Glass-ceramic articles having improved mechanical properties and low haze - Patents.com

A tailored glass-ceramic composition and heat treatment process improve mechanical strength and reduce haze, addressing limitations in existing glass-ceramics for portable devices by optimizing SiO2, Al2O3, P2O5, Li2O, ZrO2, and CaO ratios and incorporating ion exchange techniques.

JP2024544931APending Publication Date: 2024-12-05CORNING INC

Patent Information

Application Number
JP2024527576
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-11-12
Filing Date
2022-11-10
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Existing glass-ceramic compositions face challenges in achieving high mechanical strength and low haze, particularly in thin glass-ceramic articles suitable for portable electronic devices, due to limitations in compressive stress and central tension values, which are hindered by the difficulty in balancing lithium content and meltability.

Method used

A glass-ceramic composition comprising specific ratios of SiO2, Al2O3, P2O5, Li2O, ZrO2, and CaO, along with controlled heat treatment and ion exchange processes, to enhance compressive stress and central tension while maintaining low haze and improved mechanical properties.

Benefits of technology

The solution results in glass-ceramic articles with enhanced mechanical properties, including high compressive stress, central tension, and low haze, making them suitable for use in cover substrates and housings of portable electronic devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024544931000001_ABST
    Figure 2024544931000001_ABST
Patent Text Reader

Abstract

1. A glass-ceramic article having, by weight, greater than or equal to 65.00% and less than or equal to 80.00% SiO2, greater than 4.00% and less than or equal to 12.00% Al2O3, greater than or equal to 0.10% and less than or equal to 3.5% P2O5, greater than or equal to 8.00% and less than or equal to 17.00% Li2O, greater than or equal to 4.00% and less than or equal to 15.00% ZrO2, and greater than or equal to 0.05% and less than or equal to 4.00% CaO.
Need to check novelty before this filing date? Find Prior Art

Description

CROSS-REFERENCE TO RELATED APPLICATIONS

[0001] This application claims the benefit of priority under 35 U.S.C. § 119 of U.S. Provisional Patent Application No. 63 / 278,878, filed November 12, 2021, the contents of which are relied upon and incorporated by reference in its entirety into this application. [Technical field]

[0002] The present specification relates generally to glass-ceramic articles, and more particularly to glass-ceramic articles having improved mechanical properties and low haze. [Background technology]

[0003] Portable electronic devices have a demand for high strength glass. Currently, several materials are available in the market, including glass, zirconia, plastic, metal, and glass ceramic.

[0004] Although glass-ceramics have certain advantages over other materials, it can be difficult to form glass-ceramics with the properties required for high strength portable devices. Summary of the Invention [Problem to be solved by the invention]

[0005] Thus, there is a need for glass-ceramic articles with improved properties and methods for making same. [Means for solving the problem]

[0006] In Example 1, the glass-ceramic article includes, by weight, equal to or greater than 65.00% and equal to or less than 80.00% SiO2; greater than 4.00% and equal to or less than 12.00% Al2O3; equal to or greater than 0.10% and equal to or less than 3.5% P2O5; equal to or greater than 8.00% and equal to or less than 17.00% Li2O; equal to or greater than 4.00% and equal to or less than 15.00% ZrO2; and equal to or greater than 0.05% and equal to or less than 4.00% CaO.

[0007] Example 2 includes the glass-ceramic article of example 1, wherein the glass-ceramic article has a haze of less than 0.15 as measured on a 0.6 mm thick glass-ceramic article using a BYK Hazegard I Pro Setup.

[0008] Example 3 includes the glass-ceramic article of example 1 or 2, wherein the glass-ceramic article has a haze of less than 0.12, as measured on a 0.6 mm thick glass-ceramic article using a BYK Hazegard I Pro Setup.

[0009] Example 4 includes the glass-ceramic article of any of Examples 1 to 3, wherein the glass-ceramic article has an average transmittance measured at wavelengths from 450 nm to 800 nm of 85% or greater.

[0010] Example 5 includes the glass-ceramic article of any of Examples 1 to 4, wherein the glass-ceramic article comprises: greater than or equal to 30% and less than or equal to 50% by weight lithium disilicate; greater than or equal to 30% and less than or equal to 50% by weight petalite; and less than 5% by weight of a total of crystalline phases other than lithium disilicate and petalite.

[0011] Example 6 includes the glass-ceramic article of any of Examples 1 to 5, wherein the glass-ceramic article comprises greater than or equal to 5% and less than or equal to 20% by weight of residual amorphous glass.

[0012] Example 7 includes the glass-ceramic article of any of Examples 1 to 6, wherein the glass-ceramic article has a weight ratio of lithium disilicate to petalite greater than or equal to 0.5 and less than or equal to 1.5.

[0013] Example 8 includes the glass-ceramic article of any of Examples 1 to 7, comprising greater than or equal to 68.00 wt.% and less than or equal to 74.00 wt.% SiO.

[0014] Example 9 includes the glass-ceramic article of any of Examples 1 to 8, comprising greater than 5.00 wt.% and less than or equal to 9.00 wt.% Al2O3.

[0015] Example 10 includes the glass-ceramic article of any of Examples 1 to 9, comprising greater than or equal to 1.00% and less than or equal to 3.00% by weight P2O5.

[0016] Example 11 comprises the glass-ceramic article of any of Examples 1 to 10, comprising greater than or equal to 9.00 wt.% and less than or equal to 14.00 wt.% LiO.

[0017] Example 12 includes the glass-ceramic article of any of Examples 1 to 11, comprising greater than or equal to 4.50 wt.% and less than or equal to 8.00 wt.% ZrO2.

[0018] Example 13 includes the glass-ceramic article of any of Examples 1 to 12, comprising greater than or equal to 0.10 wt. % and less than or equal to 1.00 wt. % CaO.

[0019] Example 14 includes the glass-ceramic article of any of Examples 1 to 13, comprising greater than or equal to 0.01% and less than or equal to 0.5% by weight SnO2.

[0020] Example 15 includes the glass-ceramic article of any of Examples 1 to 14, wherein the glass-ceramic article has a thickness of greater than or equal to 0.1 mm and less than or equal to 2.0 mm.

[0021] Example 16 includes the glass-ceramic article of any of Examples 1 to 15, wherein the glass-ceramic article has a thickness of greater than or equal to 0.1 mm and less than or equal to 1.0 mm.

[0022] Example 17 includes an electronic device comprising a housing, a display, and a cover substrate adjacent to the display, the cover substrate comprising the glass-ceramic article of any of Examples 1 to 16.

[0023] Example 18 is a reinforced glass ceramic article including a first surface; a second surface; and a thickness, t, extending from the first surface to the second surface, wherein the reinforced glass ceramic article has a surface compressive stress at the first surface, the stress transitioning from compressive to tensile stress at a depth, measured from the first surface toward a centerline of the reinforced glass ceramic article, that is greater than or equal to 0.15t and less than or equal to 0.25t, and wherein the reinforced glass ceramic article has a maximum central tension, mCT, and the absolute value of the surface compressive stress measured at the first surface is greater than or equal to 1.5mCT and less than or equal to 2.5mCT.

[0024] Example 19 includes the reinforced glass-ceramic article of example 18, wherein the compressive stress decreases as a linear function of increasing thickness, measured from the first surface of the reinforced glass-ceramic article to a centerline of the reinforced glass-ceramic article, from a thickness of 0.07t or greater to a thickness of 0.26t.

[0025] Example 20 includes the reinforced glass-ceramic article of example 18 or 19, wherein the reinforced glass-ceramic article has a compressive stress of greater than or equal to 250 MPa and less than or equal to 400 MPa.

[0026] Example 21 includes the reinforced glass-ceramic article of any of Examples 18-20, wherein the reinforced glass-ceramic article has a compressive stress of greater than, or equal to, 300 MPa and less than, or equal to 400 MPa.

[0027] Example 22 includes the reinforced glass-ceramic article of any of Examples 18-21, wherein the reinforced glass-ceramic article has a central tension of greater than or equal to 100 MPa and less than or equal to 170 MPa.

[0028] Example 23 includes the reinforced glass-ceramic article of any of Examples 18-22, wherein the reinforced glass-ceramic article has a central tension of greater than or equal to 140 MPa and less than or equal to 170 MPa.

[0029]

[0023] Embodiment 24 relates to a reinforced glass-ceramic article having a thermal expansion coefficient of 22 J / m 2 More than 60 J / m 224. The reinforced glass-ceramic article of any of embodiments 18 to 23, having a stored strain energy of:

[0030] Example 25 includes the reinforced glass-ceramic article of any of Examples 18-22, wherein the reinforced glass-ceramic article has a fracture toughness of greater than or equal to 1.0 MPa√m and less than or equal to 2.0 MPa√m.

[0031] Example 26 includes the reinforced glass-ceramic article of any of Examples 18 to 23, wherein the reinforced glass-ceramic article has a haze of less than 0.15, as measured on a 0.6 mm thick glass-ceramic article using a BYK Hazegard I Pro Setup.

[0032] Embodiment 27 is directed to a reinforced glass-ceramic article having a hardness of 2.40 g / cm 3 More than 2.60g / cm 3 27. The reinforced glass-ceramic article of any of embodiments 18 to 26, having a density of:

[0033] Example 28 includes the reinforced glass-ceramic article of any of Examples 18 to 27, wherein the reinforced glass-ceramic article has a fracture strength of greater than or equal to 350 MPa and less than or equal to 450 MPa, measured on a glass-ceramic article having a thickness of 0.6 mm using 80 grit.

[0034] Example 29 includes the reinforced glass-ceramic article of any of Examples 18-27, wherein the reinforced glass-ceramic article has a maximum compressive stress of greater than or equal to 300 MPa and less than or equal to 400 MPa, a maximum central tensile stress of greater than or equal to 120 MPa and less than or equal to 170 MPa, and a stress at break of greater than or equal to 450 MPa and less than or equal to 550 MPa, as measured on a reinforced glass-ceramic article having a thickness of 0.6 mm.

[0035] Example 30 includes the reinforced glass-ceramic article of any of Examples 18-29, wherein the reinforced glass-ceramic article includes, at a center thereof, greater than or equal to 65.00% and less than or equal to 80.00% by weight SiO2; greater than or equal to 8.00% and less than or equal to 17.00% by weight Li2O; and greater than or equal to 4.00% and less than or equal to 15.00% by weight ZrO2.

[0036] Example 31 includes the reinforced glass-ceramic article of any of Examples 18 to 30, wherein the reinforced glass-ceramic article comprises greater than 4.00 wt.% and less than or equal to 12.00 wt.% Al2O3 at the center thereof.

[0037] Example 32 includes the reinforced glass-ceramic article of any of Examples 18 to 31, wherein the reinforced glass-ceramic article comprises, at its center, greater than or equal to 0.10% and less than or equal to 3.5% by weight P2O5.

[0038] Example 33 includes the reinforced glass-ceramic article of any of Examples 18 to 32, wherein the reinforced glass-ceramic article comprises, at a center thereof, greater than or equal to 0.05% and less than or equal to 4.00% by weight CaO.

[0039] Example 34 includes the reinforced glass-ceramic article of any of Examples 18-33, comprising at its center, greater than or equal to 68.00 wt.% and less than or equal to 74.00 wt.% SiO2.

[0040] Example 35 includes the reinforced glass-ceramic article of any of Examples 18 to 34, comprising at its center greater than 5.00% and less than or equal to 9.00% Al2O3 by weight.

[0041] Example 36 includes the reinforced glass-ceramic article of any of Examples 18 to 35, comprising at a center thereof, greater than or equal to 1.00% and less than or equal to 3.00% by weight P2O5.

[0042] Example 37 includes the reinforced glass-ceramic article of any of Examples 18 to 36, comprising at its center, greater than or equal to 9.00% and less than or equal to 14.00% by weight LiO.

[0043] Example 38 includes the reinforced glass-ceramic article of any of Examples 18 to 37, comprising at its center, greater than or equal to 4.50% and less than or equal to 8.00% by weight ZrO2.

[0044] Example 39 includes the reinforced glass-ceramic article of any of Examples 18 to 38, comprising at a center thereof, greater than or equal to 0.10% and less than or equal to 1.00% by weight CaO.

[0045] Example 40 includes the reinforced glass-ceramic article of any of Examples 18-39, comprising at its center, greater than or equal to 0.01% and less than or equal to 0.5% by weight SnO2.

[0046] Example 41 includes the reinforced glass-ceramic article of any of Examples 18 to 40, wherein the reinforced glass-ceramic article includes: greater than or equal to 30% and less than or equal to 50% by weight lithium disilicate; greater than or equal to 30% and less than or equal to 50% by weight petalite; and less than 3% by weight of a total of crystalline phases other than lithium disilicate and petalite.

[0047] Example 42 includes the reinforced glass-ceramic article of any of Examples 18 to 41, wherein the reinforced glass-ceramic article comprises greater than or equal to 5% and less than or equal to 20% by weight of residual amorphous glass.

[0048] Example 43 includes the reinforced glass-ceramic article of any of Examples 18-42, wherein the reinforced glass-ceramic article has a weight ratio of lithium disilicate to petalite greater than or equal to 0.5 and less than or equal to 1.5.

[0049] Example 44 includes the reinforced glass-ceramic article of any of Examples 18 to 43, wherein the reinforced glass-ceramic article has a haze of less than 0.15, as measured on a 0.6 mm thick glass-ceramic article using a BYK Hazegard I Pro Setup.

[0050] Example 45 includes the reinforced glass-ceramic article of any of Examples 18 to 44, wherein the reinforced glass-ceramic article has a haze of less than 0.12, as measured on a 0.6 mm thick glass-ceramic article using a BYK Hazegard I Pro Setup.

[0051] Example 46 includes the reinforced glass-ceramic article of any of Examples 18 to 45, wherein the reinforced glass-ceramic article has an average transmittance measured at wavelengths from 450 nm to 800 nm of 85% or greater.

[0052] Example 47 includes the reinforced glass-ceramic article of any of Examples 18 to 46, wherein the reinforced glass-ceramic article has a thickness of greater than or equal to 0.1 mm and less than or equal to 2.0 mm.

[0053] Example 48 includes the reinforced glass-ceramic article of any of Examples 18 to 47, wherein the reinforced glass-ceramic article has a thickness of greater than or equal to 0.1 mm and less than or equal to 1.0 mm.

[0054] Example 49 includes an electronic device comprising a housing, a display, and a cover substrate adjacent to the display, the cover substrate comprising the reinforced glass-ceramic article of any of Examples 18 to 48.

[0055] Embodiment 50 is a method of forming a glass ceramic, the method including the steps of heating a precursor glass composition to a nucleation temperature, the nucleation temperature being greater than or equal to 550° C. and less than or equal to 650° C.; holding the precursor glass composition at a temperature range greater than or equal to the nucleation temperature and less than or equal to 650° C. for a first period of time to form a nucleated precursor glass composition; heating the nucleated precursor glass composition to a growth temperature, the growth temperature being greater than or equal to 680° C. and less than or equal to 800° C.; and holding the nucleated precursor glass composition at a temperature range greater than or equal to the growth temperature and less than or equal to 800° C. for a second period of time to form a glass ceramic.

[0056] Example 51 includes the method of example 50, wherein the first period of time and the second period of time are each greater than or equal to 1 minute and less than or equal to 240 minutes.

[0057] Example 52 includes the method of example 50 or 51, wherein the step of holding the precursor glass composition at a temperature range greater than or equal to the nucleation temperature and less than or equal to 650° C. for a first period of time is an isothermal holding at the nucleation temperature for the first period of time.

[0058] Example 53 includes the method of any of Examples 50 to 52, wherein holding the nucleating precursor glass composition at a temperature range greater than or equal to the growth temperature and less than or equal to 800° C. for a second period of time includes isothermal holding at the growth temperature for the second period of time.

[0059] Example 54 includes the method of any of Examples 50 to 53, wherein the step of holding the precursor glass composition at a temperature range from the nucleation temperature or greater and 650°C or less for a first period of time includes heating the precursor glass composition from the nucleation temperature to a temperature of 650°C or less for the first period of time.

[0060] Example 55 includes the method of any of Examples 50 to 54, wherein the step of holding the nucleating precursor glass composition at a temperature range above the growth temperature and below 800° C. for a second period of time includes heating the nucleating precursor glass composition from the growth temperature to a temperature below 800° C. for the second period of time.

[0061] Example 56 includes the method of any of Examples 50 to 55, wherein the steps of heating the precursor glass composition to a nucleation temperature, the nucleation temperature being 550° C. or more and 650° C. or less, and heating the nucleated precursor glass composition to a growth temperature, the growth temperature being 680° C. or more and 800° C. or less, include heating the precursor glass composition and the nucleated precursor glass composition at a heating rate of 0.1° C. / min or more and 50° C. / min or less.

[0062] Example 57 includes the method of any of Examples 50 to 56, further including exposing the glass-ceramic to an ion exchange medium comprising a molten potassium salt, a molten sodium salt, and a molten lithium salt to form a strengthened glass-ceramic.

[0063] Example 58 includes the method of example 57, wherein the ion exchange medium includes greater than or equal to 50% and less than or equal to 70% by weight KNO3; greater than or equal to 30% and less than or equal to 50% by weight NaNO3; and greater than or equal to 0.05% and less than or equal to 0.15% by weight LiNO3.

[0064] Example 59 includes the method of example 57 or 58, wherein the ion exchange medium comprises greater than or equal to 0.08 wt. % and less than or equal to 0.12 wt. % LiNO.

[0065] Example 60 includes the method of any of Examples 57 to 59, wherein the ion exchange medium further comprises NaNO2 and silicic acid.

[0066] Example 61 includes the method of any of Examples 57 to 60, wherein the temperature of the ion exchange medium during exposure to the glass ceramic is greater than or equal to 450° C. and less than or equal to 550° C., and the glass ceramic is exposed to the ion exchange medium for a period of greater than or equal to 1 hour and less than or equal to 16 hours.

[0067]

[0043] Embodiment 62 is a glass article comprising at its center, by weight, 65.00% or more and 80.00% or less SiO2; greater than 4.00% and 12.00% or less Al2O3; 0.10% or more and 3.5% or less P2O5; 8.00% or more and 17.00% or less Li2O; 4.00% or more and 15.00% or less ZrO2; and 0.05% or more and 4.00% or less CaO.

[0068] Example 63 includes the glass article of Example 62, comprising at its center greater than or equal to 68.00% and less than or equal to 74.00% by weight SiO2.

[0069] Example 64 includes the glass article of example 62 or 63, comprising greater than 5.00% and less than or equal to 9.00% Al2O3 by weight at its center.

[0070] Example 65 includes the glass article of any of Examples 62 to 64, comprising at its center, greater than or equal to 1.00% and less than or equal to 3.00% by weight P2O5.

[0071] Example 66 includes the glass article of any of Examples 62 to 65, comprising, at a center thereof, greater than or equal to 9.00% and less than or equal to 14.00% LiO by weight.

[0072] Example 67 includes the glass article of any of Examples 62 to 66, comprising at its center, greater than or equal to 4.50% and less than or equal to 8.00% by weight ZrO2.

[0073] Example 68 includes the glass article of any of Examples 62 to 67, comprising at a center thereof, greater than or equal to 0.10% and less than or equal to 1.00% by weight CaO.

[0074] Example 69 includes the glass article of any of Examples 62 to 68, comprising at a center thereof, greater than or equal to 0.01% and less than or equal to 0.5% by weight SnO2.

[0075] Example 70 includes the glass article of any of Examples 62 to 69, wherein the glass-ceramic article has a haze of less than 0.15, as measured on a 0.6 mm thick glass-ceramic article using a BYK Hazegard I Pro Setup.

[0076] Example 71 includes the glass article of any of Examples 62 to 70, wherein the glass-ceramic article has a haze of less than 0.12, as measured on a 0.6 mm thick glass-ceramic article using a BYK Hazegard I Pro Setup.

[0077] Example 72 includes the glass article of any of Examples 62 to 71, wherein the glass-ceramic article has an average transmittance of 85% or greater.

[0078] Example 73 includes the glass article of any of Examples 62 to 72, wherein the glass article has a thickness of greater than or equal to 0.1 mm and less than or equal to 2.0 mm.

[0079] Example 74 includes the glass article of any of Examples 62 to 73, wherein the glass article has a thickness of greater than or equal to 0.1 mm and less than or equal to 1.0 mm.

[0080] Example 75 includes an electronic device comprising a housing, a display, and a cover substrate adjacent to the display, the cover substrate comprising the glass article of any of examples 62 to 74. [Brief description of the drawings]

[0081] [Figure 1] 1 is a flow chart illustrating a method according to an embodiment disclosed and described herein. [Diagram 2] 1 is a schematic diagram of a cross section of a glass-ceramic article chemically strengthened by ion exchange processing; [Diagram 3] Fluorescence speckle microscopy (FSM) images of glass-ceramics chemically strengthened by ion-exchange treatment with varying amounts of lithium in the ion-exchange medium [Figure 4A] Diagram showing the corrosion of glass-ceramics chemically strengthened by ion-exchange treatment with varying amounts of lithium in the ion-exchange medium. [Figure 4B] Diagram showing the corrosion of glass-ceramics chemically strengthened by ion-exchange treatment with varying amounts of lithium in the ion-exchange medium. [Figure 4C] Diagram showing the corrosion of glass-ceramics chemically strengthened by ion-exchange treatment with varying amounts of lithium in the ion-exchange medium. [Figure 5A] FIG. 1 shows the corrosion of comparative glass-ceramics chemically strengthened by ion-exchange treatment with varying amounts of lithium in the ion-exchange medium. [Figure 5B] FIG. 1 shows the corrosion of comparative glass-ceramics chemically strengthened by ion-exchange treatment with varying amounts of lithium in the ion-exchange medium. [Figure 6] FIG. 1 shows an X-ray diffraction diagram of a glass-ceramic assembly produced according to embodiments disclosed and described herein. [Figure 7A] Graph showing stress profile of a 0.6 mm thick glass-ceramic article manufactured according to embodiments disclosed and described herein. [Figure 7B] Graph showing stress profile of a 0.5 mm thick glass-ceramic article manufactured according to embodiments disclosed and described herein. [Figure 7C] Graph showing central tension as a function of duration of ion exchange process [Figure 8] Graph showing fracture stress test results for glass ceramics with various thicknesses [Figure 9] Graph showing fracture stress test results for glass-ceramics chemically strengthened at various temperatures [Figure 10] Graph showing stress profile of glass ceramic [Figure 11] Graph showing drop test of glass ceramics with various thicknesses [Figure 12A] Scratch test results [Figure 12B] Scratch test results [Figure 13A] FIG. 1 is a schematic diagram of an electronic device containing a glass or glass-ceramic article according to embodiments disclosed and described herein. [Figure 13B] [Figure 14] Drop test rig schematic [Figure 15] Drop test rig schematic [Figure 16] Drop test rig schematic DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0082] Reference will now be made in detail to embodiments of ceramized glass articles having advantageous properties and methods of ceramizing glass articles, the embodiments of which are illustrated in the accompanying drawings. Various embodiments will be described herein with particular reference to the accompanying drawings.

[0083] Definitions and Measurement Techniques As used herein, the term "glass-ceramic" refers to a solid prepared by controlled crystallization of a precursor glass and having one or more crystalline phases and a residual glassy phase.

[0084] As used herein, "depth of compression" or "DOC" refers to the depth of the compressive stress (CS) layer, the depth at which the stress in a glass-ceramic article changes from compressive to tensile, and has a stress value of zero. According to common practice in the art, compressive stress is expressed as a negative (<0) stress and tensile stress is expressed as a positive (>0) stress. However, unless otherwise noted, throughout this specification, CS is expressed as a positive or absolute value. That is, as described herein, CS=|CS|.

[0085] The CS, DOC, and maximum central tension (CT) values ​​are measured using a hybrid method combining measurements made using evanescent prism coupling spectroscopy (EPCS) and light scattering polarimetry (LSP), as disclosed in U.S. Patent Application Publication No. 2020 / 0300615, the entirety of which is incorporated herein by reference.

[0086] Fracture toughness (K 1C ) represents the ability of a glass composition to withstand fracture. Fracture toughness can be measured, for example, by measuring the fracture toughness of a glass article prior to ion exchange (IOX) treatment with K 1CThe fracture toughness is measured on non-chemically strengthened glass articles, such as by measuring K values, which characterize the glass substrate before IOX. The fracture toughness test methods described herein are not suitable for glass exposed to IOX processing. However, fracture toughness measurements performed as described herein on the same glass (e.g., glass substrate, etc.) before IOX processing correlate with the fracture toughness after IOX processing and are therefore used accordingly. 1C The chevron-notched short bar (CNSB) method used to measure the value was calculated by using Equation 5 of Bubsey, RT et al., “Closed-Form Expressions for Crack-Mouth Displacement and Stress Intensity Factors for Chevron-Notched Short Bar and Short Rod Specimens Based on Experimental Compliance Measurements,” NASA Technical Memorandum 83796, pp.1-30 (October 1992) to calculate Y* m Except for calculating the fracture toughness of the specimen, the fracture toughness is disclosed in Reddy, KPR et al, “Fracture Toughness Measurement of Glass and Ceramic Materials Using Chevron-Notched Specimens,” J. Am. Ceram. Soc., 71 [6], C-310-C-313 (1988). 1CThe double-torsion method and fixture used to measure K values ​​are described in Shyam, A. and Lara-Curzio, E., “The double-torsion testing technique for determination of fracture toughness and slow crack growth of materials: A review,” J. Mater. Sci., 41, pp. 4093-4104, (2006). The double-torsion method generally produces slightly higher K values ​​than the chevron-notched short bar method. 1C Unless otherwise stated, all fracture toughness values ​​were measured using the Chevron Notched Short Bar (CNSB) technique.

[0087] The Young's modulus values ​​set forth in this disclosure refer to values ​​measured by resonant ultrasonic spectroscopy of the general type specified in ASTM standard E2001-13.

[0088] The haze of a glass-ceramic article is measured, unless otherwise specified, on a glass article having a thickness of 0.6 mm using a haze meter such as, for example, a BYK Gardner Haze-Gard I according to ASTM Standard D1003 or ASTM Standard D1044.

[0089] Optical transmittance is measured using a Perkin Elmer Lambda 950 spectrophotometer in the range of 250-1000 nm on optically polished samples with plane-parallel faces with a data interval of 2 nm. The transmittance is measured on the glass-ceramic article itself, without any coatings or other applications.

[0090] X-ray diffraction (XRD) is measured on powder samples using a Bruker D4 Endeavor equipped with Cu radiation and a LynxEye detector. Phase assemblages are calculated using the Rietveld method and Bruker's Topas software package.

[0091] Scratch resistance was measured using an Anton Paar MicroCombi with a diamond tip with a 90 degree angle, tests were performed using a 10 μm radius, scratching at 5 mm / min and a loading-unloading rate of 0.14 N / s. A 10 mm scratch was performed.

[0092] The density is measured according to the measurement in accordance with ASTM standard C693.

[0093] Hardness is measured using a MITUTOYO HM114 hardness tester equipped with a Vickers indenter with an indentation load of 200 grams (dwell time 15 seconds). Measurements of the indentation diagonal are made using a calibrated optical microscope. Values ​​are the average of measurements from five indentations per sample. Tests are performed on optically polished samples with plane-parallel faces.

[0094] Unless otherwise expressly stated, it is in no way intended that any method described herein be construed as requiring that its steps be performed in a particular order, or that an apparatus requires a particular orientation. Thus, where a method claim does not actually recite an order in which its steps are to be followed, or an apparatus claim does not actually recite an order or orientation for individual components, or where the claims or specification otherwise expressly state that the steps are to be limited to a particular order, or where no particular order or orientation for the apparatus components is recited, no order or direction is intended to be inferred in any sense. This applies to any implicit basis for interpretation, such as: logical considerations regarding the arrangement of steps, operational flow, order of components, or orientation of components; plain meaning derived from grammatical organization or punctuation; and the number or type of embodiments described in the specification.

[0095] As used herein, the singular forms "a," "an," and "the" include plural referents unless the context clearly dictates otherwise. Thus, for example, reference to "a" element includes aspects having two or more such elements unless the context clearly dictates otherwise.

[0096] Directional terms used herein (e.g., up, down, right, left, front, back, upper, bottom, vertical, horizontal) are used with reference to the depicted figures only and are not intended to imply absolute directions, unless expressly stated otherwise.

[0097] As used herein, the terms "camber" and "flatness", and variations thereof, are used interchangeably and have the same meaning.

[0098] Ranges used herein include all ranges and subranges, and all values ​​therebetween, unless expressly stated otherwise.

[0099] Overview of Glass-Ceramic Articles Reference will now be made in detail to the preferred embodiments of the present invention, examples of which are illustrated in the accompanying drawings. Wherever possible, the same reference numbers will be used throughout the drawings to refer to the same or like parts.

[0100] Glass-ceramic articles have attributes that can be customized for use as cover substrates and / or housings for portable electronic devices. For example, without being bound by theory, glass-ceramic articles with high fracture toughness and / or Young's modulus can provide resistance to crack penetration and drop performance. Such glass-ceramic articles can be chemically strengthened, for example, by ion exchange, to further improve resistance to crack penetration and drop performance. High fracture toughness and / or Young's modulus can also increase the amount of stored tensile energy and maximum central tension that can be imparted to the glass-ceramic article by chemical strengthening, while maintaining the desired fragmentation of the glass-ceramic article upon fracture. As another example, the optical properties of the glass-ceramic article, such as transparency and haze, can be tailored by adjusting the heating / ceramming schedule used to convert the glass article into a glass-ceramic article, and by designing or controlling the properties of the glass-ceramic article by chemical strengthening, for example, ion exchange.

[0101] Composition of the Glass or Glass-Ceramic Precursor As glasses and glass ceramics need to be made thinner to meet the needs of increasingly smaller and thinner electronic devices, it is desirable to increase the strength of thin glass and glass ceramic articles by increasing the level of stress (both compressive and tensile) that can be imparted to the glass or glass ceramic, such as by chemical strengthening (e.g., ion exchange). However, known glass and glass ceramic compositions and methods for making such glass and glass ceramic articles indicate that the stress that can be imparted to the glass or glass ceramic article has reached a plateau. Thus, the problem addressed by the glass or glass ceramic articles disclosed and described herein is that the stress (and therefore the strength) that can be imparted to the glass or glass ceramic article has reached a plateau.

[0102] One compositional aspect that contributes to the improved stress levels of glass or glass-ceramic articles according to the embodiments disclosed and described herein is the increased amount of Li2O in the glass precursor composition. Lithium is the smallest of the alkali metal ions, and high compressive stress and central tension values ​​can be achieved when lithium is replaced by sodium or potassium ions in the glass matrix by ion-exchange chemistry. However, too much lithium in the glass precursor can make the glass composition less soluble, which can make it difficult to achieve thin glass-ceramic articles, which are desirable for portable electronic devices, such as mobile phones and tablets. Thus, simply increasing the amount of lithium in the glass precursor material does not improve the compressive stress and central tension values. Doing so results in the glass composition being unable to be easily and economically formed into thin sheets.

[0103] It has been found that the inclusion of a relatively large amount of zirconia (ZrO2) in the glass precursor composition in combination with a slightly larger amount of lithium in the glass precursor composition can provide high compressive stress and central tension in the glass ceramic without excessively affecting the meltability of the glass precursor. Without being bound to a particular theory, it is believed that the zirconia helps to trap lithium within the residual amorphous glass phase of the glass ceramic during the formation of the glass ceramic by heat treatment (described in more detail below). Thus, more lithium is present in the residual amorphous glass phase and is readily available for ion exchange with sodium and potassium during the chemical strengthening process. Thus, while zirconia is traditionally included in glass and glass ceramic compositions to prevent devitrification of the glass before it is cerammed, the relatively large amount of zirconia included in the embodiments disclosed and described herein has been found to improve the ion exchange profile of the glass ceramic beyond the previously believed improvement in devitrification of the precursor glass.

[0104] The precursor glass compositions according to the embodiments disclosed and described herein also contain a relatively large amount of calcium oxide (CaO). Without being bound to a particular theory, it is believed that the additional calcium oxide increases the density of the glass-ceramic and thus retards the diffusion of ions into the glass-ceramic during chemical strengthening. This retardation of diffusion slows down the ion exchange process but results in a glass-ceramic with higher compressive stress and central tension than a less dense glass. Zirconia is also believed to help increase the density of the glass-ceramic.

[0105] As previously discussed, a properly balanced combination of increasing amounts of LiO, ZrO, and CaO in the precursor glass composition produces superior ion exchange profiles (e.g., compressive stress and central tension) than conventional precursor glass compositions that do not have balanced increases in these components.

[0106] In various embodiments, the glass compositions are selected such that the resulting glass-ceramic article has a crystalline phase that comprises primarily a petalite crystalline phase and a lithium silicate crystalline phase, where the petalite crystalline phase and the lithium silicate crystalline phase have a higher weight percentage than other crystalline phases present in the glass-ceramic article.

[0107] By way of example and not limitation, in various embodiments, the glass sheet may be formed from a glass composition including 65% to 80% by weight SiO2, 4% to 12% by weight Al2O3, 0.10% to 3.5% by weight P2O5, 8% to 17% by weight Li2O, 4% to 15% by weight ZrO2, and 0.05% to 4% by weight CaO. In embodiments, the glass composition may further include 0% to 2% by weight Na2O, 0% to 2% by weight K2O, 0% to 1.5% by weight Fe2O3, and combinations thereof.

[0108] SiO2, an oxide involved in glass formation, can function to stabilize the network structure of glasses and glass ceramics. In various glass compositions, the concentration of SiO2 must be high enough to form a petalite crystal phase when the glass sheet is heat treated to convert it into a glass ceramic. The melting point of pure SiO2 or high SiO2 glass is undesirably high, so the amount of SiO2 may be limited to control the melting point of the glass. In an embodiment, the glass or glass ceramic composition comprises 65% to 80% by weight SiO2, 70% to 80% by weight SiO2, 75% to 80% by weight SiO2, 65% to 75% by weight SiO2, 70% to 75% by weight SiO2, or 65% to 70% by weight SiO2. It is to be understood that the above ranges include all subranges within the ranges explicitly disclosed.

[0109] Al2O3 can also provide network stabilization, leading to improved mechanical properties and chemical durability. However, too much Al2O3 may reduce the proportion of lithium silicate crystals, perhaps to the point of not being able to form an interlocking structure. The amount of Al2O3 can be adjusted to control the viscosity. Furthermore, too much Al2O3 generally also increases the viscosity of the melt. In an embodiment, the glass or glass ceramic composition comprises 4% to 12% by weight Al2O3, 6% to 12% by weight Al2O3, 8% to 12% by weight Al2O3, 10% to 12% by weight Al2O3, 4% to 10% by weight Al2O3, 6% to 10% by weight Al2O3, 8% to 10% by weight Al2O3, 4% to 8% by weight Al2O3, 6% to 8% by weight Al2O3, or 4% to 6% by weight Al2O3. It is to be understood that the above ranges include all subranges within the ranges expressly disclosed.

[0110] In the glasses and glass-ceramics herein, Li2O aids in the formation of both petalite and lithium silicate crystalline phases. Indeed, to obtain petalite and lithium silicate as the predominant crystalline phases, it is desirable to have at least about 8 wt. % Li2O in the composition. In addition, it has been found that as Li2O approaches about 17 wt. %, the composition becomes very fluid. Thus, in embodiments, the glass or glass-ceramic composition may include 8% to 17% by weight Li2O, 10% to 17% by weight Li2O, 12% to 17% by weight Li2O, 14% to 17% by weight Li2O, 16% to 17% by weight Li2O, 8% to 16% by weight Li2O, 10% to 16% by weight Li2O, 12% to 16% by weight Li2O, 14% to 16% by weight Li2O, 8% to 14% by weight Li2O, 10% to 14% by weight Li2O, 12% to 14% by weight Li2O, 8% to 12% by weight Li2O, 10% to 12% by weight Li2O, or 8% to 10% by weight Li2O. It is to be understood that the above ranges include all subranges within the ranges expressly disclosed.

[0111] As mentioned above, Li2O is generally useful in the formation of various glass ceramics, while other alkali oxides tend to reduce the formation of glass ceramics and form aluminosilicate residual glass in the glass ceramic. It has been found that about 5% by weight of Na2O or K2O, or a combination thereof, results in an undesirable amount of residual glass, which may result in deformation during crystallization and undesirable microstructure in terms of mechanical properties. The composition of the residual glass can be adjusted to control viscosity during crystallization, minimize deformation or undesirable thermal expansion, or control microstructural properties. Thus, generally, glass sheets can be made from glass compositions that have a low content of non-lithium alkali metal oxides. In embodiments, the glass or glass ceramic composition can include about 0% to about 5% by weight of R2O, where R is one or more of the alkali cations Na and K. In embodiments, the glass or glass ceramic composition can include about 1% to about 3% by weight of R2O, where R is one or more of the alkali cations Na and K. In embodiments, it is understood that the glass and glass ceramic composition is free of R2O.

[0112] In embodiments, the glass and glass ceramic compositions include greater than 0% and less than or equal to 2% Na2O, greater than 1% and less than or equal to 2% Na2O, and greater than 0% and less than or equal to 1% Na2O, by weight. In embodiments, the glass and glass ceramic compositions include greater than 0% and less than or equal to 2% K2O, greater than 1% and less than or equal to 2% K2O, and greater than 0% and less than or equal to 1% K2O, by weight. It is understood that the above ranges include all subranges within the ranges explicitly disclosed.

[0113] Glasses and glass ceramics include P2O5. P2O5 functions as a nucleating agent, producing bulk nucleation. If the concentration of P2O5 is too low, the precursor glass will crystallize, but only at high temperatures (due to low viscosity) and will crystallize from the surface inwards, resulting in a weak, easily deformed object. However, if the concentration of P2O5 is too high, it may be difficult to control devitrification upon cooling during formation of the glass sheet. Embodiments of glass and glass ceramic compositions include at least 0.1% and at most 3.5% P2O5, at least 0.5% and at most 3.5% P2O5, at least 1.0% and at most 3.5% P2O5, at least 1.5% and at most 3.5% P2O5, at least 2.0% and at most 3.5% P2O5, at least 2.5% and at most 3.5% P2O5, at least 3.0 ... and 3.5% by mass or less P2O5, 0.1% by mass or more and 3.0% by mass or less P2O5, 0.5% by mass or more and 3.0% by mass or less P2O5, 1.0% by mass or more and 3.0% by mass or less P2O5, 1.5% by mass or more and 3.0% by mass or less P2O5, 2.0% by mass or more and 3.0% by mass or less P2O5, 2.5% by mass or more and 3.0% by mass or less P2O5, 0.1% by mass or more and 2.5% by mass or less P2O5 % or less of P2O5, 0.5% or more by mass and 2.5% or less of P2O5, 1.0% or more by mass and 2.5% or less of P2O5, 1.5% or more by mass and 2.5% or less of P2O5, 2.0% or more by mass and 2.5% or less of P2O5, 0.1% or more by mass and 2.0% or less of P2O5, 0.5% or more by mass and 2.0% or less of P2O5, 1.0% or more by mass and 2.0% or less of P2O5 5, 1.5% to 2.0% by weight P2O5, 0.1% to 1.5% by weight P2O5, 0.5% to 1.5% by weight P2O5, 1.0% to 1.5% by weight P2O5, 0.1% to 1.0% by weight P2O5, 0.5% to 1.0% by weight P2O5, or 0.1% to 0.5% by weight P2O5. The above ranges are to be understood to include all subranges within the explicitly disclosed ranges.

[0114] In various glass and glass-ceramic compositions, ZrO2 has been found to improve the stability of Li2O-Al2O3-SiO2-P2O5 glasses by significantly reducing the devitrification of the glass during forming and lowering the liquidus temperature. At concentrations above 8 wt.%, ZrSiO4 can form a primary liquid phase at high temperatures, which significantly reduces the liquidus viscosity. If the glass contains more than 2 wt.% ZrO2, a transparent glass can be formed. The addition of ZrO2 can help reduce the petalite grain size, which aids in the formation of transparent glass-ceramics. In an embodiment, the glass or glass ceramic composition comprises at least 4% and at most 15% by weight ZrO2, at least 6% and at most 15% by weight ZrO2, at least 8% and at most 15% by weight ZrO2, at least 10% and at most 15% by weight ZrO2, at least 12% and at most 15% by weight ZrO2, at least 14% and at most 15% by weight ZrO2, at least 4% and at most 14% by weight ZrO2, at least 6% and at most 14% by weight ZrO2, at least 8% and at most 14% by weight ZrO2, at least 10% and at most 14% by weight ZrO2, 2, 12% to 14% by weight ZrO2, 4% to 12% by weight ZrO2, 6% to 12% by weight ZrO2, 8% to 12% by weight ZrO2, 10% to 12% by weight ZrO2, 4% to 10% by weight ZrO2, 6% to 10% by weight ZrO2, 8% to 10% by weight ZrO2, 4% to 8% by weight ZrO2, 6% to 8% by weight ZrO2, or 4% to 6% by weight ZrO2. The above ranges are understood to include all subranges within the ranges explicitly disclosed.

[0115] CaO may be present in the petalite crystals as a partial solid solution. In an embodiment, the glass or glass-ceramic composition may have at least 0.05% and at most 4.0%, at least 0.1% and at most 4.0%, at least 0.5% and at most 4.0%, at least 1.0% and at most 4.0%, at least 1.5% and at most 4.0%, at least 2.0% and at most 4.0%, at least 2.5% and at most 4.0%, at least 3.0% and at most 4.0%, at least 3.5% and at most 4.0%, at least 0.05% and at most 3.5%, at least 0.1% by weight and 3.5 mass% or less, 0.5 mass% or more and 3.5 mass% or less, 1.0 mass% or more and 3.5 mass% or less, 1.5 mass% or more and 3.5 mass% or less, 2.0 mass% or more and 3.5 mass% or less, 2.5 mass% or more and 3.5 mass% or less, 3.0 mass% or more and 3.5 mass% or less, 0.05 mass% or more and 3.0 mass% or less, 0.1 mass% or more and 3.0 mass% or less, 0.5 mass% or more and 3.0 mass% or less, 1.0 mass% or more and 3.0 mass% or less, 1.5 mass% or more and 3.0 mass% or less, 2.0 % by mass or more and 3.0% by mass or less, 2.5% by mass or more and 3.0% by mass or less, 0.05% by mass or more and 2.5% by mass or less, 0.1% by mass or more and 2.5% by mass or less, 0.5% by mass or more and 2.5% by mass or less, 1.0% by mass or more and 2.5% by mass or less, 1.5% by mass or more and 2.5% by mass or less, 2.0% by mass or more and 2.5% by mass or less, 0.05% by mass or more and 2.0% by mass or less, 0.1% by mass or more and 2.0% by mass or less, 0.5% by mass or more and 2.0% by mass or less, 1.0% by mass or more and 2.0% by mass % to 1.5%, 0.05% to 1.5%, 0.1% to 1.5%, 0.5% to 1.5%, 1.0% to 1.5%, 0.05% to 1.0%, 0.1% to 1.0%, 0.5% to 1.0%, 0.05% to 0.5%, 0.1% to 0.5%, or 0.05% to 0.1% CaO. The above ranges are to be understood to include all subranges within explicitly disclosed ranges.

[0116] Fe2O3 can reduce the melting point of glass and glass ceramic compositions. However, excessive addition of Fe2O3 can change the color of the glass and glass ceramic compositions. In an embodiment, the glass and glass ceramic compositions do not include Fe2O3. In an embodiment, the glass and glass ceramic include greater than 0.0% and less than or equal to 1.5% Fe2O3, greater than or equal to 0.5% and less than or equal to 1.5% Fe2O3, greater than or equal to 1.0% and less than or equal to 1.5% Fe2O3, greater than or equal to 0.0% and less than or equal to 1.0% Fe2O3, greater than or equal to 0.5% and less than or equal to 1.0% Fe2O3, or greater than or equal to 0.0% and less than or equal to 0.5% Fe2O3 by weight. It is to be understood that the above ranges include all subranges within the ranges explicitly disclosed.

[0117] In various embodiments, the glass or glass ceramic composition may further include one or more components, such as, by way of example and not limitation, TiO2, CeO2, and SnO2. Additionally or alternatively, an antimicrobial component may be added to the glass or glass ceramic composition. Antimicrobial components that may be added to the glass or glass ceramic may include, but are not limited to, Ag, AgO, Cu, CuO, Cu2O, and the like. In embodiments, the glass or glass ceramic composition may further include a chemical fining agent. Such fining agents include, but are not limited to, SnO2, As2O3, Sb2O3, F, Cl, and Br. In embodiments, the glass or glass ceramic includes 0.01% or more and 0.5% or less by weight SnO2. For additional details regarding glass and / or glass-ceramic compositions suitable for use in various embodiments, see, for example, U.S. Patent Application Publication No. 2016 / 0102010, filed October 8, 2015, entitled "High Strength Glass-Ceramics Having Petalite and Lithium Silicate Structures," which is hereby incorporated by reference in its entirety.

[0118] Heating Conditions for Forming Glass-Ceramic Articles A process for making a glass-ceramic according to embodiments involves heat treating a precursor glass at two preselected temperatures for one or more preselected times to induce homogenization of the glass and crystallization (i.e., nucleation and growth) of one or more crystalline phases (e.g., having one or more compositions, amounts, morphologies, sizes, or size distributions, etc.). These two temperatures are referred to as the nucleation temperature and the growth temperature, respectively.

[0119] Referring now to FIG. 1, an embodiment of a method for making a glass ceramic 100 is generally described. Initially, a precursor glass composition at 101 is heated to a nucleation temperature of 550° C. or more and 650° C. or less. The precursor glass at 102 is held at a temperature range of 550° C. or more and 650° C. or less for a first period of time. The nucleation precursor glass composition at 103 is heated to a growth temperature of 680° C. or more and 800° C. or less. The nucleation precursor glass composition at 104 is held at a temperature range of 800° C. or more and 680° C. or less for a second period of time to form a glass ceramic. In an embodiment, the glass ceramic at 105 is exposed to an ion exchange medium comprising molten potassium salts, molten sodium salts, and molten lithium salts to form a strengthened glass ceramic. Each of these steps is described in more detail below.

[0120] In an embodiment, the nucleation stage occurs when the precursor glass is held at a predetermined nucleation temperature for a predetermined period of time. In an embodiment, the nucleation temperature is 550° C. or more and 650° C. or less, 560° C. or more and 650° C. or less, 570° C. or more and 650° C. or less, 580° C. or more and 650° C. or less, 590° C. or more and 650° C. or less, 600° C. or more and 650° C. or less, 610° C. or more and 650° C. or less, 620° C. or more and 650° C. or more, 630° C. or more and 650° C. or more, 640° C. or more and 650° C. or less, 550° C. or more and 640° C. or less, 560° C. or more and 640° C. or less, 570° C. or more and 640° C. or less, 580° C. or more and 650° C. or less, 590° C. or more and 650° C. or less, 600° C. or more and 650° C. or less, 610° C. or more and 650° C. or less, 620° C. or more and 650° C. or more and 630° C. or more and 650° C. or less, 640° C. or more and 650° C. or less, 550° C. or more and 640° C. or less, 560° C. or more and 640° C. or less, 570° C. or more and 640° C. or less, 580° C. or 0℃ or higher and 640℃ or lower, 590℃ or higher and 640℃ or lower, 600℃ or higher and 640℃ or lower, 610℃ or higher and 640℃ or lower, 620℃ or higher and 640℃ or lower, 630℃ or higher and 640℃ or lower, 550℃ or higher and 630℃ or lower, 560℃ or higher and 630℃ or lower, 570℃ or higher and 630℃ or lower, 580℃ or higher and 630℃ or lower, 590℃ or higher and 630℃ or lower, 600℃ or higher and 630℃ or lower, 610℃ or higher and 630℃ or lower, 620℃ or higher and 630℃ or lower, 550 ℃ or higher and 620℃ or lower, 560℃ or higher and 620℃ or lower, 570℃ or higher and 620℃ or lower, 580℃ or higher and 620℃ or lower, 590℃ or higher and 620℃ or lower, 600℃ or higher and 620℃ or lower, 610℃ or higher and 620℃ or lower, 550℃ or higher and 610℃ or lower, 560℃ or higher and 610℃ or lower, 570℃ or higher and 610℃ or lower, 580℃ or higher and 610℃ or lower, 590℃ or higher and 610℃ or lower, 600℃ or higher and 610℃ or lower, 550℃ or higher and 600℃ or lower, 560℃ and 600° C., 570° C. and 600° C., 580° C. and 600° C., 590° C. and 600° C., 550° C. and 590° C., 560° C. and 590° C., 570° C. and 590° C., 580° C. and 590° C., 550° C. and 580° C., 560° C. and 580° C., 570° C. and 580° C., 550° C. and 570° C., 560° C. and 570° C., or 550° C. and 560° C. It is understood that the above ranges include all subranges within the explicitly disclosed ranges.

[0121] In an embodiment, the glass has a melting point of 1 min to 240 min, 30 min to 240 min, 60 min to 240 min, 90 min to 240 min, 120 min to 240 min, 150 min to 240 min, 180 min to 240 min, 210 min to 240 min, 1 min to 210 min, 30 min to 210 min, 60 min to 210 min, 90 min to 210 min, 120 min to 210 min, 150 min to 210 min, 180 min to 210 min, 1 min to 180 min, 30 min to 180 min, 60 min to 180 min 1 min to 150 min, 30 min to 150 min, 60 min to 150 min, 90 min to 150 min, 120 min to 150 min, 1 min to 120 min, 30 min to 120 min, 60 min to 120 min, 90 min to 120 min, 1 min to 90 min, 30 min to 120 min, 60 min to 120 min, 90 min to 120 min, 1 min to 90 min, 30 min to 90 min, 60 min to 90 min, 1 min to 60 min, 30 min to 60 min, or 1 min to 30 min. The above ranges are understood to include all subranges within the ranges explicitly disclosed. The precursor glass after the nucleation step is called a nucleated precursor glass.

[0122] The growth stage occurs when the nucleated precursor glass is held at a predetermined growth temperature for a predetermined period of time. In an embodiment, the growth temperature is higher than the nucleation temperature. In an embodiment, the growth temperature is 680°C or more and 800°C or less, 690°C or more and 800°C or less, 700°C or more and 800°C or less, 710°C or more and 800°C or less, 720°C or more and 800°C or less, 730°C or more and 800°C or less, 740°C or more and 800°C or less, 750°C or more and 800°C or less, 760°C or more and 800°C or less, 770°C or more and 800°C or less, 780°C or more and 800°C or less, to 790°C or less, 680°C or more and 790°C or less, 690°C or more and 790°C or less, 700°C or more and 790°C or less, 710°C or more and 790°C or less, 720°C or more and 790°C or less, 730°C or more and 790°C or less, 740°C or more and 790°C or less, 750°C or more and 790°C or less, 760°C or more and 790°C or less, 770°C or more and 790°C or less, 780°C or more and 790°C or less, 680°C or more and 780°C or less, 690°C or more and 780°C or less, 700°C or more and 780°C or less, 710°C or more and 780°C or less, 720°C or more and 780°C or less, 730°C or more and 780°C or less, 740°C or more and 780°C or less, 750℃ or higher and 780℃ or lower, 760℃ or higher and 780℃ or lower, 770℃ or higher and 780℃ or lower, 680℃ or higher and 770℃ or lower, 690℃ or higher and 770℃ or lower, 700℃ or higher and 770℃ or lower, 710℃ or higher and 770℃ or lower, 720℃ or higher and 770℃ or lower, 730℃ or higher and 770℃ or lower, 740℃ or higher and 770℃ or lower, 750℃ or higher and 770℃ or lower, 760℃ or higher and 770℃ or lower, 680℃ or higher and 760℃ or lower, 690℃ or higher and 760℃ or lower, 700℃ or higher and 760℃ or lower, 710℃ or higher or 760°C or less, 720°C or more and 760°C or less, 730°C or more and 760°C or less, 740°C or more and 760°C or less, 750°C or more and 760°C or less, 680°C or more and 750°C or less, 690°C or more and 750°C or less, 700°C or more and 750°C or less, 710°C or more and 750°C or less, 720°C or more and 750°C or less, 730°C or more and 750°C or less, 740°C or more and 750°C or less, 680°C or more and 740°C or less, 690°C or more and 740°C or less, 700°C or more and 740°C or less, 710°C or more and 740°C or less,720°C or more and 740°C or less, 730°C or more and 740°C or more, 680°C or more and 730°C or less, 690°C or more and 730°C or less, 700°C or more and 730°C or less, 710°C or more and 730°C or more, 720°C or more and 730°C or more, 680°C or more and 720°C or less, 690°C or more and 720°C or less, 700°C or more and 720°C or less, 710°C or more and 720°C or more, 680°C or more and 710°C or less, 690°C or more and 710°C or less, 700°C or more and 710°C or less, 680°C or more and 700°C or less, 690°C or more and 700°C or less, or 680°C or more and 690°C or less. It is to be understood that the above ranges include all subranges within the ranges explicitly disclosed.

[0123] In an embodiment, the glass has a melting point of 1 min to 240 min, 30 min to 240 min, 60 min to 240 min, 90 min to 240 min, 120 min to 240 min, 150 min to 240 min, 180 min to 240 min, 210 min to 240 min, 1 min to 210 min, 30 min to 210 min, 60 min to 210 min, 90 min to 210 min, 120 min to 210 min, 150 min to 210 min, 180 min to 210 min, 1 min to 180 min, 30 min to 180 min, 60 min to 180 min The growth temperature is maintained for a period of time of 90 to 180 minutes, 120 to 180 minutes, 150 to 180 minutes, 1 to 150 minutes, 30 to 150 minutes, 60 to 150 minutes, 90 to 150 minutes, 120 to 150 minutes, 1 to 120 minutes, 30 to 120 minutes, 60 to 120 minutes, 90 to 120 minutes, 1 to 90 minutes, 30 to 90 minutes, 60 to 90 minutes, 1 to 60 minutes, 30 to 60 minutes, or 1 to 30 minutes. The above ranges are understood to include all subranges within the ranges explicitly disclosed. During the growth stage, the nucleation precursor glass is converted into a glass-ceramic material.

[0124] The precursor glass articles disclosed and described herein, held at the nucleation and growth temperatures for the periods of time disclosed and described herein, exhibit an amorphous glass phase, petalite (LiAlSiO 10 ), and lithium disilicate (Li2Si2O5) rich phase assemblage. The glass ceramic may contain other crystalline phases (such as, but not limited to, lithium metasilicate (Li2SiO3), virgilite (Li x Al x S 3-x The phase assemblage comprises less than 5 wt. %, such as less than 3 wt. %, collectively of SiO, quartz (SiO, zirconia (ZrO, baddeleyite (ZrO), spodumene (LiAlSiO, and lithium phosphate (LiPO). This phase assemblage provides a glass-ceramic having low haze (high transparency) and improved mechanical properties compared to previously available glass-ceramic articles.

[0125] The nucleation and growth temperatures and durations disclosed and described herein are believed to be heat treatments that result in primarily the desired phase assemblages in the glass-ceramic material. Accordingly, additional heat treatments can be included before the nucleation step, between the nucleation and growth steps, and after the growth step without causing significant deviations in the phase assemblages of the glass-ceramic material. These additional heat treatments include isothermal holds, heating with a specific heating schedule that includes multiple different heating rates, and combinations thereof.

[0126] Thus, in embodiments, there may be one or more additional temperature holds between the nucleation temperature and the growth temperature. Thus, in embodiments, after the precursor glass is maintained at the nucleation temperature, the article can be heated to one or more intermediate temperatures (where the intermediate temperatures range between the nucleation temperature and the growth temperature), held at the one or more intermediate temperatures for a period of time (e.g., between 1 minute and 240 minutes, and all ranges and subranges therebetween), and then heated to the growth temperature.

[0127] In an embodiment, the nucleation stage comprises an isothermal hold at a single nucleation temperature for a period of time. However, in other embodiments, the nucleation stage comprises heating the precursor glass at one or more heating rates over the nucleation temperature range described herein (i.e., from 550° C. or more to 650° C. or less). Similarly, in an embodiment, the growth stage comprises an isothermal hold at a single growth temperature for a period of time. However, in other embodiments, the growth stage comprises heating or cooling the nucleated precursor glass at one or more heating rates within the growth temperature range described herein (i.e., from 680° C. or more to 800° C. or less).

[0128] According to embodiments, the heating rates used during the nucleation step, between the nucleation step and the growth step, within the growth step, and after the growth step to heat from room temperature to the nucleation temperature are 0.1° C. / min to 50° C. / min, 5° C. / min to 50° C. / min, 10° C. / min to 50° C. / min, 15° C. / min to 50° C. / min, 20° C. / min to 50° C. / min, 25° C. / min to 50° C. / min, 30° C. / min to 50° C. / min, 35° C. / min to 50° C. / min, 40° C. / min to 50° C. / min, 45° C. / min to 50° C. / min, 0.1° C. / min or less. 0.1℃ / min to 40℃ / min, 5℃ / min to 45℃ / min, 10℃ / min to 45℃ / min, 15℃ / min to 45℃ / min, 20℃ / min to 45℃ / min, 25℃ / min to 45℃ / min, 30℃ / min to 45℃ / min, 35℃ / min to 45℃ / min, 40℃ / min to 45℃ / min, 0.1℃ / min to 40℃ / min, 5℃ / min to 40℃ / min, 10℃ / min to 40℃ / min, 15℃ / min to 40℃ / min, 20℃ / min to 40℃ / min, 25℃ / min to 40℃ / min, 30°C / min or more and 40°C / min or less, 35°C / min or more and 40°C / min or less, 0.1°C / min or more and 35°C / min or less, 5°C / min or more and 35°C / min or less, 10°C / min or more and 35°C / min or less, 15°C / min or more and 35°C / min or less, 20°C / min or more and 35°C / min or less, 25°C / min or more and 35°C / min or less, 30°C / min or more and 35°C / min or less, 0.1°C / min or more and 30°C / min or less, 5°C / min or more and 30°C / min or less, 10°C / min or more and 30°C / min or less, 15°C / min or more and 30°C / min or less, 20°C / min or more and 30°C / min or less, 25°C / min or more and 30°C / min or less 0°C / min or less, 0.1°C / min to 25°C / min, 5°C / min to 25°C / min, 10°C / min to 25°C / min, 15°C / min to 25°C / min, 20°C / min to 25°C / min, 0.1°C / min to 20°C / min, 5°C / min to 20°C / min, 10°C / min to 20°C / min, 15°C / min to 20°C / min, 0.1°C / min to 15°C / min, 5°C / min to 15°C / min, 10°C / min to 15°C / min, 0.1°C / min to 10°C / min, 5°C / min to 10°C / min, or 0.≧1° C. / min and ≦5° C. / min. The above ranges should be understood to include all subranges within the ranges explicitly disclosed. Such a heating rate allows for an adequate amount of nucleation and crystal growth without damaging the glass-ceramic article. Heating too quickly can damage the material. However, heating too slowly can prevent adequate nucleation and growth.

[0129] In an embodiment, the glass-ceramic article is cooled after being held at the growth temperature. In an embodiment, the glass-ceramic article may be cooled to room temperature in one stage at a constant cooling rate, in two stages with different cooling rates, or in three or more stages with different cooling rates. In an embodiment, the glass-ceramic article is cooled at a controlled rate from the growth temperature to minimize temperature gradients throughout the article and to minimize residual stresses throughout the article. Differences in temperature gradients and residual stresses may cause the article to warp during cooling. Thus, controlling the cooling to control temperature gradients and residual stresses can also minimize warping of the glass-ceramic article.

[0130] When the precursor glass is subjected to the above heat treatment, the resulting glass ceramic has a phase assemblage in which lithium disilicate and petalite are the crystalline phases with the highest weight percent. In embodiments, the lithium disilicate and petalite are present in approximately equal amounts by weight percent, constituting 75% to 90% by weight, 80% to 90% by weight, 85% to 90% by weight, 75% to 85% by weight, 80% to 85% by weight, or 75% to 80% by weight. The above ranges should be understood to include all subranges within the ranges explicitly disclosed.

[0131] Lithium disilicate (Li2Si2O5) is an orthorhombic crystal based on corrugated sheets of {Si2O5} tetrahedral arrangement. Its crystals are usually tabular or lath shaped with pronounced cleavage planes. Lithium disilicate-based glass-ceramics exhibit highly desirable mechanical properties, including high bulk strength and fracture toughness, due to their randomly oriented, interlocking crystal microstructure (where cracks propagate through the material via tortuous paths around these crystals). In an embodiment, the weight percentage of the lithium disilicate crystalline phase in the glass-ceramic composition is 30% to 50%, by weight, 32% to 50%, by weight, 35% to 50%, by weight, 37% to 50%, by weight, 40% to 50%, by weight, 42% to 50%, by weight, 45% to 50%, by weight, 47% to 50%, by weight, 30% to 47%, by weight, 32% to 47%, by weight, 35% to 47%, by weight, 37% to 47%, by weight, 40% to 47%, by weight, 42% to 47%, by weight, 45% to 47%, by weight, 30% to 45%, by weight, 32% to 45% , 35% by mass or more and 45% by mass or less, 37% by mass or more and 45% by mass or less, 40% by mass or more and 45% by mass or less, 42% by mass or more and 45% by mass or less, 30% by mass or more and 42% by mass or less, 32% by mass or more and 42% by mass or less, 35% by mass or more and 42% by mass or less, 37% by mass or more and 42% by mass or less, 40% by mass or more and 42% by mass or less, 30% by mass or more and 40% by mass or less, 32% by mass or more and 40% by mass or less, 35% by mass or more and 40% by mass or less, 37% by mass or more and 40% by mass or less, 30% by mass or more and 37% by mass or less, 32% by mass or more and 37% by mass or less, 35% by mass or more and 37% by mass or less, 30% by mass or more and 35% by mass or less, 32% by mass or more and 35% by mass or less, or 30% by mass or more and 32% by mass or less. It is to be understood that the above ranges include all subranges within the ranges expressly disclosed.In an embodiment, the glass-ceramic has 30, 31, 32, 33, 34, 35, 36, 37, 38, 39, 40, 41, 42, 43, 44, 45, 46, 47, 48, 49, or 50% by weight of a lithium disilicate crystalline phase.

[0132] Petalite is a monoclinic crystal with a three-dimensional framework structure with a layered structure with folded SiO layers connected by Li and Al tetrahedra. Li is tetrahedrally coordinated with oxygen. The mineral petalite is a source of lithium and is used as a low thermal expansion phase to improve the thermal shock resistance of glass-ceramics or ceramic components. Furthermore, glass-ceramic articles based on the petalite phase can be chemically strengthened in a salt bath, whereby the Li in the petalite structure is dissolved. + Na + (and / or K +), resulting in surface compression and strengthening. In an embodiment, the weight percentage of the petalite crystalline phase in the glass-ceramic composition is 30% to 50%, 32% to 50%, 35% to 50%, 37% to 50%, 40% to 50%, 42% to 50%, 45% to 50%, 47% to 50%, 30% to 47%, 32% to 47%, 35% to 47%, 37% to 47%, 40% to 47%, 42% to 47%, 45% to 47%, 30% to 45%, 32% to 45%, 32% to 45%, 35 ... The range is 5% by mass or more and 45% by mass or less, 37% by mass or more and 45% by mass or less, 40% by mass or more and 45% by mass or less, 42% by mass or more and 45% by mass or less, 30% by mass or more and 42% by mass or less, 32% by mass or more and 42% by mass or less, 35% by mass or more and 42% by mass or less, 37% by mass or more and 42% by mass or less, 40% by mass or more and 42% by mass or less, 30% by mass or more and 40% by mass or less, 32% by mass or more and 40% by mass or less, 35% by mass or more and 40% by mass or less, 37% by mass or more and 40% by mass or less, 30% by mass or more and 37% by mass or less, 32% by mass or more and 37% by mass or less, 35% by mass or more and 37% by mass or less, 30% by mass or more and 35% by mass or less, 32% by mass or more and 35% by mass or less, or 30% by mass or more and 32% by mass or less. It should be understood that the above ranges include all subranges within the explicitly disclosed ranges. In embodiments, the glass-ceramic has 30, 31, 32, 33, 34, 35, 36, 37, 38, 39, 40, 41, 42, 43, 44, 45, 46, 47, 48, 49, or 50% by weight of the petalite crystalline phase.

[0133] As discussed above, in embodiments, the glass ceramic includes about equal amounts, by weight percent, of lithium disilicate and petalite. In embodiments, the weight ratio of lithium disilicate to petalite in the glass ceramic is 0.5 to 1.5, 0.6 to 1.5, 0.7 to 1.5, 0.8 to 1.5, 0.9 to 1.5, 1.0 to 1.5, 1.1 to 1.5, 1.2 to 1.5, 1.3 to 1.5, 1.4 to 1.5, 0.5 to 1.4, 0.6 ... .4 or less, 0.7 or more and 1.4 or less, 0.8 or more and 1.4 or less, 0.9 or more and 1.4 or less, 1.0 or more and 1.4 or less, 1.1 or more and 1.4 or less, 1.2 or more and 1.4 or less, 1.3 or more and 1.4 or less, 0.5 or more and 1.3 or less, 0.6 or more and 1.3 or less, 0.7 or more and 1.3 or less, 0.8 or more and 1.3 or less, 0.9 or more and 1.3 or less, 1.0 or more and 1.3 or less, 1.1 or more and 1.3 or less, 1.2 and 1.3, 0.5 and 1.2, 0.6 and 1.2, 0.7 and 1.2, 0.8 and 1.2, 0.9 and 1.2, 1.0 and 1.2, 1.1 and 1.2, 0.5 and 1.1, 0.6 and 1.1, 0.7 and 1.1, 0.8 and 1.1, 0.9 and 1.1, 1.0 and 1.1, 0.5 and 1.0 0.6 to 1.0, 0.7 to 1.0, 0.8 to 1.0, 0.9 to 1.0, 0.5 to 0.9, 0.6 to 0.9, 0.7 to 0.9, 0.8 to 0.9, 0.5 to 0.8, 0.6 to 0.8, 0.7 to 0.8, 0.5 to 0.7, 0.6 to 0.7, or 0.5 to 0.6. It is to be understood that the above ranges include all subranges within those ranges expressly disclosed.

[0134] In an embodiment, the glass ceramic is 5% by weight or more and 20% by weight or less, 7% by weight or more and 20% by weight or less, 10% by weight or more and 20% by weight or less, 12% by weight or more and 20% by weight or less, 15% by weight or more and 20% by weight or less, 17% by weight or more and 20% by weight or less, 5% by weight or more and 17% by weight or less, 7% by weight or more and 17% by weight or less, 10% by weight or more and 17% by weight or less, 12% by weight or more and 17% by weight or less, 15% by weight or more and 17% by weight or less, 5% to 15% by weight, 7% to 15% by weight, 10% to 15% by weight, 12% to 15% by weight, 5% to 12% by weight, 7% to 12% by weight, 10% to 12% by weight, 5% to 10% by weight, 7% to 10% by weight, or 5% to 7% by weight. The above ranges are understood to include all subranges within the ranges explicitly disclosed. In embodiments, the residual amorphous glass content can be 20, 19, 18, 17, 16, 15, 14, 13, 12, 11, 10, 9, 8, 7, 6, or 5% by weight.

[0135] As previously disclosed herein, in embodiments, the glass-ceramics contain less than 5 wt. %, such as less than 3 wt. %, of a total of crystalline phases other than lithium disilicate and petalite, such as, but not limited to, lithium metasilicate (LiSiO), vergilite (LiSiO), and the like. x Al x S 3-x SiO6), cristabolite (SiO2), quartz (SiO2), zirconia (ZrO2), baddeleyite (ZrO2), spodumene (LiAlSi2O6), and lithium phosphate (Li3PO4). In an embodiment, the glass-ceramic contains less than 2 wt. % of the sum of crystalline phases other than lithium disilicate and petalite, or less than 1 wt. % of the sum of crystalline phases other than lithium disilicate and petalite.

[0136] The crystalline phase population described herein limits the refractive index mismatch between the crystals and the residual amorphous glass, reducing scattering and the resulting haze of the glass-ceramic.

[0137] The particle size of the crystals in the crystalline phase is a factor that affects the transparency of the glass-ceramic. In an embodiment, the particles have a longest dimension in the range of about 5 nm to about 150 nm, about 5 nm to about 125 nm, about 5 nm to about 100 nm, about 5 nm to about 75 nm, about 5 nm to about 50 nm, about 25 nm to about 150 nm, about 25 nm to about 125 nm, about 25 nm to about 100 nm, about 25 nm to about 75 nm, about 50 nm to about 150 nm, about 50 nm to about 125 nm, about 50 nm to about 100 nm, and all ranges and subranges therebetween. In an embodiment, the longest dimension of the particles is less than 150 nm, less than 125 nm, less than 100 nm, less than 75 nm, less than 50 nm, or less than 25 nm. The longest dimension of the particles is measured using a scanning electron microscope (SEM).

[0138] In an embodiment, the glass-ceramic article has high transparency and low haze, making it suitable for use as a cover glass for portable electronic devices. In an embodiment, the glass-ceramic article is transparent in that the average transmission of light over a wavelength range of 450 nm to 600 nm for a glass-ceramic article having a thickness of 1 mm is 85% or more, 86% or more, 87% or more, 88% or more, 89% or more, 90% or more, 91% or more, 92% or more, 93% or more (including surface reflection losses). In other embodiments, the glass-ceramic can be translucent over a wavelength range of 450 nm to 600 nm. In an embodiment, the translucent glass-ceramic can have an average transmission of light over a wavelength range of about 450 nm to about 800 nm for a glass-ceramic article having a thickness of 1 mm in the range of about 20% to less than about 85%. In embodiments, the glass-ceramic article has a haze of less than or equal to 0.15, 0.14, 0.13, 0.12, 0.11, 0.10, 0.09, 0.08, 0.07, 0.06, or 0.05, measured on a glass-ceramic article having a thickness of 0.6 mm.

[0139] chemical strengthening In an embodiment, a glass-ceramic article can be strengthened to have a compressive stress layer on one or more surfaces thereof. Referring now to FIG. 2, an exemplary cross-sectional side view of a strengthened glass-ceramic article 100 is shown having a first surface 102 and an opposing second surface 104 separated by a thickness (t). In an embodiment, the strengthened glass-ceramic article 100 is ion-exchanged and has a compressive stress (CS) layer 106 (or first region) that extends from the first surface 102 to a depth of compression (DOC). In an embodiment, as shown in FIG. 2, the glass-ceramic article 100 also has a compressive stress (CS) layer 108 that extends from the second surface 104 to a depth of compression DOC'.

[0140] In embodiments, glass-ceramic articles can be chemically strengthened using one or more ion-exchange techniques. In these embodiments, ion-exchange can be performed by subjecting one or more surfaces of such glass-ceramic articles to one or more ion-exchange media (e.g., molten salt baths) having a particular composition and temperature for a specified time to impart a compressive stress layer(s) to the one or more surfaces. In embodiments, the ion-exchange media is a molten salt bath containing larger ions (e.g., alkali metal ions) than those present in the glass-ceramic article (e.g., alkali metal ions), where the larger ions from the molten bath are exchanged for smaller ions in the glass-ceramic article to impart a compressive stress to the glass-ceramic article, thereby increasing the strength of the glass-ceramic article.

[0141] In embodiments, a single-stage ion exchange process may be used, while in other embodiments, a multi-stage ion exchange process may be used. In embodiments, in both the single-stage and multi-stage ion exchange processes, the ion exchange medium (e.g., molten bath) may include potassium nitrate (KNO3) and sodium nitrate (NaNO3) as primary components. In embodiments, the ion exchange medium may further include lithium nitrate (LiNO3), sodium nitrite (NaNO2), and silicic acid.

[0142] In an embodiment, the ion exchange medium comprises 50% to 70% by weight KNO3, 55% to 70% by weight KNO3, 60% to 70% by weight KNO3, 65% to 70% by weight KNO3, 50% to 65% by weight KNO3, 55% to 65% by weight KNO3, 60% to 65% by weight KNO3, 50% to 60% by weight KNO3, 55% to 60% by weight KNO3, or 50% to 55% by weight KNO3. It is to be understood that the above ranges include all subranges within the ranges explicitly disclosed.

[0143] In an embodiment, the ion exchange medium comprises 30% to 50% by weight NaNO3, 35% to 50% by weight NaNO3, 40% to 50% by weight NaNO3, 45% to 50% by weight NaNO3, 30% to 45% by weight NaNO3, 35% to 45% by weight NaNO3, 40% to 45% by weight NaNO3, 30% to 40% by weight NaNO3, 35% to 40% by weight NaNO3, or 30% to 35% by weight NaNO3. It is to be understood that the above ranges include all subranges within the ranges explicitly disclosed.

[0144] In an embodiment, the ion exchange medium comprises 0.05% to 0.15% by weight LiNO3, 0.08% to 0.15% by weight LiNO3, 0.10% to 0.15% by weight LiNO3, 0.12% to 0.15% by weight LiNO3, 0.05% to 0.12% by weight LiNO3, 0.08% to 0.12% by weight LiNO3, 0.10% to 0.12% by weight LiNO3, 0.05% to 0.10% by weight LiNO3, 0.08% to 0.10% by weight LiNO3, or 0.05% to 0.08% by weight LiNO3. It is to be understood that the above ranges include all subranges within the ranges explicitly disclosed.

[0145] The inclusion of lithium in the ion-exchange media (by the addition of LiNO3) can improve the corrosion resistance of glass-ceramics according to embodiments disclosed and described herein. Figure 3 shows Fundamental Stress Meter (FSM) images of a glass-ceramic having a composition according to Table 1 below and ion-exchanged at 530°C for 4 hours in a molten salt bath of about 60% KNO3 / about 40% NaNO3+X% LiNO3 by weight, where "X" is 0% Li, 0.05% Li, 0.06% Li, 0.07% Li, 0.08% Li, 0.09% Li, 0.10% Li, or 0.12% Li by weight, as shown in Figures 3A-5B. As shown in Figure 3, a transition begins at about 0.05% Li by weight, with an abrupt transition observed at lithium contents of 0.08% by weight and above. This transition, shown in the FSM images of FIG. 3, shows a correlation with corrosion resistance. FIGS. 3A-3C show the surface corrosion of a glass-ceramic prepared according to the embodiments disclosed and described herein and exposed to 85° C. and 85% relative humidity for 500 hours. Referring now to FIG. 4A, a similar glass-ceramic reinforced with an ion-exchanged media without Li is severely corroded by sodium carbonate. However, the addition of lithium to the ion-exchanged media appears to counteract the sodium carbonate corrosion. FIG. 4B shows a glass-ceramic treated with an ion-exchanged media having 0.06 wt. % Li and no corrosion by sodium carbonate, and FIG. 4C shows a glass-ceramic treated with an ion-exchanged media having 0.08 wt. % lithium and no corrosion by sodium carbonate. In contrast, the glass-ceramics shown in FIGS. 5A and 5B that were not prepared according to the embodiments disclosed and described herein exhibit corrosion by sodium carbonate when exposed to 85° C. and 85% relative humidity for 500 hours, even when treated with ion exchange media having 0.05 wt % Li (FIG. 5A) and 0.65 wt % Li (FIG. 5B).Without being bound to a particular theory, it is believed that glass-ceramics prepared according to the embodiments disclosed and described herein and processed in an ion-exchange medium with lithium can achieve a higher sodium content at the surface at maximum central tension than conventional glass-ceramics, but this high sodium content does not result in the formation of an amorphous layer (which may be present in conventional glass-ceramics) that can decompose the surface crystals and cause corrosion.

[0146] In an embodiment, the ion exchange medium comprises 0.40% to 0.60% by weight NaNO2, 0.45% to 0.60% by weight NaNO2, 0.50% to 0.60% by weight NaNO2, 0.55% to 0.60% by weight NaNO2, 0.40% to 0.55% by weight NaNO2, 0.45% to 0.55% by weight NaNO2, 0.50% to 0.55% by weight NaNO2, 0.40% to 0.50% by weight NaNO2, 0.45% to 0.50% by weight NaNO2, or 0.40% to 0.45% by weight NaNO2. It is to be understood that the above ranges include all subranges within the ranges explicitly disclosed.

[0147] In an embodiment, the ion exchange medium comprises 0.40% to 0.60% by weight silicic acid, 0.45% to 0.60% by weight silicic acid, 0.50% to 0.60% by weight silicic acid, 0.55% to 0.60% by weight silicic acid, 0.40% to 0.55% by weight silicic acid, 0.45% to 0.55% by weight silicic acid, 0.50% to 0.55% by weight silicic acid, 0.40% to 0.50% by weight silicic acid, 0.45% to 0.50% by weight silicic acid, or 0.40% to 0.45% by weight silicic acid. It is to be understood that the above ranges include all subranges within the ranges explicitly disclosed.

[0148] In embodiments, the temperature of the ion exchange medium is 450° C. or more and 550° C. or less, 475° C. or more and 550° C. or less, 500° C. or more and 550° C. or less, 525° C. or more and 550° C. or less, 530° C. or more and 550° C. or more, 450° C. or more and 530° C. or less, 475° C. or more and 530° C. or less, 500° C. or more and 530° C. or more, 525° C. or more and 530° C. or more, 450° C. or more and 525° C. or more, 475° C. or more and 525° C. or less, 500° C. or more and 500° C. or more, 475° C. or more and 500° C. or less, or 450° C. or more and 475° C. or less. It is to be understood that the above ranges include all subranges within the ranges explicitly disclosed.

[0149] According to embodiments, the glass-ceramic article can have a thermal stability of at least 1 hour and at most 16 hours, at least 2 hours and at most 16 hours, at least 4 hours and at most 16 hours, at least 6 hours and at most 16 hours, at least 8 hours and at most 16 hours, at least 10 hours and at most 16 hours, at least 12 hours and at most 16 hours, at least 14 hours and at most 16 hours, at least 1 hour and at most 14 hours, at least 2 hours and at most 14 hours, at least 4 hours and at most 14 hours, at least 6 hours and at most 14 hours, at least 8 hours and at most 14 hours, at least 10 hours and at most 14 hours, at least 12 hours and at most 14 hours, at least 1 hour and at most 12 hours, at least 2 hours and at most 12 hours, at least 4 hours and at most 16 hours, at least 1 hour ... The ion exchange medium is contacted for a period of time of 12 hours or less, 6 hours or more and 12 hours or less, 8 hours or more and 12 hours or less, 10 hours or more and 12 hours or less, 1 hour or more and 10 hours or less, 2 hours or more and 10 hours or less, 4 hours or more and 10 hours or less, 6 hours or more and 10 hours or less, 8 hours or more and 10 hours or less, 1 hour or more and 8 hours or less, 2 hours or more and 8 hours or less, 4 hours or more and 8 hours or less, 6 hours or more and 8 hours or less, 1 hour or more and 6 hours or less, 2 hours or more and 6 hours or less, 4 hours or more and 6 hours or less, 1 hour or more and 4 hours or less, 2 hours or more and 4 hours or less, or 1 hour or more and 2 hours or less. It is to be understood that the above ranges include all subranges within the ranges explicitly disclosed.

[0150] It should be understood that after the ion-exchange process has been performed, the composition of the surface of the glass-ceramic may differ from the composition of the as-formed glass-ceramic (i.e., the glass-ceramic before being subjected to the ion-exchange process). + Or Na + One type of alkali metal ion in the as-formed glass-ceramic, e.g., Na + Or K + Such a change is due to the replacement of the glass ceramic composition at or near the center of the depth of the glass ceramic article with larger alkali metal ions such as . However, the glass ceramic composition at or near the center of the depth of the glass ceramic article will, in embodiments, still have the composition of the as-formed glass ceramic. As used herein, the center of the glass article refers to any location in the glass article that is at a distance of at least 0.5t from any surface of the glass article, where t is the thickness of the glass article.

[0151] Mechanical properties of glass-ceramic articles The mechanical properties of the glass-ceramic articles disclosed herein are tested against a strengthened glass-ceramic article unless otherwise specified. By forming a glass-ceramic having a composition as disclosed and described herein and using the heat treatment and chemical strengthening as disclosed and described herein, a glass-ceramic can be achieved that has a phase assemblage that provides low haze and good mechanical properties (described in detail below). As described in separate paragraphs below, glass-ceramics of embodiments have a combination of various mechanical properties. The balance of these mechanical properties results in a durable and robust glass-ceramic that is difficult to achieve without sacrificing other mechanical properties. For example, and this is just one example, it is possible to achieve only high compressive stress, but it may be more difficult to achieve both high compressive stress and central tension.

[0152] In an embodiment, DOC and DOC' are independently selected from the group consisting of: greater than or equal to 0.15t and less than or equal to 0.25t; greater than or equal to 0.16t and less than or equal to 0.25t; greater than or equal to 0.17t and less than or equal to 0.25t; greater than or equal to 0.18t and less than or equal to 0.25t; greater than or equal to 0.19t and less than or equal to 0.25t; greater than or equal to 0.20t and less than or equal to 0.25t; greater than or equal to 0.21t and less than or equal to 0.25t; greater than or equal to 0.22t and less than or equal to 0.25t; greater than or equal to 0.23t and less than or equal to 0.25t; greater than or equal to 0.24t and less than or equal to 0.25t; greater than or equal to 0.15t and less than or equal to 0.24t; greater than or equal to 0.16t and less than or equal to 0.24t; greater than or equal to 0.17t and less than or equal to 0.24t. or less, 0.18t or more and 0.24t or less, 0.19t or more and 0.24t or less, 0.20t or more and 0.24t or less, 0.21t or more and 0.24t or less, 0.22t or more and 0.24t or less, 0.23t or more and 0.24t or less, 0.15t or more and 0.23t or less, 0.16t or more and 0.23t or less, 0.17t or more and 0.23t or less, 0.18t or more and 0.23t or less, 0.19t or more and 0.23t or less, 0.20t or more and 0.23t or less, 0.21t or more and 0.23t or less, 0.22t or more and 0.23t or less, 0.15t or more and 0.22t or less, 0.16t or more and 0.22t or less, 0.17t or more and 0.22t or less, 0.18t or more and 0.22t or less, 0.19t or more and 0.22t or less, 0.20t or more and 0.22t or less, 0.21t or more and 0.22t or less, 0.15t or more and 0.21t or less, 0.16t or more and 0.21t or less, 0.17t or more and 0.21t or less, 0.18t or more and 0.21t or less, 0.19t or more and 0.21t or less, 0.20t or more and 0.21t or less, 0.15t or more and 0.20t or less, 0. 16t or more and 0.20t or less, 0.17t or more and 0.20t or less, 0.18t or more and 0.20t or less, 0.19t or more and 0.20t or less, 0.15t or more and 0.19t or less, 0.16t or more and 0.19t or less, 0.17t or more and 0.19t or less, 0.18t or more and 0.19t or less, 0.15t or more and 0.18t or less, 0.16t or more and 0.18t or less, 0.17t or more and 0.18t or less, 0.15t or more and 0.17t or less, 0.16t or more and 0.17t or less, or 0.15t or more and 0.16t or less.

[0153] There is also a central tension region 110 between the DOC and DOC' that is under tensile stress. Thus, the stress transitions from compressive to tensile stress at the aforementioned DOC and DOC', measured from the surface towards the centerline of the strengthened glass-ceramic article.

[0154] In an embodiment, the glass-ceramic article has a melting point of 200 MPa or more and 400 MPa or less, e.g., 225 MPa or more and 400 MPa or less, 250 MPa or more and 400 MPa or less, 275 MPa or more and 400 MPa or less, 300 MPa or more and 400 MPa or less, 325 MPa or more and 400 MPa or less, 350 MPa or more and 400 MPa or less, 375 MPa or more and 400 MPa or less, 200 MPa or more and 375 MPa or less, 225 MPa or more and 375 MPa or less, 250 MPa or more and 375 MPa or less, 275 MPa or more and 375 MPa or less, 300 MPa or more and 375 MPa or less, 325 MPa or more and 375 MPa or less, 350 MPa or more and 375 MPa or less, 200 MPa or more and 350 MPa or less, 225 MPa or more and 350 MPa or less, 250 MPa or more and 350 MPa or less. a or less, 275 MPa or more and 350 MPa or less, 300 MPa or more and 350 MPa or less, 325 MPa or more and 350 MPa or more, 200 MPa or more and 325 MPa or less, 225 MPa or more and 325 MPa or less, 250 MPa or more and 325 MPa or more, 275 MPa or more and 325 MPa or less, 300 MPa or more and 325 MPa or more, 200 MPa or more and 300 MPa or less, 225 MPa or more and 300 MPa or more, 250 MPa or more and 300 MPa or more, 275 MPa or more and 300 MPa or less, 200 MPa or more and 275 MPa or less, 225 MPa or more and 275 MPa or less, 250 MPa or more and 275 MPa or less, 200 MPa or more and 250 MPa or less, 225 MPa or more and 250 MPa or less, or 200 MPa or more and 225 MPa or less. It is understood that the above ranges include all subranges within the explicitly disclosed ranges.

[0155] In an embodiment, the maximum central tension (CT) is 100 MPa or more and 170 MPa or less, e.g., 110 MPa or more and 170 MPa or less, 120 MPa or more and 170 MPa or less, 130 MPa or more and 170 MPa or less, 140 MPa or more and 170 MPa or less, 150 MPa or more and 170 MPa or less, 160 MPa or more and 170 MPa or less, 100 MPa or more and 160 MPa or less, 110 MPa or more and 160 MPa or less, 120 MPa or more and 160 MPa or less, 130 MPa or more and 160 MPa or less, 140 MPa or more and 160 MPa or less, 150 MPa or more and 160 MPa or less, 100 MPa or more and 150MPa or less, 110MPa or more and 150MPa or less, 120MPa or more and 150MPa or less, 130MPa or more and 150MPa or more, 140MPa or more and 150MPa or less, 100MPa or more and 140MPa or less, 110MPa or more and 140MPa or more, 120MPa or more and 140MPa or less, 130MPa or more and 140MPa or more, 100MPa or more and 130MPa or less, 110MPa or more and 130MPa or more, 120MPa or more and 130MPa or more, 100MPa or more and 120MPa or less, 110MPa or more and 120MPa or less, or 100MPa or more and 110MPa or less. It is to be understood that the above ranges include all subranges within the ranges explicitly disclosed.

[0156] In an embodiment, the glass ceramic has a ratio of CS to CT (CS / CT) of 1.5 or more and 3.0 or less, such as 1.8 or more and 3.0 or less, such as 1.8 or more and 3.0 or less, such as 2.0 or more and 3.0 or less, such as 2.2 or more and 3.0 or less, such as 2.5 or more and 3.0 or less, such as 2.8 or more and 3.0 or less, such as 1.5 or more and 2.8 or less, such as 1.8 or more and 2.8 or less, such as 2.0 or more and 2.8 or less, such as 2.2 or more and 2.8 or less, such as 1.5 or more and 2.5 or less, such as 1.8 or more and 2.5 or less, such as 2.0 or more and 2.5 or less, such as 2.2 or more and 2.2 or less, such as 1.8 or more and 2.2 or less, such as 1.8 or more and 2.0 or less, or such as 1.5 or more and 1.8 or less. It is to be understood that the above ranges include all subranges within the ranges expressly disclosed.

[0157] Glass-ceramic articles according to embodiments have a stress that decreases with increasing distance from the surface of the glass article toward the centerline of the glass article, the stress being greater than or equal to 0.07t and less than or equal to 0.26t, greater than or equal to 0.10t and less than or equal to 0.26t, greater than or equal to 0.12t and less than or equal to 0.26t, greater than or equal to 0.15t and less than or equal to 0.26t, greater than or equal to 0.17t and less than or equal to 0.26t, greater than or equal to 0.20t and less than or equal to 0.26t, greater than or equal to 0.22t and less than or equal to 0.26t. t or more and up to 0.26t, 0.25t or more and up to 0.26t, 0.07t or more and up to 0.25t, 0.10t or more and up to 0.25t, 0.12t or more and up to 0.25t, 0.15t or more and up to 0.25t, 0.17t or more and up to 0.25t, 0.20t or more and up to 0.25t, 0.22t or more and up to 0.25t, 0.07t or more and up to 0.22t, 0.10t or more and .22t or less, 0.12t or more and 0.22t or less, 0.15t or more and 0.22t or less, 0.17t or more and 0.22t or less, 0.20t or more and 0.22t or less, 0.07t or more and 0.20t or less, 0.10t or more and 0.20t or less, 0.12t or more and 0.20t or less, 0.15t or more and 0.20t or less, 0.17t or more and 0.20t or less, 0.07t or more and 0.17t or less , 0.10t or more and 0.17t or less, 0.12t or more and 0.17t or less, 0.15t or more and 0.17t or more, 0.07t or more and 0.15t or less, 0.10t or more and 0.15t or more, 0.12t or more and 0.15t or more, 0.07t or more and 0.12t or less, 0.10t or more and 0.12t or more, or 0.07t or more and 0.10t or less, as a substantially linear function of depth. It is to be understood that the above ranges include all subranges within the explicitly disclosed ranges.

[0158] According to embodiments, the stress of the glass ceramic article is, as measured from the surface of the glass ceramic article toward the centerline of the glass ceramic article, in the range of from 0.18t to 0.25t, 0.19t to 0.25t, 0.20t to 0.25t, 0.21t to 0.25t, 0.22t to 0.25t, 0.23t to 0.25t, 0.24t to 0.25t, 0.18t to 0.24t, 0.19t to 0.24t, 0.20t to 0.24t, 0.21t to 0.24t, 0.22t to 0.24t, 0.23t to 0.24t, 0.24t to 0.24t, t, 0.18t to 0.23t, 0.19t to 0.23t, 0.20t to 0.23t, 0.21t to 0.23t, 0.22t to 0.23t, 0.18t to 0.22t, 0.19t to 0.22t, 0.20t to 0.22t, 0.21t to 0.22t, 0.18t to 0.21t, 0.19t to 0.21t, 0.20t to 0.21t, 0.18t to 0.20t, 0.19t to 0.20t, or 0.18t to 0.19t. It is to be understood that the above ranges include all subranges within the ranges explicitly disclosed.

[0159] According to an embodiment, the glass ceramic article has a maximum central tension (mCT) and an absolute value of the surface compressive stress, measured at the surface of the glass ceramic article, is 1.5 mCT or more and 2.5 mCT or less, 1.7 mCT or more and 2.5 mCT or less, 2.0 mCT or more and 2.5 mCT or less, 2.2 mCT or more and 2.5 mCT or less, 1.5 mCT or more and 2.2 mCT or less, 1.7 mCT or more and 2.2 mCT or less, 2.0 mCT or more and 2.2 mCT or less, 1.5 mCT or more and 2.0 mCT or less, 1.7 mCT or more and 2.0 mCT or less, or 1.5 mCT or more and 1.7 mCT or less. It is to be understood that the above ranges include all subranges within the ranges explicitly disclosed.

[0160] In an embodiment, the stored strain energy of the glass-ceramic article is 22 J / m 2 More than 60 J / m 2 For example, 25 J / m 2 More than 60 J / m 2 Below, 30J / m 2 More than 60 J / m 2 Below, 35J / m 2 More than 60 J / m 2 Below, 40J / m 2 More than 60 J / m 2 Below, 45J / m 2 More than 60 J / m 2 Below, 50J / m 2 More than 60 J / m 2 Below, 55J / m 2 More than 60 J / m 2 Below, 22J / m 2 Above 55 J / m 2 For example, 25 J / m 2 Above 55 J / m 2 Below, 30J / m 2 Above 55 J / m 2 Below, 35J / m 2 Above 55 J / m 2 Below, 40J / m 2 Above 55 J / m 2 Below, 45J / m 2 Above 55 J / m 2 Below, 50J / m 2 Above 55 J / m 2 Below, 22J / m 2 More than 50 J / m 2 For example, 25 J / m 2 More than 50 J / m 2 Below, 30J / m 2 More than 50 J / m 2 Below, 35J / m 2 More than 50 J / m 2 Below, 40J / m 2 More than 50 J / m 2 Below, 45J / m 2 More than 50 J / m 2 Below, 22J / m 2 Above 45 J / m 2 Less than or equal to 25 J / m2 And 45 J / m 2 Below, 30J / m 2 Above 45 J / m 2 Below, 35J / m 2 Above 45 J / m 2 Below, 40J / m 2 Above 45 J / m 2 Below, 22J / m 2 More than 40 J / m 2 For example, 25 J / m 2 More than 40 J / m 2 Below, 30J / m 2 More than 40 J / m 2 Below, 35J / m 2 More than 40 J / m 2 Below, 22J / m 2 Above 35 J / m 2 For example, 25 J / m 2 Above 35 J / m 2 Below, 30J / m 2 Above 35 J / m 2 Below, 22J / m 2 More than 30 J / m 2 For example, 25 J / m 2 More than 30 J / m 2 or less than 22 J / m 2 Above 25 J / m 2 The above ranges should be understood to include all subranges within those ranges explicitly disclosed. The glass-ceramic achieves the aforementioned stored strain energy without branching crack patterns.

[0161] In an embodiment, the glass-ceramic article has a thickness of 0.1 mm to 2.0 mm, 0.3 mm to 2.0 mm, 0.5 mm to 2.0 mm, 0.8 mm to 2.0 mm, 1.0 mm to 2.0 mm, 1.3 mm to 2.0 mm, 1.5 mm to 2.0 mm, 1.8 mm to 2.0 mm, 0.1 mm to 1.8 mm, 0.3 mm to 1.8 mm, 0.5 mm to 1.8 mm, 0.8 mm to 1.8 mm, 1.0 mm to 1.8 mm, 1.3 mm to 1.8 mm, 1.5 mm to 1.8 mm, 0.1 mm to 1.5 mm, 0.3 mm to 1.5 mm, 0.5 mm to 1.5 0.8mm to 1.5mm, 1.0mm to 1.5mm, 1.3mm to 1.5mm, 0.1mm to 1.3mm, 0.3mm to 1.3mm, 0.5mm to 1.3mm, 0.8mm to 1.3mm, 1.0mm to 1.3mm, 0.1mm to 1.0mm, 0.3mm to 1.0mm, 0.5mm to 1.0mm, 0.8mm to 1.0mm, 0.1mm to 0.8mm, 0.3mm to 0.8mm, 0.5mm to 0.8mm, 0.1mm to 0.5mm, 0.3mm to 0.5mm, or 0.1mm to 0.3mm. It is to be understood that the above ranges include all subranges within the explicitly disclosed ranges.

[0162] In embodiments, the glass-ceramic article can be substantially planar and flat. In other embodiments, the glass-ceramic article can be shaped to have, for example, a 2.5D or 3D shape. In embodiments, the glass-ceramic article can have a uniform thickness, and in other embodiments, the glass-ceramic article can not have a uniform thickness.

[0163] In an embodiment, the fracture toughness of the glass-ceramic article is from 1.0 MPa√m to 2.0 MPa√m, from 1.2 MPa√m to 2.0 MPa√m, from 1.4 MPa√m to 2.0 MPa√m, from 1.5 MPa√m to 2.0 MPa√m, from 1.6 MPa√m to 2.0 MPa√m, from 1.8 MPa√m to 2.0 MPa√m, from 1.0 MPa√m to 1.8 MPa√m, from 1.2 MPa√m to 1.8 MPa√m, from 1.4 MPa√m to 1.8 MPa√m, from 1.5 MPa√m to 2.0 MPa√m, 6 MPa√m or more and 1.8 MPa√m or less, 1.0 MPa√m or more and 1.6 MPa√m or less, 1.2 MPa√m or more and 1.6 MPa√m or more, 1.4 MPa√m or more and 1.6 MPa√m or less, 1.5 MPa√m or more and 1.6 MPa√m or more, 1.0 MPa√m or more and 1.5 MPa√m or less, 1.2 MPa√m or more and 1.5 MPa√m or more, 1.4 MPa√m or more and 1.5 MPa√m or less, 1.0 MPa√m or more and 1.4 MPa√m or less, 1.2 MPa√m or more and 1.4 MPa√m or less, or 1.0 MPa√m or more and 1.2 MPa√m or less. It is to be understood that the above ranges include all subranges within the ranges explicitly disclosed.

[0164] In an embodiment, the Young's modulus (also referred to as the elastic modulus) of the non-chemically strengthened glass-ceramic article is 90 GPa or more and 200 GPa or less, e.g., 100 GPa or more and 200 GPa or less, 120 GPa or more and 200 GPa or less, 140 GPa or more and 200 GPa or less, 160 GPa or more and 200 GPa or less, 180 GPa or more and 200 GPa or less, 90 GPa or more and 180 GPa or less, e.g., 100 GPa or more and 180 GPa or less, 120 GPa or more and 180 GPa or less, 140 GPa or more and 200 GPa or less, and 180 GPa or less, 160 GPa or more and 180 GPa or less, 90 GPa or more and 160 GPa or less, for example, 100 GPa or more and 160 GPa or less, 120 GPa or more and 160 GPa or less, 140 GPa or more and 160 GPa or more, 90 GPa or more and 140 GPa or less, for example, 100 GPa or more and 140 GPa or less, 120 GPa or more and 140 GPa or more, 90 GPa or more and 120 GPa or less, for example, 100 GPa or more and 120 GPa or less, or 90 GPa or more and 100 GPa or less. It is to be understood that the above ranges include all subranges within the ranges explicitly disclosed.

[0165] In embodiments, the non-chemically strengthened glass-ceramic article has a Poisson's ratio of 0.15 to 0.25, 0.17 to 0.25, 0.20 to 0.25, 0.22 to 0.25, 0.15 to 0.22, 0.17 to 0.22, 0.20 to 0.22, 0.15 to 0.20, 0.17 to 0.20, or 0.15 to 0.17. It is understood that the above ranges include all subranges within the explicitly disclosed ranges.

[0166] In embodiments, the non-chemically strengthened glass-ceramic article has a shear modulus of 40 GPa or more and 50 GPa or less, 43 GPa or more and 50 GPa or less, 45 GPa or more and 50 GPa or more, 48 GPa or more and 50 GPa or more, 40 GPa or more and 48 GPa or less, 43 GPa or more and 48 GPa or more, 45 GPa or more and 48 GPa or more, 40 GPa or more and 45 GPa or more, 43 GPa or more and 45 GPa or more, or 40 GPa or more and 43 GPa or less. It is understood that the above ranges include all subranges within the ranges explicitly disclosed.

[0167] The fracture stress was measured by applying fracture stress to fracture in a four-point bending test after introducing scratches of about 80 μm depth using sandpaper impact with 1000 grit, 180 grit, and 80 grit slappers. The test was carried out using a dynamic impact test based on an apparatus including a simple pendulum with a surface ranging from flat to curved, where a specimen of the glass-ceramic article is attached to the bob of the pendulum, which is then used to contact the specimen with a rough impact surface. The apparatus is described in detail in WO 2017 / 100646, which is incorporated herein by reference in its entirety. To carry out the test, the sample is loaded into a holder, then pulled backward from the equilibrium position of the pendulum and released to dynamically impact the impact surface.

[0168] The fracture stress of glass-ceramics according to embodiments, measured on glass-ceramic articles having a thickness of 0.6 mm using 1000 grit, is 450 MPa or more and 550 MPa or less, 475 MPa or more and 550 MPa or less, 500 MPa or more and 550 MPa or less, 525 MPa or more and 550 MPa or more, 450 MPa or more and 525 MPa or less, 475 MPa or more and 525 MPa or less, 500 MPa or more and 525 MPa or more, 450 MPa or more and 500 MPa or less, 475 MPa or more and 500 MPa or less, or 450 MPa or more and 475 MPa or less. It is understood that the above ranges include all subranges within the ranges explicitly disclosed.

[0169] The fracture strength of glass-ceramics according to embodiments, measured on glass-ceramic articles having a thickness of 0.5 mm using 1000 grit, is 475 MPa or more and 550 MPa or less, 500 MPa or more and 550 MPa or less, 525 MPa or more and 550 MPa or more, 475 MPa or more and 525 MPa or less, 500 MPa or more and 525 MPa or more, or 475 MPa or more and 500 MPa or less. It is understood that the above ranges include all subranges within the ranges explicitly disclosed.

[0170] The fracture strength of glass-ceramics according to embodiments, measured on glass-ceramic articles having a thickness of 0.6 mm using 180 grit, is 400 MPa to 500 MPa, 425 MPa to 500 MPa, 450 MPa to 500 MPa, 475 MPa to 500 MPa, 400 MPa to 475 MPa, 425 MPa to 475 MPa, 450 MPa to 475 MPa, 400 MPa to 450 MPa, 425 MPa to 450 MPa, or 400 MPa to 425 MPa. It is understood that the above ranges include all subranges within the ranges explicitly disclosed.

[0171] The fracture strength of glass-ceramics according to embodiments, measured on glass-ceramic articles having a thickness of 0.5 mm using 180 grit, is 350 MPa or more and 450 MPa or less, 375 MPa or more and 450 MPa or less, 400 MPa or more and 450 MPa or less, 425 MPa or more and 450 MPa or less, 350 MPa or more and 425 MPa or less, 375 MPa or more and 425 MPa or less, 400 MPa or more and 425 MPa or less, 350 MPa or more and 400 MPa or less, 375 MPa or more and 400 MPa or less, or 350 MPa or more and 375 MPa or less. It is understood that the above ranges include all subranges within the ranges explicitly disclosed.

[0172] The fracture strength of glass-ceramics according to embodiments, measured on glass-ceramic articles having a thickness of 0.6 mm using 80 grit, is 350 MPa or more and 450 MPa or less, 375 MPa or more and 450 MPa or less, 400 MPa or more and 450 MPa or less, 425 MPa or more and 450 MPa or less, 350 MPa or more and 425 MPa or less, 375 MPa or more and 425 MPa or less, 400 MPa or more and 425 MPa or less, 350 MPa or more and 400 MPa or less, 375 MPa or more and 400 MPa or less, or 350 MPa or more and 375 MPa or less. It is understood that the above ranges include all subranges within the ranges explicitly disclosed.

[0173] The fracture strength of glass-ceramics according to embodiments, measured on glass-ceramic articles having a thickness of 0.5 mm using 80 grit, is 300 MPa or more and 400 MPa or less, 325 MPa or more and 400 MPa or less, 350 MPa or more and 400 MPa or less, 375 MPa or more and 400 MPa or less, 300 MPa or more and 375 MPa or less, 325 MPa or more and 375 MPa or less, 350 MPa or more and 375 MPa or less, 300 MPa or more and 350 MPa or less, 325 MPa or more and 350 MPa or less, or 300 MPa or more and 325 MPa or less. It is understood that the above ranges include all subranges within the ranges explicitly disclosed.

[0174] The drop test method is used to measure the drop strength of glasses or glass ceramics. The drop test method involves performing a surface drop test on a puck to which a glass or glass ceramic article is attached. The glass or glass ceramic article to be tested has a thickness similar to or equal to that used in a given portable consumer electronic device. A puck refers to a structure that is intended to mimic the size, shape, and weight distribution of a given device, such as a mobile phone. Hereinafter, the term "puck" refers to a structure that weighs 126.0 grams, has a length of 133.1 mm, a width of 68.2 mm, and a height of 9.4 mm.

[0175] An exemplary device dropper that can be used to perform the drop test method is shown as reference numeral 10 in FIG. 14. The device dropper 10 includes a chuck 12 having chuck jaws 14. A puck 16 is loaded onto the chuck jaws 14 with a glass article attached and facing downward. The chuck 12 is ready to be dropped, for example, from an electromagnetic chuck lifter. Referring now to FIG. 15, the chuck 12 is released and during its drop, the chuck jaws 14 are triggered to open, for example, by a proximity sensor. Once the chuck jaws 14 open, the puck 16 is released. Referring now to FIG. 16, the dropping puck 16 impacts a drop surface 18. The drop surface 18 can be sandpaper, for example, 180 grit sandpaper (however, other grit sandpapers can be used as disclosed herein). If the glass or glass-ceramic article attached to the puck survives the drop (i.e., does not crack), the chuck 12 is set to a higher height and the test is repeated. As a result, the breakage height is the minimum height at which a puck containing glass or glass-ceramic articles can be dropped and the glass or glass-ceramic composition will break.

[0176] In an embodiment, the drop strength of a 0.6 mm thick glass-ceramic article is 190 cm or more and 250 cm or less, 200 cm or more and 250 cm or less, 210 cm or more and 250 cm or more, 220 cm or more and 250 cm or less, 230 cm or more and 250 cm or more, 240 cm or more and 250 cm or less, 190 cm or more and 240 cm or more, 200 cm or more and 240 cm or less, 210 cm or more and 240 cm or more, 220 cm or more and 240 cm or more, cm or less, 230 cm or more and 240 cm or less, 190 cm or more and 230 cm or less, 200 cm or more and 230 cm or less, 210 cm or more and 230 cm or more and 220 cm or more and 230 cm or more and 190 cm or more and 220 cm or less, 200 cm or more and 220 cm or more and 210 cm or more and 220 cm or more and 190 cm or more and 210 cm or more and 200 cm or more and 210 cm or more and 190 cm or more and 200 cm or less. It is to be understood that the above ranges include all subranges within the ranges expressly disclosed.

[0177] In an embodiment, the drop strength of a 0.5 mm thick glass-ceramic article is 180 cm or more and 240 cm or less, 190 cm or more and 240 cm or less, 200 cm or more and 240 cm or less, 210 cm or more and 240 cm or less, 220 cm or more and 240 cm or less, 230 cm or more and 240 cm or less, 180 cm or more and 230 cm or less, 190 cm or more and 230 cm or less, 200 cm or more and 230 cm or less, 210 cm or more and 230 cm or less. cm or less, 220 cm or more and 230 cm or less, 180 cm or more and 220 cm or less, 190 cm or more and 220 cm or more and 200 cm or more and 210 cm or more and 220 cm or more and 180 cm or more and 210 cm or less, 190 cm or more and 210 cm or more and 200 cm or more and 210 cm or more and 180 cm or more and 200 cm or less, 190 cm or more and 200 cm or less, or 180 cm or more and 190 cm or less. It is to be understood that the above ranges include all subranges within the ranges expressly disclosed.

[0178] Unreinforced glass-ceramics according to embodiments disclosed and described herein are also scratch resistant and have a transverse crack initiation load of 0.50 Newtons (N) or more and 0.75 N or less, e.g., 0.55 N or more and 0.75 N or less, 0.60 N or more and 0.75 N or less, 0.65 N or more and 0.75 N or less, 0.70 N or more and 0.75 N or less, 0.50 N or more and 0.70 N or less, 0.55 N or more and 0.70 N or less, 0.60 N or more and 0.70 N or less, 0.65 N or more and 0.70 N or less, 0.50 N or more and 0.65 N or less, 0.55 N or more and 0.65 N or less, 0.60 N or more and 0.65 N or less, 0.50 N or more and 0.60 N or less, 0.55 N or more and 0.60 N or less, or 0.50 N or more and 0.55 N or less. It is to be understood that the above ranges include all subranges within the ranges expressly disclosed.

[0179] The glass ceramic according to the embodiment has a strength of 740 kg, measured for the unreinforced glass ceramic. f / mm 2 (Approx. 7257MPa) or more and 820Kg f / mm 2 (approx. 8041MPa) or less, for example, 760Kg f / mm 2 (Approx. 7453MPa) or more and 820Kg f / mm 2 (approximately 8041MPa) or less, 780Kg f / mm 2 (Approx. 7649MPa) or more and 820Kg f / mm 2 (approx. 8041MPa) or less, 800Kg f / mm 2 (Approx. 7845MPa) or more and 820Kg f / mm 2 (approx. 8041MPa) or less, 740Kg f / mm 2 (Approx. 7257MPa) or more and 800Kg f / mm 2 (approximately 7845MPa) or less, for example, 760Kg f / mm 2 (Approx. 7453MPa) or more and 800Kg f / mm2 (approximately 7845MPa) or less, 780Kg f / mm 2 (Approx. 7649MPa) or more and 800Kg f / mm 2 (approximately 7845MPa) or less, 740Kg f / mm 2 (Approx. 7257MPa) or more and 780Kg f / mm 2 (approximately 7649MPa) or less, for example, 760Kg f / mm 2 (Approx. 7453MPa) or more and 780Kg f / mm 2 (approx. 7649MPa) or less, or 740Kg f / mm 2 (Approx. 7257MPa) or more and 760Kg f / mm 2 (about 7453 MPa) or less Vickers hardness (under a 200 g load). It is understood that the above ranges include all subranges within the explicitly disclosed ranges.

[0180] Embodiments of the glass-ceramic have annealing points of 750° C. or more and 770° C. or less, 755° C. or more and 770° C. or less, 760° C. or more and 770° C. or more and 765° C. or more and 770° C. or more and 750° C. or more and 765° C. or less, 755° C. or more and 765° C. or more and 760° C. or more and 765° C. or more and 750° C. or more and 755° C. It is to be understood that the above ranges include all subranges within the ranges explicitly disclosed.

[0181] Glass-ceramics according to embodiments may have a melting point of 700° C. or higher and 750° C. or lower, 710° C. or higher and 750° C. or lower, 720° C. or higher and 750° C. or lower, 725° C. or higher and 750° C. or lower, 730° C. or higher and 750° C. or lower, 740° C. or higher and 750° C. or lower, 700° C. or higher and 740° C. or lower, 710° C. or higher and 740° C. or lower, 720° C. or higher and 740° C. or lower, 725° C. or higher and 740° C. or lower, 730° C. or higher and 750° C. or lower and 740° C., 700° C. and 730° C., 710° C. and 730° C., 720° C. and 730° C., 725° C. and 730° C., 700° C. and 725° C., 710° C. and 725° C., 720° C. and 725° C., 700° C. and 720° C., 710° C. and 720° C., or 700° C. and 710° C. It is understood that the above ranges include all subranges within the explicitly disclosed ranges.

[0182] According to an embodiment, the glass ceramic has a molecular weight of 1.500 or more and 1.600 or less, 1.520 or more and 1.600 or less, 1.540 or more and 1.600 or less, 1.550 or more and 1.600 or less, 1.560 or more and 1.600 or less, 1.580 or more and 1.600 or less, 1.500 or more and 1.580 or less, 1.520 or more and 1.580 or less, 1.540 or more and 1.580 or less, 1.550 or more and 1.580 or less, 1.560 or more and 1. 0.580 or less, 1.500 or more and 1.560 or less, 1.520 or more and 1.560 or less, 1.540 or more and 1.560 or less, 1.550 or more and 1.560 or less, 1.500 or more and 1.550 or less, 1.520 or more and 1.550 or less, 1.540 or more and 1.550 or less, 1.500 or more and 1.540 or less, 1.520 or more and 1.540 or less, or 1.500 or more and 1.520 or less. It is to be understood that the above ranges include all subranges within the ranges explicitly disclosed.

[0183] The stress optical coefficient of the glass-ceramic according to the embodiment (measured at a wavelength of 546 nm) is 25.5 nm / cm / MPa or more and 26.5 nm / cm / MPa or less, 25.8 nm / cm / MPa or more and 26.5 nm / cm / MPa or less, 26.0 nm / cm / MPa or more and 26.5 nm / cm / MPa or less, 26.2 nm / cm / MPa or more and 26.5 nm / cm / MPa or less, 26.4 nm / cm / MPa or more and 26.5 nm / cm / MPa or less, 25.5 nm / cm / MPa or more and 26.4 nm / cm / MPa or less, 25.8 nm / cm / MPa or more and 26.4 nm / cm / MPa or less, 2 ≧6.0nm / cm / MPa and ≦26.4nm / cm / MPa, ≧26.2nm / cm / MPa and ≦26.4nm / cm / MPa, ≧25.5nm / cm / MPa and ≦26.2nm / cm / MPa, ≧25.8nm / cm / MPa and ≦26.2nm / cm / MPa, ≧26.0nm / cm / MPa and ≦26.2nm / cm / MPa, ≧25.5nm / cm / MPa and ≦26.0nm / cm / MPa, ≧25.8nm / cm / MPa and ≦26.0nm / cm / MPa, or ≧25.5nm / cm / MPa and ≦25.8nm / cm / MPa. It is to be understood that the above ranges include all subranges within the ranges expressly disclosed.

[0184] According to an embodiment, the glass ceramic has a hardness of 2.40 g / cm 3 More than 2.60g / cm 3 Below, 2.42g / cm 3 More than 2.60g / cm 3 Below, 2.45g / cm 3 More than 2.60g / cm 3 Below, 2.48g / cm 3 More than 2.60g / cm 3 Below 2.50g / cm 3 More than 2.60g / cm 3 Below, 2.52g / cm 3 More than 2.60g / cm 3 Below 2.55g / cm 3 More than 2.60g / cm 3 Below, 2.58g / cm 3More than 2.60g / cm 3 Below 2.40g / cm 3 More than 2.58g / cm 3 Below, 2.42g / cm 3 More than 2.58g / cm 3 Below, 2.45g / cm 3 More than 2.58g / cm 3 Below, 2.48g / cm 3 More than 2.58g / cm 3 Below 2.50g / cm 3 More than 2.58g / cm 3 Below, 2.52g / cm 3 More than 2.58g / cm 3 Below 2.55g / cm 3 More than 2.58g / cm 3 Below, 2.40g / cm or more 3 And 2.55g / cm 3 Below, 2.42g / cm 3 More than 2.55g / cm 3 Below, 2.45g / cm 3 More than 2.55g / cm 3 Below, 2.48g / cm 3 More than 2.55g / cm 3 Below 2.50g / cm 3 More than 2.55g / cm 3 Below, 2.52g / cm 3 More than 2.55g / cm 3 Below 2.40g / cm 3 More than 2.52g / cm 3 Below, 2.42g / cm 3 More than 2.52g / cm 3 Below, 2.45g / cm 3 More than 2.52g / cm 3 Below, 2.48g / cm 3 More than 2.52g / cm 3 Below 2.50g / cm 3 More than 2.52g / cm 3 Below 2.40g / cm 3 More than 2.50g / cm 3 Below, 2.42g / cm 3 More than 2.50g / cm3 Below, 2.45g / cm 3 More than 2.50g / cm 3 Below, 2.48g / cm 3 More than 2.50g / cm 3 Below 2.40g / cm 3 More than 2.48g / cm 3 Below, 2.42g / cm 3 More than 2.48g / cm 3 Below, 2.45g / cm 3 More than 2.48g / cm 3 Below 2.40g / cm 3 More than 2.45g / cm 3 Below, 2.42g / cm 3 More than 2.45g / cm 3 or less than 2.40 g / cm 3 More than 2.42g / cm 3 It has the following densities: It is understood that the above ranges include all subranges within the explicitly disclosed ranges.

[0185] final product The glass and glass-ceramic articles disclosed herein can be incorporated into other articles, such as articles with displays (or display articles) (e.g., consumer electronics, including mobile phones, tablets, computers, navigation systems, wearable devices (e.g., watches), etc.), building products, transportation products (e.g., automobiles, trains, aircraft, ships, etc., such as for use in interior display covers, windows, or windshields), consumer electronics products, or any article requiring transparency, scratch resistance, abrasion resistance, or a combination thereof. Exemplary articles incorporating any of the reinforced glass-ceramic articles disclosed herein are shown in Figures 12A and 12B.

[0186] 12A and 12B show a consumer electronic device 200 including a housing 202 having a front side 204, a back side 206, and sides 208; electrical components (not shown) at least partially within or entirely within the housing and including at least a controller, memory, and a display 210 at or adjacent the front side of the housing; and a cover substrate 212 at or on the front side of the housing such that it is above the display. In some embodiments, at least one of the cover substrate 212 or a portion of the housing 202 can include any of the glass-ceramic reinforced articles disclosed herein.

[0187] Thus, various embodiments described herein can be used to produce glass-ceramic articles having superior optical quality and reduced warpage, while not adversely affecting or even improving the stress of the glass-ceramic articles, as compared to glass articles cerammed according to conventional techniques. Such glass-ceramic articles would be particularly well suited for use in portable electronic devices due to their strength capabilities and high transmission values. EXAMPLES

[0188] Various embodiments will be further elucidated by the following examples.

[0189] Working Example Glass precursor compositions were formed by melting the compositions shown in Table 1 below, using a conventional glass melting process:

[0190] [Table 1]

[0191] The glass precursor composition was formed into a 0.6 mm thick glass article and subjected to a heat treatment in which the glass precursor was heated to a nucleation temperature of 575° C. and held for 3 hours, and then the glass precursor was heated to a growth temperature of 735° C. and held for 1 hour. FIG. 6 shows the XRD spectrum of the glass-ceramic, showing mainly petalite and lithium disilicate crystalline phases with a small amount of vergilite. A comparative sample was prepared in a similar manner from the following glass composition:

[0192] [Table 2]

[0193] Example 2 Glass precursors were molded according to Example 1 and subjected to various two-step heat treatments as shown in Table 2 below. The phase assemblages of each sample and comparative sample were measured by XRD and also the haze of 0.6 mm thick polished glass-ceramic articles using a BYK Hazegard I Pro setup. The results are shown in Table 3 below.

[0194] [Table 3]

[0195] Example 3 A glass precursor was formed according to Example 1 and subjected to the three-stage heat treatment shown in Table 4. The phase assemblages of this sample and a comparative sample were determined by XRD.

[0196] [Table 4]

[0197] Example 4 Glass precursors were formed according to Example 1 and subjected to the two-step heat treatment shown in Table 5. The phase assemblages of these comparative samples were measured by XRD. None of the comparative samples in Table 4 had the desired phase assemblages.

[0198] [Table 5]

[0199] Example 5 Glass-ceramics produced according to Sample 1 of Example 2, having thicknesses of 0.5 mm and 0.6 mm, were subjected to chemical strengthening using the ion-exchange conditions shown below in Table 6. The compressive stress (CS), depth of compression (DOC), central tension (CT), CS / CT ratio, and DOC normalized to thickness (i.e., DOC (mm) / thickness (mm)) are provided in Table 5. Comparative Examples 26 and 27 were cerammed at 580° C. for 2 hours and 45 minutes, and then cerammed at 755° C. for 45 minutes.

[0200] [Table 6]

[0201] Figure 7A shows the stress profiles of the glass-ceramics of Comparative Sample 26 and Sample 2, and Figure 7B shows the stress profiles of the glass-ceramics of Comparative Sample 27 and Sample 3. Table 7 shows the data obtained in Figures 7A and 7B.

[0202] [Table 7]

[0203] Figure 7C shows a graph of the central tension of the glass-ceramic measured as a function (square root) of the duration of the ion-exchange treatment. As shown in Figure 7C, the central tension increases with the duration of the ion-exchange process up to a point, after which the central tension begins to decrease; this indicates that while adjusting the duration of the ion-exchange process maximizes the central tension, simply performing the ion-exchange for a longer period does not necessarily achieve maximum central tension.

[0204] Example 6 The damage resistance of Sample 2, Comparative Sample 26, Sample 3, and Comparative Sample 27 was performed using a surface impact device, which was performed using an apparatus that includes a simple pendulum-based dynamic impact test with surfaces ranging from flat to curved. In this test, a specimen of a glass-ceramic article is attached to the bob of a pendulum, which is then used to contact the specimen with a rough impact surface. The apparatus is described in detail in WO 2017 / 100646, which is incorporated herein by reference in its entirety. To perform the test, the specimen is loaded into a holder, then pulled backward from the equilibrium position of the pendulum and released to dynamically impact the impact surface. The results are shown in FIG. 8.

[0205] Example 7 Stress profiles were measured using the glass-ceramics of Sample 3 and Comparative Sample 27 using different ion exchange conditions as shown in Table 8.

[0206] [Table 8]

[0207] The damage resistance of these samples was performed using the surface impact apparatus described in Example 6. The results are shown in FIG.

[0208] Example 8 The effect of ion-exchange temperature and duration on the glass-ceramics of Sample 2 and Sample 3 was tested while maintaining the same ion-exchange media of 60 wt% KNO3, 40 wt% NaNO3 with top-addition of 0.12 wt% LiNO3, 0.5 wt% NaNO2, and 0.5 wt% silicic acid. The ion-exchange temperature and duration, as well as the compressive stress, central tension, and compression depth are shown in Table 9 below.

[0209] [Table 9]

[0210] The stress profiles of sample 3 tempered at 500°C for 8 hours and at 530°C for 4 hours are shown in Figure 10. The ion exchange conditions of the comparative sample were as follows: the bath consisted of 60 wt% KNO3, 40 wt% NaNO3, and 0.12 wt% LiNO3, and was treated at 500°C for 8 hours. Sample 3 was treated in a bath consisting of 60 wt% KNO3, 40 wt% NaNO3, and 0.12 wt% LiNO3, and was treated at 500°C for 8 hours. Sample 3 was also treated in a bath consisting of 60 wt% KNO3, 40 wt% NaNO3, and 0.12 wt% LiNO3, and was treated at 530°C for 4 hours.

[0211] Example 9 A drop test was used to test the durability of the glass ceramics. In the test, sample 2 of Example 8, ion-exchanged at 530°C for 6 hours, was compared to a 0.6 mm thick glass ceramic of comparative composition, ion-exchanged under the same conditions. Sample 3 of Example 8, ion-exchanged at 530°C for 4 hours, was compared to a 0.5 mm thick glass ceramic of comparative composition, ion-exchanged under the same conditions. The samples were mounted in a Corning Clubmehd pack and dropped from a maximum height of 220 cm onto 80 grit sandpaper at 10 cm intervals, and breakage was recorded. In Figure 11, the dashed (dotted) circle represents breakage and the solid circle represents survival.

[0212] Example 10 The test is performed using a cone-spherical diamond tip (angle 90 degrees / radius 10 μm). The tip of the diamond is brought into contact with the surface of the material and a force of 0.05 N is applied, after which the tip is moved 10 mm over the sample while the load is increased from 0.05 N to 1.6 N. Once a scratch is made, the tip is removed from the surface of the material.

[0213] Figure 12A shows the results of a scratch test on a 0.5 mm thick glass-ceramic of Sample 1 that was not chemically strengthened but was cerammed at 575°C for 4 hours and at 735°C for an additional hour, and Figure 12B shows the results of a scratch test on a 0.6 mm thick glass-ceramic of a comparative sample shown in Table 2 that was cerammed at 580°C for 2.75 hours and at 755°C for an additional 0.75 hours.

[0214] It will be apparent to those skilled in the art that various modifications and variations can be made to the embodiments described herein without departing from the spirit and scope of the claimed subject matter. Accordingly, it is intended that the present specification cover modifications and variations of the various embodiments described herein, provided that such modifications and variations come within the scope of the appended claims and their equivalents.

[0215] Preferred embodiments of the present invention will be described below in detail.

[0216] EMBODIMENT 1 1. A glass-ceramic article comprising: SiO2, 65.00% by mass or more and 80.00% by mass or less; More than 4.00% by mass and not more than 12.00% by mass of Al2O3; P2O5, 0.10% by mass or more and 3.5% by mass or less; 8.00% by mass or more and 17.00% by mass or less of Li2O; 4.00% by mass or more and 15.00% by mass or less of ZrO2, and CaO: 0.05% by mass or more and 4.00% by mass or less 1. A glass-ceramic article comprising:

[0217] EMBODIMENT 2 2. The glass-ceramic article of claim 1, having a haze of less than 0.15 as measured on a 0.6 mm thick glass-ceramic article using a Hazegard I Pro Setup.

[0218] EMBODIMENT 3 3. The glass-ceramic article of claim 1 or 2, wherein the glass-ceramic article has a haze of less than 0.12 as measured on a 0.6 mm thick glass-ceramic article using a BYK Hazegard I Pro Setup.

[0219] EMBODIMENT 4 4. The glass-ceramic article of any one of claims 1 to 3, wherein the glass-ceramic article has an average transmittance measured at wavelengths from 450 nm to 800 nm of 85% or greater.

[0220] EMBODIMENT 5 the glass-ceramic article comprising: 30% by mass or more and 50% by mass or less of lithium disilicate, 30% to 50% by mass of petalite, and Less than 5% by mass of the sum of crystalline phases other than lithium disilicate and petalite 5. The glass-ceramic article of any of the preceding claims, comprising:

[0221] EMBODIMENT 6 6. The glass-ceramic article of any one of claims 1 to 5, wherein the glass-ceramic article comprises at least 5% and at most 20% by weight of residual amorphous glass.

[0222] EMBODIMENT 7 7. The glass-ceramic article of any one of claims 1 to 6, wherein the glass-ceramic article has a weight ratio of lithium disilicate to petalite greater than or equal to 0.5 and less than or equal to 1.5.

[0223] EMBODIMENT 8 8. The glass-ceramic article of any of the preceding claims, comprising greater than or equal to 68.00 wt.% and less than or equal to 74.00 wt.% SiO2.

[0224] EMBODIMENT 9 9. The glass-ceramic article of any of the preceding claims, comprising greater than 5.00% and not greater than 9.00% by weight Al2O3.

[0225] EMBODIMENT 10 10. The glass-ceramic article of any of the preceding claims, comprising greater than or equal to 1.00% and less than or equal to 3.00% by weight of P2O5.

[0226] EMBODIMENT 11 11. The glass-ceramic article of any of the preceding claims, comprising greater than or equal to 9.00% and less than or equal to 14.00% by weight LiO.

[0227] EMBODIMENT 12 12. The glass-ceramic article of any of the preceding claims, comprising greater than or equal to 4.50% and less than or equal to 8.00% by weight of ZrO2.

[0228] EMBODIMENT 13 13. The glass-ceramic article of any of the preceding claims, comprising greater than or equal to 0.10 wt.% and less than or equal to 1.00 wt.% CaO.

[0229] EMBODIMENT 14 14. The glass-ceramic article of any of the preceding claims, comprising greater than or equal to 0.01% and less than or equal to 0.5% by weight SnO2.

[0230] EMBODIMENT 15 15. The glass-ceramic article of any one of the preceding claims, wherein the glass-ceramic article has a thickness of at least 0.1 mm and at most 2.0 mm.

[0231] EMBODIMENT 16 16. The glass-ceramic article of any one of the preceding claims, wherein the glass-ceramic article has a thickness of at least 0.1 mm and at most 1.0 mm.

[0232] EMBODIMENT 17 1. An electronic device comprising: Housing, display, A cover substrate adjacent to the display comprising the glass-ceramic article of any one of claims 1 to 16. An electronic device comprising:

[0233] EMBODIMENT 18 1. A reinforced glass-ceramic article comprising: A first surface, A second surface, and A thickness t extending from the first surface to the second surface Including, the reinforced glass-ceramic article having a surface compressive stress on the first surface; the stress transitions from compressive to tensile at a depth of greater than or equal to 0.15t and less than or equal to 0.25t, measured from the first surface toward the centerline of the reinforced glass-ceramic article; and the reinforced glass-ceramic article has a maximum central tension mCT, and the absolute value of the surface compressive stress, measured at the first surface, is 1.5 mCT or more and 2.5 mCT or less; Reinforced glass-ceramic articles.

[0234] EMBODIMENT 19 19. The reinforced glass-ceramic article of claim 18, wherein the compressive stress decreases as a linear function from a thickness of 0.07t or greater to a thickness of 0.26t as a thickness increases, as measured from the first surface of the reinforced glass-ceramic article to the centerline of the reinforced glass-ceramic article.

[0235] EMBODIMENT 20 20. The reinforced glass-ceramic article of claim 18 or 19, wherein the reinforced glass-ceramic article has a compressive stress of at least 250 MPa and at most 400 MPa.

[0236] EMBODIMENT 21 21. The reinforced glass-ceramic article of any one of claims 18 to 20, wherein the reinforced glass-ceramic article has a compressive stress of 300 MPa or more and 400 MPa or less.

[0237] EMBODIMENT 22 22. The reinforced glass-ceramic article of any one of claims 18 to 21, wherein the reinforced glass-ceramic article has a central tension of at least 100 MPa and at most 170 MPa.

[0238] EMBODIMENT 23 23. The reinforced glass-ceramic article of any one of claims 18 to 22, wherein the reinforced glass-ceramic article has a central tension of at least 140 MPa and at most 170 MPa.

[0239] EMBODIMENT 24 The reinforced glass-ceramic article has a resistance of 22 J / m 2 More than 60 J / m 2 24. The reinforced glass-ceramic article of any of claims 18 to 23, having a stored strain energy of:

[0240] EMBODIMENT 25 23. The reinforced glass-ceramic article of any of claims 18 to 22, wherein the reinforced glass-ceramic article has a fracture toughness of 1.0 MPa√m or more and 2.0 MPa√m or less.

[0241] EMBODIMENT 26 24. The reinforced glass-ceramic article of any of claims 18 to 23, wherein the reinforced glass-ceramic article has a haze of less than 0.15 as measured on a 0.6 mm thick glass-ceramic article using a BYK Hazegard I Pro Setup.

[0242] EMBODIMENT 27 The reinforced glass-ceramic article has a toughness of 2.40 g / cm 3 More than 2.60g / cm 3 27. The reinforced glass-ceramic article of any of claims 18 to 26, having a density of:

[0243] EMBODIMENT 28 28. The reinforced glass-ceramic article of any of claims 18 to 27, wherein the reinforced glass-ceramic article has a fracture strength of 350 MPa or more and 450 MPa or less, measured on a glass-ceramic article having a thickness of 0.6 mm using 80 grit.

[0244] EMBODIMENT 29 the reinforced glass-ceramic article comprising: Maximum compressive stress is between 300MPa and 400MPa. A maximum central tension of 120 MPa or more and 170 MPa or less, and A fracture stress of 450 MPa or more and 550 MPa or less, measured on a reinforced glass-ceramic article having a thickness of 0.6 mm. 28. The reinforced glass-ceramic article of any of claims 18 to 27, having a structure comprising:

[0245] EMBODIMENT 30 the reinforced glass-ceramic article comprising: SiO2, 65.00% by mass or more and 80.00% by mass or less; 8.00% by mass or more and 17.00% by mass or less of Li2O, and 4.00% by mass or more and 15.00% by mass or less ZrO2 30. The reinforced glass-ceramic article of any one of claims 18 to 29, comprising at its center.

[0246] EMBODIMENT 31 31. The reinforced glass-ceramic article of any one of claims 18 to 30, wherein the reinforced glass-ceramic article comprises greater than 4.00% and less than or equal to 12.00% by weight Al2O3 at its center.

[0247] EMBODIMENT 32 32. The reinforced glass-ceramic article of any one of claims 18 to 31, wherein the reinforced glass-ceramic article comprises, at its center, greater than or equal to 0.10% and less than or equal to 3.5% by weight P2O5.

[0248] EMBODIMENT 33 33. The reinforced glass-ceramic article of any of claims 18 to 32, wherein the reinforced glass-ceramic article comprises, at its center, equal to or greater than 0.05% and equal to or less than 4.00% by weight CaO.

[0249] EMBODIMENT 34 34. The reinforced glass-ceramic article of any of embodiments 18 to 33, comprising at its center, greater than or equal to 68.00% and less than or equal to 74.00% by weight of SiO2.

[0250] EMBODIMENT 35 35. The reinforced glass-ceramic article of any one of embodiments 18 to 34, comprising greater than 5.00% and not greater than 9.00% by weight Al2O3 in its center.

[0251] EMBODIMENT 36 36. The reinforced glass-ceramic article of any one of embodiments 18 to 35, comprising, in its center, greater than or equal to 1.00% and less than or equal to 3.00% by weight P2O5.

[0252] EMBODIMENT 37 37. The reinforced glass-ceramic article of any one of embodiments 18 to 36, comprising at least 9.00% and at most 14.00% by weight LiO in its center.

[0253] EMBODIMENT 38 38. The reinforced glass-ceramic article of any one of embodiments 18 to 37, comprising, in its center, greater than or equal to 4.50% and less than or equal to 8.00% by weight of ZrO2.

[0254] EMBODIMENT 39 39. The reinforced glass-ceramic article of any one of embodiments 18 to 38, comprising, in its center, equal to or greater than 0.10% and equal to or less than 1.00% by weight CaO.

[0255] EMBODIMENT 40 40. The reinforced glass-ceramic article of any one of embodiments 18 to 39, comprising, in its center, at least 0.01% and at most 0.5% by weight SnO2.

[0256] EMBODIMENT 41 the reinforced glass-ceramic article comprising: 30% by mass or more and 50% by mass or less of lithium disilicate, 30% to 50% by mass of petalite, and Less than 3% by mass of the sum of crystalline phases other than lithium disilicate and petalite 41. The reinforced glass-ceramic article of any of claims 18 to 40, comprising:

[0257] EMBODIMENT 42 42. The reinforced glass-ceramic article of any one of claims 18 to 41, wherein the reinforced glass-ceramic article comprises at least 5% and at most 20% by weight of residual amorphous glass.

[0258] EMBODIMENT 43 43. The reinforced glass-ceramic article of any of claims 18 to 42, wherein the reinforced glass-ceramic article has a weight ratio of lithium disilicate to petalite greater than or equal to 0.5 and less than or equal to 1.5.

[0259] EMBODIMENT 44 44. The reinforced glass-ceramic article of any of claims 18 to 43, wherein the reinforced glass-ceramic article has a haze of less than 0.15 as measured on a 0.6 mm thick glass-ceramic article using a BYK Hazegard I Pro Setup.

[0260] EMBODIMENT 45 45. The reinforced glass-ceramic article of any of claims 18 to 44, wherein the reinforced glass-ceramic article has a haze of less than 0.12 as measured on a 0.6 mm thick glass-ceramic article using a BYK Hazegard I Pro Setup.

[0261] EMBODIMENT 46 46. ​​The reinforced glass-ceramic article of any one of claims 18 to 45, wherein the reinforced glass-ceramic article has an average transmittance measured at wavelengths from 450 nm to 800 nm of 85% or greater.

[0262] EMBODIMENT 47 47. The reinforced glass-ceramic article of any one of claims 18 to 46, wherein the reinforced glass-ceramic article has a thickness of at least 0.1 mm and at most 2.0 mm.

[0263] EMBODIMENT 48 48. The reinforced glass-ceramic article of any one of claims 18 to 47, wherein the reinforced glass-ceramic article has a thickness of at least 0.1 mm and at most 1.0 mm.

[0264] EMBODIMENT 49 1. An electronic device comprising: Housing, display, A cover substrate adjacent to the display comprising the reinforced glass-ceramic article of any of claims 18 to 48. An electronic device comprising:

[0265] EMBODIMENT 50 1. A method of forming a glass-ceramic, comprising: heating the precursor glass composition to a nucleation temperature, said nucleation temperature being equal to or greater than 550° C. and equal to or less than 650° C.; holding the precursor glass composition at a temperature in the range of greater than or equal to the nucleation temperature and less than or equal to 650° C. for a first period of time to form a nucleated precursor glass composition; heating the nucleation precursor glass composition to a growth temperature, the growth temperature being equal to or greater than 680° C. and equal to or less than 800° C.; and holding the nucleation precursor glass composition at a temperature in the range of greater than or equal to the growth temperature and less than or equal to 800° C. for a second period of time to form the glass ceramic. A method comprising:

[0266] EMBODIMENT 51 51. The method of embodiment 50, wherein the first period of time and the second period of time are each equal to or greater than 1 minute and equal to or less than 240 minutes.

[0267] EMBODIMENT 52 52. The method of claim 50 or 51, wherein holding the precursor glass composition at a temperature in the range of greater than or equal to the nucleation temperature and less than or equal to 650° C. for a first period of time comprises isothermal holding at the nucleation temperature for the first period of time.

[0268] EMBODIMENT 53 53. The method of any of claims 50 to 52, wherein holding the nucleation precursor glass composition at a temperature in the range of greater than or equal to the growth temperature and less than or equal to 800°C for a second period of time comprises isothermal holding at the growth temperature for the second period of time.

[0269] EMBODIMENT 54 54. The method of any of claims 50 to 53, wherein holding the precursor glass composition at a temperature in the range of greater than or equal to the nucleation temperature and less than or equal to 650°C for a first period of time comprises heating the precursor glass composition to a temperature from the nucleation temperature to less than or equal to 650°C for the first period of time.

[0270] EMBODIMENT 55 55. The method of any of claims 50 to 54, wherein holding the nucleation precursor glass composition at a temperature in the range of greater than or equal to the growth temperature and less than or equal to 800°C for a second period of time comprises heating the nucleation precursor glass composition from the growth temperature to a temperature less than or equal to 800°C for the second period of time.

[0271] EMBODIMENT 56 56. The method of any of claims 50 to 55, wherein the steps of heating a precursor glass composition to a nucleation temperature, the nucleation temperature being 550°C or more and 650°C or less, and heating the nucleation precursor glass composition to a growth temperature, the growth temperature being 680°C or more and 800°C or less, are performed at a heating rate of the precursor glass composition and the nucleation precursor glass composition of 0.1°C / min or more and 50°C / min or less.

[0272] EMBODIMENT 57 exposing the glass-ceramic to an ion-exchange medium comprising molten potassium salts, molten sodium salts, and molten lithium salts to form a strengthened glass-ceramic. 57. The method of any of embodiments 50 to 56, further comprising:

[0273] EMBODIMENT 58 The ion exchange medium is 50% by mass or more and 70% by mass or less of KNO3, 30% by mass or more and 50% by mass or less of NaNO3, and LiNO3: 0.05% by mass or more and 0.15% by mass or less 58. The method of embodiment 57, comprising:

[0274] EMBODIMENT 59 59. The method of embodiment 57 or 58, wherein the ion exchange medium comprises greater than or equal to 0.08 wt. % and less than or equal to 0.12 wt. % LiNO3.

[0275] EMBODIMENT 60 60. The method of any one of embodiments 57 to 59, wherein the ion exchange medium further comprises NaNO2 and silicic acid.

[0276] EMBODIMENT 61 the temperature of the ion exchange medium during exposure to the glass ceramic is greater than or equal to 450° C. and less than or equal to 550° C.; and The glass ceramic is exposed to the ion exchange medium for a period of at least 1 hour and not more than 16 hours. The method of any one of embodiments 57 to 60.

[0277] EMBODIMENT 62 1. A glass article comprising: SiO2, 65.00% by mass or more and 80.00% by mass or less; More than 4.00% by mass and not more than 12.00% by mass of Al2O3; P2O5, 0.10% by mass or more and 3.5% by mass or less; 8.00% by mass or more and 17.00% by mass or less of Li2O; 4.00% by mass or more and 15.00% by mass or less of ZrO2, and CaO: 0.05% by mass or more and 4.00% by mass or less 1. A glass-ceramic article comprising at its center.

[0278] EMBODIMENT 63 63. The glass article of embodiment 62, comprising at its center greater than or equal to 68.00% and less than or equal to 74.00% by weight of SiO2.

[0279] EMBODIMENT 64 64. The glass article of embodiment 62 or 63, comprising greater than 5.00% and not greater than 9.00% by weight Al2O3 in its center.

[0280] EMBODIMENT 65 65. A glass article according to any one of claims 62 to 64, comprising at least 1.00% and at most 3.00% by weight P2O5 in its center.

[0281] EMBODIMENT 66 66. A glass article according to any one of claims 62 to 65, comprising at least 9.00% and at most 14.00% by weight LiO in its center.

[0282] EMBODIMENT 67 67. A glass article according to any one of claims 62 to 66, comprising at least 4.50% and at most 8.00% by weight ZrO2 in its center.

[0283] EMBODIMENT 68 68. A glass article according to any one of claims 62 to 67, comprising at least 0.10% and at most 1.00% by weight CaO in its center.

[0284] EMBODIMENT 69 69. A glass article according to any one of claims 62 to 68, comprising at least 0.01% and at most 0.5% by weight SnO2 in its center.

[0285] EMBODIMENT 70 70. The glass article of any of claims 62 to 69, wherein the glass-ceramic article has a haze of less than 0.15 as measured on a 0.6 mm thick glass-ceramic article using a BYK Hazegard I Pro Setup.

[0286] EMBODIMENT 71 71. The glass article of any of claims 62 to 70, wherein the glass-ceramic article has a haze of less than 0.12 as measured on a 0.6 mm thick glass-ceramic article using a BYK Hazegard I Pro Setup.

[0287] EMBODIMENT 72 72. The glass article of any one of claims 62 to 71, wherein the glass-ceramic article has an average transmission of 85% or greater.

[0288] EMBODIMENT 73 73. The glass article of any one of claims 62 to 72, wherein the glass article has a thickness of greater than or equal to 0.1 mm and less than or equal to 2.0 mm.

[0289] EMBODIMENT 74 74. The glass article of any one of claims 62 to 73, wherein the glass article has a thickness of at least 0.1 mm and at most 1.0 mm.

[0290] EMBODIMENT 75 1. An electronic device comprising: Housing, display, A cover substrate adjacent to the display comprising the glass article of any of claims 62 to 74. An electronic device comprising: [Explanation of symbols]

[0291] 10 Device Drop Machine 12 Chuck 14 Chuck jaws 16 Pack 18 Falling surface 100 Reinforced glass-ceramic articles 102 First Surface 104 Second Surface 106 Compressive Stress (CS) Layer 108 Compressive Stress (CS) Layer 110 Central tension region 200 Consumer Electronics 202 Case 204 Front 206 Back 208 Side 210 Display 212 Cover board

Claims

1. 1. A glass-ceramic article comprising: 65.00% by mass or more and 80.00% by mass or less of SiO 2 , Al: more than 4.00 mass% and not more than 12.00 mass% 2 O 3 , 0.10% by mass or more and 3.5% by mass or less P 2 O 5 , Li of 8.00% by mass or more and 17.00% by mass or less 2 O. 4.00% by mass or more and 15.00% by mass or less ZrO 2 , and 0.05% by mass or more and 4.00% by mass or less of CaO 1. A glass-ceramic article comprising:

2. 10. The glass-ceramic article of claim 1, wherein the glass-ceramic article has a haze of less than 0.15 as measured on a 0.6 mm thick glass-ceramic article using a BYK Hazegard I Pro Setup.

3. 10. The glass-ceramic article of claim 1, wherein the glass-ceramic article has a haze of less than 0.12 as measured on a 0.6 mm thick glass-ceramic article using a BYK Hazegard I Pro Setup.

4. 4. The glass-ceramic article of claim 1, wherein the glass-ceramic article has an average transmission of 85% or greater measured at wavelengths from 450 nm to 800 nm.

5. the glass-ceramic article comprising: 30% by weight or more and 50% by weight or less of lithium disilicate, 30% to 50% by weight of petalite, and Less than 5% by weight of the sum of crystalline phases other than lithium disilicate and petalite 4. The glass-ceramic article of claim 1 , comprising:

6. 4. The glass-ceramic article of claim 1, wherein the glass-ceramic article comprises at least 5% and at most 20% by weight of residual amorphous glass.

7. 4. The glass-ceramic article of claim 1, wherein the glass-ceramic article has a weight ratio of lithium disilicate to petalite greater than or equal to 0.5 and less than or equal to 1.

5.

8. P: 1.00% by mass or more and 3.00% by mass or less 2 O 5 , Li of 9.00% by mass or more and 14.00% by mass or less 2 O. 0.10% by mass or more and 1.00% by mass or less of CaO, and 4.50% by mass or more and 8.00% by mass or less ZrO 2 4. The glass-ceramic article of claim 1 , comprising:

9. 4. The glass-ceramic article of claim 1, wherein the glass-ceramic article has a thickness of greater than or equal to 0.1 mm and less than or equal to 2.0 mm.

10. 1. An electronic device comprising: Housing, display, A cover substrate adjacent to the display comprising the glass-ceramic article of any one of claims 1 to 3. An electronic device comprising:

Citation Information

Patent Citations

  • Glass material and preparation method and product thereof

    CN113200678A

  • Highly fracture-resistant glass-ceramic articles and methods for their manufacture - Patents.com

    JP2021512835A

Cited By

  • Glass-ceramic

    WO2026211598A1