Platable polymeric composition

A plateable polymer composition with thermotropic liquid crystal polymer and silicate fibers addresses the limitations of LDS in MIDs by enhancing weld line tensile properties and melt processability, facilitating the formation of conductive elements in high-frequency electronic components.

JP2024543928APending Publication Date: 2024-11-26TICONA LLC
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2024531499
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-12-01
Filing Date
2022-11-21
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

Molded interconnect devices (MIDs) face challenges in forming conductive elements without conventional laser direct structuring (LDS) processes, which are hindered by spinel crystals affecting performance and fiber reinforcement extending from the surface, leading to poor tensile properties at weld lines.

Method used

A plateable polymer composition comprising a thermotropic liquid crystal polymer, silicate fibers, and a noble metal catalyst, which allows for easy plating without LDS, improving weld line tensile properties and melt processability.

Benefits of technology

The composition exhibits excellent weld line tensile properties, low melt viscosity, and thermal stability, enabling the formation of small-sized parts with conductive elements suitable for high-frequency electronic components.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024543928000001_ABST
    Figure 2024543928000001_ABST
Patent Text Reader

Abstract

A platable polymeric composition is provided that includes 100 parts by weight of a polymeric matrix including a thermotropic liquid crystalline polymer, from about 10 parts by weight to about 80 parts by weight of silicate fibers, and a precious metal catalyst.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] Related Applications

[0001] This application claims priority to U.S. Provisional Patent Application No. 63 / 284,774, having a filing date of December 1, 2021, which is incorporated herein by reference. [Background technology]

[0002] To form various electronic components, especially those used at high frequencies, molded interconnect devices (MIDs) are often formed that include a plastic substrate on which conductive elements or paths are formed. Such MID devices are thus three-dimensional molded parts with integrated printed conductors or circuit layouts. MIDs are typically formed using a laser direct structuring ("LDS") process in which a computer-controlled laser beam moves over the plastic substrate to activate its surface where the conductive paths are to be located. Various materials have been proposed to form the plastic substrate of laser direct structured devices. For example, one such material is a blend of polycarbonate, acrylonitrile butadiene styrene, and copper chromite. In the laser direct structuring process, the copper chromite cracks open, releasing metal atoms that can act as nuclei for crystal growth in a subsequent electroless copper plating process. Despite its advantages, one of the limitations of laser direct structured materials is that spinel crystals tend to negatively impact the performance of the composition under certain circumstances. Additionally, LDS compositions also tend to require fiber reinforcement to achieve a sufficient degree of strength. Unfortunately, most fiber fillers tend to extend from the surface of the molded interconnect parts, resulting in poor tensile properties at the weld line, which makes it difficult to mate with other types of electronic components.

[0003]

[0003] Therefore, a need currently exists for a molded interconnect device in which the conductive elements can be easily formed without using conventional LDS processes. Summary of the Invention [Means for solving the problem]

[0004] According to one embodiment of the present invention, a platable polymeric composition is disclosed, the polymeric composition comprising 100 parts by weight of a polymeric matrix comprising a thermotropic liquid crystalline polymer, from about 10 parts by weight to about 80 parts by weight of a silicate fiber, and a precious metal catalyst.

[0005]

[0005] Other features and aspects of the present invention are set forth in greater detail below.

[0006] A full and enabling disclosure of the present invention, including the best mode thereof, to one of ordinary skill in the art, is set forth more particularly in the remainder of the specification, including reference to the accompanying drawings. [Brief description of the drawings]

[0006] [Figure 1]

[0007] FIG. 1 is a perspective view of an antenna module according to an embodiment of the present invention. [Diagram 2]

[0008] FIG. 2 is an exploded view of the antenna module shown in FIG. [Figure 3A]

[0009] 3A-3D are four different views of the antenna module of FIG. 1, where FIG. 3A is a top view, FIG. 3B is a rear view, FIG. 3C is a front view, and FIG. 3D is a side view. [Figure 3B] 3A-3D are four different views of the antenna module of FIG. 1, where FIG. 3A is a top view, FIG. 3B is a rear view, FIG. 3C is a front view, and FIG. 3D is a side view. [Figure 3C] 3A-3D are four different views of the antenna module of FIG. 1, where FIG. 3A is a top view, FIG. 3B is a rear view, FIG. 3C is a front view, and FIG. 3D is a side view. [Figure 3D] 3A-3D are four different views of the antenna module of FIG. 1, where FIG. 3A is a top view, FIG. 3B is a rear view, FIG. 3C is a front view, and FIG. 3D is a side view. [Figure 4A]

[0010] 4A and 4B are two cross-sectional views of the antenna module of FIG. 1, where FIG. 4A is a cross-sectional view of the antenna module taken along line AA of FIG. 3A and FIG. 4B is a cross-sectional view of the antenna module taken along line BB of FIG. 3A. [Figure 4B]

[0010] Figures 4A and 4B are two cross-sectional views of the antenna module of Figure 1, where Figure 4A is a cross-sectional view of the antenna module taken along line AA of Figure 3A, and Figure 4B is a cross-sectional view of the antenna module taken along line BB of Figure 3A. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0007]

[0011] It will be understood by those skilled in the art that this discussion is a description of exemplary embodiments only, and is not intended to limit the broader aspects of the invention.

[0012] In general, the present invention relates to a plateable polymeric composition comprising a precious metal catalyst, silicate fibers, and a polymeric matrix comprising at least one thermotropic liquid crystalline polymer. By selectively controlling various aspects of the composition, the inventors have discovered that the resulting composition may be readily plated without the use of a laser direct structuring system. In this manner, the polymeric composition may be beneficially formed without the use of copper chromite (CuCr2O4) as a laser activatable additive, such that the resulting polymeric composition may generally be free of chromium and / or copper. For example, chromium may be present in the composition in an amount of about 2,000 parts per million ("ppm") or less, in some embodiments about 1,500 ppm or less, in some embodiments about 1,000 ppm or less, and in some embodiments about 0.001 to about 500 ppm, while copper is generally present in the composition in an amount of about 1,000 ppm or less, in some embodiments about 750 ppm or less, in some embodiments about 500 ppm or less, and in some embodiments about 0.001 to about 100 ppm. The copper and chromium content may be determined using known techniques such as X-ray fluoroscopy (e.g., an Innov-X Systems Model a-2000 X-ray fluorescence spectrometer equipped with a Si-PiN diode detector). Of course, apart from copper chromite, the polymer composition may also generally be free of other types of conventional laser activatable additives, such as spinel crystals (e.g., MgAl2O4, ZnAl2O4, FeAl2O4, CuFe2O4, MnFe2O4, NiFe2O4, TiFe2O4, FeCr2O4, or MgCr2O4) having the formula AB2O4, where A is a metal cation having a valence of 2 (e.g., cadmium, chromium, manganese, nickel, zinc, copper, cobalt, iron, magnesium, tin, titanium, etc.) and B is a metal cation having a valence of 3 (e.g., chromium, iron, aluminum, nickel, manganese, or tin).The polymer composition may be free of such spinel crystals (i.e., 0 wt.%), or such crystals may be present only in minor concentrations, such as amounts of about 1 wt.% or less, in some embodiments about 0.5 wt.% or less, and in some embodiments, about 0.001 wt.% to about 0.2 wt.%.

[0008]

[0013] In addition to being readily plateable, the polymeric compositions may also exhibit improved weld line tensile properties. For example, the polymeric compositions may exhibit a weld line tensile break strain of about 0.3% or greater, in some embodiments about 0.33% or greater, and in some embodiments about 0.35% or greater. Similarly, the polymeric compositions may exhibit a weld line tensile strength of about 20 MPa or greater, in some embodiments about 22 to about 60 MPa, in some embodiments about 25 to about 50 MPa, and / or a weld line tensile modulus of 7,000 MPa or greater, in some embodiments about 7,300 MPa to about 20,000 MPa, and in some embodiments about 7,500 MPa to about 12,000 MPa. The weld line tensile properties may be determined at a temperature of 23° C. in accordance with ISO 527:2019. Previously, it was believed that plateable polymeric compositions with excellent weld line tensile properties would not also have a melt viscosity low enough to allow them to easily flow into mold cavities to form small size parts. However, contrary to conventional belief, it has been found that the polymer composition has excellent melt processability. For example, the polymer composition of the present invention has a melt processability of 1000 seconds according to ISO 11443:2021. -1 and at a temperature about 15° C. above the melt temperature of the polymer composition.

[0009]

[0014] The polymeric composition also has excellent thermal properties. The melting temperature of the composition may be, for example, about 280°C to about 400°C, in some embodiments about 300°C to about 380°C, and in some embodiments about 320°C to about 370°C. Even at such melting temperatures, the ratio of the deflection temperature under load ("DTUL"), a measure of short-term heat resistance, to the melting temperature may still remain relatively high. For example, the ratio may range from about 0.5 to about 1.00, in some embodiments about 0.6 to about 0.95, and in some embodiments about 0.65 to about 0.85. Specific DTUL values ​​may be, for example, about 200°C or higher, in some embodiments about 220°C or higher, in some embodiments about 230°C to about 300°C, and in some embodiments about 240°C to about 280°C. Such high DTUL values ​​may, among other things, enable the use of fast and reliable surface attachment processes for mating the structure with other parts of the electrical component.

[0010]

[0015] The polymer composition may also have a high impact strength, useful in forming thin layers. The composition may have, for example, a thermal shock resistance of about 0.5 kJ / m2, determined at a temperature of 23° C. according to ISO 179-1:2010. 2 In some embodiments, about 1 to about 60 kJ / m 2 and in some embodiments, from about 2 to about 50 kJ / m 2 and in some embodiments, from about 5 to about 45 kJ / m 2The composition may have a Charpy notched impact strength of about 20 to about 500 MPa, in some embodiments about 50 to about 400 MPa, in some embodiments about 70 to about 350 MPa; a tensile strain at break of about 0.4% or more, in some embodiments about 0.5% to about 10%, in some embodiments about 0.6% to about 3.5%; and / or a tensile modulus of about 5,000 MPa to about 20,000 MPa, in some embodiments about 8,000 MPa to about 20,000 MPa, in some embodiments about 10,000 MPa to about 20,000 MPa. Tensile properties may be determined at a temperature of 23° C. according to ISO 527:2019. The polymeric composition may also exhibit a flexural strength of from about 20 to about 500 MPa, in some embodiments from about 50 to about 400 MPa, and in some embodiments from about 100 to about 350 MPa; a flexural elongation of about 0.4% or greater, in some embodiments from about 0.5% to about 10%, and in some embodiments from about 0.6% to about 3.5%; and / or a flexural modulus of from about 5,000 MPa to about 20,000 MPa, in some embodiments from about 8,000 MPa to about 20,000 MPa, and in some embodiments from about 10,000 MPa to about 15,000 MPa. Flexural properties may be determined at a temperature of 23° C. according to ISO 178:2019.

[0011]

[0016] As a result of the above-mentioned properties, the polymer composition can be easily formed into a substrate onto which one or more conductive elements can then be plated. Due to the beneficial properties of the polymer composition, the resulting substrate may have a very small size, such as a thickness of about 5 millimeters or less, in some embodiments about 4 millimeters or less, in some embodiments about 2 millimeters or less, and in some embodiments about 0.1 to about 1 millimeter. If desired, the conductive element may be an antenna (e.g., an antenna resonating element), whereby the resulting part is an antenna module that may be utilized in a wide variety of different electronic components, such as mobile phones, in-vehicle devices, and the like.

[0012]

[0017] Various embodiments of the invention will now be described in more detail. I. Polymer Composition A. Polymer matrix

[0018] The polymer matrix includes one or more thermotropic liquid crystal polymers. Liquid crystal polymers generally have a rod-like structure and are classified as "thermotropic" as long as they are capable of exhibiting crystalline behavior in the molten state (e.g., in a thermotropic nematic state). Liquid crystal polymers utilized in the polymer composition typically have a melting temperature of about 280°C to about 400°C, in some embodiments about 300°C to about 380°C, and in some embodiments about 310°C to about 370°C. The melting temperature may be determined as known in the art using, for example, differential scanning calorimetry ("DSC") as determined by ISO 11357-3:2018. Such polymers may be formed from one or more types of repeating units as known in the art. Liquid crystal polymers may, for example, generally be represented by the following formula (I):

[0013] [ka]

[0014] (In the formula, Ring B is a substituted or unsubstituted 6-membered aryl group (e.g., 1,4-phenylene or 1,3-phenylene), a substituted or unsubstituted 6-membered aryl group fused with a substituted or unsubstituted 5- or 6-membered aryl group (e.g., 2,6-naphthalene), or a substituted or unsubstituted 6-membered aryl group linked to a substituted or unsubstituted 5- or 6-membered aryl group (e.g., 4,4-biphenylene); Y1 and Y2 are independently O, C(O), NH, C(O)HN, or NHC(O). The aromatic ester may contain one or more aromatic ester repeat units represented by:

[0015]

[0019] Typically, at least one of Y1 and Y2 is C(O). Examples of such aromatic ester repeat units include, for example, aromatic dicarboxylic acid repeat units (Y1 and Y2 in formula I are C(O)), aromatic hydroxycarboxylic acid repeat units (Y1 in formula I is O and Y2 is C(O)), and various combinations thereof.

[0016]

[0020] For example, aromatic hydroxycarboxylic acid repeat units derived from aromatic hydroxycarboxylic acids such as 4-hydroxybenzoic acid, 4-hydroxy-4'-biphenylcarboxylic acid, 2-hydroxy-6-naphthoic acid, 2-hydroxy-5-naphthoic acid, 3-hydroxy-2-naphthoic acid, 2-hydroxy-3-naphthoic acid, 4'-hydroxyphenyl-4-benzoic acid, 3'-hydroxyphenyl-4-benzoic acid, 4'-hydroxyphenyl-3-benzoic acid, and the like, as well as alkyl, alkoxy, aryl, and halogen substituted versions thereof, and combinations thereof, may be utilized. Particularly suitable aromatic hydroxycarboxylic acids are 4-hydroxybenzoic acid ("HBA") and 6-hydroxy-2-naphthoic acid (HNA). When utilized, repeat units derived from hydroxycarboxylic acids (e.g., HBA and / or HNA) typically comprise from about 20 mol.% to about 85 mol.%, in some embodiments from about 30 mol.% to about 80 mol.%, and in some embodiments, from about 40 mol.% to 75 mol.% of the polymer.

[0017]

[0021] Aromatic dicarboxylic acid repeat units derived from aromatic dicarboxylic acids such as terephthalic acid, isophthalic acid, 2,6-naphthalenedicarboxylic acid, diphenylether-4,4'-dicarboxylic acid, 1,6-naphthalenedicarboxylic acid, 2,7-naphthalenedicarboxylic acid, 4,4'-dicarboxybiphenyl, bis(4-carboxyphenyl)ether, bis(4-carboxyphenyl)butane, bis(4-carboxyphenyl)ethane, bis(3-carboxyphenyl)ether, bis(3-carboxyphenyl)ethane, and the like, as well as alkyl, alkoxy, aryl, and halogen substituted versions thereof, and combinations thereof, may also be utilized. Particularly suitable aromatic dicarboxylic acids can include, for example, terephthalic acid ("TA"), isophthalic acid ("IA"), and 2,6-naphthalenedicarboxylic acid ("NDA"). When utilized, repeat units derived from aromatic dicarboxylic acids (e.g., IA, TA and / or NDA) typically comprise from about 1 mol.% to about 50 mol.%, in some embodiments from about 5 mol.% to about 40 mol.%, and in some embodiments, from about 10 mol.% to about 35 mol.% of the polymer.

[0018]

[0022] Other repeat units can also be utilized in the polymer. For example, in certain embodiments, repeat units derived from aromatic diols such as hydroquinone, resorcinol, 2,6-dihydroxynaphthalene, 2,7-dihydroxynaphthalene, 1,6-dihydroxynaphthalene, 4,4'-dihydroxybiphenyl (or 4,4'-biphenol), 3,3'-dihydroxybiphenyl, 3,4'-dihydroxybiphenyl, 4,4'-dihydroxybiphenyl ether, bis(4-hydroxyphenyl)ethane, and the like, as well as alkyl, alkoxy, aryl, and halogen substituted versions thereof, and combinations thereof, may be utilized. Particularly suitable aromatic diols can include, for example, hydroquinone ("HQ") and 4,4'-biphenol ("BP"). When utilized, repeat units derived from aromatic diols (e.g., HQ and / or BP) typically comprise from about 1 mol.% to about 50 mol.%, in some embodiments from about 5 mol.% to about 40 mol.%, and in some embodiments from about 10 mol.% to about 35 mol.% of the polymer. Repeat units such as those derived from aromatic amides (e.g., acetaminophen ("APAP")), and / or aromatic amines (e.g., 4-aminophenol ("AP"), 3-aminophenol, 1,4-phenylenediamine, 1,3-phenylenediamine, etc.) may also be utilized. When utilized, repeat units derived from aromatic amides (e.g., APAP) and / or aromatic amines (e.g., AP) typically comprise from about 0.1 mol.% to about 20 mol.%, in some embodiments from about 0.5 mol.% to about 15 mol.%, and in some embodiments from about 1 mol.% to about 10% of the polymer. It should also be understood that various other monomeric repeat units may be incorporated into the polymer. For example, in certain embodiments, a polymer may contain one or more repeat units derived from non-aromatic monomers, such as aliphatic or alicyclic hydroxycarboxylic acids, dicarboxylic acids, diols, amides, amines, etc. Of course, in other embodiments, the polymer may be "fully aromatic" in that it does not include repeat units derived from non-aromatic (e.g., aliphatic or alicyclic) monomers.

[0019]

[0023] Although not required, at least one liquid crystal polymer is utilized in the polymer matrix, which is typically a "low naphthenic" polymer to the extent that it contains a relatively low content of repeat units derived from naphthenic hydroxycarboxylic acids and naphthenic dicarboxylic acids, such as NDA, HNA, or a combination thereof. That is, the total amount of repeat units derived from naphthenic hydroxycarboxylic acids and / or dicarboxylic acids (e.g., NDA, HNA, or a combination of HNA and NDA) is typically about 20 mol.% or less of the polymer, in some embodiments about 15 mol.% or less, in some embodiments about 0.5 mol.% to about 10 mol.%, and in some embodiments about 1 mol.% to about 6 mol.%. In one particular embodiment, for example, the liquid crystal polymer may contain repeat units derived from HNA in an amount of 0.1 mol.% to about 10 mol.%, in some embodiments about 0.5 mol.% to about 8 mol.%, and in some embodiments about 1 mol.% to about 6 mol.%. The liquid crystal polymer may also contain various other monomers. For example, the polymer may contain repeat units derived from HBA in an amount of about 40 mol.% to about 80 mol.%, in some embodiments about 50 mol.% to about 75 mol.%, and in some embodiments about 55 mol.% to about 70 mol.%. When utilized, the molar ratio of repeat units derived from HBA to repeat units derived from HNA may be selectively controlled within a particular range to help achieve desired properties, such as about 5 to about 40, in some embodiments about 8 to about 35, and in some embodiments about 10 to about 30. The polymer may also contain repeat units derived from aromatic dicarboxylic acids (e.g., IA and / or TA) in an amount of about 10 mol.% to about 40 mol.%, and in some embodiments, about 15 mol.% to about 30 mol.%; aromatic diols (e.g., BP and / or HQ) in an amount of about 5 mol.% to about 30 mol.%, and in some embodiments, about 10 mol.% to about 20 mol.%; and / or aromatic amides (e.g., acetaminophen ("APAP")) in an amount of about 1 mol.% to about 10 mol.%, and in some embodiments, about 2 mol.% to about 8 mol.%.

[0020]

[0024] Regardless of the specific components and properties of the polymer, the liquid crystal polymer can be prepared by first introducing aromatic monomers used to form the ester repeat units (e.g., aromatic hydroxycarboxylic acids, aromatic dicarboxylic acids, etc.) and / or other repeat units (e.g., aromatic diols, aromatic amides, aromatic amines, etc.) into a reaction vessel to initiate a polycondensation reaction. The specific conditions and steps utilized in such reactions are well known and may be described in more detail in U.S. Pat. No. 4,161,470 to Calundann, U.S. Pat. No. 5,616,680 to Linstid, III et al., U.S. Pat. No. 6,114,492 to Linstid, III et al., U.S. Pat. No. 6,514,611 to Shepherd et al., and WO 2004 / 058851 to Waggoner. The vessel utilized in the reaction is not particularly limited, but it is typically desirable to utilize one commonly used for reactions of highly viscous fluids. Examples of such reaction vessels include agitation tank-type apparatuses having agitators equipped with agitation blades of various shapes, such as anchor type, multi-stage type, spiral ribbon type, screw shaft type, and modified shapes thereof. Further examples of such reaction vessels include mixing apparatuses commonly used for resin kneading, such as kneaders, roll mills, and Banbury mixers.

[0021]

[0025] If desired, the reaction can proceed by acetylation of the monomer as known in the art. This can be accomplished by adding an acetylating agent (e.g., acetic anhydride) to the monomer. Acetylation is generally initiated at a temperature of about 90° C. In the early stages of acetylation, reflux may be utilized to maintain the vapor phase temperature below the point where the acetic acid by-product and anhydride begin to distill. The temperature during acetylation typically ranges from 90° C. to 150° C., in some embodiments from about 110° C. to about 150° C. If reflux is used, the vapor phase temperature typically exceeds the boiling point of acetic acid, but remains low enough to retain residual acetic anhydride. For example, acetic anhydride vaporizes at a temperature of about 140° C. Thus, it is particularly desirable to provide the reactor with a vapor phase reflux at a temperature of about 110° C. to about 130° C. An excess of acetic anhydride can be utilized to ensure a substantially complete reaction. The amount of excess anhydride will vary depending on the particular acetylation conditions utilized, including the presence or absence of reflux. It is not uncommon to use an excess of about 1 to about 10 mole percent acetic anhydride, based on the total moles of reactant hydroxyl groups present.

[0022]

[0026] Acetylation may be carried out in a separate reaction vessel or in situ in the polymerization reaction vessel. If a separate reaction vessel is utilized, one or more of the monomers may be introduced into the acetylation reactor and then transferred to the polymerization reactor. Similarly, one or more of the monomers may be introduced directly into the reaction vessel without prior acetylation.

[0023]

[0027] In addition to the monomer and optional acetylating agent, other components that help promote polymerization may also be included in the reaction mixture. For example, catalysts such as metal salt catalysts (e.g., magnesium acetate, tin(I) acetate, tetrabutyl titanate, lead acetate, sodium acetate, potassium acetate, etc.) and organic compound catalysts (e.g., N-methylimidazole) can be optionally utilized. Such catalysts are typically used in amounts of about 50 to about 500 parts per million based on the total weight of the repeat unit precursor. When separate reactors are utilized, it is typically desirable to apply the catalyst to the acetylation reactor rather than the polymerization reactor, although this is by no means required.

[0024]

[0028] The reaction mixture is generally heated to an elevated temperature in a polymerization reactor vessel to initiate melt polycondensation of the reactants. The polycondensation may be carried out within a temperature range of, for example, about 200°C to about 400°C. For example, one suitable technique for forming aromatic polyesters may include charging the precursor monomers and acetic anhydride to a reactor, heating the mixture to a temperature of about 90°C to about 150°C to acetylate the hydroxyl groups of the monomers (e.g., to form acetoxy), and then increasing the temperature to about 200°C to about 400°C to carry out melt polycondensation. As the final polymerization temperature is approached, the volatile by-products of the reaction (e.g., acetic acid) can also be removed, thereby making it easier to achieve the desired molecular weight. The reaction mixture is generally subjected to stirring during polymerization to ensure good heat and mass transfer, and thus good material homogeneity. The rotation speed of the stirrer may vary over the course of the reaction, but typically ranges from about 10 to about 100 revolutions per minute ("rpm"), and in some embodiments, from about 20 to about 80 rpm. To increase the molecular weight of the melt, the polymerization reaction may be carried out under a vacuum, the application of which facilitates the removal of volatile materials formed in the final stages of polycondensation. The vacuum may be created by application of suction pressures, such as within the range of about 5 to about 30 pounds per square inch ("psi"), and in some embodiments, about 10 to about 20 psi.

[0025]

[0029] After melt polymerization, the molten polymer may be discharged from the reactor through an extrusion orifice, typically with a die of the desired shape, and cooled and collected. Generally, the melt is discharged through a perforated die to form strands that are captured in a water bath, pelletized, and dried. In some embodiments, the melt-polymerized polymer may also be subjected to a subsequent solid-state polymerization process to further increase its molecular weight. The solid-state polymerization may be carried out in the presence of a gas (e.g., air, an inert gas, etc.). Suitable inert gases may include, for example, nitrogen, helium, argon, neon, krypton, xenon, etc., and combinations thereof. The solid-state polymerization reaction vessel may be of virtually any design that allows the polymer to be maintained at the desired solid-state polymerization temperature for the desired residence time. Examples of such vessels may have fixed beds, stationary beds, moving beds, fluidized beds, etc. The temperature at which the solid-state polymerization is carried out may vary, but is typically in the range of about 200°C to about 400°C. The polymerization time will, of course, vary based on the temperature and the target molecular weight. In most cases, however, the solid state polymerization time is from about 2 hours to about 12 hours, and in some embodiments, from about 4 hours to about 10 hours.

[0026]

[0030] The total amount of liquid crystal polymer utilized in the polymer composition is typically about 40 wt.% to about 90 wt.%, in some embodiments about 45 wt.% to about 80 wt.%, and in some embodiments about 50 wt.% to about 70 wt.% of the total polymer composition. In certain embodiments, all of the liquid crystal polymers are "low naphthenic" polymers as described above. However, in other embodiments, "high naphthenic" liquid crystal polymers may also be utilized in compositions in which the total amount of repeat units derived from naphthenic hydroxycarboxylic acids and / or dicarboxylic acids (e.g., NDA, HNA, or combinations of HNA and NDA) may be about 10 mol.% or more, in some embodiments about 15 mol.% or more, and in some embodiments about 20 mol.% to about 75 mol.% of the polymer. When utilized, it is generally desirable that such high naphthenic polymers are present in relatively low amounts. For example, when utilized, the high naphthene liquid crystalline polymer typically comprises from about 1 wt.% to about 50 wt.%, in some embodiments from about 10 wt.% to about 45 wt.%, in some embodiments from about 20 wt.% to about 40 wt.%, and in some embodiments from about 0.5 wt.% to about 45 wt.%, in some embodiments from about 2 wt.% to about 35 wt.%, and in some embodiments from about 5 wt.% to about 25 wt.% of the total amount of liquid crystalline polymer in the composition. In contrast, the low naphthene liquid crystalline polymer typically comprises from about 50 wt.% to about 99 wt.%, in some embodiments from about 55 wt.% to about 95 wt.%, in some embodiments from about 60 wt.% to about 90 wt.%, and in some embodiments from about 25 wt.% to about 65 wt.%, in some embodiments from about 30 wt.% to about 60 wt.%, and in some embodiments from about 35 wt.% to about 55 wt.% of the total amount of liquid crystalline polymer in the composition.

[0027] B. Precious metal catalyst

[0031] As indicated above, the polymer composition contains a precious metal catalyst that can help facilitate subsequent plating of the composition. The precious metal catalyst typically includes a precious metal component, such as one selected from Groups IB, VIIA and VIIIA of the periodic table (IUPAC table), which generally have an atomic weight of at least 100. Examples of such precious metal components include palladium, ruthenium, rhodium, iridium, platinum, and alloys or combinations of any of the foregoing. Palladium is particularly preferred. To help improve the physical strength of the catalyst, the precious metal component is also typically supported by a matrix material, such as an inorganic metal oxide. Suitable inorganic metal oxides for this purpose include, for example, silica, alumina, silica-alumina, magnesia, silica-magnesia, silica-zirconia, silica-thoria, silica-beryllia, silica-titania, silica-alumina-thoria, silica-alumina-zirconia, silica-alumina-magnesia, silica-magnesia-zirconia, halloysite, kaolinite, illite, montmorillonite, vermiculite, palygorskite, pyrophyllite, calcium silicate, aluminum silicate, wollastonite, and the like. Natural and / or synthetic silicate minerals such as kaolinite are particularly suitable. The matrix material may be a mixture of simple or complex ions of the selected metal component (e.g., Pd(NH3)4 2+ The precious metal component may be combined with the matrix material in a variety of ways, such as by impregnation or ion exchange (or both), using a solution of the complex cation, such as ZnO, Fe, FeNb, FeNbO ...

[0028]

[0032] The total amount of catalyst utilized in the polymeric composition is generally such that the precious metal component comprises from about 0.1 parts by weight to about 6 parts by weight, in some embodiments from about 0.2 parts by weight to about 4 parts by weight, and in some embodiments from about 0.5 parts by weight to about 2.5 parts by weight per 100 parts by weight of the polymeric matrix. For example, the precious metal component may comprise from about 0.1 wt.% to about 5 wt.%, in some embodiments from about 0.2 wt.% to about 3 wt.%, and in some embodiments from about 0.4 wt.% to about 1.5 wt.% of the polymeric composition. Thus, the actual amount of catalyst utilized in the composition will depend on the amount of precious metal component utilized in the catalyst. Typically, the precious metal component comprises from about 0.01 wt.% to about 3 wt.%, in some embodiments from about 0.05 wt.% to about 1 wt.%, and in some embodiments from about 0.1 wt.% to about 0.8 wt.% of the catalyst. In such embodiments, the catalyst comprises from about 0.5 parts by weight to about 20 parts by weight, in some embodiments from about 1 part by weight to about 15 parts by weight, and in some embodiments from about 2 parts by weight to about 10 parts by weight, per 100 parts by weight of the polymer matrix. For example, the catalyst may comprise from about 0.1 wt.% to about 15 wt.%, in some embodiments from about 0.5 wt.% to about 10 wt.%, and in some embodiments from about 1 wt.% to about 6 wt.% of the polymer composition.

[0029] C. Silicate fiber

[0033] As noted, the polymeric composition typically includes silicate fibers distributed within the polymeric matrix in an amount of about 10 parts by weight to about 80 parts by weight, in some embodiments about 15 parts by weight to about 70 parts by weight, and in some embodiments about 30 parts by weight to about 55 parts by weight, per 100 parts by weight of the polymeric matrix. For example, the silicate fibers may comprise about 10 wt.% to about 60 wt.%, in some embodiments about 15 wt.% to about 45 wt.%, and in some embodiments about 20 wt.% to about 40 wt.% of the polymeric composition.

[0030]

[0034] The silicate fibers may be derived from neosilicates, sorosilicates, inosilicates (e.g., calcium inosilicates such as wollastonite; calcium magnesium inosilicates such as tremolite; calcium magnesium iron inosilicates such as yangtite; magnesium iron inosilicates such as anthophyllite, etc.), phyllosilicates (e.g., aluminum phyllosilicates such as palygorskite), tectosilicates, etc. Particularly suitable are silicate fibers having a hardness value on the Mohs hardness scale of about 2.0 or greater, in some embodiments about 2.5 or greater, in some embodiments about 3.0 or greater, in some embodiments about 3.0 to about 11.0, in some embodiments about 3.5 to about 11.0, and in some embodiments about 4.5 to about 6.5. Examples of such fibers include those derived from inosilicates such as wollastonite (Mohs hardness 4.5-5.0) available from Nyco Minerals under the trade name Nyglos® (e.g., Nyglos® 4W or Nyglos® 8).

[0031]

[0035] The silicate fibers may have a median diameter of about 1 to about 35 micrometers, in some embodiments about 2 to about 20 micrometers, in some embodiments about 3 to about 15 micrometers, and in some embodiments about 7 to about 12 micrometers. The silicate fibers may also have a narrow size distribution. That is, at least about 60% by volume of the fibers, in some embodiments at least about 70% by volume of the fibers, and in some embodiments at least about 80% by volume of the fibers may have a size within the ranges described above. In addition to having the above size characteristics, the silicate fibers may also have a relatively high aspect ratio (average length divided by median width) to help further improve the mechanical properties and surface quality of the resulting polymer composition. For example, the silicate fibers may have an aspect ratio of about 2 to about 50, in some embodiments about 2 to about 40, in some embodiments about 3 to about 20, and in some embodiments about 4 to about 15. The volume average length of such fibers may range, for example, from about 1 to about 200 micrometers, in some embodiments from about 2 to about 150 micrometers, in some embodiments, from about 5 to about 100 micrometers, and in some embodiments, from about 10 to about 50 micrometers.

[0032] D. Optional Additives i. Mineral particles

[0036] Optionally, mineral particles can also be used in the polymer composition. When used, the mineral particles are typically formed from materials having hardness values ​​as described above. Any of a variety of different types of mineral particles, such as those formed from natural and / or synthetic silicate minerals, such as talc, mica, silica (e.g., amorphous silica), alumina, halloysite, kaolinite, illite, montmorillonite, vermiculite, palygorskite, pyrophyllite, calcium silicate, aluminum silicate, wollastonite, etc.; sulfates; carbonates; phosphates; fluorides, borates, etc., can generally be used in the polymer composition. Particularly preferred are particles having the desired hardness values, such as calcium carbonate (CaCO3, Mohs hardness 3.0), copper hydroxide carbonate (Cu2CO3(OH)2, Mohs hardness 4.0); calcium fluoride (CaFl2, Mohs hardness 4.0); calcium pyrophosphate ((Ca2P2O7, Mohs hardness 5.0), dicalcium phosphate anhydrous (CaHPO4, Mohs hardness 3.5), hydrated aluminum phosphate (AlPO4·2H2O, Mohs hardness 4.5); silica (SiO2, Mohs hardness 5.0); hardness 5.0-6.0), potassium aluminum silicate (KAlSi3O8, Mohs hardness 6), copper silicate (CuSiO3·H2O, Mohs hardness 5.0); calcium borosilicate hydroxide (Ca2B5SiO9(OH)5, Mohs hardness 3.5); alumina (AlO2, Mohs hardness 10.0); calcium sulfate (CaSO4, Mohs hardness 3.5), barium sulfate (BaSO4, Mohs hardness 3-3.5), mica (Mohs hardness 2.5-5.3), and combinations thereof.

[0033]

[0037] In certain embodiments, it may be desirable to utilize mineral particles that are "flaky" to improve the surface and mechanical properties of the composition. In such embodiments, the particles generally have a relatively high aspect ratio (e.g., average diameter divided by average thickness), such as about 4 or more, in some embodiments about 10 or more, and in some embodiments, about 40 to about 250. The average diameter of the particles may range, for example, from about 5 micrometers to about 200 micrometers, in some embodiments from about 8 micrometers to about 150 micrometers, and in some embodiments, from about 10 micrometers to about 100 micrometers, as determined using laser diffraction techniques, for example, according to ISO 13320:2009 (e.g., using a Horiba LA-960 particle size distribution analyzer). The average thickness may similarly be about 2 micrometers or less, in some embodiments from about 5 nanometers to about 1 micrometer, and in some embodiments, from about 20 nanometers to about 500 nanometers. The flake particles are typically formed from natural and / or synthetic silicate minerals such as mica, halloysite, kaolinite, illite, montmorillonite, vermiculite, palygorskite, pyrophyllite, calcium silicate, aluminum silicate, wollastonite, and the like. For example, mica is particularly suitable. Any form of mica can generally be utilized, such as muscovite (KAl2(AlSi3)O 10 (OH)2), biotite (K(Mg,Fe)3(AlSi3)O 10 (OH)2), phlogopite (KMg3(AlSi3)O 10 (OH)2), red mica (K(Li,Al) 2-3 (AlSi3)O 10 (OH)2), glauconite (K,Na)(Al,Mg,Fe)2(Si,Al)4O 10 (OH)2). Muscovite micas are particularly suitable for use in polymer compositions.

[0034]

[0038] Of course, in other embodiments, the mineral particles may have a shape that is generally granular or nodular in nature. In such embodiments, the particles may have a median size (e.g., diameter) of about 0.5 to about 20 micrometers, in some embodiments about 1 to about 15 micrometers, in some embodiments about 1.5 to about 10 micrometers, and in some embodiments about 2 to about 8 micrometers, as determined using laser diffraction techniques (e.g., using a Horiba LA-960 particle size distribution analyzer) according to, for example, ISO 13320:2009. Examples of such granular particles include, for example, barium sulfate.

[0035] ii. Glass fiber

[0039] One beneficial aspect of the present invention is that good strength properties can be achieved without adversely affecting the surface properties of the resulting part. To help ensure that such properties are maintained, it is generally desirable for the polymer composition to remain substantially free of traditional fibrous fillers, such as glass fibers. Thus, if utilized, glass fibers typically comprise no more than about 10 wt.%, in some embodiments no more than about 5 wt.%, and in some embodiments, from about 0.001 wt.% to about 3 wt.% of the polymer composition.

[0036] iii. Other additives

[0040] A wide variety of other additional additives may also be included in the polymer composition, such as lubricants, conductive fillers (e.g., carbon fibers, carbon nanotubes, graphite, ionic liquids, etc.), thermally conductive fillers (e.g., carbon black, graphite, boron nitride, etc.), pigments, antioxidants, stabilizers, surfactants, waxes, flame retardants, anti-sag additives, nucleating agents (e.g., boron nitride), tribological agents (e.g., fluoropolymers), and other materials added to improve properties and processability. For example, lubricants that can withstand the processing conditions of liquid crystal polymers without substantial degradation can be utilized in the polymer composition. Examples of such lubricants include fatty acid esters, salts thereof, esters, fatty acid amides, organophosphate esters, and hydrocarbon waxes of the type typically used as lubricants in the processing of engineering plastic materials, including mixtures thereof. Suitable fatty acids typically have a backbone carbon chain of about 12 to about 60 carbon atoms, such as myristic acid, palmitic acid, stearic acid, arachic acid, montanic acid, octadecinic acid, parinaric acid, etc. Suitable esters include fatty acid esters, fatty alcohol esters, wax esters, glycerol esters, glycol esters, and complex esters. Fatty acid amides include fatty acid primary amides, fatty acid secondary amides, methylene and ethylene bisamides, and alkanolamides, such as palmitic acid amide, stearic acid amide, oleic acid amide, N,N'-ethylene bisstearamide, etc. Also suitable are metal salts of fatty acids, such as calcium stearate, zinc stearate, magnesium stearate, etc.; hydrocarbon waxes, including paraffin wax, polyolefin and oxidized polyolefin waxes, and microcrystalline waxes. Particularly suitable lubricants are stearic acids, salts or amides, such as pentaerythritol tetrastearate, calcium stearate, or N,N'-ethylenebisstearamide. If utilized, the lubricant typically comprises from about 0.05 wt.% to about 1.5 wt.%, and in some embodiments from about 0.1 wt.% to about 0.5 wt.% (by weight) of the polymer composition.

[0037] II. Formation

[0041] The components used to form the polymer composition may be combined together using any of a variety of different techniques, as known in the art. In one particular embodiment, for example, the liquid crystal polymer, the precious metal catalyst, the silicate fiber, and any other optional additives are melt processed as a mixture in an extruder to form the polymer composition. The mixture may be melt kneaded in a single or multiple screw extruder at a temperature of about 250°C to about 450°C. In one embodiment, the mixture may be melt processed in an extruder that includes multiple temperature zones. The temperature of the individual zones is typically set within a range of about -60°C to about 25°C relative to the melt temperature of the liquid crystal polymer. By way of example, the mixture may be melt processed using a twin screw extruder, such as a Leistritz 18mm co-rotating fully intermeshing twin screw extruder. The mixture may be melt processed using a versatile screw design. In one embodiment, the mixture containing all of the components may be fed by a volumetric feeder to a feed port in the first barrel. In another embodiment, different components may be added at different addition points in the extruder, as is known. For example, the liquid crystal polymer may be applied at a feed port and certain additives (e.g., precious metal catalysts) may be fed at the same or different temperature zones downstream therefrom. Regardless, the resulting mixture may be melted, mixed, and then extruded through a die. The extruded polymer composition may then be quenched in a water bath to solidify, pelletized in a pelletizer, and then dried.

[0038] III. Molded Interconnect Devices

[0042] In certain embodiments, the polymer composition may be utilized to mold interconnect devices. For example, the device may include a substrate comprising the polymer composition of the present invention and one or more conductive elements plated thereon. The substrate may be formed using a variety of different molding techniques. Suitable techniques may include, for example, injection molding, low pressure injection molding, extrusion compression molding, gas injection molding, foam injection molding, low pressure gas injection molding, low pressure foam injection molding, gas extrusion compression molding, foam extrusion compression molding, extrusion molding, foam extrusion molding, compression molding, foam compression molding, gas compression molding, insert molding, pin insert molding, and the like. For example, an injection molding system may be utilized that includes a mold into which the polymer composition can be injected. The time in the injector may be controlled and optimized to prevent pre-solidification of the polymer matrix. Once the cycle time is reached and the barrel is full for ejection, a piston may be used to inject the composition into the mold cavity. Compression molding systems may also be utilized. Similar to injection molding, the shaping of the polymer composition into the desired article also occurs in a mold. The composition may be placed into a compression mold using any known technique, for example by being picked up by an automated robotic arm. The temperature of the mold may be maintained at or above the solidification temperature of the polymer matrix for a desired time to allow solidification. The molded product may then be solidified by bringing it to a temperature below that of the melting temperature. The resulting product may be demolded. The cycle time of each molding process may be adjusted to suit the polymer matrix, achieve sufficient bonding, and improve the productivity of the overall process.

[0039]

[0043] The conductive elements may be deposited on the substrate using any of a variety of known plating techniques, such as electrolytic plating, electroless plating, digital printing, aerosol jet printing, and the like. The conductive elements may include one or more of a variety of conductive materials, such as metals, e.g., gold, silver, nickel, aluminum, copper, and mixtures or alloys thereof. In one embodiment, for example, the conductive elements may include copper and / or nickel (e.g., pure or alloys thereof). If desired, a seed layer may be formed on the substrate first to facilitate the plating process. Methods for forming the desired interconnect pattern may vary as known to those skilled in the art. For example, in certain cases, a pattern may first be formed on the surface of the substrate based on the desired circuit interconnect pattern. This may be accomplished using a variety of known techniques, such as laser ablation or patterning, plasma etching, ultraviolet light treatment, acid etching, and the like. After formation, the resulting interconnect pattern may be plated with the desired conductive elements. However, in other cases, the surface of the substrate (e.g., the entire surface) may be plated and then ablated using techniques such as those mentioned above to form the desired interconnect pattern. In one embodiment, for example, the plated surface may be laser ablated to form the desired interconnect pattern.

[0040]

[0044] Regardless of the method utilized, the method by which the surface is plated may also be selected based on techniques known in the art. In one embodiment, for example, the surface of the substrate may be contacted with an activation solution containing a precious metal, such as palladium, platinum, iridium, rhodium, and mixtures thereof. Palladium is particularly preferred. The presence of a precious metal catalyst in the polymer composition allows the activation solution to exhibit good adhesion to the substrate for the subsequent plating operation. Of course, in certain cases, the precious metal catalyst itself may function as an activator so that a subsequent solution is not required. In any case, after the optional activation step, a first metal layer may be formed thereon on the substrate, such as by electroless and / or electrolytic plating. Electroless plating may occur by an autocatalytic reaction in which the metal deposited on the surface acts as a catalyst for further deposition. Typically, nickel and / or copper are electrolessly plated on the surface of the substrate. Electroless nickel plating may be achieved, for example, using a solution containing a nickel salt (e.g., nickel sulfate). Electrolytic plating may also be utilized in which the substrate is contacted with a metal solution and subjected to an electric current to initiate deposition of the metal. If desired, the substrate surface may be roughened prior to plating using various known techniques, such as laser ablation, plasma etching, ultraviolet treatment, fluorination, etc. Among other things, such roughening helps to facilitate plating in the desired interconnect pattern. In addition, the substrate may also be subjected to one or more additional steps to form a final metal coating layer. For example, a second metal layer may be electrolytically deposited on the first metal layer (e.g., electrolytically and / or electrolessly plated copper and / or nickel). The second metal layer may include, for example, copper or nickel. In certain embodiments, one or more additional metal layers, such as copper and / or nickel, may also be electrolytically deposited on the second metal layer.

[0041] IV. Antenna Module

[0045] The molded interconnect device may be particularly suitable for use in antenna modules. In such embodiments, the plated conductive elements may be antenna elements (e.g., antenna resonating elements). The conductive elements may form a variety of different types of antennas, such as patch antenna elements, inverted-F antenna elements, closed and open slot antenna elements, loop antenna elements, antennas having resonating elements formed from monopoles, dipoles, planar inverted-F antenna elements, hybrids of these designs, and the like. In one particular embodiment, for example, the antenna module may include a shielding member configured to cover the communication circuitry, and a dielectric on which one or more antenna elements are disposed. The shielding member may include a substrate plated with a metal coating. Optionally, the substrate of the dielectric and / or shielding member may comprise the polymer composition of the present invention. In certain embodiments, an interconnecting member electrically connected with the communication circuitry and the antenna elements may also be utilized in the antenna module. The interconnecting member may likewise include a substrate plated with a metal coating. Optionally, the substrate of the interconnecting member may comprise the polymer composition of the present invention. One advantage of utilizing polymer compositions in such components (e.g., substrates of dielectrics and interconnect members) is that by using silicate fibers of a certain size and / or shape, it is possible to ensure that they do not substantially extend beyond the surface of the component. In this way, silicate fibers from one component do not contact the metal coating of another component, which could otherwise cause a shorted electrical connection.

[0042]

[0046] For example, referring to FIGS. 1 to 4, an example of such an antenna module 1 is shown in more detail. As shown, the antenna module 1 includes a circuit device 93 arranged on a substrate 91; a communication circuit 94 for processing radio signals; and a cover member 11 covering the communication circuit 94. The cover member 11 may be arranged on the substrate 91 so as to cover all or substantially all of the front surface (the surface on the positive area side in the -z axis) of the substrate 91. A conductive line (not shown) may be electrically connected to the circuit device 93, which is a component of the communication circuit 94. Similarly, a connection pad 95 may be formed on the rear surface (the surface on the negative area side in the -z axis) of the substrate 91. The connection pad 95 may be used to electrically connect the antenna module 1 to each part of the device to which it is attached. The cover member 11 may include a dielectric 12 on which an antenna element 51 for transmitting and receiving radio frequency signals is arranged. The dielectric 12 covers at least a portion of a shield member 71, and the shield member 71 may optionally include a conductive metal such as an aluminum alloy or a copper alloy. For convenience, the dielectric 12 is shown separately in FIG. 2, but it should be understood that the dielectric 12 may be formed as an integral member with the shield member 71 (eg, insert molded).

[0043]

[0047] The shielding member 71 in the illustrated embodiment includes a top panel 72 that is a planar member having four side panels 73 extending downward (in the negative direction on the -z axis) therefrom. Although not required, adjacent side panels 73 may be spaced apart from one another to form corner openings 73a. Similarly, one or more openings 72a that function as through holes may be formed in the top panel 72 as well. When the dielectric 12 is formed, a resin as a raw material is passed through the openings to form a connection 12e in the opening that connects between the upper panel 12a and the lower panel 12b of the dielectric 12.

[0044]

[0048] Also, a notch 74 may be formed in the shield member 71. Similarly, the interconnecting member 75 may be disposed in the notch 74 without contacting the shield member 71. For example, the notch 74 and the interconnecting member 75 may be disposed in a portion adjacent to one end (the left end in FIG. 3B ) of the long side line of the upper panel 72. The notch 74 may be formed so as to extend from a portion near the side line corresponding to the long line of the upper panel 72 to the side line, and from the side line to the lower end of the side panel 73, and open at the lower end. The interconnecting member 75 may have an elongated planar shape and be bent at a substantially right angle. The contour of the interconnecting member 75 may be a shape similar to that of the notch 74, and the dimensions of the contour may be formed to be smaller than the dimensions of the notch 74. As shown in the figure, the interconnecting member 75 has an upper portion 75a disposed generally in the same plane as the upper panel 72, and a side portion 75b disposed generally in the same plane as the side panel 73. Thus, the connection portion 12e of the dielectric 12 may be formed in a notch 74 surrounding the upper portion 75a. If desired, the interconnect member 75 and the shield member 71 may be integrally formed with the dielectric 12 (e.g., by insert molding). In such an embodiment, the interconnect member 75 and / or 71 may include a substrate, which may be formed from the polymer composition of the present invention, that is plated to form a conductive surface. In any event, at least one of the upper portions 75a is embedded in the dielectric 12 and electrically connected to the antenna element 51.

[0045]

[0049] The upper panel 12a of the dielectric 12 is positioned outside the shielding member 71 and covers almost the entire upper surface of the upper panel 72. Similarly, the lower panel 12b of the dielectric 12 is positioned inside the shielding member 71 and covers almost the entire lower surface of the upper panel 72. The connecting portion 12e of the dielectric 12 connects the upper panel 12a and the lower panel 12b, and a housing recess 12c for accommodating the upper panel 72 is provided between the panels 12a and 12b. Also, a communicating opening 12d penetrating the upper panel 12a in the thickness direction is formed at a corresponding portion of the upper portion 75a of the interconnecting member 75 on the upper panel 12a. The communicating opening 12d is a tapered opening whose diameter decreases downward, which is positioned on the upper portion 75a of the interconnecting member 75 and opens toward the upper surface 12f and the lower surface of the upper panel 12a. In this manner, the upper surface of the upper portion 75a is exposed to the outside of the cover member 11. In the example shown in the figure, a through hole is formed in the lower panel 12b at a location corresponding to the communication opening 12d, but preferably the through hole may be omitted.

[0046]

[0050] As described above, the antenna element 51 is disposed on the outer surface of the dielectric 12, i.e., the upper surface 12f of the upper panel 12a. In the illustrated embodiment, the antenna element 51 has a serpentine shape in a plan view. One end of the antenna element 51 contacts the edge of the communication opening 12d as a connection end 52, and the connection end 52 is electrically connected to the upper surface of the upper portion 75a of the interconnection member 75 through a communication pattern 53 disposed on the side of the communication opening 12d. The antenna element 51 may be plated on the upper surface 12f of the upper panel 12a by the above-mentioned method (e.g., electroless and / or electrolytic plating). The cover member 11 may also be attached to the surface of the base material 91 by soldering the lower end of the side panel 73 of the shield member 71 onto a connection pad (not shown) on the surface of the base material 91. In this way, as shown in FIGS. 4A and 4B, the communication circuit 94 and the communication circuit 93 are positioned in the box-shaped or container-shaped shield member 71. Also, at least a portion of the lower end of the side panel 73 of the shield member 71 may be in contact with a conductive line (not shown) formed on the surface of the base material 91. The lower end of the side portion 75b of the interconnection member 75 is a conductive line (not shown) for signals formed on the surface of the base material 91, and is connected to a conductive line included in the communication circuit 94. Therefore, the antenna element 51 is connected to the communication circuit 94 via the communication pattern 53 and the interconnection member 75, and is therefore able to transmit and receive radio frequency signals.

[0047]

[0051] Any of the components of the antenna module 1 described above may generally contain the polymer composition of the present invention. For example, the polymer composition may be utilized in the substrate 91, the cover member 11 (e.g., the dielectric 12, the shield member 71, the interconnect member 75, etc.), and the like. In one embodiment, for example, the dielectric 12 may include the polymer composition of the present invention and may include a metal coating plated thereon in the manner described above. Optionally, the interconnect member 75 may also include the polymer composition of the present invention and may include a metal coating plated thereon in the manner described above. As described above, one advantage of utilizing the polymer composition in such components is that silicate fibers from one component do not contact the metal coating of another component, which could otherwise cause a short circuit in the electrical connection.

[0048]

[0052] In certain embodiments, antenna modules including the polymeric compositions of the present invention may be particularly well suited for use in radio frequency antennas and antenna arrays for use in base stations, repeaters (e.g., "femtocells"), relay stations, terminals, user devices, and / or other suitable components of 5G systems. As used herein, "5G" generally refers to high-speed data communication via radio frequency signals. 5G networks and systems can communicate data at much faster rates than previous generations of data communication standards (e.g., "4G," "LTE"). For example, as used herein, "5G frequencies" may refer to frequencies of 1.5 GHz or higher, in some embodiments about 2.0 GHz or higher, in some embodiments about 2.5 GHz or higher, in some embodiments about 3.0 GHz or higher, in some embodiments about 3 GHz to about 300 GHz or higher, in some embodiments about 4 GHz to about 80 GHz, in some embodiments about 5 GHz to about 80 GHz, in some embodiments about 20 GHz to about 80 GHz, and in some embodiments about 28 GHz to about 60 GHz. Various standards and specifications have been published that quantify the requirements for 5G communications. As an example, the International Telecommunications Union (ITU) published the International Mobile Telecommunications-2020 ("IMT-2020") standard in 2015. The IMT-2020 standard specifies various data transmission criteria for 5G (e.g., downlink and uplink data rates, latency, etc.). The IMT-2020 standard defines uplink and downlink peak data rates as the minimum data rates for uploading and downloading data that a 5G system must support. The IMT-2020 standard specifies a downlink peak data rate requirement of 20 Gbit / s, and an uplink peak data rate of 10 Gbit / s. As another example, the 3G LTE standard specifies a 5G LTE standard for 5G LTE. rdThe Third Generation Partnership Project (3GPP) recently announced a new standard for 5G, referred to as "5G NR." In 2018, 3GPP published "Release 15," which defines "Phase 1" for the standardization of 5G NR. 3GPP defines the 5G frequency bands as "Frequency Range 1" (FR1), which generally includes sub-6 GHz frequencies, and "Frequency Range 2" (FR2), as frequency bands in the range of 20-60 GHz. The antenna modules described herein may meet or be certified as "5G" under standards published by 3GPP, such as Release 15 (2018), and / or the IMT-2020 standard.

[0049]

[0053] To achieve high-speed data communication at high frequencies, antenna elements and arrays may utilize small feature sizes / spacings (e.g., fine pitch technology) that can improve antenna performance. For example, the feature size (spacing between antenna elements, width of antenna elements), etc., generally depends on the wavelength ("λ") of the desired transmit and / or receive radio frequency propagating through the substrate dielectric on which the antenna elements are formed (e.g., nλ / 4, where n is an integer). Additionally, beamforming and / or beamsteering may be utilized to facilitate transmission and reception across multiple frequency ranges or channels (e.g., multiple-input multiple-output (MIMO), massive MIMO).

[0050]

[0054] High frequency 5G antenna elements can have various configurations. For example, 5G antenna elements may be or include coplanar waveguide elements, patch arrays (e.g., mesh-grid patch arrays), other suitable 5G antenna configurations. Antenna elements may be configured to provide MIMO, massive MIMO functionality, beam steering, and the like. As used herein, "massive" MIMO functionality generally refers to providing a large number of transmit and receive channels by an antenna array, for example, 8 transmit (Tx) and 8 receive (Rx) channels (abbreviated as 8x8). Massive MIMO functionality may be provided at 8x8, 12x12, 16x16, 32x32, 64x64, or more.

[0051]

[0055] The antenna elements can have a variety of configurations and arrangements and can be fabricated using a variety of manufacturing techniques. As an example, the antenna elements and / or associated elements (e.g., ground elements, feedlines, etc.) can utilize fine pitch technology. Fine pitch technology generally refers to small or fine spacing between its components or leads. For example, the feature size / dimension and / or spacing between antenna elements (or between antenna elements and a ground plane) can be about 5,000 micrometers or less, in some embodiments about 3,000 micrometers or less, in some embodiments 1,500 micrometers or less, in some embodiments 750 micrometers or less (e.g., center-to-center spacing of 1.5 mm or less), 650 micrometers or less, in some embodiments 550 micrometers or less, in some embodiments 450 micrometers or less, in some embodiments 350 micrometers or less, in some embodiments 250 micrometers or less, in some embodiments 150 micrometers or less, in some embodiments 100 micrometers or less, and in some embodiments 50 micrometers or less. However, it should be understood that smaller and / or larger feature sizes and / or spacings may be utilized within the scope of the present disclosure.

[0052]

[0056] As a result of such small feature sizes, the antenna module can be realized with a large number of antenna elements in a small footprint. For example, the antenna array may have an average antenna element density of more than 10 antenna elements per square centimeter, in some embodiments more than 50 antenna elements per square centimeter, in some embodiments more than 200 antenna elements per square centimeter, in some embodiments more than 1,000 antenna elements per square centimeter, in some embodiments more than 3,000 antenna elements per square centimeter, and in some embodiments more than about 5,000 antenna elements per square centimeter. Such a dense arrangement of antenna elements can provide a larger number of channels for MIMO functionality per unit area of ​​antenna area. For example, the number of channels may correspond to (e.g., be equal to or proportional to) the number of antenna elements.

[0053]

[0057] Regardless of its particular configuration, the antenna module may be utilized in a variety of different electronic components. As an example, the antenna module may be formed in electronic components such as desktop computers, portable computers, handheld electronic devices, and in-vehicle equipment. In one preferred configuration, the antenna module is formed in a housing of a relatively compact portable electronic component that has a relatively small available internal space. Examples of suitable portable electronic components include mobile phones, laptop computers, small portable computers (e.g., ultraportable computers, netbook computers, and tablet computers), wristwatch devices, pendant devices, headphone and earphone devices, media players with wireless communication capabilities, handheld computers (sometimes referred to as personal digital assistants), remote controllers, global positioning system (GPS) devices, handheld gaming devices, and the like. The antenna may also be integrated with other components of the handheld device, such as a camera module, a speaker, or a battery cover.

[0054]

[0058] The invention may be better understood with reference to the following examples. EXAMPLES

[0055] Test Method

[0059] Melt viscosity: Melt viscosity (Pa s) was measured at a shear rate of 400 s using a Dynisco LCR7001 capillary rheometer. -1 or 1,000s -1 and 15°C above the melt temperature (e.g., about 325°C) according to ISO11443:2021. The rheometer orifice (die) may have a diameter of 1 mm, a length of 20 mm, an L / D ratio of 20.1, and an entrance angle of 180°. The barrel diameter may be 9.55mm+0.005mm and the rod length may be 233.4mm.

[0056]

[0060] Melting temperature: Melting temperature ("Tm") can be determined by differential scanning calorimetry ("DSC") as known in the art. Melting temperature is the differential scanning calorimetry (DSC) peak melting temperature as determined by ISO11357-3:2018. For the DSC procedure, samples were heated and cooled at 20°C per minute as described in ISO standard 10350, using DSC measurements performed on a TA Q2000 Instrument.

[0057]

[0061] Deflection Temperature Under Load ("DTUL"): Deflection temperature under load may be determined in accordance with ISO 75-2:2013 (technically equivalent to ASTM D648). More specifically, a test specimen sample having a length of 80 mm, a thickness of 10 mm, and a width of 4 mm may be subjected to an edgewise three-point bending test with a prescribed load (maximum outer fiber stress) of 1.8 megapascals. The specimen may be lowered into a silicone oil bath with a temperature increase of 2°C per minute until it deflects 0.25 mm (0.32 mm for ISO Test No. 75-2:2013).

[0058]

[0062] Tensile modulus, tensile stress and tensile elongation: Tensile properties may be tested according to ISO 527:2019 (technically equivalent to ASTM D638) using a Type 1A ISO tensile bar (80 mm long, 10 mm wide, and 4 mm thick). The test temperature may be 23°C and the test speed may be 5 mm / min. "Weld line" tensile properties may also be determined using the test method described above. For such properties, a double-gate ISO tensile bar (80 mm long, 10 mm wide, and 4 mm thick) is used.

[0059]

[0063] Flexural modulus, flexural stress and flexural elongation: Flexural properties may be tested according to ISO178:2019 (technically equivalent to ASTM D790). The test may be performed with a support span of 64 mm. The test may be performed on the central section of an uncut ISO 3167 multipurpose bar. The test temperature may be 23°C and the test speed may be 2 mm / min.

[0060]

[0064] Charpy Impact Strength: Charpy properties may be tested according to ISO179-1:2010 (technically equivalent to ASTM D256-10, Method B). The test may be performed using a Type 1 specimen size (80 mm length, 10 mm width and 4 mm thickness). When testing notched impact strength, the notch may be a Type A notch (0.25 mm bottom radius). The specimen may be cut from the center of a utility bar using a single tooth milling machine. The test temperature may be 23°C.

[0061] Comparative Example 1

[0065] Comparative Example 1 is made from 58 wt.% liquid crystal polymer (LCP1), 37 wt.% calcium pyrophosphate, and 5 wt.% precious metal catalyst (3.5% palladium on kaolin). LCP1 is made from 60% HBA, 4.25% HNA, 12.5% ​​BP, 17.5% TA, and 5% APAP. Compounding was performed using a 32 mm twin screw extruder.

[0062] Comparative Example 2

[0066] Comparative Example 2 is formed from 66.2 wt.% LCP1, 30 wt.% glass fiber, 3.5 wt.% precious metal catalyst (3.5% palladium on kaolin) and 0.3 wt.% lubricant. Compounding was performed using a 32 mm twin screw extruder.

[0063] Example 1

[0067] Example 3 is formed from 66.2 wt.% LCP1, 30 wt.% wollastonite fiber (Nyglos™ 8), 3.5 wt.% precious metal catalyst (0.25% palladium on kaolin) and 0.3 wt.% lubricant.

[0064]

[0068] Comparative Examples 1-2 and Example 1 are tested for thermal and mechanical properties. The results are shown below.

[0065] [Table 1]

[0066]

[0069] These and other modifications and variations of the present invention may be practiced by those skilled in the art without departing from the spirit and scope of the present invention. In addition, it should be understood that aspects of the various embodiments may be interchanged both in whole or in part. Furthermore, those skilled in the art will appreciate that the foregoing description is for illustrative purposes only and is not intended to limit the present invention as further described in such appended claims.

Claims

1. A platable polymeric composition comprising 100 parts by weight of a polymer matrix comprising a thermotropic liquid crystal polymer, from about 10 parts by weight to about 80 parts by weight of silicate fibers, and a precious metal catalyst.

2. 10. The plateable polymeric composition of claim 1 , exhibiting a weld line tensile strain at break of greater than or equal to about 0.3% determined according to ISO 527:2019.

3. 10. The plateable polymeric composition of claim 1 , exhibiting a weld line tensile strain at break of greater than or equal to about 0.35% determined according to ISO 527:2019.

4. 1,000s -1 10. The plateable polymeric composition of claim 1, exhibiting a melt viscosity of about 0.1 to about 80 Pa·s determined at a shear rate of about 0.1 to about 80 Pa·s and at a temperature about 15° C. above the melting temperature of said polymeric composition.

5. The plateable polymeric composition of claim 1 having a melting temperature of about 280°C to about 400°C.

6. 10. The plateable polymeric composition of claim 1, exhibiting a deflection temperature under load of about 200°C or greater, determined at 1.8 MPa.

7. 10. The platable polymer composition of claim 1, wherein the liquid crystalline polymer comprises from about 40 wt.% to about 90 wt.% of the polymer composition.

8. 10. The plateable polymer composition of claim 1, wherein the thermotropic liquid crystalline polymer comprises repeat units derived from one or more aromatic dicarboxylic acids, one or more aromatic hydroxycarboxylic acids, or a combination thereof.

9. The platable polymer composition of claim 8, wherein the aromatic hydroxycarboxylic acid comprises 4-hydroxybenzoic acid, 6-hydroxy-2-naphthoic acid, or a combination thereof.

10. The plateable polymeric composition of claim 8, wherein the aromatic dicarboxylic acid comprises terephthalic acid, isophthalic acid, 2,6-naphthalenedicarboxylic acid, or a combination thereof.

11. 9. The plateable polymer composition of claim 8, wherein the thermotropic liquid crystalline polymer further comprises repeat units derived from one or more aromatic diols.

12. The plateable polymer composition of claim 11, wherein the aromatic diol comprises hydroquinone, 4,4'-biphenol, or a combination thereof.

13. The platable polymer composition of claim 1 , wherein said thermotropic liquid crystalline polymer is wholly aromatic.

14. 10. The platable polymer composition of claim 1, wherein the total amount of repeat units derived from naphthenic hydroxycarboxylic acids and / or dicarboxylic acids is about 20 mol. % or less.

15. 15. The plateable polymer composition of claim 14, wherein the liquid crystalline polymer comprises repeat units derived from 6-hydroxy-2-naphthoic acid in an amount of about 0.5 mol. % to about 10 mol. %.

16. 16. The plateable polymer composition of claim 15, wherein the liquid crystalline polymer comprises repeat units derived from 6-hydroxy-2-naphthoic acid and 4-hydroxybenzoic acid in a molar ratio of about 10 to about 30.

17. The platable polymeric composition of claim 1 , wherein said silicate fibers comprise wollastonite.

18. The plateable polymeric composition of claim 1, wherein the silicate fibers have a volume average length of about 1 to about 200 micrometers.

19. The platable polymeric composition of claim 1 , wherein said silicate fibers have an aspect ratio of about 2 to about 50.

20. The platable polymeric composition of claim 1, wherein said silicate fibers have an average diameter of about 1 to about 35 micrometers.

21. 10. The plateable polymer composition of claim 1, wherein the catalyst comprises a precious metal component comprising palladium, iridium, ruthenium, platinum, rhodium, or alloys or combinations thereof.

22. The plateable polymeric composition of claim 1 , wherein the catalyst comprises a precious metal component comprising palladium.

23. The plateable polymer composition of claim 1 , wherein the catalyst comprises a precious metal component supported by a matrix material.

24. The plateable polymeric composition of claim 23 , wherein the matrix material comprises a silicate.

25. The plateable polymer composition of claim 1, wherein the catalyst comprises a precious metal component comprising from about 0.1 parts by weight to about 6 parts by weight per 100 parts by weight of the polymer matrix.

26. The plateable polymer composition of claim 1, wherein the catalyst comprises from about 0.5 to about 20 parts by weight per 100 parts by weight of the polymer matrix.

27. The platable polymeric composition of claim 1 which is glass fiber free.

28. The platable polymeric composition of claim 1 which is free of laser activatable additives.

29. 13. A molded interconnect device comprising a substrate having a surface having at least one conductive element plated thereon, said substrate comprising the polymer composition of claim 1.

30. 30. The molded interconnect device of claim 29, wherein the conductive elements comprise copper, nickel, or a combination thereof.

31. 30. A method for forming a molded interconnect device according to claim 29, comprising forming an interconnect pattern on a surface of the substrate and then plating the patterned surface of the substrate.

32. 30. The method for forming a molded interconnect device of claim 29, comprising plating a surface of the substrate and thereafter forming an interconnect pattern on the plated surface of the substrate.

33. 32. The method of claim 31 , wherein the interconnect pattern is formed by a method including laser ablation.

34. 32. The method of claim 31 , wherein the plating step comprises electroless plating, electrolytic plating, or a combination thereof.

35. 30. An antenna module including the molded interconnect device of claim 29, wherein the conductive element is an antenna element configured to transmit and / or receive radio frequency signals.

Citation Information

Patent Citations

  • Liquid crystal polymer material for environment-friendly electroplating and preparation method thereof

    CN107674416A

  • Epoxy resin hardener and epoxy resin composition

    JP1994179800A

  • Catalyst filler for electroless metal plating, resin composition for electroless metal plating and composite formed article

    JP1996283952A

  • Liquid crystalline polyester resin for molded product and molded circuit board

    JP2003268089A

  • Liquid crystal polymer composition

    JP2016510831A