Method for producing cellulose fiber composite and cellulose fiber composite composition
By using a copolymer with a vinyl polymer grafted onto a cellulose derivative and removing excess components, the method addresses the dispersion challenges of nanocellulose in resins, enhancing dispersibility and composite properties.
Patent Information
- Application Number
- JP2020182297
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-10-30
- Publication Date
- 2024-09-17
- Estimated Expiration
- 2040-10-30
AI Technical Summary
Existing methods struggle to achieve efficient dispersion of nanocellulose in resins due to its hydrophilic nature, leading to poor adhesion and dispersibility, and often result in the production of vinyl homopolymers that affect the physical properties of the composite.
A method involving the use of a copolymer with a vinyl polymer grafted onto a cellulose derivative as a dispersant, followed by a process to adsorb the dispersant onto cellulose fibers and remove excess components like vinyl homopolymers and water, ensuring efficient dispersion in organic solvents or resins.
This approach enhances the dispersibility of cellulose fibers in resins, improving the physical properties of the composite by removing unnecessary components, thereby increasing the efficiency and effectiveness of the dispersion process.
Smart Images

Figure 0007551102000001
Abstract
Description
[Technical field]
[0001] The present invention relates to methods for producing a cellulose fiber composite and a cellulose fiber composite composition, and in particular to a method for producing a cellulose fiber composite in which a dispersant is adsorbed onto cellulose fibers and recovered as a cellulose fiber composite, and a method for producing a cellulose fiber composite composition in which cellulose fibers are dispersed in a resin or the like using the same. [Background technology]
[0002] Cellulose is a renewable resource that is used for a variety of purposes, including paper and functional materials. Nanocellulose, which is cellulose defibrated to the nano level, is attracting attention as a material with new functions. Known types of nanocellulose include cellulose nanofibers (CNF) that have fiber diameters of 10 nm or less produced by chemical processing (also called TEMPO-oxidized CNF or phosphate-esterified CNF, and also called single nanofibers), CNF with larger fiber diameters than those produced by chemical processing through mechanical or physical fiberization, microfibrils, and cellulose nanocrystals (CNC) produced by extracting highly crystalline parts from pulp by treating it with strong acids, and even bacterial cellulose produced by microorganisms. These materials are expected to have a wide range of applications, including as film materials, gas barrier materials, viscosity modifiers, lubricants, thermal conductive materials, plant growth agents, thermosetting resins, radiation curable resins such as UV and electron beam curable resins, composite materials with general-purpose resins, and composite materials with rubber.
[0003] One promising use for nanocellulose is its composite with resin. Nanocellulose has strength close to that of carbon fiber or aramid fiber, and is one-fifth the weight of steel, but more than five times stronger. For this reason, composite materials in which nanocellulose is dispersed in resin are strong and lightweight, and are expected to be used in exterior and interior materials, rubber belts, and other automotive components.
[0004] There are various approaches to dispersing and compounding nanocellulose in resin. For example, there is a method of mixing pulp with resin and, if necessary, a swelling agent, and defibrating it using a kneader, and a method of mixing a dispersion solution of single nano-sized CNFs (diameters less than 10 nm) with resin and defibrating it using a kneader in the same way.
[0005] However, with these methods, it is difficult to disperse at the single nano level, and it is difficult to obtain the desired physical properties. One of the reasons is that most nanocellulose has hydrophilic functional groups on its surface, which gives it excellent affinity and dispersibility in water, but generally has extremely poor dispersibility in highly hydrophobic resins. In particular, CNFs produced by the TEMPO oxidation method or the phosphoric acid esterification method are useful because they have a fiber diameter at the single nano level, but because they have carboxylate and phosphate groups on their surface, they have extremely poor compatibility with hydrophobic resins.
[0006] Therefore, various technical studies have been carried out to disperse the particles in resin. One of these methods involves introducing hydrophobic functional groups through chemical reactions, utilizing hydroxyl groups present on the surface of nanocellulose. For example, grafting of caprolactone (see Patent Document 1), acetylation by addition reaction of acetic anhydride (see Patent Document 2), addition reaction of alkenyl succinic anhydride, etc. are known (see Patent Document 3). Furthermore, a method is also known in which an acrylic block polymer that has affinity for both nanocellulose and the resin in which it is to be dispersed is used as a dispersant (see Patent Documents 4 and 5). The applicant of the present application has also proposed a cellulose fiber dispersion composite capable of dispersing cellulose fibers, particularly nanocellulose, in organic solvents, resins, etc. at low cost and at a sufficient level, and a cellulose fiber composition containing the same, which is a composite having a structure in which a vinyl polymer is grafted onto a cellulose derivative (this composite is referred to as a "dispersant" in the present invention), and a cellulose fiber composition containing this composite and cellulose fibers (see Patent Document 6). Specific examples of the cellulose fiber composition include those containing organic solvents, resin precursors, resins, etc. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] JP 2011-68707 A [Patent Document 2] JP 2017-165946 A [Patent Document 3] Patent No. 5757779 [Patent Document 4] JP 2016-104865 A [Patent Document 5] International Publication No. 2015 / 152188 [Patent Document 6] JP 2020-7525 A Summary of the Invention [Problem to be solved by the invention]
[0008] The technology described in Patent Document 6 allows cellulose fibers, particularly nanocellulose, to be dispersed in resin at a low cost and at a sufficient level. However, when preparing a dispersant having a structure in which a vinyl polymer is grafted to a cellulose derivative, vinyl homopolymers that are not grafted to the cellulose derivative are also by-produced, and such vinyl homopolymers may adversely affect the physical properties of the resulting cellulose fiber composition. In addition, it is not efficient to include excess dispersant that does not contribute to the dispersion of cellulose fibers. Patent Document 6 does not disclose a method for removing this vinyl homopolymer or excess dispersant. In addition, dehydration under reduced pressure is performed as a method for removing water, but if water can be removed with less energy, the value of this technology will be further increased.
[0009] Therefore, the present invention relates to an improved technology of the invention described in Patent Document 6, and aims to provide a method for producing a cellulose fiber composite that can produce a cellulose fiber composite from which water, excess dispersant, vinyl homopolymer, etc. have been removed simply and with low energy without inhibiting the dispersibility of cellulose fibers in dispersed materials such as resins, and a method for producing a cellulose fiber composite composition using the cellulose fiber composite. [Means for solving the problem]
[0010] As a result of intensive research, the present inventors have found that the above problems can be solved by adopting the following configuration.
[0011] That is, the method for producing a cellulose fiber composite of the present invention includes the steps of: preparing a dispersion in which cellulose fibers are dispersed in an organic solvent or a mixed solvent of an organic solvent and water using a copolymer in which a vinyl polymer is grafted onto a cellulose derivative as a dispersant; and removing excess dispersant that is not adsorbed by the cellulose fibers from the dispersion. and and recovering the cellulose fibers to which the dispersant is adsorbed as the desired cellulose fiber composite by separating the liquid containing the vinyl homopolymer that has not been grafted to the cellulose derivative.
[0012] In addition, the method for producing a cellulose fiber composite composition of the present invention includes a step of producing a cellulose fiber composite by the above-mentioned method, and then mixing the cellulose fiber composite with a dispersed material, which is an organic solvent, a resin and / or a resin precursor, thereby redispersing the cellulose fibers in the dispersed material.
[0013] For the sake of clarity, the terminology used in this invention is clarified. The cellulose fibers with dispersant adsorbed thereon and recovered from the dispersion liquid are referred to as a "cellulose fiber composite." Meanwhile, the cellulose fibers (re-)dispersed in a dispersed material (organic solvent, resin, resin precursor, etc.) using this "cellulose fiber composite" are referred to as a "cellulose fiber composite composition." Effect of the Invention
[0014] The present invention has the advantages of the technology described in Patent Document 6, that is, cellulose fibers can be sufficiently dispersed in resins, etc., which is effective for preparing a composite material (composite composition) of cellulose fibers and resins, and further has the advantage that grafting of a vinyl-based polymer to a cellulose derivative can be carried out relatively inexpensively. In addition, water, vinyl-based homopolymers that do not contribute to dispersibility, and excess dispersant are removed simply and with low energy, and a necessary and sufficient amount of dispersant remains in a state adsorbed on the cellulose fibers, so that when composited with resins, etc., dispersion of cellulose fibers in resins becomes more efficient, and further improvement in the effect of improving the physical properties of resins, etc. can be expected. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] Preferred embodiments of the cellulose fiber composite and the method for producing a cellulose fiber composite composition according to the present invention are described in detail below. However, the scope of the present invention is not limited to these descriptions, and modifications other than those described below may be made as appropriate without departing from the spirit of the present invention.
[0016] [Dispersant] The dispersant used in the present invention has a structure in which a vinyl polymer is grafted to a cellulose derivative. As such a dispersant, for example, the one disclosed in JP-A-2020-7525 as "composite for dispersing cellulose fibers" can be used.
[0017] The cellulose derivative is a cellulose derivative in which some of the hydroxyl groups are substituted. As the cellulose derivative, a conventionally known cellulose derivative can be used, and specific examples thereof include methyl cellulose, ethyl cellulose, butyl cellulose, hydroxypropyl cellulose, hydroxypropyl methyl cellulose, hydroxybutyl methyl cellulose, carboxymethyl cellulose, cellulose acetate, cellulose acetate butyrate, cellulose acetate propionate, triacetyl cellulose, nitrocellulose, and cationized cellulose. Among these, from the viewpoints of high solubility in organic solvents, ease of grafting with vinyl polymers, and availability, ethyl cellulose, cellulose acetate butyrate, cellulose acetate propionate, triacetyl cellulose, and cationized cellulose are preferred.
[0018] These conventionally known cellulose derivatives usually have unmodified hydroxyl groups. These hydroxyl groups can be used to introduce polymerizable unsaturated groups or thiol (mercapto) groups. By introducing polymerizable unsaturated groups or thiol groups in this way, grafting of vinyl polymers, which will be described later, can be easily performed using these functional groups as starting points. The above-mentioned polymerizable unsaturated group or thiol group can be introduced, for example, by addition reacting the above-mentioned conventionally known cellulose derivative with an isocyanate-based (meth)acrylate compound such as Karenz MOI or AOI manufactured by Showa Denko, by addition reacting an anhydride such as (meth)acrylic anhydride or maleic anhydride, by addition reacting (meth)acrylic acid or the like using a condensing agent such as carbodiimide, by reacting with (meth)acrylic acid chloride or an organic acid having a thiol group, etc. Examples of organic acids having a polymerizable unsaturated double bond or a thiol group include (meth)acrylic acid, maleic acid, crotonic acid, butene tricarboxylic acid, 4-ethenylbenzoic acid, 3-mercaptopropionic acid, etc. In this specification, the term "(meth)acrylic acid" includes both methacrylic acid and acrylic acid. The same applies to terms such as "(meth)acrylate".
[0019] In the introduction of a polymerizable unsaturated group or a thiol group, various solvents and catalysts (condensing agents, organometallic materials, amines, etc.) can be used, as in known techniques. Moreover, the number of polymerizable unsaturated groups or thiol groups introduced per molecule of the cellulose derivative is desirably 20 or less on average. If more than 20 groups are introduced, gelation may occur during graft polymerization. As the reaction solvent, aprotic solvents such as ethyl acetate, propyl acetate, butyl acetate, tetrahydrofuran, dioxane, acetone, methyl ethyl ketone, methyl isobutyl ketone, toluene, xylene, dimethylformamide, dimethylacetamide, N-methylpyrrolidone, and pyridine can be used alone or in combination.
[0020] In the present invention, the cellulose derivative may have a cationic group. The cellulose derivatives have cationic groups, which makes them excellent dispersants for CNFs produced by the TEMPO oxidation method or phosphoric acid treatment method. These CNFs have carboxylate groups or phosphate groups on their surfaces, and the affinity between the functional groups on the CNF surface and the cationic groups of the cellulose derivatives promotes the dispersion of CNFs.
[0021] As the cellulose derivative having a cationic group, a conventionally known cationic cellulose may be used, but a cationic group can also be introduced into a cellulose derivative having no cationic group as described below. That is, for example, methods for introducing amino groups include a method of reacting thionyl chloride / ammonia, and a method of reacting an epoxy group with ammonia or a polyvalent amino compound after the introduction of the epoxy group.Furthermore, a method of introducing the amino group by reacting a compound having both an amino group and a carboxyl group in the molecule with the above-mentioned condensing agent or the like can be carried out. As the reaction solvent, aprotic solvents such as ethyl acetate, propyl acetate, butyl acetate, tetrahydrofuran, dioxane, acetone, methyl ethyl ketone, methyl isobutyl ketone, toluene, xylene, dimethylformamide, dimethylacetamide, N-methylpyrrolidone, and pyridine can be used alone or in combination. The number of cationic groups per molecule of the cellulose derivative is preferably in the range of 1 to 30 on average.
[0022] Grafting of a vinyl polymer onto a cellulose derivative can be carried out, for example, by radical polymerization of a vinyl monomer in the presence of a cellulose derivative having a polymerizable unsaturated group or a thiol group introduced therein as described above. A graft chain of a vinyl polymer is formed with the polymerizable unsaturated group or the thiol group as a base point.
[0023] In the above, examples of the vinyl monomer include (meth)acrylates having an alkyl group of 1 to 20 carbon atoms, such as methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, isobutyl (meth)acrylate, tert-butyl (meth)acrylate, and 2-ethylhexyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, glyceryl (meth)acrylate, and dimethylaminoethyl (meth)acrylate. acrylate, diethylaminoethyl (meth)acrylate, tetrahydrofurfuryl (meth)acrylate, isobornyl (meth)acrylate, phenoxyethyl (meth)acrylate, benzyl (meth)acrylate, cyclohexyl (meth)acrylate, dicyclopentanyl (meth)acrylate, dicyclopentenyloxyethyl (meth)acrylate, adamantyl (meth)acrylate (Osaka Organic Chemical Industry Co., Ltd.: MADA, MADMA, EtADA, EAMA(P), etc.), methacrylates with 1 to 30 repeat units Polyethylene glycol (meth)acrylate, methoxypolypropylene glycol (meth)acrylate with 1 to 30 repeating units, butoxydiethylene glycol (meth)acrylate, 2-(meth)acryloyloxyethylhexahydrophthalic acid, 2-(meth)acryloyloxyethyl succinic acid, glycidyl (meth)acrylate, 3,4-epoxycyclohexylmethyl methacrylate, 2-(meth)acryloyloxyethyl acid phosphate, styrene, styrene derivatives, (meth)acrylic acid, (meth) Examples of such compounds include acrylamide, N-phenylmaleimide, N-cyclohexylmaleimide, maleic anhydride, (meth)acrylonitrile, N-vinylpyrrolidone, silicone-based (meth)acrylates (manufactured by JNC under the trade names Silaplane "FM-0711", "FM-0721", "FM-0725", etc., manufactured by Shin-Etsu Chemical Co., Ltd.: "X-22-174DX", "X-22-2426", "X-22-2475", etc.), and fluorine-substituted (meth)acrylates (various fluorine-substituted alkyl (meth)acrylates manufactured by Daikin Corporation).
[0024] It is also possible to use polyfunctional (meth)acrylates such as ethylene glycol di(meth)acrylate and hexanediol di(meth)acrylate, divinylbenzene, etc., in amounts that do not cause insolubilization in the solvent due to gelation. These monomers can be used alone or in combination of multiple types.
[0025] The properties of the vinyl polymer produced change depending on the combination of the vinyl monomers described above, and in particular the dispersibility of the cellulose fiber in organic solvents and resins. Generally speaking, the Solubility Parameter (SP) value is an index of affinity with the organic solvent or resin to be dispersed. It is desirable to design the SP value of the grafted vinyl polymer to be close to that of the dispersion target. In particular, when the difference between the experimental and calculated SP values is less than 1.0 ((cal / cm 3 ) 1 / 2 ) or less. In addition, when a hydroxyl group-containing monomer such as 2-hydroxyethyl (meth)acrylate or a polyalkylene oxide monomer component is used as a vinyl monomer, in particular, a methoxypolyethylene glycol (meth)acrylate having a repeating unit number of 1 to 30 or a methoxypolypropylene glycol (meth)acrylate having a repeating unit number of 1 to 30 is used, effective interaction effects can be expected even when acids and bases are present in the cellulose fibers, so it is desirable to use them as one component to be copolymerized.
[0026] Furthermore, it is also desirable to select a vinyl monomer that has an interaction with the material to be dispersed (especially resin). Examples of interactions include hydrophobic interactions such as with alkyl groups, hydrogen bonds such as with hydroxyl groups, amines, carboxyl groups, and amide groups, and conjugated stacks such as π-π with aromatic rings. This can be achieved by using a monomer that has such functional groups. Furthermore, it is also possible to introduce reactive groups into the vinyl polymer produced, forming bonds with the resin to be dispersed. One method is to copolymerize a vinyl monomer having an epoxy group, such as the above-mentioned glycidyl (meth)acrylate or 3,4-epoxycyclohexylmethyl (meth)acrylate. Another method is to introduce a polymerizable (meth)acrylate group, vinyl group, allyl group, etc., by chemical reaction using functional groups in the vinyl polymer produced, such as hydroxyl groups and carboxyl groups. The introduction of such reactive groups can be achieved by addition reaction using isocyanate group-containing (meth)acrylates such as KarenzMO-I and AO-I (manufactured by Showa Denko), glycidyl (meth)acrylate, 3,4-epoxycyclohexylmethyl (meth)acrylate, etc.
[0027] In the polymerization of the cellulose derivative having the polymerizable unsaturated group or thiol group introduced therein and the vinyl monomer, it is preferable that they are mixed in a weight ratio of 5:95 to 99:1. Outside this range, the effect as a dispersant for cellulose fibers may be reduced. In the above polymerization, it is not necessary that all of the vinyl polymer formed from the vinyl monomer is grafted (chemically bonded) to the cellulose derivative, and a polymer formed by homopolymerization of the vinyl monomer may be included.
[0028] The molecular weight of the vinyl polymer formed by grafting to the cellulose derivative is preferably selected in the range of weight average molecular weight of 1000 to 500,000.If the weight average molecular weight is less than 1000, the effect as a dispersant may decrease, and if the weight average molecular weight is more than 500,000, the viscosity tends to become too high. The weight average molecular weights of the cellulose derivative, the vinyl polymer grafted onto the cellulose derivative, and the dispersant (a copolymer in which a vinyl polymer is grafted onto a cellulose derivative) are values calculated using standard polystyrene standards by gel permeation chromatography (GPC).
[0029] The molecular weight of the dispersant is preferably in the range of 5,000 to 800,000 in terms of weight average molecular weight, which includes the vinyl polymer bonded to the cellulose derivative, and the bonded or unbonded vinyl homopolymer (single polymer). The molecular weight of the dispersant measured by GPC is thought to be due to the inherent solution properties of the cellulose derivative, but it may not be simply the sum of the cellulose derivative and the vinyl polymer. Although the details are unclear, the binding of the vinyl polymer to the cellulose derivative may change the spread of the polymer chain and the interaction between the cellulose derivatives. Therefore, it is only the molecular weight measured by GPC.
[0030] Examples of organic solvents that can be used in polymerization include ethyl acetate, butyl acetate, tetrahydrofuran, dioxane, acetone, methyl ethyl ketone, methyl isobutyl ketone, toluene, xylene, methyl alcohol, ethyl alcohol, isopropyl alcohol, butyl alcohol, benzyl alcohol, dimethylformamide, dimethylacetamide, N-methylpyrrolidone, ethyl lactate, dimethyl sulfoxide, ethylene glycol monoethyl ether, ethylene glycol monobutyl ether, ethylene glycol monomethyl ether acetate, ethylene glycol monoethyl ether acetate, ethylene glycol monobutyl ether acetate (butyl carbitol acetate), diethylene glycol monoethyl ether, diethylene glycol monobutyl ether, diethylene glycol monoethyl ether acetate, diethylene glycol monobutyl ether acetate ... Preferred are cholesteryl methyl ether, diethylene glycol isopropyl methyl ether, diethylene glycol diethyl ether, diethylene glycol butyl methyl ether, diethylene glycol dibutyl ether, triethylene glycol dimethyl ether, triethylene glycol butyl methyl ether, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol monomethyl ether acetate, propylene glycol dimethyl ether, propylene glycol diacetate, dipropylene glycol monomethyl ether, dipropylene glycol dimethyl ether, dipropylene glycol monobutyl ether, dipropylene glycol dibutyl ether, tripropylene glycol dimethyl ether, dihydroterpineol acetate, terpineol, dihydroterpineol, dihydroterpineol acetate, and the like, either alone or in admixture.
[0031] As the polymerization initiator, for example, various types of radical polymerization initiators such as peroxides and azos can be used. The concentration during polymerization, the initiator concentration, etc. can be within the range of known techniques.
[0032] After polymerizing the cellulose derivative with a vinyl monomer, it is possible to carry out precipitation purification using a poor solvent, as in conventional polymer purification, if necessary. This makes it possible to remove unreacted monomers and by-products. On the other hand, in the dispersant prepared by the above method, in addition to the ideal dispersant structure in which the cellulose derivative and the vinyl polymer are bonded, unbonded vinyl homopolymers are generated and mixed. This is unavoidable due to the mechanism of radical polymerization, which is the chain transfer of radicals. It was also found that it is difficult to completely remove the vinyl homopolymers from the generated polymer by reprecipitation purification, etc. It was also found that if a large amount of such vinyl homopolymers are contained, they will cause a decrease in physical properties when the composite material is subsequently produced. Therefore, the present production method also aims to effectively remove such vinyl homopolymers.
[0033] [Cellulose fiber] The cellulose fibers used in the present invention include, for example, cellulose nanofibers (CNF) (also called TEMPO-oxidized CNF or phosphate-esterified CNF, or also called single nanofibers) having a fiber diameter of 10 nm or less obtained by chemical treatment as described above, CNF having a larger fiber diameter than that obtained by chemical treatment through mechanical or physical fiberization, lignocellulose bound to lignin and its nanocellulose, microfibrils, cellulose nanocrystals (CNC) obtained by extracting highly crystalline parts from pulp by treating it with a strong acid or the like, and bacterial cellulose produced by microorganisms. Commercially available products include slurry CNF (phosphorylated product, name: AuroVisco) manufactured by Oji Holdings, powdered CNF, TEMPO oxidation method CNF manufactured by Nippon Paper Industries, Nanoforest-S manufactured by Chuetsu Pulp, water-dispersed CNF (name: ELLEX-S) manufactured by Daio Paper, and water-dispersed CNF manufactured by the TEMPO oxidation method (name: LeoCrysta) manufactured by Daiichi Kogyo Seiyaku, with fiber diameters ranging from 4 nm to 500 nm. In the manufacturing method of the present invention, water-dispersed nanocellulose having a fiber diameter on the micrometer to nanometer level may be used, or the raw pulp may be defibrated by mechanical or physical means after adding the above-mentioned dispersant.
[0034] [Preparation of Dispersion] The method for producing a cellulose fiber composite of the present invention includes a step of preparing a dispersion in which the cellulose fibers are dispersed in an organic solvent or a mixed solvent of an organic solvent and water using the dispersant. As for cellulose fibers, as described above, chemically treated cellulose fibers are commercially available in the form of an aqueous dispersion, and they can also be produced from raw pulp. When these are used as raw materials, the dispersion liquid can be prepared, for example, as follows.
[0035] First, when an aqueous dispersion of chemically treated cellulose fibers is used as the starting material, a dispersion can be prepared by mixing an organic solvent that dissolves in water with the aqueous dispersion of chemically treated cellulose, and then adding the above-mentioned dispersant and stirring and mixing the mixture. The ratio of the amount of organic solvent to be mixed with the aqueous dispersion of cellulose fibers dispersed in water is preferably 1 to 50 parts by weight per 1 part by weight of the aqueous dispersion. The amount of dispersant to be added is preferably in the range of 0.1 to 10 parts by weight (equivalent to polymer solids) per 1 part by weight of cellulose fibers in the aqueous dispersion of cellulose fibers. In general, the solids concentration of chemically treated cellulose fibers (in an aqueous dispersion state) is in the range of 0.5% by weight to 5% by weight, and the amount of dispersant relative to this solids weight can be adjusted within the above range. In the dispersion operation, the mixture can be dispersed into the cellulose fibers using a mechanical stirring device such as a homogenizer, a jet mill, a ball mill, or a bead mill.
[0036] In the above process, which uses an aqueous dispersion of cellulose fibers as the starting material, it is also desirable and possible to remove the majority of the water contained therein by previously mixing a specific organic solvent with the aqueous dispersion of cellulose fibers and removing the mixture of water and the organic solvent (preliminary dehydration). The organic solvent used in the preliminary dehydration is preferably an amphipathic organic solvent having high affinity for water in order to remove water. Preferred examples of such organic solvents include methyl alcohol, ethyl alcohol, isopropyl alcohol, butyl alcohol, acetone, methyl ethyl ketone, tetrahydrofuran, dioxane, N-methylpyrrolidone, dimethylformamide, dimethylacetamide, ethyl lactate, dimethyl sulfoxide, ethylene glycol monoacetate, propylene glycol monomethyl ether, propylene glycol monoethyl ether, and propylene glycol monomethyl ether acetate, and these can be used alone or in combination. By carrying out this process, it may be possible to suppress the insolubilization of the dispersant due to the influence of water. In other words, it is also possible to use multiple organic solvents and remove the excess dispersant through a multi-stage process.
[0037] Furthermore, when pulp fibers are used as the starting material, a dispersant and an organic solvent alone or a mixture of water and an organic solvent are mixed with the pulp, and the mixture is defibrated using mechanical or physical methods, allowing dispersion to the nano level. In this manufacturing method, the surface area increases as the pulp fibers are defibrated (the fiber diameter becomes smaller), so if a dispersant is added to the defibration process, the dispersant is adsorbed onto the surface of the generated cellulose fibers, forming a stable dispersed state. On the other hand, it is also possible to carry out the defibration process without adding a dispersant, and then add a dispersant in the final process to advance defibration. Pulp can be made from a variety of raw materials, such as softwood, hardwood, kenaf, and bamboo, as well as a variety of other types, such as chemical pulp, mechanical pulp, chemical-mechanical pulp, and semi-chemical pulp, which are produced using different processing methods. The above-mentioned organic solvent or a mixed solvent of water and an organic solvent is mixed in an amount of, for example, 0.5 to 100 parts by weight per part by weight of cellulose fibers before defibration, and defibration can be performed by mechanical or physical means. The amount of dispersant added is the same as when an aqueous dispersion of chemically treated cellulose fibers is used as the starting material. For defibration, in addition to the mechanical dispersion device, a kneader, a continuous twin-screw kneader, or a jet pulverizer such as a jet mill can be used.
[0038] In the above process using pulp fibers as the starting material, it is possible to defibrate cellulose fibers such as pulp using a mixture of an organic solvent and water, and optionally adding a dispersant, and then gradually replace the mixture with an organic solvent and wash the mixture to remove the water and excess dispersant.
[0039] The organic solvent used in this step may be the same as that used in the introduction of functional groups or graft polymerization when preparing the dispersant, but it is particularly preferable to use an amphiphilic organic solvent such as those exemplified for the preliminary dehydration.
[0040] As described above, by dispersing the cellulose fibers with the dispersant in an organic solvent or a mixed solvent of an organic solvent and water, the dispersant is adsorbed onto the surface of the cellulose fibers.
[0041] [Recovery of Cellulose Fiber Composites] In the method for producing a cellulose fiber composite of the present invention, the following step is carried out: removing excess dispersant that is not adsorbed by the cellulose fibers from the dispersion liquid prepared in the above step. and By separating the liquid containing the vinyl homopolymer that has not been grafted to the cellulose derivative, the cellulose fibers to which the dispersing agent is adsorbed are recovered as the desired cellulose fiber composite.
[0042] In the dispersion after the above-mentioned dispersion preparation process, cellulose fibers are dispersed in an organic solvent or a mixed solvent of an organic solvent and water. By separating the liquid from this dispersion in this process, it is possible to recover a cellulose fiber composite with an ideal structure in which a necessary and sufficient amount of dispersant is adsorbed to the cellulose fibers. In other words, components that may affect the deterioration of physical properties, such as dispersants that are not adsorbed to the cellulose fibers and vinyl homopolymers, are separated and removed. Since water can also be removed as a liquid component, it is possible to simultaneously remove water and unnecessary components such as vinyl homopolymers that may affect the deterioration of physical properties. Possible methods for separating this liquid include filtration using various filters, a method in which the cellulose fibers and the liquid are separated and then the liquid is poured off and removed, a method in which the cellulose fibers are allowed to settle and separated using a centrifugal separator, etc. In particular, it is desirable to carry out the filtration method because it is simple and low cost. The filters used in this operation include various paper filters, processed filters thereof, resin filters made of fibrous or porous bodies such as fluororesins, nylon, polypropylene, polyethersulfone, and mixed cellulose esters, membrane filters such as Millipore manufactured by MERK, resin mesh filters, metal mesh filters, glass fiber filters, and tubular ultrafiltration filters. The pore size of the openings can be in the range of 10 nm to 50 μm. Alternatively, the retention particle size is an index of the filter's performance, and a filter with a value in the range of 50 nm to 20 μm is suitable. In addition, multiple types of filters with different performance differences may be used in combination. The solution temperature during filtration or separation from the liquid is usually in the range of −10° C. to 100° C. When carrying out the filtration method, reduced pressure (suction) filtration or pressure filtration can be performed.
[0043] In the liquid separation step, it is also desirable to wash the cellulose fiber composite using an organic solvent. This washing step makes it possible to effectively remove water and vinyl homopolymers in the dispersant. In particular, repeated washing can reduce the water content to 1.0% by weight or less. By reducing the water content to 1.0% by weight or less, excellent effects can be expected in terms of physical properties and other characteristics when applied to cellulose fiber composite compositions, etc., as described below. On the other hand, the preferred amount of dispersant adsorbed to the cellulose fibers is in the range of 1 to 200 parts by weight per 100 parts by weight of the cellulose fibers. The smaller the diameter of the cellulose fibers, the greater the surface area and the greater the amount of adsorption. As a result of examining various fiber diameters, it was found that the preferred range is as described above. It was found that if the dispersant is adsorbed in this range, the cellulose fibers can be uniformly dispersed in various materials to be dispersed. If the amount is less than 1 part by weight, the dispersibility of the cellulose fibers decreases, and if the amount is more than 200 parts by weight, there is a risk that the physical properties of the composite when the cellulose fibers are composited with a resin or the like may decrease. The organic solvent used in this washing step is not particularly limited, but the amphiphilic organic solvents exemplified for the preliminary dehydration are preferably used.
[0044] The liquid separation step does not necessarily mean to completely separate the liquid component from the solid component, and the recovered cellulose fiber composite may be in a wet state with some of the organic solvent remaining in the cellulose fibers. Conversely, the organic solvent may be in a state where it has been almost completely removed, but complete removal of the organic solvent may cause aggregation between the cellulose fibers. Therefore, the preferred range of the remaining organic solvent is 1 to 200 parts by weight per part by weight of the cellulose fibers to which the dispersant is adsorbed. Furthermore, from the viewpoint of cost, it is desirable to recover and purify the organic solvent used in the manufacturing process, which includes the above-mentioned dehydration treatment, adsorption of the dispersant, and removal of the excess dispersant, so as to reuse the same.
[0045] [Cellulose fiber composite composition] By mixing the cellulose fiber composite (cellulose fibers with a dispersant adsorbed thereon) obtained as described above with a material to be dispersed (organic solvent, resin, resin precursor, etc.), a cellulose fiber composite composition in which the cellulose fibers are uniformly dispersed in the material to be dispersed can be produced. The cellulose fiber composite composition will be described below. As a specific configuration, various configurations can be used depending on the application, etc. Below, first to third configurations are given as examples of preferable configurations.
[0046] <First Configuration: Organic Solvent Dispersion Composition> The first composition is an organic solvent dispersion composition containing the cellulose fiber composite and an organic solvent. As the organic solvent, those used in the above-mentioned reaction, polymerization, and dispersion processes can be used, and examples thereof include the following. Ethyl acetate, butyl acetate, tetrahydrofuran, dioxane, methyl ethyl ketone, methyl isobutyl ketone, toluene, xylene, butyl alcohol, benzyl alcohol, dimethylformamide, dimethylacetamide, N-methylpyrrolidone, ethyl lactate, dimethyl sulfoxide, ethylene glycol monoethyl ether, ethylene glycol monobutyl ether, ethylene glycol monomethyl ether acetate, ethylene glycol monoethyl ether acetate, ethylene glycol monobutyl ether acetate (butyl carbitol acetate), diethylene glycol monoethyl ether, diethylene glycol monobutyl ether, diethylene glycol monoethyl ether acetate, diethylene glycol monobutyl ether acetate, diethylene glycol ethyl methyl ether, diethylene glycol isoprene and mixtures of the following: propyl methyl ether, diethylene glycol diethyl ether, diethylene glycol butyl methyl ether, diethylene glycol dibutyl ether, triethylene glycol dimethyl ether, triethylene glycol butyl methyl ether, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol monomethyl ether acetate, propylene glycol dimethyl ether, propylene glycol diacetate, dipropylene glycol monomethyl ether, dipropylene glycol dimethyl ether, dipropylene glycol monobutyl ether, dipropylene glycol dibutyl ether, tripropylene glycol dimethyl ether, dihydroterpineol acetate, terpineol, dihydroterpineol, and dihydroterpineol acetate.
[0047] The organic solvent is preferably in the range of 5 to 500 parts by weight per 1 part by weight of the cellulose fiber composite. The above-mentioned cellulose fiber composite is mixed with the above-mentioned organic solvent according to the intended use, and the cellulose fibers are redispersed using the above-mentioned dispersing device or the like to obtain an organic solvent dispersion composition. The cellulose fiber composite material used as the raw material may contain the organic solvent used in the above-mentioned production process. The organic solvent contained in the cellulose fiber composite material is preferably removed by a method such as desolvation under reduced pressure. The composition of the first aspect described above can be widely used as ink, adhesive, compounding material, raw material for various parts, etc.
[0048] <Second Configuration: Resin Precursor Dispersion Composition> The second composition is a composition containing the cellulose fiber composite and a resin precursor. The composition according to the second aspect can be prepared in the same manner as the composition according to the first aspect, that is, by mixing a cellulose fiber composite and a resin precursor, carrying out the above-mentioned dispersion treatment, and, if necessary, removing the organic solvent present in the cellulose fiber composite.
[0049] Here, the resin precursor is a material that forms a polymeric material through a polymerization reaction or the like, and examples of usable resin precursors include (meth)acrylate compounds, vinyl compounds, allyl compounds, acid anhydrides, amine compounds, isocyanate compounds, epoxy compounds, and reactive silicone compounds.
[0050] Among these, (meth)acrylate compounds, vinyl compounds, isocyanate compounds and epoxy compounds are preferably used because of their high reactivity and versatility. Examples of the (meth)acrylate compound include monofunctional (meth)acrylate compounds such as alkyl, methoxyethylene oxide, bisphenol A skeleton, and aromatic (meth)acrylate compounds having 1 to 30 carbon atoms; bifunctional (meth)acrylate compounds such as ethylene glycol, propylene glycol, bisphenol A skeleton, fluorene skeleton, and tricyclodecane skeleton di(meth)acrylate compounds; and more polyfunctional (meth)acrylate compounds such as glycerin skeleton (meth)acrylate compounds, (mono-, di-, and tri-)trimethylolpropane skeleton and isocyanurate skeleton polyfunctional (meth)acrylate compounds, and (mono-, di-, and tri-)pentaerythritol skeleton polyfunctional (meth)acrylate compounds.
[0051] Examples of the vinyl compound include divinylbenzene, styrene, styrene derivatives, vinylnaphthalene, and acrylonitrile.
[0052] Examples of the isocyanate compound include isocyanates such as hexamethylene diisocyanate (HDI), tolylene diisocyanate (TDI), and diphenylmethane diisocyanate (MDI), and polyisocyanates such as adducts of these with alcohols.
[0053] Examples of the epoxy compound include bisphenol A-based, bisphenol F-based, bisphenol S-based, novolak phenol-based, resol phenol-based, naphthalene-based, biphenyl-based, and hydrogenated compounds thereof; polyfunctional epoxy compounds such as glycidyl ether-based, glycidyl amide-based, glycidyl ester-based, and alicyclic epoxy-based compounds having an isocyanurate or polybutadiene skeleton; and monofunctional epoxy compounds which are reactive diluents.
[0054] As the reactive silicone compound, for example, various RTV silicone rubbers and silicones for LIM (Liquid Injection Molding) manufactured by Shin-Etsu Chemical Co., Ltd. can be used. However, without being limited thereto, various RTV silicone rubbers and silicone materials for LIM, such as condensation systems such as two-liquid systems, addition systems, and UV curing systems, can also be used.
[0055] The compounding ratio of the cellulose fiber composite to the resin precursor is preferably in the range of 5 to 100 times the weight of the cellulose fiber composite. In addition, when a (meth)acrylate compound is used, it is also possible to add a polymerization inhibitor such as hydroquinones to improve storage stability, as in the conventional technology. Furthermore, when the cellulose fiber composite contains an organic solvent, it can be removed by carrying out a heating or reduced pressure solvent removal process using a known device as necessary.
[0056] The composition of the second aspect can be widely used as a UV curing material, a material for 3D modeling, a thermosetting material, an adhesive, a compounding material, a raw material for various parts, etc.
[0057] <Third Configuration: Resin Dispersion Composition> The third composition is a composition comprising the cellulose fiber composite and a resin. Examples of the resin include various acrylic resins, polystyrene, acrylonitrile-styrene resin, acrylonitrile-butadiene-styrene resin, various polycarbonates, polyethylene, polypropylene, polyvinyl chloride, polyvinylidene chloride, nitrile rubber, butadiene rubber, poly(styrene-butadiene), polyisoprene, ethylene-propylene-diene rubber, various polyesters, various polyurethanes, various nylon resins (polyamides), polyacetal, polyvinyl acetals such as polyvinyl butyral, cellulose resins such as ethyl cellulose, cellulose acetate butyrate, and cellulose acetate, polyphenylene oxide, polyphenylene sulfide, phenol resins, silicone resins, and fluorine-based resins.
[0058] The method for producing the composition according to the third aspect is, for example, a method in which the above-mentioned cellulose fiber composite and the above-mentioned resin are mixed, and then mechanically kneaded and dispersed using a kneader, a continuous twin-screw kneader, etc., while heating as necessary. Also preferably applicable is a method in which a resin that is soluble in an organic solvent is selected from the above-mentioned resins, the resin is dissolved, the cellulose fiber composite is mixed therein, stirred, uniformly dispersed, and then the organic solvent is removed. It is preferable to use these methods appropriately depending on the type of resin used.
[0059] The compounding ratio of the cellulose fiber composite to the resin is preferably in the range of 5 to 100 parts by weight of the resin per part by weight of the cellulose fiber composite.
[0060] The third composition can be used as a raw material for various applications as an amorphous material or an amorphous material containing various organic solvents. It can also be applied to various parts, etc. as a bulk, film, spherical, fibrous, or other structure formed from itself by hot molding, mechanical processing, etc. Furthermore, it can be applied as a film shape formed by coating or melt molding, or in a form laminated on another film substrate.
[0061] <Optional components in the composition of the present invention> The composition of the present invention may contain a variety of materials in addition to the above-mentioned dispersant, cellulose fiber, organic solvent, resin precursor, and resin. Examples of these include surfactants, plasticizers, viscosity modifiers, defoamers, leveling agents, stabilizers such as UV absorbers and antioxidants, dyes, polymer particles, inorganic particles such as metal particles and ceramic particles, epoxy curing agents, curing promotion catalysts, polymerization initiators, acid anhydrides capable of reacting with epoxy compounds and isocyanate compounds, polyfunctional alcohols, polyfunctional amines, etc. These materials can be blended, for example, in the range of 0.001 to 90% by weight based on the total weight of the composition. EXAMPLES
[0062] Hereinafter, examples and comparative examples will be shown for the method for producing a cellulose fiber composite and a cellulose fiber composite composition according to the present invention, but the present invention is not limited to these examples.
[0063] [Synthesis of Dispersant] <Synthesis Example 1: Dispersant A> 100 parts by weight of ethyl cellulose (Dow Chemical Company's "Ethocel STD-10", number average molecular weight: 22,700) and 300 parts by weight of ethyl acetate were added to a reaction vessel and mixed to prepare a solution in which the ethyl cellulose was uniformly dissolved in ethyl acetate. To the above solution, 1.14 parts by weight of methacrylic acid (manufactured by Fuji Film Wako Pure Chemical Industries, Ltd.), 1.66 parts by weight of diisopropylcarbodiimide (manufactured by Fuji Film Wako Pure Chemical Industries, Ltd.) as a condensation agent, and 0.08 parts by weight of dimethylaminopyridine (manufactured by Fuji Film Wako Pure Chemical Industries, Ltd.) as a reaction accelerator were added and mixed. The mixture was then stirred at 40°C for 12 hours to carry out the reaction, and methacrylate groups were introduced into some of the hydroxyl groups of the ethyl cellulose via ester bonds (the number of methacrylate groups introduced was three on average per ethyl cellulose chain). The introduction of functional groups was confirmed by the formation of ester bonds in FT-IR spectrum measurement. The reaction solution was heated to 50°C, and nitrogen was bubbled into the solution using a glass tube, and nitrogen substitution was performed while stirring. 20 parts by weight of benzyl methacrylate was mixed as a vinyl monomer, and 0.4 parts by weight of azoisobutyronitrile (AIBN) (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was added as a polymerization initiator, and a polymerization reaction was carried out at 80°C for 8 hours. The concentration of the polymer component in the solution after the reaction was 29% by weight. A part of the produced polymer was purified and subjected to GPC molecular weight analysis and 1 Composition analysis by 1 H-NMR revealed that a polymer almost identical to the above-mentioned charged composition of ethyl cellulose and benzyl methacrylate was produced, and this was used as a dispersant.
[0064] <Synthesis Example 2: Dispersant B> 100 parts by weight of ethyl cellulose (Dow Chemical Company's "Ethocel STD-20", number average molecular weight: 39,000) and 300 parts by weight of ethyl acetate were added to a reaction vessel and mixed to prepare a solution in which the ethyl cellulose was uniformly dissolved in ethyl acetate. To the above solution, 1.1 parts by weight of methacrylic acid, 1.62 parts by weight of diisopropylcarbodiimide as a condensing agent, and 0.08 parts by weight of dimethylaminopyridine as a reaction accelerator were added and mixed. The mixture was then stirred at 40°C for 12 hours to carry out the reaction, and methacrylate groups were introduced into some of the hydroxyl groups of the ethyl cellulose via ester bonds (the number of methacrylate groups introduced was 5 on average per ethyl cellulose chain). The introduction of functional groups was confirmed by the formation of ester bonds in FT-IR spectrum measurement. The reaction solution was heated to 50°C, and nitrogen was bubbled into the solution using a glass tube, and nitrogen substitution was performed while stirring. Furthermore, 50 parts by weight of butyl methacrylate was mixed as a vinyl monomer, and 0.5 parts by weight of azoisobutyronitrile (AIBN) was added as a polymerization initiator, and a polymerization reaction was carried out at 80°C for 8 hours. The concentration of the polymer component in the solution after the reaction was 33% by weight. A part of the produced polymer was purified and subjected to GPC molecular weight analysis and 1 Composition analysis by 1 H-NMR revealed that a polymer almost identical to the above-mentioned charged composition of ethyl cellulose and butyl methacrylate was produced, and this was used as a dispersant.
[0065] <Synthesis Example 3: Dispersant C> 100 parts by weight of ethyl cellulose (Dow Chemical Company's "Ethocel STD-10", number average molecular weight: 22,700) and 300 parts by weight of ethyl acetate were added to a reaction vessel and mixed to prepare a solution in which the ethyl cellulose was uniformly dissolved in ethyl acetate. To the above solution, 1.14 parts by weight of methacrylic acid, 1.66 parts by weight of diisopropylcarbodiimide as a condensation agent, and 0.08 parts by weight of dimethylaminopyridine (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) as a reaction accelerator were added and mixed. The mixture was then stirred at 40°C for 12 hours to carry out the reaction, and methacrylate groups were introduced into some of the hydroxyl groups of the ethyl cellulose via ester bonds (the number of methacrylate groups introduced was three on average per ethyl cellulose chain). The introduction of functional groups was confirmed by the formation of ester bonds in FT-IR spectrum measurement. The reaction solution was heated to 50°C, and nitrogen was bubbled into the solution using a glass tube, and nitrogen substitution was performed while stirring. Furthermore, 50 parts by weight of dicyclopentanyl methacrylate (Hitachi Chemical Co., Ltd.) was mixed as a vinyl monomer, and 0.4 parts by weight of azoisobutyronitrile (AIBN) was added as a polymerization initiator, and a polymerization reaction was carried out at 80°C for 8 hours. The concentration of the polymer component in the solution after the reaction was about 27% by weight. A part of the produced polymer was purified and subjected to GPC molecular weight analysis and 1 Composition analysis by 1 H-NMR revealed that a polymer almost identical to the above-mentioned charged composition of ethyl cellulose and dicyclopentanyl methacrylate was produced, and this was used as a dispersant.
[0066] <Synthesis Example 4: Dispersant D> 100 parts by weight of ethyl cellulose (Dow Chemical Company's "Ethocel STD-4", number average molecular weight: 13,700) and 300 parts by weight of ethyl acetate were added to a reaction vessel and mixed to prepare a solution in which the ethyl cellulose was uniformly dissolved in ethyl acetate. To the above solution, 2.32 parts by weight of 3-mercaptopropionic acid (Tokyo Chemical Industry Co., Ltd.), 2.76 parts by weight of diisopropylcarbodiimide as a condensing agent, and 0.13 parts by weight of dimethylaminopyridine as a reaction accelerator were added and mixed. The mixture was then stirred at 40°C for 12 hours to carry out the reaction, and thiol groups were introduced into some of the hydroxyl groups of the ethyl cellulose via ester bonds (an average of three thiol groups were introduced per ethyl cellulose chain). The introduction of functional groups was confirmed by the formation of ester bonds in FT-IR spectrum measurement. The reaction solution was heated to 50°C, and nitrogen was bubbled into the solution using a glass tube, and nitrogen substitution was performed while stirring. Furthermore, 10 parts by weight of isobornyl methacrylate (manufactured by Tokyo Chemical Industry Co., Ltd.) was mixed as a vinyl monomer, and 0.4 parts by weight of azoisobutyronitrile (AIBN) was added as a polymerization initiator, and a polymerization reaction was carried out at 80°C for 8 hours. The concentration of the polymer component in the solution after the reaction was 27% by weight. A part of the produced polymer was purified and subjected to GPC molecular weight analysis and 1 Composition analysis by 1 H-NMR revealed that a polymer almost identical to the above-mentioned charged composition of ethyl cellulose and isobornyl methacrylate was produced, and this was used as a dispersant.
[0067] <Synthesis Example 5: Dispersant E> 100 parts by weight of ethyl cellulose (Dow Chemical Company's "Ethocel STD-20", number average molecular weight: 39,000) and 300 parts by weight of ethyl acetate were added to a reaction vessel and mixed to prepare a solution in which the ethyl cellulose was uniformly dissolved in ethyl acetate. 1.36 parts by weight of 3-mercaptopropionic acid, 1.62 parts by weight of diisopropylcarbodiimide as a condensing agent, and 0.08 parts by weight of dimethylaminopyridine as a reaction accelerator were added to the above solution and mixed. The mixture was then stirred at 40°C for 12 hours to carry out the reaction, and thiol groups were introduced into some of the hydroxyl groups of the ethyl cellulose via ester bonds (an average of five thiol groups were introduced per ethyl cellulose chain). The introduction of functional groups was confirmed by the formation of ester bonds in FT-IR spectrum measurement. The reaction solution was heated to 50°C, and nitrogen was bubbled into the solution using a glass tube, and nitrogen substitution was performed while stirring. Furthermore, 20 parts by weight of dicyclopentanyl methacrylate was mixed as a vinyl monomer, and 0.4 parts by weight of azoisobutyronitrile (AIBN) was added as a polymerization initiator, and a polymerization reaction was carried out at 80°C for 8 hours. The concentration of the polymer component in the solution after the reaction was 29% by weight. A part of the produced polymer was purified and subjected to GPC molecular weight analysis and 1 Composition analysis by 1 H-NMR revealed that a polymer almost identical to the above-mentioned charged composition of ethyl cellulose and dicyclopentanyl methacrylate was produced, and this was used as a dispersant.
[0068] [Preliminary dehydration and solvent replacement of cellulose fiber aqueous dispersion] <Preliminary dehydration example 1> 50 parts by weight of TEMPO oxidation CNF (2% CNF solids content aqueous dispersion: Daiichi Kogyo Seiyaku Co., Ltd.) and 1,000 parts by weight of propylene glycol monomethyl ether (PGME) as an amphipathic organic solvent were added to a glass container, and the mixture was stirred and mixed for 30 minutes using a high-speed stirrer. The mixture was then filtered by suction using No. 2 filter paper (particle retention diameter > 5 μm) and repeatedly washed with 500 parts by weight of PGME to obtain a mixture of CNF and PGME. The weight of the mixture was approximately 73.5 g. It was confirmed that there was no non-volatile matter in the filtrate after the above operation. By measuring the non-volatile matter in the deposit, the CNF content in the deposit can be determined. The CNF content in the actually extracted deposit was 1.36% by weight. The moisture content was also less than 1.0% by weight.
[0069] <Preliminary dehydration example 2> 50 parts by weight of TEMPO oxidation CNF (aqueous dispersion of CNF solid content 2% by weight: manufactured by Daiichi Kogyo Seiyaku Co., Ltd.) and 1,000 parts by weight of ethylene glycol monomethyl ether (EGME) as an amphipathic organic solvent were added to a glass container, and the mixture was stirred and mixed for 30 minutes using a high-speed stirrer. The mixture was then filtered under suction using No. 2 filter paper and repeatedly washed with EGME to obtain a mixture of CNF and EGME, weighing approximately 75 g. It was confirmed that there was no non-volatile matter in the filtrate after the above operation. By measuring the non-volatile matter in the deposit, the CNF content in the deposit can be determined. The CNF content in the actually extracted deposit was 1.33% by weight. The moisture content was also less than 1.0% by weight.
[0070] <Preliminary dehydration example 3> 50 parts by weight of TEMPO oxidation CNF (aqueous dispersion of CNF solid content 2% by weight: manufactured by Daiichi Kogyo Seiyaku Co., Ltd.) and 1,000 parts by weight of dimethylformamide (DMF) as an amphipathic organic solvent were added to a glass container, and the mixture was stirred and mixed for 30 minutes using a high-speed stirrer. The mixture was then filtered under suction using No. 2 filter paper and repeatedly washed with DMF to obtain a mixture of CNF and DMF, weighing approximately 70 g. It was confirmed that there was no non-volatile matter in the filtrate after the above operation. By measuring the non-volatile matter in the deposit, the CNF content in the deposit can be determined. The CNF content in the actually extracted deposit was 1.43% by weight. The moisture content was also less than 1.0% by weight.
[0071] [Preparation of cellulose fiber composite] Using the following process, the dispersant prepared in the above synthesis example was adsorbed onto the surface of water-dispersed TEMPO-oxidized CNF, producing a composite of CNF and dispersant that enables uniform dispersion of CNF in hydrophobic media. <Example 1> The mixture of CNF and PGME obtained in the above-mentioned Preliminary Dehydration Example 1 was weighed out into a glass container so that it was 20 parts by weight (the weight of CNF contained was approximately 0.27 parts by weight), and further mixed with 0.94 parts by weight of ethyl acetate solution containing dispersant A prepared in Synthesis Example 1 (0.27 parts by weight in terms of the solid content of the dispersant) and 100 parts by weight of ethylene glycol dimethyl ether (EGDME), and the mixture was stirred and mixed for 30 minutes using a high-speed stirrer to obtain a dispersion in which the dispersant had been adsorbed onto the CNF. Furthermore, the above dispersion was suction filtered at room temperature (25°C) using No. 2 filter paper (retention particle size >5 μm), and then washed with 100 parts by weight of EGDME, obtaining CNF (cellulose fiber composite) with the dispersant adsorbed on the filter paper as the filtration product. By measuring the non-volatile content of the filtered product on the filter paper and the filtrate after suction filtration, the amount of organic solvent in the filtered product and the amount of dispersant adsorbed to the CNF can be determined. As a result, it was found that the organic solvent (EGDME) was contained in the filtered product at approximately 95% by weight, and that approximately 42 parts by weight of dispersant was adsorbed per 100 parts by weight of CNF. Since the amount of dispersant added was 100 parts by weight per 100 parts by weight of CNF, this means that approximately 42% by weight of the added amount of dispersant was adsorbed. In addition, the dispersant in the filtrate that was not adsorbed by the CNF was 1 H - NMR analysis revealed that the acrylic polymer component (homopolymer of benzyl methacrylate) had increased compared to the initial dispersant composition, which meant that the grafted ethyl cellulose and acrylic polymer, which had the targeted dispersant structure, was preferentially adsorbed onto the CNF. Furthermore, the moisture content in the product was measured and found to be 0.5% by weight or less.The moisture content in the products in the following Examples 2 to 17 was also 0.5% by weight or less. (Note that the above-mentioned composite of CNF and dispersant may be used with or without the ethylene glycol dimethyl ether used in the preparation.)
[0072] <Examples 2 to 5> Using dispersants B to E shown in Synthesis Examples 2 to 5 as dispersants, cellulose fiber composites were produced under the same organic solvent amount and CNF to dispersant weight ratio as in Example 1. The conditions are shown in Table 1.
[0073] <Examples 6 to 7> The amount of dispersant added was increased in Example 1. The conditions are as shown in Table 1.
[0074] <Example 8> The mixture of CNF and EGME obtained in the procedure of Preliminary Dehydration Example 2 was used. The other conditions were the same as in Example 1.
[0075] <Example 9> The mixture of CNF and EGME obtained in the procedure of Preliminary Dehydration Example 2 was used. The other conditions were the same as in Example 5.
[0076] <Example 10> The mixture of CNF and DMF obtained in the procedure of Preliminary Dehydration Example 3 was used. The other conditions were the same as in Example 1.
[0077] <Example 11> The mixture of CNF and DMF obtained in the procedure of Preliminary Dehydration Example 3 was used. The other conditions were the same as in Example 5.
[0078] <Example 12> In the treatment for adsorbing the dispersant in Example 1, isopropyl alcohol (IPA) was used as the organic solvent instead of EGDME.
[0079] <Example 13> In the treatment for adsorbing the dispersant in Example 5, isopropyl alcohol (IPA) was used as the organic solvent instead of EGDME.
[0080] <Example 14> In the treatment for adsorbing the dispersant in Example 8, isopropyl alcohol (IPA) was used as the organic solvent instead of EGDME.
[0081] <Example 15> In the treatment for adsorbing the dispersant in Example 9, isopropyl alcohol (IPA) was used instead of EGDME as the organic solvent.
[0082] <Example 16> In the treatment for adsorbing the dispersant in Example 10, isopropyl alcohol (IPA) was used as the organic solvent instead of EGDME.
[0083] <Example 17> In the treatment for adsorbing the dispersant in Example 11, isopropyl alcohol (IPA) was used as the organic solvent instead of EGDME.
[0084] <Example 18> Without carrying out preliminary dehydration, the adsorption of the dispersant was carried out simultaneously with the dehydration treatment as described below. 10 parts by weight of TEMPO oxidation CNF (2% by weight CNF solid content aqueous dispersion: Daiichi Kogyo Seiyaku Co., Ltd.) (CNF solid content is approximately 0.2 parts by weight), 100 parts by weight of PGME, and 100 parts by weight of EGDME were added to a glass container and stirred and mixed for 30 minutes using a high-speed stirrer. Furthermore, 0.69 parts by weight of ethyl acetate solution containing dispersant A prepared in Synthesis Example 1 (solid content weight of dispersant is equal to the amount of CNF) was added and stirred at high speed in the same manner. The mixture was then filtered by suction using No. 2 filter paper, and repeatedly washed with 200 parts by weight of EGDME to obtain CNF (cellulose fiber composite) with the dispersant adsorbed on the filter paper as the filtration product. By measuring the non-volatile content of the filtered product on the filter paper and the filtrate after suction filtration, the amount of organic solvent in the filtered product and the amount of dispersant adsorbed to the CNF can be determined. As a result, it was found that the organic solvent (EGDME) was contained in the filtered product at about 55% by weight, and that about 45 parts by weight of dispersant was adsorbed per 100 parts by weight of CNF. Since the amount of dispersant added was 100 parts by weight per 100 parts by weight of CNF, this means that about 45% by weight of the added amount of dispersant was adsorbed. The moisture content in the product was 0.5% by weight or less. In the following Examples 19 to 22, the moisture content in the product was also 0.5% by weight or less.
[0085] <Examples 19 to 22> Using dispersants B to E shown in Synthesis Examples 2 to 5 as dispersants, cellulose fiber composites were produced under the same organic solvent amount and CNF to dispersant weight ratio as in Example 18. The conditions are shown in Table 1.
[0086] [Preparation of Cellulose Fiber Composite Composition] The cellulose fiber composites (containing organic solvents) prepared in Examples 1 to 22 were used, and the CNF content was weighed out to be 2 parts by weight. 98 parts by weight of A-TMPT was mixed therein, and the CNF was dispersed using a high-speed stirrer. Then, the organic solvent contained therein was removed using a reduced pressure desolvation device. Furthermore, 9 parts by weight of Irgacure TPO was mixed as a photoinitiator. By the above operations, a cellulose fiber composite composition (resin precursor dispersion composition) was obtained in which the cellulose fibers were redispersed in a polyfunctional acrylic monomer (A-TMPT: trimethylolpropane triacrylate: manufactured by Shin-Nakamura Chemical Co., Ltd.) which is a resin precursor.
[0087] [Evaluation of Cellulose Fiber Composite Composition] The cellulose fiber composite composition obtained above was coated on a release-treated polyethylene terephthalate film using a blade coater, and then cured with an integrated energy of 1000 mJ using a UV irradiation device with a high-pressure mercury light source, and peeled off from the release film to obtain a transparent film with a thickness of about 100 μm. Various properties of the obtained cellulose fiber-dispersed resin film were evaluated.
[0088] <Dispersibility> The dispersion state of cellulose fibers (CNF) in the film was evaluated by observation using a microscope and a polarizing microscope. The dispersion state of the CNF was evaluated under polarized light at 500x magnification as the evaluation standard for dispersibility. A level where no aggregates were observed was marked as ○, a level where only a few aggregates were observed was marked as △, and a level where many aggregates were observed was marked as ×. These results are shown in Table 1 in correspondence with each example number of the cellulose fiber composite used as the raw material.
[0089] <Film transparency> The transparency of the film was evaluated visually. The evaluation criteria were as follows: no turbidity at all in the transmission state was rated as O, and turbidity was rated as X. These evaluation results are also shown in Table 1, corresponding to each example number of the cellulose fiber composite material used as the raw material.
[0090] <Mechanical properties> The tensile strength of the film was measured (SS curve) using a tensile tester (AG-10N) manufactured by Shimadzu Corporation, and the tensile modulus was measured. The tensile modulus of the A-TMPT film alone, in which CNF was not dispersed, was 1.6 GPa. Based on this, an improvement of 20% or more was evaluated as ○, less than 20% to the same as △, and a decrease was evaluated as ×. These evaluation results are also shown in Table 1, corresponding to each example number of the cellulose fiber composite material used as the raw material.
[0091] [Table 1]
[0092] [Comparative Experiment] Below, comparative experiments were carried out to confirm the superiority of the present invention. <Comparative Example 1> In Example 18, an equal amount of dispersant was mixed with CNF, and after dispersion, filtration was not performed. Instead, a resin precursor was mixed, and water and organic solvent were removed using a reduced pressure desolvation device. Removal of water and organic solvent took a long time compared to the filtration method. Furthermore, a film sample for evaluation was prepared and evaluated in the same manner as above. As a result, the dispersibility of CNF and the transparency of the film were good, but the mechanical properties were slightly inferior to those of the examples. It was assumed that the poor mechanical properties were due to the influence of the vinyl homopolymer contained in the dispersant. The results are shown in Table 1.
[0093] <Comparative Example 2> The same treatment was carried out as in Comparative Example 1, except that the amount of dispersant relative to the CNF was halved. Furthermore, a film sample for evaluation was prepared and evaluated in the same manner as above. As a result, it was found that the dispersibility of CNF was slightly inferior to that of the Examples. Furthermore, the mechanical properties were also slightly inferior to those of the Examples. It was presumed that the cause of the inferior mechanical properties was the influence of the vinyl homopolymer contained in the dispersant and the reduced dispersibility of CNF. The results are shown in Table 1.
[0094] <Comparative Example 3> In Comparative Example 1, the treatment was carried out without adding a dispersant. Furthermore, a film sample for evaluation was prepared and evaluated in the same manner as above. As a result, the dispersibility of CNF, transparency, and mechanical properties were all significantly inferior to those of the Examples. This result shows the effect of the dispersant of the present invention. The results are shown in Table 1.
[0095] From the above examples and comparative examples, it was found that the present invention improves the dispersibility of CNF in resins, etc., and also improves the physical properties of the resulting composition such as CNF-dispersed resin by removing vinyl homopolymers, etc. contained in the dispersant. Furthermore, it was also found that the water contained in the CNF aqueous dispersion can be efficiently removed, which contributes to reducing the cost of the process.
Claims
1. a step of preparing a dispersion liquid in which cellulose fibers are dispersed in an organic solvent or a mixed solvent of an organic solvent and water by using a copolymer in which a vinyl polymer is grafted onto a cellulose derivative as a dispersant; a step of recovering the cellulose fibers with the dispersant adsorbed thereon as the target cellulose fiber composite by separating from the dispersion a liquid containing an excess dispersant not adsorbed to the cellulose fibers and a vinyl homopolymer not grafted to the cellulose derivative; A method for producing a cellulose fiber composite, comprising:
2. The method for producing a cellulose fiber composite according to claim 1, further comprising the step of washing the dispersing agent with an amphipathic organic solvent.
3. 3. A method for producing a cellulose fiber composite composition, comprising the steps of producing a cellulose fiber composite by the method according to claim 1 or 2, and then mixing the cellulose fiber composite with a dispersed material, which is an organic solvent, a resin and / or a resin precursor, thereby redispersing the cellulose fibers in the dispersed material.
Citation Information
Patent Citations
Gurafutokatatoruitoseruroosunokyushuseikongobutsu
JP1976082991A
Electrochromic display composition
JP1982057779A
Fiber composite material, optical film, method for producing optical film, and polarizing plate and liquid crystal display using the same
JP2011068707A
Method for producing graft polymer modified cellulose fiber
JP2013234283A
Resin composition containing dispersant for dispersing cellulose and macromolecular dispersant for cellulose
JP2016104865A