Reinforced composite membrane for fuel cells, method for producing same, and membrane electrode assembly for fuel cells including same
The reinforced composite membrane with a porous support and metal ion-collecting compounds addresses the durability and performance issues of conventional polymer electrolyte membranes by preventing metal ion elution and radical scavenging, ensuring long-term stability and high conductivity.
Patent Information
- Application Number
- JP2024528524
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2022-11-23
- Filing Date
- 2022-11-24
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2042-11-24
AI Technical Summary
Conventional polymer electrolyte membranes in fuel cells suffer from issues such as high cost, low hydrogen ion conductivity under high temperature/low humidity conditions, non-uniform interfacial properties, and weak durability, leading to rapid deterioration due to radical generation and metal ion elution, which reduces the lifespan and performance of the fuel cell.
A reinforced composite membrane is developed with a porous support impregnated with a hydrogen ion conductive polymer and a compound capable of collecting metal ions, such as polyethylene glycol or crown ethers, to prevent metal ion elution and radical scavenging, enhancing mechanical stability and durability.
The reinforced composite membrane maintains performance over a long period by suppressing metal ion elution and radical-induced deterioration, improving the fuel cell's lifespan and durability while maintaining high ionic conductivity.
Smart Images

Figure 2024544561000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a reinforced composite membrane for a fuel cell, a method for making the same, and a membrane electrode assembly for a fuel cell including the same. [Background technology]
[0002] Recently, with the rapid spread of portable electronic devices and wireless communication devices, much interest and research has been focused on the development of fuel cells as batteries for portable power sources, non-polluting fuel cells for automobiles, and fuel cells for generating electricity as a clean energy source.
[0003] Polymer electrolyte membrane fuel cells (PEMFCs) that use hydrogen as fuel are able to operate over a wide temperature range, simplifying cooling devices and sealing parts, minimizing the need for humidifiers by using low-humidity hydrogen as fuel, and offering fast operation, making them popular as power sources for vehicles and homes. In addition, they are high-output fuel cells with a higher current density than other types of fuel cells, operate over a wide temperature range, have a simple structure, and offer fast start-up and response characteristics.
[0004] Recently, much effort has been made to improve the long-term performance of electrolyte membranes, which are a core component of fuel cells. In order to improve performance while being price competitive, high ion conductivity at low humidity is a very important factor.
[0005] Among various types of electrolyte membranes, perfluorinated electrolyte membranes have excellent mechanical strength and electrochemical properties, but the membrane is very expensive due to the complicated manufacturing process, and the low glass transition temperature due to the fluorinated structure is a disadvantage.
[0006] As an alternative to such perfluorinated electrolyte membranes, hydrocarbon polymers have been actively developed. However, in the case of hydrocarbon polymer electrolyte membranes, it is important to ensure that they have adequate mechanical strength at the same level as perfluorinated electrolyte membranes.
[0007] In addition, it has been pointed out that a major problem with hydrocarbon polymer electrolyte membranes is that oxidation of the electrolyte membrane can be accelerated by hydrogen peroxide or hydroxyl radicals generated during the operation of a polymer electrolyte fuel cell, and when a single membrane is used, the mechanical durability is greatly reduced, which can lead to a significant decrease in the chemical and mechanical stability of the polymer electrolyte membrane. In order to achieve high performance, long-term stability, high durability, and low cost, the electrolyte membrane must have high ionic conductivity, ensure physicochemical stability, high mechanical strength, and high dimensional stability. To meet this requirement, the introduction of a reinforced composite membrane may be an alternative solution.
[0008] Meanwhile, in the process of commercializing reinforced composite membranes, there were various demands from the industry for technologies to improve various performances in addition to high durability. For example, there was a technology to adjust the gas permeability of the reinforced composite membrane, a technology to improve the stability between the electrolyte and the support, or a technology to facilitate the impregnation of the electrolyte, and there was a need to research methods to improve the performance of reinforced composite membranes in these aspects. Summary of the Invention [Problem to be solved by the invention]
[0009] The object of the present invention is to provide a reinforced composite membrane for a fuel cell, which can maintain the performance of the fuel cell for a long period of time and improve its lifespan by applying a specific compound capable of preventing metal ion elution, such as a radical scavenger, to the porous support of the reinforced composite membrane comprising a porous support and a proton-conducting polymer.
[0010] Another object of the present invention is to provide a method for producing said reinforced composite membrane.
[0011] Another object of the present invention is to provide a membrane electrode assembly comprising said reinforced composite membrane.
[0012] It is yet another object of the present invention to provide a fuel cell including the membrane electrode assembly. [Means for solving the problem]
[0013] One embodiment of the present invention provides a reinforced composite membrane for a fuel cell, comprising a porous support and a proton-conducting polymer, the proton-conducting polymer being impregnated into the porous support or comprising an electrolyte layer comprising the proton-conducting polymer on at least one surface of the porous support, the porous support further comprising a compound capable of capturing metal ions.
[0014] The compound capable of scavenging metal ions may include polyethylene glycol, polypropylene glycol, polybutylene glycol, crown ether, or a combination thereof.
[0015] The weight average molecular weight of the polyethylene glycol, polypropylene glycol, and polybutylene glycol may be 60 to 6,000 g / mol.
[0016] The crown ether may include 12-crown-4-ether, 15-crown-5-ether, 18-crown-6-ether, benzo-15-crown-5-ether, N-phenylazo-15-crown-5-ether, 2-aminomethyl-18-crown-6, or combinations thereof.
[0017] The compound capable of capturing metal ions may be included in an amount of 1 to 50% by weight based on the total weight of the porous support.
[0018] The metal ions may include cerium (Ce) ions, manganese (Mn) ions, tungsten (W) ions, cobalt (Co) ions, vanadium (V) ions, nickel (Ni) ions, chromium (Cr) ions, zirconium (Zr) ions, yttrium (Y) ions, iridium (Ir) ions, iron (Fe) ions, titanium (Ti) ions, molybdenum (Mo) ions, lanthanum (La) ions, neodymium (Nd) ions, or combinations thereof.
[0019] The porous support may have a thickness of 1 to 100 μm.
[0020] Another embodiment of the present invention provides a method for manufacturing a reinforced composite membrane for a fuel cell, comprising the steps of: preparing a porous support from a composition including a precursor of a polymer for forming a porous support and a compound capable of capturing metal ions; and impregnating the porous support with a proton-conducting polymer or forming an electrolyte layer including a proton-conducting polymer on at least one surface of the porous support.
[0021] The porous support-forming polymer may be a hydrocarbon-based polymer that is insoluble in an organic solvent.
[0022] The compound capable of scavenging metal ions may include polyethylene glycol, polypropylene glycol, polybutylene glycol, crown ether, or a combination thereof.
[0023] The compound capable of capturing metal ions may be included in an amount of 1 to 50 parts by weight based on 100 parts by weight of the composition.
[0024] The step of preparing the porous support may be carried out by electro-irradiating the composition. According to one embodiment, the electro-irradiation may be carried out by applying an electric field of 850 V / cm to 3500 V / cm.
[0025] The step of forming the electrolyte layer including the proton-conducting polymer may include dispersing the proton-conducting polymer in a solvent to prepare a mixed solution, casting the mixed solution and drying it to form an electrolyte layer, and laminating the electrolyte layer with the porous support.
[0026] Another embodiment of the present invention provides a membrane electrode assembly for a fuel cell, comprising an anode electrode and a cathode electrode positioned opposite each other, and a reinforced composite membrane positioned between the anode electrode and the cathode electrode.
[0027] Yet another embodiment of the present invention provides a fuel cell including the membrane electrode assembly. Effect of the Invention
[0028] According to the present invention, by introducing a specific compound capable of capturing metal ions, such as a radical scavenger, into the inside or outside of the porous support of the reinforced composite membrane, it is possible to reduce the mobility of the metal ions and inhibit their elution, as well as to prevent the radical scavenger itself from agglomerating and improve its dispersibility.
[0029] Therefore, the performance of the fuel cell can be maintained for a long period of time without chemical deterioration of the electrolyte membrane and / or electrodes due to radicals, specifically hydroxyl radicals, that are generated during operation of the fuel cell, and the durability of the fuel cell can be significantly improved. [Brief description of the drawings]
[0030] [Figure 1] 1 is a schematic diagram illustrating a reinforced composite membrane for a fuel cell according to an embodiment of the present invention.
[0031] [Diagram 2] 1 is a cross-sectional view illustrating a membrane electrode assembly according to an embodiment of the present invention.
[0032] [Diagram 3] 1 is a schematic diagram showing the overall configuration of a fuel cell according to an embodiment of the present invention; DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0033] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS The present invention will now be described in detail with reference to exemplary embodiments thereof, so that those skilled in the art can easily practice the present invention. However, the present invention may be embodied in many different forms and is not limited to the embodiments set forth herein.
[0034] In the drawings, the thickness of layers and regions is exaggerated to clearly show them, and similar parts are designated by the same reference numerals throughout the specification. When a part, such as a layer, film, region, or plate, is described as being "on" another part, this includes not only the case where the part is "directly on" the other part, but also the case where there is another part between them. Conversely, when a part is described as being "directly on" the other part, it means that there is no other part between them.
[0035] As used herein, the term "nano" refers to the nanoscale, including sizes below 1 μm.
[0036]
[0037] Hereinafter, a reinforced composite membrane for a fuel cell according to one embodiment will be described.
[0038] The present invention relates to a reinforced composite membrane for fuel cells, which can maintain the performance of the fuel cell for a long period of time and improve its lifespan by applying a specific compound capable of preventing metal ion elution, such as a radical scavenger, to the porous support of the reinforced composite membrane comprising a porous support and a proton-conducting polymer.
[0039] FIG. 1 is a schematic diagram showing a schematic configuration of a reinforced composite membrane for a fuel cell according to an embodiment.
[0040] Referring to FIG. 1, a reinforced composite membrane 10 for a fuel cell according to one embodiment is a reinforced composite membrane including a porous support 5 and a proton conductive polymer, the reinforced composite membrane includes an electrolyte layer (1 and / or 3) including the proton conductive polymer impregnated in the porous support 5 or on at least one surface of the porous support 5, the electrolyte layer (1 and / or 3) including the proton conductive polymer, and the porous support may further include a compound capable of collecting metal ions.
[0041] Fuel cells can be classified into alkaline electrolyte fuel cells, polymer electrolyte membrane fuel cells (PEMFC), etc. depending on the state and type of electrolyte. Among them, polymer electrolyte fuel cells are attracting attention as portable, vehicle and home power sources due to their advantages such as low operating temperature of less than 100℃, fast start-up and response characteristics and excellent durability.
[0042] Representative examples of polymer electrolyte fuel cells include the Proton Exchange Membrane Fuel Cell (PEMFC), which uses hydrogen gas as fuel, and the Direct Methanol Fuel Cell (DMFC), which uses liquid methanol as fuel.
[0043] To summarize the reactions that occur in the polymer electrolyte fuel cell, first, when a fuel such as hydrogen gas is supplied to the oxidizing electrode, hydrogen is oxidized at the oxidizing electrode to produce hydrogen ions (H + ) and electrons (e - ) is produced. The hydrogen ions produced are transferred to the reducing electrode through an ion exchange membrane, and the electrons produced are transferred to the reducing electrode through an external circuit. Oxygen is supplied to the reducing electrode, and the oxygen combines with the hydrogen ions and electrons to produce water through the reduction reaction of oxygen.
[0044] On the other hand, there are still many technical barriers to be overcome in order to commercialize polymer electrolyte fuel cells, and essential improvements are to achieve high performance, long life, and low cost. The component that has the greatest impact on this is the membrane electrode assembly, and among them, the ion exchange membrane is one of the key elements that has the greatest impact on the performance and price of the MEA.
[0045] The requirements for the ion exchange membrane required for the operation of the polymer electrolyte fuel cell include high hydrogen ion conductivity, chemical stability, low fuel permeability, high mechanical strength, low water content, excellent dimensional stability, etc. Conventional ion exchange membranes tend not to normally exhibit high performance under certain temperature and relative humidity environments, especially under high temperature / low humidity conditions. As a result, the range of use of polymer electrolyte fuel cells using conventional ion exchange membranes is limited.
[0046] Currently, fluorine-based ion exchange membranes such as Nafion, which are known to have the best performance, have limitations due to the complexity of the manufacturing process, difficulty of manufacturing technology, and high cost. Hydrocarbon-based ion exchange membranes, which have been developed as an alternative, have many technical barriers that must be overcome due to problems such as low hydrogen ion conductivity under high temperature / low humidity conditions, non-uniform interfacial characteristics, and relatively poor durability.
[0047] In addition, such an ion exchange membrane must have both high ion conductivity and excellent durability. In particular, when a fuel cell is operated for a long period of time, the poor chemical durability of the ion exchange membrane can cause the electrolyte membrane to thin and pinholes to form, resulting in degradation of the fuel cell.
[0048] Radicals generated during fuel cell operation are known to be the main cause of degradation of the polymer electrolyte membrane. For example, hydrogen peroxide (H2O2) is generated during the reduction reaction of oxygen at the reducing electrode, and this hydrogen peroxide generates hydroperoxyl radicals (HO2·) and / or hydroxyl radicals (·OH). In addition, when oxygen molecules in the air supplied to the reducing electrode pass through the polymer electrolyte membrane and reach the oxidizing electrode, hydrogen peroxide is also generated at the oxidizing electrode, which may cause hydrogen peroxide radicals and / or hydroxyl radicals. Such radicals cause degradation of the ionomer (e.g., a polymer with sulfonic acid groups) contained in the polymer electrolyte membrane, reducing the ionic conductivity of the electrolyte membrane.
[0049] In order to prevent degradation of a polymer electrolyte membrane (more specifically, an ionomer) due to radicals, the introduction of a radical scavenger capable of removing the radicals has been proposed.
[0050] However, the radical scavenger dispersed in the electrolyte membrane in the form of particles has a problem of migration during the operation of the fuel cell, that is, the amount of radical scavenger capable of removing radicals decreases, and therefore the longer the operation time of the fuel cell, the less the radical removal is performed, and the performance of the fuel cell rapidly decreases.
[0051] In addition, metal ions generated by ionization of the radical scavenger are dissolved by water, and because these metal ions have a very high reduction potential, they oxidize the components of the electrodes (e.g., platinum and / or carbon), causing a decrease in the performance of the fuel cell.
[0052] In contrast, the reinforced composite membrane for a fuel cell according to the present invention further includes a porous support in an electrolyte membrane containing a proton-conducting polymer, thereby improving the physical stability and mechanical properties of the electrolyte membrane, and at the same time, preventing the elution of metal ions, specifically, radical scavengers capable of removing radicals generated during the operation of the fuel cell, into the porous support, thereby enabling the performance of the fuel cell to be maintained for a long period of time and the lifespan of the fuel cell to be improved.
[0053] The porous support 5 serves to increase the mechanical strength of the reinforced composite membrane and to increase dimensional stability by suppressing volume expansion due to moisture. A typical porous support used in the industry may be used, or the porous support may be prepared by chemically hardening nanofibers of a polymer precursor prepared by electrospraying a solution containing a polymer precursor for forming the porous support.
[0054] It is preferable that the porous support 5 contains a hydrocarbon polymer which is insoluble in common organic solvents and therefore exhibits excellent chemical resistance, facilitates the process of filling the pores of the porous support with an ion conductor, and is hydrophobic and therefore unlikely to deform due to moisture in a high humidity environment. Examples of the hydrocarbon polymer include nylon, polyvinylidene fluoride (PVDF), polyphenylene sulfide (PPS), polyether ether ketone (PEEK), polylactic acid (PLA), polyimide (PI), polybenzoxazole (PBO), polybenzimidazole (PBI), polyamideimide (PAI), polyethyleneterephthalate (PET), polyethylene (PE), polytetrafluoroethylene (PTFE), polypropylene (PP), copolymers thereof, and mixtures thereof. Among these, polyimide or polytetrafluoroethylene, which has excellent heat resistance, chemical resistance, and dimensional stability, is preferred.
[0055] In one embodiment, the thickness of the porous support 5 may be 1 to 100 μm, for example, 1 to 75 μm, preferably 1 to 50 μm, and more preferably 3 to 40 μm. If the thickness of the porous support 5 is less than 1 μm, the physical and mechanical properties of the reinforced composite membrane may not be sufficiently ensured, so that durability and dimensional stability may be reduced, if the thickness exceeds 75 μm, the impregnation efficiency of the proton conductive polymer may be reduced, so that the membrane yield may be reduced, and if the thickness exceeds 100 μm, impregnation of the ion conductive polymer may be difficult, so that the proton conductivity and membrane performance may be reduced.
[0056] The porosity of the porous support 5 may be 40 to 95%, for example, 50 to 90%, and preferably 55 to 85%. If the porosity of the porous support 5 is less than 40%, the impregnation rate of the proton conductive polymer may decrease, which may result in a decrease in membrane performance, and if the porosity is more than 95%, the durability of the reinforced composite membrane may not be sufficiently ensured.
[0057] The reinforced composite membrane 10 may be one in which the proton-conducting polymer is impregnated into a porous support 5, or an electrolyte layer (1 and / or 3) containing the proton-conducting polymer is formed on at least one surface of the porous support 5.
[0058] In the case where the proton-conducting polymer is impregnated into the porous support 5, the proton-conducting polymer is dispersed in a solvent to prepare a mixed solution, and then the porous support 5 is immersed in the mixed solution to form a reinforced composite membrane in which the proton-conducting polymer is impregnated into the porous support 5. The solvent may be water, a hydrophilic solvent, an organic solvent, or a mixed solvent of two or more thereof.
[0059] In the case of the reinforced composite membrane 10 in which an electrolyte layer (1 and / or 3) containing the proton conductive polymer is formed on at least one surface of the porous support 5, the electrolyte membrane containing the proton conductive polymer may be formed by coating a mixed solution of the proton conductive polymer on at least one surface of the porous support 5, drying the mixed solution, or casting the mixed solution, and drying the mixed solution to form an electrolyte membrane containing the proton conductive polymer, and laminating the electrolyte membrane with at least one surface of the porous support 5. In addition, in the case of forming the electrolyte layer (1 and / or 3) in a multi-layer structure, a mixed solution having different concentrations and types of the proton conductive polymer may be sequentially coated on the porous support 5 and dried or laminated. In this case, the coating or casting of the mixed solution may be performed by bar coating, comma coating, slot die, screen printing, spray coating, doctor blade, or laminating.
[0060] Alternatively, the reinforced composite membrane 10 may have a configuration in which an electrolyte layer (1 and / or 3) is formed by laminating an electrolyte membrane containing a hydrogen ion polymer on at least one surface of the porous support 5 impregnated with the hydrogen ion conductive polymer.
[0061] The drying may be performed by applying heat at 60° C. to 100° C. for about 1 minute to 30 minutes, or preferably by applying heat at 70° C. to 90° C. for about 5 minutes to 15 minutes. If the drying temperature is less than 60° C., the liquid retention of the proton conductive polymer solution may be reduced, and if it exceeds 100° C., the bonding with the electrodes during the manufacture of the reinforced composite membrane and / or membrane electrode assembly may be reduced.
[0062] In the reinforced composite membrane 10 according to one embodiment, the porous support 5 is impregnated with a proton conductive polymer or an electrolyte layer (1 and / or 3) containing a proton conductive polymer is provided on at least one surface of the porous support 5, so that the reinforced composite membrane 10 has a structure in which the proton conductive polymer is continuously distributed from the surface of the porous support 5 to the thickness direction of the reinforced composite membrane 10, thereby improving the ionic conductivity of the reinforced composite membrane.
[0063] The proton-conducting polymer may be any polymer that is generally used as a proton conductor in an electrolyte membrane of a fuel cell, without any particular limitation. Specifically, a fluorine-based polymer, a hydrocarbon-based polymer, or a mixture thereof that has excellent proton-conducting function, is inexpensive, and is soluble in an organic solvent may be used.
[0064] Specifically, the proton conductive polymer is preferably a polymer having an ion exchange capacity (IEC) of 0.8 meq / g or more. By using a polymer having such a high ion exchange capacity, the content of the proton conductive polymer in the composition for forming a porous support can be reduced, and as a result, the decrease in strength and dimensional stability of the porous support due to the use of the proton conductive polymer can be prevented.
[0065] Specific examples thereof include poly(perfluorosulfonic acid), poly(perfluorocarboxylic acid), copolymers of tetrafluoroethylene and fluorovinyl ether containing sulfonic acid groups, fluoropolymers including defluorinated sulfurized polyether ketone or mixtures thereof, sulfonated polyimide (S-PI), sulfonated polyarylethersulfone (S-PAES), sulfonated polyetheretherketone (SPEEK), sulfonated polybenzimidazole (SPBI), sulfonated polysulfone (S-PSU), sulfonated polystyrene (S-PS), sulfonated polyphosphazene, sulfonated polyquinoxaline, sulfonated polyketone (S-PS), sulfonated polyphenylene ... sulfonated polyketone, sulfonated polyphenylene oxide, sulfonated polyether sulfone, sulfonated polyether ketone, sulfonated polyphenylene sulfone, sulfonated polyphenylene sulfide, sulfonated polyphenylene sulfide sulfone, sulfonated polyphenylene sulfide sulfone nitrile, sulfonated polyarylene ether, sulfonated polyarylene ether nitrileThe polymer may be selected from the group consisting of hydrocarbon polymers and mixtures thereof, including polyarylene ether nitrile, sulfonated polyarylene ether ether nitrile, polyarylene ether sulfone ketone, and mixtures thereof.
[0066] In an embodiment, the porous support 5 may further include a compound capable of capturing metal ions.
[0067] The metal ions are particles capable of removing peroxides or radicals that cause deterioration of the electrolyte membrane and reduce its ion conductivity during the operation of the fuel cell, and may refer to ions of transition metals or precious metals.
[0068] In one embodiment, the metal ion may be a cerium (Ce) ion, a manganese (Mn) ion, a tungsten (W) ion, a cobalt (Co) ion, a vanadium (V) ion, a nickel (Ni) ion, a chromium (Cr) ion, a zirconium (Zr) ion, a yttrium (Y) ion, an iridium (Ir) ion, an iron (Fe) ion, a titanium (Ti) ion, a molybdenum (Mo) ion, a lanthanum (La) ion, a neodymium (Nd) ion, or a combination thereof. For example, the metal ion may be a cerium trivalent ion (Ce). 3+ ) or cerium ion (Ce 4+ ) may also be used.
[0069] In one embodiment, the compound capable of capturing metal ions may be included in an amount of preferably 1 to 50 wt%, more preferably 1 to 30 wt%, based on the total weight of the porous support. If the content is less than 1 wt%, the efficiency of capturing metal ions may not be sufficient, and if it exceeds 50 wt%, the mechanical strength of the porous support may be reduced.
[0070] In one embodiment, the compound capable of capturing the metal ions may include polyethylene glycol, polypropylene glycol, polybutylene glycol, crown ether, or a combination thereof, and preferably may include polyethylene glycol, crown ether, or a combination thereof. Although the present invention is not limited to a particular theory, it can be understood that the metal ions are captured without being dissolved from the reinforced composite membrane by the unshared electron pair of the oxygen atom contained in the polyethylene glycol, polypropylene glycol, polybutylene glycol, or crown ether surrounding the metal ions.
[0071] In one embodiment, the weight average molecular weight of the polyethylene glycol, polypropylene glycol, and polybutylene glycol, especially the polyethylene glycol, may be 60 to 6,000 g / mol, for example, 100 to 4,000 g / mol, preferably 100 to 2,000 g / mol. If the weight average molecular weight is less than 60 g / mol, there is a problem that the metal ion capturing ability is reduced, and if it exceeds 6,000 g / mol, there is a problem that it is impossible to dissolve in a dispersion liquid and it is difficult to have ionicity after forming a polymer electrolyte membrane due to a decrease in the fluidity of the polymer, so it is appropriately adjusted within the above range.
[0072] In one embodiment, the crown ether may include 12-crown-4-ether, 15-crown-5-ether, 18-crown-6-ether, benzo-15-crown-5-ether, N-phenylarzo-15-crown-5-ether, 2-aminomethyl-18-crown-6, or a combination thereof.
[0073] The compound capable of capturing the metal ion (e.g., polyethylene glycol, crown ether, etc.) may be included in an amount that provides a weight ratio of 1:0.5 or more, specifically 1:0.8 or more, more specifically 1:0.8 to 1:3.5, or 1:0.8 to 1:3.3, or 1:0.8 to 1:3. If the compound capable of capturing the metal ion is less than 1:0.5, the capture is not effective, and the capture effect improves as the ratio increases, but if the ratio is 1:3.5 or more, the improvement effect may not be clear.
[0074]
[0075] Another embodiment of the present invention provides a method for manufacturing a reinforced composite membrane for a fuel cell, the method comprising the steps of: preparing a porous support from a composition including a precursor of a polymer for forming a porous support and a compound capable of capturing metal ions; and impregnating the porous support with a proton-conducting polymer or forming an electrolyte layer including a proton-conducting polymer on at least one surface of the porous support.
[0076] Each step will be described below. Step 1 is a step of preparing a porous support using a polymer precursor for forming a porous support and a compound capable of capturing metal ions.
[0077] The step of preparing the porous support in step 1 is carried out by electro-irradiating the composition.
[0078] The porous support may be prepared without being dissolved in an organic solvent, or may be prepared by forming a nanofiber precursor using a precursor of the polymer for forming the porous support that is highly soluble in an organic solvent, and then subjecting the precursor to a predetermined reaction. The precursor of the polymer for forming the porous support may be appropriately selected and used depending on the type of the polymer for forming the porous support, and specific types of the polymer for forming the porous support are as described above.
[0079] For example, a porous support made of PI (Polyimide) can be prepared by imidization of polyamic acid (PAA). The polyamic acid can be prepared by a conventional method, specifically, by mixing diamine in a solvent, adding dianhydride thereto, and then polymerizing the mixture.
[0080] The dianhydride may be a compound selected from the group consisting of pyromellitic dianhydride (PMDA), 3,3',4,4'-benzophenonetetracarboxylic dianhydride (BTDA), 4,4'-oxydiphalic anhydride (ODPA), 3,4,3',4'-biphenyltetracarboxylic dianhydride (BPDA), bis(3,4-dicarboxyphenyl)dimethylsilane dianhydride (SiDA), and mixtures thereof. The diamine may be 4,4'-oxydianiline (ODA), p-phenylenediamine (p-phenylenediamine), ... The solvent for dissolving the polyamic acid may be selected from the group consisting of m-cresol, N-methyl-2-pyrrolidone (NMP), dimethylformamide (DMF), dimethylacetamide (DMAc), dimethylsulfoxide (DMSO), acetone, diethyl acetate, tetrahydrofuran (THF), chloroform, γ-butyrolactone, and mixtures thereof.
[0081] At this time, the polymer precursor for forming the porous support is preferably included in a concentration of 5 to 20 wt % based on the total weight of the electro-emitting composition. If the concentration of the electro-emitting composition solution is less than 5 wt %, emission is not smooth, so fibers are not formed or fibers with a uniform diameter cannot be produced, while if the concentration of the electro-emitting composition exceeds 20 wt %, the discharge pressure increases rapidly, so emission is not performed or processability may be deteriorated.
[0082] The compound capable of capturing metal ions is as described above, and specifically may include polyethylene glycol, polypropylene glycol, polybutylene glycol, crown ether, or a combination thereof. It is preferable to appropriately determine the content of the compound capable of capturing metal ions contained in the composition for electric emission in consideration of the final porous support to be manufactured and the content of the compound capable of capturing metal ions.
[0083] The compound capable of capturing metal ions may be included in an amount of 1 to 50 parts by weight, preferably 1 to 20 parts by weight, and more preferably 1 to 10 parts by weight, based on 100 parts by weight of the composition, specifically, the composition for electric radiation. If the content of the compound capable of capturing metal ions is less than 1 part by weight based on 100 parts by weight of the porous support, the metal ion capturing effect may be insufficient, and thus the durability of the polymer electrolyte may not be maintained. If the content exceeds 50 parts by weight, there may be a problem that the physical properties of the support may be deteriorated, which may cause a deterioration in the physical properties of the polymer electrolyte membrane.
[0084] Next, the polymer precursor for forming a porous support and a compound capable of collecting metal ions are mixed to prepare an electric radiation composition, which is then subjected to electric radiation to prepare a nanofiber web; alternatively, an electric radiation composition containing a precursor of the polymer for forming a porous support and an electric radiation composition containing a compound capable of collecting metal ions are separately prepared, and then the compositions are simultaneously subjected to electric radiation through respective radiation nozzles to prepare a nanofiber web in which the nanofibers of the polymer precursor and the nanofibers of the compound capable of collecting metal ions are entangled together.
[0085] In preparing the composition for electric radiation, the precursor of the polymer for forming the porous support or the compound capable of capturing metal ions may be dissolved in a common organic solvent such as NMP (N-Methyl-2-Pyrrolidone), DMF (dimethyl formamide), DMAc (dimethyl acetamide), DMSO (dimethyl sulfoxide), THF (tetrahydrofuran), etc.
[0086] The electroirradiation can be carried out according to a conventional electroirradiation process for producing nanofibers.
[0087] In detail, a constant amount of the composition for electric radiation is supplied to the emitting part using a metering pump from a solution tank storing the composition for electric radiation, the composition for electric radiation is discharged through the nozzle of the emitting part, and then polymer nanofibers are formed by solidifying and hardening while scattering, and the solidified nanofibers are collected in a collector having a releasing film to produce a fiber aggregate. At this time, the strength of the electric field between the emitting part and the collector applied by the high voltage generating part is preferably 850 to 3,500 V / cm. If the strength of the electric field is less than 850 V / cm, it is difficult to produce nanofibers with a uniform thickness since the precursor solution is not continuously discharged, and the nanofibers formed after emission cannot be smoothly collected on the collector, which may make it difficult to produce a fiber aggregate. On the other hand, if the strength of the electric field exceeds 3,500 V / cm, the nanofibers are not accurately seated on the collector, and a fiber aggregate of a normal shape cannot be obtained.
[0088] The radiation process produces nanofibers having a uniform fiber diameter, preferably an average diameter of 0.01 to 5 μm, which are randomly arranged to form a fiber assembly, ie, a web.
[0089] Additionally, a chemical hardening step can be performed on the produced nanofiber web.
[0090] Generally, the curing of the precursor of the hydrocarbon polymer is performed by heat treatment, but since the nanofiber web of the present invention contains a compound capable of capturing metal ions, such as polyethylene glycol, polypropylene glycol, polybutylene glycol, and crown ether, when the curing process is performed by excessive heat treatment, the compound capable of capturing metal ions may be denatured, evaporated, or decomposed by heat. Therefore, in the present invention, the nanofiber web obtained after the electric radiation is impregnated with a curing agent to induce the curing of the polymer precursor. In this case, the curing agent used may be acetic anhydride, pyridine, triethylamine, toluenesulfonic acid, hydroxybenzyl alcohol, aminophenol, hydroxybenzaldehyde, aminobenzoic acid, or the like. The curing agent that can be used in the present invention is not limited to the above-mentioned compounds, and it is preferable to select the curing agent appropriately according to the type of the precursor of the polymer for forming the porous support used to manufacture the porous support.
[0091] The content of the curing agent is preferably determined appropriately according to the content of the polymer precursor contained in the electro-radiating composition.
[0092] In the curing process, the polymer precursor is cured to convert it into a polymer for forming a porous support. For example, if the nanofiber or fiber aggregate is made of a polyimide precursor during the electro-irradiation, it is converted into polyimide by imidization through chemical curing.
[0093] Step 2 is a step of impregnating the porous support prepared in step 1 with a proton-conducting polymer or forming an electrolyte layer including a proton-conducting polymer on at least one surface of the porous support.
[0094] In one embodiment, step 2 may include preparing a mixed solution by dispersing the proton conductive polymer in a solvent, and immersing the porous support in the mixed solution, but is not limited thereto and may be performed using various methods known in the art, such as a spray process, a screen printing process, a doctor blade process, etc. When the impregnation process is used, it is preferable to perform the impregnation process 1 to 5 times at room temperature for 5 to 30 minutes.
[0095] The solvent can dissolve the proton conductive polymer well, and examples of the solvent include, but are not limited to, N-methyl-2-pyrrolidinone (NMP), dimethylformamide (DMF), and dimethylacetamide (DMA).
[0096] As the hydrogen ion conductive polymer, the same polymer as described above can be used.
[0097] In addition, in one embodiment, step 2 may include dispersing the proton conductive polymer in a solvent to prepare a mixed solution, casting and drying the mixed solution to form an electrolyte membrane, and laminating the electrolyte membrane with the porous support.
[0098] In the step of preparing the reinforced composite membrane, the application and casting of the solvent and the mixed solution for dispersing the proton conductive polymer have been described above, and therefore, a repeated description will be omitted.
[0099] The proton conductive polymer is preferably appropriately determined in consideration of the content of the proton conductive polymer contained in the reinforced composite membrane. Specifically, the proton conductive polymer may be contained in the proton conductive polymer-containing solution at 5 to 40 wt %. If the proton conductive polymer is contained in the proton conductive polymer-containing solution at less than 5 wt %, the proton conductive polymer may not be sufficiently filled in the pores of the porous support, forming empty spaces, and if the proton conductive polymer is contained in the proton conductive polymer-containing solution at more than 40 wt %, the viscosity of the proton conductive polymer-containing solution may be too high to fill the pores of the porous support.
[0100] After filling the proton-conducting polymer-containing solution, the organic solvent in the proton-conducting polymer-containing solution is removed so that the proton-conducting polymer fills the pores of the porous support. Therefore, the method for manufacturing a reinforced composite membrane for a fuel cell according to the present invention may further include a step of removing the organic solvent after filling the proton-conducting polymer, and the organic solvent removal step may be performed by drying in a vacuum oven at 60 to 50° C. for 2 to 15 hours.
[0101] Proton Conducting Polymer The reinforced composite membrane prepared by the above-mentioned preparation method has excellent proton conductivity and therefore can exhibit improved proton conductivity when used as a polymer electrolyte membrane in a membrane electrode assembly for a fuel cell.
[0102] According to yet another embodiment of the present invention, there is provided a membrane electrode assembly and a fuel cell including the reinforced composite membrane.
[0103] Specifically, the membrane electrode assembly includes an anode electrode and a cathode electrode positioned opposite each other, and the reinforced composite membrane positioned between the anode electrode and the cathode electrode.
[0104] 2 is a schematic cross-sectional view of a membrane electrode assembly according to an embodiment of the present invention. Referring to FIG. 2, the membrane electrode assembly 100 includes the reinforced composite membrane 50 and the fuel cell electrodes 20, 20' disposed on both sides of the reinforced composite membrane 50. The electrodes 20, 20' include electrode substrates 40, 40' and catalyst layers 30, 30' formed on the surfaces of the electrode substrates 40, 40', and may further include a microporous layer (not shown) between the electrode substrates 40, 40' and the catalyst layers 30, 30' containing conductive fine particles such as carbon powder or carbon black to facilitate diffusion of materials in the electrode substrates 40, 40'.
[0105] In the membrane electrode assembly 100, the electrode 20 disposed on one side of the reinforced composite membrane 50 and performing an oxidation reaction to generate hydrogen ions and electrons from the fuel delivered to the catalyst layer 30 through the electrode substrate 40 is referred to as an anode electrode, and the electrode 20' disposed on the other side of the reinforced composite membrane 50 and performing a reduction reaction to generate water from the hydrogen ions supplied through the reinforced composite membrane 50 and the oxidant delivered to the catalyst layer 30' through the electrode substrate 40' is referred to as a cathode.
[0106] The catalyst layers 30, 30' of the anode and cathode electrodes 20, 20' include a catalyst. The catalyst can be any catalyst that participates in the cell reaction and can be used as a catalyst in a general fuel cell. Specifically, platinum-based metals can be preferably used.
[0107] The platinum-based metals include platinum (Pt), palladium (Pd), ruthenium (Ru), iridium (Ir), osmium (Os), platinum-M alloys (wherein M is palladium (Pd), ruthenium (Ru), iridium (Ir), osmium (Os), and the like. (Os), gallium (Ga), titanium (Ti), vanadium (V), chromium (Cr), manganese (Mn), iron (Fe), cobalt (Co), nickel (Ni), copper (Cu), silver (Ag), gold (Au), zinc (Zn), tin (Sn), molybdenum (Mo), tungsten (W), lanthanum (La), and rhodium (Rh), non-platinum alloys, and combinations thereof. More preferably, a combination of two or more metals selected from the platinum-based catalytic metal group can be used, but the present invention is not limited thereto, and any platinum-based catalytic metal that can be used in the present technical field can be used without limitation.
[0108] Specifically, the platinum alloy may be selected from the group consisting of Pt-Pd, Pt-Sn, Pt-Mo, Pt-Cr, Pt-W, Pt-Ru, Pt-Ru-W, Pt-Ru-Mo, Pt-Ru-Rh-Ni, Pt-Ru-Sn-W, Pt-Co, Pt-Co-Ni, Pt-Co-Fe, Pt-Co-Ir, Pt-Co-S, Pt-Co-P, Pt-Fe, Pt-Fe-Ir, Pt-Fe-S, Pt-Fe-P, Pt-Au-Co, Pt-Au-Fe, Pt-Au-Ni, Pt-Ni, Pt-Ni-Ir, Pt-Cr, Pt-Cr-Ir, and combinations thereof, and may be used alone or in combination of two or more.
[0109] The non-platinum alloy may be selected from the group consisting of Ir-Fe, Ir-Ru, Ir-Os, Co-Fe, Co-Ru, Co-Os, Rh-Fe, Rh-Ru, Rh-Os, Ir-Ru-Fe, Ir-Ru-Os, Rh-Ru-Fe, Rh-Ru-Os, and combinations thereof, and may be used alone or in combination of two or more.
[0110] Such a catalyst can be used as a catalyst itself (black) or can be supported on a carrier.
[0111] The support can be selected from carbonaceous supports, porous inorganic oxides such as zirconia, alumina, titania, silica, and ceria, and zeolites. The carbon-based support may be selected from graphite, super P, carbon fiber, carbon sheet, carbon black, Ketjen Black, Denka Black, acetylene black, carbon nano tube (CNT), carbon sphere, carbon ribbon, fullerene, activated carbon, carbon nanofiber, carbon nanowire, carbon nanoball, carbon nanohorn, carbon nanocage, carbon nanoring, ordered nano- / meso-porous carbon, carbon aerogel, mesoporous carbon, graphene, stabilized carbon, activated carbon, and combinations of one or more thereof, but is not limited thereto, and any support available in the art may be used without limitation.
[0112] The catalyst particles may be located on the surface of the support and may permeate the interior of the support, filling the internal pores of the support.
[0113] When the precious metal supported on the carrier is used as a catalyst, a commercially available product may be used, or a catalyst prepared by supporting a precious metal on a carrier may be used. The process of supporting a precious metal on a carrier is well known in the art, and therefore, even if a detailed description is omitted in this specification, it is easily understandable to those who are engaged in the art.
[0114] The catalyst particles may be contained in an amount of 20 wt % to 80 wt % based on the total weight of the catalytic electrodes 30, 30'. If the amount is less than 20 wt %, there is a problem of reduced activity, and if the amount is more than 80 wt %, the active area may decrease due to aggregation of the catalyst particles, thereby reducing the catalytic activity.
[0115] In addition, the catalytic electrodes 30 and 30' may include a binder to improve adhesion and transfer protons of the catalytic electrodes 30 and 30'. It is preferable to use an ion conductor having ion conductivity as the binder, and the ion conductor has been described above, so a repeated description will be omitted.
[0116] However, the ion conductor may be used alone or in a mixture, and may be used together with a non-conductive compound to further improve adhesion to the reinforced composite membrane 50. The amount of the ion conductor used may be adjusted to suit the intended purpose.
[0117] As the non-conductive compound, one or more selected from the group consisting of polytetrafluoroethylene (PTFE), tetrafluoroethylene-hexafluoropropylene copolymer (FEP), tetrafluoroethylene-perfluoroalkylvinylether copolymer (PFA), ethylene / tetrafluoroethylene (ETFE), ethylene chlorotrifluoro-ethylene copolymer (ECTFE), polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene copolymer (PVdF-HFP), dodecylbenzenesulfonic acid, and sorbitol may be used.
[0118] The binder may be included in an amount of 20 to 80 weight percent of the total weight of the catalytic electrodes 30 and 30'. If the binder content is less than 20 weight percent, the generated ions may not be transferred well, and if it exceeds 80 weight percent, the pores may be insufficient, making it difficult to supply hydrogen or oxygen (air), and the active area for reaction may be reduced.
[0119] The electrode substrates 40 and 40' may be porous conductive substrates so that hydrogen or oxygen can be smoothly supplied. Representative examples thereof include, but are not limited to, carbon paper, carbon cloth, carbon felt, or metal cloth (a porous film made of metal cloth in a fibrous state or a cloth made of polymeric fibers on which a metal film is formed). In addition, it is preferable to use the electrode substrates 40 and 40' that are water-repellent treated with fluorine-based resin, since this prevents the reactant diffusion efficiency from decreasing due to water generated during the operation of the fuel cell. The fluorine-based resin may be polytetrafluoroethylene, polyvinylidene fluoride, polyhexafluoropropylene, polyperfluoroalkylvinyl ether, polyperfluorosulfonyl fluoride alkoxyvinyl ether, fluorinated ethylene propylene, polychlorotrifluoroethylene, or copolymers thereof.
[0120] Also, a microporous layer for enhancing the reactant diffusion effect in the electrode substrate 40, 40' may be further included. The microporous layer may generally include a conductive powder having a small particle size, for example, carbon powder, carbon black, acetylene black, activated carbon, carbon fiber, fullerene, carbon nanotube, carbon nanowire, carbon nano-horn, or carbon nano ring.
[0121] The microporous layer is manufactured by coating the electrode substrate 40, 40' with a composition including a conductive powder, a binder resin, and a solvent. As the binder resin, polytetrafluoroethylene, polyvinylidene fluoride, polyhexafluoropropylene, polyperfluoroalkylvinyl ether, polyperfluorosulfonyl fluoride, alkoxyvinyl ether, polyvinyl alcohol, cellulose acetate, or copolymers thereof can be preferably used. As the solvent, alcohols such as ethanol, isopropyl alcohol, n-propyl alcohol, and butyl alcohol, water, dimethylacetamide, dimethylsulfoxide, N-methylpyrrolidone, and tetrahydrofuran can be preferably used. The coating process may be performed by screen printing, spray coating, or a coating method using a doctor blade, depending on the viscosity of the composition, but is not limited thereto.
[0122] The membrane electrode assembly 100 can be manufactured by a conventional method for manufacturing a membrane electrode assembly for a fuel cell, except that the reinforced composite membrane 50 according to the present invention is used as the reinforced composite membrane 50.
[0123] A fuel cell according to another embodiment of the present invention may include the membrane electrode assembly 100.
[0124] FIG. 3 is a schematic diagram showing the overall configuration of the fuel cell.
[0125] Referring to FIG. 3, the fuel cell 200 includes a fuel supply unit 210 that supplies a mixed fuel obtained by mixing fuel and water, a reformer 220 that reforms the mixed fuel to generate a reformed gas including hydrogen gas, a stack 230 in which the reformed gas including hydrogen gas supplied from the reformer 220 undergoes an electrochemical reaction with an oxidant to generate electrical energy, and an oxidant supply unit 240 that supplies the oxidant to the reformer 220 and the stack 230.
[0126] The stack 230 includes a plurality of unit cells that generate electrical energy by inducing an oxidation / reduction reaction between the reformed gas, including hydrogen gas, supplied from the reformer 220 and an oxidant supplied from the oxidant supplying unit 240 .
[0127] Each unit cell means a unit cell that generates electricity, and includes a membrane electrode assembly that oxidizes / reduces oxygen in a reformed gas containing hydrogen gas and an oxidant, and a separator plate (also called a bipolar plate, hereinafter referred to as "separator plate") for supplying the reformed gas containing hydrogen gas and the oxidant to the membrane electrode assembly. The separator plates are disposed on both sides of the membrane electrode assembly, with the membrane electrode assembly at the center. In this case, the separator plates located at the outermost positions of the stack are also referred to as end plates.
[0128] Of the separation plates, the end plate includes a pipe-shaped first supply pipe 231 for injecting reformed gas containing hydrogen gas supplied from the reforming section 220, and a pipe-shaped second supply pipe 232 for injecting oxygen gas, and the other end plate includes a first exhaust pipe 233 for discharging reformed gas containing hydrogen gas that ultimately remains unreacted in the multiple unit cells to the outside, and a second exhaust pipe 234 for discharging oxidant that ultimately remains unreacted in the unit cells to the outside.
[0129] In the fuel cell, except that the membrane electrode assembly 100 according to one embodiment of the present invention is used, the separator, fuel supply unit and oxidant supply unit constituting the electricity generating unit are the same as those used in conventional fuel cells, and therefore a detailed description thereof will be omitted in this specification.
[0130] Specific examples of the present invention will be presented below. However, the examples described below are merely for the purpose of specifically illustrating or explaining the present invention, and the present invention is not limited thereby. In addition, the contents not described here can be sufficiently inferred by those skilled in the art, and therefore the description thereof will be omitted.
[0131]
[0132] Manufacturing Example 1
[0133] (1) A polytetrafluoroethylene / THF solution having a concentration of 25% by weight and containing 1 part by weight of polyethylene glycol (Mw: 2,000) relative to 100 parts by weight of the total solution is applied to the nozzle and electrically irradiated with a voltage of 30 kV applied, to form a polytetrafluoroethylene porous support.
[0134] (2) The prepared porous support was coated twice with an ion conductor solution containing 20% by weight of Nafion as a proton conductive polymer and 2% by weight of Ce(NO3)3 in Nafion using a doctor blade. After the first coating, the support was joined and a second coating was carried out to form a reinforced composite membrane. It was then dried at 80°C for 1 hour and in a vacuum oven for 1 hour to produce a reinforced composite membrane (weight ratio of PEG in the support was 4%).
[0135]
[0136] Manufacturing Example 2
[0137] A reinforced composite membrane was prepared in the same manner as in Preparation Example 1, except that the content of polyethylene glycol was 0.2 parts by weight based on 100 parts by weight of the total radiation solution (weight ratio of PEG in the support: 0.8%).
[0138]
[0139] Production Example 3
[0140] A reinforced composite membrane was prepared in the same manner as in Preparation Example 1, except that the content of polyethylene glycol was 2 parts by weight based on 100 parts by weight of the total radiation solution (weight ratio of PEG in the support: 8%).
[0141]
[0142] Production Example 4
[0143] A reinforced composite membrane was prepared in the same manner as in Preparation Example 1, except that the content of polyethylene glycol was 5 parts by weight based on 100 parts by weight of the total radiation solution (weight ratio of PEG in the support: 20%).
[0144]
[0145] Production Example 5
[0146] A reinforced composite membrane was prepared in the same manner as in Preparation Example 1, except that the content of polyethylene glycol was 30 parts by weight based on 100 parts by weight of the total radiation solution (weight ratio of PEG in the support: 54.5%).
[0147]
[0148] Production Example 6
[0149] A reinforced composite membrane was prepared in the same manner as in Preparation Example 1, except that a polyphenylene sulfide / THF irradiating solution was used instead of the polytetrafluoroethylene / THF irradiating solution (weight ratio of PEG in the support: 4%).
[0150]
[0151] Production Example 7
[0152] A reinforced composite membrane was prepared in the same manner as in Preparation Example 6, except that the content of polyethylene glycol was 2 parts by weight based on 100 parts by weight of the total radiation solution (weight ratio of PEG in the support was 8%).
[0153]
[0154] Production Example 8
[0155] A reinforced composite membrane was prepared in the same manner as in Preparation Example 6, except that the content of polyethylene glycol was 5 parts by weight based on 100 parts by weight of the total radiation solution (weight ratio of PEG in the support: 20%).
[0156]
[0157] Production Example 9
[0158] A mixture of 117g of 2,5-dichlorobenzene, 32.0g of sulfur, and 47.5g (20mol%) of 2,5-dichlorobenzoic acid was heated from 230℃ to 300℃, and the pressure was gradually reduced from 170torr to 1torr or less, and polymerization reaction was carried out for a total of 8 hours to produce a PPS copolymer having carboxyl groups as repeating units. 1wt% of 2-Aminomethyl-18-crown-6 was introduced into this PPS polymer by dehydration condensation reaction. The polymer thus produced was applied to the solution instead of polyphenylene sulfide in Preparation Example 6. A reinforced composite membrane was produced in the same manner as Preparation Example 6, except that the solution did not contain polyethylene glycol.
[0159]
[0160] Comparative Manufacturing Example 1
[0161] A reinforced composite membrane was prepared in the same manner as in Preparation Example 1 above, except that a radiation solution not containing polyethylene glycol was used.
[0162]
[0163] Comparative Manufacturing Example 2
[0164] A reinforced composite membrane was prepared in the same manner as in Preparation Example 6 above, except that a radiation solution containing no polyethylene glycol was used.
[0165]
[0166] Examples 1 to 9 and Comparative Examples 1 to 2
[0167] A membrane electrode assembly was manufactured by forming an electrode layer on the reinforced composite membrane manufactured in Manufacturing Examples 1 to 9 and Comparative Manufacturing Examples 1 to 2 using a decal transfer method. In this case, the catalyst layer of the electrode was formed by applying a catalyst layer forming composition containing a Pt / carbon catalyst to a release film and drying it to form a catalyst layer. The release films coated with the catalyst layer were placed on both sides of the reinforced composite membrane so that the catalyst layer and the reinforced composite membrane faced each other, and then a pressure of 5 kg / cm was applied. 2 The catalyst layers were transferred to both sides of the reinforced composite membrane by hot pressing at a pressure of 100° C. and a temperature of 100° C. Then, gas diffusion layers (GDLs) were fastened to both sides of the reinforced composite membrane to which the catalyst layers were bonded, to manufacture a membrane electrode assembly.
[0168]
[0169] Evaluation example 1 - Battery performance evaluation
[0170] The membrane electrode assemblies manufactured in the above examples and comparative examples were evaluated. The output performance was evaluated by IV measurement of the membrane electrode assemblies. Specifically, to confirm the output performance under actual fuel cell operating conditions, the membrane electrode assemblies were attached to a fuel cell unit cell evaluation device and the temperature was maintained at 65°C. Hydrogen (100% RH) and air (100% RH) were supplied to the anode and cathode, respectively, in amounts that matched stoichiometry 1.2 / 2.0. The current density was measured at 0.6V, and a higher value indicates better output performance. The evaluation results are shown in Table 1 below.
[0171]
[0172] Evaluation example 2 - Dimensional stability evaluation
[0173] The reinforced composite membranes manufactured in Preparation Examples 1 to 8 and Comparative Preparation Examples 1 and 2 were dried in a vacuum oven at 80°C for 12 hours, and their dimensions were measured. They were then immersed in distilled water at room temperature for 24 hours, after which their dimensions were measured and the dimensional ratios before and after water absorption were compared. The lower the dimensional change rate, the higher the stability. The evaluation results are shown in Table 1 below.
[0174]
[0175] Evaluation example 3: Chemical durability evaluation
[0176] The membrane electrode assemblies manufactured according to the above examples and comparative examples were evaluated. The evaluation cells were placed in an OCV state, and the cell voltage was measured at regular intervals to calculate the rate of decrease compared to the initial OCV. Measurements were performed using a Scribner 850 fuel cell test system as the measurement equipment (evaluation was performed under conditions of 90°C, 30% RH, and 50 kPa). Specifically, the OCV(V) / initial OCV(V) was measured over time (hr) every 24 hours. The evaluation was terminated when this ratio was 0.8 or less, and the measurement time was used as the criterion for durability. The evaluation results are shown in Table 1 below.
[0177]
[0178] [Table 1]
[0179] It can be seen from Table 1 that the chemical durability is improved when the reinforced composite membrane according to the embodiment of the present invention is used compared to the comparative example. However, in the case of Example 2, the polyethylene glycol content was low and the support was not sufficiently coated, so the collection efficiency was not sufficient, and in the case of Example 5, the polyethylene glycol content was high and the support strength was somewhat reduced.
[0180]
[0181] Although a preferred embodiment of the present invention has been described in detail above, the embodiment is presented as a specific example of the present invention and the present invention is not limited thereto. The scope of the present invention also includes various modifications and improvements made by those skilled in the art using the basic concept of the present invention defined in the claims.
[0182]
[0183] [Explanation of symbols]
[0184] 10, 50: Reinforced composite membrane
[0185] 1,3: Electrolyte layer 5: Porous support
[0186] 20, 20': Electrode 30, 30': Catalyst layer 40, 40': Electrode base material
[0187] 100: Membrane electrode assembly
[0188] 200: Fuel cell
[0189] 210: Fuel supply section 220: Reforming section
[0190] 230: Stack 231: First supply pipe
[0191] 232: 2nd supply pipe 233: 1st discharge pipe
[0192] 234: Second exhaust pipe 240: Oxidizer supply section
Claims
1. A reinforced composite membrane comprising a porous support and a proton-conducting polymer, The reinforced composite membrane is formed by impregnating the proton-conducting polymer into the porous support or by providing an electrolyte layer including the proton-conducting polymer on at least one surface of the porous support; The porous support further comprises a compound capable of capturing metal ions. Reinforced composite membrane for fuel cells.
2. The compound capable of capturing metal ions includes polyethylene glycol, polypropylene glycol, polybutylene glycol, crown ether, or a combination thereof; 10. The reinforced composite membrane for a fuel cell according to claim 1.
3. The weight average molecular weight of the polyethylene glycol, polypropylene glycol, and polyethylene glycol is 60 to 6,000 g / mol; 3. The reinforced composite membrane for a fuel cell according to claim 2.
4. The crown ether includes 12-crown-4-ether, 15-crown-5-ether, 18-crown-6-ether, benzo-15-crown-5-ether, N-phenylazo-15-crown-5-ether, 2-aminomethyl-18-crown-6, or a combination thereof; 3. The reinforced composite membrane for a fuel cell according to claim 2.
5. The compound capable of capturing metal ions is contained in an amount of 1 to 50% by weight based on the total weight of the porous support.
10. The reinforced composite membrane for a fuel cell according to claim 1.
6. The metal ions include cerium (Ce) ions, manganese (Mn) ions, tungsten (W) ions, cobalt (Co) ions, vanadium (V) ions, nickel (Ni) ions, chromium (Cr) ions, zirconium (Zr) ions, yttrium (Y) ions, iridium (Ir) ions, iron (Fe) ions, titanium (Ti) ions, molybdenum (Mo) ions, lanthanum (La) ions, neodymium (Nd) ions, or combinations thereof.
10. The reinforced composite membrane for a fuel cell according to claim 1.
7. The thickness of the porous support is 1 to 100 μm.
10. The reinforced composite membrane for a fuel cell according to claim 1.
8. Preparing a porous support from a composition including a precursor of a polymer for forming a porous support and a compound capable of capturing metal ions; and impregnating the porous support with a proton-conducting polymer or forming an electrolyte layer including a proton-conducting polymer on at least one surface of the porous support; A method for producing a reinforced composite membrane for a fuel cell comprising the steps of:
9. The polymer for forming the porous support is a hydrocarbon polymer that is insoluble in an organic solvent. A method for producing the reinforced composite membrane for a fuel cell according to claim 8.
10. The compound capable of capturing metal ions includes polyethylene glycol, polypropylene glycol, polybutylene glycol, crown ether, or a combination thereof; A method for producing the reinforced composite membrane for a fuel cell according to claim 8.
11. The compound capable of capturing metal ions is included in an amount of 1 to 50 parts by weight based on 100 parts by weight of the composition. A method for producing the reinforced composite membrane for a fuel cell according to claim 8.
12. The step of producing the porous support is carried out by electro-discharging the composition. A method for producing the reinforced composite membrane for a fuel cell according to claim 8.
13. The step of forming an electrolyte layer including a proton conductive polymer includes: preparing a mixed solution by dispersing the proton-conducting polymer in a solvent; Casting the mixed solution and then drying it to form an electrolyte layer; and laminating the electrolyte layer with a porous support; Including, A method for producing the reinforced composite membrane for a fuel cell according to claim 8.
14. an anode electrode and a cathode electrode positioned opposite each other; 2. A reinforced composite membrane for a fuel cell according to claim 1, located between said anode and cathode electrodes. A membrane electrode assembly comprising:
15. A fuel cell comprising a membrane electrode assembly according to claim 14.
Citation Information
Patent Citations
Polymer electrolyte membrane and membrane electrode assembly for polymer electrolyte fuel cell
JP2008130460A
Composite polymer electrolyte membrane, manufacturing method of the same, and manufacturing method of membrane electrode assembly
JP2011222499A
Polymer electrolyte membrane, method for producing the same, and membrane electrode assembly including the same
JP2021503694A