Preparation method and application of organic carbon source gasified coated sodium ferric sulfate positive electrode material
By adopting asymmetric temperature-controlled dual-temperature sintering method in sodium ion batteries, the organic carbon source is vaporized and deposited on the surface of sodium ferric sulfate, solving the problem of poor conductivity of sodium ferric sulfate and realizing a low-cost and high-performance positive electrode Material preparation improves the electrochemical performance of sodium ion batteries.
Patent Information
- Application Number
- CN202411343350.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-25
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-09-25
AI Technical Summary
The conductivity of sodium ferrosulfate positive electrode material in sodium ion batteries is poor, resulting in low capacity, poor rate performance and cycle stability. It is difficult for traditional high-temperature carbonization methods to achieve effective in situ carbon coating, and the use of inorganic carbon increases costs.
The asymmetric temperature control method is used to sinter it in a dual-temperature tube furnace. The sintering temperature of the organic carbon source in the high-temperature zone is 600-800℃, and the sintering temperature of the sodium ferrosulfate in the low-temperature zone is 300-400℃. The organic carbon is made by a protective atmosphere. Source gasification is uniformly deposited on the surface of sodium ferric sulfate, achieving in-situ carbon coating.
The synthesis process is simplified, time and raw material costs are reduced, and the electronic conductivity and electrochemical properties of sodium ferrous sulfate are improved, making it exhibit higher specific capacity and cycle stability in sodium ion batteries.
Smart Images

Figure CN118919702A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of sodium ion batteries, and specifically relates to a preparation method of a sodium ferric sulfate positive electrode material, in which an organic carbon source is gasified by an asymmetric temperature control method and deposited on the surface of sodium ferric sulfate to obtain a gas-phase organic carbon source-coated sodium ferric sulfate positive electrode material, and its application in sodium ion batteries. Background Art
[0002] In recent years, the problems of global environmental pollution and resource shortage have become increasingly serious, and the development of new renewable energy has become a top priority. Lithium-ion batteries have been widely used in various portable mobile devices, electric vehicles, and energy storage due to their advantages such as high energy density, long life, good stability, and no memory effect. However, due to the limited and uneven distribution of global lithium resources, the production and use costs of lithium batteries will inevitably be greatly affected. Sodium-ion batteries are similar to lithium-ion batteries in working principles, and have significant advantages such as abundant sodium salt reserves, low raw material costs, high thermal stability, and a wide operating temperature range. They are considered to be a powerful supplement to lithium-ion batteries, especially in the fields of low-speed electric vehicles and large-scale energy storage. However, the current development of sodium-ion batteries is limited by the cost and electrochemical properties of cathode materials. Therefore, finding low-cost and high-performance cathode materials is the key to promoting the development of sodium-ion batteries.
[0003] At present, the cathode materials of sodium ion batteries are mainly divided into three types: layered oxide type, polyanion type and Prussian blue type. Among them, polyanion cathode materials show significant advantages due to their open skeleton, stable crystal structure, low-energy ion migration pathway and other characteristics. Sodium iron sulfate, as a polyanion material, not only has low raw material cost and high working voltage, but also has a green and environmentally friendly preparation process and is pollution-free. Therefore, it is considered to be one of the potential materials for the industrialization of sodium ion batteries. However, sodium iron sulfate has poor conductivity, resulting in low capacity, poor rate performance and cycle stability. In-situ carbon coating using organic carbon sources is a common method to improve the electrochemical properties of low-conductivity cathode materials, but because sodium iron sulfate decomposes above 450°C, the traditional strategy of in-situ carbon coating by high-temperature carbonization is difficult to apply to this material. The existing technology usually improves its conductivity by adding highly conductive inorganic carbon such as carbon nanotubes, graphene, and carbon fibers during solid phase ball milling, but the dispersion effect of inorganic carbon is greatly affected by raw materials and experimental conditions, and the high cost also weakens the cost advantage of sodium iron sulfate cathode materials. Therefore, developing a method to achieve in situ carbon coating of sodium ferric sulfate using an organic carbon source has broad development prospects. Summary of the invention
[0004] The invention aims to solve the problem that when sodium ferric sulfate, a polyanion positive electrode material of a sodium ion battery, is carbon-coated with an organic carbon source, the organic carbon source is not completely carbonized during a low-temperature sintering process, resulting in poor electronic conductivity of the material. A preparation method and application of a sodium ferric sulfate positive electrode material gasified and coated with an organic carbon source are provided. The method uses an asymmetric temperature control method, the organic carbon source sintering temperature on one side of an air inlet of a double-temperature zone tubular furnace is 600-800°C, so that the organic carbon source is gasified, the sodium ferric sulfate sintering temperature on one side of an air outlet of the double-temperature zone is 300-400°C, so that the sodium ferric sulfate is prevented from being decomposed during the sintering process, and the organic carbon source is uniformly deposited on the surface of the sodium ferric sulfate after being gasified, thereby realizing in-situ carbon coating of the sodium ferric sulfate.
[0005] The objective of the present invention is achieved through the following technical solutions:
[0006] A method for preparing an organic carbon source gasified sodium ferric sulfate positive electrode material comprises the following steps: adopting an asymmetric temperature control method, placing the organic carbon source in a high temperature zone, placing a mixture of sodium sulfate and ferrous sulfate in a low temperature zone, and introducing a protective gas for sintering.
[0007] Furthermore, the method is specifically as follows:
[0008] Step 1: drying ferrous sulfate heptahydrate and sodium sulfate in a vacuum oven to obtain anhydrous ferrous sulfate and anhydrous sodium sulfate; drying in a vacuum oven is also to prevent oxidation of ferrous sulfate;
[0009] Step 2: Evenly mix anhydrous sodium sulfate and anhydrous ferrous sulfate to obtain a white mixture;
[0010] Step 3: Place the organic carbon source and the mixture obtained in step 2 in the middle of two temperature zones of a dual-temperature zone tubular furnace, and sinter them in a flowing protective atmosphere to obtain a black organic carbon-coated sodium iron sulfate positive electrode.
[0011] Furthermore, in step 1, the drying temperature is 200-300° C. and the drying time is 10-20 hours.
[0012] Furthermore, in step 2, the uniform mixing is to uniformly mix the sodium sulfate and ferrous sulfate obtained in step 1 by high-energy ball milling under a protective gas atmosphere, with a ball-to-material ratio of 5-30:1, a rotation speed of 400-800r / min, and a ball milling time of 1-24h. Since ferrous sulfate is easily oxidized, and there is a certain temperature rise during the high-energy ball milling process, which may accelerate oxidation, which has a great impact on the final material properties, it is necessary to ball mill under an inert gas.
[0013] Furthermore, in step 2, the molar ratio of Na to Fe in the white mixture is 1-1.5:1.
[0014] Furthermore, in step three, the organic carbon source is at least one of sucrose, ascorbic acid, glucose, citric acid, starch, polyvinyl pyrrolidone, succinic acid, and tannic acid.
[0015] Furthermore, in step three, the mass ratio of the organic carbon source to the mixture is 0.01-10:1.
[0016] Furthermore, in step three, the sintering temperature on one side of the organic carbon source in the dual-temperature zone tubular furnace is 600-800°C to gasify the organic carbon source, and the sintering temperature on one side of the sodium sulfate and ferrous sulfate mixture is 300-400°C. The two react to generate ferrous sulfate, and the organic carbon source is deposited on its surface to achieve uniform carbon coating. The heating rate on both sides is 1-10°C / min, and the sintering time is 1-30h.
[0017] Furthermore, in step three, the protective atmosphere is at least one of argon, nitrogen or a hydrogen-argon mixed gas, and the protective atmosphere flow rate is 10-90 mL / min.
[0018] Application of sodium iron sulfate positive electrode material prepared by the above preparation method in sodium ion batteries.
[0019] The technical solution of the present invention has the following advantages:
[0020] 1. The present invention adopts a one-step sintering method to prepare organic carbon-coated sodium ferric sulfate. The low-temperature sintering of sodium ferric sulfate and the organic carbon source coating process are simultaneously carried out in a double-temperature zone tubular furnace, which optimizes the synthesis process, effectively simplifies the complex steps in the step-by-step coating and some other synthesis methods, and uses an organic carbon source for carbon coating instead of inorganic carbon, which greatly reduces the time cost and raw material cost.
[0021] 2. The present invention sintered the materials in a dual-temperature zone tubular furnace, placed the organic carbon source in the high temperature zone, and placed the sodium ferric sulfate in the low temperature zone, so that the organic carbon source was gasified and then evenly deposited on the surface of the sodium ferric sulfate, thereby avoiding the decomposition of the sodium ferric sulfate and effectively solving the problem of incomplete carbonization of the organic carbon source, realizing in-situ carbon coating of the sodium ferric sulfate during the sintering process, and forming a uniform carbon coating layer on the surface of the sodium ferric sulfate.
[0022] 3. The positive electrode material prepared by the present invention can be applied to sodium ion batteries. The prepared sodium ion batteries have good electronic conductivity, thereby exerting a higher specific capacity. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 It is a partial schematic diagram of the sintering process using a double-temperature zone tubular furnace in Example 1 of the present invention.
[0024] Figure 2 It is a schematic diagram of the reaction occurring during the sintering process of an embodiment of the present invention.
[0025] Figure 3 This is the XRD spectrum of the sodium iron sulfate positive electrode material obtained in Example 1 of the present invention.
[0026] Figure 4 It is a 0.1C first charge and discharge curve diagram of Example 1, Comparative Example 1 and Comparative Example 2 of the present invention.
[0027] Figure 5 It is a comparison chart of 1C cycle performance of Example 1 of the present invention and Comparative Example 1. DETAILED DESCRIPTION
[0028] The technical solution of the present invention is further described below in conjunction with the accompanying drawings and embodiments, but is not limited thereto. Any modification or equivalent replacement of the technical solution of the present invention that does not depart from the spirit and scope of the technical solution of the present invention should be included in the protection scope of the present invention.
[0029] The present invention adopts a one-step sintering method to prepare organic carbon-coated sodium ferric sulfate, which effectively simplifies the complex steps in the step-by-step coating and some other synthesis methods, and greatly reduces the time cost and raw material cost. The material is sintered by an asymmetric temperature control method, which avoids the decomposition of sodium ferric sulfate and effectively solves the problem of incomplete carbonization of organic carbon sources in the traditional low-temperature sintering process, realizes in-situ carbon coating of sodium ferric sulfate during the sintering process, and forms a uniform carbon coating layer on the surface of sodium ferric sulfate, thereby improving the electronic conductivity of the material and making it have better electrochemical performance.
[0030] Example 1
[0031] This embodiment prepares a sodium iron sulfate positive electrode material uniformly coated with an organic carbon source, and the specific steps include:
[0032] Step 1: Dry ferrous sulfate heptahydrate and sodium sulfate in a vacuum oven at 200° C. for 12 h to obtain anhydrous ferrous sulfate and anhydrous sodium sulfate.
[0033] Step 2: The Na2SO4 and FeSO4 obtained in step 1 are weighed and pre-mixed by hand grinding according to a molar ratio of Na to Fe of 1.5:1. After mixing evenly, the mixture is subjected to high-energy ball milling 36 times using a high-energy ball mill containing zirconium oxide balls, each time for 10 minutes with a rest of 5 minutes, to obtain a highly dispersed powder mixture. The ball milling treatment is carried out in an argon atmosphere, the ball-to-material ratio is 20:1, the ball milling speed is 600r / min, and the cumulative ball milling time is 6h.
[0034] Step 3: Transfer the mixture obtained in step 2 to a porcelain boat and place it in the middle of the heating zone on the air outlet side of the double-temperature zone tubular furnace, which is called the low-temperature zone; add sucrose to another porcelain boat, where the ratio of the mass of sucrose to the total mass of the mixture is 0.5:1, and place it in the middle of the heating zone on the air inlet side of the double-temperature zone tubular furnace, which is called the high-temperature zone.
[0035] Step 4: The sintering temperature in the high temperature zone is set to 700°C, the heating rate is 4°C / min, the sintering temperature in the low temperature zone is 350°C, the heating rate is 2°C / min, and the sintering is carried out for 12 hours in an argon atmosphere with an argon flow rate of 40 mL / min to finally obtain a black organic carbon-coated sodium iron sulfate positive electrode.
[0036] Example 2
[0037] This embodiment prepares a sodium iron sulfate positive electrode material uniformly coated with an organic carbon source. The specific steps and methods are the same as those in Example 1, except that the organic carbon source in step three is glucose.
[0038] Example 3
[0039] This embodiment prepares a sodium iron sulfate positive electrode material uniformly coated with an organic carbon source. The specific steps and methods are the same as those in Example 1, except that the organic carbon source in step three is tannic acid.
[0040] Example 4
[0041] This embodiment prepares a sodium iron sulfate positive electrode material uniformly coated with an organic carbon source. The specific steps and methods are the same as those in Example 1, except that in step three, the ratio of the mass of sucrose to the total mass of the mixture is 5:1.
[0042] Example 5
[0043] This embodiment prepares a sodium iron sulfate positive electrode material uniformly coated with an organic carbon source, and the specific steps include:
[0044] Step 1: Dry ferrous sulfate heptahydrate and sodium sulfate in a vacuum oven at 250° C. for 12 h to obtain anhydrous ferrous sulfate and anhydrous sodium sulfate.
[0045] Step 2: The Na2SO4 and FeSO4 obtained in step 1 are weighed and pre-mixed by hand grinding according to a Na to Fe molar ratio of 1.2:1. After mixing evenly, the mixture is subjected to high-energy ball milling 24 times using a high-energy ball mill containing zirconium oxide balls, each time for 20 minutes with a rest of 5 minutes, to obtain a highly dispersed powder mixture. The ball milling treatment is carried out in an argon atmosphere, the ball-to-material ratio is 15:1, the ball milling speed is 400r / min, and the cumulative ball milling time is 8h.
[0046] Step 3: Transfer the mixture obtained in step 2 to a porcelain boat and place it in the middle of the heating zone on the air outlet side of the double-temperature zone tubular furnace, which is called the low-temperature zone; add sucrose to another porcelain boat, where the ratio of the mass of sucrose to the total mass of the mixture is 1:1, and place it in the middle of the heating zone on the air inlet side of the double-temperature zone tubular furnace, which is called the high-temperature zone.
[0047] Step 4: The sintering temperature in the high temperature zone is set to 800°C, the heating rate is 4°C / min, the sintering temperature in the low temperature zone is 400°C, the heating rate is 2°C / min, and the sintering is carried out for 12 hours in an argon atmosphere with an argon flow rate of 20 mL / min to finally obtain a black organic carbon-coated sodium iron sulfate positive electrode.
[0048] Example 6
[0049] This embodiment prepares a sodium iron sulfate positive electrode material uniformly coated with an organic carbon source, and the specific steps include:
[0050] Step 1: Dry ferrous sulfate heptahydrate and sodium sulfate in a vacuum oven at 300° C. for 12 h to obtain anhydrous ferrous sulfate and anhydrous sodium sulfate.
[0051] Step 2: The Na2SO4 and FeSO4 obtained in step 1 are weighed and pre-mixed by hand grinding according to a molar ratio of Na to Fe of 1.5:1. After being evenly mixed, the mixture is subjected to high-energy ball milling 48 times using a high-energy ball mill containing zirconium oxide balls, each time for 5 minutes and resting for 5 minutes to obtain a highly dispersed powder mixture. The ball milling treatment is carried out in an argon atmosphere, the ball-to-material ratio is 30:1, the ball milling speed is 800r / min, and the cumulative ball milling time is 6h.
[0052] Step 3: Transfer the mixture obtained in step 2 to a porcelain boat and place it in the middle of the heating zone on the air outlet side of the double-temperature zone tubular furnace, which is called the low-temperature zone; add sucrose to another porcelain boat, where the ratio of the mass of sucrose to the total mass of the mixture is 10:1, and place it in the middle of the heating zone on the air inlet side of the double-temperature zone tubular furnace, which is called the high-temperature zone.
[0053] Step 4: The sintering temperature in the high temperature zone is set to 700°C, the heating rate is 4°C / min, the sintering temperature in the low temperature zone is 350°C, the heating rate is 2°C / min, and the sintering is carried out for 12 hours in an argon atmosphere with an argon flow rate of 90 mL / min to finally obtain a black organic carbon-coated sodium iron sulfate positive electrode.
[0054] Comparative Example 1:
[0055] This comparative example adopts a conventional low-temperature sintering method to prepare an organic carbon source-coated sodium iron sulfate positive electrode material, and the specific steps include:
[0056] Step 1: Dry ferrous sulfate heptahydrate and sodium sulfate in a vacuum oven at 200° C. for 12 h to obtain anhydrous ferrous sulfate and anhydrous sodium sulfate.
[0057] Step 2: Weigh the Na2SO4 and FeSO4 obtained in step 1 according to the molar ratio of Na to Fe of 1.5:1, add 50% of the total mass of sucrose to the mixture by hand milling, and after mixing evenly, use a high-energy ball mill containing zirconium oxide balls to high-energy ball mill the mixture 36 times, each time for 10 minutes and rest for 5 minutes to obtain a highly dispersed powder mixture. The ball milling process is carried out in an argon atmosphere, the ball-to-material ratio is 20:1, the ball milling speed is 600r / min, and the cumulative ball milling time is 6h.
[0058] Step 3: Transfer the mixture obtained in step 2 to a porcelain boat and place it in a tubular furnace for sintering. The sintering temperature is set to 350°C, the heating rate is 2°C / min, and it is sintered for 12 hours in an argon atmosphere with an argon flow rate of 40 mL / min to finally obtain a black organic carbon-coated sodium iron sulfate positive electrode.
[0059] Comparative Example 2:
[0060] In this comparative example, a sodium iron sulfate positive electrode material coated with an organic carbon source is prepared. The specific steps and methods are the same as those in comparative example 1, except that the mass of sucrose in step 2 is 10% of the total mass of Na2SO4 and FeSO4.
[0061] Application examples:
[0062] The organic carbon-coated sodium iron sulfate positive electrode material obtained in the above embodiments was added to a certain amount of NMP in a mass ratio of 8:1:1 with conductive carbon black and binder PVDF (configured into a 5% mass fraction NMP solution) to form a positive electrode slurry, and then evenly coated on the surface of aluminum foil, vacuum dried at 120°C in a vacuum oven for 12 hours, and then pressed under a pressure of 10MPa, and then punched into a 12mm positive electrode disc, using a sodium metal disc with a diameter of 15.6mm and a thickness of 0.5mm as the negative electrode, and a GF / D glass fiber disc with a diameter of 16mm as the diaphragm, and then configured with 1mol / L NaClO4 electrolyte, wherein the volume ratio of EC to PC in the solvent is 1:1, and 5% volume fraction of FEC is added. 2025 button-type sodium ion batteries were assembled in a glove box with a water and oxygen content of less than 0.01ppm.
[0063] The assembled sodium ion battery was charged and discharged using a NEWARE test system at a current density of 10 mA / g, with a cut-off voltage range of 2.0 V to 4.3 V.
[0064] Table 1 Charge and discharge test results
[0065] First charge capacity (mAh / g) First discharge capacity (mAh / g) First coulombic efficiency (%) Example 1 108.12 95.81 88.61 Example 2 107.42 94.36 87.84 Example 3 106.71 95.04 89.07 Example 4 105.09 90.50 86.12 Example 5 101.83 93.12 91.45 Example 6 112.12 92.22 82.25 Comparative Example 1 104.15 83.60 80.27 Comparative Example 2 94.82 77.36 81.58
Claims
1. A method for preparing an organic carbon source gasified coated sodium iron sulfate cathode material, characterized in that: The method comprises: adopting an asymmetric temperature control method, placing the organic carbon source in a high temperature zone, placing the sodium sulfate and ferrous sulfate mixture in a low temperature zone, and introducing protective gas for sintering.
2. The method for preparing an organic carbon source gasified coated sodium iron sulfate positive electrode material according to claim 1, characterized in that: The method is specifically as follows: Step 1: drying ferrous sulfate heptahydrate and sodium sulfate to obtain anhydrous ferrous sulfate and anhydrous sodium sulfate; Step 2: Evenly mix anhydrous sodium sulfate and anhydrous ferrous sulfate to obtain a white mixture; Step 3: placing the organic carbon source and the mixture obtained in step 2 in the middle of two temperature zones of a dual-temperature zone tubular furnace, and sintering them in a flowing protective atmosphere to obtain an organic carbon-coated sodium iron sulfate positive electrode.
3. The method for preparing a positive electrode material of sodium iron sulfate coated by gasification of an organic carbon source according to claim 2, characterized in that: In step 1, the drying temperature is 200-300° C. and the drying time is 10-20 hours.
4. The method for preparing a positive electrode material of sodium iron sulfate coated by gasification of an organic carbon source according to claim 2, characterized in that: In step 2, the uniform mixing is to uniformly mix the sodium sulfate and ferrous sulfate obtained in step 1 by high-energy ball milling under a protective gas atmosphere, with a ball-to-material ratio of 5-30:1, a rotation speed of 400-800 r / min, and a ball milling time of 1-24 h.
5. The method for preparing a positive electrode material of sodium iron sulfate coated by gasification of an organic carbon source according to claim 2, characterized in that: In step 2, the molar ratio of Na to Fe in the white mixture is 1-1.5:
1.
6. The method for preparing an organic carbon source gasified coated sodium iron sulfate positive electrode material according to claim 2, characterized in that: In step three, the organic carbon source is at least one of sucrose, ascorbic acid, glucose, citric acid, starch, polyvinyl pyrrolidone, succinic acid, and tannic acid.
7. The method for preparing an organic carbon source gasified coated sodium iron sulfate positive electrode material according to claim 2, characterized in that: In step three, the mass ratio of the organic carbon source to the mixture is 0.01-10:
1.
8. The method for preparing an organic carbon source gasified coated sodium iron sulfate positive electrode material according to claim 2, characterized in that: In step three, the sintering temperature on the organic carbon source side of the dual-temperature zone tubular furnace is 600-800°C, the sintering temperature on the sodium sulfate and ferrous sulfate mixture side is 300-400°C, the heating rate on both sides is 1-10°C / min, and the sintering time is 1-30h.
9. The method for preparing an organic carbon source gasified coated sodium iron sulfate positive electrode material according to claim 2, characterized in that: In step three, the protective atmosphere is at least one of argon, nitrogen or a hydrogen-argon mixed gas, and the protective atmosphere flow rate is 10-90 mL / min.
10. Use of a sodium iron sulfate positive electrode material prepared by the preparation method according to any one of claims 1 to 9 in a sodium ion battery.
Citation Information
Patent Citations
Carbon-coated sodium ferric sulfate positive electrode material and preparation method thereof
CN115020681A
Method for vapor deposition of carbon-coated modified Prussian blue sodium battery positive electrode material and positive electrode material prepared by method
CN117165914A
Sodium ferric sulfate composite positive electrode material and preparation method and application thereof
CN117374285A
Sodium ferric sulfate composite positive electrode material and preparation method and application thereof
CN117457899A
Preparation method of carbon-coated sodium ferric sulfate material
CN117613232A
Cited By
Composite positive electrode material and preparation method and application thereof
CN115663155A
A composite cathode material, its preparation method and application
CN115663155B
Novel sodium iron silicate sulfate composite polyanion positive electrode material for sodium-ion battery and preparation method of novel sodium iron silicate sulfate composite polyanion positive electrode material
CN119695149A
Carbon-coated sodium ferric sulfate positive electrode material, preparation method thereof and battery
CN121331798A
High-performance lithium manganese iron phosphate positive electrode material and preparation method thereof
CN121416457A