Molybdenum compound, its manufacturing method, and manufacturing method of thin film containing the same
A thermally stable and volatile molybdenum compound, produced via ligand coordination, addresses the performance gaps in existing precursors by enabling uniform and reliable thin film deposition for next-generation semiconductors.
Patent Information
- Application Number
- JP2024534612
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-12-13
- Filing Date
- 2022-12-01
- Publication Date
- 2024-11-28
- Estimated Expiration
- 2042-12-01
AI Technical Summary
Current molybdenum precursors do not meet the performance requirements for next-generation semiconductor manufacturing, lacking thermal stability, volatility, and uniform deposition capabilities.
A molybdenum compound represented by specific chemical formulas with improved thermal stability and volatility, produced through a method involving coordination with cyclopentadiene-based ligands, is used in thin film deposition processes like ALD and CVD to achieve high molybdenum content and uniform deposition.
The molybdenum compound enables high-yield, high-purity production of thin films with uniformity and stable deposition rates, suitable for advanced semiconductor applications.
Smart Images

Figure 2024544251000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a molybdenum compound, a method for producing the same, a method for producing a thin film containing the same, and a thin film containing the same. [Background technology]
[0002] A variety of organometallic precursors are used to form metal thin films. A variety of techniques are used for the deposition of thin films, including reactive sputtering, ion-assisted deposition, sol-gel deposition, metalorganic chemical vapor deposition (MOCVD), a type of chemical vapor deposition (CVD), and atomic layer deposition (ALD), also known as atomic layer epitaxy (ALE). Chemical vapor deposition (CVD) and atomic layer deposition (ALD) have the advantages of good composition control, high film uniformity, good doping control, and excellent conformal deposition, which can achieve uniform step coverage even in highly non-planar microelectronic device geometries.
[0003] Chemical vapor deposition (CVD) is a chemical process in which organometallic precursors are used to form thin films on substrates. In a typical chemical vapor deposition (CVD) process, precursors are reacted or decomposed on the surface of a substrate as they are passed over the substrate in a low or atmospheric pressure chamber. Volatile by-products are removed by a gas stream.
[0004] Atomic layer deposition (ALD) is a method that allows precise thickness control, uniform step coverage, and excellent conformal deposition, and is a method of growing films sequentially while reacting on the surface of a substrate. It is usually performed in four steps: pulse A, in which a first precursor made of an organic metal forms a monolayer on the substrate, purge A, which removes excess first precursor, pulse B, in which a second precursor, a non-metallic precursor, induces a reaction between the first precursor and the substrate, and purge B, which removes unreacted material. These four steps are repeated until a thin film of the desired thickness is obtained.
[0005] Thin films are used in a variety of important applications such as semiconductor device fabrication and nanotechnology. Such applications include, for example, conductive films, high refractive index optical coatings, anti-corrosion coatings, photocatalytic self-cleaning glass coatings, biocompatible coatings, gate dielectric insulating films in field effect transistors (FETs), dielectric capacitor layers, capacitor electrodes, gate electrodes, adhesive diffusion barriers, and integrated circuits. Thin films are also used in microelectronic applications such as high-k dielectric oxides for dynamic random access memory (DRAM) applications, infrared detectors, and ferroelectric perovskites used in non-volatile ferroelectric random access memories (NV-FeFAMs). As microelectronic components continue to shrink in size, the need for the use of dielectric thin films increases.
[0006] Many current molybdenum precursors for use in CVD and ALD do not meet the performance requirements required to enable new processes for the manufacture of next-generation devices such as semiconductors. There is a need for the development of molybdenum precursors with improved thermal stability, higher volatility, increased vapor pressure, uniform deposition, and stable deposition rates. Summary of the Invention [Problem to be solved by the invention]
[0007] An object of the present invention is to provide a molybdenum compound and a method for producing the same.
[0008] Another object of the present invention is to provide a composition for depositing a molybdenum-containing thin film, which comprises the molybdenum compound.
[0009] It is still another object of the present invention to provide a method for producing a molybdenum-containing thin film using the molybdenum compound.
[0010] The present invention also provides a molybdenum-containing thin film having a molybdenum content of 70% or more. [Means for solving the problem]
[0011] The present invention provides a molybdenum compound represented by the following chemical formula 1:
[0012] [ka] [In the above Chemical Formula 1, L is C1-C10 alkylene or C3-C10 cycloalkylene, and the alkylene and cycloalkylene of L may be further substituted with C1-C10 alkyl; R1 to R4 are each independently hydrogen or C1-C7 alkyl; R5 is hydrogen, C1-C10 alkyl, C6-C12 aryl, C6-C12 arylC1-C10 alkyl, or C1-C10 alkoxy; Y is -NR 11 R 12 , -OR 13 , or -SR 14 and R 11 ~R 14 are each independently C1-C10 alkyl, haloC1-C10 alkyl, C3-C10 cycloalkyl, C6-C12 aryl, C6-C12 arylC1-C10 alkyl, or11 and R 12 may be linked to form a ring.
[0013] In one embodiment, in the above Chemical Formula 1, L may be C1-C6 alkylene, and the alkylene of L may be further substituted with C1-C6 alkyl, R1 to R4 may each independently be hydrogen or C1-C4 alkyl, and R5 may be hydrogen or C1-C6 alkyl.
[0014] Also, Y is -NR 11 R 12 , -OR 13 , or -SR 14 wherein R 11 ~R 14 are each independently C1-C6 alkyl, haloC1-C6 alkyl, C3-C6 cycloalkyl, C6-C12 aryl, or C6-C12 arylC1-C6 alkyl, or 11 and R 12 may be linked by a C2-C6 alkylene to form a ring.
[0015] The molybdenum compound according to a preferred embodiment may be represented by the following formula 2:
[0016] [ka] [In the above Chemical Formula 2, R1 to R4 are each independently hydrogen or C1-C4 alkyl; R5 is hydrogen or C1-C4 alkyl; Y is -NR 11 R 12 , -OR 13 , or -SR 14 and R 11 ~R 14 are each independently C1-C4 alkyl, haloC1-C4 alkyl, or C3-C6 cycloalkyl, or 11 and R 12may be linked by a C2-C6 alkylene to form an alicyclic ring; and m is an integer from 1 to 4.
[0017] In one embodiment, the molybdenum compound may be selected from the following compounds: [ka]
[0018] The present invention provides a method for producing a molybdenum compound, and the method for producing a molybdenum compound represented by the following Chemical Formula 1 according to one embodiment may include the steps of reacting a molybdenum compound represented by the following Chemical Formula 3 with a ligand capable of coordinating with the molybdenum compound to produce an intermediate, and reacting the intermediate with a cyclopentadiene-based ligand represented by the following Chemical Formula 4 to produce the molybdenum compound represented by the following Chemical Formula 1:
[0019] [ka]
[0020] [ka]
[0021] [ka] [In the above Chemical Formulas 1 and 4, L is C1-C10 alkylene or C3-C10 cycloalkylene, and the alkylene and cycloalkylene of L may be further substituted with C1-C10 alkyl; R1 to R5 are each independently hydrogen or C1-C7 alkyl; Y is -NR 11 R 12 , -OR 13 , or -SR 14 and R 11 ~R 14are each independently C1-C10 alkyl, haloC1-C10 alkyl, C3-C10 cycloalkyl, C6-C12 aryl, C6-C12 arylC1-C10 alkyl, or 11 and R 12 may be linked to form a ring.
[0022] The present invention provides a composition for depositing a molybdenum-containing thin film, comprising a molybdenum compound according to one embodiment of the present invention.
[0023] The present invention also provides a method for producing a molybdenum-containing thin film, comprising producing a thin film using the composition for depositing a molybdenum-containing thin film.
[0024] In one embodiment, the method comprises: a) increasing the temperature of a substrate mounted in a chamber; b) injecting a reaction gas and the composition for depositing a molybdenum-containing thin film into the chamber to produce a molybdenum-containing thin film.
[0025] The reactive gas according to one embodiment may be oxygen (O2), ozone (O3), distilled water (HO), hydrogen peroxide (HO2), nitric oxide (NO), nitrous oxide (NO2), nitrogen dioxide (NO2), ammonia (NH3), nitrogen (N2), hydrazine (N2H4), amines, diamines, carbon monoxide (CO), carbon dioxide (CO2), C1 to C4, 12 The gas may be any one or more selected from the group consisting of saturated or unsaturated hydrocarbons, hydrogen (H2), argon (Ar), and helium (He).
[0026] In one embodiment, the method comprises: The method may further include a step of injecting a reaction gas into the chamber after the steps c) and b), and the steps b) and c) constitute one cycle, and the cycle may be repeated.
[0027] The present invention provides a molybdenum-containing thin film having a molybdenum content of 70% or more. Effect of the Invention
[0028] The molybdenum compound according to the present invention has improved thermal stability, high volatility, and improved vapor pressure, and therefore exhibits a uniform and stable deposition rate, allowing the formation of a thin film with high reliability.
[0029] The method for producing a molybdenum compound according to the present invention can easily produce a molybdenum compound industrially in high yield and with high purity under mild conditions and by simple steps.
[0030] The method for producing a molybdenum-containing thin film according to the present invention can have high film uniformity and good doping controllability by atomic layer deposition (ALD) and chemical vapor deposition (CVD), etc. Furthermore, the method can provide conformal step coverage for a three-dimensional semiconductor device.
[0031] The molybdenum-containing thin film according to the present invention is deposited at a high deposition rate of at least 1.36 Å per cycle and has a molybdenum content of at least 70%. [Brief description of the drawings]
[0032] [Figure 1] 1 is a photograph showing the results of scanning electron microscope measurement of the molybdenum-containing thin film of Example 3. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0033] The present invention provides a molybdenum compound, a method for producing the same, a composition for vapor deposition of a molybdenum-containing thin film containing the same, and a method for producing a thin film using the same.
[0034] As used herein, the singular forms are intended to include the plural forms as well, unless the context clearly indicates otherwise.
[0035] "Comprising" as used herein is an open-ended term having the same meaning as terms such as "comprising," "containing," "having," or "characterized by," and does not exclude additional, unrecited elements, materials, or steps.
[0036] The "alkyl" according to the present invention may be either linear or branched and may have 1 to 10 carbon atoms, preferably 1 to 6 carbon atoms, and in yet another embodiment, the alkyl may have 1 to 4 carbon atoms.
[0037] The term "cycloalkyl" as used herein means a non-aromatic monocyclic or multicyclic ring system having 3 to 10 carbon atoms, which may be a 3- to 6-membered ring and may have an unsaturated bond in the ring.
[0038] By "alkylene" and "cycloalkylene" according to the present invention is meant a divalent organic radical derived from an "alkyl" and a "cycloalkyl" by removing one hydrogen, where alkyl and cycloalkyl are as defined above.
[0039] By "halo" in the present invention is meant fluorine, chlorine, bromine, or iodine.
[0040] "Haloalkyl" according to the present invention means an alkyl group in which one or more hydrogen atoms are replaced by halogen atoms. For example, haloalkyl includes -CF3, -CHF2, -CH2F, -CBr3, -CHBr2, -CH2Br, -CCl3, -CHCl2, -CH2CI, -CHI2, -CH2I, -CH2-CF3, -CH2-CHF2, -CH2-CH2F, -CH2-CBr3, -CH2-CHBr2, -CH2-CH2Br, -CH2-CCl3, -CH2-CHCl2, -CH2-CH2CI, -CH2-CCI3, -CH2-CHI2, -CH2-CH2I, and the like, where alkyl and halogen are as defined above.
[0041] By "alkoxy" according to the present invention is meant -O-(alkyl), including -OCH, -OCHCH, -O(CH)CH, -O(CH)CH, -O(CH)CH, -O(CH)CH, -O(CH)CH, and the like, where alkyl is as defined above.
[0042] The term "aryl" as used herein means a carbocyclic aromatic group containing 6 to 20 ring atoms. Representative examples include, but are not limited to, phenyl, tolyl, xylyl, naphthyl, tetrahydronaphthyl, anthracenyl, fluorenyl, indenyl, azulenyl, and the like.
[0043] The term "arylalkyl" as used herein refers to an alkyl group in which one or more hydrogen atoms are substituted with aryl, where aryl and alkyl are as defined above. For example, arylalkyl includes, but is not limited to, benzyl, phenethyl, phenylvinyl, etc.
[0044] The number of carbon atoms described in the alkyl, alkoxy, etc. described in the present invention does not include the number of carbon atoms of the substituents. For example, C1-C10 alkyl means an alkyl having 1 to 10 carbon atoms, not including the number of carbon atoms of the alkyl substituents.
[0045] "Substituted" according to the present invention means that a hydrogen atom of the substituted moiety (eg, alkyl, aryl, or cycloalkyl) is replaced with a substituent.
[0046] The present invention will be described in detail below. In this regard, unless otherwise defined, the technical and scientific terms used have the meanings that are commonly understood by those having ordinary knowledge in the technical field to which the present invention belongs, and descriptions of known functions and configurations that may obscure the gist of the present invention in the following description will be omitted.
[0047] The present invention provides a molybdenum compound represented by the following chemical formula 1:
[0048] [ka] [In the above Chemical Formula 1, L is C1-C10 alkylene or C3-C10 cycloalkylene, and the alkylene and cycloalkylene of L may be further substituted with C1-C10 alkyl; R1 to R4 are each independently hydrogen or C1-C7 alkyl; R5 is hydrogen, C1-C10 alkyl, C6-C12 aryl, C6-C12 arylC1-C10 alkyl, or C1-C10 alkoxy; Y is -NR 11 R 12 , -OR 13 , or -SR 14 and R 11 ~R 14 are each independently C1-C10 alkyl, haloC1-C10 alkyl, C3-C10 cycloalkyl, C6-C12 aryl, C6-C12 arylC1-C10 alkyl, or 11 and R 12 may be linked to form a ring.
[0049] The molybdenum compound represented by Formula 1 according to the present invention exhibits excellent thermal stability, high volatility, and improved vapor pressure, and when used, a highly reliable molybdenum-containing thin film can be obtained.
[0050] In one embodiment, in the above formula 1, L may be C1-C6 alkylene, and the alkylene of L may be further substituted with C1-C6 alkyl, R1 to R4 may each independently be hydrogen or C1-C4 alkyl, and R5 may be hydrogen or C1-C6 alkyl.
[0051] Also, Y is -NR 11 R12 , -OR 13 , or -SR 14 wherein R 11 ~R 14 are each independently C1-C6 alkyl, haloC1-C6 alkyl, C3-C6 cycloalkyl, C6-C12 aryl, or C6-C12 arylC1-C6 alkyl, or 11 and R 12 may be linked by a C2-C6 alkylene to form an alicyclic ring.
[0052] The molybdenum compound according to a preferred embodiment may be represented by the following formula 2:
[0053] [ka] [In the above Chemical Formula 2, R1 to R4 are each independently hydrogen or C1-C4 alkyl; R5 is hydrogen or C1-C4 alkyl; Y is -NR 11 R 12 , -OR 13 , or -SR 14 and R 11 ~R 14 are each independently C1-C4 alkyl, haloC1-C4 alkyl, or C3-C6 cycloalkyl, or 11 and R 12 may be linked by a C2-C6 alkylene to form an alicyclic ring; m is an integer from 1 to 4.
[0054] A more preferred embodiment of the molybdenum compound may be represented by the following chemical formula 2-1.
[0055] [ka] [In the above Chemical Formula 2-1, R1 to R4 are each independently hydrogen or C1-C4 alkyl; R5 is hydrogen or C1-C4 alkyl; Y is -NR 11 R 12 , -OR 13 , or -SR 14 and R 11 ~R 14 are each independently C1-C4 alkyl or haloC1-C4 alkyl, or 11 and R 12 may be linked by a C2-C6 alkylene to form an alicyclic ring.
[0056] In one embodiment, the molybdenum compound may be selected from, but is not limited to, the following compounds: [ka]
[0057] The present invention provides a method for producing a molybdenum compound, and the method for producing a molybdenum compound represented by the following Chemical Formula 1 according to one embodiment may include the steps of reacting a molybdenum compound represented by the following Chemical Formula 3 with a ligand capable of coordinating with the molybdenum compound to produce an intermediate, and reacting the intermediate with a cyclopentadiene-based ligand represented by the following Chemical Formula 4 to produce the molybdenum compound represented by the following Chemical Formula 1:
[0058] [ka]
[0059] [ka]
[0060] [ka] [In the above Chemical Formulas 1 and 4, L is C1-C10 alkylene or C3-C10 cycloalkylene, and the alkylene and cycloalkylene of L may be further substituted with C1-C10 alkyl; R1 to R5 are each independently hydrogen or C1-C7 alkyl; Y is -NR 11 R 12 , -OR 13 , or -SR 14 and R 11 ~R 14 are each independently C1-C10 alkyl, haloC1-C10 alkyl, C3-C10 cycloalkyl, C6-C12 aryl, C6-C12 arylC1-C10 alkyl, or 11 and R 12 may be linked to form a ring.
[0061] The method for producing a molybdenum compound according to one embodiment of the present invention is carried out under mild conditions and is a method that can be easily mass-produced through simple steps.
[0062] The ligand capable of coordinating with the molybdenum compound according to an embodiment of the present invention may be any ligand recognizable by those skilled in the art, and specifically may be a compound capable of coordinating in place of three carbonyl groups in the molybdenum compound of Chemical Formula 3. More specifically, it may be a compound selected from 1,3,5-trimethylhexahydro-1,3,5-triazine (trimethyltriazacyclohexane) and acetonitrile.
[0063] The solvent used in the production method according to one embodiment may be any common organic solvent, but it is preferable to use one or more selected from the group consisting of hexane, pentane, dichloromethane (DCM), dichloroethane (DCE), toluene (Toluene), acetonitrile (MeCN), nitromethan, tetrahydrofuran (THF), N,N-dimethylformamide (DMF), and N,N-dimethylacetamide (DMA).
[0064] The reaction temperature can be a temperature used in ordinary organic synthesis, but may vary depending on the amount of reactants and starting materials. The reaction may be preferably performed at 20°C to 200°C, specifically, at 50°C to 150°C, and more specifically, at 70°C to 120°C.
[0065] The reaction is terminated after complete consumption of the starting material is confirmed by NMR or the like, and then extraction, distillation of the solvent under reduced pressure, and separation and purification of the target product by conventional methods such as column chromatography may be performed.
[0066] The cyclopentadiene-based ligand coordinated to the molybdenum compound according to one embodiment of the present invention is stably coordinated to molybdenum through a resonance structure, and the thermal stability of the molybdenum compound is significantly improved. As a result, a thin film made of molybdenum (Mo), molybdenum nitride (MoNx), or molybdenum oxide (MoOx) can be formed with high reliability using the molybdenum compound according to one embodiment of the present invention.
[0067] Furthermore, the cyclopentadiene-based ligand may be bonded to an aminoalkyl, an alkoxyalkyl, or an alkylsulfide, thereby improving the thermal stability of the molybdenum compound during the deposition process.
[0068] The present invention provides a composition for depositing a molybdenum-containing thin film, comprising a molybdenum compound according to one embodiment of the present invention.
[0069] The present invention also provides a method for producing a molybdenum-containing thin film using the composition for depositing a molybdenum-containing thin film.
[0070] The deposition in the method for producing the molybdenum-containing thin film may be a conventional method used in the art, specifically, atomic layer deposition (ALD), chemical vapor deposition (CVD), metalorganic chemical vapor deposition (MOCVD), low pressure chemical vapor deposition (LPCVD), plasma enhanced chemical vapor deposition (PECVD), or plasma enhanced atomic layer deposition (PEALD).
[0071] More preferably, the method for producing the molybdenum-containing thin film according to an embodiment may be atomic layer deposition (ALD), chemical vapor deposition (CVD), metal-organic chemical vapor deposition (MOCVD), or plasma-enhanced atomic layer deposition (PEALD).
[0072] A method for producing the molybdenum-containing thin film according to one embodiment of the present invention includes the steps of: a) increasing the temperature of a substrate mounted in a chamber; b) injecting a reaction gas and the composition for depositing a molybdenum-containing thin film into the chamber to produce a molybdenum-containing thin film.
[0073] In an embodiment, the deposition conditions may be adjusted depending on the structure or thermal properties of the desired thin film. The deposition conditions according to an embodiment may include the supply flow rate of the molybdenum-containing thin film deposition composition, the supply flow rates of the reaction gas and the transport gas, pressure, RF power, etc.
[0074] Non-limiting examples of the deposition conditions include a molybdenum-containing thin film deposition composition flow rate of 1 to 1000 sccm, a carrier gas flow rate of 1 to 5000 sccm, a reactive gas flow rate of 10 to 5000 sccm, a pressure of 0.1 to 10 torr, and an RF power of 10 to 1000 W, but are not limited thereto.
[0075] In one embodiment, in step a), the substrate mounted in the chamber is heated to 200° C. to 700° C., specifically, 500° C. to 600° C., but is not limited thereto.
[0076] The substrate according to an embodiment may be, but is not limited to, a substrate including one or more semiconductor materials of Si, Ge, SiGe, GaP, GaAs, SiC, SiGeC, InAs, and InP, a silicon on insulator (SOI) substrate, a quartz substrate, a glass substrate for a display, or a flexible plastic substrate such as polyimide, polyethylene terephthalate (PET, PolyEthylene Terephthalate), polyethylene naphthalate (PEN, PolyEthylene Naphthalate), polymethyl methacrylate (PMMA, Poly Methyl MethAcrylate), polycarbonate (PC, PolyCarbonate), polyethersulfone (PES), or polyester.
[0077] In one embodiment, the reactive gas may be, but is not limited to, oxygen (O), ozone (O), distilled water (HO), hydrogen peroxide (HO), nitric oxide (NO), nitrous oxide (NO), nitrogen dioxide (NO), ammonia (NH), nitrogen (N), hydrazine (NH), amines, diamines, carbon monoxide (CO), carbon dioxide (CO), C1-C 12 The gas may be any one or a mixture of two or more selected from the group consisting of saturated or unsaturated hydrocarbons, hydrogen (H2), argon (Ar), and helium (He).
[0078] Specifically, the reactive gas may be any one or more selected from oxygen (O2), hydrogen peroxide (H2O2), nitrous oxide (N2O), nitrogen (N2), and hydrogen (H2), and more specifically, may be hydrogen (H2), but is not limited thereto.
[0079] In one embodiment, the transport gas in the depositing step is an inert gas, which may be any one or more selected from argon (Ar), helium (He), and nitrogen (N2), and may be, but is not limited to, nitrogen (N2).
[0080] According to one embodiment, the method for producing a molybdenum-containing thin film includes the steps of: The method may further include a step of injecting a reaction gas into the chamber after the steps c) and b), and the steps b) and c) constitute one cycle, and the cycle may be repeated.
[0081] In one embodiment, after injecting the transfer gas and the molybdenum-containing thin film deposition composition into the chamber, a purging step may be performed to remove the molybdenum compound or composition thereof that is not adsorbed on the substrate using the transfer gas.
[0082] In one embodiment, after injecting the reaction gas into the chamber, a purging step may be performed to remove reaction by-products and residual reaction gas using the transport gas.
[0083] In an embodiment, a cycle of injecting the molybdenum-containing thin film deposition composition, purging, injecting the reactive gas, and purging may be repeated.
[0084] A thin film produced by the molybdenum-containing thin film production method according to an embodiment can exhibit uniform and stable deposition rates and provide uniform step coverage for structures having large aspect ratios.
[0085] The molybdenum-containing thin film according to the present invention has a molybdenum content of 70% or more, specifically 72% or more, and is prepared at a high deposition rate of 1.36 Å per cycle. Therefore, the molybdenum-containing thin film according to the present invention can be usefully used as a dielectric film in various semiconductor fields.
[0086] Hereinafter, the method for producing a molybdenum compound according to the present invention and the method for producing a thin film using the same will be described in more detail with reference to specific examples. However, the following examples are merely a reference for describing the present invention in detail, and the present invention is not limited thereto, and can be realized in various forms. Furthermore, the terms used in the description of the present invention are merely for the purpose of effectively describing specific examples, and are not intended to limit the present invention.
[0087] Additionally, unless otherwise noted, all examples were carried out under an inert atmosphere, e.g., purified nitrogen (N) or argon (Ar), using techniques commonly known in the art for handling air-sensitive materials.
[0088] Example 1: Preparation of ((CH)N(CH)Cp)MoH(CO) In a reactor equipped with a reflux condenser, 100g (0.38mol) of Mo(CO)6 and 300mL of toluene were added and stirred. 128.7g (1.0mol) of 1,3,5-trimethylhexahydro-1,3,5-triazine (trimethyltriazacyclohexane, TMTACH) was slowly added to the reactor and stirred at 120°C for 10 hours or more. The reaction was continued until no further CO gas generation was observed using an external oil bubbler. The temperature of the reactor was lowered to 100°C and the mixture was filtered, washed three times with 50mL of toluene, and dried in vacuum to obtain 84g (yield: 72%) of yellow powder of (TMTACH)Mo(CO)3.
[0089] In a reactor equipped with a reflux condenser, 384 g (0.27 mol) of (TMTACH)Mo(CO) obtained above and 200 mL of THF were added and stirred. 37 g (0.27 mol) of (2-dimethylaminoethyl)cyclopentadiene was slowly added to the reactor and stirred at 70°C for 10 hours or more. After confirming that the yellow mixture had all turned deep red, the solvent was evaporated under reduced pressure. The residue was extracted twice with 300 mL of hexane. The extracted deep red solution was evaporated under reduced pressure to obtain a deep red liquid. The resulting product was distilled at 92°C and 0.3 Torr to obtain about 40 g of ((CH3)2N(CH2)2Cp)MoH(CO)3 (yield: 45% from Mo(CO)6). 1 H NMR(400 MHz, C6D6) δ 4.8 - 4.95 (d, 4H), 2.0 - 2.2 (m, 4H), 2.0 (s, 6H), 1.6-1.8 (m, 1H)
[0090] Example 2: Preparation of ((CH3)O(CH2)2Cp)MoH(CO)3 In a reactor equipped with a reflux condenser, 100 g (0.32 mol) of (TMTACH)Mo(CO)3 obtained above and 200 mL of THF were added and stirred. 40.17 g (0.32 mol) of (2-methoxyethyl)cyclopentadiene was slowly added to the reactor and stirred at 70°C for more than 10 hours. After confirming that the yellow mixture had all turned deep red, the solvent was evaporated under reduced pressure. The residue was extracted twice with 300 mL of hexane. The extracted deep red solution was evaporated under reduced pressure to obtain a deep red liquid. The resulting product was distilled at 85°C and 0.25 Torr to obtain about 45 g of ((CH3)O(CH2)2Cp)MoH(CO)3 (yield: 34.6% from Mo(CO)6). 1 H NMR(400 MHz, C6D6) δ 4.8 - 4.95 (d, 4H), 3.10 (m, 2H), 3.01 (s, 3H), 2.34 (m, 2H), 1.6-1.8 (m, 1H)
[0091] [Example 3] Preparation of a molybdenum-containing thin film A molybdenum-containing thin film was manufactured by atomic layer deposition using the molybdenum compound according to Example 1 and hydrogen (H2) as a reactive gas.
[0092] While the substrate on which the silicon oxide film and the titanium nitride film were successively formed was maintained at 580° C., the molybdenum compound according to Example 1, filled in a stainless steel bubbler container at 100° C., was transferred together with 50 sccm of nitrogen (N2) for 1 second to be adsorbed onto the substrate. Then, a purge step was performed for 3 seconds using 2000 sccm of nitrogen (N2) to remove the molybdenum compound that was not adsorbed.
[0093] Next, 2000 sccm of hydrogen (H2) was supplied for 5 seconds to react with the adsorbed molybdenum compound to form a molybdenum-containing thin film, followed by a 3-second purge step using 2000 sccm of nitrogen (N2) to remove reaction by-products and residual reaction gases.
[0094] The above process constitutes one cycle, and a molybdenum-containing thin film was formed by repeating 500 cycles.
[0095] The thickness of the formed molybdenum-containing thin film was measured using a scanning electron microscope, and the results are shown in Figure 1. The thickness of the molybdenum-containing thin film was 680 Å, and the deposition rate was confirmed to be 1.36 Å per period.
[0096] Furthermore, X-ray photoelectron analysis confirmed that the thin film contained approximately 72% molybdenum.
[0097] From this, the molybdenum compound according to one embodiment of the present invention has improved thermal stability, high volatility, and improved vapor pressure, and therefore when used to produce a thin film, it exhibits a uniform and stable deposition rate, making it possible to produce a thin film having excellent deposition properties.
[0098] As described above, the present invention has been described using specific and limited examples and comparative examples. However, these are merely provided for a more general understanding of the present invention, and the present invention is not limited to the above examples. A person having ordinary knowledge in the field to which the present invention belongs can make various modifications and variations from such descriptions.
[0099] Therefore, the idea of the present invention should not be limited to the above-mentioned embodiments, and it can be said that not only the scope of the attached claims, but also equivalents to the scope of the claims or equivalent variations all fall within the scope of the idea of the present invention.
Claims
1. A molybdenum compound represented by the following chemical formula 1. 【Chemistry 1】 [In the above Chemical Formula 1, L is a C1-C10 alkylene or a C3-C10 cycloalkylene, and the alkylene and cycloalkylene of L may be further substituted with a C1-C10 alkyl; R 1 ~R 4 are each independently hydrogen or C1-C7 alkyl; R 5 is hydrogen, C1-C10 alkyl, C6-C12 aryl, C6-C12 aryl, C1-C10 alkyl, or C1-C10 alkoxy; Y is -NR 11 R 12 , -OR 13 , or -SR 14 and R 11 ~R 14 are each independently C1-C10 alkyl, haloC1-C10 alkyl, C3-C10 cycloalkyl, C6-C12 aryl, C6-C12 arylC1-C10 alkyl, or 11 and R 12 may be linked to form a ring.
2. The L is a C1-C6 alkylene, and the alkylene of the L may be further substituted with a C1-C6 alkyl; R 1 ~R 4 are each independently hydrogen or C1-C4 alkyl; R 5 is hydrogen or C1-C6 alkyl; Y is -NR 11 R 12 , -OR 13 , or -SR 14 and R 11 ~R 14 are each independently C1-C6 alkyl, haloC1-C6 alkyl, C3-C6 cycloalkyl, C6-C12 aryl, or C6-C12 arylC1-C6 alkyl, or 11 and R 12 may be linked by a C2-C6 alkylene to form a ring.
3. 2. The molybdenum compound according to claim 1, which is represented by the following chemical formula 2: 【Chemistry 2】 [In the above Chemical Formula 2, R 1 ~R 4 are each independently hydrogen or C1-C4 alkyl; R 5 is hydrogen or C1-C4 alkyl; Y is -NR 11 R 12 , -OR 13 , or -SR 14 and R 11 ~R 14 are each independently C1-C4 alkyl, haloC1-C4 alkyl, or C3-C6 cycloalkyl, or 11 and R 12 may be linked by a C2-C6 alkylene to form an alicyclic ring; m is an integer from 1 to 4.
4. 2. The molybdenum compound of claim 1, which is selected from the following compounds: 【Chemistry 3】
5. a) reacting a molybdenum compound represented by the following formula 3 with a ligand capable of coordinating with the molybdenum compound to produce an intermediate; b) reacting the intermediate with a cyclopentadiene-based ligand represented by the following formula 4 to prepare a molybdenum compound represented by the following formula 1: A method for producing a molybdenum compound represented by the following formula 1: 【Chemistry 4】 【Chemistry 5】 【Chemistry 6】 [In the above Chemical Formulas 1 and 4, L is a C1-C10 alkylene or a C3-C10 cycloalkylene, and the alkylene and cycloalkylene of L may be further substituted with a C1-C10 alkyl; R 1 ~R 5 are each independently hydrogen or C1-C7 alkyl; Y is -NR 11 R 12 , -OR 13 , or -SR 14 and R 11 ~R 14 are each independently C1-C10 alkyl, haloC1-C10 alkyl, C3-C10 cycloalkyl, C6-C12 aryl, C6-C12 arylC1-C10 alkyl, or 11 and R 12 may be linked to form a ring.
6. A molybdenum-containing thin film deposition composition comprising the molybdenum compound according to claim 1 .
7. A method for producing a molybdenum-containing thin film using the composition for vapor deposition of a molybdenum-containing thin film according to claim 6.
8. a) raising the temperature of a substrate mounted in a chamber; b) injecting a reaction gas and the composition for depositing a molybdenum-containing thin film into the chamber to produce a molybdenum-containing thin film.
9. The reaction gas is oxygen (O 2 ), ozone (O 3 ), distilled water (H 2 O), hydrogen peroxide (H 2 O 2 ), nitric oxide (NO), nitrous oxide (N 2 O), nitrogen dioxide (NO 2 ), ammonia (NH 3 ), nitrogen (N 2 ), hydrazine (N 2 H 4 ), amines, diamines, carbon monoxide (CO), carbon dioxide (CO 2 ), C 1 ~C 12 Saturated or unsaturated hydrocarbons, hydrogen (H 2 9. The method for producing a molybdenum-containing thin film according to claim 8, wherein the gas is at least one selected from the group consisting of nitrogen (N), argon (Ar), and helium (He).
10. The method for producing a molybdenum-containing thin film according to claim 8, further comprising the step of: c) injecting a reactive gas into the chamber after step b).
11. The method for producing a molybdenum-containing thin film according to claim 10 , wherein the steps b) and c) form one cycle, and the cycle is repeated.
12. A molybdenum-containing thin film, the molybdenum content of which is 70% or more.
Citation Information
Patent Citations
Molybdenum allyl complexes and their use in thin film deposition