Conjugated conductive polymer-containing dispersion and method for producing solid electrolytic capacitor

By adding a morpholine compound to a conjugated conductive polymer dispersion and forming a solid electrolyte layer on a porous pole body, the capacitor achieves high capacity and reliability under high temperatures, addressing the limitations of existing capacitors in rising temperature environments.

JP7552775B2Active Publication Date: 2024-09-18RESONAC CORP
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
JP2023063733
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2017-08-31
Filing Date
2023-04-10
Publication Date
2024-09-18
Estimated Expiration
2038-05-09

Smart Images

  • Figure 0007552775000001
    Figure 0007552775000001
  • Figure 0007552775000002
    Figure 0007552775000002
  • Figure 0007552775000005
    Figure 0007552775000005
Patent Text Reader

Abstract

To provide a conjugated conductive polymer-containing dispersion for obtaining a solid electrolytic capacitor having a high capacity appearance ratio (capacitance), excellent heat resistance, and high reliability under a high-temperature condition.SOLUTION: A conjugated conductive polymer-containing dispersion contains: seed particles which are turned into protective colloid by means of polyanions, or polyanions; conjugated conductive polymers; morpholine compounds; and dispersion media.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a conjugated conductive polymer-containing dispersion, a method for producing a solid electrolytic capacitor, and a solid electrolytic capacitor obtained by the production method. [Background technology]

[0002] A solid electrolytic capacitor is manufactured by forming a dielectric oxide film on a metal surface by anodization and then contacting the film with a solid electrolyte. A solid electrolytic capacitor using a conductive polymer as the solid electrolyte has been proposed. Examples of metals that can be covered with a dielectric oxide film by anodization include aluminum, tantalum, and niobium. Also, as conductive polymers used in solid electrolytic capacitors, conjugated conductive polymers such as polythiophene, polypyrrole, polyaniline, polyacetylene, polyphenylene, poly(p-phenylene-vinylene), polyacene, polythiophene vinylene and derivatives thereof are known. Also, a technique is known in which a polyanion such as polystyrene sulfonate is used as a counter anion of the conjugated conductive polymer to dope the conjugated conductive polymer.

[0003] A solid electrolyte is generally formed by chemically oxidizing a monomer solution and an oxidant solution to obtain a conductive polymer on a dielectric oxide film formed on a metal surface having valve action, or by electrolytic polymerization. A method of forming a solid electrolyte by coating an aqueous solution or suspension of a conductive polymer has also been proposed. For example, Japanese Patent Laid-Open Publication No. 2003-100561 (Patent Document 1) discloses a manufacturing method including a step of forming a first solid electrolyte layer by impregnating a capacitor element with a conductive polymer dispersion aqueous solution in which fine particles of a conductive polymer are dispersed, and a step of forming a second solid electrolyte layer by impregnating the surface of this first solid electrolyte layer with a solution containing a heterocyclic monomer and a solution containing an oxidizing agent separately, or with a mixed solution containing a heterocyclic monomer and an oxidizing agent.

[0004] Japanese Patent Laid-Open Publication No. 2005-109252 (Patent Document 2) discloses a method in which a capacitor element having a dielectric oxide film formed on the surface of a sintered body obtained by sintering valve metal powder is formed, and then a solid electrolyte layer made of a conductive polymer is formed by chemically polymerizing a polymerizable monomer, and the capacitor element is then immersed in a conductive polymer solution or coated with a conductive polymer solution and dried, thereby forming a thicker conductive polymer layer on the conductive polymer layer formed by chemical polymerization.

[0005] JP2011-510141A (U.S. Pat. No. 8,721,928A) (Patent Document 3) proposes a process for impregnating a conductive polymer into a capacitor by reducing the viscosity of a poly(3,4-ethylenedioxythiophene)-polystyrenesulfonic acid (PEDOT-PSS) dispersion and polymerizing it using ultrasonic irradiation.

[0006] International Publication No. 2014 / 163202 (US Pat. No. 9,640,325) (Patent Document 4) discloses a method for producing a solid electrolytic capacitor with excellent capacitor characteristics with good productivity, by a process of obtaining a conjugated conductive polymer-containing dispersion by polymerizing a monomer in a dispersion medium containing a monomer for obtaining a conjugated conductive polymer and seed particles that have been made into a protective colloid by a polyanion, and a solid electrolytic capacitor. This solid electrolytic capacitor is characterized by low equivalent series resistance (ESR), excellent frequency characteristics, and small characteristic changes with temperature changes due to the use of a conductive polymer. In recent years, solid electrolytic capacitors are expected to be applied to places where the temperature around the circuit tends to rise, such as inverter power supplies and in-vehicle devices, and further high-temperature stability and high-temperature reliability of solid electrolytic capacitors have become an issue. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] JP 2003-100561 A [Patent Document 2] JP 2005-109252 A [Patent Document 3] JP 2011-510141 A (U.S. Patent No. 8,721,928 A) [Patent Document 4] International Publication No. 2014 / 163202 (U.S. Patent No. 9,640,325) Summary of the Invention [Problem to be solved by the invention]

[0008] An object of the present invention is to provide a conjugated conductive polymer-containing dispersion for obtaining a solid electrolytic capacitor having a high capacity expression rate (electrostatic capacitance), excellent heat resistance, and high reliability under high temperature conditions. Another object of the present invention is to provide a solid electrolytic capacitor that has a high capacitance expression rate (electrostatic capacitance), excellent heat resistance, and high reliability under high-temperature conditions. [Means for solving the problem]

[0009] As a result of intensive research, the present inventors have found that the above-mentioned problems can be solved by forming a solid electrolyte layer by a process of adhering a dispersion prepared by adding a morpholine compound to a conjugated conductive polymer dispersion used as a solid electrolyte for a solid electrolytic capacitor, i.e., a dispersion containing a morpholine compound and a conjugated conductive polymer, to a porous electrode body made of a valve acting metal having a dielectric film, thereby completing the present invention. That is, the present invention relates to a method for producing a solid electrolytic capacitor and a solid electrolytic capacitor according to the following items [1] to

[14] .

[0010] [1] A step (A) of polymerizing a monomer for obtaining a conjugated conductive polymer in a dispersion medium containing seed particles protected by a polyanion or in a dispersion medium containing a polyanion to obtain a conjugated conductive polymer-containing dispersion; The conjugated conductive polymer-containing dispersion liquid is added with a compound represented by the following general formula (1): [ka] (In the formula, R 1represents (1) a hydrogen atom, (2) an alkyl group having 1 to 8 carbon atoms which may be substituted with a hydroxyl group, a cyano group, or an amino group, (3) a cycloalkenyl group having 5 to 6 carbon atoms, (4) a phenyl group which may be substituted with an amino group, a cyano group, or a formyl group, (5) an acetyl group, (6) an acetoacetyl group, (7) an allyl group, (8) an acroyl group, (9) a pyridyl group, (10) an alkylsulfo group which may be substituted with a hydroxyl group, or (11) a formyl group, and n is 0, 1, or 2. and preparing a dispersion liquid containing the morpholine compound and a conjugated conductive polymer by adding a morpholine compound represented by the following formula (B): a step (C) of adhering the dispersion liquid to a porous anode body made of a valve action metal having a dielectric coating on its surface; and a step (D) of removing a dispersion medium from the dispersion liquid containing the morpholine compound and the conjugated conductive polymer that has been adhering to the porous anode body, thereby forming a solid electrolyte layer. [2] The method for producing a solid electrolytic capacitor according to the preceding paragraph 1, wherein the morpholine compound represented by the general formula (1) is 4-n-butylmorpholine, 4-isobutylmorpholine, 4-phenylmorpholine, 4-(2-hydroxypropyl)morpholine, 4-(2-hydroxyethyl)morpholine, or 4-(3-hydroxypropyl)morpholine. [3] The method for producing a solid electrolytic capacitor according to item 1 or 2 above, wherein the seed particles are particles of a polymer of an ethylenically unsaturated monomer. [4] The method for producing a solid electrolytic capacitor according to any one of items 1 to 3 above, wherein the seed particles that have been made into a protective colloid by the polyanion have a d50 particle size of 0.01 to 10 μm. [5] The method for producing a solid electrolytic capacitor according to any one of items 1 to 4 above, wherein in the step (A) of obtaining the conjugated conductive polymer-containing dispersion, a dispersion of polyanions or seed particles made into a protective colloid by polyanions is further added during polymerization of monomers to obtain the conjugated conductive polymer. [6] The method for producing a solid electrolytic capacitor according to any one of items 1 to 5 above, wherein in the step (A) of obtaining the conjugated conductive polymer-containing dispersion liquid, the resulting conjugated conductive polymer is subjected to a dispersion treatment. [7] The method for producing a solid electrolytic capacitor according to item 6, wherein the dispersion treatment is ultrasonic irradiation. [8] The method for producing a solid electrolytic capacitor according to any one of items 1 to 7 above, wherein the monomer for obtaining the conjugated conductive polymer is at least one selected from the group consisting of pyrrole compounds, aniline compounds, and thiophene compounds, each of which may have a substituent. [9] The monomer for obtaining the conjugated conductive polymer is represented by the following formula (2): [ka] (In the formula, R 2 and R 3 each independently represents a hydrogen atom, a hydroxyl group, an alkyl group having 1 to 18 carbon atoms which may have a substituent, an alkoxy group having 1 to 18 carbon atoms which may have a substituent, or an alkylthio group having 1 to 18 carbon atoms which may have a substituent, or R 2 and R 3 and are bonded to each other to form an alicyclic ring having 3 to 10 carbon atoms which may have a substituent, an aromatic ring having 6 to 10 carbon atoms which may have a substituent, an oxygen-atom-containing heterocyclic ring having 2 to 10 carbon atoms which may have a substituent, a sulfur-atom-containing heterocyclic ring having 2 to 10 carbon atoms which may have a substituent, or a sulfur- and oxygen-atom-containing heterocyclic ring having 2 to 10 carbon atoms which may have a substituent.

[10] The method for producing a solid electrolytic capacitor according to any one of items 1 to 9 above, wherein the polyanion is a polymer having a sulfo group.

[11] The method for producing a solid electrolytic capacitor according to any one of items 1 to 10, wherein a ratio of anionic groups in the polyanion is 0.25 to 30 mol per 1 mol of the monomer for obtaining the conjugated conductive polymer.

[12] The method for producing a solid electrolytic capacitor according to any one of items 1 to 11, wherein in the step (A) of obtaining the conjugated conductive polymer-containing dispersion liquid, the dispersion medium contains water, and the polymerization is carried out using at least one oxidizing agent selected from peroxodisulfuric acid and a salt thereof.

[13] The method for producing a solid electrolytic capacitor according to any one of items 1 to 12, wherein in the step (B), at least one selected from ethylene glycol, propylene glycol, and glycerin is added as an electrical conductivity improver.

[14] A solid electrolytic capacitor obtained by the production method according to any one of items 1 to 13 above. Effect of the Invention

[0011] According to the present invention, it is possible to provide a conjugated conductive polymer-containing dispersion for obtaining a solid electrolytic capacitor having a high capacity expression rate (electrostatic capacitance), excellent heat resistance, and high reliability under high temperature conditions. Furthermore, according to the present invention, it is possible to provide a solid electrolytic capacitor that has a high capacitance expression rate (electrostatic capacitance), excellent heat resistance, and high reliability under high temperature conditions. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] The method for producing a solid electrolytic capacitor of the present invention is characterized by comprising the steps of: (A) obtaining a conjugated conductive polymer-containing dispersion by polymerizing a monomer for obtaining a conjugated conductive polymer in a dispersion medium containing seed particles that have been made into a protective colloid by a polyanion or in a dispersion medium containing a polyanion; (B) adding a morpholine compound represented by general formula (1) (details will be described later) to the conjugated conductive polymer-containing dispersion to prepare a dispersion containing a morpholine compound and a conjugated conductive polymer; (C) attaching the dispersion to a porous anode body made of a valve action metal having a dielectric coating on its surface; and (D) removing the dispersion medium from the dispersion containing the morpholine compound and the conjugated conductive polymer attached to the porous anode body to form a solid electrolyte layer. In this specification, the term "conjugated conductive polymer" refers collectively to a conjugated conductive copolymer obtained by polymerizing a monomer alone for obtaining a conjugated conductive polymer, or by copolymerizing a plurality of monomers. Moreover, the particles in a state in which the polyanion is coordinated to the surface of the seed particle to form a protective colloid are referred to as "seed particles protected by a polyanion." Note that the polyanion means a polymer having two or more anionic groups.

[0013] <Step (A) of Obtaining a Dispersion Containing a Conjugated Conductive Polymer> The step (A) of obtaining a dispersion liquid containing a conjugated conductive polymer is carried out by (1) polymerizing the monomer in a dispersion medium containing a monomer for obtaining a conjugated conductive polymer and seed particles made into a protective colloid by a polyanion, or (2) polymerizing the monomer in a dispersion medium containing a monomer for obtaining a conjugated conductive polymer and a polyanion. The conjugated conductive polymer-containing dispersion in step (A) (hereinafter, sometimes referred to as "dispersion a") is a dispersion in which at least one selected from a complex of a conjugated conductive polymer and a seed particle made into a protective colloid by a polyanion, or a complex of a conjugated conductive polymer and a polyanion is dispersed in a dispersion medium. In this step, the polyanion is considered to form a complex by doping the conjugated conductive polymer.

[0014] [Conjugated conductive polymers] In this specification, the conjugated conductive polymer is not particularly limited as long as it is an organic polymer compound having a π-conjugated system in the main chain. Examples of the conjugated conductive polymer compound include polypyrroles, polythiophenes, polyisothianaphthenes, polyacetylenes, polyphenylenes, polyphenylenevinylenes, polyanilines, polyacenes, polythiophenevinylenes, and copolymers thereof. Note that the "type" in the above-mentioned conjugated conductive polymer compound notation means a compound group containing the compound structure, for example, polypyrroles refer to a compound group containing a polypyrrole structure. Among the above-mentioned conjugated conductive polymers, polypyrroles, polythiophenes and polyanilines are preferred, and polythiophenes are more preferred. From the viewpoint of obtaining high conductivity, conjugated conductive polymers having a substituent such as an alkyl group, a carboxy group, a sulfo group, an alkoxyl group, a hydroxyl group, or a cyano group are preferred. Specific examples of preferred conjugated conductive polymers, such as polypyrroles, polythiophenes and polyanilines, are given below.

[0015] The polypyrroles include polypyrrole, poly(N-methylpyrrole), poly(3-methylpyrrole), poly(3-ethylpyrrole), poly(3-n-propylpyrrole), poly(3-butylpyrrole), poly(3-octylpyrrole), poly(3-decylpyrrole), poly(3-dodecylpyrrole), poly(3,4-dimethylpyrrole), poly(3,4-dibutylpyrrole), poly(3-carboxypyrrole), poly(3-methyl-4- ... -carboxypyrrole), poly(3-methyl-4-carboxyethylpyrrole), poly(3-methyl-4-carboxybutylpyrrole), poly(3-hydroxypyrrole), poly(3-methoxypyrrole), poly(3-ethoxypyrrole), poly(3-butoxypyrrole), poly(3-hexyloxypyrrole), poly(3-methyl-4-hexyloxypyrrole), and poly(3-methyl-4-hexyloxypyrrole).

[0016] Polythiophenes include polythiophene, poly(3-methylthiophene), poly(3-hexylthiophene), poly(3-heptylthiophene), poly(3-octylthiophene), poly(3-decylthiophene), poly(3-dodecylthiophene), poly(3-octadecylthiophene), poly(3-bromothiophene), poly(3-chlorothiophene), poly(3-iodothiophene), poly(3-cyanothiophene), poly(3-phenylthiophene), poly(3,4- dimethylthiophene), poly(3,4-dibutylthiophene), poly(3-hydroxythiophene), poly(3-methoxythiophene), poly(3-ethoxythiophene), poly(3-butoxythiophene), poly(3-hexyloxythiophene), poly(3-heptyloxythiophene), poly(3-octyloxythiophene), poly(3-decyloxythiophene), poly(3-dodecyloxythiophene), poly(3-octadecyloxythiophene), poly(3,4- dihydroxythiophene), poly(3,4-dimethoxythiophene), poly(3,4-diethoxythiophene), poly(3,4-dipropoxythiophene), poly(3,4-dibutoxythiophene), poly(3,4-dihexyloxythiophene), poly(3,4-diheptyloxythiophene), poly(3,4-dioctyloxythiophene), poly(3,4-didecyloxythiophene), poly(3,4-didodecyloxythiophene), poly(3,4-ethylenedioxythiophene), thiophene), poly(3,4-propylenedioxythiophene), poly(3,4-butylenedioxythiophene), poly(3-methyl-4-methoxythiophene), poly(3-methyl-4-ethoxythiophene), poly(3-carboxythiophene), poly(3-methyl-4-carboxythiophene), poly(3-methyl-4-carboxyethylthiophene), poly(3-methyl-4-carboxybutylthiophene), and poly(3,4-ethyleneoxythiathiophene).

[0017] Examples of the polyanilines include polyaniline, poly(2-methylaniline), poly(3-isobutylaniline), poly(2-anilinesulfonic acid), and poly(3-anilinesulfonic acid). Among these, polypyrrole, polythiophene, poly(N-methylpyrrole), poly(3-methylthiophene), poly(3-methoxythiophene) and poly(3,4-ethylenedioxythiophene) are preferred because of their high electrical conductivity. Poly(3,4-ethylenedioxythiophene) (PEDOT) is more preferred because of its particularly high electrical conductivity and excellent heat resistance. In the present invention, the conjugated conductive polymers may be used alone or in combination of two or more.

[0018] [Monomers for obtaining conjugated conductive polymers] The monomer, which is a constituent unit of the conjugated conductive polymer, preferably contains at least one selected from pyrrole which may have a substituent, aniline which may have a substituent, and thiophene which may have a substituent. Examples of the substituent include an alkyl group having 1 to 18 carbon atoms, an aryl group having 6 to 10 carbon atoms, a heteroaryl group having 5 to 10 carbon atoms, an alkoxy group having 1 to 18 carbon atoms, an alkylthio group having 1 to 18 carbon atoms, a carboxy group, a hydroxyl group, a halogen atom, and a cyano group. The alkyl group, the aryl group, the heteroaryl group, the alkoxy group, and the alkylthio group may be substituted with at least one selected from a carboxy group, a hydroxyl group, a halogen atom, and a cyano group. Two or more of the substituents may be condensed to form a ring.

[0019] Specific examples of the monomer include pyrrole, N-methylpyrrole, 3-methylpyrrole, 3-ethylpyrrole, 3-n-propylpyrrole, 3-butylpyrrole, 3-octylpyrrole, 3-decylpyrrole, 3-dodecylpyrrole, 3,4-dimethylpyrrole, 3,4-dibutylpyrrole, 3-carboxylpyrrole, 3-methyl-4-carboxylpyrrole, 3-methyl-4-carboxyethylpyrrole, 3-methyl-4-carboxybutylpyrrole, 3-hydroxypyrrole, 3-methoxypyrrole, 3-ethoxypyrrole, 3-butoxypyrrole, 3-hexyloxypyrrole, 3-methyl-4-hexyloxypyrrole, and 3-methyl-4-hexyloxypyrrole;

[0020] Thiophene, 3-methylthiophene, 3-ethylthiophene, 3-propylthiophene, 3-butylthiophene, 3-hexylthiophene, 3-heptylthiophene, 3-octylthiophene, 3-decylthiophene, 3-dodecylthiophene, 3-octadecylthiophene, 3-bromothiophene, 3-chlorothiophene, 3-iodothiophene, 3-cyanothiophene, 3-phenylthiophene, 3,4-dimethylthiophene, 3,4-dibutylthiophene, 3-hydroxythiophene, 3-methoxythiophene, 3-ethoxythiophene, 3-butoxythiophene, 3-hexyloxythiophene, 3-heptyloxythiophene, 3-octyloxythiophene, 3-decyloxythiophene, 3-dodecyloxythiophene, 3-octadecyloxythiophene, 3,4-dihydroxythiophene, 3,4-dimethoxythiophene, 3,4-diethoxythiophene, 3,4-dipropoxythiophene, 3,4-dibutoxythiophene, 3,4-dihexyloxythiophene, 3,4-diheptyloxythiophene, 3,4-dioctyloxythiophene, 3,4-didecyloxythiophene, 3,4-didodecyloxythiophene, 3,4-ethylenedioxythiophene, 3,4-propylenedioxythiophene, 3,4-butylenedioxythiophene, 3-methyl-4-methoxythiophene, 3-methyl-4-ethoxythiophene, 3-carboxythiophene, 3-methyl-4-carboxythiophene, 3-methyl-4-carboxyethylthiophene, 3-methyl-4-carboxybutylthiophene, 3,4-ethyleneoxythiathiophene; aniline, 2-methylaniline, 3-isobutylaniline, 2-anilinesulfonic acid, 3-anilinesulfonic acid, and the like. In the present invention, the monomers for obtaining the conjugated conductive polymer may be used alone or in combination of two or more.

[0021] As a monomer for obtaining a conjugated conductive polymer, among the above-mentioned monomers, it is preferable to include a compound represented by the following formula (2), it is more preferable to include a compound represented by the following formula (3), and it is even more preferable to include 3,4-ethylenedioxythiophene.

[0022] [ka]

[0023] In the formula (2), R 2 and R 3 R each independently represents a hydrogen atom, a hydroxyl group, an alkyl group having 1 to 18 carbon atoms which may have a substituent, an alkoxy group having 1 to 18 carbon atoms which may have a substituent, or an alkylthio group having 1 to 18 carbon atoms which may have a substituent. 2 and R 3 represents an alicyclic ring having 3 to 10 carbon atoms which may have a substituent, an aromatic ring having 6 to 10 carbon atoms which may have a substituent, an oxygen atom-containing heterocyclic ring having 2 to 10 carbon atoms which may have a substituent, a sulfur atom-containing heterocyclic ring having 2 to 10 carbon atoms which may have a substituent, or a sulfur and oxygen atom-containing heterocyclic ring having 2 to 10 carbon atoms which may have a substituent, which are bonded to each other to form a ring. Examples of the substituent include an alkyl group having 1 to 18 carbon atoms, an aryl group having 6 to 10 carbon atoms, a heteroaryl group having 5 to 10 carbon atoms, an alkoxy group having 1 to 18 carbon atoms, an alkylthio group having 1 to 18 carbon atoms, a carboxy group, a hydroxyl group, a halogen atom, and a cyano group. The alkyl group, aryl group, heteroaryl group, alkoxy group, and alkylthio group may be substituted with a carboxy group, a hydroxyl group, a halogen atom, or a cyano group. Two or more substituents may be condensed to form a ring.

[0024] Examples of the oxygen atom-containing heterocycle include an oxirane ring, an oxetane ring, a furan ring, a hydrofuran ring, a pyran ring, a pyrone ring, a dioxane ring, and a trioxane ring. Examples of the sulfur atom-containing heterocycle include a thiirane ring, a thietane ring, a thiophene ring, a thiane ring, a thiopyran ring, a thiopyrylium ring, a benzothiopyran ring, a dithiane ring, a dithiolane ring, and a trithiane ring. Examples of the sulfur- and oxygen-atom-containing heterocycle include an oxathiolane ring and an oxathiane ring.

[0025] In formula (3), R 4 and R 5 each independently represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms which may have a substituent, or R 4 and R 5 and are bonded to each other to form a ring, which represents an oxygen atom-containing heterocycle having 3 to 6 carbon atoms and which may have a substituent. R 4 and R 5 is preferably R 4 and R 5 and are bonded to each other to form a ring, and are an oxygen atom-containing heterocycle having 3 to 6 carbon atoms, which may have a substituent. Examples of the oxygen atom-containing heterocycle include a dioxane ring and a trioxane ring, and a dioxane ring is preferred. Examples of the substituent include an alkyl group having 1 to 18 carbon atoms, an aryl group having 6 to 10 carbon atoms, a heteroaryl group having 5 to 10 carbon atoms, an alkoxy group having 1 to 18 carbon atoms, an alkylthio group having 1 to 18 carbon atoms, a carboxy group, a hydroxyl group, a halogen atom, and a cyano group. The alkyl group, the aryl group, the heteroaryl group, the alkoxy group, and the alkylthio group may be substituted with a carboxy group, a hydroxyl group, a halogen atom, or a cyano group. Two or more substituents may be condensed to form a ring.

[0026] [Polyanion] The polyanion is a polymer having two or more anionic groups, which coordinates with the surface of the seed particle to form a protective colloid and also functions as a dopant for the conjugated conductive polymer. Examples of the anionic group include a group consisting of sulfonic acid or a salt thereof, a group consisting of phosphoric acid or a salt thereof, a mono-substituted phosphate ester group, a group consisting of carboxylic acid or a salt thereof, a mono-substituted sulfate ester group, etc. Among these, a strongly acidic group is preferred, a group consisting of sulfonic acid or a salt thereof, and a group consisting of phosphoric acid or a salt thereof are more preferred, and a group consisting of sulfonic acid or a salt thereof is even more preferred. The anionic group may be directly bonded to the main chain of the polymer or may be bonded to a side chain. When the anionic group is bonded to a side chain, the doping effect becomes more pronounced, so that it is preferably bonded to the end of the side chain.

[0027] The polyanion may have a substituent other than the anionic group. Examples of the substituent include an alkyl group, a hydroxyl group, an alkoxy group, a phenol group, a cyano group, a phenyl group, a hydroxyphenyl group, an ester group, a halogeno group, an alkenyl group, an imide group, an amide group, an amino group, an oxycarbonyl group, and a carbonyl group. Among these, an alkyl group, a hydroxyl group, a cyano group, a phenol group, and an oxycarbonyl group are preferred, and an alkyl group, a hydroxyl group, and a cyano group are more preferred. The substituent may be directly bonded to the polymer main chain or may be bonded to the side chain. When a substituent is bonded to a side chain, the effect of each substituent is exhibited, so that the substituent is preferably bonded to the side chain end.

[0028] The alkyl group that can be substituted in the polyanion is expected to have the effect of increasing the solubility and dispersibility in the dispersion medium, and the compatibility and dispersibility with the conjugated conductive polymer. Examples of the alkyl group include chain alkyl groups such as methyl, ethyl, propyl, butyl, isobutyl, t-butyl, pentyl, hexyl, octyl, decyl, and dodecyl groups; and cycloalkyl groups such as cyclopropyl, cyclopentyl, and cyclohexyl groups. In consideration of the solubility in the dispersion medium, the dispersibility in the conjugated conductive polymer, and steric hindrance, an alkyl group having 1 to 12 carbon atoms is more preferable.

[0029] The hydroxyl group that can be substituted in the polyanion is expected to facilitate the formation of hydrogen bonds with other hydrogen atoms, etc., and to have the effect of increasing the solubility in the dispersion medium, the compatibility with the conjugated conductive polymer, the dispersibility, and the adhesiveness. The hydroxyl group is preferably bonded to the end of an alkyl group having 1 to 6 carbon atoms bonded to the polymer main chain.

[0030] The cyano group and hydroxyphenyl group which can be substituted in the polyanion are expected to have the effect of increasing the compatibility with the conjugated conductive polymer, the solubility in the dispersion medium, and the heat resistance. The cyano group is preferably one which is directly bonded to the polymer main chain, one which is bonded to the end of an alkyl group having 1 to 7 carbon atoms which is bonded to the polymer main chain, or one which is bonded to the end of an alkenyl group having 2 to 7 carbon atoms which is bonded to the polymer main chain.

[0031] The oxycarbonyl group which can be substituted in the polyanion is preferably an alkyloxycarbonyl group, an aryloxycarbonyl group, or an alkyloxycarbonyl group or aryloxycarbonyl group bonded directly to the polymer main chain via another functional group.

[0032] The composition of the polymer main chain of the polyanion is not particularly limited. Examples of the polymer main chain include polyalkylene, polyimide, polyamide, polyester, etc. Among these, polyalkylene is preferred from the viewpoint of synthesis and availability.

[0033] Polyalkylene is a polymer composed of repeating units of ethylenically unsaturated monomers. Polyalkylene may have a carbon-carbon double bond in the main chain. Examples of polyalkylene include polyethylene, polypropylene, polybutene, polypentene, polyhexene, polyvinyl alcohol, polyvinylphenol, poly(3,3,3-trifluoropropylene), polyacrylonitrile, polyacrylate, polymethacrylate, polystyrene, polybutadiene, and polyisoprene.

[0034] Examples of polyimides include those obtained by a polycondensation reaction between an acid anhydride such as pyromellitic dianhydride, biphenyltetracarboxylic dianhydride, benzophenonetetracarboxylic dianhydride, 2,2,3,3-tetracarboxydiphenylether dianhydride, or 2,2-[4,4'-di(dicarboxyphenyloxy)phenyl]propane dianhydride and a diamine such as oxydianiline, paraphenylenediamine, metaphenylenediamine, or benzophenonediamine.

[0035] Examples of polyamides include polyamide 6, polyamide 6,6, and polyamide 6,10. Examples of the polyester include polyethylene terephthalate and polybutylene terephthalate.

[0036] Specific examples of polymers having a sulfo group that are preferably used as polyanions include polyvinyl sulfonic acid, polystyrene sulfonic acid, polyallyl sulfonic acid, polyethyl acrylate sulfonic acid, polybutyl acrylate sulfonic acid, poly(2-acrylamido-2-methylpropane sulfonic acid), polyisoprene sulfonic acid, etc. These may be homopolymers or copolymers of two or more kinds. Among these, from the viewpoint of imparting electrical conductivity, polystyrene sulfonic acid, polyisoprene sulfonic acid, polyethyl acrylate sulfonic acid, and polybutyl acrylate sulfonic acid are preferred, and polystyrene sulfonic acid (PSS) is more preferred. A polyanion, particularly a polymer having a sulfo group, improves the dispersibility in a dispersion medium of a monomer for obtaining a conjugated conductive polymer, and further functions as a dopant for the conjugated conductive polymer.

[0037] The polyanion used in the present invention has a weight-average molecular weight of preferably 1000 to 1,000,000, more preferably 5,000 to 500,000, and even more preferably 50,000 to 300,000. When the weight-average molecular weight is within this range, the solubility of the polyanion in the dispersion medium and the doping of the polyanion into the conjugated conductive polymer are improved. The weight-average molecular weight referred to here is a value measured as a polystyrene-equivalent molecular weight using gel permeation chromatography.

[0038] The polyanion may be selected from commercially available products having the above properties, or may be synthesized by a known method, for example, as described in JP-A-2005-76016.

[0039] The amount of polyanion used, i.e., the total amount of polyanion used including that used to form a protective colloid for seed particles, that charged before the start of polymerization, and / or that added during polymerization, is an amount such that the anionic group in the polyanion is preferably 0.25 to 30 mol, more preferably 0.8 to 25 mol, per mol of the monomer for obtaining the conjugated conductive polymer. In addition, the amount of polyanion used in this step is preferably 10 to 30,000 parts by mass, more preferably 50 to 25,000 parts by mass, based on 100 parts by mass of the conjugated conductive polymer. When the amount of polyanion used is 10 parts by mass or more, the conductivity of the conductive polymer is appropriate, and when it is 30,000 parts by mass or less, the dispersibility of the conductive polymer in the dispersion medium is good.

[0040] [Seed particles] The seed particles used in the present invention are polymer particles that are converted into protective colloids by polyanions in a dispersion medium. For example, the seed particles are preferably made of a polymer containing one or more ethylenically unsaturated monomers as constituent units. The polymer may be one type alone or a mixture of two or more types, and may be either crystalline or amorphous. In the case of a crystalline polymer, the degree of crystallinity is preferably 50% or less.

[0041] The ethylenically unsaturated monomer may be any monomer having at least one polymerizable ethylenic carbon-carbon double bond. Examples of the ethylenically unsaturated monomer include (meth)acrylates having linear, branched or cyclic alkyl chains; aromatic vinyl compounds such as styrene and α-methylstyrene; heterocyclic vinyl compounds such as vinylpyrrolidone; hydroxyalkyl (meth)acrylates; dialkylaminoalkyl (meth)acrylates such as 2-ethylhexyl (meth)acrylate; vinyl esters such as vinyl acetate and vinyl alkanoate; monoolefins such as ethylene, propylene, butylene and isobutylene; conjugated diolefins such as butadiene, isoprene and chloroprene; α,β-unsaturated mono- or dicarboxylic acids such as acrylic acid, methacrylic acid, crotonic acid, itaconic acid, maleic acid and fumaric acid; cyanide vinyl compounds such as acrylonitrile; and carbonyl group-containing vinyl compounds such as acrolein and diacetone acrylamide. These ethylenically unsaturated monomers may be used alone or in combination of two or more. In this specification, "(meth)acrylic" refers to acrylic or methacrylic, and "(meth)acrylate" refers to acrylate or methacrylate.

[0042] The ethylenically unsaturated monomer may contain a crosslinkable monomer, and may be crosslinked with itself or in combination with an ethylenically unsaturated compound having an active hydrogen group. By forming a crosslinked copolymer, the water resistance, moisture resistance, heat resistance, etc. of the conductive film can be improved. The crosslinkable monomer refers to a compound having two or more ethylenic carbon-carbon double bonds, or a compound having one or more ethylenic carbon-carbon double bonds and one or more other reactive groups. Examples of the crosslinkable monomer include epoxy group-containing α,β-ethylenically unsaturated compounds such as glycidyl (meth)acrylate; hydrolyzable alkoxysilyl group-containing α,β-ethylenically unsaturated compounds such as vinyltriethoxysilane and γ-methacryloxypropyltrimethoxysilane; and polyfunctional vinyl compounds such as ethylene glycol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, allyl (meth)acrylate, divinylbenzene, and diallyl phthalate. In addition, a crosslinkable monomer such as a carbonyl group-containing α,β-ethylenically unsaturated compound (containing a ketone group) may be used in combination with a polyhydrazine compound (particularly one having two or more hydrazide groups, such as oxalic acid dihydrazide, succinic acid dihydrazide, adipic acid dihydrazide, or polyacrylic acid hydrazide) for crosslinking. The content of the crosslinkable monomer in the ethylenically unsaturated monomer is preferably 50% by mass or less, more preferably 35% by mass or less, and even more preferably 25% by mass or less.

[0043] Preparation of seed particles protected by polyanion: The seed particles are converted into a protective colloid by the polyanion in the dispersion medium, and a dispersion of the protective colloidal seed particles dispersed in the dispersion medium can be produced as a resin emulsion.

[0044] The polymerization reaction of the resin emulsion is a radical polymerization reaction, and is carried out by any of batch, semi-continuous, and continuous methods using a normal pressure reactor or a pressure-resistant reactor. From the viewpoint of reaction stability during polymerization and uniformity of the polymer, it is preferable to polymerize by continuously or intermittently adding an ethylenically unsaturated monomer solution to a polyanion-containing liquid in which an ethylenically unsaturated monomer and a polyanion are dissolved, emulsified, or dispersed in a dispersion medium, respectively. The reaction temperature is usually 10 to 100° C., generally 30 to 90° C. The reaction time is not particularly limited and may be appropriately adjusted depending on the amounts of each component used, the type of polymerization initiator, the reaction temperature, etc.

[0045] During radical polymerization, the polyanion, which is a protective colloid, contributes to the stability of the emulsion particles, but if necessary, an emulsifier such as an anionic emulsifier, a nonionic emulsifier, or a reactive emulsifier, or an aliphatic amine, etc. may be added to the polymerization system. The type and amount of the emulsifier and the aliphatic amine may be appropriately adjusted depending on various conditions including the amount of the polyanion used and the composition of the ethylenically unsaturated monomer.

[0046] Examples of emulsifiers used in such radical polymerization reactions include anionic emulsifiers such as alkyl sulfate salts, alkyl benzene sulfonates, alkyl sulfosuccinates, alkyl diphenyl ether disulfonates, polyoxyalkylene alkyl sulfates, and polyoxyalkylene alkyl phosphates; and nonionic surfactants such as polyoxyalkylene alkyl ethers, polyoxyalkylene alkylphenol ethers, polyoxyalkylene fatty acid esters, and polyoxyalkylene sorbitan fatty acid esters.

[0047] Examples of the aliphatic amine include primary amines such as octylamine, laurylamine, myristylamine, stearylamine, and oleylamine; secondary amines such as dioctylamine, dilaurylamine, distearylamine, and dioleylamine; and tertiary amines such as N,N-dimethyllaurylamine, N,N-dimethylmyristylamine, N,N-dimethylpalmitylamine, N,N-dimethylstearylamine, N,N-dimethylbehenylamine, N,N-dimethyloleylamine, N-methyldidecylamine, and N-methyldioleylamine. The emulsifiers and aliphatic amines may be used alone or in combination of two or more.

[0048] Furthermore, water-soluble polymers such as polyvinyl alcohol, methyl cellulose, carboxymethyl cellulose, hydroxyethyl cellulose, hydroxypropyl cellulose, polyvinylpyrrolidone, etc. may be used in combination within the range that does not impair the properties of the resulting conjugated conductive polymer.

[0049] The dispersion medium is an aqueous medium, and examples thereof include water or a mixed solvent of water and a water-soluble solvent. The ratio of the water-soluble solvent in the mixed solvent is preferably 0 to 30% by mass. If the ratio of the water-soluble solvent is 30% by mass or less, the polymerization reaction of the resin emulsion can be stabilized. Examples of the water-soluble solvent include alcohols such as methanol, ethanol, and isopropyl alcohol, ketones such as acetone, glycols such as ethylene glycol and propylene glycol, and ethers such as ethylene glycol monomethyl ether and ethylene glycol monobutyl ether.

[0050] The polymerization initiator used in the radical polymerization may be any known or commonly used one. Examples of the polymerization initiator include inorganic peroxides such as hydrogen peroxide, persulfuric acid, ammonium persulfate, potassium persulfate, and sodium persulfate, organic peroxides such as benzoyl peroxide and t-butyl hydroperoxide, and azo compounds such as 2,2'-azobisisobutyronitrile and 4,4'-azobis(4-cyanovaleric acid). If necessary, these polymerization initiators may be combined with sodium sulfoxylate formaldehyde, ascorbic acid, sulfites, tartaric acid or its salts, iron(II) sulfate, and the like to perform redox polymerization. If necessary, chain transfer agents such as alcohols and mercaptans may be used.

[0051] The amount of polyanion and ethylenically unsaturated monomer used during the production of protective colloidal seed particles is preferably 10 to 100 parts by mass, more preferably 20 to 90 parts by mass, per 100 parts by mass of polyanion. When the amount of ethylenically unsaturated monomer used is 10 parts by mass or more, the ratio of the conductive polymer containing the seed particles that have been made into a protective colloid by the polyanion in the conjugated conductive polymer is appropriate, and thickening due to polymerization can be suppressed. When the amount is 100 parts by mass or less, the stability of the protective colloidal seed particles is good. The d50 (50% median diameter on a volume basis) of the particle size of the seed particles which are converted into a protective colloid and dispersed in the dispersion medium is preferably 0.01 to 10 μm, more preferably 0.05 to 1 μm, and even more preferably 0.1 to 0.8 μm. The particle size distribution of the seed particles can be measured using a Microtrack UPA type particle size distribution measuring device manufactured by Nikkiso Co., Ltd. If the d50 of the particle size of the seed particles dispersed in the dispersion medium is 0.01 μm or more, the dispersibility of the seed particles is good, and if it is 10 μm or less, the particles are unlikely to settle.

[0052] Polymerization of monomers to obtain conjugated conducting polymers: Polymerization of a monomer to obtain a conjugated conductive polymer is carried out (1) in a dispersion medium containing the monomer and seed particles protected as a protective colloid by a polyanion, or (2) in a dispersion medium containing the monomer and a polyanion.

[0053] [Monomer solution for obtaining conjugated conductive polymers] In order to polymerize a monomer in a dispersion medium to obtain a conjugated conductive polymer, a dispersion containing a monomer and seed particles treated as a protective colloid, or a dispersion containing a monomer and a polyanion (hereinafter, these may be collectively referred to simply as a "monomer liquid") is prepared. The monomer liquid may be any liquid in which the monomer for obtaining a conjugated conductive polymer is uniformly dispersed. For the dispersion treatment, a powerful stirring device such as a homogenizer or an ultrasonic irradiation device is usually used, but ultrasonic irradiation treatment is preferred. The ultrasonic irradiation energy is not particularly limited as long as a uniform monomer liquid is obtained, but it is preferable to perform the ultrasonic irradiation at a power consumption of 5 to 500 W / L (liter) and an irradiation time of 0.1 to 2 hours / L (liter).

[0054] In addition, when a dispersion liquid containing a monomer for obtaining a conjugated conductive polymer and seed particles made into a protective colloid by a polyanion is used as the monomer liquid, it is preferable to contain the same polyanion as that used for making the seed particles into a protective colloid from the viewpoint of suppressing aggregation of the conjugated conductive polymer produced by polymerization. The polyanion can be contained by adding it to the monomer liquid and dissolving, emulsifying or dispersing it. When a polyanion other than that contained in the dispersion liquid of the seed particles made into a protective colloid is contained in the monomer liquid, the amount is preferably 5 to 99% by mass, more preferably 10 to 90% by mass, and even more preferably 20 to 80% by mass of the total amount of the polyanion used.

[0055] [Dispersion medium] The dispersion medium used in the polymerization of monomers to obtain a conjugated conductive polymer is not particularly limited as long as it can disperse a complex of a conjugated conductive polymer and a seed particle made into a protective colloid by a polyanion, or a complex of a conjugated conductive polymer and a polyanion, but is preferably the same type as that used for the dispersion liquid of the seed particles. Examples of the dispersion medium include water; amides such as N-vinylpyrrolidone, hexamethylphosphortriamide, N-vinylformamide, and N-vinylacetamide; phenols such as cresol, phenol, and xylenol; polyhydric alcohols such as dipropylene glycol, 1,3-butylene glycol, 1,4-butylene glycol, diglycerin, isoprene glycol, butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,9-nonanediol, and neopentyl glycol; carbonate compounds such as ethylene carbonate and propylene carbonate; ethers such as dioxane, diethyl ether, propylene glycol dialkyl ether, polyethylene glycol dialkyl ether, and polypropylene glycol dialkyl ether; heterocyclic compounds such as 3-methyl-2-oxazolidinone; and nitriles such as acetonitrile, glutarodinitrile, methoxyacetonitrile, propionitrile, and benzonitrile. These solvents can be used alone or in combination of two or more. Of these, it is preferable to use a dispersion medium containing water at 1 to 99 mass %, more preferably a dispersion medium containing water at 50 to 99 mass %, and even more preferably water alone.

[0056] The amount of the dispersion medium used is preferably 1 to 50,000 parts by mass, more preferably 50 to 10,000 parts by mass, relative to 100 parts by mass in total of the monomer for obtaining the conjugated conductive polymer, the seed particles made into a protective colloid by the polyanion, and the polyanion. If the amount of the dispersion medium used is 1 part by mass or more, the viscosity during polymerization is appropriate, and if it is 50,000 parts by mass or less, the performance of the solid electrolytic capacitor is good.

[0057] [Oxidizing agent] In the polymerization of the monomers, for example, when a dispersion containing polypyrroles or polythiophenes as the conjugated conductive polymer is produced, the polymerization is initiated by raising the temperature to a predetermined level in the presence of an oxidizing agent. Examples of the oxidizing agent include peroxodisulfuric acid, ammonium peroxodisulfate, sodium peroxodisulfate, potassium peroxodisulfate, and other peroxodisulfates, metal halide compounds such as boron trifluoride, transition metal compounds such as ferric chloride, ferric sulfate, and cupric chloride, metal oxides such as silver oxide and cesium oxide, peroxides such as hydrogen peroxide and ozone, organic peroxides such as benzoyl peroxide, and oxygen. Among these, peroxodisulfuric acid and peroxodisulfates are preferred, and peroxodisulfates are more preferred. The oxidizing agents can be used alone or in combination of two or more.

[0058] [Polymerization temperature] The temperature during polymerization of the monomer is usually 5 to 80°C, preferably 10 to 60°C, and more preferably 15 to 40°C. When the temperature during polymerization is within this range, the polymerization can be carried out at an appropriate reaction rate, an increase in viscosity can be suppressed, a dispersion containing a conductive polymer can be produced stably and in an economical time, and the conductivity of the obtained conductive polymer tends to be high. The temperature during polymerization can be controlled by using a known heater or cooler. Furthermore, the polymerization may be carried out while changing the temperature within the above range, as necessary.

[0059] [Distributed processing] In the step (A) of obtaining a conjugated conductive polymer-containing dispersion, it is preferable to disperse the conjugated conductive polymer produced by polymerization of the monomer during the polymerization reaction. This dispersion treatment is preferably carried out using a powerful stirring device such as a homogenizer or by ultrasonic irradiation. This dispersion treatment can suppress the aggregation of the conjugated conductive polymer having a long main chain. For example, the dispersion treatment at a shear rate of 5000 s described in JP 2007-332183 A can be carried out. -1 In the above-mentioned method of polymerization with stirring or ultrasonic irradiation, it is preferable to continue until the end of the reaction at a power consumption of 5 to 500 W / L per dispersion treatment liquid.

[0060] [Addition of protective colloidal seed particle dispersion] In addition, during the polymerization of the monomer using a dispersion containing the monomer and protective colloidal seed particles, it is preferable to further add a dispersion of seed particles that have been made into a protective colloid by a polyanion. By further adding a predetermined amount of a dispersion of seed particles that have been made into a protective colloid during the polymerization of the monomer, it is possible to suppress thickening of the reaction solution during polymerization, improve the stirring and mixing efficiency, and reduce the load on the production equipment. The amount of the dispersion of seed particles that have been made into a protective colloid added during the polymerization is preferably 10 to 90% by mass, more preferably 20 to 70% by mass, of the total amount of the dispersion of seed particles that have been made into a protective colloid used.

[0061] [Polyanion addition] A polyanion may be further added during polymerization of the monomer liquid. By further adding a portion of a predetermined amount of polyanion during polymerization of the monomer, thickening of the reaction liquid during polymerization can be suppressed, and the stirring and mixing efficiency can be improved and the load on the production equipment can be reduced. The amount of polyanion added during polymerization is preferably 0 to 90% by mass, more preferably 20 to 70% by mass, of the total amount of polyanion used.

[0062] <Step (B) of preparing a dispersion containing a morpholine compound and a conjugated conductive polymer> The production method of the present invention includes a step of adding a morpholine compound to the conjugated conductive polymer-containing dispersion (dispersion a) obtained in the above-mentioned step (A) to prepare a dispersion containing a morpholine compound and a conjugated conductive polymer (hereinafter sometimes referred to as "dispersion b").

[0063] [Morpholine compounds] The morpholine compound is represented by the following general formula (1): [ka] The addition of a morpholine compound makes it possible to produce a solid electrolytic capacitor that has a high capacity expression rate (electrostatic capacitance), excellent heat resistance, and high reliability under high temperature conditions. It also makes it possible to impart corrosion resistance to the solid electrolytic capacitor and to adjust the pH of the dispersion containing the conjugated conductive polymer. In formula (1), R 1 is (1) a hydrogen atom, (2) an alkyl group having 1 to 8 carbon atoms which may be substituted with a hydroxyl group, a cyano group, or an amino group, (3) a cycloalkenyl group having 5 to 6 carbon atoms, (4) a phenyl group which may be substituted with an amino group, a cyano group, or a formyl group, (5) an acetyl group, (6) an acetoacetyl group, (7) an allyl group, or (8) an acyl group. R (9) a pyridyl group, (10) an alkylsulfo group which may be substituted with a hydroxyl group, or (11) a formyl group, and n is 0, 1, or 2.

[0064] Specific examples of the compound represented by the general formula (1) include morpholine, 4-methylmorpholine, 4-ethylmorpholine, 4-n-propylmorpholine, 4-isopropylmorpholine, 4-n-butylmorpholine, 4-isobutylmorpholine, 4-pentylmorpholine, 4-hexylmorpholine, (R)-3-methylmorpholine, (S)-3-methylmorpholine, cis-2,6-dimethylmorpholine, 4-(1-cyclohexenyl)morpholine, 1-morpholino-1-cyclopentene, 4-phenylmorpholine, 4-(p-tolyl)morpholine, 4-(2-aminoethyl)morpholine, 4-(3-aminopropyl)morpholine, 2-morpholinoaniline, 4-morpholinoaniline, and the like. phosphorus, 4-(2-morpholinoethoxy)aniline, 4-(4-pyridyl)morpholine, 4-aminomorpholine, 4-(2-hydroxypropyl)morpholine, 4-(2-hydroxyethyl)morpholine, 4-(3-hydroxypropyl)morpholine, 2-hydroxy-3-morpholinopropanesulfonic acid, 2-morpholinoethanesulfonic acid, 3-morpholinopropanesulfonic acid, 4-acetylmorpholine, 4-acetoacetylmorpholine, 4-acryloylmorpholine, 4-allylmorpholine, phenyl)morpholine, 3-(morpholino)ethylpropionate, 4-formylmorpholine, 4-(4-formylphenyl)morpholine, and salts of the above compounds.

[0065] Among these, morpholine, 4-ethylmorpholine, 4-n-butylmorpholine, 4-isobutylmorpholine, 4-phenylmorpholine, 4-(2-hydroxypropyl)morpholine, 4-(2-hydroxyethyl)morpholine, and 4-(3-hydroxypropyl)morpholine are preferred in terms of productivity.

[0066] The amount of the morpholine compound added to the dispersion liquid a is preferably 0.1 to 4 equivalents, more preferably 0.4 to 2 equivalents, relative to the neutralization equivalent of the dispersion liquid a. If the amount is 0.1 equivalent or more, the effect of the addition is remarkable. If the amount is 4 equivalents or less, the polyanion doped in the conjugated conductive polymer is unlikely to be dedoped.

[0067] The amount of the morpholine compound added to the dispersion liquid a is preferably adjusted so that the pH is in the range of 3 to 13, more preferably 4 to 7. If the pH is 3 or higher, corrosion due to the valve metal used, such as aluminum, is less likely to progress. If the pH is 13 or lower, undoping of the polyanion doped in the conductive polymer is less likely to occur.

[0068] [Other additives] In addition to the morpholine compound represented by the general formula (1), other additives may be added to the dispersion liquid b as necessary. The other additives are not particularly limited as long as they can be mixed with the conjugated conductive polymer and the seed particles or polyanions that have been made into a protective colloid by the polyanions. The other additives may also be added in step (A). Examples of such additives include water-soluble polymer compounds, water-dispersible compounds, alkaline compounds, surfactants, antifoaming agents, coupling agents, antioxidants, electrical conductivity improvers, etc. These additives may be used alone or in combination of two or more.

[0069] The water-soluble polymer compound is a water-soluble polymer having a cationic group or a nonionic group in the main chain or side chain of the polymer.Specific examples of the water-soluble polymer compound include polyoxyalkylene, water-soluble polyurethane, water-soluble polyester, water-soluble polyamide, water-soluble polyimide, water-soluble polyacrylic, water-soluble polyacrylamide, polyvinyl alcohol, polyacrylic acid, etc.Among these, polyoxyalkylene is preferred.

[0070] Specific examples of polyoxyalkylenes include diethylene glycol, triethylene glycol, oligopolyethylene glycol, triethylene glycol monochlorhydrin, diethylene glycol monochlorhydrin, oligoethylene glycol monochlorhydrin, triethylene glycol monobromohydrin, diethylene glycol monobromohydrin, oligoethylene glycol monobromohydrin, polyethylene glycol, glycidyl ethers, polyethylene glycol glycidyl ethers, polyethylene oxide, triethylene glycol dimethyl ether, tetraethylene glycol dimethyl ether, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, diethylene glycol dibutyl ether, dipropylene glycol, tripropylene glycol, polypropylene glycol, polypropylene dioxide, polyoxyethylene alkyl ethers, polyoxyethylene glycerin fatty acid esters, and polyoxyethylene fatty acid amides.

[0071] The water-dispersible compound is a compound in which a part of a compound with low hydrophilicity is replaced with a functional group with high hydrophilicity, or a compound with a functional group with high hydrophilicity is adsorbed around the compound with low hydrophilicity (for example, an emulsion, etc.), and can be dispersed in water without precipitating.Specific examples include polyester, polyurethane, acrylic resin, silicone resin, and emulsions of these polymers.Furthermore, block copolymers and graft copolymers of acrylic resin and other copolymers such as polyester and polyurethane can be mentioned. The water-soluble polymer compound and the water-dispersible compound can be used alone or in combination of two or more. By adding the water-soluble polymer compound and the water-dispersible compound, the viscosity of the dispersion containing the conductive polymer can be adjusted and the coating performance can be improved.

[0072] The amount of the water-soluble polymer compound and the water-dispersible compound used is preferably 1 to 4000 parts by mass, more preferably 50 to 2000 parts by mass, relative to 100 parts by mass in total of the conjugated conductive polymer and the seed particles made into a protective colloid by a polyanion. When the amount of the water-soluble polymer compound and the water-dispersible compound is in the range of 1 to 4000 parts by mass, appropriate conductivity can be exhibited, and a good equivalent series resistance (ESR) of the solid electrolytic capacitor can be obtained.

[0073] In addition to the morpholine compound, an alkaline compound may be added to the dispersion B. The addition of the alkaline compound can impart corrosion resistance to the article to which the dispersion is applied, and can also adjust the pH of the dispersion containing the conjugated conductive polymer.

[0074] As the alkaline compound, known inorganic alkaline compounds and organic alkaline compounds other than morpholine compounds can be used. Examples of inorganic alkaline compounds include ammonia, sodium hydroxide, potassium hydroxide, calcium hydroxide, and ammonia. Examples of organic alkaline compounds include aromatic amines, aliphatic amines, and alkali metal alkoxides.

[0075] Among aromatic amines, nitrogen-containing heteroaryl ring compounds are preferred. Nitrogen-containing heteroaryl ring compounds are nitrogen-containing heterocyclic compounds that exhibit aromaticity. In aromatic amines, the nitrogen atom contained in the heterocyclic ring has a conjugated relationship with other atoms. Examples of the nitrogen-containing heteroaryl ring compound include pyridines, imidazoles, pyrimidines, pyrazines, triazines, etc. Among these, pyridines, imidazoles, and pyrimidines are preferred from the viewpoint of solvent solubility, etc.

[0076] Examples of the aliphatic amine include ethylamine, n-octylamine, diethylamine, diisobutylamine, methylethylamine, trimethylamine, triethylamine, allylamine, 2-ethylaminoethanol, 2,2'-iminodiethanol, and N-ethylethylenediamine.

[0077] Examples of the alkali metal alkoxide include sodium alkoxides such as sodium methoxide and sodium ethoxide, potassium alkoxides, and calcium alkoxides.

[0078] Examples of the surfactant include anionic surfactants such as carboxylates, sulfonates, sulfate salts, and phosphate salts; cationic surfactants such as amine salts and quaternary ammonium salts; amphoteric surfactants such as carboxybetaine, aminocarboxylate salts, and imidazolium betaine; and nonionic surfactants such as polyoxyethylene alkyl ethers, polyoxyethylene glycerin fatty acid esters, ethylene glycol fatty acid esters, and polyoxyethylene fatty acid amides.

[0079] The antifoaming agent includes silicone resin, polydimethylsiloxane, silicone resin, and the like. Examples of the antioxidant include phenol-based antioxidants, amine-based antioxidants, phosphorus-based antioxidants, sulfur-based antioxidants, sugars, vitamins, and the like.

[0080] The electrical conductivity enhancer is not particularly limited as long as it increases the electrical conductivity of the dispersion containing the conductive polymer. Examples of the electrical conductivity improver include compounds containing an ether bond such as tetrahydrofuran; compounds containing a lactone group such as γ-butyrolactone and γ-valerolactone; compounds containing an amide or lactam group such as caprolactam, N-methylcaprolactam, N,N-dimethylacetamide, N-methylacetamide, N,N-dimethylformamide, N-methylformamide, N-methylformanilide, N-methylpyrrolidone, N-octylpyrrolidone, and pyrrolidone; sulfone compounds or sulfoxide compounds such as tetramethylene sulfone and dimethyl sulfoxide; sugars or sugar derivatives such as sucrose, glucose, fructose, and lactose; sugar alcohols such as sorbitol and mannitol; imides such as succinimide and maleimide; furan derivatives such as 2-furan carboxylic acid and 3-furan carboxylic acid; and dialcohols or polyalcohols such as ethylene glycol, propylene glycol, glycerin, diethylene glycol, and triethylene glycol. Among these, from the viewpoint of improving electrical conductivity, tetrahydrofuran, N-methylformamide, N-methylpyrrolidone, ethylene glycol, propylene glycol, glycerin, dimethyl sulfoxide, and sorbitol are preferred, and among these, ethylene glycol, propylene glycol, and glycerin are more preferred. The electrical conductivity improver can be used alone or in combination of two or more kinds.

[0081] <Step (C) of applying a dispersion liquid (dispersion liquid b) containing a morpholine compound and a conjugated conductive polymer to a porous anode body> The method for producing a solid electrolytic capacitor of the present invention includes a step (C) of depositing the dispersion liquid b obtained in the above-described step (B) onto the surface of a porous anode body having an anode body made of a valve metal and a dielectric coating formed on at least a portion of the surface of the anode body. The solid electrolytic capacitor according to the manufacturing method of the present invention may have, for example, a porous electrode formed by sintering valve metal powder having a large surface area, or a porous film obtained by etching a valve metal foil. The valve metal includes aluminum (Al), beryllium (Be), bismuth (Bi), magnesium (Mg), germanium (Ge), hafnium (Hf), niobium (Nb), antimony (Sb), silicon (Si), tin (Sn), tantalum (Ta), titanium (Ti), vanadium (V), tungsten (W) and zirconium (Zr), as well as alloys or compounds of at least one of these metals with other elements.Among these, the electrode material made of the valve metal of Al, Nb or Ta is preferred.

[0082] A porous electrode made of a valve metal is turned into a porous anode body by forming a dielectric oxide film on the surface thereof, for example, by anodization. The porous electrode can be anodized by applying a voltage in a phosphoric acid solution to form a dielectric oxide film. The formation voltage can be determined based on the thickness of the dielectric oxide film and the withstand voltage of the capacitor. The formation voltage is preferably 1 to 800 V, more preferably 1 to 300 V.

[0083] Next, the dispersion liquid b is applied to the porous anode body. Examples of the application method include known methods such as coating, spraying, and immersion. Among these, the immersion method is preferred because the dispersion liquid b can be applied and permeated uniformly into the porous anode body without unevenness. In order to impregnate the fine parts of the porous anode body, the impregnation may be performed under reduced pressure. The immersion time is usually about 10 seconds to 5 minutes, and the temperature of the dispersion liquid b is usually about 10 to 35° C., although it depends on the type of the dispersion medium.

[0084] <Step (D) of forming solid electrolyte layer> The method for producing a solid electrolytic capacitor of the present invention includes a step (D) of forming a solid electrolyte layer by removing the dispersion medium from the dispersion liquid b attached to the porous anode body obtained in the above-mentioned step (C). The removal of the dispersion medium in this step (D) does not mean removing all of the dispersion medium, and it is acceptable for some of the dispersion medium to remain within a range that does not affect the production of the solid electrolytic capacitor. The dispersion medium is preferably removed by drying through a heat treatment from the viewpoint of efficiency. The heating conditions can be determined taking into consideration the boiling point and volatility of the dispersion medium. Heating is preferably carried out within a temperature range where the conductive polymer is not deteriorated by oxygen, for example, from room temperature to 300°C, and preferably from 50 to 200°C. The heat treatment time is preferably from 5 seconds to several hours. The heat treatment may be carried out, for example, in the atmosphere using a hot plate, an oven, or a hot air dryer, or under reduced pressure to carry out the heat treatment quickly.

[0085] In the present invention, depending on the type of the electrode body, the step (C) of applying the above-mentioned dispersion liquid and the step (D) of forming the solid electrolyte layer may be repeated once or twice or more. A heat treatment may be performed each time the dispersion liquid is applied to remove part or all of the dispersion medium, or the dispersion liquid may be applied several times in succession and the dispersion medium may be removed at the end. Furthermore, after removing part or all of the dispersion medium contained in the applied dispersion liquid, any electrolyte solution may be impregnated. EXAMPLES

[0086] The present invention will be described in detail below with reference to examples and comparative examples, but the present invention is not limited to these examples. The methods for measuring the various physical properties of the dispersions in the examples and comparative examples are as follows.

[0087] (1) Solid content concentration The solids concentration in each example was measured using an infrared moisture meter (Kett Electric Laboratory, Model FD-720, heating conditions 110°C / 30 minutes) on approximately 10 g of the sample obtained in each example, and the evaporation residue was calculated as the solids content. (2) pH The pH of the dispersion obtained in each example was measured at 25° C. using a pH meter (manufactured by DKK-TOA Corporation, Model HM-30G). (3) Seed particle size The measurement was performed using a Microtrac UPA type particle size distribution measuring device manufactured by Nikkiso Co., Ltd. (4) Weight average molecular weight of sodium polystyrene sulfonate Measurements were performed using gel permeation chromatography. For the measurements, Showa Denko K.K.'s "Shodex (registered trademark) GPC 101" (column OHPak SB-806M HQ) was used, and the measurement conditions were a column temperature of 40°C, water as the eluent, and an elution rate of 1 ml / min. The molecular weights were expressed in terms of standard polystyrene (Mw).

[0088] Example 1: [Preparation of a dispersion of seed particles protected by polyanion] 86 g of styrene, 49 g of 2-ethylhexyl acrylate, 15 g of divinylbenzene, and 500 g of 22% by mass aqueous solution of sodium polystyrene sulfonate (Polynas PS-5, manufactured by Tosoh Organic Chemical Co., Ltd., weight average molecular weight: about 120000) were mixed with stirring to prepare a monomer mixture. Meanwhile, 1000 g of 22% by mass aqueous solution of sodium polystyrene sulfonate (same as above) was heated to 80°C while stirring, and 2 g of potassium persulfate was added thereto. The monomer mixture and 40 g of 2.5% by mass aqueous solution of potassium persulfate were dropped into this solution over 2 hours and 2.5 hours, respectively. After the dropwise addition, the mixture was kept at 80°C for 2 hours, and then cooled to room temperature (25°C). 1500 ml of a cation exchange resin (IR120B-H, manufactured by Organo Corporation) and 1500 ml of an anion exchange resin (IRA410-OH, manufactured by Organo Corporation) were added to the obtained reaction solution, and after stirring for 12 hours, the ion exchange resin was filtered off. Ion exchange water (hereinafter simply referred to as water) was added to adjust the solid content concentration to 15.0 mass%, and a dispersion of seed particles (Tg: 30°C, particle size d50: 0.46 μm) that were made into a protective colloid with polyanion was obtained.

[0089] [Step (A): Production of a conjugated conductive polymer-containing dispersion (dispersion a) containing seed particles protected by a polyanion] In a 1L polyethylene container, 223.2 g of water, 31.5 g of a 12% by mass aqueous solution of sodium polystyrene sulfonate, and 34.0 g of the dispersion of seed particles protected by polyanion prepared above were mixed by stirring at 32°C. 2.80 g of 3,4-ethylenedioxythiophene was added to this mixture at 32°C, and emulsified and mixed for 30 minutes with a homomixer (manufactured by Tokushu Kika Kogyo Co., Ltd., Robomix; 4000 rpm) to prepare a monomer dispersion (sulfo group content per mole of 3,4-ethylenedioxythiophene: 1.9 moles). The sulfo groups are derived from the 12% by mass aqueous solution of sodium polystyrene sulfonate and the sodium polystyrene sulfonate in the dispersion. The monomer dispersion was put into a 1L stainless steel vessel connected to a high-shear mixer (Milder (registered trademark) 303V; 5000 rpm, manufactured by Pacific Machinery Co., Ltd.) and a circulation pump, and stirred while circulating at 32°C with a stirring blade and a high-shear mixer. 5.89 g of sodium peroxodisulfate and 6.88 g of a 1% by mass aqueous solution of iron (III) sulfate hexahydrate were added as oxidizing agents, and a polymerization reaction was carried out for 24 hours. 221 g of the obtained reaction liquid and 79 g of water were put into a 1L stainless steel vessel connected to a high-shear mixer (Magic Lab; 1800 rpm, manufactured by IKA Co., Ltd.) and a circulation pump, and stirred while circulating for 12 hours to carry out a dispersion treatment. To 300 g of the obtained dispersion, 300 mL of the cation exchange resin (same as above) and 300 mL of the anion exchange resin (same as above) were added, and the mixture was stirred for 6 hours. The ion exchange resin was then filtered off. By this operation, the unreacted monomer and the oxidizing agent were removed, and a dispersion (solid concentration 2.7 mass %, pH 1.9) containing a complex of the seed particles protected by a polyanion and the conjugated conductive polymer was obtained. [Step (B): Preparation of a dispersion containing a morpholine compound and a conjugated conductive polymer (dispersion b)] Morpholine was added to the obtained dispersion, and pure water was further added to obtain a dispersion having a solid content concentration of 1.6 mass% and a pH of 4.9. Furthermore, 5 parts by mass of ethylene glycol was added to 100 parts by mass of the obtained dispersion to obtain an impregnation solution (1-1) for preparing a solid electrolytic capacitor.

[0090] [Formation of a porous anode body having a dielectric oxide film on its surface] A porous anode body having a dielectric oxide coating on its surface for use in a solid electrolytic capacitor was manufactured by the method described in JP 2011-77257 A. That is, a porous anode body with an anode lead was manufactured using niobium powder for capacitors, in which a dielectric oxide coating having diniobium pentoxide was formed on the anode body surface. The capacitance of this porous anode body in 20% sulfuric acid was 21.4 μF.

[0091] [Steps (C) and (D): Preparation of solid electrolytic capacitor] The porous anode body obtained by the above method was immersed in the dispersion liquid (1-1) for 1 minute under the atmosphere at 25°C, and then dried in a hot air dryer (TABAI, model ST-110) at 120°C for 30 minutes. This process was repeated 10 times. Next, carbon paste was applied to the porous anode body so as not to contact the anode lead terminal, and then dried. Furthermore, silver paste was applied to the anode and cathode to establish contact, and the anode was placed on a lead frame and dried. The anode lead wire of the element was electrically connected to the anode lead part of the lead frame, and the element was sealed with resin, thereby obtaining a solid electrolytic capacitor element. The capacitance (μF) of the obtained solid electrolytic capacitor element at 120 Hz was measured using an LCR meter, and was taken as the initial capacitance. Next, the element was left in a hot air dryer at 130°C for 250 hours, and then the capacitance (μF) at 120 Hz was measured. The results are shown in Table 1.

[0092] Example 2: Instead of morpholine in Example 1, 4-ethylmorpholine was added to obtain a dispersion with a solid content concentration of 1.7% by mass and a pH of 4.5. Furthermore, 5 parts by mass of ethylene glycol was added to 100 parts by mass of the obtained dispersion to obtain an impregnation solution (1-2) for preparing a solid electrolytic capacitor. A solid electrolytic capacitor element was prepared in the same manner as in Example 1, and the capacitance (μF) at 120 Hz was measured using an LCR meter. Furthermore, the obtained element was left in a hot air dryer at 130° C. for 250 hours, after which the capacitance (μF) at 120 Hz was measured. The results are shown in Table 1.

[0093] Example 3: Instead of morpholine in Example 1, 4-(2-hydroxyethyl)morpholine was added to obtain a dispersion with a solid content concentration of 1.7% by mass and a pH of 4.7. Furthermore, 5 parts by mass of ethylene glycol was added to 100 parts by mass of the obtained dispersion to obtain an impregnation solution (1-3) for preparing a solid electrolytic capacitor. A solid electrolytic capacitor element was prepared in the same manner as in Example 1, and the capacitance (μF) at 120 Hz was measured using an LCR meter. Furthermore, the obtained element was left in a hot air dryer at 130° C. for 250 hours, after which the capacitance (μF) at 120 Hz was measured. The results are shown in Table 1.

[0094] Example 4: [Step (A): Production of a polyanion-containing conjugated conductive polymer-containing dispersion (dispersion a) (not including seed particles)] In a 1 L polyethylene container, 231.0 g of water and 60.0 g of a 12 mass % aqueous solution of sodium polystyrene sulfonate were mixed by stirring at 32° C. To this mixture, 2.80 g of 3,4-ethylenedioxythiophene was added at 32° C., and the mixture was emulsified and mixed for 30 minutes with a homomixer (Robomix, manufactured by Tokushu Kika Kogyo Co., Ltd.; 4000 rpm) to prepare a monomer dispersion. The monomer dispersion was put into a 1L stainless steel vessel connected to a high-shear mixer (Milder (registered trademark) 303V; 5000 rpm, manufactured by Pacific Machinery Co., Ltd.) and a circulation pump, and stirred while circulating at 32°C with a stirring blade and a high-shear mixer. 5.89 g of sodium peroxodisulfate and 6.88 g of a 1% by mass aqueous solution of iron (III) sulfate hexahydrate were added as oxidizing agents, and a polymerization reaction was carried out for 24 hours. 221 g of the obtained reaction liquid and 79 g of water were put into a 1L stainless steel vessel connected to a high-shear mixer (Magic Lab; 1800 rpm, manufactured by IKA Co., Ltd.) and a circulation pump, and stirred while circulating for 12 hours to carry out a dispersion treatment. To 300 g of the obtained dispersion, 300 mL of the cation exchange resin (same as above) and 300 mL of the anion exchange resin (same as above) were added, and the mixture was stirred for 6 hours. After that, the ion exchange resin was filtered off. By this operation, the unreacted monomer and the oxidizing agent were removed, and a dispersion containing a complex of the polyanion and the conjugated conductive polymer (solid concentration: 2.6 mass%, pH 1.8) was obtained.

[0095] [Step (B): Preparation of a dispersion (dispersion b) containing a morpholine compound and a conjugated conductive polymer (not including seed particles)] Morpholine was added to the obtained dispersion to obtain a dispersion with a solid content concentration of 1.6% by mass and a pH of 4.6. Furthermore, 5 parts by mass of ethylene glycol was added to 100 parts by mass of the obtained dispersion to obtain an impregnation solution (1-4) for preparing a solid electrolytic capacitor. A solid electrolytic capacitor element was prepared in the same manner as in Example 1, and the capacitance (μF) at 120 Hz was measured using an LCR meter. Furthermore, the obtained element was left in a hot air dryer at 130° C. for 250 hours, after which the capacitance (μF) at 120 Hz was measured. The results are shown in Table 1.

[0096] Comparative Example 1: A dispersion liquid with a solid content concentration of 1.4% by mass and a pH of 1.9 was obtained without adding morpholine as in Example 1. Five parts by mass of ethylene glycol was added to 100 parts by mass of the dispersion liquid to obtain an impregnation liquid (1-5) for preparing a solid electrolytic capacitor. A solid electrolytic capacitor element was prepared in the same manner as in Example 1, and the capacitance (μF) at 120 Hz was measured using an LCR meter. Furthermore, the obtained element was left in a hot air dryer at 130° C. for 250 hours, after which the capacitance (μF) at 120 Hz was measured. The results are shown in Table 1.

[0097] Comparative Example 2: Ammonia water was added instead of morpholine in Example 1 to obtain a dispersion liquid having a solid content concentration of 1.5 mass% and a pH of 4.8. Furthermore, 5 parts by mass of ethylene glycol was added to 100 parts by mass of the obtained dispersion liquid to obtain an impregnation solution (1-6) for preparing a solid electrolytic capacitor. A solid electrolytic capacitor element was prepared in the same manner as in Example 1, and the capacitance (μF) at 120 Hz was measured using an LCR meter. Furthermore, the capacitance (μF) at 120 Hz of the obtained element was measured after leaving it in a hot air dryer at 130° C. for 250 hours. The results are shown in Table 1.

[0098] [Table 1]

[0099] The results in Table 1 show that the solid electrolytic capacitor elements of Examples 1 to 4, which used a dispersion liquid containing a conjugated conductive polymer to which a morpholine compound was added in the process of attaching the dispersion liquid to a porous electrode body made of a valve action metal having a dielectric coating, have a more stable capacitance expression rate (capacitance), are more heat resistant, and are more reliable under high temperature conditions than the solid electrolytic capacitor elements of Comparative Examples 1 and 2, which do not contain a morpholine compound. [Industrial Applicability]

[0100] According to the present invention, it is possible to provide a conjugated conductive polymer-containing dispersion for obtaining a solid electrolytic capacitor having a high capacity expression rate (electrostatic capacitance), excellent heat resistance, and high reliability under high temperature conditions. Furthermore, according to the present invention, it is possible to produce an industrially useful solid electrolytic capacitor that has a high capacitance expression rate (electrostatic capacitance), excellent heat resistance, and high reliability under high temperature conditions.

Claims

1. A seed particle protected by a polyanion or a polyanion; A conjugated conductive polymer; The following general formula (1) 【Chemistry 1】 (In the formula, R 1 represents (1) a hydrogen atom, (2) an alkyl group having 1 to 8 carbon atoms which may be substituted with a hydroxyl group, a cyano group, or an amino group, (3) a cycloalkenyl group having 5 to 6 carbon atoms, (4) a phenyl group which may be substituted with an amino group, a cyano group, or a formyl group, (7) an allyl group, (9) a pyridyl group, or (10) an alkylsulfo group which may be substituted with a hydroxyl group, and n is 0, 1, or 2.

2. The conjugated conductive polymer-containing dispersion according to claim 1 , wherein the dispersion medium is an aqueous medium.

3. The conjugated conductive polymer-containing dispersion according to claim 1 or 2, wherein the morpholine compound represented by the general formula (1) is morpholine, 4-ethylmorpholine, 4-n-butylmorpholine, 4-isobutylmorpholine, 4-phenylmorpholine, 4-(2-hydroxypropyl)morpholine, 4-(2-hydroxyethyl)morpholine, or 4-(3-hydroxypropyl)morpholine.

4. 4. The conjugated conductive polymer-containing dispersion according to claim 3, wherein the morpholine compound is 4-ethylmorpholine.

5. The conjugated conductive polymer-containing dispersion according to any one of claims 1 to 4, further comprising an electrical conductivity improver as an additive, and the electrical conductivity improver comprises at least one selected from ethylene glycol, propylene glycol, and glycerin.

6. A step (A) of polymerizing a monomer for obtaining a conjugated conductive polymer in a dispersion medium containing seed particles that have been made into a protective colloid by a polyanion or in a dispersion medium containing a polyanion to obtain a conjugated conductive polymer-containing dispersion; The conjugated conductive polymer-containing dispersion liquid is added with a compound represented by the following general formula (1): 【Chemistry 2】 (In the formula, R 1 represents (1) a hydrogen atom, (2) an alkyl group having 1 to 8 carbon atoms which may be substituted with a hydroxyl group, a cyano group, or an amino group, (3) a cycloalkenyl group having 5 to 6 carbon atoms, (4) a phenyl group which may be substituted with an amino group, a cyano group, or a formyl group, (5) an acetyl group, (6) an acetoacetyl group, (7) an allyl group, (8) an acryloyl group, (9) a pyridyl group, (10) an alkylsulfo group which may be substituted with a hydroxyl group, or (11) a formyl group, and n is 0, 1, or 2; A step (C) of depositing the dispersion onto a porous anode body made of a valve metal having a dielectric coating on its surface; and (D) removing the dispersion medium from the dispersion liquid containing the morpholine compound and the conjugated conductive polymer attached to the porous anode body to form a solid electrolyte layer, The method for producing a solid electrolytic capacitor, wherein in the step (B), the dispersion liquid containing the morpholine compound and the conjugated conductive polymer has a pH of 3 to 13.

7. A step (A) of polymerizing a monomer for obtaining a conjugated conductive polymer in a dispersion medium containing seed particles that have been made into a protective colloid by a polyanion or in a dispersion medium containing a polyanion to obtain a conjugated conductive polymer-containing dispersion; A step (B) of adding 4-ethylmorpholine to the conjugated conductive polymer-containing dispersion liquid to prepare a dispersion liquid containing the 4-ethylmorpholine and the conjugated conductive polymer; A step (C) of depositing the dispersion onto a porous anode body made of a valve metal having a dielectric coating on its surface; and (D) removing a dispersion medium from the dispersion liquid containing 4-ethylmorpholine and a conjugated conductive polymer adhered to the porous anode body to form a solid electrolyte layer.

8. The method for producing a solid electrolytic capacitor according to claim 6, wherein the morpholine compound represented by the general formula (1) is morpholine, 4-ethylmorpholine, 4-n-butylmorpholine, 4-isobutylmorpholine, 4-phenylmorpholine, 4-(2-hydroxypropyl)morpholine, 4-(2-hydroxyethyl)morpholine, or 4-(3-hydroxypropyl)morpholine.

9. 9. The method for producing a solid electrolytic capacitor according to claim 6, wherein the seed particles are particles of a polymer of an ethylenically unsaturated monomer.

10. 10. The method for producing a solid electrolytic capacitor according to claim 6, wherein the seed particles which have been made into a protective colloid by the polyanion have a d50 particle size of 0.01 to 10 μm.

11. The method for producing a solid electrolytic capacitor according to any one of claims 6 to 10, wherein in the step (A) of obtaining the conjugated conductive polymer-containing dispersion liquid, the resulting conjugated conductive polymer is subjected to a dispersion treatment.

12. The method for producing a solid electrolytic capacitor according to claim 11, wherein the dispersion treatment is ultrasonic irradiation.

13. The monomer for obtaining the conjugated conductive polymer is represented by the following formula (2): 【Chemistry 3】 (In the formula, R 2 and R 3 each independently represents a hydrogen atom, a hydroxyl group, an alkyl group having 1 to 18 carbon atoms which may have a substituent, an alkoxy group having 1 to 18 carbon atoms which may have a substituent, or an alkylthio group having 1 to 18 carbon atoms which may have a substituent, or R 2 and R 3 and are bonded to each other to form an alicyclic ring having 3 to 10 carbon atoms which may have a substituent, an aromatic ring having 6 to 10 carbon atoms which may have a substituent, an oxygen-atom-containing heterocyclic ring having 2 to 10 carbon atoms which may have a substituent, a sulfur-atom-containing heterocyclic ring having 2 to 10 carbon atoms which may have a substituent, or a sulfur-atom and oxygen-atom-containing heterocyclic ring having 2 to 10 carbon atoms which may have a substituent.

14. The method for producing a solid electrolytic capacitor according to any one of claims 6 to 13, wherein the polyanion is a polymer having a sulfo group.

15. The method for producing a solid electrolytic capacitor according to any one of claims 6 to 14, wherein a ratio of an anion group in the polyanion is 0.25 to 30 mol per 1 mol of the monomer for obtaining the conjugated conductive polymer.

16. 16. The method for producing a solid electrolytic capacitor according to claim 6, wherein in the step (B), at least one selected from the group consisting of ethylene glycol, propylene glycol, and glycerin is added as an electrical conductivity improver.

17. A seed particle protected by a polyanion or a polyanion; A conjugated conductive polymer; The following general formula (1) 【Chemistry 4】 (wherein R 1 represents (1) a hydrogen atom, (2) an alkyl group having 1 to 8 carbon atoms which may be substituted with a hydroxyl group, a cyano group or an amino group, (3) a cycloalkenyl group having 5 to 6 carbon atoms, (4) a phenyl group which may be substituted with an amino group, a cyano group or a formyl group, (5) an acetyl group, (6) an acetoacetyl group, (7) an allyl group, (8) an acryloyl group, (9) a pyridyl group, (10) an alkylsulfo group which may be substituted with a hydroxyl group, or (11) a formyl group, and n is 0, 1 or 2), a dispersion medium, and an electrical conductivity improver as an additive, wherein the electrical conductivity improver comprises at least one selected from ethylene glycol, glycerin, diethylene glycol and triethylene glycol.

18. The conjugated conductive polymer-containing dispersion according to claim 17, wherein the electrical conductivity enhancer is at least one selected from ethylene glycol and glycerin.

Citation Information

Patent Citations

  • Disk type electric contact

    JP1980028214A

  • Method of manufacturing solid electrolytic capacitor

    JP2003100561A

  • Method of manufacturing solid electrolytic capacitor

    JP2005109252A

  • Electrolytic solution for driving electrolytic capacitor, and electrolytic capacitor

    JP2008085240A

  • Hard coat film, and, antireflection film, polarizing plate and displaying device using the same

    JP2009196202A