Rubber composition for tires and tires
A rubber composition combining isoprene rubber, styrene-butadiene rubber, and aromatic vinyl polymer addresses the challenge of improving wet grip performance during high-speed driving by adjusting elastic modulus for enhanced friction.
Patent Information
- Application Number
- JP2020071868
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-04-13
- Publication Date
- 2024-09-18
- Estimated Expiration
- 2040-04-13
AI Technical Summary
Existing tire compositions do not adequately enhance wet grip performance during high-speed running, despite efforts to improve this aspect such as adding silica or low softening point resins.
A rubber composition comprising isoprene rubber, styrene-butadiene rubber, C5 resin, and an aromatic vinyl polymer, which forms pseudo-crosslinks and adjusts elastic modulus to improve wet grip performance by maintaining rigidity in high-strain regions.
The composition enhances wet grip performance during high-speed driving by ensuring rigidity in high-strain regions while maintaining low strain region rigidity, thereby increasing tread surface friction.
Smart Images

Figure 0007552062000002 
Figure 0007552062000003 
Figure 0007552062000006
Abstract
Description
[Technical field]
[0001] The present invention relates to a rubber composition for tires and a tire using the same. [Background technology]
[0002] As techniques for improving the wet grip performance of tires, methods such as blending silica into a tread rubber composition, increasing the blending amount of a low-softening point resin or liquid polymer, blending a cold-resistant plasticizer, etc. have been considered (see, for example, Patent Document 1). However, in recent years, further improvement in wet grip performance has been required. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2000-159935 A Summary of the Invention [Problem to be solved by the invention]
[0004] The present invention has been made in consideration of the above-mentioned current situation, and has an object to provide a rubber composition for tires that improves wet grip performance during high-speed running, and a tire using the same. [Means for solving the problem]
[0005] The present invention relates to a rubber composition for tires, which comprises a rubber component (A) containing an isoprene-based rubber and a styrene-butadiene-based rubber, a C5 resin and / or a C5-C9 resin (B), and an aromatic vinyl polymer (C).
[0006] The aromatic vinyl polymer is preferably at least one selected from the group consisting of an aromatic vinyl thermoplastic elastomer, a homopolymer of an aromatic vinyl compound, and a copolymer of an aromatic vinyl compound and a terpene compound.
[0007] The aromatic vinyl polymer is preferably a polymer containing a styrene unit.
[0008] The styrene-butadiene rubber preferably has a styrene content of 30% by mass or more.
[0009] The content of the aromatic vinyl polymer is preferably 10 to 60 parts by mass based on 100 parts by mass of the rubber component.
[0010] The total content of the C5 resin and the C5-C9 resin is preferably 10 to 60 parts by mass based on 100 parts by mass of the rubber component.
[0011] The present invention also relates to a tire having a tread made with said rubber composition. Effect of the Invention
[0012] The present invention relates to a rubber composition for tires, which comprises a rubber component (A) containing an isoprene-based rubber and a styrene-butadiene-based rubber, a C5-based resin and / or a C5-C9-based resin (B), and an aromatic vinyl-based polymer (C), and therefore improves wet grip performance during high-speed running. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] The present invention relates to a rubber composition for tires, which comprises a rubber component (A) containing an isoprene-based rubber and a styrene-butadiene-based rubber, a C5-based resin and / or a C5-C9-based resin (B), and an aromatic vinyl-based polymer (C), and which provides excellent wet grip performance during high-speed driving.
[0014] It is presumed that the above-mentioned effects of the rubber composition are achieved by the following functions. In the low strain region, the polymer of isoprene rubber or styrene butadiene rubber and the aromatic vinyl polymer (styrene polymer, etc.) form pseudo crosslinks through intermolecular interactions, improving the elastic modulus of the rubber, while in the high strain region, the intermolecular distance increases and the interaction is eliminated, decreasing the elastic modulus. In contrast, C5 resin and / or C5-C9 resin reduce the elastic modulus of the rubber in the entire strain region. As a result, the elastic modulus hardly changes in the low strain region, and only the elastic modulus in the high strain region decreases, ensuring the rigidity of the non-grounding surface that is not subject to much strain, while the grounding surface that is subject to high strain due to high-speed running is greatly deformed, and the friction coefficient of the tread surface increases. It is presumed that the above-mentioned rubber composition exhibits such functions, thereby improving the wet grip performance during high-speed running.
[0015] (Rubber component (A)) The rubber composition contains a rubber component (component (A)) containing an isoprene-based rubber and a styrene-butadiene-based rubber.
[0016] The isoprene-based rubber is a polymer having isoprene as a structural unit, and is a polymer in which the amount of isoprene units is 95% by mass or more out of 100% by mass of all structural units of the polymer. The amount of such units is preferably 98% by mass or more, and may be 100% by mass.
[0017] In the rubber composition, the content of the isoprene-based rubber in 100% by mass of the rubber component is preferably 20% by mass or more, more preferably 30% by mass or more, even more preferably 40% by mass or more, and particularly preferably 45% by mass or more. The upper limit of the content is preferably 90% by mass or less, more preferably 75% by mass or less, and even more preferably 65% by mass or less. By keeping the content within the above range, good wet grip performance during high-speed driving tends to be obtained.
[0018] The weight average molecular weight (Mw) of the isoprene rubber is preferably 60,000 or more, more preferably 80,000 or more, and even more preferably 100,000 or more. The upper limit of the Mw is preferably 3 million or less, more preferably 2.5 million or less, and even more preferably 2 million or less. By keeping the Mw within the above range, good wet grip performance during high-speed driving tends to be obtained.
[0019] Examples of isoprene-based rubber include natural rubber (NR), isoprene rubber (IR), modified NR, modified NR, and modified IR. NR can be SIR20, RSS♯3, TSR20, and the like, and IR can be IR2200, and the like, which are common in the tire industry. Modified NR can be deproteinized natural rubber (DPNR), high-purity natural rubber (UPNR), and the like. Modified NR can be epoxidized natural rubber (ENR), hydrogenated natural rubber (HNR), grafted natural rubber, and the like. Modified IR can be epoxidized isoprene rubber, hydrogenated isoprene rubber, grafted isoprene rubber, and the like. These may be used alone or in combination of two or more.
[0020] Styrene-butadiene rubber (SBR) is a polymer having styrene and butadiene as structural units, and the total amount of styrene units and butadiene units is 95% by mass or more out of 100% by mass of all structural units of the polymer. The total amount of units is preferably 98% by mass or more, and may be 100% by mass.
[0021] In the rubber composition, the content of the styrene-butadiene rubber in 100% by mass of the rubber component is preferably 5% by mass or more, more preferably 20% by mass or more, even more preferably 35% by mass or more, and particularly preferably 45% by mass or more. The upper limit is preferably 80% by mass or less, more preferably 70% by mass or less, and even more preferably 60% by mass or less. By keeping it within the above range, good wet grip performance during high-speed driving tends to be obtained.
[0022] The weight average molecular weight (Mw) of the styrene butadiene rubber is preferably 60,000 or more, more preferably 200,000 or more, even more preferably 300,000 or more, and particularly preferably 350,000 or more. The upper limit of the Mw is preferably 1,500,000 or less, more preferably 800,000 or less, even more preferably 600,000 or less, and particularly preferably 450,000 or less. By keeping it within the above range, good wet grip performance during high-speed driving tends to be obtained.
[0023] The styrene content of the styrene-butadiene rubber is preferably 15% by mass or more, more preferably 20% by mass or more, even more preferably 25% by mass or more, and even more preferably 30% by mass or more. The styrene content is preferably 60% by mass or less, more preferably 50% by mass or less, and even more preferably 40% by mass or less. By keeping it within the above range, good wet grip performance during high-speed driving tends to be obtained. In particular, it is presumed that the more the styrene content, the more likely it is that interactions occur, and the more likely it is that the more likely it is that the effect of improving wet grip performance during high-speed driving is obtained.
[0024] The vinyl bond content of the styrene-butadiene rubber is preferably 5% by mass or more, more preferably 10% by mass or more, more preferably 20% by mass or more, and even more preferably 25% by mass or more. The vinyl bond content is preferably 50% by mass or less, more preferably 40% by mass or less, and even more preferably 35% by mass or less. By keeping it within the above range, good wet grip performance during high-speed driving tends to be obtained.
[0025] As the styrene-butadiene rubber, either a non-oil-extended styrene-butadiene rubber or an oil-extended styrene-butadiene rubber can be used. In addition, either a non-modified styrene-butadiene rubber or a modified styrene-butadiene rubber can be used.
[0026] The non-modified styrene butadiene rubber may be any rubber having a functional group that interacts with a filler such as silica, and examples thereof include terminal-modified styrene butadiene rubber (terminal-modified styrene butadiene rubber having the above-mentioned functional group at the terminal) in which at least one terminal of the styrene butadiene rubber is modified with a compound (modifier) having the above-mentioned functional group, main chain-modified styrene butadiene rubber having the above-mentioned functional group in the main chain, main chain terminal-modified styrene butadiene rubber having the above-mentioned functional group in the main chain and at least one terminal (for example, main chain terminal styrene butadiene rubber having the above-mentioned functional group in the main chain and modified with the above-mentioned modifier at least one terminal), and terminal-modified styrene butadiene rubber modified (coupled) with a polyfunctional compound having two or more epoxy groups in the molecule and having a hydroxyl group or an epoxy group introduced therein. These may be used alone or in combination of two or more.
[0027] Examples of the functional group include an amino group, an amide group, a silyl group, an alkoxysilyl group, an isocyanate group, an imino group, an imidazole group, a urea group, an ether group, a carbonyl group, an oxycarbonyl group, a mercapto group, a sulfide group, a disulfide group, a sulfonyl group, a sulfinyl group, a thiocarbonyl group, an ammonium group, an imide group, a hydrazo group, an azo group, a diazo group, a carboxyl group, a nitrile group, a pyridyl group, an alkoxy group, a hydroxyl group, an oxy group, and an epoxy group. These functional groups may have a substituent. Among them, an amino group (preferably an amino group in which a hydrogen atom of an amino group is substituted with an alkyl group having 1 to 6 carbon atoms), an alkoxy group (preferably an alkoxy group having 1 to 6 carbon atoms), an alkoxysilyl group (preferably an alkoxysilyl group having 1 to 6 carbon atoms), and an amide group are preferable.
[0028] As the styrene-butadiene rubber, for example, SBR manufactured and sold by Sumitomo Chemical Co., Ltd., JSR Corporation, Asahi Kasei Corporation, Nippon Zeon Co., Ltd., and the like can be used.
[0029] As a usable rubber component (component (A)) other than isoprene rubber and styrene-butadiene rubber, rubbers used in the tire field can be used, such as butadiene rubber (BR), acrylonitrile butadiene rubber (NBR), chloroprene rubber (CR), and butyl rubber (IIR).
[0030] In this specification, the weight average molecular weight (Mw) and number average molecular weight (Mn) can be determined by standard polystyrene conversion based on the measured value by gel permeation chromatography (GPC) (GPC-8000 series manufactured by Tosoh Corporation, detector: differential refractometer, column: TSKGEL SUPERMULTIPORE HZ-M manufactured by Tosoh Corporation). The vinyl bond amount (amount of 1,2-bonded butadiene units) can be measured by infrared absorption spectroscopy, and the styrene content can be measured by infrared absorption spectroscopy. 1 It can be measured by H-NMR measurement.
[0031] (C5 resin, C5-C9 resin (B)) The rubber composition contains a C5 resin and / or a C5-C9 resin (component (B)). The C5 resin and the C5-C9 resin may be either a solid or liquid resin at room temperature (25° C.), and among these, a solid resin is preferred.
[0032] C5 resins are polymers containing structural units of hydrocarbons having 5 carbon atoms and their polymers (dimers, etc.). Examples of hydrocarbons having 5 carbon atoms and their polymers include isoprene, pentane, cyclopentadiene, etc. Specific examples of C5 resins include copolymers of isoprene and styrene. C5 resins also include aliphatic petroleum resins obtained by (co)polymerizing C5 fractions obtained by thermal cracking of naphtha in the petrochemical industry. C5 fractions include olefinic hydrocarbons such as 1-pentene, 2-pentene, and 2-methyl-1-butene, and diolefinic hydrocarbons such as 2-methyl-1,3-butadiene, 1,2-pentadiene, and 1,3-pentadiene.
[0033] The C5-C9 resin may be a mixture of the C5 resin and the C9 resin. The C9 resin is a polymer containing a structural unit of a hydrocarbon having 9 carbon atoms and a polymer (dimer, etc.) thereof. Examples of the hydrocarbon having 9 carbon atoms and a polymer (dimer, etc.) thereof include indene, methylstyrene, vinyltoluene, etc. Specific examples of the C9 resin include solid polymers obtained by (co)polymerizing a C9 fraction using a Friedel-Crafts catalyst, etc., such as a copolymer mainly composed of indene, a copolymer mainly composed of methylindene, a copolymer mainly composed of α-methylstyrene, and a copolymer mainly composed of vinyltoluene. It is preferable that the C5 resin is an aliphatic resin, and the C9 resin is an alicyclic resin.
[0034] The total content of the C5 resin and the C5-C9 resin is preferably 3 parts by mass or more, more preferably 5 parts by mass or more, and even more preferably 10 parts by mass or more, based on 100 parts by mass of the rubber component. The content is preferably 60 parts by mass or less, more preferably 30 parts by mass or less, and even more preferably 20 parts by mass or less. By keeping the content within the above range, good wet grip performance during high-speed driving tends to be obtained. In particular, it is presumed that by blending a predetermined amount or more of resin, the elastic modulus is sufficiently reduced, and by adjusting the amount to a predetermined amount or less, rigidity can be ensured. The content of the C5 resin and the C5-C9 mixed resin alone is also preferably within the same range.
[0035] The softening point of the C5 resin and the C5-C9 resin is preferably 30° C. or higher, more preferably 60° C. or higher, and is preferably 160° C. or lower, more preferably 150° C. or lower. By keeping the softening point within the above range, good wet grip performance during high-speed driving tends to be obtained. In the present invention, the softening point of a polymer (resin, polymeric polymer, etc.) is the temperature at which the ball drops when the softening point as specified in JIS K 6220-1:2001 is measured using a ring and ball softening point tester.
[0036] The weight average molecular weight (Mw) of the C5 resin and the C5-C9 resin is preferably 1000 or more, more preferably 2000 or more, and even more preferably 2500 or more, and is preferably 5000 or less, more preferably 4000 or less, and even more preferably 3500 or less. By keeping it within the above range, good wet grip performance during high-speed driving and the like tend to be obtained.
[0037] The number average molecular weight (Mn) of the C5 resin and the C5-C9 resin is preferably 500 or more, more preferably 800 or more, and even more preferably 1000 or more, and is preferably 2000 or less, more preferably 1300 or less, and even more preferably 1100 or less. By keeping it within the above range, good wet grip performance during high-speed driving and the like tend to be obtained.
[0038] (Aromatic vinyl polymer (C)) The rubber composition contains an aromatic vinyl polymer (component (C)). The aromatic vinyl polymer, C5-C9 resin, may be either a polymer in a solid state or a polymer in a liquid state at room temperature (25° C.), and among them, a polymer in a solid state is preferable. The aromatic vinyl polymer may be used alone or in combination of two or more kinds.
[0039] An aromatic vinyl polymer is a polymer containing a structural unit of an aromatic vinyl compound (a structural unit derived from an aromatic vinyl compound (aromatic vinyl unit)). Examples of aromatic vinyl compounds include styrene, α-methylstyrene, 1-vinylnaphthalene, 3-vinyltoluene, ethylvinylbenzene, divinylbenzene, 4-cyclohexylstyrene, and 2,4,6-trimethylstyrene. These may be used alone or in combination of two or more kinds, with styrene and α-methylstyrene being preferred, and styrene being more preferred. That is, the aromatic vinyl unit is preferably a styrene unit.
[0040] As the aromatic vinyl polymer, an aromatic vinyl thermoplastic elastomer (a thermoplastic elastomer having an aromatic vinyl compound block) can be preferably used. The aromatic vinyl thermoplastic elastomer is a copolymer (block copolymer) composed of a hard segment that serves as a crosslinking point and a soft segment that exhibits rubber elasticity.
[0041] Examples of the hard segment include polystyrene, polypropylene, polyester, polyamide, polyvinyl chloride, polyurethane, etc., and examples of the soft segment include vinyl-polydiene, polyisoprene, polybutadiene, polyethylene, polychloroprene, poly2,3-dimethylbutadiene, etc. These may be one type or two or more types.
[0042] The aromatic vinyl thermoplastic elastomer preferably has a non-conjugated olefin unit in addition to the aromatic vinyl unit. The non-conjugated olefin unit is a structural unit derived from a non-conjugated olefin, and examples of the non-conjugated olefin include ethylene, propylene, 1-butene, 3-methyl-1-butene, 1-pentene, 1-hexene, 1-heptene, and 1-octene. These may be used alone or in combination of two or more kinds, but ethylene, 1-butene, and 3-methyl-1-butene are preferred, and ethylene is more preferred.
[0043] The non-conjugated olefin unit in the aromatic vinyl thermoplastic elastomer may be one obtained by polymerizing a non-conjugated olefin such as ethylene, or one obtained by polymerizing a conjugated diene compound such as 1,3-butadiene and hydrogenating the resulting conjugated diene unit. In other words, the aromatic vinyl thermoplastic elastomer having a non-conjugated olefin unit may be a copolymer of a non-conjugated olefin and another monomer, or a hydrogenated product (hydrogenated copolymer) of the copolymer.
[0044] The ratio of aromatic vinyl compound units in the aromatic vinyl thermoplastic elastomer is preferably 5% by mass or more, more preferably 10% by mass or more, even more preferably 15% by mass or more, and is preferably 70% by mass or less, more preferably 50% by mass or less, even more preferably 40% by mass or less, and particularly preferably 30% by mass or less. By keeping it within the above range, good wet grip performance during high-speed driving tends to be obtained.
[0045] The ratio of aromatic vinyl compound units and non-conjugated olefin units is H 1 -It can be calculated from the results of NMR measurements.
[0046] As the aromatic vinyl thermoplastic elastomer, it is preferable to use a thermoplastic elastomer having a styrene block (a styrene thermoplastic elastomer). Specific examples of styrene-based thermoplastic elastomers include styrene-vinylisoprene-styrene triblock copolymer (SIS), styrene-isobutylene diblock copolymer (SIB), styrene-butadiene-styrene triblock copolymer (SBS), styrene-ethylene-butylene-styrene triblock copolymer (SEBS), styrene-ethylene-propylene-styrene triblock copolymer (SEPS), styrene-ethylene-ethylene-propylene-styrene triblock copolymer (SEEPS), styrene-butadiene-butylene-styrene triblock copolymer (SBBS), styrene-ethylene-butadiene copolymer, etc. These may be used alone or in combination of two or more. Among them, styrene-ethylene-butylene-styrene triblock copolymer (SEBS) and styrene-ethylene-butadiene copolymer are preferred.
[0047] In addition, examples of aromatic vinyl polymers include homopolymers of aromatic vinyl compounds (such as styrene) and copolymers of aromatic vinyl compounds (such as styrene) and other monomers. Examples of other monomers include terpene compounds and α-methylstyrene. Among them, terpene compounds, that is, copolymers of aromatic vinyl compounds and terpene compounds, are preferred. In the case of homopolymers of aromatic vinyl compounds and copolymers of aromatic vinyl compounds and terpene compounds, it is presumed that the higher the compatibility with both isoprene rubber and styrene-butadiene rubber, the easier it is to promote the formation of pseudo-crosslinks between them, and the effect of improving wet grip performance during high-speed driving is easily obtained.
[0048] Terpene compounds are (C5H8) n The hydrocarbons and their oxygen-containing derivatives represented by the composition 10 H 16 ), sesquiterpenes (C 15 H 24 ), diterpenes (C 20 H 32 ), and examples thereof include α-pinene, β-pinene, dipentene, limonene, myrcene, alloocimene, ocimene, α-phellandrene, α-terpinene, γ-terpinene, terpinolene, 1,8-cineole, 1,4-cineole, α-terpineol, β-terpineol, and γ-terpineol.
[0049] The softening point of the aromatic vinyl polymer is preferably 40° C. or higher, more preferably 70° C. or higher, and even more preferably 90° C. or higher, and is preferably 160° C. or lower, more preferably 140° C. or lower, and even more preferably 130° C. or lower. By keeping the softening point within the above range, good wet grip performance during high-speed driving and the like tend to be obtained.
[0050] The content of the aromatic vinyl polymer is preferably 3 parts by mass or more, more preferably 5 parts by mass or more, and even more preferably 10 parts by mass or more, based on 100 parts by mass of the rubber component. The content is preferably 60 parts by mass or less, more preferably 30 parts by mass or less, and even more preferably 20 parts by mass or less. By keeping the content within the above range, good wet grip performance during high-speed driving tends to be obtained. In particular, it is presumed that the greater the amount of the aromatic vinyl polymer, the more likely it is that an interaction occurs, and the more likely it is that the effect of improving the wet grip performance during high-speed driving can be obtained.
[0051] In this specification, a polymer containing an isoprene unit as a constituent unit is considered to be an isoprene-based rubber if the content of isoprene units is 95% by mass or more and Mw is 5000 or more out of 100% by mass of all constituent units of the polymer, and a polymer with said content less than 95% by mass or Mw less than 5000 is considered to be a C5-based resin. A polymer containing styrene and butadiene as constituent units is considered to be a styrene-butadiene-based rubber if the total content of styrene units and butadiene units is 95% by mass or more and Mw is 5000 or more out of 100% by mass of all constituent units of the polymer, and a polymer with said total content less than 95% by mass or Mw less than 5000 is considered to be an aromatic vinyl-based polymer. . Fang Polymers containing aromatic vinyl units and structural units of hydrocarbons having 9 carbon atoms and / or their polymers (such as indene units) as structural units are considered to be C9 resins and not aromatic vinyl polymers. These polymers (polymers having an isoprene unit content of 95% by mass or more and an Mw of 5000 or more, polymers having a total content of styrene units and butadiene units of 95% by mass or more and an Mw of 5000 or more, etc.) may be solid or liquid at room temperature (25°C).
[0052] As the aromatic vinyl polymer, products available from Asahi Kasei Corporation, Yasuhara Chemical Co., Ltd., etc. can be used.
[0053] The rubber composition may contain a resin (solid resin) that is in a solid state at room temperature (25° C.) other than the C5 resin, C5-C9 resin, and aromatic vinyl polymer. The solid resin is not particularly limited as long as it is one that is commonly used in the tire industry, and examples of the solid resin include pt-butylphenol acetylene resin and acrylic resin.
[0054] (silica) From the viewpoint of wet grip performance during high-speed driving, the rubber composition preferably contains silica as a filler. Examples of silica include dry process silica (anhydrous silica) and wet process silica (hydrated silica). Among them, wet process silica is preferred because it has a large number of silanol groups. Commercially available products include those from Degussa, Rhodia, Tosoh Silica, Solvay Japan, and Tokuyama. These may be used alone or in combination of two or more.
[0055] The content of silica is preferably 25 parts by mass or more, more preferably 50 parts by mass or more, and even more preferably 60 parts by mass or more, based on 100 parts by mass of the rubber component. The upper limit of the content is preferably 150 parts by mass or less, more preferably 100 parts by mass or less, and even more preferably 80 parts by mass or less. By keeping the content within the above range, good wet grip performance during high-speed driving tends to be obtained.
[0056] The nitrogen adsorption specific surface area (N2SA) of the silica is preferably 70 m 2 / g or more, more preferably 140m 2 / g or more, more preferably 160m 2 / g or more, particularly preferably 200m 2 The upper limit of the N2SA of silica is preferably 300 m 2 / g or less, more preferably 250m 2 By keeping it within the above range, good wet grip performance during high speed driving and the like tend to be obtained. The N2SA of silica is a value measured by the BET method in accordance with ASTM D3037-93.
[0057] In the rubber composition, the silica content in the total content of silica and carbon black (100% by mass) is preferably 50% by mass or more, more preferably 80% by mass or more, and even more preferably 90% by mass or more, from the viewpoint of wet grip performance during high-speed driving.
[0058] (Silane coupling agent) When the rubber composition contains silica, it is preferable that the rubber composition contains a silane coupling agent together with the silica. The silane coupling agent is not particularly limited, and examples thereof include bis(3-triethoxysilylpropyl)tetrasulfide, bis(2-triethoxysilylethyl)tetrasulfide, bis(4-triethoxysilylbutyl)tetrasulfide, bis(3-trimethoxysilylpropyl)tetrasulfide, bis(2-trimethoxysilylethyl)tetrasulfide, bis(2-triethoxysilylethyl)trisulfide, bis(4-trimethoxysilylbutyl)trisulfide, bis(3-triethoxysilylpropyl)disulfide, bis(2-triethoxysilylethyl)disulfide, bis(4-trimethoxysilylbutyl)disulfide, bis(3-trimethoxysilylpropyl)disulfide, bis(2-trimethoxysilylethyl)disulfide, bis(4-trimethoxysilylbutyl)disulfide, bis(3-trimethoxysilylpropyl)disulfide, bis(2-trimethoxysilylethyl)disulfide, bis(4-trimethoxysilylbutyl)disulfide, 3-trimethoxysilylpropyl-N Examples of such silanes include sulfide-based silanes such as 3-mercaptopropyltrimethoxysilane, 2-mercaptoethyltriethoxysilane, vinyl-based silanes such as vinyltriethoxysilane, vinyltrimethoxysilane, amino-based silanes such as 3-aminopropyltriethoxysilane, 3-aminopropyltrimethoxysilane, glycidoxy-based silanes such as γ-glycidoxypropyltriethoxysilane, γ-glycidoxypropyltrimethoxysilane, nitro-based silanes such as 3-nitropropyltrimethoxysilane, 3-nitropropyltriethoxysilane, and chloro-based silanes such as 3-chloropropyltrimethoxysilane, 3-chloropropyltriethoxysilane. As commercially available products, for example, products from Degussa, Momentive, Shin-Etsu Silicone Co., Ltd., Tokyo Chemical Industry Co., Ltd., Azumax Co., Ltd., Dow Corning Toray Co., Ltd., etc. can be used. These may be used alone or in combination of two or more. Among them, sulfide-based silane coupling agents and mercapto-based silane coupling agents are preferred, and mercapto-based silane coupling agents are more preferred.
[0059] Examples of the mercapto-based silane coupling agent include a silane coupling agent having a mercapto group, a silane coupling agent in which the mercapto group is protected, etc. These may be used alone or in combination of two or more kinds.
[0060] Suitable mercapto-based silane coupling agents include (i) a silane coupling agent represented by the following formula (2-1), and (ii) a silane coupling agent containing a bond unit A represented by the following formula (2-2) and a bond unit B represented by the following formula (2-3). [ka] (In formula (2-1), R 101 -Cl, -Br, -OR 106 , -O(O=)CR 106 , -ON=CR 106 R 107 , -ON=CR 106 R 107 , -NR 106 R 107 and-(OSiR 106 R 107 ) h (OSiR 106 R 107 R 108 ) a monovalent group (R 106 , R 107 and R 108 may be the same or different, each is a hydrogen atom or a monovalent hydrocarbon group having 1 to 18 carbon atoms, and h has an average value of 1 to 4; 102 is R 101 , a hydrogen atom or a monovalent hydrocarbon group having 1 to 18 carbon atoms, R 103 is -[O(R 109 O) j ]-group(R 109 is an alkylene group having 1 to 18 carbon atoms, and j is an integer of 1 to 4. 104 is a divalent hydrocarbon group having 1 to 18 carbon atoms, R 105represents a monovalent hydrocarbon group having 1 to 18 carbon atoms, and xa, ya, and za are numbers that satisfy the relationship: xa+ya+2za=3, 0≦xa≦3, 0≦ya≦2, 0≦za≦1. [ka] [ka] (In formulas (2-2) and (2-3), xb is an integer of 0 or more, and yb is an integer of 1 or more. R 201 R represents hydrogen, halogen, a branched or unbranched alkyl group having 1 to 30 carbon atoms, a branched or unbranched alkenyl group having 2 to 30 carbon atoms, a branched or unbranched alkynyl group having 2 to 30 carbon atoms, or an alkyl group in which the terminal hydrogen atom has been substituted with a hydroxyl group or a carboxyl group. 202 R represents a branched or unbranched alkylene group having 1 to 30 carbon atoms, a branched or unbranched alkenylene group having 2 to 30 carbon atoms, or a branched or unbranched alkynylene group having 2 to 30 carbon atoms. 201 and R 202 may form a ring structure.)
[0061] R in the above formula (2-1) 102 , R 105 , R 106 , R 107 and R 108 Specific examples of the alkyl group include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a sec-butyl group, a tert-butyl group, a pentyl group, a hexyl group, an octyl group, a decyl group, a dodecyl group, a cyclopentyl group, a cyclohexyl group, a vinyl group, a propenyl group, an allyl group, a hexenyl group, an octenyl group, a cyclopentenyl group, a cyclohexenyl group, a phenyl group, a tolyl group, a xylyl group, a naphthyl group, a benzyl group, a phenethyl group, and a naphthylmethyl group. R in the above formula (2-1) 109Examples of the linear alkylene group include a methylene group, an ethylene group, an n-propylene group, an n-butylene group, and a hexylene group, and examples of the branched alkylene group include an isopropylene group, an isobutylene group, and a 2-methylpropylene group.
[0062] Specific examples of the silane coupling agent represented by the above formula (2-1) include 3-hexanoylthiopropyl triethoxysilane, 3-octanoylthiopropyl triethoxysilane, 3-decanoylthiopropyl triethoxysilane, 3-lauroylthiopropyl triethoxysilane, 2-hexanoylthioethyl triethoxysilane, 2-octanoylthioethyl triethoxysilane, 2-decanoylthioethyl triethoxysilane, 2-lauroylthioethyl triethoxysilane, 3-hexanoylthiopropyl trimethoxysilane, 3-octanoylthiopropyl trimethoxysilane, 3-decanoylthiopropyl trimethoxysilane, 3-lauroylthiopropyl trimethoxysilane, 2-hexanoylthioethyl trimethoxysilane, 2-octanoylthioethyl trimethoxysilane, 2-decanoylthioethyl trimethoxysilane, and 2-lauroylthioethyl trimethoxysilane. Among these, 3-octanoylthiopropyltriethoxysilane (NXT manufactured by Momentive Corp.) is particularly preferred. The above silane coupling agents may be used alone or in combination of two or more kinds.
[0063] The silane coupling agent containing the bond unit A represented by the above formula (2-2) and the bond unit B represented by the above formula (2-3) shows less increase in viscosity during processing than polysulfide silanes such as bis-(3-triethoxysilylpropyl)tetrasulfide. This is thought to be because the sulfide portion of the bond unit A is a CSC bond, which is more thermally stable than tetrasulfides and disulfides, resulting in less increase in Mooney viscosity.
[0064] In addition, compared to mercaptosilanes such as 3-mercaptopropyltrimethoxysilane, the reduction in scorch time is suppressed. This is because the bond unit A has a mercaptosilane structure, but the -CH of the bond unit A 15 This is thought to be because the -SH group of the bonding unit B is covered by this moiety, making it less likely to react with the polymer and less likely to cause scorch.
[0065] In the silane coupling agent of the above structure, the content of the bond unit A is preferably 30 mol% or more, more preferably 50 mol% or more, and preferably 99 mol% or less, more preferably 90 mol% or less.In addition, the content of the bond unit B is preferably 1 mol% or more, more preferably 5 mol% or more, even more preferably 10 mol% or more, and preferably 70 mol% or less, more preferably 65 mol% or less, even more preferably 55 mol% or less, from the viewpoint of reactivity with silica.In addition, the total content of the bond units A and B is preferably 95 mol% or more, more preferably 98 mol% or more, and particularly preferably 100 mol%. The content of the bond units A and B includes the case where the bond units A and B are located at the terminals of the silane coupling agent. When the bond units A and B are located at the terminals of the silane coupling agent, the form is not particularly limited, and it is sufficient that they form units corresponding to the formulas (2-2) and (2-3) representing the bond units A and B.
[0066] R 201 Examples of the halogen include chlorine, bromine, and fluorine.
[0067] R 201 Examples of the branched or unbranched alkyl group having 1 to 30 carbon atoms include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an iso-butyl group, a sec-butyl group, a tert-butyl group, a pentyl group, a hexyl group, a heptyl group, a 2-ethylhexyl group, an octyl group, a nonyl group, a decyl group, etc. The number of carbon atoms of the alkyl group is preferably 1 to 12.
[0068] R 201Examples of the branched or unbranched alkenyl group having 2 to 30 carbon atoms include a vinyl group, a 1-propenyl group, a 2-propenyl group, a 1-butenyl group, a 2-butenyl group, a 1-pentenyl group, a 2-pentenyl group, a 1-hexenyl group, a 2-hexenyl group, a 1-octenyl group, etc. The number of carbon atoms of the alkenyl group is preferably 2 to 12.
[0069] R 201 Examples of the branched or unbranched alkynyl group having 2 to 30 carbon atoms include an ethynyl group, a propynyl group, a butynyl group, a pentynyl group, a hexynyl group, a heptynyl group, an octynyl group, a nonynyl group, a decynyl group, an undecynyl group, a dodecynyl group, etc. The number of carbon atoms of the alkynyl group is preferably 2 to 12.
[0070] R 202 Examples of the branched or unbranched alkylene group having 1 to 30 carbon atoms include an ethylene group, a propylene group, a butylene group, a pentylene group, a hexylene group, a heptylene group, an octylene group, a nonylene group, a decylene group, an undecylene group, a dodecylene group, a tridecylene group, a tetradecylene group, a pentadecylene group, a hexadecylene group, a heptadecylene group, an octadecylene group, etc. The number of carbon atoms of the alkylene group is preferably 1 to 12.
[0071] R 202 Examples of the branched or unbranched alkenylene group having 2 to 30 carbon atoms include a vinylene group, a 1-propenylene group, a 2-propenylene group, a 1-butenylene group, a 2-butenylene group, a 1-pentenylene group, a 2-pentenylene group, a 1-hexenylene group, a 2-hexenylene group, a 1-octenylene group, etc. The number of carbon atoms in the alkenylene group is preferably 2 to 12.
[0072] R 202 Examples of the branched or unbranched alkynylene group having 2 to 30 carbon atoms include an ethynylene group, a propynylene group, a butynylene group, a pentynylene group, a hexynylene group, a heptynylene group, an octynylene group, a nonynylene group, a decynylene group, an undecynylene group, a dodecynylene group, etc. The number of carbon atoms of the alkynylene group is preferably 2 to 12.
[0073] In a silane coupling agent containing a bonding unit A represented by formula (2-2) and a bonding unit B represented by formula (2-3), the total number of repetitions (xb+yb) of the bonding unit A and the bonding unit B is preferably in the range of 3 to 300. When it is in this range, the mercaptosilane of the bonding unit B is preferably -CH of the bonding unit A. 15 Since the rubber component is covered with the silica, the scorch time can be prevented from becoming shorter and good reactivity with the silica and rubber components can be ensured.
[0074] As the silane coupling agent containing the bond unit A represented by formula (2-2) and the bond unit B represented by formula (2-3), for example, NXT-Z30, NXT-Z45, NXT-Z60, etc. manufactured by Momentive Corp. can be used. These may be used alone or in combination of two or more kinds.
[0075] As the mercapto-based silane coupling agent, (iii) a silane coupling agent represented by the following formula (2-4) can also be suitably used.
[0076] [ka]
[0077] (In formula (2-4), R 6 ~R 8 represents a branched or unbranched alkyl group having 1 to 12 carbon atoms, a branched or unbranched alkoxy group having 1 to 12 carbon atoms, or -O-(R 10 -O) z -R 11 (z R 10 represents a branched or unbranched divalent hydrocarbon group having 1 to 30 carbon atoms. 10 may be the same or different. 11represents a branched or unbranched alkyl group having 1 to 30 carbon atoms, a branched or unbranched alkenyl group having 2 to 30 carbon atoms, an aryl group having 6 to 30 carbon atoms, or an aralkyl group having 7 to 30 carbon atoms. z represents an integer of 1 to 30. R 6 ~R 8 may be the same or different. 9 represents a branched or unbranched alkylene group having 1 to 6 carbon atoms.
[0078] R 6 ~R 8 represents a branched or unbranched alkyl group having 1 to 12 carbon atoms, a branched or unbranched alkoxy group having 1 to 12 carbon atoms, or -O-(R 10 -O) z -R 11 R represents a group represented by the formula: 6 ~R 8 has at least one -O-(R 10 -O) z -R 11 Preferably, two of the groups are represented by -O-(R 10 -O) z -R 11 and one of them is a branched or unbranched alkoxy group having 1 to 12 carbon atoms.
[0079] R 6 ~R 8 Examples of the branched or unbranched alkyl group having 1 to 12 carbon atoms (preferably 1 to 5 carbon atoms) include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an iso-butyl group, a sec-butyl group, a tert-butyl group, a pentyl group, a hexyl group, a heptyl group, a 2-ethylhexyl group, an octyl group, and a nonyl group.
[0080] R 6 ~R 8Examples of the branched or unbranched alkoxy group having 1 to 12 carbon atoms (preferably 1 to 5 carbon atoms) include a methoxy group, an ethoxy group, an n-propoxy group, an isopropoxy group, an n-butoxy group, an iso-butoxy group, a sec-butoxy group, a tert-butoxy group, a pentyloxy group, a hexyloxy group, a heptyloxy group, a 2-ethylhexyloxy group, an octyloxy group, and a nonyloxy group.
[0081] R 6 ~R 8 -O-(R 10 -O) z -R 11 In R 10 represents a branched or unbranched divalent hydrocarbon group having 1 to 30 carbon atoms (preferably 1 to 15 carbon atoms, more preferably 1 to 3 carbon atoms). Examples of the hydrocarbon group include a branched or unbranched alkylene group having 1 to 30 carbon atoms, a branched or unbranched alkenylene group having 2 to 30 carbon atoms, a branched or unbranched alkynylene group having 2 to 30 carbon atoms, and an arylene group having 6 to 30 carbon atoms. Among these, a branched or unbranched alkylene group having 1 to 30 carbon atoms is preferred.
[0082] R 10 Examples of the branched or unbranched alkylene group having 1 to 30 carbon atoms (preferably 1 to 15 carbon atoms, more preferably 1 to 3 carbon atoms) include a methylene group, ethylene group, propylene group, butylene group, pentylene group, hexylene group, heptylene group, octylene group, nonylene group, decylene group, undecylene group, dodecylene group, tridecylene group, tetradecylene group, pentadecylene group, hexadecylene group, heptadecylene group, and octadecylene group.
[0083] R 10Examples of the branched or unbranched alkenylene group having 2 to 30 carbon atoms (preferably 2 to 15 carbon atoms, more preferably 2 to 3 carbon atoms) include a vinylene group, a 1-propenylene group, a 2-propenylene group, a 1-butenylene group, a 2-butenylene group, a 1-pentenylene group, a 2-pentenylene group, a 1-hexenylene group, a 2-hexenylene group, and a 1-octenylene group.
[0084] R 10 Examples of the branched or unbranched alkynylene group having 2 to 30 carbon atoms (preferably having 2 to 15 carbon atoms, more preferably having 2 to 3 carbon atoms) include an ethynylene group, a propynylene group, a butynylene group, a pentynylene group, a hexynylene group, a heptynylene group, an octynylene group, a nonynylene group, a decynylene group, an undecynylene group, and a dodecynylene group.
[0085] R 10 Examples of the arylene group having 6 to 30 carbon atoms (preferably 6 to 15 carbon atoms) include a phenylene group, a tolylene group, a xylylene group, and a naphthylene group.
[0086] z represents an integer of 1 to 30 (preferably 2 to 20, more preferably 3 to 7, and further preferably 5 to 6).
[0087] R 11 represents a branched or unbranched alkyl group having 1 to 30 carbon atoms, a branched or unbranched alkenyl group having 2 to 30 carbon atoms, an aryl group having 6 to 30 carbon atoms, or an aralkyl group having 7 to 30 carbon atoms. Among these, a branched or unbranched alkyl group having 1 to 30 carbon atoms is preferred.
[0088] R 11Examples of the branched or unbranched alkyl group having 1 to 30 carbon atoms (preferably 3 to 25 carbon atoms, more preferably 10 to 15 carbon atoms) include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an iso-butyl group, a sec-butyl group, a tert-butyl group, a pentyl group, a hexyl group, a heptyl group, a 2-ethylhexyl group, an octyl group, a nonyl group, a decyl group, an undecyl group, a dodecyl group, a tridecyl group, a tetradecyl group, a pentadecyl group, and an octadecyl group.
[0089] R 11 Examples of the branched or unbranched alkenyl group having 2 to 30 carbon atoms (preferably 3 to 25 carbon atoms, more preferably 10 to 15 carbon atoms) include a vinyl group, a 1-propenyl group, a 2-propenyl group, a 1-butenyl group, a 2-butenyl group, a 1-pentenyl group, a 2-pentenyl group, a 1-hexenyl group, a 2-hexenyl group, a 1-octenyl group, a decenyl group, an undecenyl group, a dodecenyl group, a tridecenyl group, a tetradecenyl group, a pentadecenyl group, and an octadecenyl group.
[0090] R 11 Examples of the aryl group having 6 to 30 carbon atoms (preferably 10 to 20 carbon atoms) include a phenyl group, a tolyl group, a xylyl group, a naphthyl group, and a biphenyl group.
[0091] R 11 Examples of the aralkyl group having 7 to 30 carbon atoms (preferably 10 to 20 carbon atoms) include a benzyl group and a phenethyl group.
[0092] -O-(R 10 -O) z -R 11 Specific examples of the group represented by the formula are, for example, -O-(C2H4-O)5-C 11 H 23 , -O-(C2H4-O)5-C 12 H 25 , -O-(C2H4-O)5-C 13 H 27 , -O-(C2H4-O)5-C 14 H 29, -O-(C2H4-O)5-C 15 H 31 , -O-(C2H4-O)3-C 13 H 27 , -O-(C2H4-O)4-C 13 H 27 , -O-(C2H4-O)6-C 13 H 27 , -O-(C2H4-O)7-C 13 H 27 Among them, -O-(C2H4-O)5-C 11 H 23 , -O-(C2H4-O)5-C 13 H 27 , -O-(C2H4-O)5-C 15 H 31 , -O-(C2H4-O)6-C 13 H 27 is preferred.
[0093] R 9 Examples of the branched or unbranched alkylene group having 1 to 6 carbon atoms (preferably 1 to 5 carbon atoms) include R 10 Examples of the branched or unbranched alkylene group having 1 to 30 carbon atoms include the same groups as those mentioned above.
[0094] Examples of the compound represented by the above formula (2-4) include 3-mercaptopropyltrimethoxysilane, 3-mercaptopropyltriethoxysilane, 2-mercaptoethyltrimethoxysilane, 2-mercaptoethyltriethoxysilane, and the compound represented by the following formula (Si363 manufactured by EVONIK-DEGUSSA), and the compound represented by the following formula can be preferably used. These may be used alone or in combination of two or more kinds. [ka]
[0095] When the rubber composition contains a silane coupling agent, the content is preferably 1 part by mass or more, more preferably 2 parts by mass or more, based on 100 parts by mass of silica. The content is preferably 20 parts by mass or less, more preferably 15 parts by mass or less. By making the content equal to or more than the lower limit, the effect of improving dispersibility tends to be sufficiently obtained. By making the content equal to or less than the upper limit, the coupling effect tends to be sufficient, and good reinforcement tends to be obtained.
[0096] (Carbon Black) The rubber composition may contain carbon black as a filler. The carbon black is not particularly limited, but may be N134, N110, N220, N234, N219, N339, N330, N326, N351, N550, N762, etc. Commercially available products include those from Asahi Carbon Co., Ltd., Cabot Japan Co., Ltd., Tokai Carbon Co., Ltd., Mitsubishi Chemical Co., Ltd., Lion Co., Ltd., Shin-Nichika Carbon Co., Ltd., Columbia Carbon Co., Ltd., etc. These may be used alone or in combination of two or more kinds.
[0097] When carbon black is contained, the content thereof is preferably 1 part by mass or more, more preferably 3 parts by mass or more, based on 100 parts by mass of the rubber component, and preferably 10 parts by mass or less, more preferably 7 parts by mass or less.
[0098] The nitrogen adsorption specific surface area (N2SA) of carbon black is 50m 2 / g or more is preferable, and 80m 2 / g or more is more preferable, and 100m 2 / g or more is more preferable. 2 / g or less is preferable, and 150m 2 / g or less is more preferable, and 130m 2 / g or less is more preferable. The nitrogen adsorption specific surface area of carbon black can be determined in accordance with JIS K6217-2:2001.
[0099] In the rubber composition, the total content of silica and carbon black is preferably 50 parts by mass or more, more preferably 55 parts by mass or more, and even more preferably 60 parts by mass or more, per 100 parts by mass of the rubber component, from the viewpoint of wet grip performance during high-speed driving, etc. The upper limit is preferably 120 parts by mass or less, more preferably 100 parts by mass or less, and even more preferably 80 parts by mass or less.
[0100] (Liquid plasticizer) The rubber composition may include a liquid plasticizer. The liquid plasticizer is not particularly limited as long as it is a plasticizer that is in a liquid state at 25° C., and examples thereof include oils, etc. These may be used alone or in combination of two or more kinds.
[0101] Examples of the oil include process oil, vegetable oil, or a mixture thereof. Examples of the process oil include paraffin-based process oil, aromatic process oil, and naphthenic process oil. Examples of the vegetable oil include castor oil, cottonseed oil, linseed oil, rapeseed oil, soybean oil, palm oil, coconut oil, peanut oil, rosin, pine oil, pine tar, tall oil, corn oil, rice oil, safflower oil, sesame oil, olive oil, sunflower oil, palm kernel oil, camellia oil, jojoba oil, macadamia nut oil, and tung oil. Examples of commercially available products include products from Idemitsu Kosan Co., Ltd., Sankyo Yuka Kogyo Co., Ltd., Japan Energy Co., Ltd., Orisoi Co., Ltd., H&R Co., Ltd., Toyokuni Oil Mill Co., Ltd., Showa Shell Sekiyu K.K., Fuji Kosan Co., Ltd., and Nisshin Oillio Group Co., Ltd.
[0102] The content of the liquid plasticizer (total amount of liquid plasticizer) is preferably 10 parts by mass or more, more preferably 15 parts by mass or more, and even more preferably 20 parts by mass or more, based on 100 parts by mass of the rubber component. The upper limit is preferably 50 parts by mass or less, more preferably 40 parts by mass or less, and even more preferably 35 parts by mass or less. By keeping the content within the above range, good wet grip performance during high-speed driving tends to be obtained. The total amount of liquid plasticizer includes the oil extension oil of the oil-extended rubber.
[0103] (Other materials) The rubber composition may contain sulfur. Examples of sulfur include powdered sulfur, precipitated sulfur, colloidal sulfur, insoluble sulfur, highly dispersible sulfur, soluble sulfur, etc., which are commonly used in the rubber industry. Commercially available products include those from Tsurumi Chemical Industry Co., Ltd., Karuizawa Sulfur Co., Ltd., Shikoku Chemical Industry Co., Ltd., Flexis Corporation, Nippon Kanzuri Kogyo Co., Ltd., Hosoi Chemical Industry Co., Ltd., etc. These may be used alone or in combination of two or more kinds.
[0104] The amount of sulfur is preferably 0.5 parts by mass or more, more preferably 1.5 parts by mass or more, and is preferably 6 parts by mass or less, more preferably 4 parts by mass or less, based on 100 parts by mass of the rubber component. By keeping the amount within the above range, good wet grip performance during high-speed driving and the like tend to be obtained.
[0105] The rubber composition may contain a vulcanization accelerator. Examples of the vulcanization accelerator include thiazole-based vulcanization accelerators such as 2-mercaptobenzothiazole and di-2-benzothiazolyl disulfide; thiuram-based vulcanization accelerators such as tetramethylthiuram disulfide (TMTD), tetrabenzylthiuram disulfide (TBzTD), and tetrakis(2-ethylhexyl)thiuram disulfide (TOT-N); sulfenamide-based vulcanization accelerators such as N-cyclohexyl-2-benzothiazylsulfenamide (CBS), N-tert-butyl-2-benzothiazolylsulfenamide (TBBS), N-oxyethylene-2-benzothiazolesulfenamide, and N,N'-diisopropyl-2-benzothiazolesulfenamide; and guanidine-based vulcanization accelerators such as diphenylguanidine, di-orthotolylguanidine, and orthotolylbiguanidine. Commercially available products include products from Sumitomo Chemical Co., Ltd., Ouchi Shinko Chemical Co., Ltd., and the like. These may be used alone or in combination of two or more kinds.
[0106] The content of the vulcanization accelerator is preferably 1.5 parts by mass or more, more preferably 3.0 parts by mass or more, and even more preferably 3.5 parts by mass or more, and is preferably 6.0 parts by mass or less, more preferably 5.0 parts by mass or less, and even more preferably 4.0 parts by mass or less, based on 100 parts by mass of the rubber component. By keeping the content within the above range, good wet grip performance during high-speed driving and the like tend to be obtained.
[0107] The rubber composition may contain zinc oxide. As the zinc oxide, a conventionally known one can be used, and as a commercially available product, it is possible to use products from Mitsui Mining & Smelting Co., Ltd., Toho Zinc Co., Ltd., Hakusui Tech Co., Ltd., Seido Chemical Industry Co., Ltd., Sakai Chemical Industry Co., Ltd., etc. These may be used alone or in combination of two or more kinds.
[0108] The amount of zinc oxide per 100 parts by mass of the rubber component is preferably 1 part by mass or more, more preferably 2 parts by mass or more, and even more preferably 3 parts by mass or more, and is preferably 8 parts by mass or less, and more preferably 6 parts by mass or less.
[0109] The rubber composition may contain a wax. The wax is not particularly limited, and examples thereof include petroleum waxes such as paraffin wax and microcrystalline wax; natural waxes such as vegetable wax and animal wax; and synthetic waxes such as polymers of ethylene, propylene, etc. Commercially available products include those from Ouchi Shinko Chemical Industry Co., Ltd., Nippon Seiro Co., Ltd., Seiko Chemical Co., Ltd., etc. These may be used alone or in combination of two or more kinds.
[0110] The amount of the wax per 100 parts by mass of the rubber component is preferably 1 part by mass or more, more preferably 2 parts by mass or more, and preferably 6 parts by mass or less, more preferably 4 parts by mass or less.
[0111] The rubber composition may contain an antioxidant. Examples of the antioxidant include naphthylamine-based antioxidants such as phenyl-α-naphthylamine; diphenylamine-based antioxidants such as octylated diphenylamine and 4,4'-bis(α,α'-dimethylbenzyl)diphenylamine; N-isopropyl-N'-phenyl-p-phenylenediamine, N-(1,3-dimethylbutyl)-N'-phenyl-p-phenylenediamine, and N,N'-di-2-naphthyl-p-phenylenediamine. Examples of the antioxidant include p-phenylenediamine antioxidants such as quinolinone; quinoline antioxidants such as polymers of 2,2,4-trimethyl-1,2-dihydroquinoline; monophenol antioxidants such as 2,6-di-t-butyl-4-methylphenol and styrenated phenol; and bis, tris, and polyphenol antioxidants such as tetrakis-[methylene-3-(3',5'-di-t-butyl-4'-hydroxyphenyl)propionate]methane. Commercially available products include those from Seiko Chemical Co., Ltd., Sumitomo Chemical Co., Ltd., Ouchi Shinko Chemical Co., Ltd., and Flexis Co., Ltd. These may be used alone or in combination of two or more.
[0112] The amount of the antioxidant per 100 parts by mass of the rubber component is preferably 1 part by mass or more, more preferably 2 parts by mass or more, and is preferably 6 parts by mass or less, more preferably 4 parts by mass or less.
[0113] The rubber composition may contain stearic acid. As the stearic acid, a conventionally known one can be used, and as a commercially available product, a product from NOF Corp., Kao Corp., Fujifilm Wako Pure Chemical Corp., Chiba Fatty Acid Corp., etc. can be used. These may be used alone or in combination of two or more kinds.
[0114] The amount of stearic acid per 100 parts by mass of the rubber component is preferably 1 part by mass or more, more preferably 2 parts by mass or more, and is preferably 6 parts by mass or less, more preferably 4 parts by mass or less.
[0115] In addition to the above components, the rubber composition may further contain additives commonly used in the rubber industry, such as organic peroxides, etc. The content of these additives is preferably 0.1 to 200 parts by mass per 100 parts by mass of the rubber component.
[0116] The rubber composition can be produced, for example, by kneading the above-mentioned components using a rubber kneading device such as an open roll or a Banbury mixer, and then vulcanizing the mixture.
[0117] As for the kneading conditions, in the base kneading step in which additives other than sulfur and the vulcanization accelerator are kneaded, the kneading temperature is usually 100 to 180°C, preferably 120 to 170°C. In the finish kneading step in which sulfur and the vulcanization accelerator are kneaded, the kneading temperature is usually 120°C or lower, preferably 85 to 110°C. Furthermore, the composition kneaded with sulfur and the vulcanization accelerator is usually subjected to a vulcanization treatment such as press vulcanization. The vulcanization temperature is usually 140 to 190°C, preferably 150 to 185°C. The vulcanization time is usually 5 to 15 minutes.
[0118] The rubber composition can be suitably used, for example, in a tire tread (cap tread).
[0119] The tire (pneumatic tire, etc.) of the present invention is manufactured by a normal method using the above rubber composition. That is, the above rubber composition is extruded in an unvulcanized state according to the shape of the tread, etc., and molded together with other tire components in a tire building machine by a normal method to form an unvulcanized tire. The unvulcanized tire is heated and pressurized in the vulcanizer to obtain a tire.
[0120] The above-mentioned tires can be used as tires for passenger cars, tires for large passenger cars, tires for large SUVs, tires for heavy loads such as trucks and buses, tires for light trucks, tires for two-wheeled vehicles, racing tires (high performance tires), etc. They can also be used as all-season tires, summer tires, winter tires (studless tires, etc.), etc. EXAMPLES
[0121] The present invention will be specifically described based on examples, but the present invention is not limited to these examples. Using the various chemicals shown below, rubber compositions with different formulations according to each table were used in the tread of a tire with a tire size of 195 / 65R15, and the wet grip performance of the tire during high-speed running was calculated. The results are shown in the evaluation column of each table.
[0122] The various chemicals used in the examples and comparative examples will be described below. NR:RSS#3 SBR1: SBR1502 manufactured by JSR Corporation (styrene content 25% by mass, vinyl bond content 16% by mass, Mw 490,000) SBR2: Tufuden 3830 manufactured by Asahi Kasei Corporation (styrene content 33% by mass, vinyl bond content 31% by mass, Mw 420,000, contains 37.5 parts by mass of oil per 100 parts by mass of rubber solids) Carbon black: Diablack N220 (manufactured by Mitsubishi Chemical Corporation, N2SA114m 2 / g) Silica 1: Uratosil VN3 (N2SA175m) manufactured by Evonik Degussa 2 / g) Silica 2: Ultrasil 9000GR (N2SA229m) manufactured by Evonik 2 / g) Silane coupling agent: Momentive's NXT (3-octanoylthiopropyltriethoxysilane) C5 resin 1: ESCOREZ 1102B manufactured by ExxonMobil (copolymer of isoprene and styrene, softening point 95°C) C5-C9 resin 1: Petrotac 100V (C5 / C9 resin, softening point 94°C, Mw 3900, Mn 1200) manufactured by Tosoh Corporation C5 resin 2: Marukarez T-100AS (C5 petroleum resin, softening point 102°C) manufactured by Maruzen Petrochemical Co., Ltd. Aromatic vinyl polymer 1: Production example below (styrene content 19% by mass, ethylene content 78% by mass, butadiene content 3.3% by mass) Aromatic vinyl polymer 2: Tuftec H1521 (SEBS (hydrogenated SBS), styrene content 18% by mass, total ethylene-butylene-butadiene content 82% by mass) manufactured by Asahi Kasei Corporation Aromatic vinyl polymer 3: YS Resin SX100 (styrene homopolymer, softening point 100°C) manufactured by Yasuhara Chemical Co., Ltd. Aromatic vinyl polymer 4: YS Resin TO125 (aromatic modified terpene resin (copolymer of terpene compound and styrene), softening point 125°C) manufactured by Yasuhara Chemical Co., Ltd. Aromatic vinyl polymer 5: Hybra 7125 (SEPS (hydrogenated SIS), styrene content 20% by mass) manufactured by Kuraray Co., Ltd. Aromatic vinyl polymer 6: Tuftec H1043 (SEBS (hydrogenated SBS), styrene content 67% by mass) manufactured by Asahi Kasei Corporation Oil: Diana Process NH-70S (aromatic process oil) manufactured by Idemitsu Kosan Co., Ltd. Zinc oxide: Zinc oxide No. 1 manufactured by Mitsui Mining & Smelting Co., Ltd. Anti-aging agent: Nocrac 6C (N-(1,3-dimethylbutyl)-N'-phenyl-p-phenylenediamine) manufactured by Ouchi Shinko Chemical Industry Co., Ltd. Stearic acid: NOF Corporation's "Tsubaki" stearic acid Wax: Ozoace 0355 manufactured by Nippon Seiro Co., Ltd. Sulfur: Powdered sulfur manufactured by Tsurumi Chemical Co., Ltd. Vulcanization accelerator 1: Noccelaer D (1,3-diphenylguanidine) manufactured by Ouchi Shinko Chemical Industry Co., Ltd. Vulcanization accelerator 2: Noccela CZ (N-cyclohexyl-2-benzothiazolyl sulfenamide) manufactured by Ouchi Shinko Chemical Industry Co., Ltd.
[0123] <Production Example> Styrene as an aromatic vinyl compound and cyclohexane are added to a thoroughly dried pressure-resistant stainless steel reactor. Meanwhile, in a glove box under a nitrogen atmosphere, 1-benzyldimethylsilyl-3-methylindene [[1-(PhCH2)Me2Si]-3-Me]C9H6, tris(bis(dimethylsilyl)amide) gadolinium complex Gd[N(SiHMe2)2]3, and trimethylaluminum are charged into a glass container, toluene is added, and the mixture is reacted at 80°C for 6 hours. After that, diisobutylaluminum hydride and toluene are added, followed by the addition of dimethylanilinium tetrakis(pentafluorophenyl)borate [Me2NHPhB(C6F5)4] to obtain a catalyst solution. The obtained catalyst solution is added to the above-mentioned pressure-resistant stainless steel reactor and heated to 75°C. Next, ethylene as a non-conjugated olefin compound is charged into the pressure-resistant stainless steel reactor, and further, a toluene solution containing 5 g of 1,3-butadiene as a conjugated diene compound is charged, and a polymerization reaction is carried out at 75° C. for a total of 4 hours. Thereafter, an isopropanol solution of 2,2'-methylene-bis(4-ethyl-6-t-butylphenol) (NS-5) is added to the pressure-resistant stainless steel reactor to terminate the reaction, and a large amount of methanol is used to separate the reaction product, which is then vacuum-dried at 50°C to obtain aromatic vinyl polymer 1.
[0124] (Manufacturing conditions) According to the compounding recipe shown in Table 1, chemicals other than sulfur and vulcanization accelerator are kneaded for 4 minutes at 150°C using a 1.7L Banbury mixer manufactured by Kobe Steel, Ltd., and then sulfur and vulcanization accelerator are added and kneaded for 5 minutes at 80°C using an open roll to obtain an unvulcanized rubber composition. Each of the obtained unvulcanized rubber compositions is molded into a cap tread shape, laminated together with other tire components, and vulcanized at 170°C for 15 minutes to produce a test tire (tire size: 195 / 65R15).
[0125] (Wet grip performance during high speed driving (calculation of actual vehicle evaluation based on simulation)) The test tires were attached to all wheels of a vehicle (domestic FF 2000cc), and the wet grip performance (braking distance) during high-speed running of the actual vehicle was calculated based on the braking distance from an initial speed of 100 km / h on a wet asphalt road surface. The wet grip performance (braking distance) during high-speed running of Comparative Example 6 was set as 100, and each compounding was expressed as an index. The larger the index, the better the wet grip performance during high-speed running.
[0126] [Table 1]
Claims
1. A rubber composition for tires comprising a rubber component (A) containing an isoprene-based rubber and a styrene-butadiene-based rubber, a C5-based resin and / or a C5-C9-based resin (B), and an aromatic vinyl-based polymer (C), The styrene-butadiene rubber is a polymer having styrene and butadiene as constituent units, in which the total amount of styrene units and butadiene units is 95% by mass or more out of 100% by mass of all constituent units of the polymer, and the weight average molecular weight is 60,000 or more, The C5 resin is at least one selected from the group consisting of a copolymer of isoprene and styrene, and an aliphatic petroleum resin obtained by polymerizing or copolymerizing a C5 fraction obtained by thermal cracking of naphtha; the aromatic vinyl polymer is at least one polymer selected from the group consisting of an aromatic vinyl thermoplastic elastomer, a homopolymer of an aromatic vinyl compound, and a copolymer of an aromatic vinyl compound and a terpene compound (excluding the styrene-butadiene rubber, the C5 resin, and the C5-C9 resin); The content of the isoprene-based rubber in 100% by mass of the rubber component is 30% by mass or more, The styrene-butadiene rubber is a rubber composition for tires having a styrene content of 30% by mass or more (however, this does not include a rubber composition for tires that contains a rubber component and a styrene-alkylene block copolymer, the styrene-alkylene block copolymer having a total content of styrene units of 30% by mass or more and a foaming ratio after vulcanization of 5 to 30%).
2. A rubber composition for tires comprising: a rubber component (A) containing an isoprene-based rubber and a styrene-butadiene-based rubber; a C5-based resin and / or a C5-C9-based resin (B); an aromatic vinyl-based polymer (C); and a liquid plasticizer, The styrene-butadiene rubber is a polymer having styrene and butadiene as constituent units, in which the total amount of styrene units and butadiene units is 95% by mass or more out of 100% by mass of all constituent units of the polymer, and the weight average molecular weight is 60,000 or more, The C5 resin is at least one selected from the group consisting of a copolymer of isoprene and styrene, and an aliphatic petroleum resin obtained by polymerizing or copolymerizing a C5 fraction obtained by thermal cracking of naphtha; the aromatic vinyl polymer is at least one polymer selected from the group consisting of an aromatic vinyl thermoplastic elastomer, a homopolymer of an aromatic vinyl compound, and a copolymer of an aromatic vinyl compound and a terpene compound (excluding the styrene-butadiene rubber, the C5 resin, and the C5-C9 resin); The content of the isoprene-based rubber in 100% by mass of the rubber component is 30% by mass or more, The rubber composition for tires has a liquid plasticizer content of 10 parts by mass or more per 100 parts by mass of the rubber component.
3. 3. The rubber composition for tires according to claim 1, wherein the aromatic vinyl polymer is a polymer containing a styrene unit.
4. The rubber composition for tires according to claim 2 or 3, wherein the styrene-butadiene rubber has a styrene content of 30% by mass or more.
5. 5. The rubber composition for tires according to claim 1, wherein the content of the aromatic vinyl polymer is 10 to 60 parts by mass based on 100 parts by mass of the rubber component.
6. The rubber composition for tires according to any one of claims 1 to 5, wherein the total content of the C5 resin and the C5-C9 resin is 10 to 60 parts by mass based on 100 parts by mass of the rubber component.
7. A tire having a tread made using the rubber composition according to any one of claims 1 to 6.
Citation Information
Patent Citations
Rubber composition for tire tread
JP2000159935A
Pneumatic tire
JP2019026712A
Rubber composition for tire, and tire
JP2019182982A
Rubber composition and tire
WO2019117168A1
Rubber composition and tire
WO2019117217A1