.845, 0.846, 0.85, 0.852, 0.86, 0.87, 0.88, 0.89, 0.896, 0.9, 0.91, 0.92, 0.93, 0.94, 0.95, 0.952, 0.958, 0.96, 0.97, 0.98, 0.99, 1.0, 1.05, 1.10.

[0043] The present application increases the reversible capacity of the battery positive electrode sheet through a redundant design of the positive electrode sheet, and adopts a constant capacity method through charging test control during the battery operation process to make the positive electrode sheet release only a portion of lithium ions, and uses the surplus lithium ions as reserve to compensate for the loss of active lithium during the operation process of the secondary battery, thereby keeping the active lithium within an appropriate range at all times and improving the recovery rate of storage capacity and energy efficiency.

[0044] In some embodiments, PD (g / cm 3 ) may be any one of 1.5, 1.6, 1.8, 1.9, 2.0, 2.2, 2.4, 2.5, 2.7, 2.8, 2.9, 3.0, and 3.1, or a range consisting of any two of these values.

[0045] In the present invention, the compressed density of the positive electrode sheet is further limited, thereby increasing the usable capacity of the battery and improving the cycle life of the battery. In the manufacturing process of lithium-ion batteries, the compressed density has a significant impact on the battery performance. Experiments have proven that the compressed density is closely related to the specific capacity, efficiency, internal resistance and battery cycle performance, so the compressed density is also one of the reference indicators of material energy density.

[0046] In some embodiments, the positive electrode active material particles Dv50 (unit: μm) and the negative electrode active material particles Dv50' (unit: μm) of the present application satisfy 2≦Dv50' / Dv50≦25.

[0047] In some embodiments, 5≦Dv50′ / Dv50≦25.

[0048] In some embodiments, 10≦Dv50′ / Dv50≦25.

[0049] In some embodiments, 14≦Dv50′ / Dv50≦25.

[0050] In some embodiments, Dv50' / Dv50 is 5.0, 5.5, 5.9, 6.0, 6.3, 6.5, 6.8, 7.0, 7.3, 7.8, 8.0, 8.3, 8.5, 8.8, 9.0, 9.1, 9.2, 9.3, 9.4, 9.5, 9.6, 9.7, 9.8, 9.9, 10.0, 10.1, 10.2, 10.3, 10.4, 10.5, 10.6, 10.7, 10.8, 10.9, 11.0, 11.1, 11.2, 11.3, 11.4, 11.5, 11.6, 11.7, 11.8, 11.9, 12.0, 12.1, 12.2, 12.3, 12.4, 12.5, 12.6, 12.7, 12.8, 12.9, 13.0, 13.1, 13.2, 13.3, 13.4, 13.5, 13.6, 13.7, 13.8, 13.9, 14.0, 14.1, 14.2, 14.3, 14.4, 14.5, 14.6, 14.7, 14.8, 14.9, 15.0, 15.1, 15.2, 15.3, 15.4, 15.5, 15.6, 15.7, 15.8, 15.9, 16.0, 16.1, 16. The range may be any one of 2.3, 12.5, 12.7, 13.0, 13.3, 13.5, 13.7, 13.9, 14.0, 14.3, 14.5, 14.8, 15.0, 15.3, 15.5, 15.7, 16.0, 16.3, 16.5, 16.7, 17.0, 17.3, 17.5, 17.7, 18.0, 18.3, 18.5, 18.7, 19.0, 19.3, 19.5, 19.9, 20.0, 20.5, 21.0, 21.5, 22.0, 23.0, 24.0, and 25.0, or a range consisting of any two of these values.

[0051] The present application further optimizes the particles of the positive electrode active material and the particles of the negative electrode active material to improve the matching of the lithium ion absorption / desorption rates of the positive and negative electrode active materials, thereby improving the cycle life of the secondary battery.

[0052] In some embodiments, the particle size of the positive electrode active material satisfies 0.3≦Dv50≦3.5, 0.1≦Dv10≦1.0, 0.5≦Dv90≦6.5, 3.5≦Dv99≦20, 0.1≦Dn50≦2.5, 0.05≦Dn10≦1.0, 0.5≦Dn90≦3.5, or 1.5≦Dn99≦10, and the unit of particle size is μm.

[0053] In some embodiments, the particle size Dv50 (μm) of the positive electrode active material may be any one of 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1.0, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9, 2.0, 2.1, 2.2, 2.3, 2.4, 2.5, 2.6, 2.7, 2.8, 2.9, 3.0, 3.1, 3.2, 3.3, 3.4, and 3.5, or a range consisting of any two of these values.

[0054] In some embodiments, the particle size of the negative electrode active material satisfies 5.0≦Dv50′≦25.0, 0.5≦Dv10′≦10.0, 2.5≦Dv90′≦45.0, Dv99′≦50.0, 0.5≦Dn50′≦10.5, Dn10′≦4.0, 1.5≦Dn90′≦25.0, or Dn99′≦40.0, and the unit of particle size is μm.

[0055] In some embodiments, the particle size Dv50′ (μm) of the negative electrode active material is 5.0, 5.5, 6.0, 6.3, 6.5, 6.7, 7.0, 7.3, 7.5, 7.8, 8.0, 8.3, 8.5, 8.8, 9.0, 9.3, 9.5, 9.8, 10.0, 10.3, 10.5, 10.8, 11.0, 11.3, 11.5, 11.8, 12.0, 12.3, 12.5, 12.8, 13.0, 14.0, 15.0, 16.0, 17.0, 18.0, 19.0, 20.0, 21.0, 22.0, 23.0, 24.0, 25.0, 26.0, 27.0, 28.0, 29.0, 30.0, 31.0, 32.0, 33.0, 34.0, 35.0, 36.0, 37.0, 38.0, 39.0, 40.0, 41.0, 42.0, 43.0, 44.0, 45.0, 46.0, 47.0, 48.0, 49.0, 50.0, 51.0, 52.0, 53.0, 54.0, 55.0, 56.0, 57.0, 58.0, 59.0, 60.0, 61.0, 62.0, 63.0, 64.0, 65.0, 66.0, 6 The value may be any one of 3.3, 13.5, 13.8, 14.0, 14.3, 14.5, 14.8, 15.0, 15.3, 15.5, 15.8, 16.0, 16.3, 16.5, 16.8, 17.0, 17.5, 18.0, 18.5, 19.0, 19.5, 20.0, 21.0, 22.0, 23.0, 24.0, or 25.0, or a range consisting of any two of these values.

[0056] The definitions of the particle size of the positive electrode material and the particle size of the negative electrode material in this application have the meanings well known in the art. Dv10' is the particle size corresponding to the cumulative volume percentage of the negative electrode active material particles reaching 10%. Dv50' is the particle size corresponding to the cumulative volume percentage of the negative electrode active material particles reaching 50%. Dv90' is the particle size corresponding to the cumulative volume percentage of the negative electrode active material particles reaching 90%. Dv99' is the particle size corresponding to the cumulative volume percentage of the negative electrode active material particles reaching 99%. Dn10' is the particle size corresponding to the distribution number of the negative electrode active material particles reaching 10%. Dn50' is the particle size corresponding to the distribution number of the negative electrode active material particles reaching 50%. Dn99' is the particle size corresponding to the distribution number of the negative electrode active material particles reaching 99%.

[0057] Dv10 is the particle size corresponding to the cumulative volume percentage of the positive electrode active material particles reaching 10%. Dv50 is the particle size corresponding to the cumulative volume percentage of the positive electrode active material particles reaching 50%. Dv90 is the particle size corresponding to the cumulative volume percentage of the positive electrode active material particles reaching 90%. Dv99 is the particle size corresponding to the cumulative volume percentage of the positive electrode active material particles reaching 99%. Dn10 is the particle size corresponding to the distribution number of the positive electrode active material particles reaching 10%. Dn50 is the particle size corresponding to the distribution number of the positive electrode active material particles reaching 50%. Dn99 is the particle size corresponding to the distribution number of the positive electrode active material particles reaching 99%.

[0058] In some embodiments, the positive electrode active material layer (the thickness of the active material on one side, H1, in μm) and the negative electrode active material layer (the thickness of the active material on one side, H2, in μm) satisfy 0≦(H1-H2) / H2≦0.9. When the thicknesses of the positive electrode active material layer and the negative electrode active material layer are within this range, the consistency of the lithium ion desorption rate of the positive and negative electrode materials is improved, and the cycle life of the secondary battery is improved.

[0059] In some embodiments, (H1 - H2) / H2 may be any one of 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, or a range consisting of any two of these values.

[0060] In some embodiments, 40 ≤ H1 ≤ 160 is satisfied.

[0061] In some embodiments, H1 (unit: μm) may be any one of 40, 50, 60, 70, 80, 90, 100, 110, 120, 130, 140, 150, 160, or a range consisting of any two of these values.

[0062] In some embodiments, 30 ≤ H2 ≤ 120 is satisfied.

[0063] In some embodiments, H2 (unit: μm) may be any one of 30, 40, 50, 60, 70, 80, 90, 100, 110, 120, or a range consisting of any two of these values.

[0064] In some embodiments, the chemical formula of the positive electrode active material is Li y A x Fe (1-x) PO4, where 0.8 ≤ y ≤ 1.2 and 0 < x < 1, and the element A contains at least one of Ni, Co, Mn, Mg, Ca, Ba, Ti, V.

[0065] In some embodiments, the content of element A in the lithium-containing compound of the positive electrode active material is appropriate, whereby high energy density and stability can be imparted to the positive electrode active material particles, and the electrical use device can have better comprehensive performance.

[0066] In some embodiments, element A accounts for 0% - 36% of the weight of the positive electrode active material.

[0067] In some embodiments, element A may comprise 1% by weight, 2% by weight, 3% by weight, 4% by weight, 5% by weight, 6% by weight, 7% by weight, 8% by weight, 9% by weight, 10% by weight, 11% by weight, 12% by weight, 13% by weight, 14% by weight, 15% by weight, 16% by weight, 17% by weight, 18% by weight, 19% by weight, 20% by weight, 21% by weight, 22% by weight, 23% by weight, 24% by weight, 25% by weight, 26% by weight, 27% by weight, 28% by weight, 29% by weight, 30% by weight, 31% by weight, 32% by weight, 33% by weight, 34% by weight, 35% by weight, 36% by weight of the cathode active material, or a range consisting of any two of these values.

[0068] In the present application, by adding element A to the positive electrode active material and limiting the content of element A, the working voltage platform of the secondary battery is improved, the energy density is improved, and the kinetics of the positive electrode material is improved, thereby improving the cycle life and energy efficiency of the secondary battery.

[0069] In some embodiments, a secondary battery includes an electrolyte, the electrolyte includes a first additive, the first additive includes at least one of vinylene carbonate and vinyl ethylene carbonate, and the content of the first additive is a% based on the total weight of the electrolyte.

[0070] In some embodiments, the electrolyte includes a second additive, the second additive including at least one of LiFSI, LiODFB, LiPO2F2, LiBF4, and LiBOB, and the content of the second additive is b% based on the total weight of the electrolyte.

[0071] In some embodiments, 0.2≦a*CB / PD≦3.

[0072] In some embodiments, 0.1≦a+b≦5.

[0073] In some embodiments, 0.1≦a / b≦10.

[0074] In some embodiments, the value of a*CB / PD may be any one of the following values, or a range consisting of any two of the following values: 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1.0, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9, 2.0, 2.1, 2.2, 2.3, 2.4, 2.5, 2.6, 2.7, 2.8, 2.9, 3.0.

[0075] In some embodiments, the value of a+b may be any of the following values: 0.1, 0.5, 0.8, 1.0, 1.3, 1.5, 1.8, 2.0, 2.3, 2.5, 2.8, 3.0, 3.3, 3.5, 3.8, 4.0, 4.3, 4.5, 4.8, 5.0, or a range consisting of any two of these values.

[0076] In some embodiments, the value of a / b may be any of the following values, or a range consisting of any two of the following values: 0.1, 0.3, 0.5, 0.7, 0.9, 1.0, 1.3, 1.5, 1.7, 2.0, 2.3, 2.5, 2.8, 3.0, 3.3, 3.5, 3.7, 4.0, 4.3, 4.5, 4.8, 5.0, 5.3, 5.5, 5.8, 6.0, 6.3, 6.5, 7.0, 7.3, 7.5, 7.8, 8.0, 8.3, 8.5, 8.8, 9.0, 9.3, 9.5, 9.7, 10.0.

[0077] In the present invention, by ensuring sufficient amounts of the first additive and the second additive throughout the entire life cycle of the secondary battery, accelerated capacity decay due to insufficient amounts of additives is not caused.

[0078] In some embodiments, due to the relative excess of positive electrode capacity, a constant capacity charging method is used during the operation of the secondary battery to prevent lithium deposition on the negative electrode during the charging process from affecting the life and safety performance of the secondary battery.

[0079] In some embodiments, the secondary battery is charged at n1 / n2 (unit: A) for n2 hours during charging in the pre-cycle period, where n2≧0.5, where n1 is the nominal capacity of the secondary battery, i.e., the actual usage capacity, in Ah, and n2 is the charging time of the secondary battery, in h.

[0080] The nominal capacity is the standard capacity determined at the time of shipment of the battery.

[0081] In some embodiments, the secondary battery satisfies 1.10≦n4 / n1≦1.3, 0.8≦n4 / n3≦1.1, where n3 is the positive electrode reversible capacity of the secondary battery, also in Ah, and n4 is the negative electrode reversible capacity of the secondary battery, also in Ah.

[0082] In some embodiments, the actual use CB' value is 1.10≦CB'≦1.30, ie, the reversible capacity of the negative electrode of the battery / the actual capacity of the positive electrode of the battery is in the range of 1.10 to 1.30.

[0083] In some embodiments, the CB' value may be any one of 1.10, 1.11, 1.12, 1.13, 1.14, 1.15, 1.16, 1.17, 1.18, 1.19, 1.20, 1.21, 1.22, 1.23, 1.24, 1.25, 1.26, 1.27, 1.28, 1.29, 1.30, or a range consisting of any two of these values.

[0084] In some embodiments, the positive electrode sheet includes a positive electrode current collector and a positive electrode active material disposed on the positive electrode current collector.

[0085] In some examples, the positive electrode active material can be one or more of lithium iron phosphate, lithium cobalt oxide, lithium nickel oxide, or lithium manganese oxide.

[0086] In some embodiments, the cathode active material is lithium iron phosphate, lithium cobalt oxide, lithium nickel oxide, and lithium manganese oxide, and the manufacturing method thereof may be a high temperature solid-state method, a carbothermal reduction method, a spray drying method, a template method, or a hydrothermal synthesis method.

[0087] Specifically, lithium iron phosphate, which is a positive electrode active material, can be prepared by the following method: A lithium source (Li2CO3), an iron source (FePO4), and a carbon source are mixed and pre-treated at 300°C to 500°C, and then sintered at 600°C to 850°C to prepare lithium iron phosphate, which is used as a positive electrode active material.

[0088] In some embodiments, the cathode active material is lithium cobalt oxide and the method of manufacture may be conventional techniques such as high temperature solid state methods, sol-gel methods, and the like.

[0089] Specifically, the positive electrode active material lithium cobalt oxide can be prepared by the following method: A lithium source (Li2CO3), a cobalt source (Co3O4), and ethanol are mixed and ground, pretreated at 300°C, sintered at 600°C, and then reacted in a solid state at 800°C to obtain lithium cobalt oxide.

[0090] In some embodiments, in order to obtain a cathode active material having an optimized particle size distribution and specific surface area, an intermediate product obtained in the manufacturing process of the cathode active material is crushed and sieved. Here, the crushing method is not particularly limited and can be selected according to actual requirements, for example, a particle crusher is used. The manufacturing method of the cathode active material of the present application is not limited to the above manufacturing method, and may be any method as long as the formed cathode active material has the characteristics described in the present application.

[0091] In some embodiments, the manufacturing process for the positive electrode sheet can include steps such as stirring, coating, drying, cold pressing, slitting, and sheeting.

[0092] In some embodiments, the positive electrode sheet further includes a conductive agent and a binder, and the type and content of the conductive agent and the binder are not particularly limited and can be selected according to actual requirements. In some embodiments, the conductive agent can include conductive carbon black, carbon nanotubes, graphene, etc., and the binder can include polyvinylidene fluoride.

[0093] In some embodiments, the method for producing the positive electrode sheet includes dispersing the positive electrode active material, the conductive agent, and the binder in a specific ratio in N-methylpyrrolidone (NMP), coating the resulting slurry on an aluminum foil, drying, and then cold pressing and slitting to obtain a positive electrode sheet.

[0094] Negative electrode sheet

[0095] In some embodiments, the negative electrode sheet includes a negative electrode current collector, a negative electrode active material covering the negative electrode current collector, a binder, and a conductive agent. The types and contents of the negative electrode active material, the binder, and the conductive agent are not particularly limited and can be selected according to actual requirements. In some embodiments, the negative electrode active material includes one or more of artificial graphite, natural graphite, mesocarbon microbeads, amorphous carbon, lithium titanate, or silicon carbon alloy. The negative electrode active material should also have characteristics such as high compressed density, high mass-specific capacity, and high volume-specific capacity.

[0096] electrolyte

[0097] In some embodiments, the main components of the electrolyte include a lithium salt, an organic solvent, and an additive. Here, the types and compositions of the lithium salt and the organic solvent are not particularly limited and can be selected according to actual requirements. Here, the lithium salt can include lithium hexafluorophosphate, and the solvent can include ethylene carbonate, methyl ethyl carbonate, dimethyl carbonate, propyl propionate, etc.

[0098] Separator

[0099] In some embodiments, the type of the separator is not particularly limited and can be selected according to actual requirements. The separator can be a polypropylene film, a polyethylene film, a polyvinylidene fluoride film, a spandex film, an aramid film, or a multi-layer composite film after coating modification.

[0100] In some embodiments, the secondary battery is manufactured by stacking a positive electrode sheet, a separator, and a negative electrode sheet in order, with the separator located between the positive electrode sheet and the negative electrode sheet to play the role of insulation, then winding it around a square bare electric core, placing it in a battery housing, baking it at 65°C to 95°C to remove water, then injecting electrolyte and sealing it, and going through processes such as standing, hot and cold pressing, chemical formation, clamping, and volume separation to obtain a secondary battery.

[0101] In some embodiments, the fabrication of a secondary battery includes the following steps. (1) Lithium iron phosphate, a positive electrode conductive agent, a positive electrode binder, and a positive electrode solvent are mixed to prepare a positive electrode slurry, and the positive electrode slurry is applied to the surface of a positive electrode current collector to obtain a positive electrode sheet. (2) Graphite, anode dispersant, anode conductive agent, anode binder and anode solvent are mixed to prepare anode slurry, which is then applied to the surface of anode current collector to obtain anode sheet. (3) In the manufacturing process of the lithium ion battery, the positive electrode sheet, negative electrode sheet, separator and other battery parts manufactured in the present application are assembled, and then undergo processes such as shaping, sintering, sealing, liquid injection, chemical formation, and capacity separation to obtain a lithium iron phosphate lithium ion battery with a long life, and the battery types include soft pack, cylindrical, aluminum housing, etc., where the design CB value of the battery satisfies 0.8≦CB≦1.10, that is, the reversible capacity of the negative electrode sheet of the battery / the reversible capacity of the positive electrode sheet of the battery is 0.8-1.10, and satisfies 0.258≦battery design CB / positive electrode sheet PD≦0.700, 2.0≦negative electrode Dv50' / positive electrode Dv50≦25.

[0102] In some embodiments, during the use of the battery, the charging rules of the battery are optimized and the charging capacity of the battery is strictly controlled, so that the actual use CB value of the battery is stabilized at 1.10-1.30, that is, the reversible capacity of the negative electrode sheet of the battery / the actual capacity of the positive electrode sheet of the battery is 1.10-1.30.

[0103] In some embodiments, the secondary battery includes a lithium ion battery. Although only soft-pack lithium ion batteries are given above as examples, the present application is not limited to applications to soft-pack batteries, but also includes applications to common lithium ion battery configurations such as aluminum housing batteries, cylindrical batteries, etc.

[0104] Electrical equipment

[0105] In some embodiments, the present application provides an electrical appliance including the above-mentioned secondary battery, and the electrical appliance may be used in, but is not limited to, a backup power source, a motor, an electric vehicle, an electric motorcycle, an electric-assisted bicycle, a bicycle, an electric tool, a large-scale household battery, and the like.

[0106] Example 1

[0107] A positive electrode slurry is prepared by mixing lithium iron phosphate, a positive electrode conductive agent, a positive electrode binder, and a positive electrode solvent, and the positive electrode slurry is applied to the surface of a positive electrode current collector to obtain a positive electrode sheet.

[0108] The manufacturing method of the positive electrode sheet is as follows: Lithium iron phosphate, conductive carbon black (SP), polyvinylidene fluoride (PVDF) are mixed in a weight ratio of 97:0.7:2.3, then they are added to NMP and mixed thoroughly, and after uniform mixing, they are coated on both sides of a (12+1+1)μm carbon aluminum foil, then the sheet is dried, rolled, stripped, and cut into pieces to obtain a positive electrode sheet, the thickness of the positive electrode active material layer on one side is 81μm, and the particle diameter of lithium iron phosphate is Dv50 (0.67μm), Dv10 (0.15μm), Dv90 (5.5μm), Dv99 (9.2μm), Dn50 (0.33μm), Dn10 (0.10μm), Dn90 (1.15μm), Dn99 (3.20μm).

[0109] Graphite, anode dispersant, anode conductive agent, anode binder and anode solvent are mixed to prepare anode slurry, which is then applied to the surface of anode current collector to obtain anode sheet.

[0110] The manufacturing method of the negative electrode sheet is as follows: Graphite, conductive carbon black (SP), carboxymethyl cellulose (CMC), and styrene-butadiene rubber (SBR) are mixed in a mass ratio of 96.3:0.7:1.1:1.9, then thoroughly mixed in water, and after uniform mixing, the mixture is applied to two surfaces of 6μm copper foil, and then the sheet is dried, rolled, slit, and cut to obtain a negative electrode sheet, the thickness of the negative electrode active material layer on one side is 65μm, and the particle diameter of the negative electrode active material is Dv50' (16.3μm), Dv10' (8.5μm), Dv90' (30.2μm), Dv99' (40.4μm), Dn50' (8.2μm), Dn10' (3.1μm), Dn90' (15.2μm), and Dn99' (25.3μm).

[0111] The separator is a polyethylene film.

[0112] The preparation method of the electrolyte is as follows: Vinylene carbonate, methyl ethyl carbonate, and dimethyl carbonate are mixed in a mass ratio of 1:1:1, and then lithium hexafluorophosphate is added, mixed uniformly, and additives are added. Here, based on the mass of the electrolyte, the content of lithium hexafluorophosphate is 12%, and the content of the additive vinylene carbonate is 0.5%.

[0113] In the manufacturing process of a lithium-ion battery, the positive electrode sheet, negative electrode sheet, separator and other battery components manufactured in the present application are assembled, and then undergo processes such as shaping, firing, sealing, electrolyte injection, chemical formation and capacity separation to obtain a lithium iron phosphate lithium-ion battery having a long life.

[0114] The preparation of Examples 2 to 16 is as follows: the particle size of the active material is screened to obtain active material materials with different particle sizes, the coating weight of the active material material of the positive electrode sheet and the negative electrode sheet is adjusted to control the design CB value, and the rolling thickness of the active material layer is adjusted to control the compression density, and Examples 2 to 16 are prepared according to the method of Example 1, and the parameters of Examples 2 to 16 are shown in Table 1.

[0115] Battery performance testing

[0116] The cycle capacity retention rate is as follows: The nominal capacity of the secondary battery is C1, and the battery is cycled at a specific temperature (25°C, 45°C, 60°C) at 1C / 1C for the corresponding number of cycles to obtain the discharge capacity C2, and the capacity retention rate is C2 / C1 x 100%.

[0117] Energy efficiency is the ratio of the energy output during discharge of a lithium-ion battery to the energy input during the previous charge.

[0118] The energy efficiency test method is as follows:

[0119] The secondary battery is charged to the battery's nominal capacity at a constant current of 1C, the charging energy is E1, left for 30 minutes, and then discharged to the lower voltage limit (2.5V) at a constant current of 1C, the discharging energy is E2, and the energy efficiency value of the secondary battery is E2 / E1.

[0120] The test method for the recovery rate of storage capacity is as follows.

[0121] At room temperature, charge the secondary battery at a constant current of 1C up to the battery's nominal capacity of X1Ah.

[0122] The secondary battery is transferred to a 60°C oven and stored for 400 days. At room temperature, the secondary battery is discharged to 2.5V at 1C and left for 30 minutes. Then, the secondary battery is charged to 3.65V at 1C constant current and constant voltage, and the cut-off current is 0.05C. After leaving for 30 minutes, the secondary battery is discharged to 2.5V at 1C constant current. The discharge capacity is X2Ah, and the capacity recovery rate of the secondary battery is X2 / X1×100%.

[0123] [Table 1]

[0124] Referring to the results in Table 1, when the battery design CB / positive electrode sheet PD is within the range of 0.258-0.700 and Dv50' / Dv50 is within the range of 2-25, particularly when Dv50' / Dv50 shown in Examples 1-16 is limited to the range of 14-25, the consistency of the lithium ion desorption rate of the positive and negative electrode materials is improved, and the cycle life of the secondary battery is improved. When the battery design CB / positive electrode sheet PD is within the range of 0.258-0.700 and the range of Dv50' / Dv50 is not within the above range, a mismatch in the desorption rate of the positive and negative electrodes occurs, and the cycle life of the battery is insufficient. When Dv50' / Dv50 is within the range of 2.0-20 and the battery design CB / positive electrode sheet PD is not within the range of 0.258-0.700, the cycle and storage life of the secondary battery are not satisfied, and the cycle life of the battery cannot be extended. In the present application, the actual use CB value is limited to the range of 1.1 to 1.3, so that the negative electrode can ensure that it has an appropriate amount of lithium vacancies during operation. If the actual use CB value is greater than 1.3, the negative electrode will have excess lithium vacancies during operation, and excessive active lithium will be consumed in the process of generating SEI, which is disadvantageous to improving cycle life / storage life. If the actual use CB value is less than 1.1, the negative electrode will have insufficient lithium vacancies during operation, causing lithium precipitation, which will increase side reactions of the secondary battery and affect the cycle storage life.

[0125] Comparing the battery test results in the above table, the long-life lithium iron phosphate lithium-ion battery manufactured in this application is obviously superior to the ordinary lithium iron phosphate lithium-ion battery without a positive electrode redundant design in terms of cycle capacity retention rate at 25°C 1C / 1C and 45°C 1C / 1C, storage capacity recovery rate at 60°C 100% SOC, and energy efficiency.

[0126] Examples 17 to 20 are produced by the following method.

[0127] A positive electrode slurry is prepared by mixing lithium iron phosphate, a positive electrode conductive agent, a positive electrode binder, and a positive electrode solvent, and the positive electrode slurry is applied to the surface of a positive electrode current collector to obtain a positive electrode sheet.

[0128] The manufacturing method of the positive electrode sheet is as follows: Lithium iron phosphate, conductive carbon black (SP), polyvinylidene fluoride (PVDF) are mixed in a weight ratio of 96.7:0.9:2.4, then they are added to NMP and mixed thoroughly, and after uniform mixing, they are coated on both sides of a (12+1+1)μm carbon aluminum foil, then the sheet is dried, rolled, slit and cut to obtain a positive electrode sheet, and the thickness of the positive electrode active material layer on one side is 81μm.

[0129] The manufacturing method of the negative electrode sheet is as follows: Graphite, conductive carbon black (SP), carboxymethyl cellulose (CMC), and styrene-butadiene rubber (SBR) are mixed in a mass ratio of 96.1:0.7:1.1:2.1, then thoroughly mixed in water, and after uniform mixing, the mixture is applied to two surfaces of 6μm copper foil, and then the sheet is dried, rolled, slit and cut to obtain the negative electrode sheet, and the thickness of the negative electrode active material layer on one side is 65μm.

[0130] The separator is a polyethylene film.

[0131] The production method was the same as in Example 1, with the difference being the amount of vinylene carbonate shown in Table 2.

[0132] In the manufacturing process of a lithium ion battery, the positive electrode sheet, negative electrode sheet, separator and other battery components manufactured in the present application are assembled, and then undergo processes such as shaping, firing, sealing, liquid injection, chemical formation and capacity separation to obtain a lithium lithium ion battery.

[0133] [Table 2]

[0134] The a value in different embodiments can be obtained by adjusting the amount of the first additive in the electrolyte. In the present application, by controlling the relationship between the first additive a, CB and PD in the electrolyte, a*CB / PD is ensured to be within the range of 0.2-3, and the content of the first additive is ensured to be sufficient during the entire life cycle of the secondary battery, and the acceleration of capacity decay due to insufficient additive amount does not occur. If a*CB / PD is greater than 3, the film of the negative electrode SEI becomes too thick, the system dynamics of the secondary battery is deteriorated, and the risk of lithium precipitation in the room temperature cycle increases, which is unfavorable to the room temperature cycle life. If a*CB / PD is less than 0.2, the film thickness of the negative electrode SEI becomes insufficient, the consumption of the negative electrode active lithium in the cycle process increases, and the cycle becomes poor; therefore, at the same time, the range of the actual use CB value needs to meet 1.10-1.30, thereby ensuring that there are suitable lithium vacancies in the negative electrode and improving the life of the battery.

[0135] Comparing the battery test results in the above table, the long-life lithium iron phosphate lithium-ion battery manufactured according to the present application by controlling the values ​​of a, PD and a*CB1 / PD based on the positive electrode redundancy design is obviously superior to the ordinary lithium iron phosphate lithium-ion battery without the positive electrode redundancy design in terms of 25°C 1C / 1C, 45°C 1C / 1C cycle capacity retention rate, 60°C 100% SOC storage capacity recovery rate and energy efficiency.

[0136] Examples 21 to 24 are all produced by the following method.

[0137] A positive electrode slurry is prepared by mixing lithium iron phosphate, a positive electrode conductive agent, a positive electrode binder, and a positive electrode solvent, and the positive electrode slurry is applied to the surface of a positive electrode current collector to obtain a positive electrode sheet.

[0138] The manufacturing method of the positive electrode sheet is as follows: Lithium iron phosphate, conductive carbon black (SP), polyvinylidene fluoride (PVDF) are mixed in a weight ratio of 97.3:0.5:2.2, then they are added to NMP and mixed thoroughly, and after uniform mixing, they are coated on both sides of a (12+1+1)μm carbon aluminum foil, then the sheet is dried, rolled, slit and cut to obtain a positive electrode sheet, and the thickness of the positive electrode active material layer on one side is 81μm.

[0139] The manufacturing method of the negative electrode sheet is as follows: Graphite, conductive carbon black (SP), carboxymethyl cellulose (CMC), and styrene-butadiene rubber (SBR) are mixed in a mass ratio of 96.5:0.5:1.2:1.8, then thoroughly mixed in water, and after uniform mixing, the mixture is applied to two surfaces of 6μm copper foil, and then the sheet is dried, rolled, slit and cut to obtain the negative electrode sheet, and the thickness of the negative electrode active material layer on one side is 65μm.

[0140] Graphite, anode dispersant, anode conductive agent, anode binder and anode solvent are mixed to prepare anode slurry, which is then applied to the surface of anode current collector to obtain anode sheet.

[0141] The preparation method of the electrolyte is as follows: Vinylene carbonate, methyl ethyl carbonate, and propyl propionate are mixed in a mass ratio of 1:1:1, and then lithium hexafluorophosphate is added, mixed uniformly, and additives are added. Here, based on the mass of the electrolyte, the content of lithium hexafluorophosphate is 12%, the first additive is vinylene carbonate, and the second additive is lithium bis(oxalato)borate, and the contents of the first additive and the second additive are as shown in Table 3.

[0142] In the manufacturing process of a lithium-ion battery, the positive electrode sheet, negative electrode sheet, separator and other battery components manufactured in the present application are assembled, and then undergo processes such as shaping, firing, sealing, electrolyte injection, chemical formation and capacity separation to obtain a lithium iron phosphate lithium-ion battery having a long life.

[0143] [Table 3]

[0144] As shown in Table 3, the above values ​​of a and b can be obtained by adjusting the amount of the first additive and the second additive, and when a+b is within this range, the amount of the film-forming additive in the negative electrode is sufficient, and the cycle life and storage life can be ensured; and when a / b is within this range, the cycle life and storage life of the secondary battery can be improved and the energy efficiency can be ensured. Comparing the battery test results shown in the above table, the long-life lithium iron phosphate lithium-ion battery manufactured by controlling the values ​​of a, a+b and a / b based on the positive electrode redundancy design of the present application is obviously superior to the ordinary lithium iron phosphate lithium-ion battery without the positive electrode redundancy design in terms of 25°C 1C / 1C, 45°C 1C / 1C cycle capacity retention rate, 60°C 100% SOC storage capacity recovery rate, and energy efficiency.

[0145] In the above embodiments, the description of each embodiment has its own focus, and the parts of the embodiments that are not described in detail may be referred to the relevant descriptions of other embodiments.

[0146] Although the secondary battery and the electrical appliance according to the embodiment of the present application have been described in detail above, the present specification describes the principle and the embodiment of the present application by applying specific examples, and the description of the above examples is intended to help understand the method and the core idea of ​​the present application. In addition, it should be understood that a person skilled in the art may make modifications in the specific embodiments and the scope of application in light of the idea of ​​the present application, and the contents of the present specification are not intended to limit the present application.

Claims

1. A secondary battery comprising a positive electrode sheet and a negative electrode sheet, the secondary battery satisfying 0.258≦CB / PD≦0.700; Here, CB is the ratio of the capacity of the negative electrode sheet per unit area to the capacity of the positive electrode sheet per unit area, PD is the compressed density of the positive electrode sheet, and its unit is g / cm 3 That is, Secondary battery.

2. 0.275≦CB / PD≦0.55 is satisfied; The secondary battery according to claim 1 .

3. 0.31≦CB / PD≦0.48 is satisfied; The secondary battery according to claim 1 .

4. 0.8≦CB≦1.1 is satisfied; The secondary battery according to claim 1 .

5. 1.5≦PD≦3.1 is satisfied; The secondary battery according to any one of claims 1 to 4.

6. the positive electrode sheet includes a positive electrode active material layer, the positive electrode active material layer includes a positive electrode active material, the negative electrode sheet includes a negative electrode active material layer, and the negative electrode active material layer includes a negative electrode active material, the positive electrode active material and the negative electrode active material satisfy 2≦Dv50′ / Dv50≦25, Here, Dv50' is the particle size corresponding to when the cumulative volume percentage of the negative electrode active material reaches 50%, and is expressed in μm. Dv50 is the particle size corresponding to when the cumulative volume percentage of the positive electrode active material reaches 50%, and is expressed in μm. The secondary battery according to claim 1 .

7. The positive electrode active material layer and the negative electrode active material layer have a structure in which 0≦(H 1 -H 2 ) / H 2 ≦0.9 is satisfied, Here, H 1 is the thickness of the positive electrode active material layer on one side, in μm, H 2 is the thickness of the negative electrode active material layer on one side, in μm; The secondary battery according to claim 6.

8. The secondary battery includes an electrolyte, the electrolyte includes a first additive, and the first additive includes at least one of vinylene carbonate and vinyl ethylene carbonate. The secondary battery according to claim 1 .

9. The electrolyte solution includes a second additive, and the second additive is LiFSI, LiODFB, LiPO 2 F 2 , LiBF 4 , LiBOB; The secondary battery according to claim 8.

10. The first additive accounts for a% of the total weight of the electrolyte, where a, CB, and PD satisfy 0.2≦a×CB / PD≦3; The secondary battery according to claim 8.

11. The second additive accounts for b% of the total weight of the electrolyte; a and b satisfy at least one of the following characteristics: (I) 0.1≦a+b≦5; (II) 0.1≦a / b≦10, The secondary battery according to claim 10.

12. The particle size of the negative electrode active material satisfies 5≦Dv50′≦25, and the particle size of the positive electrode active material satisfies 0.3≦Dv50≦3.

5. The secondary battery according to claim 6.

13. The particle diameter of the negative electrode active material satisfies 0.5≦Dv10′≦10, 2.5≦Dv90′≦45, Dv99′≦50, Dn10′≦4, 0.5≦Dn50′≦10.5, 1.5≦Dn90′≦25, and Dn99′≦40, and the unit of the particle diameter is μm. The secondary battery according to claim 6.

14. The particle diameter of the positive electrode active material satisfies 0.1≦Dv10≦1, 0.5≦Dv90≦6.5, 3.5≦Dv99≦20, 0.05≦Dn10≦1, 0.1≦Dn50≦2.5, 0.5≦Dn90≦3.5, and 1.5≦Dn99≦10, and the unit of the particle diameter is μm. The secondary battery according to claim 6.

15. 40≦H 1 ≦160, 30≦H 2 ≦120, The secondary battery according to claim 7.

16. A secondary battery comprising the secondary battery according to any one of claims 1 to 15. Electrical usage equipment.

Citation Information

Patent Citations

  • Lithium ion battery with long cycle performance

    CN104993135A

  • High-energy density lithium ion battery

    CN105047903A

  • Negative pole piece and battery

    CN109461880A

  • Lithium ion battery

    JP2016072226A

  • Secondary battery, battery module including said secondary battery, battery pack, and device

    JP2022534453A