Thermal nitridation of NH radicals to form metal silicon nitride films
The use of ammonia plasma to form NH radicals in titanium silicon nitride films addresses the challenge of silicon nitride formation in bit line contacts, resulting in a low-resistivity TiSiN film suitable for DRAMs, enhancing manufacturing efficiency.
Patent Information
- Application Number
- JP2024531299
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2022-11-28
- Filing Date
- 2022-11-30
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2042-11-30
AI Technical Summary
Current manufacturing methods for bit line contacts in integrated circuits face challenges with high contact resistance due to the formation of silicon nitride (SiN) during titanium silicon nitride (TiSiN) formation, which is difficult to deposit with high step coverage and reacts with silicon (Si) to form silicon nitride (SiN).
A method involving the use of ammonia (NH3) plasma to form NH radicals that diffuse through a titanium film, forming a titanium silicon nitride (TiSiN) film substantially free of silicon nitride (SiN) by heating the metal-silicon compound film to temperatures between 450°C and 1000°C, using a plasma processing apparatus.
The method results in a titanium silicon nitride (TiSiN) film with low resistivity and minimal silicon nitride content, suitable for bit line contacts in DRAMs, reducing contact resistance and improving manufacturing efficiency.
Smart Images

Figure 2024543156000001_ABST
Abstract
Description
[Technical field]
[0001]
[0001] Embodiments of the present disclosure relate to the field of electronic devices and electronic device manufacturing. More particularly, embodiments of the present disclosure provide electronic devices including metal silicon nitride films that are substantially free of silicon nitride (SiN), and methods of forming the same.
[0002]
[0002] [Background technology]
[0003]
[0003] Integrated circuits have evolved into complex devices that can contain millions of transistors, capacitors, and resistors on a single chip. During the evolution of integrated circuits, the functional density (i.e., the number of interconnected devices per chip area) has generally increased, while the feature size (i.e., the smallest component (or line) that can be made using a manufacturing process) has decreased.
[0004]
[0004] The density of integrated circuits on semiconductor substrates is increasing dramatically while minimum feature sizes, such as the channel length of field effect transistors (FETs) and the word line width of dynamic random access memories (DRAMs), are shrinking dramatically.
[0005] One difficulty with DRAM is that the bit line contacts are small metal-to-silicon contacts formed early in the process flow. The bit line contacts must be able to withstand high temperatures without the silicide agglomerating. Current manufacturing methods use tungsten nitride (WN) or nitrogen (N2) to react with titanium silicide (TiSi) in rapid thermal processing (RTP) to form titanium silicon nitride (TiSiN). However, tungsten nitride (WN) is difficult to deposit with high step coverage, and nitrogen (N2) reacts directly with silicon (Si) to form silicon nitride (SiN) on the substrate, leading to high contact resistance.
[0006] Therefore, there is a need in the art for a method of forming a bit line contact that results in minimal silicon nitride (SiN) formation during the formation of titanium silicon nitride (TiSiN). Summary of the Invention
[0007]
[0007] One or more embodiments of the present disclosure are directed to a method for forming a semiconductor device. In one or more embodiments, the method includes exposing a metal silicide film to a plasma containing ammonia (NH3) at a temperature ranging from 450° C. to 1000° C. to form NH radicals that diffuse through the metal silicide film and form a metal silicon nitride film that is substantially free of silicon nitride (SiN).
[0008]
[0008] Additional embodiments of the present disclosure are directed to a method of forming a semiconductor device. In one or more embodiments, the method includes exposing a titanium film to a plasma containing ammonia (NH3) at a temperature ranging from 450° C. to 1000° C. to form NH radicals that diffuse through the titanium film and form a titanium silicon nitride (TiSiN) film that is substantially free of silicon nitride (SiN).
[0009]
[0009] A further embodiment of the present disclosure is directed to a non-transitory computer readable medium comprising instructions that, when executed by a controller of a processing chamber, cause the processing chamber to perform a step of exposing a metal silicon nitride film to a plasma comprising ammonia (NH3) at a temperature in the range of 450°C to 1000°C to form NH radicals that diffuse through the metal silicon nitride film and form a metal silicon nitride film that is substantially free of silicon nitride (SiN).
[0010]
[0010] In order that the above-mentioned features of the present disclosure may be understood in detail, the present disclosure summarized above will now be more particularly described with reference to embodiments, some of which are illustrated in the accompanying drawings. It should be noted, however, that the accompanying drawings only illustrate exemplary embodiments of the present disclosure and therefore should not be considered as limiting the scope of the present disclosure, which may admit of other equally effective embodiments. The embodiments described herein are presented by way of example and are not limited to the figures of the accompanying drawings in which like references indicate similar elements. [Brief description of the drawings]
[0011] [Figure 1] FIG. 1 illustrates a process flow for film formation in accordance with one or more embodiments of the present disclosure. [Diagram 2] 1A-D are cross-sectional views illustrating an exemplary substrate during the formation of a film in accordance with one or more embodiments of the present disclosure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012]
[0013] Before describing several example embodiments of the present disclosure, it is to be understood that the present disclosure is not limited to the details of structure or process steps set forth in the following description as the present disclosure is capable of other embodiments and of being practiced or carried out in various ways.
[0013]
[0014] The term "substrate" as used herein and in the appended claims refers to a surface, or a portion of a surface, upon which a process acts. Additionally, unless the context clearly indicates otherwise, those skilled in the art will understand that a reference to a substrate may refer to only a portion of a substrate. Additionally, a reference to deposition on a substrate may refer to both a bare substrate and a substrate having one or more films or features deposited or formed thereon.
[0014]
[0015] As used herein, "substrate" refers to any substrate or material surface formed on a substrate on which a film treatment is performed during a manufacturing process. For example, substrate surfaces on which treatment may be performed include materials such as silicon, silicon oxide, strained silicon, silicon-on-insulator (SOI), carbon-doped silicon oxide, amorphous silicon, doped silicon, germanium, gallium arsenide, glass, sapphire, and any other materials such as metals, metal nitrides, metal alloys, and other conductive materials, depending on the application. Substrates include, but are not limited to, semiconductor wafers. Substrates may be exposed to pretreatment processes to polish, etch, reduce, oxidize, hydroxylate, anneal, and / or bake the substrate surface. In addition to performing film treatments directly on the surface of the substrate itself, in the present disclosure, any of the disclosed film treatment steps may be performed on an underlying layer formed on the substrate, as disclosed in more detail below, and the term "substrate surface" is intended to include such underlying layers as the context indicates. Thus, for example, when a film / layer or partial film / layer is deposited on a substrate surface, the exposed surface of the newly deposited film / layer becomes the substrate surface.
[0015]
[0016] As used herein and in the appended claims, the terms "precursor," "reactant," "reactive gas," and the like are used interchangeably to refer to any gaseous species capable of reacting with the substrate surface.
[0016]
[0017] As used herein, the term "dynamic random access memory" or "DRAM" refers to a memory cell that stores datum bits by storing a packet of charge (i.e., a binary 1) or no charge (i.e., a binary 0) on a capacitor. The charge is gated onto the capacitor through an access transistor and sensed by looking at the voltage fluctuation caused by turning on the same transistor to dump the charge packet onto an interconnect line at the transistor output. Thus, a single DRAM cell is made of one transistor and one capacitor.
[0017]
[0018] The present disclosure relates to a method for forming a metal silicon nitride film, such as titanium silicon nitride (TiSiN), that is substantially free of silicon nitride (SiN). The metal silicon nitride film may be formed from a titanium (Ti) or titanium / titanium nitride (Ti / TiN) film on silicon (Si), or a titanium silicide (TiSi) film. The metal silicon nitride film may be formed using a thermal plasma process.
[0018]
[0019] FIG. 1 illustrates a general method 10 for forming a metal silicon nitride film on a substrate, according to one or more embodiments of the present disclosure. Method 10 generally begins at step 12, where a substrate having a metal film thereon is provided and placed in a processing chamber. As used herein and in the appended claims, the term "provided" means that the substrate or substrate surface is made available for processing (e.g., positioned in a processing chamber). In step 14, the substrate having the metal film thereon is exposed to an ammonia plasma to form a metal silicon nitride film. In step 16, method 10 proceeds to an optional post-processing step.
[0019]
[0020] 2A-2D are cross-sectional views illustrating an exemplary device 100 during formation of a metal silicon nitride film in accordance with one or more embodiments of the present disclosure. With reference to FIGS. 1 and 2A, in step 12, a substrate 102 having a metal film 104 thereon is provided. The substrate 102 may comprise any suitable material known to those of skill in the art. In some embodiments, the substrate 102 comprises silicon (Si) or silicon germanium (SiGe).
[0020]
[0021] The metal film 104 may include any suitable metal known to one of ordinary skill in the art. In one or more embodiments, the metal film 104 includes a metal selected from titanium (Ti), cobalt (Co), molybdenum (Mo), ruthenium (Ru), tungsten (W), nickel (Ni), and the like. One of ordinary skill in the art will appreciate that when the metal film 104 is formed on the substrate 102, a metal silicide 103 may result. In one or more embodiments, the metal silicide 103 may include titanium silicide (TiSi), cobalt silicide (CoSi), molybdenum silicide (MoSi), ruthenium silicide (RuSi), tungsten silicide (WSi), nickel silicide (NiSi), and the like.
[0021]
[0022] In one or more embodiments, the metal film 104 comprises titanium (Ti) or titanium / titanium nitride (Ti / TiN) on a silicon-containing substrate 102. Thus, in some embodiments, the metal silicide 103 is titanium silicide (TiSi).
[0022]
[0023] The metal film 104 or metal silicide 103 may have any suitable thickness. In one or more embodiments, the metal film 104 or metal silicide 103 has a thickness in the range of 0.5 nm to 15 nm, or in the range of 1 nm to 10 nm, or in the range of 2 nm to 6 nm.
[0023]
[0024] The metal film 104 may be formed by any suitable deposition process known to those of skill in the art. In one or more embodiments, the deposition process includes atomic layer deposition (ALD), physical vapor deposition (PVD), chemical vapor deposition (CVD), etc.
[0024]
[0025] The process of forming the metal film 104 can be initiated by exposing the substrate to a precursor for a period of time. In some embodiments, the precursor is delivered without the use of a plasma.
[0025]
[0026] As used herein, "pulse" or "dose" refers to an amount of source gas that is intermittently or non-continuously introduced into a process chamber. The amount of a particular compound in each pulse may vary over time depending on the duration of the pulse. A particular process gas may include a single compound or a mixture / combination of two or more compounds, such as the process gases described below.
[0026]
[0027] The precursor may be any suitable compound for adsorbing a layer of reactive species on the substrate surface for subsequent reaction. The reactive species may also be referred to by its identity as the precursor. For example, when a substrate is exposed to a titanium precursor, a reactive species called a titanium species is formed.
[0027]
[0028] In some embodiments, the precursor comprises a metal selected from one or more of titanium (Ti), cobalt (Co), molybdenum (Mo), ruthenium (Ru), tungsten (W), nickel (Ni), etc. Thus, in some embodiments, the metal film 104 comprises one or more of titanium (Ti), cobalt (Co), molybdenum (Mo), ruthenium (Ru), tungsten (W), nickel (Ni), etc.
[0028]
[0029] In some embodiments, the metal film 104 comprises or consists essentially of titanium (Ti) and titanium nitride (TiN). In some embodiments, the metal film 104 comprises or consists essentially of titanium (Ti).
[0029]
[0030] 1 and 2B, in step 14, the device 100 is exposed to or treated with a plasma. In one or more embodiments, the plasma is an ammonia (NH3) plasma. The ammonia plasma may be generated from a plasma gas that forms radicals. In one or more embodiments, the ammonia plasma forms NH3 on the surface of the metal film 104 or metal silicide 103. * Forming radicals 106. In one or more embodiments, the plasma is NH *In some embodiments, the plasma gas includes ammonia gas (NH3). In some embodiments, the plasma gas further includes an inert gas. The inert gas may include any suitable inert gas, including, but not limited to, argon (Ar), helium (He), and xenon (Xe). In some embodiments, the inert gas is flowed continuously while the ammonia gas is pulsed. In one or more embodiments, the ammonia plasma generates a maximum of NH * It is diluted with an inert gas to generate radicals. In one or more embodiments, the ratio of ammonia to an inert gas (i.e., NH3:Ar, NH3:He, NH3:Xe) ranges from 1:10000 to 10:1, or ranges from 1:100 to 1:5, or is a ratio of 1:10.
[0030]
[0031] In some embodiments, the ammonia plasma gas is flowed into the processing chamber and then ignited to form a direct plasma, hi some embodiments, the ammonia plasma gas is ignited outside the processing chamber to form a remote plasma.
[0031]
[0032] In some embodiments, the ammonia plasma is an inductively coupled plasma (ICP). In some embodiments, the ammonia plasma is a conductively coupled plasma (CCP). In some embodiments, the ammonia plasma is a microwave plasma. In some embodiments, the ammonia plasma is generated by passing an ammonia plasma gas over a hot wire.
[0032]
[0033] 2C and 2D, exposing the metal film 104 or metal silicide 103 to a plasma containing ammonia (NH) at a temperature ranging from 450° C. to 1000° C. causes NH to diffuse through the metal film 104 (or metal silicide 103) and form a metal silicon nitride film 108 that is substantially free of silicon nitride (SiN). * Radicals 106 are formed. In some embodiments, the metal film 104 is exposed to an ammonia plasma at a temperature in the range of 600°C to 850°C.
[0033]
[0034] The plasma treatment may be performed at any suitable pressure. In one or more embodiments, the device 100 is treated with an ammonia plasma at a pressure ranging from 0.2 Torr to less than 5 Torr, or ranging from 0.2 Torr to 4.5 Torr, or ranging from 0.2 Torr to 3.5 Torr, or ranging from 0.2 Torr to 2.5 Torr, or ranging from 0.2 Torr to 1.5 Torr.
[0034]
[0035] The plasma treatment may be performed for any suitable time. In one or more embodiments, the device 100 is treated with ammonia plasma for a time ranging from 10 seconds to 10 minutes, or from 10 seconds to 5 minutes, or from 10 seconds to 4.5 minutes, or from 10 seconds to 3 minutes, or from 10 seconds to 2 minutes, or from 30 seconds to 2 minutes.
[0035]
[0036] Without wishing to be bound by theory, NH from ammonia plasma * It is believed that the nitrogen atom N of the radical 106 only bonds with the metal of the metal film 104 or the metal of the metal silicide 103, and silicon nitride (SiN) is not formed. * This means that NH does not react with silicon (Si) (bulk or substrate silicon layer) to form a silicon nitride (SiN) layer that is present under the metal silicide layer and at the interface between the metal silicide and the silicon substrate. Without wishing to be bound by theory, NH * In addition to N from Ti bonding only to Ti, NH * N from the NH may bond with Ti on one side and with Si in the TiSI layer on the other side to form a Ti-N-Si bond. * N from does not bond with Si in any Si-Si bonding environment such as a Si substrate.
[0036]
[0037] Thus, the metal silicon nitride film 108 is substantially free of silicon nitride (SiN). As used herein, the term "substantially free" means that the metal silicon nitride film 108 contains less than 5%, less than 4%, less than 3%, less than 2%, less than 1%, or less than 0.5% silicon nitride (SiN).
[0037]
[0038] In one or more embodiments, the metal silicon nitride film 108 is selected from titanium silicon nitride (TiSiN), cobalt silicon nitride (CoSiN), molybdenum silicon nitride (MoSiN), ruthenium silicon nitride (RuSiN), tungsten silicon nitride (WSiN), nickel silicon nitride (NiSiN), etc. In one or more embodiments, the metal silicon nitride film 108 is substantially free of silicon nitride (SiN).
[0038]
[0039] In one or more embodiments, the metal silicon nitride film 108 is a titanium silicon nitride (TiSiN) film and contains less than 10% silicon nitride (SiN) by weight. In other embodiments, the titanium silicon nitride (TiSiN) film contains less than 5% silicon nitride (SiN) by weight. In yet further embodiments, the titanium silicon nitride (TiSiN) film contains less than 1% silicon nitride (SiN) by weight.
[0039]
[0040] In some embodiments, the metal silicon nitride film 108 of the present disclosure has a lower resistivity. In some embodiments, the resistivity of the metal silicon nitride film 108, such as titanium silicon nitride (TiSiN) film, is 200 μΩ·cm or less, 180 μΩ·cm or less, 160 μΩ·cm or less, 150 μΩ·cm or less, or 140 μΩ·cm or less. In some embodiments, the metal silicon nitride film of the present disclosure has a lower resistivity than a metal silicon nitride film deposited by a plasma process involving nitrogen plasma exposure. In some embodiments, the metal silicon nitride film of the present disclosure has a lower resistivity than a metal silicon nitride film deposited by a thermal process.
[0040]
[0041] The metal silicon nitride film 108 may have any suitable thickness. In one or more embodiments, the metal silicon nitride film 108 has a thickness in the range of 0.5 nm to 15 nm, or in the range of 1 nm to 10 nm, or in the range of 2 nm to 6 nm.
[0041]
[0042] The method 10 may end at step 16 or may proceed to optional further processing (eg, bulk deposition of a metal film, annealing).
[0042]
[0043] In one or more embodiments, the metal silicon nitride film 108 is part of a DRAM bitline contact. As used herein, the term "bitline" refers to a layer or layers of material that are electrical conductors. The bitline contact is the connection between the bitline on which the metal silicon nitride film is formed and silicon.
[0043]
[0044] In the above embodiment, the substrate 102 may include silicon (Si) and the metal film 104 may include titanium (Ti) or titanium nitride (TiN). Thus, the metal silicide 103 is titanium silicide (TiSi). Treating titanium silicide with ammonia plasma forms titanium silicon nitride (TiSiN) that is substantially free of silicon nitride (SiN).
[0044]
[0045] In one or more embodiments, a plasma processing apparatus is used to generate a plasma and process the metal film with an ammonia plasma. In one or more embodiments, the plasma processing apparatus is a stand-alone tool and is not part of a cluster tool. In other embodiments, the plasma processing apparatus is part of a cluster tool.
[0045]
[0046] Some well-known cluster tools that can be adapted for the present disclosure are Olympia®, Continuum®, and Trillium®, all available from Applied Materials, Inc., Santa Clara, Calif. However, the exact arrangement and combination of chambers can be varied to perform the specific steps of the processes described herein. Other process chambers that can be used include, but are not limited to, cyclic layer deposition (CLD), atomic layer deposition (ALD), chemical vapor deposition (CVD), physical vapor deposition (PVD), plasma treatment, etching, pre-cleaning, chemical cleaning, thermal treatment such as RTP, plasma nitridation, degassing, hydroxylation, and other substrate processes. By performing the process in a chamber on a cluster tool, contamination of the substrate surface with atmospheric impurities can be avoided without oxidation before depositing a subsequent film.
[0046]
[0047] According to one or more embodiments, the substrate is continuously under vacuum or "load-lock" conditions and is not exposed to ambient air when being transferred from one chamber to the next. The transfer chamber is therefore under vacuum and is "pumped down" under vacuum pressure. An inert gas may be present in the processing chamber or the transfer chamber. In some embodiments, an inert gas is used as a purge gas to remove some or all of the reactants (e.g., reactants). According to one or more embodiments, a purge gas is injected at the outlet of the deposition chamber to prevent the reactants (e.g., reactants) from transferring from the deposition chamber to the transfer chamber and / or additional processing chambers. In this way, the flow of the inert gas forms a curtain at the outlet of the chamber.
[0047]
[0048] Substrates may be processed in a single substrate deposition chamber, where a single substrate is loaded, processed, and unloaded before another substrate is processed. Substrates may also be processed in a continuous manner, similar to a conveyor system, where multiple substrates are individually loaded into a first portion of the chamber, moved through the chamber, and unloaded from a second portion of the chamber. The geometry of the chamber and associated conveyor system may form a linear or curved path. Additionally, the processing chamber may be a carousel, where multiple substrates move about a central axis and are exposed to processes such as deposition, etching, annealing, cleaning, etc., throughout the carousel path.
[0048]
[0049] During processing, the substrate may be heated or cooled. Such heating or cooling may be accomplished by any suitable means, including, but not limited to, varying the temperature of the substrate support and flowing a heated or cooled gas over the substrate surface. In some embodiments, the substrate support includes a heater / cooler that is controllable to conductively vary the substrate temperature. In one or more embodiments, the gas employed (either reactive or inert gas) is heated or cooled to locally vary the substrate temperature. In some embodiments, a heater / cooler is positioned within the chamber adjacent to the substrate surface to convectively vary the substrate temperature.
[0049]
[0050] The substrate can be stationary or rotated during processing. A rotating substrate can be rotated continuously (about the substrate axis) or in discontinuous steps. For example, the substrate can be rotated throughout the entire process, or the substrate can be rotated only a small amount between exposures to different reactive or purge gases. Rotating the substrate (continuously or in steps) during processing can help minimize the effects of local variations in the geometry of the gas flow, for example, resulting in a more uniform deposition or etching.
[0050]
[0051] One or more embodiments provide a non-transitory computer readable medium comprising instructions that, when executed by a controller of a process chamber, cause the process chamber to perform steps of exposing the substrate to a metal precursor and a reactant to form a metal film on the substrate comprising a metal silicon compound, and exposing the metal film to a plasma comprising ammonia (NH3) at a temperature in the range of 450° C. to 1000° C. to form NH radicals that diffuse through the metal film and form a metal silicon nitride film that is substantially free of silicon nitride (SiN).
[0051]
[0052] The use of the terms "a" and "an" and "the" and similar referents in the context of describing the materials and methods described herein (particularly in the context of the claims below) should be construed to cover both the singular and the plural, unless otherwise stated herein or clearly contradicted by context. The recitation of ranges of values herein is merely intended as a shorthand method of referring individually to each individual value falling within the range, unless otherwise stated herein, and each individual value is incorporated herein as if the value were individually recited herein. All methods described herein may be performed in any suitable order, unless otherwise stated herein or clearly contradicted by context. The use of any and all examples, or exemplary language (e.g., "etc.") provided herein is intended merely to better illuminate the materials and methods, and does not impose limitations on the scope unless otherwise claimed. No language in the specification should be construed as indicating any non-claimed element as essential to the practice of the disclosed materials and methods.
[0052]
[0053] As used throughout this specification, the terms "one embodiment," "particular embodiment," "one or more embodiments," or "embodiments" mean that a particular feature, structure, material, or characteristic described in connection with that embodiment is included in at least one embodiment of the present disclosure. Thus, the appearances of phrases such as "in one or more embodiments," "in a particular embodiment," "in one embodiment," or "in an embodiment" in various places throughout this specification are not necessarily all referring to the same embodiment of the present disclosure. Furthermore, in one or more embodiments, the particular features, structures, materials, or characteristics may be combined in any suitable manner.
[0053]
[0054] Although the disclosure herein has been described with reference to particular embodiments, it is to be understood that these embodiments are merely illustrative of the principles and applications of the disclosure. It will be apparent to those skilled in the art that various modifications and variations can be made to the disclosed method and apparatus without departing from the spirit and scope of the disclosure. Thus, the disclosure is intended to cover modifications and variations that come within the scope of the appended claims and their equivalents.
Claims
1. 1. A method of forming a semiconductor device, comprising: Ammonia (NH) is added at a temperature in the range of 450° C. to 1000° C. to form NH radicals that diffuse through the metal silicide film and form a metal silicon nitride film that is substantially free of silicon nitride (SiN). 3 exposing the metal silicide film to a plasma containing The method includes:
2. The method of claim 1 , wherein the plasma further comprises an inert gas selected from argon (Ar), helium (He), and xenon (Xe).
3. The ammonia (NH 3 3. The method of claim 2, wherein the ratio of the inert gas to the vapor is from 1:1000 to 1:
5.
4. The method of claim 1 , wherein the plasma has a pressure in the range of 0.2 Torr to 5 Torr.
5. 10. The method of claim 1, wherein the metal silicon nitride film comprises less than 10% by weight silicon nitride (SiN).
6. The method of claim 1 , wherein the plasma is a remote plasma.
7. The method of claim 1 , wherein the metal silicide film is exposed to the plasma at a temperature in the range of 600° C. to 850° C.
8. 10. The method of claim 1, wherein the metal silicide film comprises a metal selected from titanium (Ti), cobalt (Co), molybdenum (Mo), ruthenium (Ru), tungsten (W), and nickel (Ni).
9. 2. The method of claim 1, wherein the metal silicide film is selected from titanium silicide (TiSi), cobalt silicide (CoSi), molybdenum silicide (MoSi), ruthenium silicide (RuSi), tungsten silicide (WSi), and nickel silicide (NiSi).
10. 2. The method of claim 1, wherein the metal silicon nitride film is selected from titanium silicon nitride (TiSiN), cobalt silicon nitride (CoSiN), molybdenum silicon nitride (MoSiN), ruthenium silicon nitride (RuSiN), tungsten silicon nitride (WSiN), and nickel silicon nitride (NiSiN).
11. The method of claim 1 , wherein the metal silicide film has a thickness in the range of 2 nm to 6 nm.
12. 2. The method of claim 1, wherein the metal silicide film comprises a metal film on a substrate, the metal film comprising one or more of titanium (Ti), cobalt (Co), molybdenum (Mo), ruthenium (Ru), tungsten (W), nickel (Ni), titanium nitride (TiN), and the substrate is selected from silicon (Si) or silicon germanium (SiGe).
13. The method of claim 1 , wherein the metal silicide film is exposed to the plasma for a time ranging from 30 seconds to 2 minutes.
14. 1. A method of forming a semiconductor device, comprising: Ammonia (NH) is added at a temperature in the range of 450° C. to 1000° C. to form NH radicals that diffuse through the titanium film and form a titanium silicon nitride (TiSiN) film that is substantially free of silicon nitride (SiN). 3 exposing the titanium film to a plasma containing The method includes:
15. 15. The method of claim 14, wherein the titanium film is selected from titanium (Ti), titanium / titanium nitride (Ti / TiN), and titanium silicide (TiS).
16. 15. The method of claim 14, wherein the titanium silicon nitride (TiSiN) film comprises less than 10% by weight silicon nitride (SiN).
17. The method of claim 14 , wherein the titanium film is exposed to the plasma at a temperature in the range of 600° C. to 850° C.
18. The method of claim 14 , wherein the titanium film is exposed to the plasma for a time ranging from 30 seconds to 2 minutes.
19. 15. The method of claim 14, wherein the plasma is flowed with an inert gas having a ratio of ammonia to inert gas of 1:100 to 1:5, and the plasma has a pressure in the range of 0.2 Torr to 5 Torr.
20. 16. A non-transitory computer readable medium, the non-transitory computer readable medium being configured, when executed by a controller of a process chamber, to cause the process chamber to: Ammonia (NH) is added at a temperature in the range of 450° C. to 1000° C. to form NH radicals that diffuse through the metal silicide film and form a metal silicon nitride film that is substantially free of silicon nitride (SiN). 3 The metal silicide film is exposed to a plasma containing A non-transitory computer readable medium containing instructions for carrying out a process.
Citation Information
Patent Citations
Semiconductor device and manufacture thereof
JP1991266466A
Barrier metal, its formation, gate electrode, and its formation
JP1999195621A
Film forming method, pretreatment method and film forming system
JP2006294861A
Method for depositing metal silicon nitride
JP2009007670A
Method and device for forming barrier metal layer
JP2013058565A