Method and straightener for straightening rod-shaped material

The method and machine use an integrated measuring probe with a straightening hammer and a characteristic diagram to predict and achieve precise plastic deformation, addressing inefficiencies in straightening non-linear rod-shaped materials by minimizing rework and enhancing process efficiency.

JP2024544451AActive Publication Date: 2024-12-03ラトゥンデアーゲー

Patent Information

Application Number
JP2024507121
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2022-01-05
Filing Date
2022-12-08
Publication Date
2024-12-03
Estimated Expiration
2042-12-08

AI Technical Summary

Technical Problem

Existing straightening machines for non-linear rod-shaped materials face challenges in accurately predicting the necessary plastic deformation required to achieve desired straightness due to unpredictable material properties and residual stresses, leading to inefficiencies and rework.

Method used

A method and machine that utilize an integrated measuring probe with a straightening hammer to measure actual plastic deformation during the first forming stroke, using a characteristic diagram to determine subsequent strokes based on statistical and machine learning methods, ensuring precise plastic deformation within a defined range.

Benefits of technology

This approach significantly reduces the need for rework by accurately determining and achieving the target plastic deformation with high probability, improving efficiency and reducing time consumption in the straightening process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024544451000001_ABST
    Figure 2024544451000001_ABST
Patent Text Reader

Abstract

The present invention relates to a method for straightening a non-straight rod-shaped material (1), the method being carried out by determining a target plastic deformation (s_soll) at a forming position (12) of the rod-shaped material (1) and moving a straightening hammer (8) with an integrated measuring probe (7) to the forming position (12), a first forming stroke (h_1) of the straightening hammer (8) is performed, an actual plastic deformation (s_ist) caused by the first forming stroke (h_1) is determined using the integrated measuring probe (7), and a second forming stroke (h_2) is determined from the actual plastic deformation (s_ist) caused by the first forming stroke (h_1) and the target plastic deformation (s_soll).
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for straightening a non-straight bar of material by determining a target plastic deformation at a forming location of the bar of material.

[0002] The present invention also relates to a straightener for non-linear rod material for performing a targeted plastic deformation at a forming location of the rod material using a control mechanism. [Background technology]

[0003] Bar-shaped material, e.g. tubes, profiles, solid profiles, are processed in a cutting machine. Short sections are cut from a long starting material, which may have a length of, e.g., 12 meters. These short sections may be, e.g., 2 meters long.

[0004] Essentially, the pretreated material is not perfectly straight. As a consequence, the cut length sections are also not perfectly straight. In the following, a "perfect straight line" will also be referred to as a "straight line".

[0005] The straightness of the starting material depends on the material, production, material quality, the straightening process in multi-roll straighteners, transport, finishing, etc. A minimum straightness is often required for cut-to-length sections, e.g. for sections for camshafts, engine shafts or card shafts. As a rule, it is technically impossible or too costly to achieve perfect straightness already in the pre-processed material.

[0006] The idea is to use a straightener to produce sections with the required straightness. Essentially, sections are measured for straightness and those that are outside a given tolerance are sent to the straightener. The straightener then straightens the section and sends the straightened section back through the normal process sequence so that the straightness can be checked again. Then, only those workpieces that achieve the required straightness before or after the straightening process are output as good parts of the material stream.

[0007] In the prior art, straightening machines with a straightening anvil on the right and a straightening anvil on the left and one or more straightening hammers between them are known, for example from DE 10 2005 021 946 A1. Firstly, the workpiece is clamped on both sides, for example clamped center-to-center and measured in a tactile or non-contact manner while rotating. A suitable computing unit calculates the straightness of the workpiece. The deviation profile is determined. The computing unit also calculates the deformations and support points required to achieve the straightness tolerances. Then the workpiece is placed on the straightening anvils according to the precalculated target values ​​and is plastically deformed with the straightening hammers until the workpiece achieves the required straightness.

[0008] In order to plastically deform the section, the straightening hammer must be used to go beyond the elastic range of deformation. Only after the elastic deformation does the plastic deformation occur and remain permanently. The forming stroke of the straightening hammer must match the elastic deformation in addition to the plastic deformation. Again, when the straightening hammer relaxes the section, essentially the elastic deformation component bounces back and only the plastic deformation component remains in place. It is known how much plastic deformation is required at the forming position from the straightness measurements mentioned above and the calculation of the straightness function in the calculation unit.

[0009] However, the problem arises that the function between the elastic and plastic parts of the forming stroke is not constant or does not follow a known correct function: it depends on many conditions such as residual stresses in the material, strain hardening, material variations, etc., which are not constant and therefore not predictable even within the length of the pretreated material.

[0010] Thus, using measurements and mathematical calculations, it is known how much and where the workpiece needs to be deformed to achieve a specified tolerance, but it is not known how large the target stroke of the associated straightening hammer needs to be with any certainty. Using statistical techniques it is possible to predict the target stroke, but then there is also a significant probability that a significant amount of material will be plastically under- or over-deformed. Either this is accepted, to its detriment, or the workpiece is again lifted off the straightening anvil, measured, returned to the straightening anvil and straightened again, which is disadvantageously very time consuming. [Prior art documents] [Patent documents]

[0011] [Patent Document 1] DE 102005021946 [Non-patent literature]

[0012] [Non-Patent Document 1] Deep Learning with Python and Keras(ISBN978-3-95845-838-3) Summary of the Invention

[0013] Therefore, in a first aspect, it is an object of the present invention to provide a method for straightening a non-straight rod material which reduces at least the above-mentioned disadvantages.

[0014] Therefore, in a second aspect, it is an object of the present invention to provide a straightener for non-straight rod material, which reduces at least the above-mentioned disadvantages.

[0015] That object is met in a first aspect by a method having the features of claim 1.

[0016] First, one or more target plastic deformations are determined at one or more forming positions of the rod-shaped material by measuring and mathematical methods. A forming position is understood here as a position or area of ​​the material where a forming force acts in order to realize a deformation of the material. The measuring and mathematical methods in this regard are state of the art and are known, for example, from Deep Learning with Python and Keras (ISBN978-3-95845-838-3).

[0017] According to the invention, a straightening hammer with an integrated measurement probe moves alongside or above the forming location. Integrated probe is generally understood to mean that the hammer and the integrated probe are interconnected. The integrated probe is physically located on the straightening hammer, so that the probe is preferably located in the center of the pressure face of the straightening hammer. The pressure face of the straightening hammer contacts the forming location of the material during the forming process caused by the forming stroke.

[0018] A first forming stroke of the straightening hammer is performed and the actual plastic deformation caused by the first forming stroke is measured using the integrated measurement probe. If necessary, a second forming stroke or further strokes are determined from the actual plastic deformation caused by the first forming stroke and the target deformation.

[0019] Preferably, to determine the first forming stroke, a characteristic diagram is provided that defines the actual plastic deformation range for the material for each possible forming stroke, within which the actual deformation falls with a high probability. Preferably, the maximum limit of the actual plastic deformation range is selected as the forming stroke. However, the forming stroke can also be selected within the upper 10%, 9%, or any lower value range within the actual plastic deformation range.

[0020] This takes into account the fact that it is not possible to predict with certainty which forming strokes need to be performed to achieve a given target plastic deformation at the forming location of the bar material, but rather it is known from statistical methods, experience, and artificial intelligence and machine learning evaluation that a unique first forming stroke will result in deformation within the actual plastic deformation range, i.e., within the characteristic diagram.

[0021] The straightening hammer acts on the forming position in a first forming stroke. As a result, the bar material first becomes elastic and then deforms plastically. After releasing the straightening hammer, the elastic part rebounds and the state of actual plastic deformation is maintained. However, this cannot be predicted with certainty during the defined first forming stroke.

[0022] However, since the actual deformation range is known, i.e., the actual deformation is realized within a certain range with a very high probability, i.e., more than 99%-99.9%, for a particular forming stroke, the target deformation is conveniently selected as a high value, preferably as the maximum value of the actual deformation range.

[0023] This means that a target deformation is determined by known methods, to which the first shaping stroke is assigned, the actual deformation span of which, in its maximum value, corresponds to the target deformation, i.e. is equal to it. However, in principle, other assignments are also conceivable. For example, the target deformation can be in the upper 1 / 10, 1 / 5, etc. of the actual deformation caused by the first shaping stroke.

[0024] Advantageously, the first forming stroke performs an elastic deformation of the material and an actual deformation within the actual plastic deformation range.

[0025] By conveniently and carefully selecting the first forming stroke, only in the best case will the actual deformation caused by the first forming stroke match the target deformation, and since the target deformation is at the maximum value of the actual deformation range, the actual plastic deformation caused by the first forming stroke will in most cases be less than the target plastic deformation. Therefore, a second forming stroke is necessary.

[0026] The actual deformation caused by the first forming stroke is measured by the integrated measuring probe and evaluated together with the target deformation. Conveniently, a characteristic curve within the characteristic field range is determined by the actual deformation and a characteristic curve is selected to determine the second forming stroke.

[0027] In the method steps, the idea is utilized that in a specific configuration the actual deformation cannot be predicted with certainty for a given forming stroke, but only the actual deformation range recorded in the characteristic diagram can be defined. However, if the measurement data of the aforementioned first deformation are evaluated at the forming position where the actual deformation has already taken place, the actual deformation can be predicted very accurately by the second forming stroke.

[0028] It has been found that within the characteristic diagram the characteristic curve can be determined quite precisely, or preferably quite accurately, for a specific forming position, if the actual plastic deformation of the already performed first forming stroke is known for this forming position. Not only is the characteristic curve determined precisely by the zero point, but the actual deformation of the first forming stroke is performed and the characteristic curve is used according to the invention to determine the second forming stroke.

[0029] Advantageously, the characteristic curve defines the second forming stroke precisely, preferably precisely, with a defined target plastic deformation.

[0030] Preferably, the characteristic curve of the rod-shaped material within the range of the characteristic diagram is determined from the actual deformation after the first forming stroke, which is led through the zero point, and the measured actual deformation. The characteristic curves essentially have a comparable course within the range of the characteristic diagram. The characteristic curve for the forming position can therefore already be determined by a single measurement.

[0031] A second shaping stroke is determined from the characteristic curve, the second shaping stroke corresponding to an intersection of the characteristic curve and the target deformation.

[0032] In a preferred embodiment of the process according to the invention, the target deformation at the forming position of the bar-shaped material is determined during the process by means of the integrated measuring probe. The bar-shaped material is clamped. The zero position of the straightening hammer is determined and stored. A first measurement value of the integrated measuring probe at the zero position of the straightening hammer is determined and stored. A first forming stroke of the straightening hammer is performed. The straightening hammer is then returned to the zero position, a second measurement value of the integrated probe at the zero position of the straightening hammer is determined and the actual plastic deformation of the bar-shaped material resulting from the first forming stroke at the forming position is determined from the first and second measurement values ​​of the integrated probe.

[0033] Advantageously, the integrated probe only needs to determine a difference value between its first measurement and its second measurement, from which the actual plastic deformation caused by the first forming stroke can be determined. This can preferably be done by the integrated probe by determining the distance between the measuring head of the integrated probe and the forming location on the outer surface of the rod material in the first and second measurements, and creating a difference value from this value.

[0034] Preferably, a tolerance range is defined, which determines the distance the rod may deviate from the straight rod, and if after the first forming stroke is performed the difference between the actual deformation and the target deformation is outside the tolerance range, a second forming stroke is performed at the forming position. If necessary, a third forming stroke and a fourth forming stroke can also be performed.

[0035] Preferably, the actual outer surface of the bar is first measured and a deviation profile of the actual outer surface from a linear target outer surface is determined. The deviation profile is used to determine a forming location where a first forming stroke is applied. In addition to the forming location, typically one, two or more contact points of the bar on the anvil are determined, as well as their distance.

[0036] The forming position is determined from the deviation profile as an angular position about the longitudinal direction of the bar material and also along the longitudinal direction of the straightener as a position along the axis of movement of the straightening hammer. A control mechanism of the machine then enables the bar material, preferably clamped between two holders, to be rotated about the longitudinal axis to the angular position determined from the deviation profile and then to move the straightening hammer along the transverse axis beside the bar material in a longitudinal progression until the hammer is positioned directly at the forming position and can act against the forming position to perform a first forming stroke.

[0037] Conveniently, the target deformation is determined in a known manner from the deviation profile at the forming position, and the first forming stroke, which is to be assigned to the target deformation, is determined from a characteristic diagram, as explained above.

[0038] Conveniently, the rod of material is mounted on two anvils and the forming station is disposed longitudinally between the two anvils.

[0039] The object is solved in a second aspect thereof by a straightener having the features of claim 12.

[0040] The straightener is suitable for carrying out one of the processes described above. Conversely, the above-mentioned process is suitable for carrying out with one of the straighteners described below.

[0041] It is also believed that what is said about the method should be disclosed mutatis mutandis for the straightening machine.

[0042] The straightening machine according to the invention for non-linear rod-shaped material is also suitable for carrying out a target plastic deformation at the forming position of the rod-shaped material. The straightening machine comprises a control mechanism for a transverse device having a straightening hammer with an integrated measuring probe. The control system advantageously comprises a computing unit and a memory. A characteristic diagram is stored in the memory, which defines the actual plastic deformation range for the material for each forming stroke, and the actual deformation falls within said range with a high probability, i.e. with values ​​above 95%, 96%, preferably 99% or more.

[0043] Advantageously, the control unit, using its computing unit, determines the first forming stroke from a target deformation, advantageously with the aid of a characteristic diagram. The target deformation is preferably within the upper 10% or less range, preferably the maximum value within the actual deformation range. However, other arrangements between the actual plastic deformation range and the target plastic deformation are also conceivable.

[0044] Advantageously, the first forming stroke is selected such that for a given material, the actual plastic deformation performed by the first forming stroke is less than the determined target plastic deformation with a high probability of at least 95%, or more preferably 99% or more. Preferably, excessive deformation should be avoided.

[0045] The integrated measuring probe according to the invention measures the actual plastic deformation caused by the first forming stroke and transmits the measured value to the control mechanism via a data communication connection. Due to the actual deformation actually determined for the specific forming position based on the actual forming stroke, the characteristic diagram can be limited to a characteristic curve. The characteristic curve within the characteristic diagram can be determined from the actual deformation. As explained above, the control system can then determine a second forming stroke from the target deformation and the characteristic curve. The second forming stroke is the value on the characteristic curve that generates the target deformation, i.e. after which the target deformation is ideally realized or, if this still does not realize it, at least only an under-plastic deformation is realized, and the process cycle explained above is carried out a second time.

[0046] Preferably, the straightening machine comprises at least two anvils separated from each other in the longitudinal direction for supporting the bar-shaped material. The bar-shaped material can preferably be placed on the two anvils, whereby it is advantageously clamped by two holders, which are arranged opposite each other and rotatable. Between the two opposing holders, a measuring probe is advantageously arranged beside the clamped bar-shaped material, which makes it possible to measure the actual outer surface of the bar-shaped material and to determine the deviation profile of the actual outer surface from a linear target outer surface. From this, as explained above, the forming position of the straightening hammer and the contact point of the bar-shaped material on the anvils can be determined by known methods.

[0047] Particularly preferably, the integrated measuring probe with the measuring head is guided centrally by the straightening hammer, whereby the measuring head allows a distance measurement beyond the impact surface of the straightening hammer. Advantageously, the distance between the measuring head and the forming position of the rod-shaped material can be determined. Advantageously, before the first forming stroke is performed, a first distance measurement is performed and after the first forming stroke is performed, a second distance measurement is performed, which are performed in order to determine the actual plastic deformation at the forming position caused by the forming stroke by making their difference.

[0048] The straightening hammer is preferably arranged on an NC-controllable transverse axis transverse to the actual outer surface of the bar material, the NC-controllable transverse axis being very accurate, allowing the straightening hammer to be controlled in the micrometer range.

[0049] The rod-like material can advantageously be positioned on a receptacle, which can be a cone, however it is also conceivable that the receptacle can be shaped as just an empty area between two opposing holders, whereby the holders can be, for example, two opposing ends, in which the tube can be clamped and rotated.

[0050] The invention is illustrated using example embodiments in six figures. [Brief description of the drawings]

[0051] [Figure 1] 1 is a schematic structure of a straightener according to the present invention for non-straight rod-shaped material. [Diagram 2] 2 is a straightening machine for the non-straight rod material of FIG. 1 in a first processing step. [Diagram 3] 2 is a straightening machine for the non-straight rod material of FIG. 1 in a second processing step. [Figure 4] 2 is a straightening machine for non-straight rod-shaped material according to FIG. 1 in a third processing step. [Diagram 5] 2 is a straightening machine for non-straight rod-shaped material according to FIG. 1 in a fourth processing step. [Figure 6] 1 is a diagram relating to the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0052] The straightening machine 10, shown diagrammatically in Figures 1 to 5, and the process according to the invention implemented therein, are used to straighten non-straight rod-shaped material. Rod-shaped material here means in particular a tube, a profile, a solid profile etc. extending along a longitudinal direction L, preferably of circular cross-section, but which may also be angular, in particular square.

[0053] The example embodiment refers to, but is in no way limited to, a tube 1. The tube 1 may have a length of several meters and a diameter of several centimeters or decimeters. Other dimensions are also conceivable.

[0054] At a cursory glance at the figure, the tube 1 appears straight in a longitudinal direction L along its outer surface 11. On closer inspection, and this is the gist of the present invention, the tube 1 is not straight.

[0055] The tube 1 shown in FIG. 1 is for example corrugated in the Y direction. The corrugations are not shown here to scale but are greatly exaggerated. Typically, the amplitude of the waves formed in the tube is in the mm range or down to a tube length of 1-2 meters. The waves extend along the longitudinal direction L, which here corresponds to the Z direction. Wavy bulges can also occur in the X direction (not shown), which are superimposed on the corrugations in the Y direction. The bulges do not have to have corrugations.

[0056] The tube 1 has an actual outer surface 11, which deviates from a linear target outer surface extending in a longitudinal direction L. A deviation profile can be determined along the longitudinal direction L. The deviation profile can be determined along the longitudinal direction L by creating a difference between the actual outer surface and the target outer surface. For this purpose, the straightener 10 has a receptacle 16, on whose end faces the tool tips 5, 6 are arranged to clamp the tube and rotate it. The receptacle 16 may preferably have a conical support surface for supporting the tube 1. Here, the receptacle 16 is understood as a clearance between the two tool tips 5, 6. The tool tips 5, 6 can be moved individually back and forth along a transverse axis A and a transverse axis B, respectively, the tool tips 5, 6 being both arranged in the Z direction. The tool tips 5, 6 can also be moved individually in the XY plane of FIG. 1. In FIG. 1, a horizontal axis C is drawn for one tool tip 5 and a horizontal axis D is drawn for the other tool tip 6, both of which run in the Y direction. Two horizontal axes are not drawn in the X direction for the two tool tips 5,6. Due to the two tool tips 5,6 being arranged diametrically opposite each other, their rotation axes run in extension of each other. By moving the tool tips 5,6 towards each other, the tube 1 can be clamped between the tool tips 5,6. By rotating the tool tips 5,6, the clamped tube 1 can itself be rotated.

[0057] Along the receptacle 16 located between the tool tips 5, 6, the measuring probes 2 for measuring the straightness of the tube 1 are arranged at fixed distances from each other along the longitudinal direction L. The distances may be equidistant. The distances from each other may be equidistant. Also different distances can be selected. The probes 2 can also be arranged at different angles in a section perpendicular to the longitudinal direction L around the receptacle 16 and the tube 1. The measuring probes 2 can be tactile or optical or designed in other ways. They allow distance measurements in the range with an accuracy of 0.1 μm or less. The measuring probes 2 for measuring the straightness of the tube 1 are connected in a data communication manner to a control system with a data memory, in which in particular the measured distance values ​​for the individual measuring probes 2 and for the measuring points on the outer surface 11 of the tube 2 are stored. As shown in Fig. 1, the straightness of the tube 1 is measured such that the tube 1 is clamped, the measurement probe 2 performs a first distance measurement, the tube 1 is rotated over a short distance by angles α, β, the measurement probe 2 performs a second distance measurement at the rotated angular position, the tube 1 is further rotated by angles α, β, and the measurement probe 2 performs a third distance measurement, etc. The distance measurements are stored and evaluated together with the position of the probe 2 along the longitudinal direction L and the angular position to determine the actual outer surface 11 of the tube 1. The actual outer surface 11 of the tube 1 deviates from the target outer surface of a straight tube 1. In Fig. 1, the tube 1 is shown with an exaggerated curvature.

[0058] Deviations from straightness to a given tolerance, usually less than 1 μm, are tolerated for further processing of the tube 1. Non-straightness outside the tolerance range is classified and straightened according to the invention. The tube 1 is straightened by the straightener 10 according to the invention and brought back within the tolerance range.

[0059] Straightening of the tube 1 is preferably performed with the aid of two anvils 3, 4 as shown diagrammatically in Fig. 1 and with a straightening hammer 8 according to the invention, in which an integrated measuring probe 7 is centrally arranged. The straightening hammer 8 is a cylindrical structure with a central bore, preferably a central circular bore, in which the tactile or optical integrated measuring probe 7 is preferably integrated. The integrated measuring probe 7 can be moved back and forth relative to the straightening hammer 8 along a vertical movement axis J within the straightening hammer 8 and can be obscured by the straightening hammer 8, with the measuring surface 7a aligned with the striking surface 8a of the straightening hammer 8.

[0060] The integrated measuring probe 7 is mounted on a straightening hammer 8 together with a return spring 15 which presses the measuring surface 7a outwards from the striking surface 8a in an unloaded state.

[0061] According to Fig. 1, the straightening hammer 8 can be moved towards and away from the tube 1 along a vertical transverse axis H, and can be moved along a horizontal transverse axis G along the longitudinal direction L of the tube 1, and can also be moved along a horizontal transverse axis perpendicular to the longitudinal direction L (not shown). As shown in Fig. 1, the measuring surface 7a of the measuring probe 7 can also be moved parallel to the transverse axis H of the straightening hammer 8, preferably very easily, i.e. with almost no resistance.

[0062] Figure 2 shows the arrangement of the straightening hammer 8, the measuring probe 7 as well as the two anvils 3,4 and the tube 1 clamped between the tool tips 5,6 just prior to straightening. The two anvils 3,4 can move back and forth along the longitudinal direction L along transverse axes E,F.

[0063] From the actual deviation profile of the tube 1 from the target outer surface, the forming position 12 of the straightening hammer 8 on the tube 1 and the support points 13, 14 of the tube 1 on the anvils 3, 4 are calculated, and thus the positions of the transverse axis G and angles α, β of the two angle tips 5, 6 and the required target deformation of the tube 1 at the forming position 12 are calculated, which calculation is performed in order to straighten the tube 1 when it is supported between two anvils 3, 4 separated by a certain distance from each other.

[0064] The problem arises that the target deformation of the forming location 12 of the tube 1 and the forming stroke h of the straightening hammer 8 cannot be clearly assigned to one another.

[0065] The straightening process of the prior art is essentially always the same process. To plastically deform the tube 1, first a forming stroke h must be applied to the tube 1 with the straightening hammer 8, exceeding the elastic range of deformation. Only after the elastic deformation does the plastic deformation s occur. The forming stroke h of the straightening hammer 8 must essentially correspond to the elastic deformation in addition to the plastic deformation s. Again, when the straightening hammer 8 retreats and the tube 1 becomes unloaded, the elastic deformation component essentially bounces back and only the plastic deformation component remains in place, which now also corresponds to the actual plastic deformation s_ist.

[0066] In principle, it should be known how large the plastic deformation s is at the forming position 12 in order to achieve sufficient straightness of the tube 1 by straightening. However, it is known that there is no function between the elastic and plastic deformation components of the forming stroke h. The function between the elastic and plastic deformation components depends on many conditions, in particular on the material properties, work hardening, or other material changes. However, they are very different, so that the function between the elastic and plastic parts is unpredictable even within the length of the tube 1. It is therefore not known with certainty and a forming stroke h needs to be performed by the straightening hammer 8 in order to achieve the target deformation s_soll. Using statistical methods, the possible forming strokes h can be predicted and then, also, there is a fairly high probability that the tube 1 will be plastically over- or under-deformed. If over-forming occurs, the tube 1 will have to be measured again, the anvils 3, 4 will be raised, the tube 1 will be rotated again and placed back down, and it will be straightened again. This takes time.

[0067] FIG. 6 shows, in a schematic way, the idea of ​​the procedure implemented in FIG. 2, FIG. 3, FIG. 4, FIG. 5. FIG. 6 first shows a given characteristic diagram 60, which can be obtained by statistical methods related to artificial intelligence, machine learning, etc., for example according to Deep Learning with Python and Keras (ISBN978-3-95845-838-3). There is shown a statistical association between the forming stroke h of the straightening hammer 8 and the plastic deformation s generated by the forming stroke h for a specific material. The distance between the two anvils 3, 4 and the position of the straightening hammer 8 is also included in the characteristic diagram 60. The characteristic diagram 60 is interpreted such that when the first forming stroke h_1 is performed, the actual plastic deformation s_ist is within the deformation span b along the X-axis within the range of the characteristic diagram 60. The actual plastic deformation s_ist is located within the deformation span b with a probability of 95%, 99%, 99.9%. The width of the characteristic diagram 60, i.e. the length of the deformation span b in the X-direction, mainly depends on the material properties. Its width depends in particular on the residual stresses, strain hardening or other material variations of the material. On the other hand, the spherical shape of the characteristic diagram 60 also depends on the distance at which the anvils 3, 4 are separated from one another, on the diameter that the tube 1 has, on the wall thickness that the tube 1 has, etc., which are all parameters that make it possible to predict the correct bending behavior and therefore do not significantly influence the width of the characteristic diagram 60. They only influence the spherical shape, i.e. the slope of the characteristic diagram 60, etc.

[0068] Furthermore, it is known that the actual deformation s_ist of the rod-shaped material, in particular the tube 1, subjected to different first forming strokes h at the forming position 12 follows a characteristic curve 61 moving within a characteristic diagram 60 shown in figure 6. The characteristic curve 61 is inserted within the characteristic diagram 60. It has been found that the characteristic curve 61 within the characteristic diagram 60 can also be precisely defined in real units by two points.

[0069] The process according to the invention proceeds as described below.

[0070] The tube 1 is positioned on the anvils 3, 4 at certain angles α, β according to the known scheme of FIG. 2. The forming position 12 of the straightening hammer 8 and the support points 13, 14 on the anvils 3, 4 are known. In a first process step according to FIG. 2, the straightening hammer 8 is placed above the forming position 12 with a transverse axis G. The straightening hammer 8 is positioned on the anvils 3, 4. In order to be able to provide a tube 1 that is as straight as possible after the straightening process, it is necessary to know how large the target plastic deformation s_soll at the forming position 12 is.

[0071] In a second processing step, the straightening hammer 8 moves along the transverse axis H in the direction of the forming position 12 of the tube 1, until the measuring surface 7a of the probe 7 touches the outer surface of the tube 1, as shown in FIG. 3. However, the probe 7 does not apply any pressure to the forming position 12, which would already bend the tube. The straightening hammer 8 returns to the zero position. The zero position is determined and its coordinates are recorded. Now, a first measurement is performed in the zero position by the measuring probe 7, and the first measured value of the measuring probe 7 is stored. For example, the measurement data is recorded in terms of the distance that the measuring surface 7a of the measuring probe is away from the striking surface 8a, in the Y direction, or a similar measurement value. The first measured value is a measurement that determines the distance between the forming position 12 and the striking surface 8a of the straightening hammer 8. However, this does not have to be so, but it is important to record only the position of the forming position 12 relative to the straightening hammer 8.

[0072] In a third process step, a first forming stroke h_1 is applied to the forming position 12, as shown in FIG.

[0073] The first forming stroke h_1 is pre-determined from the known target deformation s_soll at the forming position 12. For this purpose, the intersection of the target deformation s_soll with the lower minimum of the characteristic diagram 60 is determined according to FIG. 6. From the intersection, the first forming stroke h_1 is determined. The selected first forming stroke h_1 statistically generates the target deformation s_soll in the deformation span b for the material. Through the first forming stroke h_1, the target deformation s_soll is realized only in the best case. If this is not realized, an actual deformation s_ist occurs, which is below the target deformation s_soll within the deformation span b. The tube 1 is therefore deformed less than it should actually be deformed.

[0074] The deformation process is performed by a straightening hammer 8, which is rigidly mounted on a NC-controllable axis H, as shown in Fig. 4. The straightening hammer 8 moves in the opposite direction to the Y direction with a first forming stroke h_1. The straightening hammer 8 moves in the opposite direction to the Y direction with a first forming stroke h_1 with a NC-controllable axis H, as shown in Fig. 4, and bends the tube 1 to a certain extent, as shown in Fig. 4. The bend includes an elastic part and a plastic part.

[0075] In Figure 5, the straightening hammer 8 is again withdrawn, and the elastic deformation subsides. The state of plastic deformation continues, straightening the tube 1.

[0076] The information acquisition according to the invention is carried out by means of the measuring probe 7. Then, in a fourth processing step, according to Fig. 5 the straightening hammer 8 is retracted, the tube 1 is relaxed, according to Fig. 3 the straightening hammer 8 returns to the zero position and a second measurement is carried out with the measuring probe 7 to determine a second measured value. The second measured value is compared with the first measured value of the measuring probe 7 and from the difference in the measured values, for example the difference in the distance from the striking face 8a of the straightening hammer 8 to the forming position 12, the actual deformation s_ist is determined after the first forming stroke h_1.

[0077] The idea of ​​the invention is to make it possible to execute the second forming stroke h_2 very accurately and to narrow the range of the characteristic diagram 60 considerably using information about the first actual deformation s_ist in order to bring it very close to the target deformation s_soll.

[0078] The actual plastic deformation s_ist after the first forming stroke h_1 does not usually correspond to the target plastic deformation s_soll, but is lower than the target deformation s_soll. However, the measurement of the measuring probe 7 makes it possible to show the absolute value of the actual deformation s_ist caused by the first forming stroke H_1, so that according to FIG. 6 the actual deformation s_ist actually caused can be assigned to the first forming stroke h_1 and thus the characteristic curve 61 within the range of the characteristic diagram 60 of FIG. 6 can be assigned to the forming position 12 with its specific material properties. The characteristic curve 61 shows the plastic deformation behavior at different strokes h for the forming position 12.

[0079] In a further process loop, according to figures 3, 4 and 5, the tube 1 is straightened in the forming position 12 with a second forming stroke h_2. The size of the second forming stroke h_2 is determined from the characteristic curve 61 in figure 6 and its intersection with the target deformation s_soll.

[0080] If necessary, the process loop can also be performed three or four times. Actual implementations of the process have shown that several process loops are necessary. However, it has also been shown that the process can iteratively approach the target deformation s_soll and maintain the specified straightness tolerance with a high degree of accuracy. [Explanation of symbols]

[0081] 1 Tube / rod material 2. Probe 3. Anvil 4. Anvil 5 Tool tip 6 Tool Tip 7 7a Measuring surface 8 Judging Hammer 8a Stroke surface 10 Orthodontic device 11 Actual Surface 12 Molding position 13 Support points 14 Support points 15 Return spring 16 Receptacle 60 Known Fields 61 Feature Lines b Deformation span h Forming stroke h_1 First forming stroke h_2 Second forming stroke s Plastic deformation s_ist Plastic deformation s_soll target transformation A axis of movement B Movement axis C Movement axis D Movement axis E Movement axis F moving axis G Vertical movement axis H Horizontal movement axis J moving axis L Vertical α angle β angle

Claims

1. A method for straightening a non-straight rod-shaped material (1), comprising the steps of: A target plastic deformation (s_soll) is determined at a forming position (12) of the bar-shaped material (1), A straightening hammer (8) with an integrated measuring probe (7) moves into said forming position (12), A first forming stroke (h_1) of the straightening hammer (8) is performed, the actual plastic deformation (s_ist) caused by said first forming stroke (h_1) is determined using said integrated measurement probe (7), A method according to claim 1, wherein a second forming stroke (h_2) is determined from the actual plastic deformation (s_ist) due to the first forming stroke (h_1) and the target plastic deformation (s_soll).

2. 2. The method of claim 1, wherein a characteristic diagram (60) is provided that indicates the plastic deformation span (b) for the material per forming stroke (h).

3. 3. The method according to claim 2, characterized in that the target deformation (s_soll) within the top 10% of the deformation span (b) is preferably selected as the maximum value of the deformation span (b) of the first forming stroke (h_1).

4. 4. The method according to claim 1, characterized in that the elastic deformation of the material within the deformation span (b) and the actual plastic deformation (s_ist) have been performed by the first forming stroke (h_1).

5. 5. The method according to claim 1, characterized in that the first deformation stroke (h_1) is selected such that the associated deformation span (b) has a maximum value corresponding to the target deformation (s_soll), and the actual deformation (s_ist) caused by the first shaping stroke (h_1) defines a characteristic curve (61) within the range of the characteristic diagram (60), and the characteristic curve (61) is selected for determining the second shaping stroke (h_2).

6. the target plastic deformation (s_soll) is determined at the forming position (12) of the bar-shaped material (1); The rod-shaped material (1) is clamped, The zero position of the straightening hammer (8) is determined, a first measurement value of the integrated measuring probe (7) is determined at the zero position of the straightening hammer (8); The first forming stroke (h_1) of the straightening hammer (8) is carried out, The straightening hammer (8) returns to the zero position, 6. The method according to claim 1, characterized in that a second measured value of the measuring probe (7) is determined in the zero position of the straightening hammer (8), the actual plastic deformation (s_ist) of the bar-shaped material (1) due to the first forming stroke (h_1) is determined from the first measured value and the second measured value, and the actual plastic deformation (s_ist) is compared with the target plastic deformation (s_soll).

7. 7. Method according to any one of claims 1 to 6, characterized in that a tolerance range is defined and, if, after the first forming stroke (h_1) has been performed, the difference between the actual deformation (s_ist) and the target deformation (s_soll) is outside said tolerance range, the second forming stroke (h_2) is performed at the forming position (12).

8. 8. The method according to claim 1, characterized in that the characteristic curve (61) of the rod-shaped material (1) within the characteristic diagram (60) is determined from the actual deformation (s_ist) after the first forming stroke (h_1) and the second forming stroke (h_2) is determined from the characteristic curve (61), the second forming stroke (h_2) corresponding to a forming stroke (h) for the target plastic deformation (s_soll) along the characteristic curve (61).

9. An actual outer surface of the bar of material (1) is measured and a deviation profile of the actual outer surface from a linear target outer surface is determined; Method according to any one of the preceding claims, characterized in that the forming position (12) is determined from the deviation profile.

10. Method according to any one of claims 1 to 9, characterized in that the forming position (12) is determined from the deviation profile as an angle (α, β) around the longitudinal direction (L) of the bar-shaped material (1) and also as a position along the longitudinal direction (L) and along the axis of movement (G) of the straightening hammer (8).

11. 11. The method according to any one of claims 1 to 10, characterized in that the rod-shaped material (1) is placed on two anvils (5, 6) spaced apart from one another and the forming station (12) is arranged in the longitudinal direction (L) between the two anvils (5, 6).

12. A straightening machine for a non-linear rod-shaped material (1) for performing a targeted plastic deformation (s_soll) at a forming position (12) of said rod-shaped material (1), comprising: a control mechanism for a crossing device having a straightening hammer (8) with an integrated measurement probe (7); a memory for a characteristic diagram (60) showing the actual plastic deformation span (b) for said material for each forming stroke (h), Thereby, the control mechanism determines a first forming stroke (h_1) from the target deformation (s_soll), said integrated measuring probe (7) measuring the actual plastic deformation (s_ist) caused by said first forming stroke (h_1) and feeding said measurements to said control mechanism via a data communication connection; A characteristic curve (61) within the range of the characteristic diagram (60) can be determined from the actual deformation (s_ist) in the control system, A straightening machine, characterized in that a second forming stroke (h_2) can be determined by said control mechanism from said target deformation (s_soll) and said characteristic curve (61).

13. 13. A straightening machine according to claim 12, characterized by at least two anvils (3, 4) separated from each other in a longitudinal direction (L) for supporting the rod-shaped material (1).

14. 14. Straightening machine according to claim 12 or 13, characterized in that the integrated measuring probe (7) with a measuring head (7a) is guided centrally by the straightening hammer (8), the measuring head (7a) enabling distance measurements beyond the impact surface (8a) of the straightening hammer (8).

15. 15. A straightening machine according to claim 12, 13 or 14, characterized in that the integrated measuring probe (7) is a tactile measuring probe, the measuring head (7a) of the integrated measuring probe (7) protruding centrally from the bore of the straightening hammer (8) and being able to return completely inside behind the striking face (8a) of the straightening hammer (8).

16. A straightening machine according to any one of claims 12 to 15, characterised in that the straightening hammers (8) are arranged on a transverse axis (H) which can be NC-controlled transversely of the solid outer surface of the bar material.

17. A straightening machine according to any one of claims 12 to 16, characterized in that a measuring system for measuring the outer surface of the rod-shaped material (1) is arranged along the receptacle (16) for the rod-shaped material (1).

18. 18. The straightening machine according to claim 17, characterized in that the measuring system comprises rotatable holders (5, 6) arranged oppositely to clamp the rod-shaped material (1) and a measuring probe (2) arranged between the holders (5, 6) arranged next to the clamped rod-shaped material (1).

Citation Information

Patent Citations

  • Special straightening machine for moving head type guide rail

    CN113828656A

  • Method for automatically bending longitudinal workpieces comprises using a spacer measuring step with a spacer measuring device with slides

    DE102005027640A1

  • Adapting method for correcting strain of form of body and its device

    JP1982177831A

  • Method and apparatus for straightening elongated pieces

    US3481170A

  • Method for straightening long metal workpieces especially rail track lengths by applying bending forces between a pair of thrust supports and a pair of thrust hammers with variable position and spacing

    DE102005021946A1

Cited By

  • Artificial intelligence-based planarization process control system

    JP7892865B1