target
A target with controlled Ni-Fe-W composition and dispersed FeW phases in a NiW matrix addresses low leakage magnetic flux and particle issues, enhancing efficiency in magnetic recording media production.
Patent Information
- Application Number
- JP2021546593
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-09-19
- Filing Date
- 2020-09-03
- Publication Date
- 2024-09-18
- Estimated Expiration
- 2040-09-03
AI Technical Summary
Existing seed layers formed using a Ni-Fe-W alloy target in magnetic recording media suffer from low leakage magnetic flux, high particle generation, and reduced target efficiency during sputtering, making it difficult to achieve high-speed film formation.
A target composition of Ni100-X-Y-FeX-WY with controlled atomic ratios and dispersed FeW phases in a NiW matrix is used, minimizing Ni-Fe alloying and optimizing magnetic properties to enhance leakage magnetic flux and reduce particle generation.
The target achieves high leakage magnetic flux, reduces particle formation, and enables efficient high-speed film formation, improving target usage efficiency in manufacturing magnetic recording media.
Smart Images

Figure 0007552604000003 
Figure 0007552604000004 
Figure 0007552604000005
Abstract
Description
[Technical field]
[0001] The present invention relates to a target for forming, for example, a seed layer of a magnetic recording medium. [Background technology]
[0002] As a means of improving the recording density of magnetic recording media, the perpendicular magnetic recording method has been put to practical use. This perpendicular magnetic recording method is a method in which the magnetic recording layer is formed so that the axis of easy magnetization is oriented perpendicular to the medium surface, and is suitable for high recording density because the demagnetizing field within the bit is small even when the recording density is increased, and the deterioration of the recording and reproducing characteristics is small. In order to orient the magnetic easy axis of the magnetic recording layer perpendicular to the medium surface, it has been proposed to use Ru as the intermediate layer and a Ni alloy as the seed layer.
[0003] The Ni alloy used as the seed layer of such magnetic recording media is composed of a soft magnetic material with an fcc structure and orientation to the (111) plane, and is required to attract the magnetic field generated by the magnetic head, as well as to control the crystallinity of the intermediate layer and the grain boundary segregation of oxides in the magnetic recording layer; for example, a Ni-Fe-W alloy has been proposed (see Patent Document 1). In order to form the seed layer made of the Ni-Fe-W alloy, a sputtering method using a target is generally used. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2010-287260 A Summary of the Invention [Problem to be solved by the invention]
[0005] The seed layer disclosed in Patent Document 1 is a useful technique in that it can suppress deterioration of the magnetic properties of the magnetic recording layer and can improve the write performance even when the intermediate layer is thick. However, according to the study by the present inventors, when a seed layer is formed by sputtering using a target made of Ni-Fe-W alloy disclosed in Patent Document 1, it has been confirmed that leakage flux is low, making it difficult to form a film at high speed, and the usage efficiency of the target may be low. In addition, it has been confirmed that when a seed layer is formed by sputtering using a target made of Ni-Fe-W alloy disclosed in Patent Document 1, many defects called particles may be generated.
[0006] An object of the present invention is to provide a target which has high leakage magnetic flux and generates a small amount of particles during sputtering, and which is useful, for example, in the manufacture of magnetic recording media. [Means for solving the problem]
[0007] The target of the present invention has a composition formula of Ni 100-X-Y -Fe X -W Y , 5≦X≦40, 1≦Y≦15, and the remainder consisting of unavoidable impurities. The FeW phase is dispersed in a matrix phase consisting of NiW.
[0008] The target of the present invention is 0.12 mm 2 It is preferable that there is less than one FeW phase having an inscribed circle diameter of 400 μm or more per one piece.
[0009] The target of the present invention is 0.12 mm 2 It is preferable that the number of W phase particles having an inscribed circle diameter of 15 μm or more is less than one per one. Effect of the Invention
[0010] The present invention can provide a target which has high leakage magnetic flux and generates a small amount of particles during sputtering, and is useful, for example, for producing magnetic recording media. [Brief description of the drawings]
[0011] [Figure 1] 1 is a photograph of the metal structure of a target according to an embodiment of the present invention. [Diagram 2] Photograph of the metal structure of a target according to Example 2 of the present invention. [Diagram 3] 1 is a photograph of the metal structure of a target according to Example 3 of the present invention. [Figure 4] Photograph of the metal structure of a target serving as a comparative example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] In the target of the present invention, an FeW phase is dispersed in a matrix phase made of NiW. When Ni and Fe are alloyed, the magnetism (magnetic permeability) becomes high, and high leakage magnetic flux cannot be obtained. For this reason, the target of the present invention suppresses the alloying of Ni and Fe, and has a metal structure in which the FeW phase is dispersed in a matrix phase made of NiW. Specifically, the target of the present invention is alloyed with non-magnetic W and ferromagnetic Ni and Fe, respectively, to form a matrix of NiW phase, and the FeW phase is dispersed, thereby weakening the magnetism of each phase, obtaining high leakage magnetic flux, and enabling high-speed film formation, i.e., the utilization efficiency of the target can be increased. If NiFeW phase or NiFe phase exists in the metal structure of the target, the alloying of Ni and Fe increases the magnetism, and high leakage magnetic flux cannot be obtained. If Fe phase exists in the metal structure of the target, the effect of weakening the magnetism by non-magnetic W cannot be obtained, and the leakage magnetic flux becomes low. For this reason, it is preferable that the target according to the embodiment of the present invention does not have NiFeW phase, NiFe phase, or Fe phase in the metal structure, and is composed of NiW phase, FeW phase, and W phase.
[0013] The target of the present invention contains Ni, Fe, and W, with the remainder being unavoidable impurities. The contents of Ni, Fe, and W can be appropriately adjusted within a range that does not significantly impair the soft magnetic properties, such as the fcc structure and orientation to the (111) plane, required for the seed layer. Specifically, the composition formula in atomic ratio is Ni 100-X-Y -Fe X -W Y , 5≦X≦40, 1≦Y≦15, and the remainder consisting of unavoidable impurities. In the target of the present invention, a seed layer having low coercivity can be obtained by setting the Fe content, i.e., X in the composition formula, to 5 or more. For the same reasons as above, it is preferable that the target according to the embodiment of the present invention has X set to 10 or more. Furthermore, in the target of the present invention, a seed layer having a stable fcc structure and orientation to the (111) plane can be obtained by setting X to 40 or less. For the same reasons as above, it is preferable that X is set to 20 or less in the target according to the embodiment of the present invention.
[0014] The target of the present invention can obtain a seed layer having a stable fcc structure and orientation to the (111) plane by setting the W content, i.e., Y in the composition formula, to 1 or more. For the same reasons as above, it is preferable that the target according to the embodiment of the present invention has Y of 2 or more. Furthermore, in the target of the present invention, a seed layer having a high saturation magnetic flux density can be obtained by setting Y to 15 or less. And, in the target according to the embodiment of the present invention, for the same reason as above, it is preferable that Y is set to 8 or less.
[0015] The target according to the embodiment of the present invention has a diameter of 0.12 mm. 2 It is preferable that the number of FeW phases having an inscribed circle diameter of 400 μm or more is less than one per target, thereby making it possible to suppress the generation of particles in the target of the present invention. The FeW phase is the most magnetic of the metal structures (NiW phase, FeW phase, W phase) constituting the target of the present invention. If a coarse FeW phase with an inscribed circle diameter of 400 μm or more is present among the FeW phases, the leakage magnetic flux becomes too low locally, making it difficult for sputtering to proceed, and protrusions called nodules may occur on the target surface, which may become the starting point of abnormal discharge called arcing. For this reason, it is more preferable that the target according to the embodiment of the present invention has less than one FeW phase with an inscribed circle diameter of 300 μm or more. Here, the inscribed circle diameter in the present invention is the diameter of the circle that has the largest area (diameter) among the circles that can be drawn inside a certain contour shape and that touch the contour at at least one point. The inscribed circle diameter of the FeW phase in the present invention is the diameter of the circle that has the largest area (diameter) among the circles that can be drawn inside a certain contour shape and that touch the contour at at least one point. 2 The number of FeW phases having an inscribed circle diameter of 400 μm or more can be measured by photographing the FeW phases shown in dark gray in the backscattered electron image taken with a scanning electron microscope in the field of view of 0.12 mm 2 The number of FeW phases with an inscribed circle diameter of 400 μm or more in the observed field is counted. From the viewpoint of suppressing particle generation, the number of FeW phases with an inscribed circle diameter of 400 μm or more is counted within 0.12 mm on the surface to be sputtered. 2 Alternatively, multiple visual fields (for example, five visual fields) may be observed so that the number of FeW phases having an inscribed circle diameter of 400 μm or more present in each visual field may be counted, and the average value may be calculated.
[0016] The target according to the embodiment of the present invention has a diameter of 0.12 mm. 2 It is preferable that the number of W phases having an inscribed circle diameter of 15 μm or more is less than one per target, thereby making it possible for the target of the present invention to suppress the generation of particles. The sputtering rate of W with respect to Ar ions is extremely low compared to Ni and Fe, and if a W phase with an inscribed circle diameter of 15 μm or more is present, a convex portion of the W phase may be generated on the target surface, which may become a starting point for arcing. For this reason, it is more preferable that the target according to the embodiment of the present invention has less than one W phase with an inscribed circle diameter of 10 μm or more. Here, the inscribed circle diameter of the W phase in the present invention is an arbitrary diameter of 0.12 mm on the surface that becomes the sputtering surface of the target. 2 The number of W phases having an inscribed circle diameter of 15 μm or more can be measured by photographing the W phases shown as white in the backscattered electron image by a scanning electron microscope in the field of view of 0.12 mm 2 The number of W phases with an inscribed circle diameter of 15 μm or more in the field of view is counted. From the viewpoint of suppressing particle generation, the number of W phases with an inscribed circle diameter of 15 μm or more is counted within 0.12 mm on the surface to be sputtered. 2 Alternatively, multiple visual fields (for example, five visual fields) may be observed, the number of W phases having an inscribed circle diameter of 15 μm or more present in each visual field may be counted, and the average value may be calculated.
[0017] The target of the present invention can be obtained, for example, by a powder sintering method. Specifically, the target can be obtained by pressure sintering a mixed powder obtained by mixing NiW alloy powder and FeW alloy powder. As a manufacturing method for each alloy powder, it is possible to manufacture the target by a method of crushing an ingot cast from an alloy melt, or a gas atomization method in which the alloy melt is sprayed with an inert gas to form a powder. Among them, it is preferable to use the gas atomization method, which has a small amount of impurities, a high filling rate, and can obtain spherical powder suitable for sintering. Here, in order to suppress oxidation of the spherical powder, it is preferable to use an inert gas, such as Ar gas or nitrogen gas, as the atomization gas. As the pressure sintering, for example, a hot isostatic press (HIP) method, a hot press method, an electric current sintering method, or the like can be applied.
[0018] The pressure sintering is preferably carried out under conditions of a sintering temperature of 700 to 1300° C., a pressing pressure of 30 to 200 MPa, and a time of 1 to 10 hours. By setting the sintering temperature at 700°C or higher, the sintering of the powder can be promoted and the generation of voids can be suppressed. By setting the sintering temperature at 1300°C or lower, the melting of the powder can be suppressed. In order to suppress the generation of voids and the diffusion of the NiW alloy powder and the FeW alloy powder, it is preferable to sinter at a temperature of 850 to 1050°C. Furthermore, by setting the pressure at 30 MPa or more, the progress of sintering can be promoted and the occurrence of voids can be suppressed, while by setting the pressure at 200 MPa or less, the introduction of residual stress into the target during sintering can be suppressed and the occurrence of cracks after sintering can be suppressed. In addition, by setting the sintering time to 1 hour or more, the progress of sintering can be promoted and the generation of voids can be suppressed, and by setting the sintering time to 10 hours or less, the decrease in manufacturing efficiency can be suppressed. EXAMPLES
[0019] The composition formula in atomic ratio is Ni by gas atomization using Ar gas. 96.98 W 3.02 Powder and Fe 97.12 W 2.88 The powders were each sieved through a 250 μm sieve to remove coarse particles, and then the composition formula in atomic ratio was Ni 82 Fe 15 After weighing out the ingredients so that the weight was W3, the ingredients were mixed in a V-type mixer to obtain a mixed powder. The mixed powder was then filled into a capsule made of soft iron and degassed and sealed at 450°C for 4 hours. The capsule was then pressure-sintered by HIP at 950°C, 122 MPa, and 1 hour to produce a sintered body. The sintered body was machined to obtain a target having a diameter of 180 mm and a thickness of 7 mm, which is Example 1 of the present invention.
[0020] The composition formula in atomic ratio is Ni by gas atomization using Ar gas. 96.20 W 3.80 Powder and Fe 97.12W 2.88 The powders were each sieved through a 250 μm sieve to remove coarse particles, and then the composition formula in atomic ratio was Ni 91.25 Fe5W 3.75 The ingredients were weighed and mixed in a V-type mixer to obtain a mixed powder. The mixed powder was then filled into a capsule made of soft iron and degassed and sealed at 450°C for 4 hours. The capsule was then pressure-sintered by HIP at 950°C, 122 MPa, and 1 hour to produce a sintered body. The sintered body was machined to obtain a target of Example 2 of the present invention, with a diameter of 180 mm and a thickness of 7 mm.
[0021] The composition formula in atomic ratio is Ni by gas atomization using Ar gas. 96.20 W 3.80 Powder and Fe 97.12 W 2.88 The powders were each sieved through a 250 μm sieve to remove coarse particles, and then the composition formula in atomic ratio was Ni 56.58 Fe 40 W 3.42 The ingredients were weighed and mixed in a V-type mixer to obtain a mixed powder. The mixed powder was then filled into a capsule made of soft iron and degassed and sealed at 450°C for 4 hours. The capsule was then pressure-sintered by HIP at 950°C, 122 MPa, and 1 hour to produce a sintered body. The sintered body was machined to obtain a target of Example 3 of the present invention, with a diameter of 180 mm and a thickness of 7 mm.
[0022] The composition formula in atomic ratio is Ni by gas atomization using Ar gas. 82 Fe 15 W3 powder was produced. The obtained powder was sieved through a 250μm sieve to remove coarse powder, then packed into a soft iron capsule and degassed and sealed at 450℃ for 4 hours. The capsule was then pressure-sintered by HIP at 1250℃, 146MPa, and 1 hour to produce a sintered body. This sintered body was machined to obtain a target having a diameter of 180mm and a thickness of 7mm, which serves as a comparative example.
[0023] The leakage magnetic flux of the targets of the invention examples 1 to 3 and the comparative example prepared above was measured by the following method. First, a gaussmeter was placed above the horseshoe-shaped permanent magnet, and the magnetic flux when no target was placed between the horseshoe-shaped permanent magnet and the gaussmeter was set to 100 G. Next, the magnetic flux at the center was measured when the target was placed between the horseshoe-shaped permanent magnet and the gaussmeter. The magnetic flux measured when the target was placed was then divided by the 100 G set above to obtain the leakage magnetic flux. The results are shown in Table 1.
[0024] A test piece measuring 10 mm x 10 mm x 5 mm was taken from the end material of each target prepared above, and the 10 mm x 10 mm surface was buffed. The test pieces of Inventive Example 1 and Comparative Example were observed for metal structure using a scanning electron microscope S-3600N manufactured by Hitachi High-Technologies Corporation, and the test pieces of Inventive Example 2 and Inventive Example 3 were observed for metal structure using a scanning electron microscope JSM-6610LA manufactured by JEOL Ltd. In addition, the presence of the phases formed was confirmed by energy dispersive X-ray spectroscopy for the test pieces of Inventive Examples 1 to 3 and Comparative Example. The metal structure was observed by a backscattered electron image of the surface to be sputtered of each sample, taken from a 0.12 mm 2 One field of view was observed, the inscribed circle diameters of the FeW phase and W phase present in the field of view were measured, and the number of FeW phases with an inscribed circle diameter of 400 μm or more and W phases with an inscribed circle diameter of 15 μm or more were counted. The metal structures of the eroded surfaces of the targets of Examples 1 to 3 of the present invention are shown in FIGS. 1 to 3, and the metal structure of the eroded surface of the target of the comparative example is shown in FIG.
[0025] [Table 1]
[0026] As shown in Figs. 1 to 3, the targets of Examples 1 to 3 of the present invention each have a NiW matrix phase shown in light gray with an FeW phase shown in dark gray dispersed therein. 2In the field of view shown in FIG. 1, there was no FeW phase with an inscribed circle diameter of 400 μm or more, and no W phase with an inscribed circle diameter of 15 μm or more, as shown in white, and a high leakage magnetic flux of 5.0% or more was obtained. On the other hand, it was confirmed that the target of the comparative example was made of a NiFeW phase as shown in FIG. 4, and exhibited a low leakage flux of less than 5.0%.
Claims
1. The atomic ratio of the composition formula is Ni 100-X-Y -Fe X -W Y , 5≦X≦40, 1≦Y≦15, with the remainder consisting of unavoidable impurities, and a target in which an FeW phase is dispersed in a matrix phase consisting of NiW.
2. 0.12mm 2 2. The target according to claim 1, wherein the number of FeW phases having an inscribed circle diameter of 400 μm or more is less than one per target.
3. 0.12mm 2 3. The target according to claim 1 or claim 2, wherein the number of W phases having an inscribed circle diameter of 15 μm or more per one target is less than one.
Citation Information
Patent Citations
Ni-Fe-W alloy target and manufacturing method thereof
CN104651788A
Magnetic recording medium, manufacturing method therefor and magnetic recording device
JP2002222518A
Perpendicular magnetic recording medium
JP2010287260A
Nickel based target material excellent in sputtering property
JP2016145394A