High bio-based waterborne polyurethane resin as well as preparation method and application thereof

By combining petroleum-based polyol with castor oil-modified polyol in aqueous polyurethane, and through specific chemical reaction steps, the mechanical properties and water resistance of the polyurethane are improved, and the poor stability of existing aqueous polyurethanes in humid environments is solved. The problem of insufficient environmental friendliness has achieved the multiple performance improvement of high-biologically based water-based polyurethane resin.

CN118930789AInactive Publication Date: 2024-11-12GUANGDONG RITOP FINE CHEM

Patent Information

Application Number
CN202411051660.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-01
Publication Date
2024-11-12
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing water-based polyurethane has poor mechanical stability in humid environments. The hardness, elasticity and wear resistance of water-based polyurethane made of bio-based raw materials are not as good as that of water-based polyurethane made of petrochemical-based raw materials. The reduction of petroleum reserves and strict carbon emission standards have led to development. Face challenges.

Method used

Using a high bio-based aqueous polyurethane resin, the amount of petroleum-based polyol is reduced by combining petroleum-based polyol with castor oil-modified polyol, and the prepolymerization reaction between isocyanate and polyol, cross-linking of methyl methacrylate and Chain extension reaction improves the mechanical strength, wear resistance and hydrolysis resistance of polyurethane.

Benefits of technology

It has achieved good heat resistance, wear resistance, mechanical strength and hydrolysis resistance of high bio-based water-based polyurethane resin, meeting the application needs of different fields, while reducing environmental pollution and meeting the requirements of sustainable development.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004975097060000041
    Figure BDA0004975097060000041
  • Figure BDA0004975097060000051
    Figure BDA0004975097060000051
  • Figure BDA0004975097060000052
    Figure BDA0004975097060000052
Patent Text Reader

Abstract

The invention relates to high-bio-based waterborne polyurethane resin as well as a preparation method and application thereof, and belongs to the technical field of polyurethane resin. The polyurethane resin is prepared from the following components in parts by weight: 15 to 30 parts of isocyanate, 80 to 100 parts of polyol, 5 to 10 parts of methyl methacrylate, 0.5 to 2 parts of chain extender, 0.2 to 0.6 part of catalyst, 1 to 2 parts of initiator, 5 to 10 parts of neutralizer, 2 to 10 parts of emulsifier and 150 to 400 parts of water, wherein the polyhydric alcohol comprises petroleum-based polyhydric alcohol and castor oil modified polyhydric alcohol in a mass ratio of 1: (8-10). The polyurethane resin is excellent in strength, wear resistance, water resistance and the like, and can meet various application requirements. And compared with other synthetic polyols, the castor oil modified polyols are relatively low in price and have cost benefits. Meanwhile, the source is wide and easy to obtain, and the stability and sustainability of production are guaranteed.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of waterborne polyurethane, and in particular to a high-biobased waterborne polyurethane resin and a preparation method and application thereof. Background Art

[0002] Waterborne polyurethane is a multifunctional papermaking additive that can be used as a surface sizing agent, adhesive, retention and drainage aid, etc. Waterborne polyurethane has the advantages of being non-toxic, having good film-forming properties, good structural adjustability, and being easy to modify, and it occupies an important position in the field of papermaking additives. At present, the raw materials of waterborne polyurethane mainly rely on petroleum resources. With the decreasing petroleum reserves and the strict control of the country's carbon emission standards, the development of waterborne polyurethane is facing increasingly severe challenges.

[0003] Common waterborne polyurethanes made from bio-based raw materials may have poor hydrolysis resistance, which will affect their mechanical stability in humid environments. The intermolecular forces (such as hydrogen bonds) that may be formed by bio-based polyols are different from those of petrochemical-based raw materials, so the hardness, elasticity and wear resistance of polyurethanes made from bio-based raw materials are not as good as those made from pure petrochemical-based raw materials. Summary of the invention

[0004] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a high-biobased waterborne polyurethane resin and a preparation method and application thereof, which reduces the amount of petroleum-based polyols used and also has good heat resistance, wear resistance, hydrolysis resistance, mechanical strength and yellowing resistance, and can meet the application requirements of different fields.

[0005] To achieve the above object, the technical solution adopted by the present invention is:

[0006] In a first aspect, the present invention provides a high bio-based waterborne polyurethane resin, comprising the following components in parts by weight: 15 to 30 parts of isocyanate, 80 to 100 parts of polyol, 5 to 10 parts of methyl methacrylate, 0.5 to 2 parts of chain extender, 0.2 to 0.6 parts of catalyst, 1 to 2 parts of initiator, 5 to 10 parts of neutralizer, 2 to 10 parts of emulsifier and 150 to 400 parts of water; wherein the polyol comprises a petroleum-based polyol and a castor oil-modified polyol in a mass ratio of 1: (8 to 10).

[0007] Preferably, the high bio-based waterborne polyurethane resin comprises the following components in parts by weight: 18 to 25 parts of isocyanate, 95 to 100 parts of polyol, 0.5 to 1.5 parts of chain extender, 0.3 to 0.5 parts of catalyst, 1 to 2 parts of initiator, 4 to 6 parts of emulsifier and 180 to 360 parts of water.

[0008] Preferably, the chain extender is at least one of an aromatic diamine chain extender, an aromatic diol chain extender, an aspartic acid ester, a polyurethane chain extender, an epoxy chain extender, and a phosphite chain extender. More preferably, the number average molecular weight of the chain extender is 150-155.

[0009] Preferably, the neutralizing agent is at least one of triethylamine, triethanolamine, sodium hydroxide, potassium hydroxide, sodium carbonate, sodium acetate, sodium pyrophosphate, ammonia water, hydrochloric acid, phosphoric acid, formic acid, acetic acid, aminoacetic acid, 2-amino-2-methyl-1-propanol, and sodium bicarbonate, and more preferably potassium hydroxide.

[0010] Preferably, the initiator is benzoyl peroxide.

[0011] Preferably, the emulsifier is polyvinylpyrrolidone (PVP).

[0012] Preferably, the catalyst is dimethylaminoethoxyethanol and / or pentamethyldiethylenetriamine.

[0013] Preferably, the isocyanate is at least one of an aromatic diisocyanate and an aliphatic diisocyanate.

[0014] Preferably, the petroleum-based polyol is at least one of 1,4-butanediol, 1,6-hexanediol, neopentyl glycol, dipropylene glycol, and trimethylolpropane.

[0015] Preferably, the mass ratio of the isocyanate group in the isocyanate is 15-20%. After testing, if it exceeds 20%, the tensile strength, wear resistance and water resistance of the polyurethane will be reduced, so it is appropriate to set the mass ratio of the isocyanate group to 15-20%. Among them, the determination of the isocyanate (-NCO) value is measured by the di-n-butylamine method.

[0016] Preferably, the hydroxyl value of the castor oil modified polyol is 270-290 mgKOH / g. The use of castor oil modified polyol within this range can increase the molecular weight and crosslinking density of polyurethane, improve its mechanical strength and chemical resistance, and also take into account the flexibility and processing properties of the material. The acid value is 0.1-0.2 mgKOH / g. Within this acid value range, the polyurethane can have viscosity stability and good reactivity.

[0017] Preferably, the viscosity of the high bio-based waterborne polyurethane resin is 2100-2600 mPa·s, more preferably 2100 mPa·s. Therefore, within this viscosity range, the polyurethane resin of the present invention has high solid strength and durability, and also has better mechanical properties and wear resistance. Therefore, it can be used to prepare sealant products.

[0018] In a second aspect, the present invention provides a method for preparing the highly bio-based waterborne polyurethane resin, comprising the following steps:

[0019] S1. Preparation of prepolymer: stirring and mixing polyol, isocyanate and catalyst, and heating to carry out prepolymerization reaction to obtain prepolymer;

[0020] Preparation of S2 polymer: mixing the prepolymer, methyl methacrylate and initiator, heating to carry out cross-linking reaction, and obtaining a polymer;

[0021] S3: mixing the polymer with part of water and a chain extender to carry out a chain extension reaction, and then adding a neutralizer to obtain a waterborne polyurethane; S4: mixing the waterborne polyurethane with the remaining water and an emulsifier to emulsify the waterborne polyurethane to obtain the high bio-based waterborne polyurethane resin.

[0022] In the preparation method of the waterborne polyurethane resin of the present invention, the synthesis of polyurethane and the polymerization with methyl methacrylate (PMMA) and the cross-linking reaction are carried out step by step, thus ensuring that the polyurethane can be fully polymerized, and then methyl methacrylate is in-situ polymerized to form PMMA and then cross-linked with the polyurethane, thus increasing the cross-linking degree of the two, thereby promoting the performance of the resin.

[0023] Preferably, in step S1, the parameters of the prepolymerization reaction are: temperature of 75-85°C and time of 2-3h. More preferably, in the prepolymerization reaction, the polyol is first mixed uniformly at 50-60°C, then the temperature is raised to 75-85°C and the isocyanate is added, and then the reaction is carried out at 75-85°C to obtain the prepolymer.

[0024] Preferably, in step S2, the parameters of the cross-linking reaction are: temperature of 80-90° C. and time of 2-3 h.

[0025] Preferably, in step S3, the parameters of the chain extension reaction are: temperature of 70-80° C., time of 1-2 h, and when the chain extension reaction is terminated, the system temperature is reduced to 30-40° C.

[0026] In a third aspect, the present invention provides the use of the high bio-based waterborne polyurethane resin in the preparation of coatings, adhesives, fabric coatings and finishing agents, and leather and synthetic leather finishing agents.

[0027] Compared with the prior art, the present invention has the following beneficial effects:

[0028] (1) The high bio-based waterborne polyurethane resin of the present invention adopts bio-based raw materials such as castor oil-modified polyols, which reduces the amount of petroleum-based polyols used. The resin is more easily degraded in the environment, reducing pollution to the environment. The molecular structure of castor oil-modified polyols contains multiple hydroxyl groups, which can react with isocyanates and also compound with a small amount of petroleum-based polyols to form a high molecular weight polyurethane resin. This resin performs well in terms of strength, wear resistance, water resistance, etc., and can meet various application requirements. Moreover, compared with other synthetic polyols, castor oil-modified polyols are relatively low in price and cost-effective. At the same time, they are widely available and easy to obtain, ensuring the stability and sustainability of production.

[0029] (2) The polyurethane resin preparation method is to add methyl methacrylate monomer after synthesizing waterborne polyurethane with isocyanate and polyol, further cross-link to form polymethyl methacrylate modified polyurethane, and then carry out chain extension reaction to increase the cross-linking degree of the polyurethane network, thereby improving its thermal stability and solvent resistance. PMMA modification can improve the surface hardness, wear resistance and scratch resistance of polyurethane. Compared with traditional petroleum-based polyurethane resins, the production process and product of this waterborne polyurethane resin are more environmentally friendly and meet the requirements of sustainable development. DETAILED DESCRIPTION

[0030] In order to better illustrate the purpose, technical solutions and advantages of the present invention, the present invention will be further described below in conjunction with specific embodiments.

[0031] In the embodiments and comparative examples, the experimental methods used are conventional methods unless otherwise specified, and the materials, reagents, etc. used are all commercially available unless otherwise specified.

[0032] The sources of reagents used in the embodiments and comparative examples are as follows:

[0033] Petroleum-based polyols:

[0034] 1,4-Butanediol, 1,6-hexanediol, and trimethylolpropane were purchased from Guangdong Wengjiang Chemical Reagent Co., Ltd.

[0035] Methyl methacrylate: The manufacturer is Guangdong Wengjiang Chemical Reagent Co., Ltd., and the brand number is WB00992.

[0036] Neutralizer:

[0037] Triethylamine, triethanolamine, sodium hydroxide, potassium hydroxide, sodium carbonate, sodium acetate, sodium pyrophosphate, sodium bicarbonate, ammonia water, hydrochloric acid, phosphoric acid, formic acid, and acetic acid were all purchased from Guangdong Wengjiang Chemical Reagent Co., Ltd.

[0038] Glycine and 2-amino-2-methyl-1-propanol were purchased from Shanghai MacLean Biochemical Technology Co., Ltd.

[0039] Initiator:

[0040] Benzoyl peroxide, manufacturer is Guangdong Wengjiang Chemical Reagent Co., Ltd.

[0041] Emulsifier:

[0042] Polyvinyl pyrrolidone, the manufacturer is Guangdong Wengjiang Chemical Reagent Co., Ltd.

[0043] catalyst:

[0044] Pentamethyldiethylenetriamine: The manufacturer is Shanghai MacLean Biochemical Technology Co., Ltd., and the brand number is N822749.

[0045] The raw materials used for castor oil modified polyol are shown in Table 1

[0046] Table 1 Reagent sources and related parameters of castor oil modified polyols

[0047]

[0048]

[0049] The description of the raw materials used for isocyanate is shown in Table 2. The test method for the mass content of isocyanate group is DIN EN ISO 11909.

[0050] Table 2 Sources of isocyanates and related parameters

[0051]

[0052]

[0053] The raw materials used for chain extenders are shown in Table 3.

[0054] Table 3 Sources and related parameters of chain extenders

[0055]

[0056] Examples 1 to 17 and Comparative Examples 1 to 3

[0057] The components and weight parts used in Examples 1 to 17 and Comparative Examples 1 to 13 are shown in Table 4.

[0058] Table 4 Component dosage (parts by weight) in Examples 1 to 17 and Comparative Examples 1 to 13

[0059]

[0060]

[0061] Embodiments 18 to 32

[0062] The components and weight parts used in Examples 18 to 32 are shown in Table 5.

[0063] Table 5 Component dosage in Examples 18 to 32 (parts by weight)

[0064]

[0065]

[0066] Embodiments 33 to 45

[0067] The components and weight parts used in Examples 33 to 45 are shown in Table 6.

[0068] Table 6 Component dosage in Examples 33 to 45 (parts by weight)

[0069]

[0070] Embodiments 46 to 59

[0071] The components and weight parts used in Examples 46 to 59 are shown in Table 7.

[0072] Table 7 Component dosage in Examples 46 to 59 (parts by weight)

[0073]

[0074]

[0075] Comparative Example 4

[0076] The difference between Comparative Example 4 and Example 3 is that: Comparative Example 4 uses epoxy soybean oil-modified dimer acid polyester polyol (purchased from Shanghai Xiaoyan Technology Co., Ltd., brand Nourypol 200) to replace the modified castor oil polyol.

[0077] Comparative Example 5

[0078] The difference between Comparative Example 5 and Example 3 is that in Comparative Example 5, methyl methacrylate and initiator are not added.

[0079] The difference between Comparative Example 6 and Example 3 is that in Comparative Example 6, the polyol, isocyanate, methyl methacrylate, initiator and chain extender are directly mixed.

[0080] The preparation method of the waterborne polyurethane resin of Examples 1 to 58 and Comparative Examples 1 to 4 comprises the following steps:

[0081] S1. Preparation of prepolymer: firstly, the polyol is stirred and mixed uniformly at 50°C, then the temperature is raised to 80°C, isocyanate is added, and then a prepolymerization reaction is carried out at 80°C for 2h to obtain a prepolymer;

[0082] Preparation of S2 polymer: the prepolymer, methyl methacrylate and initiator are mixed, and a cross-linking reaction is carried out at 85° C. for 2.5 hours to obtain a polymer;

[0083] S3: cooling the system to 60° C., then mixing the polymer with a portion of water and a chain extender, performing a chain extension reaction at 75° C. for 1.5 hours, then adding a neutralizing agent, cooling the system temperature to 35° C., and then terminating the chain extension reaction to obtain a waterborne polyurethane;

[0084] S4: mixing the waterborne polyurethane with the remaining water and the emulsifier for emulsification to obtain the high bio-based waterborne polyurethane resin.

[0085] Performance Testing

[0086] 1. Determination of viscosity and molecular weight of polyurethane resin

[0087] The viscosity of the polyurethane resins of Examples 1 to 17 and Comparative Examples 1 to 6 was measured respectively. The viscosity test method is as shown in GB / T 7193-2008 "Test method for unsaturated polyester resins", see Table 8 for details.

[0088] 2. Determination of mechanical properties of polyurethane resin

[0089] The tensile strength and elongation at break of the polyurethane resins of Examples 1 to 32 and Comparative Examples 1 to 6 were measured using GB1040-79 “Plastic Tensile Test Methods”. The data are shown in Table 8.

[0090] 3. Determination of wear resistance of polyurethane resin

[0091] The polyurethane resins of Examples 1 to 32 and Comparative Examples 1 to 6 were respectively made into coating products, and the specific steps were: 10 g of the polyurethane resin was evenly coated on a glass slide, cured at room temperature for 20 minutes, and the cured film was lightly pressed with a finger. If there was no stickiness and no fingerprint marks were left, the surface had been cured to obtain a cured film.

[0092] The wear resistance of the cured film was measured according to GB / T 1768-2006 (rotating rubber grinding wheel method). The cured films of Examples 3 to 32 and Comparative Examples 1 to 6 were tested for wear resistance using 60# sandpaper, with one back and forth counted once, and a total of 1000 times of grinding. The weight loss due to wear was calculated using the following formula:

[0093] Abrasion weight loss = M0-M1; where M0 is the original film mass, mg; M1 is the mass of the cured film after friction, mg. See Table 8 for data.

[0094] 4. Determination of water resistance of polyurethane resin

[0095] The polyurethane resins of Examples 1 to 32 and Comparative Examples 1 to 6 were respectively made into coating products, and the specific steps were: 10 g of the polyurethane resin was evenly coated on a glass slide, cured at room temperature for 20 minutes, and the cured film was lightly pressed with a finger. If there was no stickiness and no fingerprint marks were left, the surface had been cured to obtain a cured film.

[0096] The cured film samples of Examples 3, 33 to 59 and Comparative Examples 1 to 6 were tested for water resistance using GB / T 1733-93 "Determination of water resistance of paint films", and the specific data are shown in Table 8. The standard classification is one to three and unqualified. Among them, the specific classification standards are as follows:

[0097] Level 1: The paint film remains completely original;

[0098] Level 2: The paint film surface has slight changes;

[0099] Level 3: The paint film surface has obvious changes;

[0100] Unqualified: The paint film has serious bubbling, peeling and other phenomena.

[0101] 5. Determination of hardness of polyurethane resin

[0102] The polyurethane resins of Examples 1 to 3, 33 to 59 and Comparative Examples 1 to 6 were respectively made into coating products, and the specific steps were as follows: 10 g of the polyurethane resin was evenly coated on a glass slide, cured at room temperature for 20 minutes, and the cured film was lightly pressed with a finger. If there was no stickiness and no fingerprint indentation was left, the surface had been cured to obtain a cured film.

[0103] The hardness values ​​of the cured film samples of Examples 1 to 3, 33 to 59 and Comparative Examples 1 to 6 were measured by a Shore hardness tester using an indentation method. The Shore hardness test standard adopted Shore D. The data are shown in Table 10.

[0104] 6. Determination of adhesion of polyurethane resin

[0105] The polyurethane resins of Examples 1 to 3, 33 to 59 and Comparative Examples 1 to 6 were respectively made into coating products, and the specific steps were as follows: 10 g of the polyurethane resin was evenly coated on a glass slide, cured at room temperature for 20 minutes, and the cured film was lightly pressed with a finger. If there was no stickiness and no fingerprint indentation was left, the surface had been cured to obtain a cured film.

[0106] The cured film samples of Examples 1 to 3, 33 to 59 and Comparative Examples 1 to 6 were subjected to the cross-hatch method to measure the adhesion of the cured coating film in accordance with GB / T9286-1998. Six parallel cuts (about 10 to 20 mm long and 1 mm apart) were cut on the coating film fixed on the glass slide with a blade. The depth should be appropriate to cut the cured film. Then six more cuts were made in the same direction perpendicular to the former. The film was brushed back and forth 5 times with a soft brush to observe whether the coating film fell off and the area of ​​the falling off. The film adhesion grading evaluation table listed in Table 9 was used for rating, where Grade 0 indicates the best adhesion and Grade 5 indicates the worst adhesion. The data are shown in Table 10.

[0107] Table 9 Adhesion Grading Evaluation Table

[0108]

[0109]

[0110] 7. Determination of salt spray resistance of polyurethane resin

[0111] The polyurethane resins of Examples 1 to 3, 33 to 59 and Comparative Examples 1 to 6 were respectively made into coating products, and the specific steps were as follows: 10 g of the polyurethane resin was evenly coated on a glass slide, cured at room temperature for 20 minutes, and the cured film was lightly pressed with a finger. If there was no stickiness and no fingerprint indentation was left, the surface had been cured to obtain a cured film. The data is shown in Table 10.

[0112] 8. Determination of flexibility of polyurethane resin

[0113] The polyurethane resins of Examples 1 to 3, 33 to 45 and Comparative Examples 1 to 6 were respectively made into coating products, and the specific steps were as follows: 10 g of the polyurethane resin was evenly coated on a PP board substrate, cured at room temperature for 20 minutes, and the cured film was lightly pressed with a finger. If there was no stickiness and no fingerprint indentation was left, the surface had been cured to obtain a cured film.

[0114] According to the paint film flexibility determination method GB / T1731-1993, the flexibility of the cured film is determined. The UV coating prepared in 2.3.4 is evenly coated on a special tinplate using a wet film preparation device with a coating thickness of 20μm and cured by UV curing machine. With the coating side facing up, press the sample tightly on the shaft rod with both hands and quickly bend the sample around the shaft rod. The bending action is required to be completed within 2-3s, and observe whether the coating film is damaged. Only observe whether the coating film is damaged. Film shedding and damage caused by film shedding are not used as evaluation basis. The minimum shaft rod diameter that does not cause coating film damage is used to characterize the flexibility of the cured film. The data is shown in Table 10.

[0115] 9. Determination of storage stability of polyurethane resin

[0116] The polyurethane resins of Examples 1 to 3, 46 to 59 and Comparative Examples 1 to 6 were tested for storage stability. The specific method was as follows: the polyurethane resins were stored at room temperature for 1 to 8 months using the method of GB 6753.3-86. The samples were taken out for testing after each month of storage. If any of the items such as crusting, pressure, corrosion and rancid smell of the sample exceeded Level 4 (medium), it means that the storage stability time is that month. The data is shown in Table 10.

[0117] Table 8 Data of polyurethane resins of Examples 1 to 17 and Comparative Examples 1 to 6

[0118]

[0119]

[0120]

[0121] Table 10 Data of Examples 1 to 3, 33 to 59 and Comparative Examples 1 to 6

[0122]

[0123]

[0124] It can be seen from Table 8 and Table 10 that the polyurethane resins of each embodiment have good heat resistance, wear resistance, hydrolysis resistance and mechanical strength. In Comparative Example 1, castor oil-modified polyol is not added, and its viscosity is improved, but tensile strength, hardness, adhesion, wear resistance and water resistance are all reduced. Therefore, the present invention uses castor oil-modified polyol and petroleum-based polyol to compound, which meets environmental protection requirements and can also improve the mechanical properties of polyurethane.

[0125] The mass ratios of castor oil modified polyol to petroleum-based polyol in Comparative Examples 2 and 3 are different, and their performances are both reduced, indicating that when the mass ratio of petroleum-based polyol to castor oil modified polyol is 1:(8-10), the polyurethane resin with the best performance can be obtained.

[0126] Comparative Example 4 uses epoxy soybean oil modified polyol to replace castor oil modified polyol, and its performance is lower than that of the polyurethane resin of Example 3, indicating that castor oil modified polyol has better performance than other synthetic polyols, and the price of castor oil modified polyol is relatively low, which is cost-effective. At the same time, it has a wide range of sources and is easy to obtain, which ensures the stability and sustainability of production. The molecular structure of castor oil polyol contains multiple hydroxyl groups, which can react with isocyanate to form a high molecular weight polyurethane resin. This resin performs well in terms of strength, wear resistance, water resistance, etc., and can meet various application requirements.

[0127] The polyurethane resin in Comparative Example 5 is not modified with polymethyl methacrylate, so the mechanical properties, water resistance, wear resistance, stability and flexibility of the resin are significantly reduced, indicating that polymethyl methacrylate-modified polyurethane can increase the crosslinking degree of the polyurethane network, thereby improving the above properties.

[0128] In the preparation method of the polyurethane resin in Comparative Example 6, prepolymerization, crosslinking, and chain extension are all performed in one step, resulting in uneven crosslinking of polyurethane and PMMA, thereby significantly reducing the performance of the resin. This indicates that in the preparation method of the waterborne polyurethane resin of the present invention, the synthesis of polyurethane and the polymerization with methyl methacrylate (PMMA) and the crosslinking reaction are performed in steps, which ensures that the polyurethane can be fully polymerized, and then methyl methacrylate is in-situ polymerized to form PMMA and then crosslinked with polyurethane, which can improve the crosslinking degree of the two, thereby promoting the performance of the resin.

[0129] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.

Claims

1. A high bio-based waterborne polyurethane resin, characterized in that: The invention comprises the following components in parts by weight: 15 to 30 parts of isocyanate, 80 to 100 parts of polyol, 5 to 10 parts of methyl methacrylate, 0.5 to 2 parts of chain extender, 0.2 to 0.6 parts of catalyst, 1 to 2 parts of initiator, 5 to 10 parts of neutralizer, 2 to 10 parts of emulsifier and 150 to 400 parts of water; wherein the polyol comprises petroleum-based polyol and castor oil-modified polyol in a mass ratio of 1:(8 to 10).

2. The high bio-based waterborne polyurethane resin according to claim 1, characterized in that: The invention comprises the following components in parts by weight: 18 to 25 parts of isocyanate, 95 to 100 parts of polyol, 0.5 to 1.5 parts of chain extender, 0.3 to 0.5 parts of catalyst, 1 to 2 parts of initiator, 4 to 6 parts of emulsifier and 180 to 360 parts of water.

3. The high bio-based waterborne polyurethane resin according to claim 1 or 2, characterized in that: At least one of the following (I) to (III): (I) the chain extender is at least one of an aromatic diamine chain extender, an aromatic diol chain extender, an aspartic acid ester, a polyurethane chain extender, an epoxy chain extender, and a phosphite chain extender; (II) the neutralizing agent is at least one of triethylamine, triethanolamine, sodium hydroxide, potassium hydroxide, sodium carbonate, sodium acetate, sodium pyrophosphate, ammonia water, hydrochloric acid, phosphoric acid, formic acid, acetic acid, aminoacetic acid, 2-amino-2-methyl-1-propanol, and sodium bicarbonate; (III) The initiator is benzoyl peroxide.

4. The high bio-based waterborne polyurethane resin according to claim 1 or 2, characterized in that: At least one of the following (I) to (II): (I) the isocyanate is at least one of an aromatic diisocyanate and an aliphatic diisocyanate; (II) The petroleum-based polyol is at least one of 1,4-butanediol, 1,6-hexanediol, neopentyl glycol, dipropylene glycol, and trimethylolpropane.

5. The high bio-based waterborne polyurethane resin according to claim 1, characterized in that: At least one of the following (I) to (III): (I) the mass ratio of isocyanate groups in the isocyanate is 15 to 20%; (II) the castor oil-modified polyol has a hydroxyl value of 270 to 290 mgKOH / g and an acid value of 0.1 to 0.2 mgKOH / g; (III) The number average molecular weight of the chain extender is 150-155.

6. The high bio-based waterborne polyurethane resin according to claim 1, characterized in that: The viscosity of the high bio-based waterborne polyurethane resin is 2100-2600 mPa·s.

7. The method for preparing a highly bio-based waterborne polyurethane resin according to any one of claims 1 to 6, characterized in that: The following steps are involved: S1. Preparation of prepolymer: stirring and mixing polyol, isocyanate and catalyst, and heating to carry out prepolymerization reaction to obtain prepolymer; Preparation of S2 polymer: mixing the prepolymer, methyl methacrylate and initiator, heating to carry out cross-linking reaction, and obtaining a polymer; S3: mixing the polymer with part of water and a chain extender to carry out a chain extension reaction, and then adding a neutralizer to obtain a waterborne polyurethane; S4: mixing the waterborne polyurethane with the remaining water and an emulsifier to emulsify the waterborne polyurethane to obtain the high bio-based waterborne polyurethane resin.

8. The method for preparing a highly bio-based waterborne polyurethane resin according to claim 7, characterized in that: In the step S1, the parameters of the prepolymerization reaction are: temperature of 75-85° C. and time of 2-3 hours.

9. The method for preparing a highly bio-based waterborne polyurethane resin according to claim 7, wherein: In step S2, the parameters of the cross-linking reaction are: temperature of 80-90°C, time of 2-3h; and / or, in step S3, the parameters of the chain extension reaction are: temperature of 70-80°C, time of 1-2h, and the system temperature is reduced to 30-40°C when the chain extension reaction is terminated.

10. Use of the high bio-based waterborne polyurethane resin according to any one of claims 1 to 7 in the preparation of coatings, adhesives, fabric coatings and finishing agents, and leather and synthetic leather finishing agents.

Citation Information

Patent Citations

  • Waterborne polyurethane-acrylate hybrid copolymer and preparation method thereof

    CN110951041A

  • Bio-based water-based light-cured polyurethane resin as well as preparation method and application thereof

    CN112592434A

  • Waterborne polyurethane-acrylate hybrid copolymer and preparation method thereof

    CN114763395A

  • Modified bio-based waterborne polyurethane, method for preparing same, and use thereof

    WO2024031542A1

Cited By

  • Modified polyurethane resin and preparation method thereof

    CN121378672A

  • A modified polyurethane resin and a method for preparing the same

    CN121378672B