Paint-resistant welded joints and structures
A welded joint with controlled chemical compositions and multi-layer coatings addresses the high maintenance costs of steel structures in severe corrosive environments by enhancing corrosion resistance and durability, reducing repainting frequency.
Patent Information
- Application Number
- JP2020174571
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-10-16
- Publication Date
- 2024-09-18
- Estimated Expiration
- 2040-10-16
AI Technical Summary
Existing steel structures in severe corrosive environments, such as near the sea or coast, face high maintenance costs due to frequent repainting needs, with welded joints being particularly prone to paint defects and corrosion, leading to increased labor and material expenses.
A welded joint with controlled chemical compositions for both base metal and weld metal, using specific ranges of elements like Cu, Ni, Mo, Sn, and Sb, combined with a multi-layer coating system, to enhance corrosion resistance and durability, reducing the frequency of repainting.
The solution provides excellent coating durability, reducing maintenance costs and extending the repainting cycle, thereby lowering the life cycle cost of steel structures.
Smart Images

Figure 0007552245000005 
Figure 0007552245000002 
Figure 0007552245000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a welded joint and a structure that are applied to welded structures and the like where structural safety is highly required and have a coating film on the surface. The present invention relates to a welded joint formed by welding structural steel materials together, which are mainly used in outdoor atmospheric corrosive environments on land such as bridges, and in particular in severe corrosive environments such as at sea or on the coast where there is a large amount of airborne salt, and to a structure that has the welded joint of the present invention and exhibits excellent coating durability. [Background technology]
[0002] Steel structures used outdoors, such as bridges, are usually subjected to some kind of corrosion prevention treatment before use. For example, weathering steel is often used in environments with low levels of airborne salt. Weathering steel is a steel material whose surface is covered with a highly protective rust layer containing concentrated alloy elements such as Cu, P, Cr, and Ni when used in an atmospheric exposure environment, greatly reducing the corrosion rate. It is known that bridges using such weathering steel can withstand decades of use without painting in environments with low levels of airborne salt.
[0003] On the other hand, in environments with high levels of airborne salt, such as at sea or near the coast, it is difficult for weathering steel to form a highly protective rust layer, making it difficult to use weathering steel without painting. For this reason, in environments with high levels of airborne salt, such as at sea or near the coast, ordinary steel that has been subjected to anticorrosion treatment, such as painting, is generally used.
[0004] However, painted steel products require periodic repairs such as repainting due to deterioration of the paint film over time, the occurrence of rust, and swelling of the paint film. The painting work required for repainting is often carried out at high altitudes, which is difficult and increases the labor costs involved. Therefore, when painted steel products are used, there is a problem that the repainting work increases the maintenance costs of the structure, which in turn increases the life cycle costs.
[0005] For these reasons, there is a need for the development of steel materials with excellent corrosion resistance, in particular structural steel materials with excellent paint durability, that can extend the repainting cycle, thereby reducing the frequency of painting and reducing the maintenance costs of structures.
[0006] Moreover, such steel structures, especially bridges, have many welded joints at their joints. Compared to the base material, welded joints are not flat because of the weld beads, and are prone to paint defects. Furthermore, in welded joints, it is necessary to consider dissimilar metal corrosion between the weld metal and the base material. Therefore, the corrosion characteristics of welded joints are thought to be different from those of the base material, and they are prone to become the starting point of paint film blisters due to corrosion. The cost of maintaining safety by repeatedly inspecting, repairing, and repainting all the numerous welds on bridges is enormous. Therefore, improving the corrosion resistance of welded joints is very important from the perspective of maintenance costs.
[0007] Here, as an example of a steel material and welded joint having excellent corrosion resistance, Patent Document 1 discloses a highly weather-resistant steel material containing 0.15 to 0.30% P and more than 2.0% and less than 3.0% Cr.
[0008] Patent Document 2 discloses a steel material with excellent paint durability that contains 0.03 to 0.15% P and 0.2 to 0.5% Cu.
[0009] Patent Document 3 discloses a coated steel material having excellent durability, which contains 0.05 to 3.0% Cu, 0.05 to 6.0% Ni, and 0.01 to 1.0% Ti.
[0010] Patent Document 4 discloses a steel material for painting that contains 0.05 to 3.0% Cu, 0.05 to 6.0% Ni, and 0.025 to 0.15% Ti and has excellent paint film durability.
[0011] Patent Document 5 discloses a steel material having excellent bare weather resistance and weldability, which contains 0.05 to 3.0% Cu, 0.05 to 6.0% Ni, and 0.01 to 1.0% Ti.
[0012] Patent Document 6 discloses a high weldability and high weather resistance steel containing 0.30 to 1.00% of Cu and 1.0 to 5.5% of Ni.
[0013] Patent Document 7 discloses a steel material excellent in corrosion resistance and weldability containing one or two of Cu: 0.05 to 3.0% and Ni: 0.05 to 6.0%.
[0014] Patent Document 8 discloses a coated steel sheet excellent in coating durability and pitting corrosion resistance containing Ti + Zr in an amount of 0.03% < Ti + Zr < 0.4%.
[0015] Patent Document 9 discloses a steel material excellent in coastal weather resistance containing 0.05 to 1.0% of Cu, 0.01 to 0.5% of Ni, 0.01 to 3.0% of Cr, and 0.03 to 0.50% of Sn and / or Sb.
[0016] Patent Document 10 discloses a method for manufacturing a steel material excellent in corrosion resistance and toughness in the Z direction containing 0.01 to 3.0% of Cr and 0.03 to 0.50% of Sn.
[0017] Patent Document 11 discloses a steel material excellent in corrosion resistance used in a dry - wet repeated environment containing chlorides and containing 0.15 to 0.5% of Sn.
[0018] Patent Document 12 discloses a steel material excellent in corrosion resistance containing 2.6 to 13.0% of Cr and 0.01 to 0.5% of Sn.
[0019] Patent Document 13 discloses a welded joint excellent in corrosion resistance containing 0.01 to 5.0% of Cu and 0.01 to 5.0% of Cr in the base metal and the weld metal.
[0020] Patent Document 14 discloses a welded joint excellent in corrosion resistance containing 0.01 to 5.00% of Co and 0.0005 to 0.020% of Mg in the base metal and the weld metal.
[0021] Patent Document 15 discloses a welded joint for a crude oil tank, the base metal containing Cu: 0.01-1.5%, and one or two of Mo: 0.01-0.096% and W: 0.01-1%. [Prior art documents] [Patent documents]
[0022] [Patent Document 1] Japanese Patent Application Publication No. 6-93372 [Patent Document 2] Japanese Patent Application Publication No. 6-143489 [Patent Document 3] Japanese Patent Application Publication No. 10-330881 [Patent Document 4] JP 2000-169939 A [Patent Document 5] Japanese Patent Application Publication No. 11-241139 [Patent Document 6] Japanese Patent Application Publication No. 11-172370 [Patent Document 7] Japanese Patent Application Publication No. 11-71632 [Patent Document 8] JP 2003-171732 A [Patent Document 9] JP 2006-118011 A [Patent Document 10] JP 2010-7109 A [Patent Document 11] JP 2012-255184 A [Patent Document 12] JP 2013-166992 A [Patent Document 13] JP 2012-135817 A [Patent Document 14] JP 2007-69265 A [Patent Document 15] Patent No. 4088231 Summary of the Invention [Problem to be solved by the invention]
[0023] However, weldability is significantly reduced when the P content is increased as in Patent Documents 1 and 2. Furthermore, Patent Document 1 does not pay any attention to the corrosion resistance of the coated steel material, i.e., the durability of the coating.
[0024] Moreover, excessive increase in the content of Cu or Ni as in Patent Documents 3 to 7 leads to an increase in alloy costs. Furthermore, inclusion of a large amount of Ti as in Patent Documents 3 to 5 and 8 leads to a deterioration in the toughness of the steel material. In addition, excessive increase in the content of Cr, Sn, etc. as in Patent Documents 9 to 13 also leads to an increase in alloy costs and a deterioration in the toughness of the steel material.
[0025] Moreover, excessive increase in the contents of Co and Mg, as in Patent Document 14, leads to an increase in alloy costs. Moreover, Patent Document 15 takes into consideration corrosion in a crude oil environment, but does not take into consideration the corrosive environment that is the subject of the present invention, that is, corrosion in an environment in which a coating film is present on the steel sheet surface and the steel sheet is exposed to the atmosphere.
[0026] The present invention has been made in consideration of the above-mentioned circumstances, and has an object to provide a welded joint that has excellent paint durability by extending the cycle for repainting, reducing the frequency of painting, even when used in outdoor atmospheric corrosive environments such as bridges, particularly in severe corrosive environments such as at sea or near coasts with high levels of airborne salt, without incurring an excessive increase in alloy costs.
[0027] In the present invention, "excellent paint durability" refers to a coating film formed on the surface of a steel sheet, and when a corrosion test is carried out under the following conditions, the blister area of the coating film is 480 mm 2 This means that: (Corrosion test conditions) Initial defect in the coating: Straight cut 1mm wide and 40mm long Artificial sea salt deposition amount: 6.0g / m 2 Test time: 1200 cycles (9600 hours) Cycle conditions: (Condition 1. Temperature: 60°C, Relative humidity: 35%, Holding time: 3 hours), (Condition 2. Temperature: 40°C, Relative humidity: 95%, Holding time: 3 hours), transition time from condition 1 to condition 2 and from condition 2 to condition 1 was 1 hour, total 8 hours cycle [Means for solving the problem]
[0028] The inventors have discovered that it is possible to effectively suppress deterioration of the coating film from damaged areas such as paint scratches by specifying the chemical components of the base material and the weld metal within appropriate ranges without adding large amounts of Cu, Ni, Cr, Sn, Co, Mg, etc., which may increase the alloy cost and deteriorate the toughness.
[0029] The present invention has been completed based on the above findings and through further investigation. That is, the gist and configuration of the present invention are as follows. [1] A welded joint formed by welding base materials together, the composition of the base material being, in mass%, C: 0.020% or more, 0.200% or less, Si: 0.05% or more, 1.00% or less, Mn: 0.20% or more, 2.00% or less, P: 0.003% or more, 0.030% or less, S: 0.010% or less, Al: 0.001% or more and 0.100% or less; Furthermore, Cu: 0.50% or less, Ni: 0.50% or less, W: 1.000% or less, Mo: 0.500% or less Sn: 0.200% or less, Sb: 0.200% or less, and the balance being Fe and unavoidable impurities, The composition of the weld metal is, in mass%, C: 0.020% or more, 0.200% or less, Si: 0.05% or more, 1.00% or less, Mn: 0.20% or more, 2.00% or less, P: 0.003% or more, 0.030% or less, S: 0.010% or less, Al: 0.001% or more and 0.100% or less; Furthermore, Cu: 1.00% or less, Ni: 5.00% or less, W: 1.000% or less, Mo: 1.000% or less Sn: 0.200% or less, Sb: 0.200% or less and the balance being Fe and unavoidable impurities, Furthermore, the present invention provides a welded joint having excellent paint durability, characterized in that the P values of the respective components of the base metal and the weld metal part calculated using the following formula (1) are all 0.90 or less, and the formula (2) is satisfied. P-value: |P (Cu) ×P (Ni) ×P (W) ×P (Mo) ×P (Sn) ×P (Sb) |…(1) Where: P (Cu) =1-0.0288[Cu]…(1-1) P (Ni) =1-0.497[Ni]…(1-2) and W: Less than 0.05% P (W) =1-3.54[W]…(1-3-1) W: 0.05% or more, P (W) =1-0.056[W]-0.174…(1-3-2) Mo: Less than 0.05% P (Mo) =1-3.03[Mo]…(1-4-1) Mo: 0.05% or more, P (Mo) =1-0.098[Mo]-0.147…(1-4-2) Sn: Less than 0.03% P(Sn) =1-3.41[Sn]…(1-5-1) Sn: 0.03% or more P (Sn) =1-1.04[Sn]-0.071…(1-5-2) Sb: When less than 0.05%, P (Sb) =1-2.32[Sb]…(1-6-1) Sb: 0.05% or more P (Sb) =1-0.0351[Sb]-0.114…(1-6-2) It is. In (1-1), (1-2), (1-3-1), (1-3-2), (1-4-1), (1-4-2), (1-5-1), (1-5-2), (1-6-1), and (1-6-2), [Cu][Ni][W][Mo][Sn][Sb] are the contents (mass%) of each element. P B ≧P W …(2) In addition, in formula (2), P B : P value calculated from the composition of the base material P W : P value calculated from the chemical composition of the weld metal It is. [2] Furthermore, the composition of the base material is, in mass%, V: 0.200% or less, Ti: 0.050% or less, Zr: 0.100% or less, B: 0.0050% or less, Ca: 0.0100% or less, Mg: 0.0100% or less, REM: 0.0100% or less Contains one or more selected from the following: Furthermore, the composition of the weld metal part is, in mass%, V: 0.200% or less, Ti: 0.050% or less, Zr: 0.100% or less, B: 0.0050% or less, Ca: 0.0100% or less, Mg: 0.0100% or less, REM: 0.0100% or less The welded joint having excellent paint durability described in [1], characterized in that it contains one or more types selected from the following: [3] A welded joint having excellent paint durability as described in [1] or [2], characterized in that the base material is a structural steel material and the welded joint has a paint film. [4] The welded joint having excellent paint durability according to [3], characterized in that the coating film has a corrosion-resistant base layer, a primer layer, an intermediate coat layer and a top coat layer, the corrosion-resistant base layer being made of inorganic zinc-rich paint, the primer layer being made of epoxy resin paint, the intermediate coat layer being made of intermediate paint for a fluororesin top coat paint, and the top coat layer being made of a fluororesin top coat paint. [5] A welded joint having excellent paint durability as described in [3] or [4], characterized in that the structural steel surface has a zinc-rich primer layer. [6] A structure having a welded joint according to any one of [1] to [5]. Effect of the Invention
[0030] According to the present invention, it is possible to obtain a welded joint having excellent paint durability, which makes it possible to reduce the maintenance costs of steel structures and, in turn, the life cycle costs. [Brief description of the drawings]
[0031] [Figure 1] FIG. 1 is a schematic diagram showing the shape of a corrosion test piece in the examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0032] The present invention will be specifically described below.
[0033] First, the reason for limiting the composition of the base material in the present invention will be described. Note that the unit of the content of elements in the composition of steel is always "mass%", but hereinafter, unless otherwise specified, it will be simply indicated as "%".
[0034] C: 0.020% or more, 0.200% or less C is an element that increases the strength of steel and increases the volume fraction of the hard second phase. Therefore, C must be contained at 0.020% or more to ensure the required strength for structural steel. On the other hand, if the C content exceeds 0.200%, the weldability and toughness deteriorate. Therefore, the C content is set to 0.020% or more and 0.200% or less.
[0035] Si: 0.05% or more, 1.00% or less Silicon must be present at 0.05% or more to ensure deoxidation and strength. However, if the silicon content exceeds 1.00%, toughness and weldability deteriorate significantly. Therefore, the silicon content is set to 0.05% or more and 1.00% or less.
[0036] Mn: 0.20% or more, 2.00% or less Mn is an element that increases the strength of steel. Therefore, in order to ensure a certain strength as a structural steel, Mn must be contained in an amount of 0.20% or more. On the other hand, if the Mn content exceeds 2.00%, toughness and weldability deteriorate. Therefore, the Mn content is set to 0.20% or more and 2.00% or less. It is preferably set to 0.75% or more and 1.80% or less.
[0037] P: 0.003% or more, 0.030% or less P is an element that contributes to improving the paint durability of steel materials. In order to obtain this effect, P must be contained at 0.003% or more. On the other hand, if the P content exceeds 0.030%, weldability deteriorates. Therefore, the P content is set to 0.003% or more and 0.030% or less.
[0038] S: 0.010% or less S is an element that deteriorates weldability and toughness. For this reason, the S content must be 0.010% or less. There is no particular lower limit, but if the S content is reduced to less than 0.0001%, production costs will increase, so the realistic lower limit is 0.0001%.
[0039] Al: 0.001% or more, 0.100% or less Al is an element necessary for deoxidation during steelmaking. To obtain this effect, it is necessary to include 0.001% or more of Al. On the other hand, if the Al content exceeds 0.100%, it adversely affects weldability. Therefore, the Al content is set to 0.001% or more and 0.100% or less. Preferably, it is set to 0.005% or more and 0.050% or less. More preferably, it is set to 0.010% or more and 0.030% or less.
[0040] Furthermore, the present invention contains one or more selected from Cu: 0.50% or less, Ni: 0.50% or less, W: 1.000% or less, Mo: 0.500% or less, Sn: 0.200% or less, and Sb: 0.200% or less.
[0041] Cu: 0.50% or less Cu has the effect of forming a dense rust layer by refining the rust grains in the rust layer, and suppressing the permeation of oxygen and chloride ions, which are corrosion-promoting factors, into the base steel. In order to obtain such an effect, it is preferable that the Cu content is 0.01% or more. On the other hand, if the Cu content exceeds 0.50%, the alloy cost increases. Therefore, the Cu content is 0.50% or less. It is preferably 0.01% or more and 0.50% or less, more preferably 0.03% or more and 0.40% or less, and more preferably 0.04% or more and 0.30% or less. It is further preferably 0.05% or more and 0.25% or less.
[0042] Ni: 0.50% or less Ni has the effect of forming a dense rust layer by refining the rust grains in the rust layer, and suppressing the permeation of oxygen and chloride ions, which are corrosion-promoting factors, into the base steel. In order to obtain such an effect, the Ni content is preferably 0.01% or more. On the other hand, if the Ni content exceeds 0.50%, the alloy cost increases. Therefore, the Ni content is set to 0.50% or less. Preferably, it is 0.01% or more and 0.50% or less, more preferably, it is 0.03% or more and 0.40% or less, and even more preferably, it is 0.04% or more and 0.30% or less. Even more preferably, it is 0.05% or more and 0.15% or less.
[0043] W: 1.000% or less W is an important element in the structural steel material of the present invention, which has excellent paint durability. W dissolves during the anodic reaction and is dissolved in the rust layer as WO4 2- By distributing as tungsten, chloride ions, which are corrosion accelerating factors, are electrostatically prevented from penetrating the rust layer and reaching the base steel. Furthermore, compounds containing W are precipitated on the steel surface, suppressing the anodic reaction of the steel. In addition, by forming fine rust and densifying the rust layer, chloride ions, which are corrosion factors, are prevented from penetrating the rust layer and reaching the base steel. In order to obtain these effects, it is preferable that the W content is 0.005% or more. On the other hand, if the W content exceeds 1.000%, the alloy cost increases. Therefore, the W content is 1.000% or less. It is preferably 0.005% or more and 1.000% or less, more preferably 0.010% or more and 0.700% or less, more preferably 0.030% or more and 0.500% or less. It is even more preferably 0.050% or more and 0.100% or less.
[0044] Mo: 0.500% or less Mo dissolves during the anodic reaction of steel and forms MoO4 in the rust layer. 2-The distribution of Mo in the steel prevents chloride ions, which are corrosion-promoting factors, from penetrating the rust layer and reaching the base steel. In addition, compounds containing Mo are precipitated on the steel surface, suppressing the anodic reaction of the steel. To obtain such an effect, the Mo content is preferably 0.005% or more. On the other hand, if the Mo content exceeds 0.500%, the alloy cost increases. Therefore, when Mo is contained, the Mo content is set to 0.500% or less. The Mo content is preferably 0.005% or more and 0.500% or less.
[0045] Sn: 0.200% or less Sn is present in the rust layer near the surface of the base steel, and by refining the rust particles, it prevents chloride ions, which are corrosion-promoting factors, from penetrating the rust layer and reaching the base steel. Sn also suppresses the anodic reaction on the steel surface. To obtain such an effect, the Sn content is preferably 0.005% or more. On the other hand, if the Sn content exceeds 0.200%, it leads to deterioration of the ductility and toughness of the steel. Therefore, when Sn is contained, the Sn content is set to 0.200% or less. It is preferably 0.005% or more and 0.200% or less, more preferably 0.010% or more and 0.100% or less. It is more preferably 0.020% or more and less than 0.050%.
[0046] Sb: 0.200% or less Sb is present in the rust layer near the surface of the base steel, and by refining the rust particles, it prevents chloride ions, which are corrosion-promoting factors, from penetrating the rust layer and reaching the base steel. Sb also suppresses the anodic reaction on the steel surface. To obtain such an effect, the Sb content is preferably 0.005% or more. On the other hand, if the Sb content exceeds 0.200%, it leads to deterioration of the ductility and toughness of the steel. Therefore, when Sb is contained, the Sb content is set to 0.200% or less. It is preferably 0.005% or more and 0.200% or less, more preferably 0.010% or more and 0.150% or less, and more preferably 0.020% or more and 0.100% or less.
[0047] The basic components of the base material have been described above, but in the present invention, the following elements can be appropriately contained as necessary.
[0048] V:0.200% or less V is present in the rust layer near the surface of the steel substrate. 3- The presence of V as a Cr-Cr alloy prevents chloride ions, which are corrosion-accelerating factors, from penetrating the rust layer and reaching the base steel. To fully obtain this effect, it is preferable to include 0.005% or more of V. On the other hand, if the V content exceeds 0.200%, the effect saturates. Therefore, if V is included, the V content is set to 0.200% or less. Preferably, it is 0.005% or more and 0.200% or less.
[0049] Ti: 0.050% or less Ti is an element that increases strength. In order to fully obtain such an effect, it is preferable to contain Ti at 0.005% or more. On the other hand, if the Ti content exceeds 0.050%, it will cause a deterioration in toughness. Therefore, when Ti is contained, the Ti content is set to 0.050% or less. Preferably, it is 0.005% or more and 0.050% or less.
[0050] Zr: 0.100% or less Zr is an element that enhances strength. In order to fully obtain this effect, it is preferable to contain Zr at 0.005% or more. On the other hand, if the Zr content exceeds 0.100%, the strength-enhancing effect is saturated. Therefore, when Zr is contained, the Zr content is set to 0.100% or less. Preferably, it is 0.005% or more and 0.100% or less.
[0051] B: 0.0050% or less B is an element that increases strength. In order to fully obtain this effect, it is preferable to contain 0.0001% or more of B. On the other hand, if the B content exceeds 0.0050%, it will cause a deterioration in toughness. Therefore, when B is contained, the B content is set to 0.0050% or less. Preferably, it is 0.0001% or more and 0.0050% or less.
[0052] Ca:0.0100% or less Ca is an element that fixes S in steel and improves the toughness of the weld heat affected zone. To fully obtain this effect, it is preferable to contain Ca at 0.0001% or more. On the other hand, if the Ca content exceeds 0.0100%, the amount of inclusions in the steel increases, which actually leads to a deterioration in toughness. Therefore, if Ca is contained, the Ca content is set to 0.0100% or less. Preferably, it is 0.0001% or more and 0.0100% or less.
[0053] Mg: 0.0100% or less Mg is an element that fixes S in steel and improves the toughness of the welded heat affected zone. In order to fully obtain such an effect, it is preferable to contain 0.0001% or more of Mg. On the other hand, if the Mg content exceeds 0.0100%, the amount of inclusions in the steel increases, which leads to a deterioration in toughness. Therefore, when Mg is contained, the Mg content is set to 0.0100% or less. Preferably, it is 0.0001% or more and 0.0100% or less.
[0054] REM: 0.0100% or less REM is an element that fixes S in steel and improves the toughness of the weld heat affected zone. In order to fully obtain this effect, it is preferable to contain 0.0001% or more of REM. On the other hand, if the REM content exceeds 0.0100%, the amount of inclusions in the steel increases, which leads to a deterioration in toughness. Therefore, when REM is contained, the REM content is set to 0.0100% or less. Preferably, it is 0.0001% or more and 0.0100% or less.
[0055] The balance other than the above is Fe and unavoidable impurities. Incidentally, examples of unavoidable impurities include N and O (oxygen), and N: 0.010% or less and O: 0.010% or less are permissible.
[0056] Next, the chemical composition of the weld metal part in the welded joint contains C: 0.020% or more and 0.200% or less, Si: 0.05% or more and 1.00% or less, Mn: 0.20% or more and 2.00% or less, P: 0.003% or more and 0.030% or less, S: 0.010% or less, and Al: 0.001% or more and 0.100% or less. The welding material components are adjusted so that the C, Si, Mn, P, S, and Al of the weld metal are within the same range as the allowable range of the base metal so that the weld metal part also has the specified strength as structural steel.
[0057] Furthermore, the present invention contains one or more elements selected from Cu: 1.00% or less, Ni: 5.00% or less, Mo: 1.000% or less, W: 1.000% or less, Sn: 0.200% or less, and Sb: 0.200% or less.
[0058] Cu: 1.00% or less Cu has the effect of forming a dense rust layer by refining the rust grains in the rust layer, and suppressing the permeation of oxygen and chloride ions, which are corrosion-promoting factors, into the base steel. To obtain such an effect, the Cu content is preferably 0.01% or more. On the other hand, if the Cu content exceeds 1.00%, it will lead to an increase in alloy costs. Therefore, when Cu is contained, the Cu content is set to 1.00% or less. Preferably, it is 0.01% or more and 1.00% or less.
[0059] Ni: 5.00% or less Ni has the effect of forming a dense rust layer by refining the rust grains in the rust layer, and suppressing the permeation of oxygen and chloride ions, which are corrosion-promoting factors, into the base steel. To obtain such an effect, the Ni content is preferably 0.01% or more. On the other hand, if the Ni content exceeds 5.00%, it leads to an increase in alloy costs. Therefore, when Ni is contained, the Ni content is 0.01% or more and 5.00% or less. Preferably, it is 0.01% or more and 5.00% or less.
[0060] Mo: 1.000% or less Mo is also one of the important elements for improving corrosion resistance in the weld metal of the welded joint of the present invention. To obtain this effect, it is preferable that the Mo content is 0.005% or more. However, if the Mo content exceeds 1.000%, it has a negative effect on the toughness of the weld metal. The reason why Mo has the above-mentioned effect of improving corrosion resistance is that MoO4 2- is generated, and this MoO4 2- The presence of Mo prevents chloride ions from penetrating the weld metal surface, thereby effectively preventing corrosion of the weld metal. Therefore, when Mo is contained, the Mo content is set to 1.000% or less. The Mo content is preferably 0.005% or more and 1.000% or less.
[0061] W: 1.000% or less W is one of the most important elements for improving corrosion resistance in the weld metal of the welded joint of the present invention. To obtain this effect, it is preferable that the W content is 0.005% or more. However, if the W content exceeds 1.000%, it has an adverse effect on the toughness of the weld metal. The reason why W has the above-mentioned effect of improving corrosion resistance is that as the weld metal corrodes, the rust that is formed contains WO4 2- This WO4 2- The presence of FeWO4 inhibits chloride ions from penetrating the weld metal surface, and furthermore, the insoluble FeWO4 is formed at the anode portion of the weld metal surface. The presence of FeWO4 also inhibits chloride ions from penetrating the weld metal surface, and by inhibiting the penetration of chloride ions into the weld metal surface, corrosion of the weld metal is effectively inhibited. In addition, WO4 2- This is because the corrosion of the weld metal is also suppressed by the inhibitor effect due to the adsorption of W to the weld metal surface. Therefore, if W is contained, the W content is set to 1.000% or less. Preferably, it is 0.005% or more and 1.000% or less.
[0062] Sn: 0.200% or less Sn has the effect of improving the corrosion resistance of the weld metal. This effect of Sn is to suppress corrosion at parts where the pH is low, such as the anode part of the weld metal surface. In order to obtain this effect, the Sn content is preferably 0.005% or more. However, if the Sn content exceeds 0.200%, the weld metal toughness is deteriorated. Therefore, when Sn is contained, the Sn content is set to 0.200% or less. Preferably, it is 0.005% or more and 0.200% or less.
[0063] Sb: 0.200% or less Sb is present in the rust layer near the surface of the base steel, and by refining the rust particles, it prevents chloride ions, which are corrosion-promoting factors, from penetrating the rust layer and reaching the base steel. Sb also suppresses the anodic reaction on the steel surface. To achieve this effect, it is preferable that the Sb content be 0.005% or more. On the other hand, if the Sb content exceeds 0.200%, it will cause a deterioration in the ductility and toughness of the steel. Therefore, if Sb is contained, the Sb content is 0.200% or less. Preferably, it is 0.005% or more and 0.200% or less.
[0064] The basic components of the weld metal part have been described above, but in the present invention, one or more selected from V: 0.200% or less, Ti: 0.050% or less, Zr: 0.100% or less, B: 0.0050% or less, Ca: 0.0100% or less, Mg: 0.0100% or less, and REM: 0.0100% or less may be appropriately contained as necessary. The reasons for limiting the upper limit and the preferred upper and lower limits are the same as those for the base metal components.
[0065] The balance other than the above is Fe and unavoidable impurities.
[0066] When the base metal and the weld metal are cut out and subjected to a corrosion resistance test, the above-mentioned compositional limitations are sufficient, but in an actual structure having both the base metal and the weld metal, even if the above limitations are met, problems such as the weld metal rusting first may occur. Therefore, the present inventors have studied in detail the relationship between each element and corrosion resistance and found a relationship. That is, the present invention is further characterized in that the P value calculated using the following formula (1) for each component of the base metal and the weld metal is 0.90 or less and also satisfies formula (2). P-value: |P (Cu) ×P (Ni) ×P (W) ×P (Mo) ×P (Sn) ×P (Sb) |…(1) Where: P (Cu) =1-0.0288[Cu]…(1-1) P (Ni) =1-0.497[Ni]…(1-2) and W: Less than 0.05% P (W) =1-3.54[W]…(1-3-1) W: 0.05% or more, P (W) =1-0.056[W]-0.174…(1-3-2) Mo: Less than 0.05% P (Mo) =1-3.03[Mo]…(1-4-1) Mo: 0.05% or more, P (Mo) =1-0.098[Mo]-0.147…(1-4-2) Sn: Less than 0.03% P (Sn) =1-3.41[Sn]…(1-5-1) Sn: 0.03% or more P (Sn) =1-1.04[Sn]-0.071…(1-5-2) Sb: When less than 0.05%, P (Sb)=1-2.32[Sb]…(1-6-1) Sb: 0.05% or more P (Sb) =1-0.0351[Sb]-0.114…(1-6-2) It is. In (1-1), (1-2), (1-3-1), (1-3-2), (1-4-1), (1-4-2), (1-5-1), (1-5-2), (1-6-1), and (1-6-2), [Cu][Ni][W][Mo][Sn][Sb] are the contents (mass%) of each element. P B ≧P W …(2) In addition, in formula (2), P B : P value calculated from the composition of the base material P W : P value calculated from the chemical composition of the weld metal It is.
[0067] The circumstances that led to the definition of the P value and formula (2) in the present invention will be described below.
[0068] In order to estimate the corrosion-resistant effect of the chemical components Cu, Ni, Mo, W, Sn, and Sb in the base metal and weld metal, steel pieces containing various amounts of these components were prepared as test pieces and investigated by the following tests. The surfaces of these test pieces were shot blasted to a surface roughness of ISO Sa 2.5, ultrasonically degreased in acetone for 5 minutes, and air-dried. Next, one side of the test piece was used as the painted surface, and inorganic zinc-rich paint (thickness: 75 μm) was applied as a corrosion-resistant base coat, followed by epoxy resin paint (thickness: 120 μm) as a base coat, followed by fluororesin top coat paint (thickness: 30 μm) as a middle coat, and then fluororesin paint top coat paint (thickness: 25 μm) as a top coat, forming a coating film consisting of a corrosion-resistant base coat layer, a base coat layer, a middle coat layer, and a top coat layer. The other surface and end surface of the test piece were sealed with a solvent-based epoxy resin paint and further coated with a silicone-based sealant.
[0069] After painting, a straight cut of width 1 mm and length 40 mm was made across the base metal, weld metal and base metal, reaching the base steel, to create an initial defect, as shown in Figure 1. Then, a corrosion test was carried out under the following conditions.
[0070] The amount of artificial sea salt attached to the surface of the test piece was 6.0 g / m 2 A solution of artificial sea salt diluted with pure water to a predetermined concentration was sprayed to adhere the artificial sea salt to the test piece so that the artificial sea salt was adhered to the test piece. Next, a corrosion test was carried out using this test piece, in which a total of 8 hours of cycles were performed, with the transition time from condition 1 (temperature: 60°C, relative humidity: 35%, retention time: 3 hours) to condition 2 (temperature: 40°C, relative humidity: 95%, retention time: 3 hours), and from condition 2 to condition 1 being 1 hour, and this cycle was repeated 1200 times. Note that the adhesion of the artificial sea salt was once a week. The width of the coating film blister that occurred on the test piece was measured by the above test. From this result, the contribution of each of the coating film blister width and Cu, Ni, Mo, W, Sn, and Sb to the corrosion resistance was calculated, and the formula (1) of the P value was found. Note that the P value is 1.00 when Cu, Ni, Mo, W, Sn, and Sb are not contained at all, but the corrosion resistance required in the present invention can be obtained by making the P value 0.90 or less. Furthermore, the composition of the weld metal was changed by changing the composition of the welding material in various ways, and the relationship between the base material and the weld metal was examined. As a result, the P value of the weld metal (P W ) is the P value of the base material component (P B ) It has also been found necessary to
[0071] When the P value of the base metal and the weld metal is 0.90 or less, sufficient corrosion resistance is achieved. On the other hand, when the P value of both the base metal and the weld metal is greater than 0.90, the corrosion resistance is significantly reduced. Note that Cu, Ni, Mo, W, Sn, and Sb in the weld metal do not necessarily need to be added in combination, since sufficient corrosion resistance is achieved as long as the P value is 0.90 or less. In addition, the P value of the base metal and the weld metal is preferably 0.80 or less.
[0072] Furthermore, the present invention is characterized in that the following formula (2) is satisfied. P B ≧PW …(2) In addition, in formula (2), P B : P value calculated from the composition of the base material P W : P value calculated from the chemical composition of the weld metal It is.
[0073] In actual structures, the weld metal part is not flat compared to the base metal due to weld beads and other factors, and the paint film thickness is thinner than the base metal, making it more likely to become a starting point for corrosion. Therefore, the weld metal is required to have corrosion resistance greater than that of the base metal. By satisfying formula (2), corrosion resistance greater than that of the base metal is guaranteed.
[0074] There are no particular limitations on the method for adding appropriate amounts of Cu, Ni, Mo, W, Sn, and Sb to the weld metal, and although this depends on the welding method, when the weld metal is formed by melting and solidifying the base metal components, flux, welding wire, and the like, it is sufficient to add the above-mentioned components to these components.
[0075] Depending on the size of the weld metal part and the welding method, the composition of the weld metal part can be estimated from the composition of the base material and the composition of the welding material, and the amounts of Cu, Ni, W, Mo, Sn, and Sb to be added can be appropriately determined so that the P value is in the appropriate range.
[0076] In the present invention, the welding means is not particularly limited, and any commonly used welding method can be appropriately selected and used so as to ensure the mechanical properties and corrosion resistance of the welded joint. Representative examples include automatic welding such as submerged arc welding (SAW), semi-automatic arc welding such as flux-cored wire (FCW) or solid wire (GMAW), and manual arc welding such as shielded metal arc welding (SMAW).
[0077] The welded joint of the present invention is a welded joint formed by welding structural steel materials (base materials) together, and the welded joint of the present invention has a coating film. Usually, a coating film is applied to the surface of the structural steel material and then welded to form a welded joint, or a coating film is applied to the structural steel material after welding to form a welded joint. Examples of the coating film include a coating film having a corrosion-resistant base layer, a primer layer, a middle coat layer, and a top coat layer in this order.
[0078] It is preferable that the anticorrosive base layer is formed using an inorganic zinc-rich paint (e.g., SD Zinc 1500), the undercoat layer is formed using an epoxy resin paint (e.g., Epomarine HB(K)), the intermediate layer is formed using an intermediate paint for a fluororesin topcoat paint (e.g., Ceratect F intermediate coat), and the topcoat layer is formed using a fluororesin topcoat paint (e.g., Ceratect F(K) topcoat). The coating film on the steel surface may be a coating film having a primer layer, an undercoat layer, an intermediate layer, and a topcoat layer in this order, or a coating film having an anticorrosive base layer, an undercoat layer, and a topcoat layer in this order.
[0079] Furthermore, for the purpose of primary rust prevention, it is preferable that the surface of the structural steel material has a zinc-rich primer layer at the time of product shipment. The zinc-rich primer layer is a primer layer formed using a zinc-rich primer specified in JIS K 5552 (2002).
[0080] The base material (structural steel material) of the welded joint of the present invention is obtained by hot rolling a slab obtained by ordinary continuous casting or blooming of steel having the above-mentioned composition into a steel material such as a thick plate, a shaped steel, a thin steel plate, a steel bar, etc. Heating and rolling conditions may be appropriately determined according to the required properties, and a combination of controlled rolling, accelerated cooling, reheating heat treatment, etc. is also possible.
[0081] The content of each element in the base metal and the weld metal can be determined by spark discharge optical emission spectrometry, X-ray fluorescence spectrometry, ICP optical emission spectrometry, ICP mass spectrometry, combustion method, or the like. EXAMPLES
[0082] Steel containing the chemical composition shown in Table 1 (the balance being Fe and unavoidable impurities) was melted, heated to 1100-1150°C, hot rolled, and air-cooled to room temperature to obtain steel plates with a thickness of 25 mm. These steel plates were welded to produce welded joints. The amounts of Cu, Ni, W, Mo, Sn, and Sb in the weld metal were adjusted by adding Cu, Ni, W, Mo, Sn, and Sb to the flux and wire, in addition to dilution from the base metal.
[0083] Welded joints were fabricated using base metals with the chemical compositions shown in Table 1 and welding materials with the chemical compositions shown in Table 2. The welding methods used were shielded metal arc welding (SMAW), submerged arc welding (SAW), and semi-automatic arc welding using flux-cored wire (FCW) and solid wire (GMAW). The welded joints were subjected to a composition analysis of the center of the weld metal (a sample taken from the center to account for 50% of the area ratio of the entire weld metal was analyzed). The chemical compositions of the welded joints fabricated are shown in Table 3.
[0084] In order to investigate the paint durability of the welded joints thus prepared, a test piece measuring 120 mm x 50 mm x 5 mm was taken across the weld metal as shown in Figure 1. The surface of the test piece was shot blasted to achieve a surface roughness of ISO Sa 2.5, ultrasonically degreased in acetone for 5 minutes, and air-dried. Next, one side of the test piece was used as the painted surface, and inorganic zinc-rich paint (thickness: 75 μm) was applied as a corrosion-resistant base coat, followed by epoxy resin paint (thickness: 120 μm) as a base coat, then intermediate paint for fluororesin top coat paint (thickness: 30 μm) as an intermediate coat, and then fluororesin paint top coat paint (thickness: 25 μm) as a top coat, forming a coating film consisting of a corrosion-resistant base coat layer, an undercoat layer, an intermediate coat layer, and an overcoat layer. The other side and end face of the test piece were sealed with a solvent-based epoxy resin paint, and further covered with a silicone-based sealant.
[0085] After painting, a straight cut 1 mm wide and 40 mm long was made across the weld metal to reach the base steel, as shown in Figure 1 (the ratio of the length of the weld metal part to the base metal part in the cut was 1:1), creating an initial defect. Then, a corrosion test was carried out under the following conditions.
[0086] The amount of artificial sea salt attached to the surface of the test piece was 6.0 g / m 2 A solution of artificial sea salt diluted with pure water to a prescribed concentration was sprayed onto the test piece so that the artificial sea salt adhered to the test piece. Next, using this test piece, a corrosion test was carried out in which a total of 8 hours was defined as one cycle, with the transition time from condition 1 (temperature: 60°C, relative humidity: 35%, retention time: 3 hours) to condition 2 (temperature: 40°C, relative humidity: 95%, retention time: 3 hours), and from condition 2 to condition 1 being 1 hour, and this cycle was repeated 1200 times. The artificial sea salt was applied once a week.
[0087] After the corrosion test, the blister area from the initial defect in the paint was measured to evaluate the paint durability. 2 If the coating had a resistance of 0.1% or less, it was determined that the coating had excellent durability.
[0088] The results are shown in Table 4.
[0089] When the P value of the base metal and weld metal is 0.90 or less, the blister area of the paint is 480 mm 2 On the other hand, in the case of steel grade BW26, the P value of the base material and weld metal is less than 0.90, but the P value is less than 0.90. B <P W If the paint bulge area is 480 mm 2 It can be seen that the paint durability has decreased, exceeding the P value. Also, it can be seen that the paint durability has deteriorated even in cases where only one of the base material or the weld metal meets the P value, such as in the case of steel type BW29.
[0090] [Table 1]
[0091]
Table 2
[0092]
Table 3
[0093]
Table 4
Claims
1. A welded joint formed by welding base materials together, the composition of the base materials being, in mass%, C: 0.020% or more, 0.200% or less, Si: 0.05% or more, 1.00% or less, Mn: 0.20% or more, 2.00% or less, P: 0.003% or more, 0.030% or less, S: 0.010% or less, Al: 0.001% or more, 0.100% or less, Cu: 0.50% or less; Further, Ni: 0.50% or less, W: 1.000% or less, Mo: 0.500% or less, Sn: 0.200% or less, Sb: 0.200% or less, and the balance being Fe and unavoidable impurities, The composition of the weld metal part is, in mass%, C: 0.020% or more, 0.200% or less, Si: 0.05% or more, 1.00% or less, Mn: 0.20% or more, 2.00% or less, P: 0.003% or more, 0.030% or less, S: 0.010% or less, Al: 0.001% or more, 0.100% or less, Cu: 1.00% or less; Further, Ni: 5.00% or less, W: 1.000% or less, Mo: 1.000% or less, Sn: 0.200% or less, Sb: 0.200% or less and the balance being Fe and unavoidable impurities, Furthermore, the present invention provides a welded joint having excellent paint durability, characterized in that the P values of the respective components of the base metal and the weld metal part calculated using the following formula (1) are all 0.80 or less, and the following formula (2) is satisfied: P value: |P (Cu) ×P (Ni) ×P (W) ×P (Mo) ×P (Sn) ×P (Sb) |…(1) Where: P (Cu) =1-0.0288[].(1-1) P (Ni) =1-0.497 [N]…(1-2) and W: When less than 0.05%, P (W) =1-3.54[W]…(1-3-1) W: 0.05% or more, P (W) =1-0.056[W]-0.174…(1-3-2) Mo: When the content is less than 0.05%, P (Mo) =1-3.03[Mo]…(1-4-1) Mo: 0.05% or more, P (Mo) =1-0.098[Mo]-0.147…(1-4-2) Sn: When less than 0.03%, P (Sn) =1-3.41[Sn]…(1-5-1) Sn: 0.03% or more, P (Sn) =1-1.04[Sn]-0.071…(1-5-2) Sb: When less than 0.05%, P (Sb) =1-2.32[Sb]…(1-6-1) Sb: 0.05% or more, P (Sb) =1-0.0351[Sb]-0-112…(1-6-2) It is. In (1-1), (1-2), (1-3-1), (1-3-2), (1-4-1), (1-4-2), (1-5-1), (1-5-2), (1-6-1), and (1-6-2), [Cu], [Ni], [W], [Mo], [Sn], and [Sb] are the contents (mass%) of each element. P B ≧P W …(2) In addition, in formula (2), P B : P value calculated from the composition of the base material P W : P value calculated from the chemical composition of the weld metal It is.
2. Furthermore, the composition of the base material is, in mass%, V: 0.200% or less, Ti: 0.050% or less, Zr: 0.100% or less, B: 0.0050% or less, Ca: 0.0100% or less, Mg: 0.0100% or less, REM: 0.0100% or less Contains one or more selected from Furthermore, the composition of the weld metal part is, in mass%, V: 0.200% or less, Ti: 0.050% or less, Zr: 0.100% or less, B: 0.0050% or less, Ca: 0.0100% or less, Mg: 0.0100% or less, REM: 0.0100% or less 2. The welded joint having excellent paint durability according to claim 1, characterized in that it contains one or more selected from the following:
3. A welded joint with excellent paint durability as described in claim 1 or 2, characterized in that the base material is structural steel and the welded joint has a paint film.
4. 4. A welded joint having excellent paint durability as described in claim 3, characterized in that the coating film has a corrosion-resistant base layer, a primer layer, an intermediate coat layer and a top coat layer, the corrosion-resistant base layer being made of inorganic zinc-rich paint, the primer layer being made of epoxy resin paint, the intermediate coat layer being made of intermediate paint for a fluororesin top coat paint, and the top coat layer being made of a fluororesin top coat paint.
5. 5. A welded joint having excellent paint durability according to claim 3 or 4, characterized in that the structural steel material surface has a zinc-rich primer layer.
6. A structure comprising the welded joint according to any one of claims 1 to 5.
Citation Information
Patent Citations
Steel material with high weather resistance
JP1994093372A
Steel material extremely enhanced in coating durability
JP1994143489A
Coated steel product excellent in durability
JP1998330881A
Steel excellent in bare weatherability and weldability
JP1999071632A