Fabric for protective clothing, and protective clothing for infection prevention formed with the fabric
By using a non-permeable breathable waterproof film composed of polyester-polyether-based resin, combined with slip agent and nonwoven fabric lamination, the problem of insufficient breathability in the prior art is solved, and protective clothing with high breathability and waterproofness is achieved.
Patent Information
- Application Number
- JP2023121176
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-07-26
- Publication Date
- 2025-02-06
AI Technical Summary
Although the non-permeable breathable polyurethane film in the prior art has good barrier properties, it is easy to accumulate sweat when worn, resulting in insufficient breathability.
A non-permeable breathable waterproof film consisting mainly of polyester-polyether-based resin is used, combined with a polyester-polyether block copolymer, and a slip agent is added therein to form a non-permeable breathable waterproof film for lamination with non-woven fabrics to improve breathability and manufacturing efficiency.
It achieves high breathability and water resistance, while improving manufacturing efficiency, avoiding the problem of sweat accumulation, and is suitable for protective clothing in medical environments.
Smart Images

Figure 2025017869000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a fabric for protective clothing and to a protective clothing for preventing infection formed from this fabric. [Background technology]
[0002] Patent Document 1 describes a protective suit for preventing infection used in medical settings that uses a composite sheet formed by laminating a nonwoven fabric in which the constituent fibers are partially heat-bonded together, the constituent fibers being core-sheath composite fibers having a core made of polyethylene terephthalate and a sheath made of polyethylene, and a nonporous moisture-permeable polyurethane film. The nonporous moisture-permeable polyurethane film is imparted with moisture permeability by introducing hydrophilic groups into the polyurethane resin structure. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Utility Model Registration No. 3190510 Summary of the Invention [Problem to be solved by the invention]
[0004] However, the protective clothing using the nonporous moisture-permeable polyurethane film described in Patent Document 1 has good barrier properties, but even though it is breathable, sweat may still be trapped when worn, and there is room for further improvement in breathability, i.e., moisture permeability.
[0005] An object of the present invention is to provide a fabric having improved moisture permeability that is used for protective clothing worn in medical settings, with good manufacturability. [Means for solving the problem]
[0006] To achieve this objective, the fabric of the protective clothing of the present invention is characterized in that a nonwoven fabric is laminated on at least one side of a non-porous moisture-permeable waterproof film composed of a polyester-polyether resin composition having a polyester-polyether block copolymer as its main component, and the polyester-polyether resin composition contains a slip agent.
[0007] In this configuration, the non-porous moisture-permeable waterproof film is a non-porous moisture-permeable waterproof film mainly composed of a polyester-polyether resin composition, and therefore can exhibit good moisture permeability. Moreover, since the non-porous moisture-permeable waterproof film contains a slip agent, it can be smoothly formed into a film even though it uses a polyester-polyether block copolymer having adhesive properties, and therefore the fabric for protective clothing can be obtained with good manufacturability.
[0008] According to the protective clothing fabric of the present invention, it is preferred that the slip agent is a fatty acid amide.
[0009] According to the fabric of the protective suit of the present invention, it is preferred that the fatty acid amide is oleic acid amide. According to the fabric for protective clothing of the present invention, it is preferable that the polyester-polyether resin composition contains polyethylene.
[0010] According to the fabric of the protective clothing of the present invention, it is preferable that the polyester-polyether resin composition constituting the non-porous moisture-permeable waterproof film contains fatty acid amide and polyethylene in a dispersed state in a polyester-polyether block copolymer.
[0011] According to the fabric for protective clothing of the present invention, it is preferable that the polyester-polyether resin composition contains 0.03 to 0.10% by mass of fatty acid amide.
[0012] According to the protective suit fabric of the present invention, it is preferable that the nonwoven fabric is composed of a laminated nonwoven fabric in which a spunbonded nonwoven fabric is laminated on both sides of a meltblown nonwoven fabric.
[0013] According to the protective suit fabric of the present invention, it is preferable that the meltblown nonwoven fabric is colored.
[0014] According to the protective suit fabric of the present invention, it is preferable that the non-porous moisture-permeable waterproof film and the nonwoven fabric are bonded to each other by a hot melt resin.
[0015] The method for producing a fabric for protective clothing of the present invention is characterized in that, when producing a fabric for protective clothing, a polyester-polyether resin composition containing an added slip agent is prepared, this resin composition is formed into a film, and a nonwoven fabric is laminated on at least one side of the obtained film.
[0016] Another method for producing a fabric for protective clothing of the present invention includes the steps of: A master batch is prepared by melt-mixing a fatty acid amide, which is a slip agent, with polyethylene. A predetermined amount of the master batch and a polyester-polyether block copolymer are mixed and melt-kneaded to prepare a polyester-polyether resin composition in which an aliphatic amide and polyethylene are dispersed in the polyester-polyether block copolymer; This resin composition is formed into a film, The method is characterized in that a nonwoven fabric is laminated on at least one surface of the obtained film.
[0017] The infection-preventing protective clothing of the present invention is characterized in that it is made of the protective clothing fabric of the present invention. Effect of the Invention
[0018] According to the present invention, the non-porous moisture-permeable waterproof film is a polyester-polyether-based non-porous moisture-permeable waterproof film, and therefore exhibits good moisture permeability. Moreover, since the polyester-polyether-based non-porous moisture-permeable waterproof film contains a slip agent, it can be smoothly formed into a film and fabric can be manufactured even though a polyester-polyether block copolymer having adhesive properties is used. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0019] The fabric of the protective suit of the present invention is a polyester / polyether non-porous moisture-permeable waterproof film with a nonwoven fabric laminated on at least one side thereof.
[0020] The non-porous moisture-permeable waterproof film is formed of a polyester-polyether resin mainly composed of a polyester-polyether block copolymer. The polyester-polyether block copolymer is a polymer having a structural unit composed of an aromatic polyester and a structural unit composed of an aliphatic polyether. In particular, it is preferable that the aromatic polyester is polytetramethylene terephthalate and the aliphatic polyether is polyalkylene ether terephthalate. By block-copolymerizing the aliphatic polyether, the film is non-porous without pores, but can still exhibit the required moisture permeability. As a polyester-polyether resin mainly composed of such a polyester-polyether block copolymer, specifically, a resin commercially available under the name "Arnitel" from DCM can be preferably used.
[0021] Polyester-polyether resins contain slip agents. As slip agents, fatty acid amides are preferably used, and oleic acid amide is particularly suitable. It is preferable to melt-mix oleic acid amide with polyethylene into polyester-polyether block copolymers. This is because melt-mixing oleic acid amide with polyethylene into polyester-polyether block copolymers improves dispersibility and mixability with the polyester-polyether block copolymers.
[0022] That is, the polyester-polyether resin composition containing oleic acid amide thus obtained has oleic acid amide dispersed well in the resin composition, and therefore exhibits uniform slip properties without unevenness. At the same time, the polyester-polyether resin composition also contains the above-mentioned polyethylene.
[0023] The content of oleic acid amide in the polyester-polyether resin composition containing oleic acid amide is preferably 0.03 to 0.10% by mass. By containing oleic acid amide in this range, good slip properties can be exhibited and good film formation can be achieved. The more preferred content is 0.05 to 0.10% by mass.
[0024] Polyester-polyether block copolymer is an elastomeric resin. Therefore, if the oleic acid amide content falls below 0.03% by mass, it becomes difficult to form the film, and problems such as poor manufacturability and low yield rate occur. On the other hand, even if the oleic acid amide content exceeds 0.10% by mass, no further improvement in slip properties is observed.
[0025] In other words, since the polyester-polyether block copolymer is an elastomeric resin as described above, if no measures are taken, even if the resin is melted and then used to produce a film, the molten resin will adhere to various parts of the film production equipment, making it difficult to carry out a good film formation process. In contrast, by adding a slip agent, such as a fatty acid amide, to the polyester-polyether block copolymer as in the present invention, the slip properties of the resin can be improved, and accidents such as the molten resin adhering to various parts of the film production equipment can be prevented. This allows the protective clothing fabric of the present invention to be produced with good manufacturability.
[0026] By melt-mixing the slip agent oleic acid amide with polyethylene into a polyester-polyether resin, the compatibility between the polyester-polyether block copolymer and the fatty acid amide can be improved, thereby improving the dispersibility and mixability of the fatty amide in the polyester-polyether block copolymer as described above.
[0027] More specifically, a master batch is prepared by melt-mixing a fatty acid amide, which serves as a slip agent, with polyethylene. A predetermined amount of this master batch is then mixed with a polyester-polyether block copolymer and melt-kneaded to prepare a polyester-polyether resin composition in which the fatty amide and polyethylene are dispersed in the polyester-polyether block copolymer, and this resin composition is then formed into a film.
[0028] Generally, a masterbatch is a mixture of various additives, colorants, and other compounding agents in a certain ratio at a high concentration, and the use of a masterbatch has the effect of enabling good dispersion and mixing. In the masterbatch, the resin into which the slip agent, an additive, is mixed is always the resin that is the main component of the film. However, the present invention is characterized in that, instead of using the polyester-polyether block copolymer or polyester resin that is the main component of the film as the resin for the masterbatch, polyethylene is used. The mixing ratio of fatty acid amide to polyethylene in the masterbatch is preferably (fatty acid amide):(polyethylene)=1:99 to 5:95 by mass.
[0029] From the viewpoint of comfort and required performance of protective clothing manufactured using a fabric containing this nonporous moisture-permeable waterproof film, the nonporous moisture-permeable waterproof film preferably has a thickness of 5 to 50 μm, and more preferably 10 to 25 μm.
[0030] From the viewpoint of the moisture permeability of the fabric, the non-porous moisture-permeable waterproof film has a water vapor transmission rate (moisture permeability) of 2000 to 10000 g / m2, measured by the method A-1 specified in JIS L-1099-2012. 2 It is preferable that the durability is 2000 to 20000 mm when measured in accordance with JIS L-1092·2020.
[0031] From the viewpoint of barrier properties of the fabric, it is preferable that the non-porous moisture-permeable waterproof film has a blood barrier property of "Class 6" as specified in JIS T8122-2015 when tested according to "Procedure B" specified in JIS T8060-2015, and a virus barrier property of "Class 6" as specified in JIS T8122-2015 when tested according to "Procedure B" specified in JIS T 8061-2015.
[0032] Similarly, from the viewpoint of barrier properties of the fabric, it is preferable that the non-porous moisture-permeable waterproof film has a blood barrier property of "compliant: no penetration or wet marks" when tested by "Method B" specified in ASTM F1670, and a virus barrier property of "passed: phage count (PFU / ml) < 1" when tested by "Method B" specified in ASTM F1670.
[0033] This section explains nonwoven fabrics. Nonwoven fabrics are the building blocks for the fabric of protective clothing, including nonporous, breathable, waterproof films made primarily of polyester-polyether block copolymers.
[0034] Any nonwoven fabric may be used as long as it is capable of forming a protective clothing fabric. In particular, a laminated nonwoven fabric having a spunbonded nonwoven fabric laminated on both sides of a meltblown nonwoven fabric is particularly suitable as the outer surface of the fabric.
[0035] Since the fabric for protective clothing is used as clothing material, it is preferable that it is appropriately colored. Meltblown nonwoven fabrics are generally finely woven nonwoven fabrics made of ultrafine fibers and have high uniformity, so they have the advantage of being easily colorable and less prone to color unevenness.
[0036] As described above, meltblown nonwoven fabrics are generally finely woven fabrics made of ultrafine fibers, and therefore are too soft and difficult to handle as a component of protective clothing fabrics. Therefore, by laminating spunbond nonwoven fabrics on both sides of the meltblown nonwoven fabric, these spunbond nonwoven fabrics can be made to have the self-supporting properties as a component of protective clothing fabrics.
[0037] From the above viewpoint, the meltblown nonwoven fabric is a fabric obtained by the meltblown method, the constituent fibers of which are formed from thermoplastic resins such as polypropylene and polyester, the fiber diameter of which is in the range of about 1 to 8 μm, and the basis weight of the nonwoven fabric is 3 to 8 g / m. 2 It is preferable that:
[0038] In the spunbond nonwoven fabric, the constituent fibers obtained by melt spinning are formed from thermoplastic resins such as polypropylene and polyester, and the single fiber fineness is preferably 2 to 5 dtex. The melt-spun constituent fibers are bonded to each other by heat fusion or the like to form a nonwoven fabric. The basis weight of one of the nonwoven fabrics laminated on both sides of the meltblown nonwoven fabric is 7 to 15 g / m 2 The total weight of both sides is preferably 15 to 25 g / m 2 From the viewpoint of flexibility, it is preferable that the meltblown nonwoven fabric and the spunbonded nonwoven fabric laminated on both sides thereof are both made of polypropylene fibers.
[0039] The meltblown nonwoven fabric and the pair of spunbond nonwoven fabrics on the front and back can be laminated and integrated by, for example, a heat-pressure bonding process, in which the constituent fibers of the meltblown nonwoven fabric or the constituent fibers of the spunbond nonwoven fabric are softened and melted. The conditions for the heat-pressure bonding process for this purpose can be set appropriately. In addition, the meltblown nonwoven fabric and the spunbond nonwoven fabric can be integrated by softening and melting by manufacturing them in a continuous process. A laminated nonwoven fabric comprising a meltblown nonwoven fabric and a pair of spunbond nonwoven fabrics on the front and back that meets the above-mentioned conditions has a dense structure, and is therefore particularly excellent as a material for protective clothing fabrics.
[0040] The thus-produced laminated nonwoven fabric is placed on one or both sides of the nonporous moisture-permeable waterproof film, and then thermally bonded using, for example, a hot melt resin to obtain the fabric for the protective clothing of the present invention. For example, when the laminated nonwoven fabric is a polypropylene nonwoven fabric, the hot melt resin is preferably one containing synthetic rubber as a main component, but an olefin-based hot melt resin or an ethylene vinyl acetate-based hot melt resin may also be used.
[0041] When a laminated nonwoven fabric of a meltblown nonwoven fabric and a pair of spunbond nonwoven fabrics on the front and back is placed on one side of the nonporous moisture-permeable waterproof film, the laminated nonwoven fabric can function as the outer fabric of the protective clothing by coloring the meltblown nonwoven fabric. In this case, the other side of the nonporous moisture-permeable waterproof film becomes the lining, so coloring treatment is not necessary, and therefore it is advisable to form it from a single layer of spunbond nonwoven fabric, for example. Of course, there is no problem even if a laminated nonwoven fabric of a meltblown nonwoven fabric and a pair of spunbond nonwoven fabrics on the front and back are placed on both sides of the nonporous moisture-permeable waterproof film.
[0042] The protective clothing fabric of the present invention exhibits the same water vapor transmission rate, water pressure resistance, blood barrier property, and virus barrier property as the nonporous moisture-permeable waterproof film described above, because the nonwoven fabric laminated to the nonporous moisture-permeable waterproof film is a material for establishing the fabric, but does not contribute to these properties, and does not have any effect on these properties exhibited by the nonporous moisture-permeable waterproof film.
[0043] That is, from the viewpoint of moisture permeability, the fabric of the protective suit of the present invention has a water vapor transmission rate of 2000 to 10000 g / m2 as measured by the method A-1 specified in JIS L-1099-2012, similar to the non-porous moisture-permeable waterproof film. 2 It is preferable that the water pressure resistance measured in accordance with JIS L-1092-2020 is 2000 to 20000 mm.
[0044] Furthermore, from the viewpoint of barrier properties, like the nonporous moisture-permeable waterproof film, it is preferable that the fabric of the protective clothing of the present invention has a blood barrier property of "Class 6" as specified in JIS T8122-2015 when tested according to "Procedure B" specified in JIS T8060-2015, and a virus barrier property of "Class 6" as specified in JIS T8122-2015 when tested according to "Procedure B" specified in JIS T 8061-2015.
[0045] Similarly, from the viewpoint of barrier properties, the fabric of the protective clothing of the present invention, like the nonporous moisture-permeable waterproof film, is preferably such that the blood barrier property tested by "Method B" specified in ASTM F1670 is "compliant: no penetration or wet marks" and the virus barrier property tested by "Method B" specified in ASTM F1670 is "passed: phage count (PFU / ml)<1".
[0046] According to the present invention, by using the above-mentioned protective suit fabric, it is possible to obtain protective suit having excellent performance in all of moisture permeability, water pressure resistance, blood barrier property, and virus barrier property, and the manufacturability thereof is good. EXAMPLES
[0047] Various physical properties in the following Examples and Comparative Examples were measured by the following methods.
[0048] (1) Moisture permeability of non-porous moisture-permeable waterproof film (g / m 2 24h) The moisture permeability was determined according to the A-1 method of JIS L1099. Measurements were carried out on three samples, and the average value was taken as the moisture permeability.
[0049] (2) Water pressure resistance of non-porous breathable waterproof film (mmH2O) Measurement was performed according to JIS L1092, Method B (high water pressure method). Taking into account the properties of the film, the water pressure resistance was measured using a perforated plate (JIS K6404-3).
[0050] (3) Blood barrier properties The test was conducted according to ASTM F1670 / F1670M-17a Method B. The blood barrier properties were evaluated by visually checking whether artificial blood had penetrated the material. Specifically, the cases where there was no penetration or wet marks were evaluated as "◯: Passed", and the cases where there was penetration were evaluated as "×: Failed".
[0051] (4) Virus barrier properties The test was conducted according to ASTM F1671 / F1671M-13 Method B. The virus barrier properties were evaluated by visual inspection of the presence or absence of penetration of the phage suspension. Specifically, the phage count (PFU / ml) < 1 was evaluated as "Good: Passed," and the phage count (PFU / ml) ≥ 1 was evaluated as "Poor: Failed."
[0052] (5) Film thickness Measurements were taken using a Peacock instrument.
[0053] (6) Film weight Measurements were performed based on JIS P8124.
[0054] Example 1 A non-porous moisture-permeable waterproof film was manufactured as follows. A polyester-polyether block copolymer (commercially available from DCM under the name "Arnitel") was prepared. To this resin, 3% by mass of a master batch obtained by melt-mixing oleic acid amide and polyethylene as a slip agent in a mass ratio of (oleic acid amide):(polyethylene) = 2:98 was added and melt-mixed. The molten mixture was then extruded through a T-die to produce a film with a thickness of 15 μm and a basis weight of 18 g / m. 2 Thus, a non-stretched, non-porous, moisture-permeable, waterproof film was produced.
[0055] The obtained non-porous moisture-permeable waterproof film contained 0.06% by mass of oleic acid amide as a slip agent and 2.94% by mass of polyethylene. As a result, although the film was mainly composed of polyester-polyether resin with elastomeric properties, no problems such as adhesion to the manufacturing equipment occurred during film production. The obtained film had polyethylene and oleic acid amide as a slip agent well dispersed in the main polyester-polyether resin.
[0056] The following laminated nonwoven fabric was manufactured as a first nonwoven fabric to be laminated as a surface layer on a nonporous moisture-permeable waterproof film. That is, a spunbond nonwoven fabric (polypropylene continuous fiber single fiber fineness 3 dtex, basis weight 10 g / m) was manufactured by melt spinning continuous fibers obtained by the spunbond method using polypropylene into a web shape. 2 Then, on this spunbonded nonwoven fabric, a meltblown nonwoven fabric (single fiber diameter of constituent fibers: about 1 to 7 μm, basis weight: 5 g / m) was obtained by meltblown method using polypropylene with blue pigment mixed therein. 2 Then, a spunbonded nonwoven fabric (polypropylene continuous fiber single fiber fineness 3 dtex, basis weight 10 g / m2) was formed on the meltblown nonwoven fabric of the two-layer laminate. 2 ) was further laminated on the nonwoven fabric. In other words, three layers of spunbond nonwoven fabric / meltblown nonwoven fabric / spunbond nonwoven fabric were laminated and integrated to obtain a three-layer laminated nonwoven fabric. This laminated nonwoven fabric was used as a surface nonwoven fabric to be laminated on a nonporous moisture-permeable waterproof film. This laminated nonwoven fabric had the above-mentioned three-layer structure and had a basis weight of 25 g / m2. 2 It was.
[0057] A second nonwoven fabric to be laminated as a lining to a nonporous moisture-permeable waterproof film is made by melt-spinning polypropylene using the spunbond method, forming a continuous fiber group into a web shape, and then heat-treating it to produce a web with a basis weight of 23 g / m2, made of polypropylene fibers with a single fiber fineness of 3 dtex. 2 Thus, a single-layered spunbond nonwoven fabric was obtained.
[0058] A three-layered first nonwoven fabric as a surface layer was laminated on one side of the nonporous moisture-permeable waterproof film, and a single-layered second nonwoven fabric as a lining was laminated on the other side of the nonporous moisture-permeable waterproof film. These were then heat-pressed together using a synthetic rubber hot melt adhesive (MORESCO Corporation). This resulted in a laminate of the three-layered first nonwoven fabric, the nonporous moisture-permeable waterproof film, and the single-layered second nonwoven fabric, with a basis weight of 66 g / m. 2Thus, a protective suit fabric of Example 1 was obtained.
[0059] The properties of the resulting fabric and film are shown in Table 1.
[0060] [Table 1]
[0061] Example 2 Compared to Example 1, the weight of the non-porous moisture-permeable waterproof film was increased to 15 g / m 2 The rest of the material was changed to the same as in Example 1, with a basis weight of 63 g / m 2 Thus, a protective suit fabric of Example 2 was obtained.
[0062] The properties of the resulting fabric and film are shown in Table 1.
[0063] Comparative Example 1 In comparison with Example 1, the non-porous moisture-permeable waterproof film does not substantially contain oleic acid amide as a slip agent, i.e., it does not contain enough oleic acid amide to exhibit slip function, but contains only 0.02 mass% for the purpose of mold releasability. The rest of the film is the same as Example 1, and the basis weight is 66 g / m. 2 An attempt was made to obtain the protective suit fabric of Comparative Example 1. However, the molten resin adhered to various parts of the film manufacturing device, and film formation was not possible.
[0064] The fabrics of Examples 1 and 2 all had the required moisture permeability, water pressure resistance, blood barrier property, and virus barrier property. In addition, the non-porous moisture-permeable waterproof films obtained in Examples 1 and 2 were evaluated for blood barrier property and virus barrier property by themselves, and both were acceptable. Furthermore, the non-porous moisture-permeable waterproof films obtained in Examples 1 and 2 were evaluated for blood barrier property tested according to "Procedure B" specified in JIS T8060·2015 and virus barrier property tested according to "Procedure B" specified in JIS T 8061·2015, and both films had blood barrier property and virus barrier property of "Class 6" as specified in JIS T8122·2015. Moreover, since the non-porous moisture-permeable waterproof films contained oleic acid amide as a slip agent, they also had good releasability from the film manufacturing equipment. For this reason, protective clothing fabrics could be manufactured with good manufacturability.
[0065] Furthermore, the fabric of Example 1 had the following performance characteristics:
[0066] That is, the tensile strength and elongation rate (JIS T8115, tensile speed 100mm / min, grip interval 100mm) were 62N (transverse direction), 120N (vertical direction), 127.2% (transverse direction), 162.2% (vertical direction), and the tear strength (JIS T8115) was 88.9N (transverse direction) and 48.4N (vertical direction). In addition, when three test pieces were measured, all three test pieces showed grade 4 in water repellency (JIS L1092 spray test, initial stage). The impact permeability (test method AATCC42) was 0.0g and the judgment was "Compliant (in accordance with AAMI PB70 level 3)". The hydrostatic pressure (test method AATCC127) was 173cm and the judgment was "Compliant (in accordance with AAMI PB70 level 3)".
[0067] In contrast, in Comparative Example 1, the non-porous moisture-permeable waterproof film did not substantially contain a slip agent, which resulted in the material adhering to the manufacturing equipment during the production of the non-porous moisture-permeable waterproof film, resulting in reduced manufacturability, as described above.
Claims
1. A fabric for protective clothing, comprising a nonwoven fabric laminated on at least one side of a nonporous moisture-permeable waterproof film made of a polyester-polyether resin composition having a polyester-polyether block copolymer as a main component, and the polyester-polyether resin composition contains a slip agent.
2. 2. The protective suit fabric of claim 1, wherein the slip agent is a fatty acid amide.
3. 3. The fabric for protective clothing according to claim 2, characterized in that the fatty acid amide is oleic acid amide.
4. 3. The protective suit fabric according to claim 2, characterized in that the polyester-polyether resin composition contains polyethylene.
5. The fabric for protective clothing according to claim 4, characterized in that the polyester-polyether resin composition constituting the non-porous moisture-permeable waterproof film contains fatty acid amide and polyethylene in a dispersed state in a polyester-polyether block copolymer.
6. 6. The fabric for protective clothing according to claim 5, characterized in that the polyester-polyether resin composition contains 0.03 to 0.10% by mass of a fatty acid amide.
7. 7. The protective clothing fabric according to claim 1, wherein the nonwoven fabric is a laminated nonwoven fabric in which a spunbonded nonwoven fabric is laminated on both sides of a meltblown nonwoven fabric.
8. 8. The protective suit fabric according to claim 7, characterized in that the meltblown nonwoven fabric is colored.
9. 8. The protective suit fabric according to claim 7, wherein the non-porous moisture-permeable waterproof film and the non-woven fabric are bonded to each other with a hot melt resin.
10. A method for producing a fabric for protective clothing, comprising the steps of preparing a polyester-polyether resin composition containing a slip agent, forming the resin composition into a film, and laminating a nonwoven fabric on at least one side of the obtained film.
11. A master batch is prepared by melt-mixing a fatty acid amide, which is a slip agent, with polyethylene. a polyester-polyether block copolymer is mixed with the master batch in a predetermined amount and melt-kneaded to prepare a polyester-polyether resin composition in which an aliphatic amide and polyethylene are dispersed in the polyester-polyether block copolymer; This resin composition is formed into a film, A method for producing fabric for protective clothing, comprising laminating a nonwoven fabric on at least one side of the obtained film.
12. A protective suit for preventing infection, which is made of the protective suit fabric according to any one of claims 1 to 9.
Citation Information