Spunbond nonwoven fabric for filters, filter media for automobile oil filters and automobile oil filters
A spunbond nonwoven fabric with controlled fiber fusion and specific properties addresses the balance between liquid permeability and rigidity in automobile oil filters, ensuring effective contaminant collection and reduced environmental impact.
Patent Information
- Application Number
- JP2020214123
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-12-23
- Filing Date
- 2020-12-23
- Publication Date
- 2024-09-18
- Estimated Expiration
- 2040-12-23
AI Technical Summary
Conventional spunbond nonwoven fabrics for automobile oil filters face challenges in achieving a balance between liquid permeability and rigidity, leading to issues such as decreased permeability due to strong fiber fusion or shape retention loss at high flow rates.
A spunbond nonwoven fabric composed of thermoplastic continuous filaments with specific properties, including a defined average single fiber diameter, bending resistance, and a controlled ratio of fused and non-fused areas, is developed to enhance both liquid permeability and pleatability.
The fabric achieves excellent liquid permeability and pleatability, maintaining shape retention under high flow rates, and does not require thermosetting resins, thus reducing environmental impact.
Smart Images

Figure 0007552345000005 
Figure 0007552345000003 
Figure 0007552345000004
Abstract
Description
[Technical field]
[0001] The present invention relates to a spunbond nonwoven fabric for filters, which has excellent liquid permeability and pleatability, a filter material for automobile oil filters, and an automobile oil filter. [Background technology]
[0002] Conventionally, engine oil has been used in automobiles to make the engine run efficiently, and this engine oil is circulated inside the engine and used repeatedly. The engine oil that circulates inside the engine contains contaminants such as carbon particles and metal powder that have been generated due to dirt and wear, and these contaminants must be collected before it can be sent back into the engine. In order to collect impurities contained in engine oil, oil filters made of nonwoven fabrics are used. The nonwoven fabrics used in such oil filters are paper-made nonwoven fabrics made by mixing cotton linter pulp, wood pulp, and chemical fibers such as polyester, rayon, and acrylic, and processed with thermosetting resins such as phenolic resins to impart physical strength, or fused-type long-fiber nonwoven fabrics. In particular, spunbond nonwoven fabrics that do not use thermosetting resins such as phenolic resins during production have been attracting attention in recent years from the perspective of environmental load. Nonwoven fabrics for automobile oil filters are known to be used in a pleated shape, and pleating can significantly increase the filtration area, reduce pressure loss, and increase collection efficiency.
[0003] Among the nonwoven fabrics used for such automobile oil filters, spunbond nonwoven fabrics are particularly used as filters to be installed in engine oil because they are superior in lint-free properties and strength performance to short fiber nonwoven fabrics, and it is easy to obtain spunbond nonwoven fabrics that have excellent properties. For example, Patent Documents 1 and 2 disclose nonwoven fabrics used for automobile oil filters, in which thermoplastic continuous filaments are first heated and pressed by a pair of flat rolls and then partially fused by a pair of engraved embossing rolls. Patent Document 3 discloses a nonwoven fabric made by mixing thermoplastic continuous filaments of a high melting point component and thermoplastic continuous filaments of a low melting point component, and a nonwoven fabric made of multi-lobed composite fibers made of a high melting point component and a low melting point component. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Patent No. 5422874 [Patent Document 2] Patent No. 5298803 [Patent Document 3] Patent No. 4522671 Summary of the Invention [Problem to be solved by the invention]
[0005] However, conventional spunbond nonwoven fabrics for oil filters used to remove impurities from automobile engine oil do not have sufficient rigidity for pleating when balancing oil permeability and pleating processability. In other words, if the fusion between fibers is strengthened in an attempt to improve rigidity, the mesh size becomes smaller, leading to a decrease in liquid permeability. On the other hand, if the fusion between fibers is loosened in an attempt to improve liquid permeability, the mesh size becomes larger, and when oil is circulated and filtered at a hydraulic pressure of 300 to 500 kPa, the pleat shape retention decreases, and there is a problem that impurities flow into the oil, which has a negative effect on the engine. For example, with the techniques disclosed in Patent Documents 1 and 2, it was difficult to achieve both sufficient liquid permeability and rigidity. On the other hand, in Patent Document 3, the fusion between the fibers is weak, and the fused parts break during pleating, reducing the rigidity of the nonwoven fabric. When used as a filter, there is an issue that the shape retention of the pleats is reduced at high flow rates.
[0006] In view of the above problems, the object of the present invention is to provide a spunbond nonwoven fabric for filters, a filter material for automobile oil filters, and an automobile oil filter, which have high rigidity and excellent pleat processability while achieving a balance between the performance of capturing contaminants in automobile engine oil and liquid permeability. [Means for solving the problem]
[0007] As a result of extensive investigations to achieve the above object, the inventors have discovered that a spunbonded nonwoven fabric for filters having excellent liquid permeability and sufficient rigidity for pleating and shape retention can be obtained by using a nonwoven fabric made of partially fused thermoplastic continuous filaments, in which the average brightness of fused parts and non-fused parts obtained from a cross section of the nonwoven fabric is within a specified range. The present invention has been completed based on these findings, and provides the following inventions.
[0008] That is, the spunbond nonwoven fabric for filters of the present invention is a spunbond nonwoven fabric for filters composed of thermoplastic continuous filaments consisting of a high melting point component and a low melting point component, which are partially fused, wherein the average single fiber diameter of the thermoplastic continuous filaments is 8.0 μm or more and 15.0 μm or less, the bending resistance in the MD direction is 20 mN or more and 80 mN or less, and the ratio of the average reflected light luminance (S1) of the fused parts to the average reflected light luminance (S2) of the non-fused parts in the cross section, represented by the following formula (1), is 0.20 or more and 1.00 or less. R = 1 − S2 / S1 (1)
[0009] According to a preferred embodiment of the spunbonded nonwoven fabric for filters of the present invention, the basis weight CV value is 5.0% or less. According to a preferred embodiment of the spunbonded nonwoven fabric for filters of the present invention, the area ratio of the fused portions is 5% or more and 20% or less. The spunbond nonwoven fabric for filters of the present invention is a spunbond nonwoven fabric for automobile oil filters. The spunbond nonwoven fabric for automobile oil filters of the present invention is used as a filter material for automobile oil filters. The filter material for automobile oil filters of the present invention is used in automobile oil filters. Effect of the Invention
[0010] According to the present invention, a spunbond nonwoven fabric for filters, a filter material for automobile oil filters, and an automobile oil filter, which are excellent in liquid permeability and pleat processability, can be obtained. [Brief description of the drawings]
[0011] [Figure 1] FIG. 1 is a schematic perspective view illustrating an example of a filter medium of the present invention. [Diagram 2] FIG. 2 is a cross-sectional photograph illustrating the structure of the spunbonded nonwoven fabric for filters according to the present invention. [Diagram 3] FIG. 3 is a diagram for explaining the configuration of a test system for carrying out a collection performance test according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] The spunbond nonwoven fabric for filters of the present invention is a spunbond nonwoven fabric for filters composed of thermoplastic continuous filaments consisting of a high melting point component and a low melting point component and partially fused, wherein the average single fiber diameter of the thermoplastic continuous filaments is 8.0 μm or more and 15.0 μm or less, the bending resistance in the MD direction is 20 mN or more and 80 mN or less, and the ratio of the average reflected light luminance (S1) of the fused parts to the average reflected light luminance (S2) of the non-fused parts in the cross section, represented by the following formula (1), is 0.20 or more and less than 1.00. R = 1 − S2 / S1 (1) Hereinafter, each component of the spunbonded nonwoven fabric for filters of the present invention will be described in detail.
[0013] (Thermoplastic continuous filament) As the thermoplastic resin that is the raw material of the thermoplastic continuous filaments that constitute the spunbonded nonwoven fabric for filters of the present invention, polyester is particularly preferably used. Polyester is a polymer having an acid component and an alcohol component as monomers. As the acid component, aromatic carboxylic acids such as phthalic acid (ortho form), isophthalic acid, and terephthalic acid, aliphatic dicarboxylic acids such as adipic acid and sebacic acid, and alicyclic dicarboxylic acids such as cyclohexane carboxylic acid can be used. As the alcohol component, ethylene glycol, diethylene glycol, polyethylene glycol, and the like can be used.
[0014] Examples of polyesters include polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polytrimethylene terephthalate (PTT), polyethylene naphthalate, polylactic acid, polybutylene succinate, etc. As the polyester used as the high melting point polymer described later, PET is most preferably used because it has a high melting point, excellent heat resistance, and excellent rigidity.
[0015] Additives such as crystal nucleating agents, matting agents, pigments, mildewproofing agents, antibacterial agents, flame retardants, metal oxides, aliphatic bisamides and / or aliphatic monoamides, and hydrophilic agents can be added to these polyester raw materials within the scope of the present invention. Among them, metal oxides such as titanium oxide have the effect of improving spinnability by reducing surface friction of fibers and preventing fusion between fibers, and also of improving the fusion property of nonwoven fabrics by increasing thermal conductivity during fusion molding of nonwoven fabrics with heated rolls. In addition, aliphatic bisamides such as ethylene bisstearic acid amide and / or alkyl-substituted aliphatic monoamides have the effect of increasing the releasability between the heated roll and the nonwoven fabric web, improving transportability.
[0016] The thermoplastic continuous filament used in the present invention is composed of a high melting point component and a low melting point component. The thermoplastic continuous filament is preferably a composite filament in which a polyester-based low melting point polymer, which is a low melting point component having a melting point 10°C to 140°C lower than the melting point of the polyester-based high melting point polymer, is arranged around the polyester-based high melting point polymer, which is a high melting point component. In this way, when a spunbonded nonwoven fabric is formed by fusion, the composite polyester fibers (filaments) constituting the spunbonded nonwoven fabric are firmly fused to each other, so that the spunbonded nonwoven fabric for filters has excellent mechanical strength and can fully withstand oil treatment under high flow rates.
[0017] The melting point of the polyester-based low melting point polymer in the present invention can be made 10° C. or more, more preferably 20° C. or more, and even more preferably 30° C. or more lower than the melting point of the polyester-based high melting point polymer to ensure the desired fusion properties. On the other hand, the melting point of the polyester-based low melting point polymer can be made 140° C. or less, more preferably 120° C. or less, and even more preferably 100° C. or less lower than the melting point of the polyester-based high melting point polymer to prevent a decrease in heat resistance.
[0018] The melting point of the polyester-based high melting point polymer in the present invention is preferably in the range of 200° C. or more and 320° C. or less. By setting the melting point of the polyester-based high melting point polymer to preferably 200° C. or more, more preferably 210° C. or more, and even more preferably 220° C. or more, a filter having excellent heat resistance can be obtained. On the other hand, by setting the melting point of the polyester-based high melting point polymer to preferably 320° C. or less, more preferably 300° C. or less, and even more preferably 280° C. or less, a large consumption of thermal energy for melting during the production of the nonwoven fabric and a decrease in productivity can be suppressed.
[0019] On the other hand, the melting point of the polyester-based low melting point polymer is preferably in the range of 160° C. or more and 250° C. or less. By setting the melting point of the polyester-based low melting point polymer to preferably 160° C. or more, more preferably 170° C. or more, and even more preferably 180° C. or more, the shape retention is excellent even if the pleated filter is passed through a process in which heat is applied during production, such as heat setting during pleating. On the other hand, by setting the melting point of the polyester-based low melting point polymer to preferably 250° C. or less, more preferably 240° C. or less, a filter having excellent fusion properties during nonwoven fabric production and excellent mechanical strength can be obtained.
[0020] In the present invention, the melting point of a thermoplastic resin is measured using a differential scanning calorimeter (e.g., PerkinElmer's "DSC-2" model) at a heating rate of 20° C. / min and a measurement temperature range of 30° C. to 300° C., and the temperature at which the obtained melting endothermic curve gives an extreme value is defined as the melting point of the thermoplastic resin. For resins whose melting endothermic curve does not show an extreme value in the differential scanning calorimeter, the resin is heated on a hot plate, and the temperature at which the resin melts under a microscope is defined as the melting point.
[0021] When the thermoplastic resin is polyester, examples of the combination of a polyester-based high melting point polymer and a polyester-based low melting point polymer (hereinafter, the combinations may be described in the order of polyester-based high melting point polymer / polyester-based low melting point polymer) include PET / PBT, PET / PTT, PET / polylactic acid, and PET / copolymerized PET, among which the combination of PET / copolymerized PET is preferably used because of its excellent spinnability. As the copolymerization component of the copolymerized PET, isophthalic acid copolymerized PET is preferably used because of its excellent spinnability.
[0022] The composite filament may have a composite form, for example, a concentric sheath-core type, an eccentric sheath-core type, or an island-in-the-sea type, among which the concentric sheath-core type is preferred because it can fuse the filaments uniformly and firmly. The cross-sectional shape of the composite filament may be a circular cross-section, a flat cross-section, a polygonal cross-section, a multi-lobal cross-section, a hollow cross-section, or the like. Among these, a preferred embodiment is one in which the filament has a circular cross-sectional shape.
[0023] Incidentally, the form of the composite filament may be, for example, a method of blending fibers made of a polyester-based high melting point polymer with fibers made of a polyester-based low melting point polymer, but in the case of blending, uniform fusion is difficult, and for example, fusion is weak in areas where the fibers made of the polyester-based high melting point polymer are densely packed, resulting in poor mechanical strength and rigidity, making the fabric unsuitable for a spunbonded nonwoven fabric for filters. On the other hand, there is also a method of applying a low melting point polymer to fibers made of a polyester-based high melting point polymer by immersion or spraying, but in either case, it is difficult to apply the low melting point polymer uniformly on the surface layer or in the thickness direction, and the mechanical strength and rigidity are poor, making the fabric unsuitable for a spunbonded nonwoven fabric for filters.
[0024] The content ratio of the polyester-based high melting point polymer and the polyester-based low melting point polymer in the thermoplastic continuous filaments is preferably in the range of 90:10 to 60:40 by mass ratio, and more preferably in the range of 85:15 to 70:30. By making the polyester-based high melting point polymer 60% by mass or more and 90% by mass or less, the rigidity and heat resistance of the spunbonded nonwoven fabric for filters can be excellent. On the other hand, by making the polyester-based low melting point polymer 10% by mass or more and 40% by mass or less, when the spunbonded nonwoven fabric for automobile oil filters is formed and used by fusion, the composite filaments constituting the spunbonded nonwoven fabric for filters can be firmly fused to each other, the mechanical strength is excellent, and the fabric can sufficiently withstand oil treatment under high flow rate.
[0025] The average single fiber diameter of the thermoplastic continuous filaments constituting the spunbonded nonwoven fabric for filters of the present invention is in the range of 8.0 μm or more and 15.0 μm or less. By making the average single fiber diameter of the thermoplastic continuous filaments 8.0 μm or more, preferably 8.2 μm or more, more preferably 8.5 μm or more, the liquid permeability of the spunbonded nonwoven fabric for filters can be improved and the pressure loss can be reduced. In addition, the number of thread breaks during the formation of the thermoplastic continuous filaments can be reduced, and the stability during production can be improved. On the other hand, by making the single fiber diameter of the thermoplastic continuous filaments 15.0 μm or less, more preferably 14.8 μm or less, the uniformity of the spunbonded nonwoven fabric for filters can be improved, the surface of the nonwoven fabric can be made dense, and the collection performance can be improved, such as making it easier to filter engine oil at the surface layer.
[0026] In the present invention, the average single fiber diameter (μm) of the spunbonded nonwoven fabric for filters is determined by the following method. (i) Ten small sample pieces are randomly taken from the spunbond nonwoven fabric for filters. (ii) The surface of the collected small sample is photographed using a scanning electron microscope or the like at a magnification range of 500 to 2000 times so that the fiber thickness can be measured. (iii) From the photographs taken from each small sample, 10 fibers are randomly selected (100 fibers in total) and their diameters are measured. The fibers are assumed to have a circular cross section, and the diameter is taken as the single fiber diameter. (iv) The average single fiber diameter is calculated by rounding off the arithmetic mean value to one decimal place.
[0027] (Manufacturing method of spunbond nonwoven fabric for filters) Next, a method for producing the spunbonded nonwoven fabric for filters of the present invention will be described. The spunbonded nonwoven fabric for filters of the present invention is produced by sequentially carrying out the following steps (a) to (c). (a) A process in which a thermoplastic polymer is molten and extruded from a spinneret, and then pulled and drawn by an air sucker to obtain a thermoplastic continuous filament. (b) A process in which the obtained filaments are deposited on a moving net conveyor while regulating the fiber arrangement with a fiber-spreading plate to form a fiber web. (c) subjecting the resulting fibrous web to partial fusion bonding. Each of the above steps will now be described in more detail.
[0028] (a) Thermoplastic continuous filament forming process First, a thermoplastic polymer is melt-extruded from a spinneret. In particular, when a composite filament in which a polyester-based low-melting point polymer having a melting point lower than that of a polyester-based high-melting point polymer is used as a thermoplastic continuous filament, the polyester-based high-melting point polymer and the polyester-based low-melting point polymer are melted at a temperature higher than the melting point and lower than (melting point + 70°C), respectively, and a composite filament in which a polyester-based low-melting point polymer having a melting point lower than that of the polyester-based high-melting point polymer is arranged around the polyester-based high-melting point polymer by 10°C to 140°C is spun out of a fine hole with a spinneret temperature higher than the melting point and lower than (melting point + 70°C), and then pulled and stretched by an air sucker at a spinning speed of 4000m / min to 6000m / min to spin a filament having a circular cross-sectional shape.
[0029] (b) Fiber web forming process The spunbond nonwoven fabric for filters of the present invention comprises a process in which spun thermoplastic continuous filaments are sucked by an ejector, ejected from a fiber-spreading plate having a slit at the bottom of the ejector, and deposited on a moving net conveyor to obtain a fiber web. Even when composite polyester fibers are used, it is important that the spunbonded nonwoven fabric for filters is made of the filaments (long fibers). This makes it possible to increase the rigidity and mechanical strength compared to nonwoven fabrics made of short fibers composed of discontinuous fibers, and makes it preferable as a pleated filter. In the manufacturing method of the spunbonded nonwoven fabric for filters of the present invention, it is also a preferred embodiment to temporarily fuse the fiber web collected on the net conveyer. For the temporary fusion, a method is preferably used in which the collected fiber web is fused with a pair of flat rolls, or a flat roll is placed on the net conveyer and fused between the net conveyer and the flat roll.
[0030] The fusion temperature for temporary fusion is preferably 70° C. to 120° C. lower than the melting point of the polyester-based low melting point polymer. By setting the temperature in this manner, the fibers are not excessively fused to each other, and the conveyability can be improved. In addition, the line pressure for temporary fusion is preferably 30 kg / cm or more and 70 kg / cm or less. By setting the line pressure for temporary fusion to 30 kg / cm or more, more preferably 40 kg / cm or more, it is possible to impart the mechanical strength required for transporting the fiber web to the next process. By setting the line pressure for temporary fusion to 70 kg / cm or less, more preferably 65 kg / cm or less, it is possible to prevent excessive fusion between the fibers.
[0031] (c) Partial fusion process The spunbonded nonwoven fabric for filters of the present invention is partially fused, but the method of partially fusion is not particularly limited. Here, the fused portion of the spunbonded nonwoven fabric for filters is called the fused portion, and the other unfused portion is called the nonfused portion. Fusion by a hot embossing roll or a combination of an ultrasonic oscillator and an embossing roll is preferred. In particular, fusion by an embossing roll is most preferred from the viewpoint of improving the strength of the nonwoven fabric. The partial fusion step is preferably processed continuously from the web forming step. By processing continuously from the web forming step, the density of the fused portion is increased, and a nonwoven fabric with excellent waist strength and excellent pleat processability can be obtained as a spunbonded nonwoven fabric for filters. The temperature of fusion by a hot embossing roll is preferably 5°C to 60°C lower than the melting point of the polymer with the lowest melting point present on the fiber surface of the nonwoven fabric, and more preferably 10°C to 50°C lower. Excessive fusion can be prevented by setting the temperature difference between the melting points of the polymers with the lowest melting points present on the fiber surfaces of the nonwoven fabric by the hot embossing roll to 5° C. or more, more preferably 10° C. or more. On the other hand, uniform fusion can be achieved within the nonwoven fabric by setting the temperature difference to 60° C. or less, more preferably 50° C. or less. The line pressure for fusion is preferably 30 kg / cm or more and 90 kg / cm or less. By setting the line pressure for fusion to 30 kg / cm or more, more preferably 40 kg / cm or more, the strength required for pleating can be imparted to the nonwoven fabric when used as a spunbonded nonwoven fabric for filters. By setting the line pressure for fusion to 90 kg / cm or less, more preferably 80 kg / cm or less, excessive fusion can be prevented.
[0032] The proportion of the fused area of the partial fusion of the spunbonded nonwoven fabric for filters of the present invention (hereinafter, sometimes simply referred to as the fused area ratio) is the proportion of the fused part to the total area of the nonwoven fabric, and is preferably in the range of 5% to 20% of the total area of the nonwoven fabric. If the fused area ratio is 5% or more, more preferably 6% or more, and even more preferably 8% or more, the nonwoven fabric has sufficient mechanical strength and is not prone to fluffing on the surface. On the other hand, if the fused area ratio is 20% or less, more preferably 19% or less, and even more preferably 18% or less, the gaps between the fibers are reduced, the pressure loss increases, and the collection performance does not decrease. The fusion area ratio of the spunbonded nonwoven fabric is measured using a digital microscope (for example, "VHX-5000" manufactured by Keyence Corporation) and 100 rectangular frames of 1.0 cm x 1.0 cm parallel to the MD and CD directions of the nonwoven fabric are taken from any part of the spunbonded nonwoven fabric at a magnification of 20 times using the microscope. The area of the fusion part within the rectangular frame is measured for each of the 100 points and the average value is calculated as a percentage and rounded off to the first decimal place to obtain the fusion area ratio (%). When not expressed as a percentage, the area (cm2) of the fusion part within the rectangular frame is used. 2 ) to the area of the rectangular frame, 1.0 cm 2 Then, the fused area ratio can be calculated by rounding off to two decimal places.
[0033] In the present invention, the MD direction refers to the sheet conveying direction during the production of the spunbond nonwoven fabric for filters, i.e., the winding direction of the nonwoven fabric roll, and the CD direction refers to the direction perpendicular to the sheet conveying direction, i.e., the winding direction of the nonwoven fabric roll. When the spunbond nonwoven fabric for filters is not in a rolled state due to being cut, for example, the MD direction and CD direction are determined by the following procedure. (a) Within the plane of the spunbond nonwoven fabric for filters, select one arbitrary direction and take a test piece 38.1 mm long and 25.4 mm wide along that direction. (b) Similarly, test pieces measuring 38.1 mm in length and 25.4 mm in width are taken at angles rotated 30 degrees, 60 degrees, and 90 degrees from the direction in which the test piece was taken. (c) For each test piece in each direction, the bending resistance of each test piece is measured based on the method for measuring the bending resistance of spunbond nonwoven fabric for filters described below. (d) The direction in which the measured value is highest is defined as the MD direction of the spunbond nonwoven fabric for filters, and the direction perpendicular to this is defined as the CD direction. In addition, when determining the MD and CD directions from a filter material for a filter, in the case of a filter material for an automobile oil filter as illustrated in Figure 1, the direction 25 parallel to the ridge line of the peak portion 22 is the CD direction, and the direction 24 perpendicular to the CD direction is the MD direction. In the present invention, the MD direction refers to the sheet conveying direction during the production of the spunbonded nonwoven fabric, i.e., the winding direction of the nonwoven fabric roll, and the CD direction refers to the direction perpendicular to the sheet conveying direction, i.e., the winding direction of the nonwoven fabric roll. When the spunbonded nonwoven fabric is not in a rolled state, for example, because it is cut, the MD direction and CD direction are determined by the following procedure. (a) Within the plane of the spunbond nonwoven fabric, select one arbitrary direction and take a test piece 38.1 mm long and 25.4 mm wide along that direction. (b) Similarly, test pieces measuring 38.1 mm in length and 25.4 mm in width are taken at angles rotated 30 degrees, 60 degrees, and 90 degrees from the direction in which the test piece was taken. (c) For each test piece in each direction, the bending resistance of each test piece is measured based on the method for measuring the bending resistance of spunbond nonwoven fabric described below. (d) The direction in which the measured value is highest is the MD direction of the spunbond nonwoven fabric, and the direction perpendicular to this is the CD direction. In addition, when determining the MD and CD directions from a filter material for an automobile oil filter, in the case of a filter material for a dust collector pleated filter as illustrated in Figure 1, the direction 25 parallel to the ridge line of the peak portion 22 is the CD direction, and the direction 24 perpendicular to the CD direction is the MD direction.
[0034] The fused portion forms a depression, and is formed by fusing the thermoplastic continuous filaments constituting the nonwoven fabric together by heat and pressure. That is, the fused portion is the portion where the thermoplastic continuous filaments are fused and aggregated compared to other portions. When fusing by a thermal embossing roll is adopted as the fusing method, the portion where the thermoplastic continuous filaments are fused and aggregated by the convex portion of the embossing roll becomes the fused portion. For example, when a roll having a predetermined pattern of unevenness only on the upper or lower side is used, and the other roll is a flat roll without unevenness, the fused portion refers to the portion where the thermoplastic continuous filaments of the nonwoven fabric are fused by the convex portion of the roll having unevenness and the flat roll and aggregated. In addition, for example, when an embossing roll is used, which is composed of a pair of upper and lower rolls having a plurality of linear grooves arranged in parallel on the surface, and is arranged so that the grooves of the upper roll and the grooves of the lower roll cross at a certain angle, the fused portion refers to the portion where the thermoplastic continuous filaments of the nonwoven fabric are fused by the convex portion of the upper roll and the convex portion of the lower roll and aggregated. In this case, the portion fused between the upper convex portion and the lower concave portion or between the upper concave portion and the lower convex portion is not included in the fused portion referred to here.
[0035] The area of each fused part is 0.3 mm 2 More than 5.0mm 2 Less than 0.3mm is preferred. 2 By setting the thickness to 5.0 mm or more, sufficient mechanical strength can be obtained as a spunbond nonwoven fabric for filters, and fuzzing on the surface of the nonwoven fabric can be suppressed. 2 By satisfying the following conditions, the mechanical strength and breathability required for a spunbonded nonwoven fabric for automobile oil filters can be maintained, and sufficient collection performance can be obtained.
[0036] The shape of the fused portion is not particularly specified, and even when a roll having a predetermined pattern of unevenness only on the upper or lower side is used and the other roll is a flat roll without unevenness, or when an embossing roll is composed of a pair of upper and lower rolls having a plurality of parallel linear grooves formed on the surface, and the grooves of the upper roll and the grooves of the lower roll are arranged so as to intersect at a certain angle, and the convex portions of the upper roll and the convex portions of the lower roll are fused, the shape of the fused portion may be a circle, a triangle, a rectangle, a parallelogram, an ellipse, a rhombus, or the like. The arrangement of these fused portions is not particularly specified, and they may be arranged regularly at equal intervals, randomly, or a mixture of different shapes. Among them, it is preferable that the fused portions are arranged at equal intervals from the viewpoint of uniformity of the nonwoven fabric. Furthermore, in terms of achieving partial fusion without peeling off the nonwoven fabric, it is preferable to use an embossing roll consisting of a pair of upper and lower rolls having a plurality of parallel linear grooves formed on the surface thereof, in which the grooves of the upper roll and the grooves of the lower roll are arranged so as to intersect at a certain angle, and to form a parallelogram-shaped fused portion formed by fusion between the convex portions of the upper roll and the convex portions of the lower roll.
[0037] (Spunbond nonwoven fabric for filters) The spunbond nonwoven fabric for filters of the present invention has a bending resistance in the MD direction of the nonwoven fabric of 20 mN or more and 80 mN or less. If the bending resistance is 20 mN or more, more preferably 25 mN or more, and even more preferably 30 mN or more, the nonwoven fabric can be pleated while maintaining its strength and shape retention. On the other hand, if the bending resistance is 80 mN or less, more preferably 75 mN or less, and even more preferably 70 mN or less, the folding resistance during pleating is reduced, and the pleats have a sharp peak-valley shape.
[0038] The bending resistance in the present invention is a value obtained as follows in accordance with JIS L1913:2010 "General nonwoven fabric testing methods" 6.7 "Bending resistance (JIS method and ISO method)" 6.7.4 "Gurley method (JIS method)". (i) Test pieces with a length of 38.1 mm (effective sample length L = 25.4 mm) and a width of d = 25.4 mm are taken from any five points on the sample. In the present invention, the longitudinal direction of the nonwoven fabric is defined as the MD direction of the sample. (ii) Attach each of the collected test pieces to a chuck and fix the chuck so that it is aligned with the 1-1 / 2" (1.5 inches = 38.1 mm) scale on the movable arm A. In this case, 1 / 2" (0.5 inches = 12.7 mm) of the sample length is applied to the chuck by 1 / 4" (0.25 inches = 6.35 mm), and 1 / 4" (0.25 inches = 6.35 mm) is applied to the tip of the pendulum at the free end of the sample, so the effective sample length L for measurement is the test piece length minus 1 / 2" (0.5 inches = 12.7 mm). (iii) Next, insert a suitable weight W into the lower weight mounting holes a, b, and c (mm) from the fulcrum of the pendulum B. a , W b , W c (g) is attached to the movable arm A, and the movable arm A is rotated at a constant speed, and the scale RG (mgf) is read when the test piece separates from the pendulum B. The scale is read to the first decimal place. The weight to be attached to the weight attachment hole can be selected appropriately, but it is preferable to set the scale RG to 4 to 6. (iv) Measurements are performed on five test pieces, five times on each side, for a total of 50 times. (v) The bending resistance value was calculated from the obtained RG scale value using the following formula, rounded off to one decimal place. The average value of 50 measurements was rounded off to one decimal place to calculate the bending resistance in the MD direction.
number
[0039] In the spunbonded nonwoven fabric for filters of the present invention, the ratio of the average reflected light brightness (S1) of the fused portion to the average reflected light brightness (S2) of the nonfused portion in the cross section represented by the following formula (1) is 0.20 or more and less than 1.00. FIG. 2 is a cross-sectional photograph for explaining the structure of the spunbonded nonwoven fabric for filters according to the present invention. As shown in FIG. 2, when the cross section of the spunbonded nonwoven fabric for oil filters according to the present invention is observed with a scanning electron microscope (SEM), the fused portion where the thermoplastic continuous filaments are fused has a high brightness due to the dense presence of thermoplastic continuous filaments, and the nonfused portion has a low brightness due to the sparse presence of thermoplastic continuous filaments. The present inventors have found that when the ratio of the average reflected light brightness (S1) of the fused portion to the average reflected light brightness (S2) of the nonfused portion in the cross section represented by the formula (1) is within a predetermined range, a spunbonded nonwoven fabric for filters having a good balance between dust collection performance and breathability, excellent pleatability, and high rigidity can be obtained. When the value of formula (1) is 0.20 or more, more preferably 0.25 or more, and even more preferably 0.30 or more, the fusion between the fibers is loose and excellent liquid permeability is obtained. On the other hand, when the value of formula (1) is less than 1.00, more preferably 0.90 or less, and even more preferably 0.80 or less, the fusion between the fibers is strong and excellent shape retention is obtained even under high flow rates when used as a filter. R = 1 − S2 / S1 (1) In the present invention, the average reflected light luminance (S1) of the fused portion, the average reflected light luminance (S2) of the non-fused portion, and the value of formula (1) are determined as follows.
[0040] (1) Average reflected light brightness of the fused part (S1) (i) In any fused portion, the intersection of the center line in the MD direction and the center line in the CD direction is defined as the center point of the fused portion. (ii) Draw a straight line parallel to the CD direction through the center point of the fused portion. (iii) Starting from two points on the line 0.5 cm apart from the center point of the fused portion, a line is drawn 1.0 cm long in the MD direction, and a straight line is drawn connecting the end points of the line. (iv) Cut out the area enclosed by the 1.0 cm x 1.0 cm squares formed in (i) through (iii) with a razor blade. (v) In the same manner, a total of 100 measurement samples of 1.0 cm x 1.0 cm fused portions are taken from any positions on the spunbond nonwoven fabric for filters. (vi) Using a scanning electron microscope (SEM) (for example, "VHX-D500" manufactured by Keyence Corporation), the cross section of the fused portion in the measurement sample for the fused portion is observed by adjusting the magnification to 150 times. (vii) Visually draw a line perpendicular to the cross section of the nonwoven fabric sheet at the thinnest point of the fused portion of each observed image, and take a photograph of the center position at 500x magnification, one for each fused portion measurement sample, for a total of 100 photographs, and save the photographs in JPG format. (viii) Cut out an image of 1000 x 1000 pixels from the saved image. (ix) Divide into grid units of 40x40 pixels. (x) For each grid, the average reflected light luminance (average reflected light luminance S1) defined in the YUV color space is calculated for each pixel using the following formula: (Reflected light brightness of each pixel) = 0.29891 x R + 0.58661 x G + 0.11448 x B Here, R, G, and B represent the reflected light intensity of red, green, and blue, respectively, in the RGB color model.
[0041] (2) Average reflected light brightness of unfused parts (S2) (i) The midpoint between the center point of any fused portion and the center point of the closest fused portion among the adjacent fused portions is defined as the center point of the non-fused portion. (ii) Draw a straight line parallel to the CD direction through the center point of the non-fused portion. (iii) Starting from two points on the line 0.5 cm apart from the center point of the non-fused portion, a line is drawn 1.0 cm long in the MD direction, and a straight line is drawn connecting the end points of the line. (iv) Cut out the area enclosed by the 1.0 cm x 1.0 cm squares formed in (i) through (iii) with a razor blade. (v) Similarly, a total of 100 measurement samples of 1.0 cm x 1.0 cm for the non-fused portions are taken from any location within the spunbond nonwoven fabric for filters. (vi) Using a scanning electron microscope (SEM) (for example, "VHX-D500" manufactured by Keyence Corporation), the cross section of the non-fused portion in the sample for non-fused portion is observed by adjusting the magnification to 150 times. (vii) Visually draw a line perpendicular to the cross section of the nonwoven fabric sheet at the thickest point of the non-fused portion of each observed image, and take a photograph of the center position at 500x magnification, one for each measurement sample for the non-fused portion, for a total of 100 photographs, and save the photographs in JPG format. (viii) Cut out an image of 1000 x 1000 pixels from the saved image. (ix) Divide into grid units of 40x40 pixels. (x) For each grid, the average reflected light luminance (average reflected light luminance S2) defined in the YUV color space is calculated for each pixel using the following formula: (Reflected light brightness of each pixel) = 0.29891 x R + 0.58661 x G + 0.11448 x B Here, R, G, and B represent the reflected light intensity of red, green, and blue, respectively, in the RGB color model.
[0042] (3) Average luminance ratio The average reflected light luminance (S2) obtained in the above "average reflected light luminance (S2) of non-fused portions" was divided by the average reflected light luminance (S1) obtained in the "average reflected light luminance (S1) of the cross section of the fused portions" to obtain the value (S2 / S1). The calculated value (R) was used as the average luminance ratio. R = 1 - (S2 / S1) (1)
[0043] The basis weight of the spunbond nonwoven fabric for filters in the present invention is 150 g / m 2 More than 300g / m 2 The following range is preferable: Weight per unit area is 150 g / m 2 If the weight is more than 300 g / m, the necessary rigidity for the pleats can be obtained, which is preferable. 2 Less than 270 g / m 2Less than 260 g / m 2 If it is equal to or less than this, an increase in pressure loss can be suppressed, and it is also preferable in terms of cost. The basis weight here is calculated by taking three samples of 50cm length x 50cm width, measuring the mass of each, and calculating the average value (g) of the obtained values per unit area (1m 2 ) and round off to the first decimal place.
[0044] The CV value of the spunbonded nonwoven fabric for filters of the present invention is preferably 5.0% or less. More preferably, it is 4.8% or less, and even more preferably, it is 4.5% or less, because the nonwoven fabric can be made dense with improved uniformity of the nonwoven fabric, which makes it easier to improve the collection efficiency and to obtain a satisfactory filter life. On the other hand, the CV value of the spunbonded nonwoven fabric for automobile oil filters is more preferably 1.0% or more, because the amount of liquid permeation of the spunbonded nonwoven fabric for automobile oil filters is ensured to be constant and the pressure loss is reduced, thereby extending the filter life.
[0045] In the present invention, the basis weight CV value (%) of the spunbonded nonwoven fabric for filters is determined as follows. (i) A total of 100 small pieces measuring 5 cm x 5 cm are taken from a spunbond nonwoven fabric for automobile oil filters. (ii) Measure the mass (g) of each piece and calculate the unit area (1 m 2 ) per unit. (iii) The average of the conversion results of (ii) (W ave ), standard deviation (W sdv ) are calculated respectively. (iv) Based on the results of (i) to (iii), calculate the basis weight CV value (%) using the following formula, and round off to one decimal place. Weight CV value (%) = W sdv / W ave ×100
[0046] The thickness of the spunbonded nonwoven fabric for filters in the present invention is preferably 0.50 mm or more and 0.80 mm or less, more preferably 0.51 mm or more and 0.78 mm or less. By making the thickness 0.50 mm or more, the rigidity can be improved, and the spunbonded nonwoven fabric for filters suitable for use as a filter can be obtained. In addition, by making the thickness 0.80 mm or less, the spunbonded nonwoven fabric for filters excellent in handleability and processability as a filter can be obtained.
[0047] In the present invention, the thickness (mm) of the spunbond nonwoven fabric for filters is determined by the following method. (i) Using a thickness meter (for example, "TECLOCK" (registered trademark) SM-114 manufactured by Teclock Corporation), the thickness of the nonwoven fabric is measured at 10 equally spaced points in the CD direction. (ii) The thickness of the nonwoven fabric (mm) is determined by rounding off the above arithmetic average value to two decimal places.
[0048] The apparent density of the spunbond nonwoven fabric for filters in the present invention is 0.25 g / cm 3 More than 0.40g / cm 3 It is preferable that the apparent density is 0.25 g / cm or less. 3 More than 0.40g / cm 3 If the apparent density is less than 0.26 g / cm, the spunbond nonwoven fabric for filters has a dense structure, which makes it difficult for dust to get inside, and the dust can be easily removed. A more preferable apparent density range is 0.26 g / cm. 3 More than 0.38g / cm 3 The range is as follows: In the present invention, the apparent density (g / cm 3 ) is the value calculated from the basis weight and thickness of the spunbond nonwoven fabric for filters using the following formula. Apparent density (g / cm 3 )=Weight (g / m 2 ) / Thickness(mm) / 1000
[0049] The spunbonded nonwoven fabric for filters of the present invention has excellent liquid permeability and pleatability, and can be suitably used as a filter for filtering impurities in oil circulating at a hydraulic pressure of 300 to 500 kPa. Such a filter material can be obtained, for example, by pleating the spunbonded nonwoven fabric for filters. Furthermore, this filter material for automobile oil filters can be a cylindrical automobile oil filter in which the entire filter material is made cylindrical around the axis of the element, and then the upper and lower ends of the cylinder are fixed.
[0050] The automobile oil filter of the present invention uses the filter material for automobile oil filters, and the automobile oil filter has a structure in which a filter element is housed in a pressure-resistant container made of metal or resin, for example. Engine oil filtration methods include, for example, a full-flow type that mainly filters metal powder generated by friction, a bypass type that removes carbon particles generated by incomplete combustion, and a combination type that combines both types, and the automobile oil filter of the present invention is particularly suitable for the combination type automobile oil filter that is widely used in recent automobiles.
[0051] As described above, the spunbond nonwoven fabric for filters of the present invention achieves a balance between the performance of capturing contaminants in automobile engine oil and liquid permeability, has high rigidity, is excellent in pleating processability, and can be used as an automobile oil filter by itself without using thermosetting resins such as phenolic resins, and therefore can be suitably used as an automobile oil filter with low environmental impact. EXAMPLES
[0052] Next, the spunbonded nonwoven fabric for filters of the present invention will be specifically described based on examples, although the present invention is not limited to these examples.
[0053] [Measurement method] The respective characteristic values in the following examples were measured by the following methods. In addition, in the measurement of each physical property, unless otherwise specified, the measurement was carried out based on the above-mentioned method. (1) Melting point of polyester (℃) The differential scanning calorimeter used was a "DSC-2" model manufactured by PerkinElmer Japan Co., Ltd. (2) Intrinsic viscosity of polyester (IV) The intrinsic viscosity (IV) of the polyester was measured by the following method. Dissolve 8 g of sample in 100 mL of orthochlorophenol, and measure the relative viscosity η using an Ostwald viscometer at 25°C. r was calculated by the following formula. η r =η / η0=(t×d) / (t0×d0) (Here, η is the viscosity of the polymer solution, η0 is the viscosity of orthochlorophenol, t is the drop time of the solution (sec), and d is the density of the solution (g / cm 3 ), t0 is the fall time of orthochlorophenol (sec), and d0 is the density of orthochlorophenol (g / cm 3 ) and Next, the relative viscosity η r The intrinsic viscosity (IV) was calculated from the following formula. Intrinsic viscosity (IV)=0.0242η r +0.2634.
[0054] (3) Average single fiber diameter of thermoplastic continuous filaments (μm) The average single fiber diameter of the thermoplastic continuous filaments was calculated by the above-mentioned method using a scanning electron microscope (SEM) "VHX-D500" manufactured by Keyence Corporation. (4) Basis weight of spunbond nonwoven fabric for filters (g / m 2 ) The basis weight of the spunbond nonwoven fabric for filters was calculated by the above-mentioned method. (5) CV value (%) of spunbond nonwoven fabric for filters The CV value of the basis weight of the spunbond nonwoven fabric for filters was calculated by the above-mentioned method. (6) Thickness of spunbond nonwoven fabric for filters (mm) The thickness was evaluated by the above-mentioned method using a "TECLOCK" (registered trademark) SM-114 manufactured by TECLOCK Corporation as a thickness gauge. (7) Bending resistance of spunbond nonwoven fabric for filters (mN) The bending resistance was measured by the above-mentioned method using a Gurley flexibility tester "GAS-10" manufactured by Daiei Seiki Seisakusho Co., Ltd.
[0055] (8) Average reflected light brightness (S1) of the fused portion of the spunbond nonwoven fabric for filters A scanning electron microscope (SEM) "VHX-D500" manufactured by Keyence Corporation was used, and the average reflected light luminance (S1) of the fused portion of the spunbond nonwoven fabric for filters was calculated by the above-mentioned method. (9) Average reflected light brightness (S2) of the unfused portion of spunbond nonwoven fabric for filters A scanning electron microscope (SEM) "VHX-D500" manufactured by Keyence Corporation was used, and the average luminance (S2) of reflected light of the non-fused portion of the spunbond nonwoven fabric for filters was calculated by the above-mentioned method. (10) Average luminance ratio (R) The average brightness ratio (R) of the spunbond nonwoven fabric for filters is calculated by dividing the average reflected light brightness (S2) obtained in the above "(9) Average reflected light brightness (S2) of the non-fused portions of the spunbond nonwoven fabric for filters" by the average reflected light brightness (S1) obtained in "(8) Average reflected light brightness (S1) of the fused portions of the spunbond nonwoven fabric for filters" and substituting the result (S2 / S1) into the following formula (1), and the calculated value (R) is the average brightness ratio. R = 1 - (S2 / S1) (1)
[0056] (11) Pleating processability of spunbond nonwoven fabric for filters (points) (i) A spunbond nonwoven fabric for filters was cut to a width of 240 mm, and this spunbond nonwoven fabric for filters was heated to 150°C and compressed while being pleated so that the distance from the ridgeline of one apex of the pleated body to the ridgeline of the next apex was 35 mm, thereby obtaining a pleated body. (ii) This pleated body was wound 45 times around a porous cylindrical polypropylene core, the ends of the pleated body were heat sealed, and then injection-molded caps were attached to both ends of the cylinder to produce a pleated filter. (iii) Twenty panelists visually inspected the appearance of the pleated filters and judged the pleatability of the spunbond nonwoven fabric for automobile oil filters on a five-point scale based on the following criteria. The total score ranged from a minimum of 0 points to a maximum of 100 points, with a score of 80 points or more being considered a pass. 5 points: Very good (There is no contact between the pleats of the pleated body, and the pleats are not distorted, and adjacent pleats are aligned parallel to each other in straight lines.) 4 points: Good (Between 5 and 3) 3 points: Average (There is no contact between the peaks of the pleated body, but the pleat shape is distorted.) 2 points: Bad (Between 3 and 1) 1 point: Very bad (The pleat shape is distorted and the peaks of the pleated body are in contact with each other.)
[0057] (12) Liquid permeability of spunbond nonwoven fabric for filters (sec / cm 3 ) (i) Five samples of 100 mm in MD x 100 mm in CD are cut out from the spunbond nonwoven fabric for filters at equal intervals in the CD direction of the spunbond nonwoven fabric for filters, for a total of five samples. (ii) A cylinder with a diameter of 2 cm was fixed onto the spunbond nonwoven fabric for the filter, and 1 cm of rapeseed oil with a viscosity of 43 mPa sec (30°C) was poured into it. 3 Pour from the top of the cylinder. (iii) 1 cm rapeseed oil 3 The time until the liquid completely penetrated into the nonwoven fabric was measured, rounded off to the first decimal place, and this value was taken as the liquid permeability. (13) Apparent density of spunbond nonwoven fabric for filters The apparent density of the spunbond nonwoven fabric for filters was calculated by the above-mentioned method.
[0058] (12) Collection efficiency of spunbond nonwoven fabric for filters (%) FIG. 3 is a diagram for explaining the configuration of a test system for carrying out a collection performance test according to an embodiment of the present invention. The test system 51 shown in FIG. 3 includes a sample holder 52 for setting a test sample M, a flowmeter 53, a flow rate control valve 54, a blower 55, a dust supply device 56, a changeover cock 57, and a particle counter 58. The flowmeter 53, the flow rate control valve 54, the blower 55, and the dust supply device 56 are connected to the sample holder 52. The flowmeter 53 is connected to the blower 55 via the flow rate control valve 54. Dust is supplied from the dust supply device 56 to the sample holder 52 by the intake of the blower 55. A particle counter 58 is connected to the sample holder 52, and the number of dust particles on the upstream side and the downstream side of the test sample M can be measured via the changeover cock 57. First, three samples of 15 cm×15 cm are taken from any part of the nonwoven fabric, and the taken test sample M is set in the sample holder 52. The evaluation area of the test sample is 115 cm 2 In measuring the collection performance, a 10% by weight solution of polystyrene 0.309U (manufactured by Nacalai Tesque, Inc.) was diluted 200 times with distilled water and filled into the dust supply device 56. The air volume was adjusted with the flow rate control valve 54 so that the filter passing speed was 3.0 m / min, and the dust concentration was set to 20,000 to 70,000 particles / (2.83×10 -4 m 3 (0.01ft 3 The dust counts upstream and downstream of test sample M were measured for dust particle sizes in the range of 0.3 to 0.5 μm using a particle counter 58 (KC-01D, manufactured by Rion Co., Ltd.). The values obtained were substituted into the following calculation formula, and the resulting value was rounded off to the nearest whole number to determine the collection performance (%). Collection performance (%)=[1-(D1 / D2)]×100 Here, D1 is the number of dust particles downstream (total of three measurements), and D2 is the number of dust particles upstream (total of three measurements).
[0059] (13) Pressure loss (Pa) The static pressure difference between the upstream and downstream of the test sample M during the above collection performance measurement was read by the pressure gauge 59, and the average value obtained from the three samples was rounded off to the first decimal place to calculate the average value.
[0060] [Resin used] Next, the resins used in the examples and comparative examples will be described in detail. Polyester resin A: Polyethylene terephthalate (PET) dried to a moisture content of 50 ppm by mass or less, with an intrinsic viscosity (IV) of 0.65 and a melting point of 260°C. Polyester resin B: Copolymerized polyethylene terephthalate (CO-PET) dried to a moisture content of 50 ppm by mass or less, with an intrinsic viscosity (IV) of 0.64, an isophthalic acid copolymerization rate of 11 mol%, and a melting point of 230°C.
[0061] [Example 1] The polyester resin A and the polyester resin B were melted at temperatures of 295°C and 280°C, respectively. Then, the polyester resin A was used as the core component and the polyester resin B was used as the sheath component, and the core:sheath=80:20 mass ratio was spun out from the fine holes at a spinneret temperature of 295°C, and then a filament having a circular cross section was spun at a spinning speed of 4900m / min by an air sucker, and the fiber arrangement was regulated by a fiber spreader plate and deposited on a moving net conveyor, and a fiber web consisting of fibers with an average single fiber diameter of 14.8μm was collected. The collected fiber web was temporarily fused by a calendar roll consisting of a pair of flat rolls at a temperature of 140°C and a linear pressure of 50kg / cm. Then, the fused area ratio was 10% and the area per fused portion was 1.6mm. 2 The upper and lower embossing rolls are fused at a temperature of 200°C and a line pressure of 70 kg / cm, resulting in a basis weight of 260 g / m. 2 The spunbond nonwoven fabric for filters obtained had a basis weight CV value of 3.3%, a thickness of 0.74 mm, a bending resistance in the MD direction of 53 mN, and a ratio of average reflected light brightness (R) of 0.57. The results are shown in Table 1.
[0062] [Example 2] The upper and lower embossing rolls are set to a fusion area ratio of 10% and the area of each fusion part is 1.6 mm 2 The fusion area ratio is 18%, and the area of each fusion part is 0.7 mm. 2 The same conditions as in Example 1 were used except that an embossing roll consisting of a pair of engraved rolls with a basis weight of 260 g / m was used instead. 2 The spunbond nonwoven fabric for filters obtained had a basis weight CV value of 3.3%, a thickness of 0.73 mm, a bending resistance in the MD direction of 25 mN, and a ratio of average reflected light brightness (R) of 0.41. The results are shown in Table 1.
[0063] [Example 3] The discharge amount and spinning speed were changed so that the average single fiber diameter was 10.0 μm, and the net conveyor speed was changed so that the basis weight was the same as in Example 1. The same conditions as in Example 1 were used to obtain a basis weight of 260 g / m. 2 The resulting spunbond nonwoven fabric for filters had a basis weight CV value of 2.7%, a thickness of 0.61 mm, a bending resistance in the MD direction of 62 mN, and a ratio of average reflected light brightness (R) of 0.62. The results are shown in Table 1.
[0064] [Example 4] The fabric was embossed to a weight of 260 g / m under the same conditions as in Example 1, except that the temperatures of the upper and lower embossing rolls were both changed from 200° C. to 180° C. and the line pressure was changed from 70 kg / cm to 80 kg / cm. 2 The spunbond nonwoven fabric for filters obtained had a basis weight CV value of 3.6%, a thickness of 1.02 mm, a bending resistance in the MD direction of 57 mN, and a ratio of average reflected light brightness (R) of 0.75. The results are shown in Table 1.
[0065] [Example 5] The upper and lower embossing rolls are set to a fusion area ratio of 10% and the area of each fusion part is 1.6 mm 2The fusion area ratio is 8.5%, and the area of each fusion part is 1.6 mm. 2 The same conditions as in Example 1 were used except that an embossing roll consisting of a pair of engraved rolls with a basis weight of 260 g / m was used instead. 2 The spunbond nonwoven fabric for filters obtained had a basis weight CV value of 3.5%, a thickness of 1.21 mm, a bending resistance in the MD direction of 73 mN, and a ratio of average reflected light brightness (R) of 0.67. The results are shown in Table 1.
[0066] [Example 6] The upper and lower embossing rolls are set to a fusion area ratio of 10% and the area of each fusion part is 1.6 mm 2 The fusion area ratio is 16%, and the area of each fusion part is 0.5 mm 2 The same conditions as in Example 1 were used except that an embossing roll consisting of a pair of engraved rolls with a basis weight of 260 g / m was used instead. 2 The spunbond nonwoven fabric for filters obtained had a basis weight CV value of 4.4%, a thickness of 0.61 mm, a bending resistance in the MD direction of 37 mN, and a ratio of average reflected light brightness (R) of 0.37. The results are shown in Table 1.
[0067] [Table 1]
[0068] [Comparative Example 1] In the manufacturing process of Example 1, a step was added between the step of pre-fusing the collected fiber web and the step of partially fusing the collected fiber web using an embossing roll, in which the sheet obtained in the pre-fusing step was once wound up and cooled to room temperature, and then this sheet was sent to the embossing roll. In other words, the step of partially fusing the collected fiber web using an embossing roll was not performed subsequent to the pre-fusing step. The other conditions were the same as those of Example 1, except that a basis weight of 260 g / m 2The spunbond nonwoven fabric for filters obtained had a basis weight CV value of 3.2%, a thickness of 0.62 mm, a bending resistance in the MD direction of 25 mN, and a ratio of average reflected light brightness (R) of 0.16. The results are shown in Table 1.
[0069] [Comparative Example 2] The discharge amount and spinning speed were changed so that the average single fiber diameter was 29.2 μm, and the net conveyor speed was changed so that the basis weight was the same as in Example 1. The same conditions as in Example 1 were used to obtain a basis weight of 260 g / m. 2 The spunbond nonwoven fabric for filters obtained had a basis weight CV value of 6.1%, a thickness of 1.01 mm, a bending resistance in the MD direction of 81 mN, and a ratio of average reflected light brightness (R) of 0.57. The results are shown in Table 1.
[0070] [Comparative Example 3] The upper and lower embossing rolls are set to a fusion area ratio of 10% and the area of each fusion part is 1.6 mm 2 The fusion area ratio is 24%, and the area of each fusion part is 0.5 mm 2 The same conditions as in Example 1 were used except that an embossing roll having a basis weight of 260 g / m was used instead of an embossing roll consisting of a pair of engraved rolls having a basis weight of 260 g / m. 2 The spunbond nonwoven fabric for filters obtained had a basis weight CV value of 3.2%, a thickness of 0.69 mm, a bending resistance in the MD direction of 18 mN, and a ratio of average reflected light brightness (R) of 0.58. The results are shown in Table 1.
[0071] [Comparative Example 4] The polyester resin A and the polyester resin B were melted at temperatures of 295°C and 280°C, respectively. Then, the polyester resin A was used as the core component and the polyester resin B was used as the sheath component, and the core:sheath = 80:20 mass ratio was spun out from the fine holes at a spinneret temperature of 300°C, and then a filament having a circular cross section was spun at a spinning speed of 4400 m / min by an air sucker. The filament was collided with a metal collision plate installed at the outlet of the air sucker, and the fibers were charged and opened by frictional charging, and the fiber web consisting of fibers with an average single fiber diameter of 17.2 μm was collected on a moving net conveyor. Subsequently, a fusion area ratio of 18% and an area per fusion part of 0.7 mm were obtained. 2 The upper and lower embossing rolls are fused at a temperature of 205°C and a line pressure of 70 kg / cm, resulting in a basis weight of 260 g / m. 2 The resulting spunbond nonwoven fabric for filters had a basis weight CV value of 10.5%, a thickness of 0.50 mm, a bending resistance in the MD direction of 25 mN, and a ratio of average reflected light luminance (R) of 0.41.
[0072] The properties of the obtained spunbonded nonwoven fabric for filters are as shown in Table 1, but Comparative Example 1 had a low average reflected light brightness ratio and poor pleatability. Comparative Example 2, which had a thicker fiber diameter under the same conditions as Example 1, had an improved thickness, high stiffness, and poor pleatability and liquid permeability. Comparative Example 3, which was embossed at a fusion rate of 24%, had a reduced thickness, low stiffness, and poor pleatability. Comparative Example 4 had a worsening CV value per unit area, low stiffness, and poor pleatability. [Explanation of symbols]
[0073] 21: Filter media for automobile oil filters 22: Yamabe 23: Valley 24:MD direction arrow 25: CD direction arrow M: Test sample 51: Collection performance measuring device 52: Sample holder 53:Flow meter 54: Flow control valve 55: Blois 56: Dust supply device 57: Switching cock 58: Particle Counter 59: Pressure gauge
Claims
1. A spunbond nonwoven fabric for filters, which is composed of thermoplastic continuous filaments consisting of a high melting point component and a low melting point component and is partially fused, A spunbond nonwoven fabric for automobile oil filters, wherein the average single fiber diameter of the thermoplastic continuous filaments is 8.0 μm or more and 15.0 μm or less, the bending resistance in the MD (warp) direction is 20 mN or more and 80 mN or less, and the ratio of the average reflected light luminance (S1) of the fused portion to the average reflected light luminance (S2) of the non-fused portion in the cross section, represented by the following formula (1), is 0.20 or more and less than 1.
0. R=1-S2 / S1...(1)
2. 2. The spunbond nonwoven fabric for automobile oil filters according to claim 1, having a basis weight CV value of 5.0% or less.
3. 3. The spunbond nonwoven fabric for automobile oil filters according to claim 1, wherein the area ratio of the fused portions is 5% or more and 20% or less.
4. An automobile oil filter medium comprising the spunbond nonwoven fabric for automobile oil filters according to any one of claims 1 to 3.
5. An automobile oil filter comprising the filter material for automobile oil filters according to claim 4.
Citation Information
Patent Citations
Chemical cleaning for forced onceethrough boiler
JP1977098803A
Angle sensor
JP1979022874A
Nonwoven fabric for filter and method for producing the same
JP2007231500A
Filter material
JP2014138928A
Laminated nonwoven fabric and air cleaner
JP2016128221A