Method for manufacturing positive electrode active material for lithium secondary battery and positive electrode active material manufactured by the same
By using urea and citric acid to form single-particle lithium metal oxide active materials at lower temperatures, the method addresses manufacturing inefficiencies and environmental issues, resulting in improved battery performance and reduced gas generation.
Patent Information
- Application Number
- JP2023511851
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-10-06
- Filing Date
- 2021-10-06
- Publication Date
- 2024-09-17
- Estimated Expiration
- 2041-10-06
AI Technical Summary
Conventional methods for producing lithium metal oxide positive electrode active materials face issues such as complex manufacturing processes, long processing times, environmental pollution from alkali use, particle cracking during electrode rolling, increased resistance due to high firing temperatures, and reduced lithium mobility, leading to decreased battery performance.
A method involving the use of specific fuels like urea and citric acid, along with lithium, nickel, and cobalt sources, to produce a mixed solution, followed by heating and heat-treating at lower temperatures to form single-particle lithium metal oxide active materials, avoiding the formation of electrochemically inactive rock salt phases and reducing gas generation.
This approach shortens the manufacturing process, produces uniform single-particle active materials with improved resistance and capacity characteristics, and reduces gas generation, enhancing battery lifespan and performance.
Smart Images

Figure 0007551215000003 
Figure 0007551215000004 
Figure 0007551215000002
Abstract
Description
[Technical field]
[0001] This application claims the benefit of priority based on Korean Patent Application No. 10-2020-0128547, filed on October 6, 2020, the entire contents of which are incorporated herein by reference.
[0002] The present invention relates to a method for producing a positive electrode active material for a lithium secondary battery, a positive electrode active material produced thereby, and a lithium secondary battery including the positive electrode active material. [Background technology]
[0003] With the development of technology and increasing demand for mobile devices, the demand for secondary batteries as an energy source is rapidly increasing. Among these secondary batteries, lithium secondary batteries, which have high energy density and voltage, long cycle life, and low self-discharge rate, have been commercialized and are widely used.
[0004] Lithium secondary batteries can be broadly divided into a positive electrode active material, a negative electrode active material, a separator, and an electrolyte. The negative electrode active material mainly contains a carbon material, and active research is being actively conducted to use lithium metal, sulfur compounds, silicon compounds, tin compounds, and the like.
[0005] In addition, lithium metal oxides containing lithium are mainly used as positive electrode active materials, and layered lithium metal oxides such as cobalt-based, nickel-based, and ternary systems in which cobalt, nickel, and manganese coexist are mainly used.
[0006] A common method for producing layered lithium metal oxide is to produce a precursor by adding a metal salt containing the metal to be used as a positive electrode active material and an alkali to water to precipitate the metal hydroxide. This method has problems such as a complicated and time-consuming production process and the use of alkali to generate a large amount of wastewater that can cause environmental pollution.
[0007] In addition, conventional lithium metal oxides are generally in the form of spherical secondary particles formed by agglomeration of tens to hundreds of primary particles. However, in the case of lithium metal oxides in the form of secondary particles formed by agglomeration of many primary particles, there is a problem that the primary particles are easily broken during the rolling process in the manufacture of the positive electrode, and cracks are generated inside the particles during charging and discharging. When the particles of the positive electrode active material are broken or cracked, the contact area with the electrolyte increases, and gas generation and deterioration of the active material due to side reactions with the electrolyte increase, resulting in a problem of reduced life characteristics.
[0008] To solve this problem, a method of producing a lithium metal oxide in a single particle form by increasing the firing temperature during firing of the precursor has been used. However, in this case, the size of the primary particles is relatively large compared to the secondary particle form, and there are few interfaces between the primary particles that serve as diffusion paths for lithium ions, so the mobility of lithium is reduced and the initial resistance is high. In addition, since it is produced at a relatively high firing temperature, the amount of lithium by-products increases and it is easily converted into a rock salt phase, which is an electrochemically inactive phase, resulting in high surface resistance.
[0009] Therefore, various methods for producing positive electrode active materials to solve this problem have been researched. Summary of the Invention [Problem to be solved by the invention]
[0010] An object of the present invention is to provide a method for producing a positive electrode active material that can shorten the process time as compared with the conventional techniques.
[0011] Another object of the present invention is to produce a positive electrode active material in a single particle form at a relatively low firing temperature. [Means for solving the problem]
[0012] The present invention relates to 1) adding one or more first fuels selected from the group consisting of urea, glycine, carbohydrazide, oxalyldihydrazide, and hexamethylenetetramine, one or more second fuels selected from the group consisting of citric acid, oxalic acid, sucrose, glucose, and acetylacetone, and metal source materials including a lithium source material, a nickel source material, a cobalt source material, and a manganese source material, into water and stirring to prepare a mixed solution; 2) heating the mixed solution to combust it into powder; 3) a step of heat-treating the powder obtained in step 2).
[0013] The present invention also provides a positive electrode active material for a lithium secondary battery produced by the above-mentioned production method.
[0014] The present invention also provides a lithium secondary battery including a positive electrode containing the positive electrode active material, a negative electrode, a separator interposed between the positive electrode and the negative electrode, and an electrolyte. Effect of the Invention
[0015] The method for producing a positive electrode active material according to the present invention has the advantage that the precursor formation step is omitted, and therefore the process time is shortened.
[0016] In addition, in the conventional technology, a heat treatment of 850°C or more was required in the precursor calcination step to produce a positive electrode active material in a single particle shape, but the present invention has the advantage that a positive electrode active material in a single particle shape can be produced at a lower temperature than this.
[0017] In addition, by lowering the sintering temperature, it is possible to prevent the formation of a rock salt phase on the surface, thereby improving the resistance and capacitance characteristics, prevent the cation mixing phenomenon that occurs during phase change, and reduce the amount of lithium by-products, thereby reducing the amount of gas generated due to side reactions with the electrolyte.
[0018] In addition, the shape and growth direction of the positive electrode active material particles can be adjusted depending on the type of fuel used, which is advantageous in producing single particles with a large particle diameter. [Brief description of the drawings]
[0019] [Figure 1] FIG. 2 is a low-magnification TEM image of the positive electrode active material prepared in Example 1 of the present invention. [Diagram 2] FIG. 2 shows a high-magnification TEM image and a selected area electron diffraction (SAED) pattern of the positive electrode active material prepared in Example 1 of the present invention. [Diagram 3] FIG. 2 is a SEM image of the positive electrode active material prepared in Example 1 of the present invention. [Figure 4] FIG. 2 is a SEM image of the positive electrode active material prepared in Comparative Example 1 of the present invention. [Diagram 5] FIG. 2 is a diagram showing the results of an experiment to evaluate a capacity retention rate carried out in Experimental Example 1 of the present invention. [Figure 6] FIG. 11 is a diagram showing the results of a gas generation rate evaluation experiment carried out in Experimental Example 2 of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0020] In the following, the present invention will be described in more detail in order to facilitate understanding of the present invention.
[0021] In this specification, the term "average particle size (D 50The "average particle size (D )" can be defined as the particle size at 50% of the particle size distribution, and can be measured, for example, by using a laser diffraction method. More specifically, the positive electrode active material is dispersed in a solution, introduced into a commercially available laser diffraction particle size measuring device (e.g., Microtrac MT 3000), and irradiated with ultrasonic waves of about 28 kHz at an output of 60 W. The average particle size (D ) can be measured at 50% of the particle size distribution in the measuring device. 50 ) can be calculated.
[0022] In the present specification, the term "primary particle" refers to the smallest particle unit that can be distinguished as one mass when observing a cross section of a positive electrode active material through a scanning electron microscope (SEM), and can be composed of one crystal grain or multiple crystal grains. Specifically, the average particle size of the primary particles can be measured by measuring the particle sizes of each particle distinguished in cross-sectional SEM data of the positive electrode active material particles and then calculating the arithmetic average value of these.
[0023] In this specification, the term "secondary particle" refers to a secondary structure formed by aggregation of a plurality of primary particles. The average particle size of the secondary particles can be measured by the above-mentioned laser diffraction method.
[0024] In this specification, the term "single particle" is used to distinguish it from the commonly used positive electrode active material particles having a secondary particle shape formed by the aggregation of tens to hundreds of primary particles, and is a concept that includes a single particle consisting of one primary particle and an aggregate particle of 10 or less primary particles.
[0025] In the past, a cathode active material was generally prepared by adding a basic substance to an aqueous solution containing a metal salt to precipitate the metal hydroxide, and then dry-mixing the precursor with a lithium source, a doping source, and a coating source, followed by high-temperature heat treatment.
[0026] In this case, the precursor mainly consists of spherical secondary particles formed by the aggregation of primary particles of several nm to several tens of nm. In order to convert this into a single particle shape, it is necessary to perform a process of firing at a high temperature of 850°C or more, firing multiple times at a relatively low temperature, or lowering the firing temperature by adding a flux material.
[0027] When the firing temperature is increased to form the single particles, a phase change occurs in which the existing layered structure changes to a spinel structure, and the spinel structure changes to a rock salt phase structure, resulting in a drawback in that the resistance characteristics of the single particles themselves are reduced due to the electrochemically inactive rock salt phase. In addition, the phase change process causes lithium ions to be released and nickel ions to be replaced by the lithium layer, i.e., cation mixing, which leads to deterioration of the positive electrode material, and the release of lithium ions relatively increases the amount of lithium by-products such as Li2CO3 and LiOH, which increases the amount of gas generated due to side reactions with the electrolyte when used as a positive electrode material in lithium secondary batteries.
[0028] Meanwhile, the method for producing a positive electrode active material for a lithium secondary battery according to the present invention has an advantage that a positive electrode active material in the form of a single particle can be produced even at a temperature of 700° C. to 800° C., since it includes a combustion reaction from a solution state to a gel state to a powder state. That is, it is possible to prevent a phase change to a rock salt phase, reduce the cation mixing phenomenon and the amount of lithium by-products, and contribute to improving the resistance and stability as a positive electrode material for a lithium secondary battery.
[0029] In addition, when trying to increase the particle size by applying the conventional high-temperature sintering to form single particles, a high temperature of 900°C or more is required, which is disadvantageous in that it is difficult to apply to practical processes. However, according to the present invention, there is an advantage that single particles having a large particle size can be formed at a relatively low temperature.
[0030] In addition, in the present invention, the lithium source material and the transition metal source material are mixed at the same time, so that a uniform positive electrode active material can be produced without agglomeration of lithium.
[0031] In particular, the inventors have confirmed that when two or more fuels are used in the combustion reaction, the size, shape and degree of dispersion of the positive electrode active material particles can be easily controlled. In particular, they have found that when one or more first fuels selected from the group consisting of urea, glycine, carbohydrazide, oxalyl dihydrazide and hexamethylenetetramine are used together with one or more second fuels selected from the group consisting of citric acid, oxalic acid, sucrose, glucose and acetylacetone, particles having a uniform shape can be obtained at a relatively low process temperature.
[0032] The method for producing a positive electrode active material for a lithium secondary battery of the present invention includes the following steps 1) to 3), and each step will be described in more detail below.
[0033] 1) Producing a mixed solution Step 1) is a step of adding the first fuel, the second fuel and the metal source material to water and stirring them to produce a mixed solution.
[0034] Specifically, the first fuel may be selected from the group consisting of urea, glycine, carbohydrazide, oxalyldihydrazide, and hexamethylenetetramine, and the second fuel may be selected from the group consisting of citric acid, oxalic acid, sucrose, glucose, and acetylacetone.
[0035] Preferably, the first fuel may be urea and the second fuel may be citric acid.
[0036] The first fuel, including urea, decomposes into water to generate amino functional groups, which amplify combustion through a redox reaction, and thus have the advantage of being able to lower the process temperature. However, when the first fuel is used alone as a fuel, it is difficult to control the size and shape of the cathode active material nanoparticles. This can be compensated for by the second fuel, including citric acid, which generates carboxylic functional groups when decomposed, and these have strong binding power, allowing the components of the mixed solution to be firmly bound, thereby allowing cathode active material nanoparticles of a relatively uniform size and shape to be manufactured.
[0037] In addition, the first fuel is decomposed to produce ammonia, which increases the pH of the mixed solution containing it, which has the advantage of causing gelation of the solution and amplifying the combustion reaction. However, if the pH becomes excessively high, precipitation of metal hydroxides in the solution occurs, which can have the opposite effect of reducing the efficiency of the combustion reaction. To compensate for this, when the second fuel is added, the acidic carboxyl anions decomposed from the second fuel lower the pH, creating a pH suitable for the combustion reaction to occur.
[0038] In the present invention, the weight ratio of the first fuel and the second fuel may be 60:40 to 90:10, preferably 70:30 to 90:10, and more preferably 75:35 to 85:15, in which case the effect of the combination of the first fuel and the second fuel described above can be maximized.
[0039] The amount of gas generated during the combustion process in step 2) described below is proportional to the amount of fuel input, but when both the first and second fuels are used, the pressure of this gas generated increases as the weight of the first fuel increases.
[0040] The metallic fuel materials of the present invention include a lithium source material, a nickel source material, a cobalt source material and a manganese source material.
[0041] The lithium source material may be a lithium-containing sulfate, nitrate, acetate, carbonate, oxalate, citrate, halide, hydroxide, oxyhydroxide, or a combination thereof, and is not particularly limited as long as it is soluble in water.
[0042] Specifically, the lithium source material may be at least one selected from Li2CO3, LiNO3, LiNO2, LiOH, LiOH·H2O, LiH, LiF, LiCl, LiBr, LiI, CH3COOLi, Li2O, Li2SO4, CH3COOLi, and Li3C6H5O7, and may be preferably LiNO3, but is not limited thereto.
[0043] In the present invention, the nickel source material may be, for example, nickel-containing acetate, nitrate, sulfate, halide, sulfide, hydroxide, oxide, oxyhydroxide, or a combination thereof, and specifically may be at least one selected from Ni(OH)2, NiO, NiOOH, NiCO3·2Ni(OH)2·4H2O, NiC2O2·2H2O, Ni(NO3)2·6H2O, NiSO4, NiSO4·6H2O, fatty acid nickel salts, and nickel halides, and preferably Ni(NO3)2·6H2O, but is not limited thereto.
[0044] In the present invention, the cobalt source material may be a cobalt-containing acetate, nitrate, sulfate, halide, sulfide, hydroxide, oxide, or oxyhydroxide, and specifically may be at least one selected from Co(OH)2, CoOOH, Co(OCOCH3)2·4H2O, Co(NO3)2·6H2O, CoSO4, and Co(SO4)2·7H2O, and preferably Co(NO3)2·6H2O, but is not limited thereto.
[0045] In the present invention, the manganese-containing raw material may be, for example, manganese-containing acetate, nitrate, sulfate, halide, sulfide, hydroxide, oxide, oxyhydroxide, or a combination thereof, and specifically may be one or more selected from manganese oxides such as Mn2O3, MnO2, and Mn3O4, manganese salts such as MnCO3, Mn(NO3)2·6H2O, MnSO4, manganese acetate, manganese dicarboxylate, manganese citrate, and fatty acid manganese salt, manganese oxyhydroxide, and manganese chloride, and is preferably Mn(NO3)2·6H2O, but is not limited thereto.
[0046] The composition of the final cathode active material may be adjusted by adjusting the concentrations of the lithium source material, the nickel source material, the cobalt source material, and the manganese source material, and the metal source material may further include a doping source material, if necessary.
[0047] In step 1), the total content of the first fuel and the second fuel may be 20wt% to 60wt%, preferably 30wt% to 50wt%, based on the total content of the metal raw material. When the content of the fuel is within this range, it is preferable in terms of obtaining a suitable primary calcination effect and a suitable yield of the final positive electrode active material due to sufficient combustion. If it is less than 10wt%, combustion does not occur sufficiently, making it difficult to produce a single-particle positive electrode active material, and if it exceeds 90wt%, there is a problem that the yield of the final positive electrode active material is significantly reduced.
[0048] In step 1), the content of the metal source material may be 15wt% to 50wt%, preferably 25wt% to 45wt%, more preferably 30wt% to 40wt% based on the total content of the mixed solution. When the content of the metal source material is within the above range, it is preferable that a uniform initial solution can be prepared. If it is less than 15wt%, the amount of the finally obtained positive electrode active material may be small, and if it exceeds 50wt%, the solution prepared at the beginning is not dissolved uniformly, and it is difficult to finally obtain a positive electrode active material with a uniform shape.
[0049] The remainder of the mixed solution other than the fuel and the metal source material may be water, such as distilled water, unless otherwise specified.
[0050] In the present invention, the mixed solution may be stirred at a temperature of 40° C. to 60° C. for 30 to 60 minutes, but is not limited thereto.
[0051] 2) Heat the mixture and burn it into powder. Step 2) is a step in which the mixed solution is heated using a hot plate to evaporate water and turn into a gel, and then heat is continued to be applied to cause a combustion reaction in the gel, turning it into a powder.
[0052] The heating in step 2) is carried out at a temperature of 300° C. to 500° C., preferably 300° C. to 400° C. If the heating temperature in step 2) is less than 300° C., spontaneous combustion is unlikely to occur.
[0053] 3) Heat treating the powder Step 3) is a step of heat-treating the powder obtained in step 2) to convert the single particle, which is in an incomplete state due to the previous combustion, i.e., the particle may have a single particle shape but does not form a completely layered crystal phase and is mixed with a nickel oxide phase, into a positive electrode active material particle having electrochemical properties as a battery material.
[0054] Specifically, the powder obtained in step 2) is dried, then pulverized into finer powder using a mortar, and then heat-treated.
[0055] The heat treatment in step 3) is performed at a temperature of 700°C to 800°C. If the heat treatment temperature is less than 700°C, the layered crystal phase that functions as the positive electrode active material may not be properly formed. If the heat treatment temperature exceeds 800°C, the rock salt crystal phase that occurs in the step of degrading the positive electrode active material is likely to occur, which may lead to a decrease in the capacity and lifespan of the battery including this.
[0056] positive electrode active material The positive electrode active material for a lithium secondary battery of the present invention is produced by the above-mentioned method for producing a positive electrode active material for a lithium secondary battery.
[0057] The positive electrode active material has an average particle size (D 50 ) is 0.5 μm to 2.5 μm, preferably 1 μm to 2 μm. Whether or not a single particle is contained can be confirmed by SEM, TEM or EBSD analysis.
[0058] The positive electrode active material has an average particle size (D 50 When the particle size is within the above range, it is preferable that the capacity can be increased due to the large surface area. In addition, the deterioration degree of the positive electrode active material can be extended due to the shape of the single particle, which is preferable in terms of extending the lifespan.
[0059] The positive electrode active material may be a lithium composite transition metal oxide represented by the following Chemical Formula 1.
[0060] [Chemical formula 1] Li 1+x (Ni a Co b Mn c M d )O2
[0061] In the above Chemical Formula 1, M is one or more selected from W, Cu, Fe, V, Cr, Ti, Zr, Zn, Al, In, Ta, Y, La, Sr, Ga, Sc, Gd, Sm, Ca, Ce, Nb, Mg, B, and Mo; x, a, b, c and d are the atomic fractions of each independent element. 0≦x≦0.20, 0.50≦a≦0.95, 0.025≦b≦0.25, 0.025≦c≦0.25, 0≦d≦0.05, and a+b+c+d=1.
[0062] Lithium secondary battery The lithium secondary battery of the present invention includes a positive electrode including the positive electrode active material, a negative electrode, a separator interposed between the positive electrode and the negative electrode, and an electrolyte, and may be manufactured by a conventional manufacturing method well known in the art, except for using the positive electrode active material according to the present invention.
[0063] The positive electrode according to the present invention may be prepared by coating a positive electrode current collector with a positive electrode slurry including the positive electrode active material, a binder, a conductive material, a solvent, and the like, followed by drying and rolling.
[0064] The positive electrode current collector is not particularly limited as long as it does not cause a chemical change in the battery and has conductivity. For example, stainless steel; aluminum; nickel; titanium; calcined carbon; or aluminum or stainless steel whose surface has been treated with carbon, nickel, titanium, silver, or the like may be used.
[0065] The binder is a component that facilitates binding of the active material and conductive material and binding to the current collector, and may be added in an amount of 1 wt% to 30 wt% based on the total weight of the solid content of the positive electrode slurry. Examples of such binders include polyvinylidene fluoride, polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene termonomer, styrene-butadiene rubber, and fluororubber.
[0066] The conductive material is a substance that does not cause a chemical change in the battery and provides conductivity, and can be added in an amount of 1 wt % to 20 wt % based on the total weight of the solid content of the positive electrode slurry.
[0067] Examples of the conductive material include carbon powders such as carbon black, acetylene black, ketjen black, channel black, furnace black, lamp black, or thermal black; graphite powders such as natural graphite, artificial graphite, carbon nanotubes, or graphite with highly developed crystal structures; conductive fibers such as carbon fibers or metal fibers; conductive powders such as carbon fluoride powder, aluminum powder, or nickel powder; conductive whiskers such as zinc oxide or potassium titanate; conductive metal oxides such as titanium oxide; or conductive materials such as polyphenylene derivatives.
[0068] The solvent for the positive electrode slurry may include an organic solvent such as N-methyl-2-pyrrolidone (NMP), and may be used in an amount that provides a preferred viscosity when the positive electrode active material, binder, conductive material, etc. are included. For example, the solvent may be included so that the solids concentration in the positive electrode slurry including the positive electrode active material, binder, and conductive material is 10 wt % to 90 wt %, preferably 10 wt % to 50 wt %.
[0069] The negative electrode according to the present invention includes a negative electrode active material, and may be prepared by coating a negative electrode current collector with a negative electrode slurry including the negative electrode active material, a binder, a conductive material, a solvent, and the like, followed by drying and rolling.
[0070] The negative electrode current collector generally has a thickness of 3 μm to 500 μm. Such a negative electrode current collector is not particularly limited as long as it does not cause a chemical change in the battery and has high conductivity, and for example, copper; stainless steel; aluminum; nickel; titanium; calcined carbon; copper or stainless steel surface treated with carbon, nickel, titanium, silver, etc.; or aluminum-cadmium alloy, etc. can be used. In addition, like the positive electrode current collector, the surface can be formed with fine irregularities to strengthen the binding force of the negative electrode active material, and it can be used in various shapes such as a film, sheet, foil, net, porous body, foam, nonwoven fabric, etc.
[0071] In addition, the negative electrode active material may include at least one selected from the group consisting of a carbon material capable of reversibly intercalating / deintercalating lithium ions; a metal or an alloy of the metal and lithium; a metal composite oxide; a material capable of doping and dedoping lithium; lithium metal; and a transition metal oxide.
[0072] The carbonaceous material capable of reversibly intercalating / deintercalating lithium ions may be any carbonaceous negative electrode active material commonly used in lithium ion secondary batteries, and representative examples thereof include crystalline carbon, amorphous carbon, or both. Examples of the crystalline carbon include graphite such as amorphous, plate-like, flake-like, spherical, or fibrous natural graphite or artificial graphite, and examples of the amorphous carbon include soft carbon (low-temperature calcined carbon), hard carbon, mesophase pitch carbide, and calcined coke.
[0073] The metal or the alloy of the metal and lithium may be a metal selected from the group consisting of Cu, Ni, Na, K, Rb, Cs, Fr, Be, Mg, Ca, Sr, Si, Sb, Pb, In, Zn, Ba, Ra, Ge, Al, and Sn, or an alloy of the metal and lithium.
[0074] Examples of the metal composite oxides include PbO, PbO2, Pb2O3, Pb3O4, Sb2O3, Sb2O4, Sb2O5, GeO, GeO2, Bi2O3, Bi2O4, Bi2O5, Li x Fe2O3 (0 ≦ x ≦ 1), Li x WO2 (0 ≦ x ≦ 1) and Sn x Me 1-x Me’ y O z (Me: Mn, Fe, Pb, Ge; Me’: Al, B, P, Si, Group 1, Group 2, Group 3 elements of the periodic table, halogen; 0 < x ≦ 1; 1 ≦ y ≦ 3; 1 ≦ z ≦ 8), and one or more selected from the group consisting of these can be used.
[0075] Examples of the substances that can dope and undope lithium include Si, SiO x (0 < x ≦ 2), Si - Y alloy (where Y is an element selected from the group consisting of alkali metals, alkaline earth metals, Group 13 elements, Group 14 elements, transition metals, rare earth elements, and combinations thereof, and is not Si), Sn, SnO2, Sn - Y (where Y is an element selected from the group consisting of alkali metals, alkaline earth metals, Group 13 elements, Group 14 elements, transition metals, rare earth elements, and combinations thereof, and is not Sn), etc. Also, at least one of these can be mixed with SiO2 and used. The element Y can be selected from the group consisting of Mg, Ca, Sr, Ba, Ra, Sc, Y, Ti, Zr, Hf, Rf, V, Nb, Ta, Db, Cr, Mo, W, Sg, Tc, Re, Bh, Fe, Pb, Ru, Os, Hs, Rh, Ir, Pd, Pt, Cu, Ag, Au, Zn, Cd, B, Al, Ga, Sn, In, Ge, P, As, Sb, Bi, S, Se, Te, Po, and combinations thereof.
[0076] Examples of the transition metal oxides include lithium - containing titanium composite oxide (LTO), vanadium oxide, lithium vanadium oxide, etc.
[0077] The negative electrode active material may be included in an amount of 80% by weight to 99% by weight based on the total weight of the solid content of the negative electrode slurry.
[0078] The binder is a component that facilitates bonding between the conductive material, the active material, and the current collector, and may be added in an amount of 1 wt% to 30 wt% based on the total weight of the solid content of the negative electrode slurry. Examples of such binders include polyvinylidene fluoride, polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene monomer, styrene-butadiene rubber, and fluororubber.
[0079] The conductive material is a component for further improving the conductivity of the negative electrode active material, and may be added in an amount of 1% by weight to 20% by weight based on the total weight of the solid content of the negative electrode slurry. Such a conductive material is not particularly limited as long as it does not cause a chemical change in the battery and has conductivity, and examples thereof include carbon powders such as carbon black, acetylene black, ketjen black, channel black, furnace black, lamp black, and thermal black; graphite powders such as natural graphite, artificial graphite, carbon nanotubes, and graphite with highly developed crystal structures; conductive fibers such as carbon fibers and metal fibers; conductive powders such as carbon fluoride powder, aluminum powder, and nickel powder; conductive whiskers such as zinc oxide or potassium titanate; conductive metal oxides such as titanium oxide; and conductive materials such as polyphenylene derivatives.
[0080] The solvent for the negative electrode slurry may include water or an organic solvent such as NMP or alcohol, and may be used in an amount that provides a preferred viscosity when the negative electrode active material, binder, conductive material, etc. are included. For example, the solvent may be included so that the solid content concentration in the slurry including the negative electrode active material, binder, and conductive material is 30 wt% to 80 wt%, preferably 40 wt% to 70 wt%.
[0081] The separator of the present invention separates the negative electrode and the positive electrode and provides a path for lithium ion migration. Any separator that is typically used as a separator in a lithium secondary battery can be used without any particular limitation. In particular, a separator that has low resistance to ion migration in the electrolyte, excellent electrolyte impregnation ability, and excellent stability is preferred.
[0082] Specifically, the separator may be a porous polymer film, for example, a porous polymer film made of a polyolefin polymer such as an ethylene homopolymer, a propylene homopolymer, an ethylene / butene copolymer, an ethylene / hexene copolymer, or an ethylene / methacrylate copolymer; or a laminate structure of two or more layers thereof. Also, a conventional porous nonwoven fabric, for example, a nonwoven fabric made of a high melting point glass fiber, a polyethylene terephthalate fiber, or the like, may be used. Also, in order to ensure heat resistance or mechanical strength, a coated separator containing a ceramic component or a polymeric substance may be used, and may be used in a single layer or multilayer structure.
[0083] Examples of the electrolyte of the present invention include organic liquid electrolytes, inorganic liquid electrolytes, solid polymer electrolytes, gel polymer electrolytes, solid inorganic electrolytes, and molten inorganic electrolytes that can be used in the production of lithium secondary batteries, but are not limited to these.
[0084] Specifically, the electrolyte may include an organic solvent and a lithium salt.
[0085] The organic solvent may be any organic solvent that can act as a medium through which ions involved in the electrochemical reaction of the battery can move. Specifically, examples of the organic solvent include ester-based solvents such as methyl acetate, ethyl acetate, γ-butyrolactone, and ε-caprolactone; ether-based solvents such as dibutyl ether and tetrahydrofuran; ketone-based solvents such as cyclohexanone; aromatic hydrocarbon-based solvents such as benzene and fluorobenzene; carbonate-based solvents such as dimethylcarbonate (DMC), diethylcarbonate (DEC), ethylmethylcarbonate (EMC), ethylene carbonate (EC), and propylene carbonate (PC); alcohol-based solvents such as ethyl alcohol and isopropyl alcohol; and R-CN (R is C2 to C4). 20 Nitriles such as dimethylformamide; amides such as dimethylformamide; dioxolanes such as 1,3-dioxolane; or sulfolanes may be used. Among them, carbonate-based solvents are preferred, and a mixture of a cyclic carbonate (e.g., ethylene carbonate or propylene carbonate) having high ionic conductivity and high dielectric constant that can enhance the charge / discharge performance of a battery and a linear carbonate compound with low viscosity (e.g., ethyl methyl carbonate, dimethyl carbonate, or diethyl carbonate) is more preferred. In this case, the cyclic carbonate and the linear carbonate are mixed in a volume ratio of about 1:1 to about 1:9, so that the electrolyte can exhibit excellent performance.
[0086] The lithium salt can be used without any particular limitation as long as it is a compound capable of providing lithium ions used in a lithium secondary battery. Specifically, the lithium salt can be LiPF6, LiClO4, LiAsF6, LiBF4, LiSbF6, LiAlO4, LiAlCl4, LiCF3SO3, LiC4F9SO3, LiN(C2F5SO3)2, LiN(C2F5SO2)2, LiN(CF3SO2)2, LiCl, LiI, or LiB(C2O4)2. The concentration of the lithium salt is preferably within the range of 0.1M to 2.0M. When the concentration of the lithium salt is within the above range, the electrolyte has appropriate conductivity and viscosity, and therefore can exhibit excellent electrolyte performance, and lithium ions can move effectively.
[0087] In addition to the constituents of the electrolyte, the electrolyte may further contain one or more additives such as haloalkylene carbonate compounds such as difluoroethylene carbonate, pyridine, triethyl phosphite, triethanolamine, cyclic ethers, ethylenediamine, n-glyme, hexaphosphoric acid triamide, nitrobenzene derivatives, sulfur, quinoneimine dyes, N-substituted oxazolidinones, N,N-substituted imidazolidines, ethylene glycol dialkyl ethers, ammonium salts, pyrrole, 2-methoxyethanol, or aluminum trichloride, for the purpose of improving the life characteristics of the battery, suppressing the decrease in the capacity of the battery, improving the discharge capacity of the battery, etc. In this case, the additives may be contained in an amount of 0.1 to 5 wt % based on the total weight of the electrolyte.
[0088] The lithium secondary battery including the positive electrode active material according to the present invention exhibits improved performance in terms of gas generation rate and life span compared to conventional positive electrode active materials, and is therefore useful in portable devices such as mobile phones, notebook computers, and digital cameras, and in electric vehicles such as hybrid electric vehicles (HEVs).
[0089] According to another embodiment of the present invention, there is provided a battery module including the lithium secondary battery as a unit cell, and a battery pack including the same. The battery module or the battery pack can be used as a power source for one or more medium to large devices, such as a power tool, an automobile including an electric vehicle (EV), a hybrid electric vehicle, and a plug-in hybrid electric vehicle (PHEV), or a power storage system.
[0090] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS Hereinafter, the embodiments of the present invention will be described in detail so that those skilled in the art can easily carry out the present invention.
[0091] <Examples and Comparative Examples: Production of Positive Electrode Active Material> Example 1 Urea and citric acid were added to distilled water as fuel in a weight ratio of 80:20 and mixed until completely dissolved. The metal raw materials LiNO3, Ni(NO3)2·6H2O, Co(NO3)2·6H2O, Mn(NO3)2·6H2O, and Al(NO3)3·9H2O were added to the aqueous solution in which the fuel was completely dissolved and stirred until completely dissolved. LiNO3 was added so that the Li / M molar ratio, which is the ratio of the number of moles of lithium to the total number of moles of metals other than lithium (M), i.e., nickel, cobalt, manganese, and aluminum, was 1.07, and the molar ratio between nickel, cobalt, manganese, and aluminum was 86:5:7:2. The content of the fuel was 40wt% of the total content of the metal raw materials. The stirred solution was heated to 380℃ using a hot plate to evaporate all water, and then a spontaneous combustion reaction was caused to occur.
[0092] The powder obtained after the combustion reaction was pulverized into fine particles, which were then calcined at 800° C. for 10 hours in an oxygen atmosphere, and then crushed and sieved to produce a positive electrode active material.
[0093] The average particle size (D 50 ) was 2 μm. A low-magnification TEM image is shown in FIG 1, a high-magnification TEM image and SAED pattern in FIG 2, and an SEM image in FIG 3. This confirms that the positive electrode active material prepared in Example 1 exhibits a single phase with almost no aggregation between particles.
[0094] Comparative Example 1 The positive electrode active material was manufactured in the same manner as in Example 1, except that urea alone was used as the fuel instead of urea and citric acid. 50 ) is 3μm, and the photograph taken with a scanning electron microscope (SEM) is shown in Figure 4. Referring to Figure 4, it can be seen that the combustion of fuel occurs rapidly, and the shape of many secondary particles formed by the aggregation of many primary particles due to the uneven particle growth can be observed.
[0095] [Experimental example 1: Evaluation of lifespan] The positive electrode active materials prepared in Example 1 and Comparative Example 1 were mixed with a conductive material (carbon black) and a binder (polyvinylidene fluoride, PVdF) in a weight ratio of 95:2.2:2.8 in N-methyl-2-pyrrolidone (NMP) solvent to prepare positive electrode slurries (solid content: 16 wt%).
[0096] Next, aluminum foil (Al foil) was attached flatly as a positive electrode current collector on a flat glass substrate so that no air could enter, and the prepared slurry was coated on the aluminum foil (on the Al foil) using a stainless steel spatula. The aluminum foil (Al foil) coated with the slurry was placed in a dryer at 90°C to 120°C for 15 minutes, and the aluminum foil (Al foil) coated with the dried slurry was then manufactured into a circular positive electrode sample with a diameter of 14 mm using a punching machine. The positive electrode sample was rolled with an electric rolling machine to adjust the overall porosity to 24%. The coin half cell was assembled in the following order. The prepared circular positive electrode was placed in a coin cell can and an electrolyte was injected, and then a gasket, a separator, lithium, a spacer, and a washer were sequentially stacked on the can. The electrolyte used was a mixture of ethylene carbonate (EC): ethyl methyl carbonate (EMC): dimethyl carbonate (DMC) in a volume ratio of 3:3:4, in which 1.0M LiPF6, 3% by weight of vinylene carbonate (VC), 0.5% by weight of 1,3-propanesultone (PS), and 1% by weight of ethylene sulfate (Esa) were dissolved. Finally, the cap was tightened and the coin half cell was completed by joining the cells with a manual crimper to remove any air bubbles inside.
[0097] The lifespan of the manufactured coin half-cell was evaluated at a voltage range of 2.5V to 4.25V and a temperature of 45°C. In the first cycle, charging and discharging were performed at 0.2C, and in the second to 30th cycles (a total of 30 cycles), charging and discharging were performed at 0.5C and 1.0C, respectively, and the change in capacity with the progress of the cycles is shown in Figure 5.
[0098] From FIG. 5, it can be seen that the cathode active material prepared in Example 1, in which a mixture of urea and citric acid was used as a fuel in preparing the cathode active material, was more effective in improving the battery life characteristics than the cathode active material prepared in Comparative Example 1, in which urea was used alone.
[0099] [Experimental Example 2: Evaluation of gas generation rate] Lithium secondary batteries using the positive electrode active materials of Example 1 and Comparative Example 1 were manufactured in the same manner as in Experimental Example 1, and then fully charged to 4.3 V at 0.33 C. The charged batteries were disassembled, and three separated positive electrodes were placed in a pouch, and the electrolyte of Experimental Example 1 was further injected thereinto. The pouch was then stored in an oven at 60° C. for 12 weeks, and the change in the volume of the pouch was measured every week. Specifically, the change in mass of the pouch in water was measured using Archimedes' principle using the change in buoyancy caused by the change in the volume of the pouch, and the result was converted into a volume change, which is shown in FIG. 6.
[0100] From FIG. 6, it can be seen that the cathode active material prepared in Example 1, in which a mixture of urea and citric acid was used as a fuel when preparing the cathode active material, was more effective in reducing the gas generation rate of the battery during high-temperature storage than the cathode active material prepared in Comparative Example 1, in which urea was used alone.
Claims
1. 1) one or more first fuels selected from the group consisting of urea, glycine, carbohydrazide, oxalyldihydrazide, and hexamethylenetetramine; and one or more second fuels selected from the group consisting of citric acid, oxalic acid, sucrose, glucose, and acetylacetone; Adding metal source materials, including a lithium source material, a nickel source material, a cobalt source material, and a manganese source material, to water and stirring to prepare a mixed solution; 2) heating the mixed solution to combust it into powder; and 3) a step of heat-treating the powder obtained in step 2).
2. 2. The method for producing a positive electrode active material for a lithium secondary battery according to claim 1, wherein the first fuel is urea and the second fuel is citric acid.
3. 3. The method for producing a positive electrode active material for a lithium secondary battery according to claim 1, wherein a weight ratio of the first fuel to the second fuel is 60:40 to 90:
10.
4. 4. The method for producing a positive electrode active material for a lithium secondary battery according to claim 1, wherein a weight ratio of the first fuel to the second fuel is 70:30 to 90:
10.
5. 5. The method of claim 1, wherein in step 1), a total content of the first fuel and the second fuel is 20 wt % to 60 wt % based on a total content of the metal source material.
6. The method for producing a positive electrode active material for a lithium secondary battery according to any one of claims 1 to 5, wherein the heating in step 2) is performed at a temperature of 300°C to 500°C.
7. The method for producing a positive electrode active material for a lithium secondary battery according to any one of claims 1 to 6, wherein the heat treatment in step 3) is carried out at a temperature of 700°C to 800°C.
8. The positive electrode active material has an average particle size (D 50 8. The method for producing a positive electrode active material for a lithium secondary battery according to claim 1, wherein the positive electrode active material comprises a single particle having a size of 0.5 μm to 2.5 μm.
9. 8. A method for producing a lithium secondary battery including a positive electrode, a negative electrode, a separator interposed between the positive electrode and the negative electrode, and an electrolyte, the method comprising the step of producing a positive electrode active material for a lithium secondary battery by the production method according to any one of claims 1 to 7.
Citation Information
Patent Citations
Light metal element-doped ternary lithium ion battery positive electrode material and synthesis method thereof
CN104112849A
Method for preparing uniform lithium ion battery ternary cathode material by one-step in-situ complexation
CN109802114A
Positive active material for lithium ion battery and its manufacture
JP1999025984A
Method for producing lithium-manganese-nickel composite oxide, and positive pole active material for nonaqueous electrolytic secondary battery using the same
JP2005060162A