Ionic liquid toughened anti-precipitation polylactic acid / nanocellulose composite material and preparation method thereof

By using sulfonated nanocellulose and ionic liquid in polylactic acid composite materials, combined with homogenization treatment and twin-screw extrusion technology, the problem of degradation of mechanical properties of polylactic acid composite materials after plasticization is solved, achieving high The effect of tough low precipitation has expanded its application range.

CN118956128AInactive Publication Date: 2024-11-15NINGBO UNIV

Patent Information

Application Number
CN202411443913.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-16
Publication Date
2024-11-15
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

After plasticizing, the mechanical properties of polylactic acid composites are degraded due to the precipitation of plasticizers. The prior art is difficult to effectively reduce the precipitation of ionic liquids, which limits its application range.

Method used

The sulfonated modified nanocellulose is combined with the ionic liquid, and the dipole interaction between the sulfonic acid groups and the ionic liquid is bound, reducing its precipitation, and pelletized through homogenization and twin-screw extruder Technology to improve the dispersion and binding effect of nanocellulose in polylactic acid.

Benefits of technology

It significantly improves the mechanical strength and toughness of polylactic acid composite materials, while reducing the precipitation of plasticizers, extending its application range in food packaging, medical machinery and agriculture.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118956128A_ABST
    Figure CN118956128A_ABST
Patent Text Reader

Abstract

The invention discloses an ionic liquid toughened anti-precipitation polylactic acid / nanocellulose composite material and a preparation method thereof. The polylactic acid / nanocellulose composite material comprises the following components in parts by mass: 100 parts of polylactic acid, 1-10 parts of sulfonated nanocellulose, 1-10 parts of ionic liquid, 1-5 parts of a compatibilizer, 0.5-2 parts of a lubricant and 0.5-2 parts of a coupling agent. According to the invention, the ionic liquid is used as a green plasticizer of the polylactic acid composite material, and sulfonated nano cellulose is creatively added. While the mechanical strength of the plasticized polylactic acid composite material is complemented, the precipitation of the ionic liquid plasticizer is reduced. And moreover, by adjusting the sulfonation degree of the nano cellulose, the toughness and precipitation resistance of the polylactic acid composite material are regulated and controlled. The polylactic acid composite material prepared by the invention has good mechanical strength and toughness, low plasticizer precipitation property, low production cost and equipment requirements, simple, convenient and efficient process, and is suitable for large-scale production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of degradable plastics, and in particular is an ionic liquid toughened anti-precipitation polylactic acid / nanocellulose biodegradable composite material and a preparation method thereof. Background Art

[0002] Polylactic acid is a biodegradable and environmentally friendly polymer that can be obtained by ring-opening polymerization of lactide. Lactide can be prepared from natural resources such as corn starch, cassava, and wheat, thus getting rid of dependence on petroleum resources. Polylactic acid has many significant advantages, such as biocompatibility, transparency, Young's modulus and tensile strength. Despite this, the low toughness of polylactic acid limits its application. Adding plasticizers to polylactic acid is an effective way to improve toughness. Common plasticizers include petroleum-based and bio-based plasticizers: the former is widely used, but its application field is limited due to safety issues; the latter is safer to use, but the types and plasticizing effects need to be improved. Therefore, ionic liquids have entered people's field of vision as a new type of "green plasticizer". Ionic liquids are organic salts composed entirely of ions, which have the characteristics of low melting point, low vapor pressure, and high thermal stability. However, the precipitation of plasticizers and the reduction of material strength / modulus after plasticization are still serious challenges. How to reduce the precipitation of ionic liquids in composite materials and ensure the mechanical properties of polylactic acid composite materials after plasticization are key technical issues worthy of in-depth exploration.

[0003] The introduction of bionanomaterials into the PLA plasticizer system can effectively solve the problem of decreased mechanical strength of PLA composites. Nanocellulose is a low-cost, degradable nano-reinforced filler extracted from biomass materials such as bamboo. It has the advantages of high strength, large specific surface area and rich surface reaction sites. At present, research results show that nanocellulose has a significant reinforcing effect on PLA plasticizer composites. Tian et al. (Nanotechnology Reviews, 2022, 11(1): 2469-2482.) reported a citrate / nanocellulose / PLA composite material. They found that after adding 4 wt% nanocellulose, the tensile strength of the PLA composite material increased by 110% and the impact toughness increased by 230%. Xu et al. (Composites Science and Technology, 2021, 203: 108613.) also found that the addition of nanocellulose to the PLA plasticizer system not only significantly improved the mechanical strength and toughness of the PLA composite material, but also improved the thermal stability of the PLA composite material. It can be seen that adding nanocellulose to the polylactic acid plasticizing system is beneficial to reinforcement, but the effect of improving its tensile strength is still not obvious, and there is still the problem of plasticizer precipitation. The patent with application publication number CN117946502A discloses a polylactic acid degradable composition and its application in pharmaceutical packaging bottles. Among them, 30 to 90 parts of polylactic acid, 9 to 60 parts of toughening agent, and 1 to 11 parts of other additives are mixed and granulated in a twin-screw extruder to obtain a degradable bio-based material with good barrier properties and impact strength. Although this method improves the toughness of polylactic acid composite materials, the mechanical strength and modulus are seriously reduced, and the problem of plasticizer precipitation in the composite material cannot be solved.

[0004] In our recent research, we found that sulfonated nanocellulose and ionic liquids have strong Coulomb forces. Therefore, in the preparation process of polylactic acid composites, adding sulfonated nanocellulose can restrain the free ionic liquid in the composite material, thereby improving the precipitation problem of the ionic liquid, and also compensating for the mechanical strength and elastic modulus of the composite material after plasticization. How to compound ionic liquid with sulfonated nanocellulose to achieve the enhancement and toughness of polylactic acid composites and reduce the precipitation of plasticizers at the same time is a technical problem worthy of study. This composite material is expected to replace traditional petroleum-based polypropylene, polystyrene, etc., and be used in food packaging, medical machinery and agricultural fields.

[0005] In order to improve the toughness of polylactic acid composite materials and reduce the precipitation of plasticizers, and expand their application range, it is urgent to invent a method for preparing high-toughness and low-precipitation polylactic acid composite materials to expand the application of polylactic acid composite materials in daily plastics. Therefore, the present invention proposes an ionic liquid toughened and precipitation-resistant polylactic acid / nanocellulose composite material and a preparation method thereof. Summary of the invention

[0006] The problem to be solved by the present invention is that, in view of the poor toughness of existing polylactic acid, the addition of plasticizer will cause the precipitation of plasticizer in polylactic acid composite materials, and an ionic liquid toughened precipitation-resistant polylactic acid / nanocellulose composite material and a preparation method thereof are proposed.

[0007] The technical solution adopted by the present invention to solve the above technical problems is: a toughened and anti-precipitation polylactic acid / nanocellulose composite material, whose mass percentage composition is: 100 parts of polylactic acid, 1-10 parts of sulfonated nanocellulose, 1-10 parts of ionic liquid, 1-5 parts of compatibilizer, 0.5-2 parts of lubricant, and 0.5-2 parts of coupling agent.

[0008] Preferably, the raw material powder is one or a combination of two or more of wood powder, bamboo powder, straw powder and bagasse powder.

[0009] Preferably, the sulfonation degree of the sulfonated nanocellulose is 10% to 80%, 10% to 29% sulfonation degree (low degree sulfonation), 30% to 59% sulfonation degree (medium degree sulfonation), 60% to 80% sulfonation degree (high degree sulfonation).

[0010] Preferably, the ionic liquid is one or a combination of two or more of 1-butyl-3-methylimidazolium tetrafluoroborate, 1-butyl-1-methylpyrrolidium hexafluorophosphate, and 1-allyl-3-methylimidazolium chloride.

[0011] Preferably, the compatibilizer is at least one of glycidyl methacrylate, octaaminopropyl cage-type polysilsesquioxane, and triacetin.

[0012] Preferably, the lubricant is one or a combination of two or more of sodium cocoyl aminopropionate, polyvinyl acetate resin, ethylene bisstearamide, oleamide, and erucamide.

[0013] Preferably, the coupling agent is at least one of a silane coupling agent (KH151, KH550, KH580, KH792), a titanate coupling agent CS-101 and an aluminate coupling agent DL-411.

[0014] The method for preparing the toughened and anti-precipitation polylactic acid / nanocellulose composite material comprises the following steps:

[0015] 1. Preparation of sulfonated nanocellulose

[0016] (1) Mix 1 to 10 parts of raw material powder with 70 to 80 parts of sodium hydroxide solution, heat and stir at 60 to 95°C for 2 to 4 hours, wash with pure water until neutral, add 40 to 60 parts of sodium chlorite solution and 3 to 4 parts of glacial acetic acid, heat and stir at 60 to 80°C for 1 to 2 hours, and then wash with pure water until neutral;

[0017] (2) The solid-liquid mixture obtained in (1) is subjected to high-speed shearing treatment using a homogenizer for 1 to 2 h at a speed of 10,000 to 20,000 rpm; the homogenized sample is centrifuged and washed, and then freeze-dried to obtain nanocellulose;

[0018] (3) Disperse 1-10 parts of the nanocellulose sample obtained in (2) in 40-100 parts of sodium periodate solution at 30°C-40°C, stir the mixture in a lightless nitrogen environment for 1-2 hours, and then wash it with pure water by centrifugation until it becomes neutral; then disperse the obtained product in 80-90 parts of sodium sulfite, stir it at room temperature for 1-2 hours, wash the sample by centrifugation until it becomes neutral, and then freeze-dry it to obtain (low, medium, high) degree of sulfonated nanocellulose.

[0019] Preferably, in step (1), the raw material powder has a mesh size of 80 to 200 meshes, the concentration of the sodium hydroxide solution is 10 to 20 w / v%, and the concentration of the sodium chlorite solution is 10 to 20 w / v%; in step (3), the concentration of sodium periodate is 10 to 20 w / v%, and the concentration of sodium sulfite is 10 to 15 w / v%.

[0020] In step (3) of the above method of the present invention, sodium periodate and sodium sulfite are used to sulfonate the nanocellulose, so that the electrically neutral hydroxyl groups on its surface are converted into highly electronegative sulfonic acid groups. The degree of sulfonation is regulated by the amount of sodium periodate solution added. The sulfonic acid groups introduced by the sulfonation reaction can reduce the hydrogen bonding between celluloses, effectively reduce the agglomeration of nanocellulose, and improve its dispersion effect in the polylactic acid / nanocellulose composite material. In addition, the sulfonic acid groups and the ionic liquid groups form a strong dipole interaction, which effectively limits the free ionic liquid in the polylactic acid / nanocellulose composite material and reduces the precipitation of the ionic liquid. The present invention regulates the degree of sulfonation of nanocellulose to achieve anti-plasticizer precipitation of the polylactic acid composite material when different plasticizers are added. The introduction of highly sulfonated nanocellulose can better improve the mechanical strength of the polylactic acid composite material and has a significant inhibitory effect on the precipitation of ionic liquids. The introduction of low-level sulfonated nanocellulose can significantly improve the mechanical strength of the polylactic acid composite material, ensure the toughness of the composite material, and have a certain inhibitory effect on the precipitation of ionic liquids. Moderately sulfonated nanocellulose better balances the mechanical strength of polylactic acid composites and the inhibition of ionic liquid precipitation.

[0021] 2. Preparation of polylactic acid / nanocellulose composites

[0022] a: Add 1-10 parts of sulfonated nanocellulose to 100 parts of deionized water and ultrasonicate for 5-10 min. Add 1-10 parts of ionic liquid to the suspension. Dry the solid-liquid mixture at 60-70°C for 72 h to obtain dry ionic liquid-modified sulfonated nanocellulose;

[0023] b: adding the ionic liquid modified sulfonated nanocellulose obtained in step a, 100 parts of polylactic acid, 1 to 5 parts of a compatibilizer, 0.5 to 2 parts of a lubricant, and 0.5 to 2 parts of a coupling agent into a high-speed mixer and mixing for 60 to 120 minutes at a speed of 300 to 800 rpm to obtain a premix;

[0024] c: adding the premix obtained in step b into a twin-screw extruder for extrusion and granulation, wherein the processing temperature of the twin-screw extruder is 110-190° C., the screw aspect ratio is 25-50, and the rotation speed is 50-250 rpm to obtain polylactic acid / nanocellulose composite material particles;

[0025] d: Processing the composite material particles obtained in step c into a polylactic acid / nanocellulose composite material by an injection molding machine or a hot press.

[0026] The method of the present invention enables the ionic liquid to be uniformly attached to the surface of the nanocellulose through step a, thereby improving the combination effect of the two. The ionic liquid with strong polarity can penetrate into the nanocellulose molecular chain, destroy the hydrogen bonds between the nanocellulose, and is beneficial to improving the dispersibility of the nanocellulose and the reinforcing effect of the nanocellulose on the polylactic acid; it is also beneficial to improve the effect of the sulfonic acid group and the ionic liquid, and reduce the migration and precipitation of the ionic liquid.

[0027] According to the method of the present invention, in step b, the functional groups on the nanocellulose molecular chains that are not modified by the ionic liquid are further modified by the coupling effect of the coupling agent and the compatibilization effect of the compatibilizer under the action of high-speed mechanical mixing, thereby further enhancing the interfacial compatibility between the nanocellulose and the polylactic acid molecular chains.

[0028] The method of the present invention is carried out through step c, and the premix gives full play to the volume expansion and coupling effects under the melt blending conditions, improves the interface affinity between the ionic liquid modified sulfonated nanocellulose and polylactic acid, improves the stress transfer efficiency between the nanocellulose and the polylactic acid, and improves the mechanical strength of the polylactic acid composite material. Due to the strong dipole interaction between the sulfonic acid group in the nanocellulose and the functional group of the ionic liquid, while enhancing the affinity with the polylactic acid, the precipitation of the ionic liquid is also effectively reduced. At the same time, the ionic liquid is compounded into the polylactic acid matrix along with the nanocellulose, which reduces the cohesive force between the polylactic acid molecules, makes the polylactic acid molecular chain easier to move, plays a plasticizing effect, and is combined with the reinforcement of the sulfonated nanocellulose itself to achieve a synergistic effect of toughening and reinforcement.

[0029] Compared with the prior art, the present invention has the following advantages:

[0030] 1. The toughened and precipitation-resistant polylactic acid / nanocellulose composite material of the present invention is compounded with biomass-derived nanocellulose and biodegradable materials. Nanocellulose has high modulus, high strength, and high specific surface area, and is a high-quality reinforcing filler. Nanocellulose makes up for the decrease in mechanical strength and modulus of the polylactic acid composite material due to the plasticizer, and plays a reinforcing role. The composite material has a wide range of applications and can be used in the fields of textiles, catering, and medical treatment.

[0031] 2. The present invention adopts sulfonation treatment to enhance the dispersibility of nanocellulose itself, and can also effectively combine with ionic liquid through Coulomb force. The interfacial bonding effect between the prepared ionic liquid modified sulfonated nanocellulose and polylactic acid is further enhanced, which improves the toughness of the composite material and inhibits the precipitation of plasticizer, thereby expanding the application of nanocellulose in biodegradable materials.

[0032] 3. Compared with the preparation method of traditional polylactic acid / nanocellulose composite materials, the method of the present invention is easy to process, has low equipment requirements, uses less modification additives, and adds less modified nanocellulose, which can reduce the cost of biodegradable composite materials.

[0033] 4. The polylactic acid, nanocellulose and ionic liquid in the present invention are all biodegradable materials, and have the characteristics of good biocompatibility, natural sources, and green and renewable. The composite material of the present invention has a simple preparation process and is non-toxic and harmless. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 : Tensile properties of polylactic acid / nanocellulose composites with different ionic liquid addition amounts;

[0035] Figure 2 : Impact properties of polylactic acid / nanocellulose composites with different ionic liquid addition amounts;

[0036] Figure 3 : Precipitation properties of polylactic acid / nanocellulose composites with different ionic liquid addition amounts;

[0037] Figure 4 : Tensile properties of polylactic acid / nanocellulose composites with different amounts of sulfonated nanocellulose added;

[0038] Figure 5 : Impact properties of polylactic acid / nanocellulose composites with different amounts of sulfonated nanocellulose added;

[0039] Figure 6 : Precipitation properties of polylactic acid / nanocellulose composites with different amounts of sulfonated nanocellulose added;

[0040] Figure 7 : Tensile properties of polylactic acid / nanocellulose composites with different amounts of compatibilizer added;

[0041] Figure 8 : Impact properties of polylactic acid / nanocellulose composites with different amounts of compatibilizer added;

[0042] Fig. 9 : Precipitation properties of polylactic acid / nanocellulose composites with different amounts of compatibilizer added;

[0043] Fig.10 : Tensile properties of polylactic acid / nanocellulose composites with different degrees of sulfonation of nanocellulose;

[0044] Fig.11 : Impact properties of polylactic acid / nanocellulose composites with different degrees of sulfonation of nanocellulose;

[0045] Fig.12 : Precipitation properties of polylactic acid / nanocellulose composites with different degrees of sulfonation of nanocellulose;

[0046] Fig.13 : SEM image of tensile fracture of the polylactic acid / nanocellulose composite material of Example 3;

[0047] Fig.14 : SEM image of tensile fracture of the polylactic acid / nanocellulose composite material of Comparative Example 1;

[0048] Fig.15 : SEM image of tensile fracture of the polylactic acid / nanocellulose composite material of Comparative Example 2. DETAILED DESCRIPTION

[0049] The present invention is further described in detail below with reference to the accompanying drawings.

[0050] The mass fraction compositions of the polylactic acid / nanocellulose composite materials of Examples 1 to 5 are shown in Table 1, and the polylactic acid / nanocellulose composite materials of Examples 1 to 5 are numbered C1, C2, C3, C4, and C5, respectively, and a single factor experiment is performed.

[0051] In Examples 1 to 5, the nanocellulose is bamboo nanocellulose, the sulfonated nanocellulose is medium-sulfonated nanocellulose, the ionic liquid is 1-butyl-3-methylimidazole tetrafluoroborate, the compatibilizer is glycidyl methacrylate, the lubricant is sodium coconut aminopropionate, and the coupling agent is silane coupling agent KH580.

[0052] Table 1

[0053]

[0054] The method for preparing the polylactic acid / nanocellulose composite material of Example 1 comprises the following steps:

[0055] 1. Preparation of moderately sulfonated nanocellulose

[0056] (1) 10 parts of 200-mesh bamboo powder were mixed with 80 parts of 20 w / v% sodium hydroxide solution, heated and stirred at 95°C for 4 h, washed with pure water until neutral, and then 60 parts of 15 w / v% sodium chlorite solution and 3 parts of glacial acetic acid were added, heated and stirred at 80°C for 2 h, and then washed with pure water until neutral;

[0057] (2) The solid-liquid mixture obtained in (1) was subjected to high-speed shearing treatment using a homogenizer at a speed of 20,000 rpm for 2 h; the homogenized sample was centrifuged and washed, and then freeze-dried to obtain nanocellulose;

[0058] (3) Disperse 10 parts of the nanocellulose sample obtained in (2) in 60 parts of 15 w / v% sodium periodate solution at 40°C, stir the mixture for 2 h in a lightless nitrogen environment, and then wash it with pure water until it is neutral. Disperse the obtained product in 90 parts of 15 w / v% sodium sulfite, stir it at room temperature for 2 h, wash the sample by centrifugation until it is neutral, and then freeze-dry it to obtain medium-degree sulfonated nanocellulose.

[0059] 2. Preparation of polylactic acid / nanocellulose composites

[0060] a: Add 3 parts of medium-level sulfonated nanocellulose to 100 parts of deionized water and sonicate for 10 min. Add 1 part of ionic liquid to the suspension. Dry the solid-liquid mixture at 60°C for 72 h to obtain dry ionic liquid-modified sulfonated nanocellulose;

[0061] b: adding the ionic liquid modified sulfonated nanocellulose obtained in step a, 100 parts of polylactic acid, 2 parts of a compatibilizer, 0.5 parts of a lubricant, and 2 parts of a coupling agent into a high-speed mixer and mixing for 120 min at a speed of 800 rpm to obtain a premix;

[0062] c: adding the premix obtained in step b into a twin-screw extruder for extrusion and granulation, the processing temperature of the twin-screw extruder is 190° C., the screw aspect ratio is 50, and the rotation speed is 250 rpm to obtain polylactic acid / nanocellulose composite particles;

[0063] d: Processing the composite material particles obtained in step c into a polylactic acid / nanocellulose composite material through an injection molding machine.

[0064] The preparation methods of the polylactic acid / nanocellulose composite materials of Examples 2 to 5 are basically the same as those of Example 1, except that in the preparation step a of Examples 2 to 5, the amounts of ionic liquid added are 3 parts, 5 parts, 7 parts and 10 parts, respectively, to prepare the polylactic acid / nanocellulose composite materials of Examples 2 to 5, respectively.

[0065] As a comparison, the following polylactic acid composite materials of Comparative Example 1 and Comparative Example 2 were prepared.

[0066] The plasticizer of the polylactic acid / nanocellulose composite material of Comparative Example 1 is changed to epoxidized soybean oil, 100 parts of polylactic acid, 3 parts of moderately sulfonated nanocellulose, 2 parts of compatibilizer, 1 part of plasticizer, 0.5 parts of lubricant, 2 parts of coupling agent, the nanocellulose is prepared by 200-mesh bamboo powder, the compatibilizer is octaaminopropyl cage-type polysilsesquioxane, the lubricant is polyvinyl acetate resin, and the coupling agent is titanate coupling agent CS-101.

[0067] The preparation method of the polylactic acid / nanocellulose composite material of Comparative Example 1 is basically the same as that of Example 1, except that step a is not required when preparing the polylactic acid / nanocellulose composite material, and step b requires adding 100 parts of polylactic acid, 1 part of epoxy soybean oil, 2 parts of coupling agent, 2 parts of compatibilizer, 0.5 parts of lubricant and 3 parts of moderately sulfonated nanocellulose for blending.

[0068] In the polylactic acid / nanocellulose composite material of comparative example 2, unsulfonated modified nanocellulose is used, and its mass proportion is as follows: 100 parts of polylactic acid, 3 parts of nanocellulose, 2 parts of a compatibilizer, 1 part of a plasticizer, 0.5 parts of a lubricant, and 2 parts of a coupling agent. The nanocellulose is prepared using 200-mesh bamboo powder, the plasticizer is ionic liquid 1-butyl-3-methylimidazole tetrafluoroborate, the compatibilizer is triacetin, the lubricant is ethylene bisstearamide, and the coupling agent is aluminate coupling agent DL-411.

[0069] The preparation method of the polylactic acid / nanocellulose composite material of Comparative Example 2 is substantially the same as that of Example 1, except that the cellulose sulfonation modification operation in step (3) is not required when preparing the nanocellulose.

[0070] For the polylactic acid / nanocellulose composite materials of Examples 1 to 5, tensile and impact test specimens were prepared respectively. The mechanical properties of the polylactic acid / nanocellulose composite materials of Examples 1 to 5 were tested in groups according to the methods of GB / T1040 and GB / T1843 standards; the plasticizer migration and precipitation rates of the polylactic acid / nanocellulose composite materials of Examples 1 to 5 were tested in groups according to the methods of HG / T4454 standards.

[0071] The tensile test specimens are dumbbell-shaped specimens with a length of 75 mm, a gauge length of 30 mm, a middle width of 4 mm, and a thickness of 2 mm. The tensile speed is 20 mm / min, and at least 5 specimens are tested in each group. The average values ​​of the tensile strength and tensile elongation at break are taken. The results are as follows: Figure 1 As shown; the impact test uses a notched impact specimen, the pendulum weight is 1.245 kg, the angle is 150°, at least 5 samples are tested in each group, and the average impact strength of the samples is taken. The results are shown in Figure 2 The plasticizer migration and precipitation samples are long strip samples with a length of 80 mm, a width of 10 mm, and a thickness of 4 mm. The plasticizer migration rate of each sample is tested in a rheological heat aging test chamber at 50℃~150℃ to characterize the amount of plasticizer precipitation on the polylactic acid / nanocellulose surface. At least 5 sample points are tested in each group and the average value is taken. The results are shown in Figure 3 shown.

[0072] The same method as that of the polylactic acid / nanocellulose composite material of Example 1 was used to perform tensile test, impact test and plasticizer precipitation test on the polylactic acid / nanocellulose composite material of Comparative Example 1, and the tensile strength was 45 MPa, the elongation at break was 6.8%, and the impact strength was 3.1 KJ / m 2 The migration and precipitation rate is 10.2%.

[0073] The same method as the polylactic acid / nanocellulose composite material of Example 1 was used to perform tensile test, bending test, impact test and heat resistance test on the polylactic acid / nanocellulose composite material of Comparative Example 2, and the tensile strength was 54.7 MPa, the elongation at break was 7.5%, and the impact strength was 3.5 KJ / m 2 The migration and precipitation rate is 4.7%.

[0074] from Figure 1 , Figure 2 and Figure 3 It can be seen that as the amount of ionic liquid added increases, the tensile strength of the polylactic acid / nanocellulose composite materials of Examples 1 to 5 decreases, the elongation at break increases, and the migration and precipitation rate of the plasticizer increases, but the impact strength shows a trend of first increasing and then decreasing. The decrease in tensile strength and the increase in elongation at break of the polylactic acid / nanocellulose composite materials are mainly due to the addition of ionic liquids, which destroy the crystal structure of polylactic acid and weaken its mechanical strength, making the polylactic acid molecular chains easier to slide, thus playing a plasticizing effect. The change in impact strength is caused by the synergistic effect of the reinforcing effect of nanocellulose and the plasticizing effect of ionic liquids. As the content of ionic liquid increases, the sulfonated nanocellulose sites cannot effectively bind to free ionic liquids, resulting in an increase in the precipitation rate of ionic liquids. Combining these performance values, Examples 1 to 5 have obvious advantages over Comparative Examples 1 and 2. Among them, the tensile strength, tensile elongation at break and impact strength are at least increased by 6.6%, 22.1% and 19.3% respectively compared with the comparative example 1 adding epoxidized soybean oil, and the migration precipitation rate is reduced by 72.5%; compared with the comparative example 2 adding unmodified nanocellulose, the tensile elongation at break and impact strength are at least increased by 14.1% and 9.0% respectively, and the migration precipitation rate is reduced by 37.2%. The microscopic morphology of the tensile fracture surface of the polylactic acid / nanocellulose composite material of Example 3 ( Fig.13 ) compared with Comparative Example 1 ( Fig.14 ) and Comparative Example 2 ( Fig.15 ) is rougher and shows the morphological characteristics of tough fracture, which shows that nanocellulose and polylactic acid have good compatibility and the ionic liquid has a stronger plasticizing effect on polylactic acid.

[0075] The mass fraction compositions of the polylactic acid / nanocellulose composite materials of Examples 6 to 10 are shown in Table 2, and the polylactic acid / nanocellulose composite materials of Examples 6 to 10 are numbered S1, S2, S3, S4, and S5, respectively, and a single factor experiment is performed.

[0076] In Examples 6 to 10, the nanocellulose is straw nanocellulose, the sulfonated nanocellulose is highly sulfonated nanocellulose, the ionic liquid is 1-butyl-1-methylpyrrolidone hexafluorophosphate, the compatibilizer is triacetin, the lubricant is oleamide, and the coupling agent is titanate coupling agent CS-101.

[0077] Table 2

[0078]

[0079] The preparation method of polylactic acid / nanocellulose of Example 6 comprises the following steps:

[0080] 1. Preparation of highly sulfonated nanocellulose

[0081] (1) Mix 8 parts of 100-mesh straw powder with 80 parts of 20 w / v% sodium hydroxide solution, heat and stir at 95°C for 6 h, wash with pure water until neutral, add 60 parts of 20 w / v% sodium chlorite solution and 3 parts of glacial acetic acid, heat and stir at 60°C for 2 h, and then wash with pure water until neutral;

[0082] (2) The solid-liquid mixture obtained in (1) was subjected to high-speed shearing treatment using a homogenizer at a speed of 15,000 rpm for 2 h; the homogenized sample was centrifuged and washed, and then freeze-dried to obtain nanocellulose;

[0083] (3) The 6 nanocellulose samples obtained in (2) were dispersed in 100 parts of 20 w / v% sodium periodate solution at 40°C, and the mixture was stirred for 4 h in a lightless nitrogen environment, and then washed with pure water until neutral. The obtained product was dispersed in 90 parts of 15 w / v% sodium sulfite, stirred at room temperature for 2 h, and the sample was centrifuged and washed until neutral, and then freeze-dried to obtain highly sulfonated nanocellulose.

[0084] 2. Preparation of polylactic acid / nanocellulose composites

[0085] a: Add 1 part of highly sulfonated nanocellulose to 100 parts of deionized water and ultrasonicate for 15 min. Add 3 parts of ionic liquid to the suspension. Dry the solid-liquid mixture at 65°C for 72 h to obtain dry ionic liquid-modified sulfonated nanocellulose;

[0086] b: adding the ionic liquid modified sulfonated nanocellulose obtained in step a, 100 parts of polylactic acid, 2 parts of a compatibilizer, 0.5 parts of a lubricant, and 1 part of a coupling agent into a high-speed mixer and mixing for 80 minutes at a speed of 300 rpm to obtain a premix;

[0087] c: adding the premix obtained in step b into a twin-screw extruder for extrusion and granulation, the processing temperature of the twin-screw extruder is 180° C., the screw aspect ratio is 35, and the rotation speed is 50 rpm to obtain polylactic acid / nanocellulose composite particles;

[0088] d: Processing the polylactic acid / nanocellulose composite material particles obtained in step c into a polylactic acid / nanocellulose composite material by a hot press.

[0089] The preparation methods of the polylactic acid / nanocellulose composite materials of Examples 7 to 10 are basically the same as those of Example 6, except that in step a of the preparation methods of Examples 7 to 10, the addition amounts of highly sulfonated nanocellulose are 3 parts, 5 parts, 7 parts, and 10 parts, respectively, to prepare the polylactic acid / nanocellulose composite materials of Examples 7 to 10, respectively.

[0090] The same method as that of the polylactic acid / nanocellulose composite material of Example 1 was used to perform tensile test, impact test and plasticizer migration and precipitation test on the polylactic acid / nanocellulose composite materials of Examples 6 to 10. The test results of tensile strength and tensile elongation at break are shown in Figure 1. Figure 4 As shown, the impact strength is Figure 5 The results of the migration and precipitation tests are shown in Figure 6 shown.

[0091] from Figure 4 , Figure 5 and Figure 6It can be seen that as the amount of highly sulfonated nanocellulose added increases, the tensile strength of the polylactic acid / nanocellulose composite materials of Examples 6 to 10 increases, the elongation at break decreases, the impact strength increases, and the plasticizer migration and precipitation rate decreases. The increase in tensile strength, the decrease in elongation at break, and the increase in impact toughness of the polylactic acid / nanocellulose composite materials are mainly because nanocellulose, as an effective reinforcement of polylactic acid, is dispersed in the polylactic acid matrix and plays a toughening role. At the same time, the rigidity of nanocellulose leads to a decrease in the elongation at break of the polylactic acid / nanocellulose composite material. With the increase of highly sulfonated nanocellulose, it is ensured that the number of sites for the binding of ionic liquids on cellulose increases, the freeness of ionic liquids in the polylactic acid matrix is ​​reduced, and the precipitation of ionic liquids is reduced. Combining these performance values, Examples 6 to 10 have obvious advantages over Comparative Examples 1 and 2. Among them, the tensile strength, tensile elongation at break and impact strength were at least increased by 21.1%, 49.4% and 40.8% respectively compared with the addition of epoxidized soybean oil, and the migration and precipitation rate was reduced by 61.7%; compared with the polylactic acid / nanocellulose composite material comparative example 2 with the addition of unmodified nanocellulose, its tensile strength, tensile elongation at break and impact strength were at least increased by 4.0%, 44.2% and 33.3% respectively, and the migration and precipitation rate was reduced by 17.1%.

[0092] The mass fraction compositions of the polylactic acid / nanocellulose composite materials of Examples 11 to 15 are shown in Table 3, and the polylactic acid / nanocellulose composite materials of Examples 11 to 15 are numbered E1, E2, E3, E4, and E5, respectively, and single factor experiments are performed.

[0093] In Examples 11 to 15, the nanocellulose is bagasse nanocellulose, the sulfonated nanocellulose is low-level sulfonated nanocellulose, the ionic liquid is 1-allyl-3-methylimidazole chloride, the compatibilizer is octaaminopropyl cage-type polysilsesquioxane, the lubricant is erucamide, and the coupling agent is aluminate coupling agent DL-411.

[0094] Table 3

[0095]

[0096] The method for preparing the polylactic acid / nanocellulose composite material of Example 11 comprises the following steps:

[0097] 1. Preparation of low-sulfonated nanocellulose

[0098] (1) Mix 5 parts of 150-mesh bagasse powder with 70 parts of 10 w / v% sodium hydroxide solution, heat and stir at 85°C for 2 h, wash with pure water until neutral, add 60 parts of 10 w / v% sodium chlorite solution and 4 parts of glacial acetic acid, heat and stir at 80°C for 1 h, and then wash with pure water until neutral;

[0099] (2) The solid-liquid mixture obtained in (1) was subjected to high-speed shearing treatment using a homogenizer at a speed of 10,000 rpm for 1 h; the homogenized sample was centrifuged and washed, and then freeze-dried to obtain nanocellulose;

[0100] (3) Disperse 10 parts of the nanocellulose sample obtained in (2) in 40 parts of 10 w / v% sodium periodate solution at 40°C, stir the mixture for 1 hour in a lightless nitrogen environment, and then wash it with pure water until it is neutral. Disperse the obtained product in 80 parts of 15 w / v% sodium sulfite, stir it at room temperature for 1 hour, wash the sample by centrifugation until it is neutral, and then freeze-dry it to obtain low-level sulfonated nanocellulose.

[0101] 2. Preparation of polylactic acid / nanocellulose composites

[0102] a: Add 3 parts of low-level sulfonated nanocellulose to 100 parts of deionized water and sonicate for 5 minutes. Add 3 parts of ionic liquid to the suspension. Dry the solid-liquid mixture at 60°C for 72 hours to obtain a dry ionic liquid-modified sulfonated nanocellulose product;

[0103] b: adding the ionic liquid modified sulfonated nanocellulose obtained in step a, 100 parts of polylactic acid, 1 part of a compatibilizer, 1 part of a lubricant, and 1 part of a coupling agent into a high-speed mixer and mixing for 80 minutes at a speed of 600 rpm to obtain a premix;

[0104] c: adding the premix obtained in step b into a twin-screw extruder for extrusion and granulation, the processing temperature of the twin-screw extruder is 180° C., the screw aspect ratio is 25, and the rotation speed is 100 rpm to obtain polylactic acid / nanocellulose composite particles;

[0105] d: Processing the polylactic acid / nanocellulose composite material particles obtained in step c into a polylactic acid / nanocellulose composite material by an injection molding machine.

[0106] The preparation method of the polylactic acid / nanocellulose composite materials of Examples 12 to 15 is basically the same as that of Example 11, except that in step b of the preparation method of Examples 12 to 15, the amount of the compatibilizer added is 2 parts, 3 parts, 4 parts, and 5 parts, respectively, to prepare the polylactic acid / nanocellulose composite materials of Examples 12 to 15, respectively.

[0107] The same method as that of the polylactic acid / nanocellulose composite material of Example 1 was used to perform tensile test, impact test and plasticizer migration and precipitation test on the polylactic acid / nanocellulose composite materials of Examples 11 to 15. The test results of tensile strength and tensile elongation at break are shown in Figure 1. Figure 7 As shown, the impact strength is Figure 8 The results of the migration and precipitation tests are shown in Fig. 9 shown.

[0108] from Figure 7 , Figure 8 and Fig. 9 It can be seen that as the amount of the compatibilizer added increases, the tensile strength of the polylactic acid / nanocellulose composite material of Example 11 to Example 15 gradually decreases, the elongation at break gradually increases, the impact strength gradually increases, and the plasticizer migration precipitation rate gradually decreases. As the content of the compatibilizer increases, the functional groups of the compatibilizer molecules combine with the unmodified functional groups on the nanocellulose molecular chain, enhancing the hydrophobicity of the nanocellulose, making it have better interfacial compatibility with polylactic acid, enhancing the dispersion effect of nanocellulose in polylactic acid, and then showing at the macro level that the mechanical properties of the polylactic acid composite material are enhanced. At the same time, the increase in the content of the compatibilizer can attract free ionic liquids, limit the molecular motion of the ionic liquid, and then reduce its precipitation in the polylactic acid composite material. Among these performance values, even the minimum value has advantages over Comparative Examples 1 and 2. Among them, the tensile strength, tensile elongation at break and impact strength were at least increased by 21.0%, 68.7% and 21.5% respectively compared with the comparative example 1 with the addition of epoxidized soybean oil, and the migration and precipitation rate was reduced by 71.5%; compared with the comparative example 2 of the polylactic acid / nanocellulose composite material with the addition of unmodified nanocellulose, its tensile strength, tensile elongation at break and impact strength were at least increased by 4.1%, 65.4% and 11.4% respectively, and the migration and precipitation rate was reduced by 38.3%.

[0109] The mass fraction compositions of the polylactic acid / nanocellulose composite materials of Examples 16 to 18 are shown in Table 4, and the polylactic acid / nanocellulose composite materials of Examples 16 to 18 are respectively denoted by numbers R1, R2, and R3, and a single factor experiment is performed.

[0110] In Examples 16 to 18, the nanocellulose is bamboo nanocellulose, the ionic liquid is 1-allyl-3-methylimidazole chloride, the compatibilizer is glycidyl methacrylate, the lubricant is sodium mustard coconut aminopropionate, and the coupling agent is titanate coupling agent CS-101.

[0111] Table 4

[0112]

[0113] The preparation method of the polylactic acid / nanocellulose composite material of Example 16 comprises the following steps:

[0114] 1. Preparation of low-level sulfonated nanocellulose

[0115] (1) 10 parts of 200-mesh bamboo powder were mixed with 70 parts of 10 w / v% sodium hydroxide solution, heated and stirred at 90°C for 2 h, washed with pure water until neutral, and then 60 parts of 10 w / v% sodium chlorite solution and 4 parts of glacial acetic acid were added, heated and stirred at 80°C for 2 h, and then washed with pure water until neutral;

[0116] (2) The solid-liquid mixture obtained in (1) was subjected to high-speed shearing treatment using a homogenizer at a speed of 20,000 rpm for 2 h; the homogenized sample was centrifuged and washed, and then freeze-dried to obtain nanocellulose;

[0117] (3) Disperse 10 parts of the nanocellulose sample obtained in (2) in 40 parts of 10 w / v% sodium periodate solution at 40°C, stir the mixture for 2 h in a lightless nitrogen environment, and then wash it with pure water until it is neutral. Disperse the obtained product in 90 parts of 15 w / v% sodium sulfite, stir it at room temperature for 1 h, wash the sample by centrifugation until it is neutral, and then freeze-dry it to obtain low-level sulfonated nanocellulose.

[0118] 2. Preparation of polylactic acid / nanocellulose composites

[0119] a: Add 3 parts of low-level sulfonated nanocellulose to 100 parts of deionized water and ultrasonicate for 10 min. Add 3 parts of ionic liquid to the suspension. Dry the solid-liquid mixture at 65°C for 72 h to obtain a dry ionic liquid-modified sulfonated nanocellulose product;

[0120] b: adding the ionic liquid modified sulfonated nanocellulose obtained in step a, 100 parts of polylactic acid, 2 parts of a compatibilizer, 2 parts of a lubricant, and 0.5 parts of a coupling agent into a high-speed mixer and mixing for 120 min at a speed of 800 rpm to obtain a premix;

[0121] c: adding the premix obtained in step b into a twin-screw extruder for extrusion and granulation, the processing temperature of the twin-screw extruder is 190° C., the screw aspect ratio is 40, and the rotation speed is 200 rpm to obtain polylactic acid / nanocellulose composite material particles;

[0122] d: Processing the polylactic acid / nanocellulose composite material particles obtained in step c into a polylactic acid / nanocellulose composite material by an injection molding machine.

[0123] The preparation method of the polylactic acid / nanocellulose composite materials of Examples 17 and 18 is basically the same as that of Example 16, except that in step (3) of the preparation method of Examples 17 and 18, the amount of sodium periodate solution added is 60 parts and 100 parts, respectively, to prepare the polylactic acid / nanocellulose composite materials of Examples 17 and 18, respectively.

[0124] The same method as that of the polylactic acid / nanocellulose composite material of Example 1 was used to perform tensile test, impact test and plasticizer migration and precipitation test on the polylactic acid / nanocellulose composite materials of Examples 16 to 18. The test results of tensile strength and tensile elongation at break are shown in Figure 1. Fig.10 As shown, the impact strength is Fig.11 The results of the migration and precipitation tests are shown in Fig.12 shown.

[0125] from Fig.10 , Fig.11 and Fig.12 It can be seen that as the degree of sulfonation of nanocellulose increases, the tensile strength of the polylactic acid / nanocellulose composite materials of Examples 16 to 18 gradually decreases, the elongation at break gradually increases, the plasticizer migration and precipitation rate gradually decreases, and the impact toughness first increases and then decreases. This is mainly because the higher the degree of sulfonation modification of nanocellulose, the stronger its damage to the nanocellulose chain, which reduces the aspect ratio of nanocellulose and leads to the weakening of its reinforcing effect on the polylactic acid composite material. But at the same time, due to the increase in the degree of sulfonation, the negative charge on the surface of nanocellulose is enhanced, which strengthens the attraction of nanocellulose to ionic liquids, further limits the freeness of ionic liquids in polylactic acid, and reduces the precipitation of ionic liquids in polylactic acid. Among these performance values, even the minimum value has advantages over Comparative Examples 1 and 2. Among them, the tensile strength, tensile elongation at break and impact strength were at least increased by 24.0%, 55.6% and 59.5% respectively compared with the comparative example 1 with the addition of epoxidized soybean oil, and the migration and precipitation rate was reduced by 72.5%; compared with the comparative example 2 of the polylactic acid / nanocellulose composite material with the addition of unmodified nanocellulose, its tensile strength, tensile elongation at break and impact strength were at least increased by 24.4%, 51.0% and 41.3% respectively, and the migration and precipitation rate was reduced by 40.4%.

Claims

1. A toughened and anti-precipitation polylactic acid / nanocellulose composite material, characterized in that: The mass fraction is as follows: 100 parts of polylactic acid, 1 to 10 parts of sulfonated nanocellulose, 1 to 10 parts of ionic liquid, 1 to 5 parts of a compatibilizer, 0.5 to 2 parts of a lubricant, and 0.5 to 2 parts of a coupling agent. The preparation method of the toughened and anti-precipitation polylactic acid / nanocellulose composite material comprises the following steps: 1) Mix 1 to 10 parts of raw material powder with 70 to 80 parts of sodium hydroxide solution, heat and stir at 60 to 95°C for 2 to 4 hours, wash with pure water until neutral, add 40 to 60 parts of sodium chlorite solution and 3 to 4 parts of glacial acetic acid, heat and stir at 60 to 80°C for 1 to 2 hours, and then wash with pure water until neutral; 2) The solid-liquid mixture obtained in step 1) is subjected to high-speed shearing treatment using a homogenizer for 1 to 2 hours, with the speed of the homogenizer being 10,000 to 20,000 rpm; the homogenized sample is centrifuged and washed, and then freeze-dried to obtain sulfonated nanocellulose; 3) Dispersing 1 to 10 parts of the nanocellulose sample obtained in step 2) in 40 to 100 parts of sodium periodate solution at 30°C to 40°C, stirring the mixture in a lightless nitrogen environment for 1 to 2 hours, and then washing with pure water until neutral; then dispersing the obtained product in 80 to 90 parts of sodium sulfite, stirring at room temperature for 1 to 2 hours, centrifuging and washing the sample until neutral, and then freeze-drying to obtain sulfonated nanocellulose; 4) adding 1 to 10 parts of the sulfonated nanocellulose obtained in step 3) to 100 parts of deionized water, ultrasonicating for 5 to 10 minutes, dropping 1 to 10 parts of ionic liquid into the suspension, and drying the solid-liquid mixture at 60 to 70° C. for 72 hours to obtain dry ionic liquid-modified sulfonated nanocellulose; 5) adding the ionic liquid modified sulfonated nanocellulose obtained in step 4), 100 parts of polylactic acid, 1 to 5 parts of a compatibilizer, 0.5 to 2 parts of a lubricant, and 0.5 to 2 parts of a coupling agent into a high-speed mixer and mixing for 60 to 120 minutes at a speed of 300 to 800 rpm to obtain a premix; 6) adding the premix obtained in step 5) into a twin-screw extruder for extrusion and granulation, wherein the processing temperature of the twin-screw extruder is 110-190° C., the screw aspect ratio is 25-50, and the rotation speed is 50-250 rpm to obtain polylactic acid / nanocellulose composite material particles; 7) Processing the composite material particles obtained in step 6) into a polylactic acid / nanocellulose composite material by an injection molding machine or a hot press.

2. The toughened and anti-precipitation polylactic acid / nanocellulose composite material according to claim 1, characterized in that: The raw material powder is one or a combination of two or more of wood powder, bamboo powder, straw powder and bagasse powder.

3. The toughened and anti-precipitation polylactic acid / nanocellulose composite material according to claim 1, characterized in that: The sulfonated nanocellulose is one of low-degree sulfonated nanocellulose, medium-degree sulfonated nanocellulose and high-degree sulfonated nanocellulose. The low degree is 10% to 29% sulfonation degree, the medium degree is 30% to 59% sulfonation degree and the high degree is 60% to 80% sulfonation degree.

4. The toughened and anti-precipitation polylactic acid / nanocellulose composite material according to claim 1, characterized in that: The ionic liquid is one or a combination of two or more of 1-butyl-3-methylimidazolium tetrafluoroborate, 1-butyl-1-methylpyrrolidine hexafluorophosphate, and 1-allyl-3-methylimidazolium chloride.

5. The toughened and anti-sedimentation polylactic acid / nanocellulose composite material according to claim 1, characterized in that: The compatibilizer is at least one of glycidyl methacrylate, octaaminopropyl cage-type polysilsesquioxane, and triacetin.

6. The toughened and anti-precipitation polylactic acid / nanocellulose composite material according to claim 1, characterized in that: The lubricant is one or a combination of two or more of sodium cocoyl aminopropionate, polyvinyl acetate resin, ethylene bisstearic acid amide, oleic acid amide and erucic acid amide.

7. The toughened and anti-precipitation polylactic acid / nanocellulose composite material according to claim 1, characterized in that: The coupling agent is at least one of a silane coupling agent, a titanate coupling agent CS-101 and an aluminate coupling agent DL-411.

8. The toughened and anti-sedimentation polylactic acid / nanocellulose composite material according to claim 7, characterized in that: The silane coupling agent is at least one of KH151, KH550, KH580 or KH790.

Citation Information

Patent Citations

  • Biodegradable cellulose blending material and preparation method thereof

    CN104151622A

  • High-length-diameter-ratio nano-cellulose-reinforced polylactic acid composite material and preparation method thereof

    CN104910422A

  • Polylactic acid composite material

    CN105440610A

  • Method for improving mechanical property of polylactic acid, application thereof and method for preparing biodegradable bionic bait

    CN109517349A

  • Water-resistant nanocellulose film and preparation method thereof

    CN110551301A

Cited By

  • Modified resin composition for high-pressure-resistant and high-wear-resistant PVC (polyvinyl chloride) hose

    CN119529442A

  • Zinc ion battery electrolyte containing sulfonated cellulose nanowhisker additive as well as preparation method and application of zinc ion battery electrolyte

    CN121123433A

  • Preparation method of full-ecosphere degradation injection molding raw material of PHA (Polyhydroxyalkanoate) base material

    CN121227057A

  • Bamboo-based material as well as preparation method and application thereof

    CN121801344A