Clad sheet material for metal masks and metal masks

The clad plate material for metal masks, using an Fe-based alloy with controlled etching, addresses thickness and handling issues, enabling efficient production of thin, stable metal masks with improved definition and productivity.

JP7552780B2Active Publication Date: 2024-09-18PROTERIAL LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023068084
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2023-04-18
Publication Date
2024-09-18
Estimated Expiration
2039-03-27

Smart Images

  • Figure 0007552780000001
    Figure 0007552780000001
  • Figure 0007552780000019
    Figure 0007552780000019
  • Figure 0007552780000006
    Figure 0007552780000006
Patent Text Reader

Abstract

To provide a plate material for a metal mask, facilitating handling, capable of thinning a metal mask, and preferably, enabling productivity improvement of a metal mask, and to provide a metal mask using the same.SOLUTION: A clad plate material for a metal mask comprises a substrate layer comprising Fe base alloy containing 30 mass% or more and 50 mass% or less of at least one kind selected from Ni and Co, and a first carrier layer pressure-welded to one side of the substrate layer in a view of a cross section cut in a thickness direction. The substrate layer and the first carrier layer can be etched with a homogenous ferric chloride solution, and the substrate layer has higher corrosion resistance to the ferric chloride solution than the first carrier layer. A metal mask using the clad plate material for a metal mask is also provided.SELECTED DRAWING: Figure 3
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a clad sheet material for a metal mask and a metal mask. More specifically, the present invention relates to a clad plate material for metal masks having a metal surface on which a corrosion-resistant protective film against etching solutions can be formed, and a metal mask using this clad plate material for metal masks, for example, a clad plate material for metal masks for producing metal masks for organic EL elements, and a metal mask for organic EL elements. [Background technology]

[0002] For example, Patent Document 1 discloses a method for manufacturing a masking jig (metal mask) made of a single type of metal used in the manufacture of organic EL elements. This metal mask is manufactured by the process shown in FIG. 1. In FIG. 1, step (a) is a material preparation process. In this material preparation process, a masking jig made of a single type of metal with a thickness T 100 A single-layered metal plate 100a is prepared. The metal plate 100a is made of an Fe-Ni alloy containing, for example, about 36% by mass of Ni (nickel) and about 64% by mass of Fe (iron). The Fe-Ni alloy is a well-known 36 alloy, which has a small linear expansion coefficient of about 1.2×10 -6 / °C. The thickness T of the metal plate 100a 100is, for example, 10 μm or more and 50 μm or less. Step (b) is a first coating step. In this first coating step, a protective film 101 for forming a predetermined etching pattern is formed on the first surface 100b of the metal plate 100a, and a protective film 102 for preventing etching is formed on the second surface 100c of the metal plate 100a. Step (c) is a first etching step. In this first etching step, the metal plate 100a is etched using an etching solution suitable for the Fe-Ni alloy. By this first etching, a portion of the first surface 100b made of the Fe-Ni alloy that does not have the protective film 101 is etched, and for example, an etching hole 100d is formed. Step (d) is a second coating step. In this second coating step, a protective film 103 for forming a predetermined etching pattern is formed on the second surface 100c of the metal plate 100a, and a protective film 104 for preventing etching is formed on the first surface 100b and the etching hole 100d of the metal plate 100a. Step (e) is a second etching step. In this second etching step, the metal plate 100a is etched using an etching solution of the same quality as that used in the first etching step. This second etching etches the portion of the second surface 100c made of an Fe-Ni alloy that does not have the protective film 103, and for example, an etching hole 100e is formed. Step (f) is a finishing step. In this finishing step, the protective film 103 and the protective film 104 are removed, and the entire surface of the metal plate 100a is cleaned and finished into a metal mask 100. Through these steps, the metal plate 100a is used to etch a metal mask 100 having, for example, a mask pattern 100f and a thickness T substantially equal to that of the metal plate 100a. 100 Thus, a metal mask 100 having a single layer structure made of an Fe-Ni alloy is obtained.

[0003] Also, for example, Patent Document 2 discloses a method for manufacturing a metal mask for thick films used in screen printing. This metal mask is manufactured by the steps shown in FIG. 2. In FIG. 2, step (a) is a material preparation step. In this material preparation step, a clad plate material 200a with a two-layer structure in which two types of metal are bonded, which will become the metal mask, is prepared. Patent Document 2 does not disclose the thickness of the clad plate material 200a, but the clad plate material 200a has a thickness T suitable for a thick film metal mask. 200It is considered that the clad plate material 200a has a first layer 201 made of, for example, copper, and a second layer 202 made of, for example, stainless steel, which is different from the first layer 201. Since an etching solution suitable for copper and an etching solution suitable for stainless steel are different, the first layer 201 made of copper is not etched with an etching solution suitable for the second layer made of stainless steel, and the second layer 202 made of stainless steel is not etched with an etching solution suitable for the first layer 201 made of copper. Step (b) is a coating step. In this coating step, a protective film 203 for forming a predetermined etching pattern is formed on the surface 201a of the first layer 201, and a protective film 204 for forming a predetermined etching pattern is formed on the surface 202a of the second layer 202. Step (c) is a first etching step. In this first etching step, the surface 201a of the first layer 201 is etched using an etching solution suitable for copper. By this first etching, the surface 201a portion of the first layer 201 made of copper that does not have the protective film 203 is etched, and for example, an etching hole 201b is formed. At this time, the surface 202a portion of the second layer 202 made of stainless steel that does not have the protective film 204 is not etched. Step (d) is a second etching step. In this second etching step, the surface 202a of the second layer 202 is etched using an etching solution suitable for stainless steel, which is different from that in the first etching step. By this second etching, the surface 202a portion of the second layer 202 made of stainless steel that does not have the protective film 204 is etched, and for example, an etching hole 202b is formed. At this time, the etching hole 201b of the first layer 201 made of copper that does not have the protective film 203 is not etched. Step (e) is a finishing step. In this finishing step, the protective film 203 and the protective film 204 are removed, and the entire surface of the clad plate material 200a is cleaned and finished into a metal mask 200. Through these steps, the clad plate material 200a is used to form a mask pattern 200f having a thickness T 200 Thus, a metal mask 200 having a two-layer structure made of copper and stainless steel is obtained. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Patent No. 643072 [Patent Document 2] Special Publication No. 62-21629 Summary of the Invention [Problem to be solved by the invention]

[0005] In recent years, there has been a demand for even higher definition mask patterns. To achieve this, it is necessary to further reduce the thickness of the metal mask. The target thickness of the metal mask is, for example, 20 μm or less, and preferably 15 μm or less. The thickness T of the metal plate material 100a with the single-layer structure described above is 100 The thickness of the clad plate is, for example, 10 μm to 50 μm, but such a thin metal plate is prone to defects such as wrinkles and breaks. For example, it is technically possible to further thin a metal plate having a thickness of 20 μm, but a metal plate that is simply thinned becomes difficult to handle due to a decrease in mechanical strength. The above-mentioned two-layer clad plate 200a is considered to have a thickness suitable for a thick-film metal mask. If such a two-layer clad plate is simply further thinned, the asymmetry of the layer structure in the thickness direction (Z direction shown in FIG. 2) will cause a large warp in the clad plate. Therefore, it is technically not easy to obtain a clad plate having a thickness of, for example, 20 μm or less. A clad plate having a large warp is difficult to handle, and it is not easy to manufacture a metal mask. For these reasons, it is necessary to develop a metal mask plate that enables a metal mask to be further thinned.

[0006] In developing metal mask plate materials, in addition to making them thinner and easier to handle, it is expected that the productivity of metal masks will be maintained at the same level as before, and more preferably that the productivity of metal masks will be improved. In the above-mentioned method for manufacturing a metal mask using a single type of metal plate material 100a, at least two coating steps and two etching steps are required. In addition, in the above-mentioned method for manufacturing a metal mask using a two-layer clad plate material 200a in which different metals are bonded, the number of coating steps can be reduced compared to the method using a single type of metal plate material 100a. However, even in the method using the two-layer clad plate material 200a, at least two etching steps are required to form the mask pattern 200f, and the etchant used in each etching step cannot be shared. Therefore, a favorable change in the metal mask plate material may favorably change the manufacturing process of the metal mask, leading to an improvement in the productivity of the metal mask.

[0007] An object of the present invention is to provide a metal mask sheet material that is easy to handle, enables the production of thin metal masks, and preferably enables improved productivity of metal masks, and to provide a metal mask using this metal mask sheet material. [Means for solving the problem]

[0008] The inventors discovered that the above-mentioned problems can be solved by bonding two types of metal that can be etched with the same etching solution in a two-layer clad plate material in which two types of metal are bonded together, and arrived at the configuration of the invention relating to a clad plate material for use in metal masks.

[0009] One of the inventions relating to a clad plate for metal masks is a clad plate for metal masks, comprising, in a cross-sectional view cut in the thickness direction, a base layer made of an Fe-based alloy containing at least one of Ni and Co in the range of 30% by mass to 50% by mass, and a first carrier layer directly pressed against one side of the base layer, the base layer and the first carrier layer being etchable with a ferric chloride solution of the same quality, and the base layer being more corrosion-resistant to the ferric chloride solution than the first carrier layer. In this invention, etching is performed using a ferric chloride solution of the same quality under the same environment to measure the corrosion loss of the base layer by M. b The corrosion loss of the first carrier layer is M C1 When the base layer and the first carrier layer are b / M c1 The relationship is ≦0.9.

[0010] One of the inventions relating to a clad plate material for metal masks is a clad plate material for metal masks, comprising a base layer made of an Fe-based alloy containing at least one of Ni and Co in the range of 30% by mass to 50% by mass in a cross section cut in the thickness direction, a first carrier layer directly pressed against one side of the base layer, and a second carrier layer directly pressed against the other side of the base layer, wherein the base layer, the first carrier layer, and the second carrier layer can be etched with a ferric chloride solution of the same quality, and the base layer has higher corrosion resistance to the ferric chloride solution than the first carrier layer and the second carrier layer. In this invention, etching is performed using a ferric chloride solution of the same quality under the same environment, and the corrosion loss of the base layer is measured by measuring the corrosion loss of M b The corrosion loss of the first carrier layer is M C1 The corrosion loss of the second carrier layer is M C2 wherein the base layer, the first carrier layer and the second carrier layer are M b / M c1 ≦0.9 and M b / M c2 The relationship is ≦0.9.

[0011] The inventors have come up with a configuration of an invention relating to a metal mask by using any of the above-mentioned clad plate materials for a metal mask. That is, one invention relating to a metal mask is a metal mask formed by using any of the above-mentioned clad plate materials for a metal mask including the base layer and the first carrier layer, or any of the above-mentioned clad plate materials for a metal mask including the base layer, the first carrier layer, and the second carrier layer, and the metal mask is made of the Fe-based alloy constituting the base layer.

[0012] Another invention relating to a metal mask is a metal mask formed using any of the above-mentioned clad plate materials for metal masks comprising the base layer and the first carrier layer, or any of the above-mentioned clad plate materials for metal masks comprising the base layer, the first carrier layer and the second carrier layer, the metal mask comprising a first metal layer made of the Fe-based alloy constituting the base layer, and a second metal layer made of a metal constituting the first carrier layer, and the first metal layer and the second metal layer are directly bonded to each other.

[0013] Another invention relating to a metal mask is a metal mask formed using any of the above-mentioned clad plate materials for metal masks, which has the base layer, the first carrier layer, and the second carrier layer, and which comprises a first metal layer made of the Fe-based alloy constituting the base layer, a second metal layer made of a metal constituting the first carrier layer, and a third metal layer made of a metal constituting the second carrier layer, in which the second metal layer, the first metal layer, and the third metal layer are directly bonded in this order. Effect of the Invention

[0014] According to the present invention, a clad plate material for metal masks is obtained that is easy to handle and enables the production of thinner metal masks. By using this clad plate material for metal masks, metal masks that are easy to handle and thinner than conventional ones can be obtained. Furthermore, by using this clad plate material for metal masks, improvement in productivity of metal masks can be expected. [Brief description of the drawings]

[0015] [Figure 1] FIG. 1 is a diagram for explaining a method for manufacturing a metal mask using a metal plate material having a single-layer structure made of a single type of metal, as a conventional technique. [Diagram 2] FIG. 1 is a diagram for explaining a method for manufacturing a metal mask using a clad plate material having a two-layer structure in which two kinds of metals are bonded together, as a conventional technique. [Diagram 3] FIG. 1 is a diagram showing an example of a clad plate material for a metal mask having a two-layer structure as one embodiment of the present invention. [Figure 4] FIG. 1 is a diagram showing an example of a clad plate material for a metal mask having a three-layer structure as one embodiment of the present invention. [Diagram 5] FIG. 1 is a diagram showing another example of a clad plate material for a metal mask having a three-layer structure as one embodiment of the present invention. [Figure 6] FIG. 1 is a diagram showing an example of a metal mask having a single layer structure as one embodiment of the present invention. [Figure 7] FIG. 11 is a diagram showing another example of a metal mask having a single layer structure as an embodiment of the present invention. [Figure 8] FIG. 1 is a diagram showing an example of a metal mask having a two-layer structure as one embodiment of the present invention. [Figure 9] FIG. 11 is a diagram showing another example of a metal mask having a two-layer structure as an embodiment of the present invention. [Figure 10] FIG. 1 is a diagram showing an example of a metal mask having a three-layer structure as one embodiment of the present invention. [Figure 11] FIG. 11 is a diagram showing another example of a metal mask having a three-layer structure as an embodiment of the present invention. [Figure 12] FIG. 2 is a diagram for explaining a method for manufacturing a metal mask using a two-layer clad plate material for a metal mask. [Figure 13] FIG. 2 is a diagram for explaining a method for manufacturing a metal mask using a two-layer clad plate material for a metal mask. [Figure 14]FIG. 2 is a diagram for explaining a method for manufacturing a metal mask using a two-layer clad plate material for a metal mask. [Figure 15] FIG. 2 is a diagram for explaining a method for manufacturing a metal mask using a two-layer clad plate material for a metal mask. [Figure 16] FIG. 2 is a diagram for explaining a method for manufacturing a metal mask using a two-layer clad plate material for a metal mask. [Figure 17] FIG. 1 is a diagram for explaining a method for manufacturing a metal mask using a three-layer clad plate material for a metal mask. [Figure 18] FIG. 1 is a diagram for explaining a method for manufacturing a metal mask using a three-layer clad plate material for a metal mask. [Figure 19] FIG. 1 is a diagram for explaining a method for manufacturing a metal mask using a three-layer clad plate material for a metal mask. [Figure 20] FIG. 1 is a diagram for explaining a method for manufacturing a metal mask using a three-layer clad plate material for a metal mask. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] The present invention will be described with reference to specific embodiments of a clad plate material for metal masks according to the present invention.

[0017] First Embodiment A first embodiment of a clad plate material for metal masks according to the present invention is shown in Fig. 3. Fig. 3 is a cross-sectional view of a clad plate material for metal masks 1S (hereinafter referred to as "clad plate material 1S") cut in the thickness direction (Z direction).

[0018] The clad plate material 1S has a two-layer structure in a cross-sectional view cut in the thickness direction. 1S) includes a base layer 10 (thickness t0) and a first carrier layer 11 (thickness t1) pressed against one side (Z1 side) of the base layer 10. The pressed-bonding form between the base layer 10 and the first carrier layer 11 can be obtained, for example, by rolling (clad rolling) a plate material for constituting the base layer 10 and a plate material for constituting the first carrier layer 11 in a state of being directly superimposed on each other, and performing diffusion annealing as necessary. The clad plate material 1S is an example of a "clad plate material for metal masks" in the claims, the base layer 10 is an example of a "base layer" in the claims, and the first carrier layer 11 is an example of a "first carrier layer" in the claims.

[0019] The base layer 10 constituting the clad plate material 1S can be the main part of the metal mask. In this case, it is possible to obtain a single-layered metal mask consisting of the base layer 10, or a two-layered metal mask consisting of the base layer 10 and the first carrier layer 11. As described above, the target thickness of the metal mask is, for example, 20 μm or less, and preferably 15 μm or less. In light of this target, from the viewpoint of thinning, the thickness T 1S The upper limit of the thickness t0 of the base layer 10 when the base layer 10 is used as the main part of the metal mask is preferably 20 μm or less, more preferably 15 μm or less, and even more preferably 10 μm or less. 1S The lower limit of the thickness t0 of the clad plate material 1S or the thickness t0 of the base layer 10 when the base layer 10 is used as the main part of the metal mask is preferably 1 μm or more, more preferably 3 μm or more, and even more preferably 5 μm or more. 1S The thinner the thickness t0 of the base layer 10, or in the case where the base layer 10 is the main part of the metal mask, the thinner the thickness t0 of the base layer 10, the more the amount of side etching in the etching is suppressed, and therefore the dimensional accuracy of the mask pattern, such as the etching holes formed by etching, is improved, and it is possible to obtain a metal mask with a more precise mask pattern.

[0020] The base layer 10 constituting the clad plate material 1S is made of an Fe-based alloy. This Fe-based alloy contains at least one of Ni (nickel) and Co (cobalt) in the range of 30% by mass to 50% by mass. The remainder excluding Ni and Co may be Fe (iron) and unavoidable impurities, and may further contain at least one additive element. In addition, the Fe-based alloy containing Ni and Co is preferably one in which Co is 10% by mass or less (i.e., Ni is 20% by mass to 40% by mass). Many Fe-based alloys containing at least one of Ni and Co in the range of 30% by mass to 50% by mass relative to Fe have a small linear expansion coefficient that is effective in suppressing thermal deformation (distortion) during deposition when using a metal mask for an organic EL element, for example, and are suitable for constituting a metal mask plate material. This Fe-based alloy may contain elements (additive elements) other than Ni and Co in the range of 10% by mass or less. Examples of the additive elements include Mn (manganese), Mo (molybdenum), Nb (niobium), and Cr (chromium). An Fe-based alloy containing these additive elements in the range of 0% by mass to 10% by mass may have mechanical strength and various properties that are preferable as a metal material for forming a metal mask plate material, such as 0.2% proof stress, tensile strength, elongation, Young's modulus, hardness, and linear expansion coefficient. The substrate layer 10 made of the above-mentioned Fe-based alloy can be etched with a general ferric chloride solution suitable for the above-mentioned Fe-based alloy.

[0021] The first carrier layer 11 constituting the clad plate material 1S is directly pressed against one side (Z1 side) of the base layer 10. The first carrier layer 11 is effective in reinforcing the thinned base layer 10 which is the main body of the metal mask, and is effective in improving the mechanical strength of the thin clad plate material 1S. The first carrier layer 11 becomes a carrier for the thinned base layer 10, facilitating handling of the thinned base layer 10, and suppressing large warping of the clad plate material 1S including the base layer 10, thereby contributing to stabilization of etching. In addition, the first carrier layer 11 can be the main body of the metal mask, similar to the base layer 10. In this case, it is possible to obtain a single-layered metal mask consisting of the first carrier layer 11 portion, and it is also possible to obtain a two-layered metal mask consisting of the first carrier layer 11 portion and the base layer 10 portion. The thickness t1 of the first carrier layer 11 is preferably set in consideration of the various characteristics of the entire clad plate material 1S in addition to the various characteristics of the base layer 10. For example, when the purpose is to reinforce the base layer 10 from the viewpoint of facilitating handling, the thickness t1 of the first carrier layer 11 is preferably 5 μm or more and 100 μm or less, more preferably 20 μm or more and 100 μm or less. For example, when the first carrier layer 11 portion is to be the main part of the metal mask, the upper limit of the thickness t1 of the first carrier layer 11 is preferably 20 μm or less, more preferably 15 μm or less, and even more preferably 10 μm or less.

[0022] The first carrier layer 11 can be etched with a ferric chloride solution capable of etching the base layer 10. That is, the base layer 10 and the first carrier layer 11 can be etched simultaneously with the same ferric chloride solution. In this invention, when the base layer 10 and the first carrier layer 11 can be etched simultaneously with the ferric chloride solution, the base layer 10 only needs to have higher corrosion resistance than the first carrier layer 11 with respect to the ferric chloride solution. As a result, when etching of the base layer 10 and the first carrier layer 11 is started simultaneously with the ferric chloride solution, the base layer 10 is less likely to be etched than the first carrier layer 11, so that the etching rate of the base layer 10 can be slower than the etching rate of the first carrier layer 11. Therefore, for example, when etching holes are formed simultaneously in the base layer 10 and the first carrier layer 11, the depth of the etching hole formed from the surface (Z2 side) of the base layer 10 toward the Z1 side becomes shallower than the depth of the etching hole formed from the surface (Z1 side) of the first carrier layer 11 toward the Z2 side. By using a metal mask plate material (clad plate material 1S) that can achieve such a difference in the depth of etching holes, it becomes possible to construct a metal mask having a mask pattern in which the depths of the holes arranged on one side are different from the depths of the holes arranged on the other side.

[0023] In addition, the clad plate material 1S was etched using the same ferric chloride solution under the same environment to measure the corrosion loss of the base layer 10. b The corrosion loss of the first carrier layer 11 is M C1 In this case, the base layer 10 and the first carrier layer 11 have a thickness of M b / M c1It is preferable that the relationship of ≦0.9 is satisfied. In a clad plate material 1S satisfying this relationship, when the base layer 10 and the first carrier layer 11 are etched simultaneously, the etching rate of the base layer 10 can be reliably made slower than the etching rate of the first carrier layer 11. As a result, when etching holes are to be formed simultaneously, for example, the depth of the etching hole formed from the surface (Z2 side) of the base layer 10 toward the Z1 side can be reliably made shallower than the depth of the etching hole formed from the surface (Z1 side) of the first carrier layer 11 toward the Z2 side. Note that the base layer 10 and the first carrier layer 11, which are etched simultaneously, have a thickness of M b / M c1 >0(M b >0, M c1 >0).

[0024] For example, when plate material A made of an Fe-based alloy containing about 32% by mass of Ni and about 5.5% by mass of Co, and plate material B made of an Fe-based alloy containing about 36% by mass of Ni are etched with a 40% by mass concentration of ferric chloride solution (aqueous solution), the corrosion weight loss (M A ) and corrosion weight loss of plate B (M B ) ratio (M A / M B It was confirmed that the M is approximately 0.89. When the clad plate material 1S is constructed by using the plate material A as the base layer 10 (thickness t0) and the plate material B as the first carrier layer 11 (thickness t1=t0), which have this relationship, the above-mentioned M b / M c1 Therefore, the base layer 10 and the first carrier layer 11 have an M b / M c1 The relationship is ≦0.9.

[0025] The clad plate material 1S preferably has mechanical strength and various properties suitable for a metal mask, such as 0.2% proof stress, tensile strength, elongation, Young's modulus, hardness, and linear expansion coefficient. For example, from the viewpoint of facilitating handling, the clad plate material 1S having a large tensile strength and a large Young's modulus is preferable. In this case, the clad plate material 1S, particularly the base layer 10 which is the main part of the metal mask, preferably has a tensile strength of 700 MPa or more and a Young's modulus of 100 GPa or more. In addition, from the viewpoint of suppressing thermal deformation (distortion) during deposition when using a metal mask for an organic EL element, the clad plate material 1S is preferably one which has a small warp caused by heating, and it is preferable that the difference between the linear expansion coefficient of the base layer 10 constituting the clad plate material 1S and the linear expansion coefficient of the first carrier layer 11 is small. In this case, it is preferable that the linear expansion coefficient of the base layer 10 is 5 ppm / °C or less, and the linear expansion coefficient of the first carrier layer 11 is within ±2 ppm / °C of the linear expansion coefficient of the base layer 10.

[0026] <Second embodiment> A second embodiment of a clad plate material for metal masks according to the present invention is shown in Fig. 4. For simplicity, the reference symbols shown in Fig. 3 are used in Fig. 4. Fig. 4 is a cross-sectional view of a clad plate material 2S for metal masks (hereinafter referred to as "clad plate material 2S") cut in the thickness direction (Z direction). The clad plate material 2S shown in Fig. 4 is different from the clad plate material 1S shown in Fig. 3 in terms of the number of layers. The base layer 10 and the first carrier layer 11 provided in the clad plate material 2S may or may not have the same configuration as the base layer 10 and the first carrier layer 11 provided in the clad plate material 1S.

[0027] The clad plate material 2S has a three-layer structure in a cross-sectional view cut in the thickness direction. 2S4 includes a base layer 10 (thickness t0), a first carrier layer 11 (thickness t1) pressed against one side (Z1 side) of the base layer 10, and a second carrier layer 12 (thickness t2) pressed against the other side (Z2 side) of the base layer 10. The first carrier layer 11 and the second carrier layer 12 shown in FIG. 4 have substantially the same thickness (t1=t2). The pressing form of the base layer 10, the first carrier layer 11, and the second carrier layer 12 can be obtained, for example, by rolling (clad rolling) a plate material for forming the base layer 10, a plate material for forming the first carrier layer 11, and a plate material for forming the second carrier layer 12 in a state of being directly stacked on top of each other, and performing diffusion annealing as necessary. The clad plate material 2S is an example of a "clad plate material for a metal mask" as claimed in the claims, the base layer 10 is an example of a "base layer" as claimed in the claims, the first carrier layer 11 is an example of a "first carrier layer" as claimed in the claims, and the second carrier layer 12 is an example of a "second carrier layer" as claimed in the claims.

[0028] The base layer 10 constituting the clad plate material 2S can be the main part of the metal mask. In this case, it is possible to obtain a single-layer metal mask consisting of the base layer 10, a two-layer metal mask consisting of the base layer 10 and the first carrier layer 11, a two-layer metal mask consisting of the base layer 10 and the second carrier layer 12, or a three-layer metal mask consisting of the first carrier layer 11, the base layer 10, and the second carrier layer 12. As described above, the target thickness of the metal mask is, for example, 20 μm or less, and preferably 15 μm or less. In light of this target, from the viewpoint of thinning, the thickness T 2S The upper limit of the thickness t0 of the base layer 10 when the base layer 10 is used as the main part of the metal mask is preferably 20 μm or less, more preferably 15 μm or less, and even more preferably 10 μm or less. 2SThe lower limit of the thickness t0 of the clad plate material 2S or the thickness t0 of the base layer 10 when the base layer 10 is used as the main part of the metal mask is preferably 1 μm or more, more preferably 3 μm or more, and even more preferably 5 μm or more. 2S The thinner the thickness t0 of the base layer 10, or in the case where the base layer 10 portion is the main part of the metal mask, the thinner the thickness t0 of the base layer 10, the more the amount of side etching in the etching is suppressed, and therefore the dimensional accuracy of the mask pattern, such as the etching holes formed by etching, is improved, and it is possible to obtain a metal mask with a more precise mask pattern.

[0029] The base layer 10 constituting the clad plate material 2S is made of an Fe-based alloy. This Fe-based alloy contains at least one of Ni and Co in the range of 30% by mass to 50% by mass. The remainder excluding Ni and Co may be Fe and unavoidable impurities, and may further contain at least one additive element. The Fe-based alloy containing Ni and Co is preferably one in which Co is 10% by mass or less (i.e., Ni is 20% by mass to 40% by mass). Many Fe-based alloys containing at least one of Ni and Co in the range of 30% by mass to 50% by mass relative to Fe have a small linear expansion coefficient that is effective in suppressing thermal deformation (distortion) during deposition when using a metal mask for an organic EL element, and are suitable for constituting a metal mask plate material. This Fe-based alloy may contain elements (additive elements) other than Ni and Co in the range of 10% by mass or less. The additive elements are, for example, Mn, Mo, Nb, and Cr. An Fe-based alloy containing these additive elements in the range of 0% by mass to 10% by mass may have favorable mechanical strength and various properties as a metal material constituting a metal mask plate material, such as 0.2% proof stress, tensile strength, elongation, Young's modulus, hardness, linear expansion coefficient, etc. The substrate layer 10 made of the above-mentioned Fe-based alloy can be etched with a general ferric chloride solution suitable for the above-mentioned Fe-based alloy.

[0030] The first carrier layer 11 constituting the clad plate material 2S is directly pressed against one side (Z1 side) of the base layer 10. The second carrier layer 12 constituting the clad plate material 2S is directly pressed against the other side (Z2 side) of the base layer 10. The first carrier layer 11 and the second carrier layer 12 are effective in reinforcing the thinned base layer 10 which is the main body of the metal mask, and are effective in increasing the mechanical strength of the thin clad plate material 2S. The first carrier layer 11 and the second carrier layer 12 become carriers for the thinned base layer 10, making it easier to handle the thinned base layer 10 and contributing to stabilizing the etching of the clad plate material 2S including the base layer 10. The first carrier layer 11 and the second carrier layer 12 can be the main body of the metal mask, just like the base layer 10. In this case, it is possible to obtain a metal mask having a single layer structure made of the first carrier layer 11, a metal mask having a single layer structure made of the second carrier layer 12, a metal mask having a two-layer structure made of the first carrier layer 11 and the base layer 10, a metal mask having a two-layer structure made of the second carrier layer 12 and the base layer 10, or a metal mask having a three-layer structure made of the first carrier layer 11, the base layer 10, and the second carrier layer 12. When the purpose is to reinforce the base layer 10 from the viewpoint of facilitating handling, the thickness t1 of the first carrier layer 11 and the thickness t2 of the second carrier layer 12 are each preferably 5 μm or more and 100 μm or less, more preferably 20 μm or more and 100 μm or less. When the first carrier layer 11 portion or the second carrier layer 12 portion is used as the main part of the metal mask, the upper limit value of the thickness t1 of the first carrier layer 11 and the upper limit value of the thickness t2 of the second carrier layer 12 are preferably 20 μm or less, more preferably 15 μm or less, and even more preferably 10 μm or less, respectively.

[0031] Both the first carrier layer 11 and the second carrier layer 12 can be etched with a ferric chloride solution capable of etching the base layer 10. That is, the base layer 10 and the first carrier layer 11, the base layer 10 and the second carrier layer 12, and the first carrier layer 11 and the second carrier layer 12 can be simultaneously etched with the same ferric chloride solution in each combination. In this invention, when the base layer 10 and the first carrier layer 11 can be simultaneously etched, when the base layer 10 and the second carrier layer 12 can be simultaneously etched, and when the first carrier layer 11 and the second carrier layer 12 can be simultaneously etched, the base layer 10 may have higher corrosion resistance to the ferric chloride solution than the first carrier layer 11 and the second carrier layer 12. Note that the first carrier layer 11 may have higher corrosion resistance to the same ferric chloride solution than the second carrier layer 12, or the second carrier layer 12 may have higher corrosion resistance to the same ferric chloride solution than the first carrier layer 11. As a result, for example, if the first carrier layer 11 and the second carrier layer 12 are made of the same material and have the same thickness (t1=t2), the first carrier layer 11 and the second carrier layer 12 can be simultaneously half-etched to simultaneously remove the first carrier layer 11 and the second carrier layer 12, thereby simultaneously exposing the surface on one side (Z1 side) and the surface on the other side (Z2 side) of the base layer 10, and a single-layered metal plate material made of the base layer 10 can be obtained. In this case, by adjusting the half-etching conditions, a three-layered clad plate material can be obtained in which the first carrier layer 11 and the second carrier layer 12 each have a predetermined thickness and are provided on both sides of the base layer 10. In addition, if the first carrier layer 11 and the second carrier layer 12 are made of different materials, it is also possible to leave only one of the first carrier layer 11 or the second carrier layer 12, which has a higher corrosion resistance to ferric chloride solution, with a predetermined thickness by half-etching. In this case, it is possible to obtain a clad plate material having a two-layer structure in which only one of the first carrier layer 11 or the second carrier layer 12 has a predetermined thickness and is provided on the base layer 10 .

[0032] The base layer 10 has higher corrosion resistance to this ferric chloride solution than the first carrier layer 11 and the second carrier layer 12. As a result, when etching of the above-mentioned two-layer clad plate material is started with this ferric chloride solution, the base layer 10 is less likely to be etched than the first carrier layer 11 (or the second carrier layer 12), so the etching rate of the base layer 10 can be slower than the etching rate of the first carrier layer 11 (or the second carrier layer 12). Therefore, for example, when etching holes are simultaneously formed in a two-layer clad plate material having the base layer 10 and the first carrier layer 11, the depth of the etching hole formed from the surface (Z2 side) of the base layer 10 toward the Z1 side is shallower than the depth of the etching hole formed from the surface (Z1 side) of the first carrier layer 11 toward the Z2 side. Alternatively, when etching holes are simultaneously formed in a two-layer clad plate material having a base layer 10 and a second carrier layer 12, the depth of the etching holes formed from the surface (Z1 side) of the base layer 10 toward the Z2 side is shallower than the depth of the etching holes formed from the surface (Z2 side) of the second carrier layer 12 toward the Z1 side. By using a metal mask plate material (clad plate material 2S) that can achieve such a difference in etching hole depth, it is possible to configure a metal mask having a mask pattern in which the depth of the holes arranged on one side differs from the depth of the holes arranged on the other side.

[0033] In addition, the clad plate material 2S was etched using the same ferric chloride solution under the same environment to measure the corrosion loss of the base layer 10. b The corrosion loss of the first carrier layer 11 is M C1 The corrosion loss of the second carrier layer 12 is M C2 In this case, the base layer 10, the first carrier layer 11 and the second carrier layer 12 are M b / M c1 ≦0.9 and M b / M c2It is preferable that the relationship of ≦0.9 is satisfied. In the clad plate material 2S satisfying this relationship, when the base material layer 10 and the first carrier layer 11 are etched simultaneously, the etching rate of the base material layer 10 can be reliably slower than the etching rate of the first carrier layer 11, or when the base material layer 10 and the second carrier layer 12 are etched simultaneously, the etching rate of the base material layer 10 can be reliably slower than the etching rate of the second carrier layer 12. As a result, when etching holes are to be formed simultaneously, for example, the depth of the etching hole formed from the surface (Z2 side) of the base material layer 10 toward the Z1 side can be reliably made shallower than the depth of the etching hole formed from the surface (Z1 side) of the first carrier layer 11 toward the Z2 side, or the depth of the etching hole formed from the surface (Z1 side) of the base material layer 10 toward the Z2 side can be reliably made shallower than the depth of the etching hole formed from the surface (Z2 side) of the second carrier layer 12 toward the Z1 side. Note that the base material layer 10 and the first carrier layer 11, which are etched simultaneously, are M b / M c1 >0(M b >0, M c1 >0), or the substrate layer 10 and the second carrier layer 12 that are etched simultaneously satisfy the relationship M b / M c2 >0(M b >0, M c2 >0). The first carrier layer 11 and the second carrier layer 12 satisfy the relationship of M c1 / M c2 ≦0.9, or M c2 / M c1 ≦0.9.

[0034] The clad plate material 2S preferably has mechanical strength and various properties suitable for a metal mask, such as 0.2% proof stress, tensile strength, elongation, Young's modulus, hardness, and linear expansion coefficient. For example, from the viewpoint of facilitating handling, the clad plate material 2S having a large tensile strength and a large Young's modulus is preferable. In this case, the clad plate material 2S, particularly the base layer 10 which is the main part of the metal mask, preferably has a tensile strength of 700 MPa or more and a Young's modulus of 100 GPa or more. Also, for example, from the viewpoint of suppressing thermal deformation (distortion) during deposition when using a metal mask for an organic EL element, the clad plate material 2S having a small warp caused by heating is preferable, and it is preferable that the difference between the linear expansion coefficient of the base layer 10, the linear expansion coefficient of the first carrier layer 11, and the linear expansion coefficient of the second carrier layer 12 constituting the clad plate material 2S is small. In this case, it is preferable that the linear expansion coefficient of the base layer 10 is 5 ppm / °C or less, and the linear expansion coefficients of the first carrier layer 11 and the second carrier layer 12 are each within ±2 ppm / °C of the linear expansion coefficient of the base layer 10.

[0035] <Third embodiment> A third embodiment of the clad plate material for metal masks according to the present invention is shown in FIG. 5. For simplicity, the reference symbols shown in FIG. 3 and FIG. 4 are used in FIG. 5. FIG. 5 is a cross-sectional view of a clad plate material for metal masks 3S (hereinafter referred to as "clad plate material 3S") cut in the thickness direction (Z direction). The clad plate material 3S shown in FIG. 5 and the clad plate material 2S shown in FIG. 4 have different thicknesses of the second carrier layer 12 (for convenience, the reference symbols for both thicknesses are written as t2). The base layer 10, the first carrier layer 11, and the second carrier layer 12 constituting the clad plate material 3S may or may not have the same configuration as the base layer 10, the first carrier layer 11, and the second carrier layer 12 constituting the above-mentioned clad plate material 2S, except that the thickness t1 of the first carrier layer 11 is different from the thickness t2 of the second carrier layer 12 (t1>t2).

[0036] The clad plate material 3S has a three-layer structure in a cross-sectional view cut in the thickness direction. 3S) includes a base material layer 10 (thickness t0), a first carrier layer 11 (thickness t1) pressed against one side (Z1 side) of the base material layer 10, and a second carrier layer 12 (thickness t2) pressed against the other side (Z2 side) of the base material layer 10. The first carrier layer 11 and the second carrier layer 12 shown in FIG. 5 have different thicknesses (t1>t2). Note that for the clad plate material 3S, for example, the thickness t2 of the second carrier layer 12 may be greater than the thickness t1 of the first carrier layer 11 (t1<t2). The pressing form of the base material layer 10, the first carrier layer 11, and the second carrier layer 12 is, for example, obtained by rolling (clad rolling) in a state where the plate material for forming the base material layer 10, the plate material for forming the first carrier layer 11, and the plate material for forming the second carrier layer 12 are directly overlapped, and performing diffusion annealing as necessary. Note that the clad plate material 3S is an example of the "clad plate material for a metal mask" in the claims, the base material layer 10 is an example of the "base material layer" in the claims, the first carrier layer 11 is an example of the "first carrier layer" in the claims, and the second carrier layer 12 is an example of the "second carrier layer" in the claims.

[0037] The base material layer 10 constituting the clad plate material 3S can be the main body of the metal mask. In this case, it is possible to obtain a single-layer metal mask composed of the base material layer 10 portion, a two-layer metal mask composed of the base material layer 10 portion and the first carrier layer 11 portion, a two-layer metal mask composed of the base material layer 10 portion and the second carrier layer 12 portion, or a three-layer metal mask composed of the first carrier layer 11 portion, the base material layer 10 portion, and the second carrier layer 12 portion. As described above, the thickness of the target metal mask is, for example, 20 μm or less, preferably 15 μm or less. In light of this target, from the perspective of thinning, the upper limit of the thickness T 3S of the clad plate material 2S or the upper limit of the thickness t0 of the base material layer 10 when the base material layer 10 portion is the main body of the metal mask is preferably 20 μm or less, more preferably 15 μm or less, and even more preferably 10 μm or less. Also, from the perspective of facilitating handling, the thickness T 3SThe lower limit of the thickness t0 of the clad plate material 2S or the thickness t0 of the base layer 10 when the base layer 10 is used as the main part of the metal mask is preferably 1 μm or more, more preferably 3 μm or more, and even more preferably 5 μm or more. 3S The thinner the thickness t0 of the base layer 10, or in the case where the base layer 10 portion is the main part of the metal mask, the thinner the thickness t0 of the base layer 10, the more the amount of side etching in the etching is suppressed, and therefore the dimensional accuracy of the mask pattern, such as the etching holes formed by etching, is improved, and it is possible to obtain a metal mask with a more precise mask pattern.

[0038] The base layer 10 constituting the clad plate material 3S is made of an Fe-based alloy. This Fe-based alloy contains at least one of Ni and Co in the range of 30% by mass to 50% by mass. The remainder excluding Ni and Co may be Fe and unavoidable impurities, and may further contain at least one additive element. The Fe-based alloy containing Ni and Co is preferably one in which Co is 10% by mass or less (i.e., Ni is 20% by mass to 40% by mass). Many Fe-based alloys containing at least one of Ni and Co in the range of 30% by mass to 50% by mass relative to Fe have a small linear expansion coefficient that is effective in suppressing thermal deformation (distortion) during deposition when using a metal mask for an organic EL element, and are suitable for constituting a metal mask plate material. This Fe-based alloy may contain elements (additive elements) other than Ni and Co in the range of 10% by mass or less. The additive elements are, for example, Mn, Mo, Nb, and Cr. An Fe-based alloy containing these additive elements in the range of 0% by mass to 10% by mass may have preferable mechanical strength and various properties as a metal material constituting a metal mask plate material, such as 0.2% proof stress, tensile strength, elongation, Young's modulus, hardness, linear expansion coefficient, etc. The substrate layer 10 made of the above-mentioned Fe-based alloy can be etched with a general etching solution suitable for the above-mentioned Fe-based alloy (e.g., ferric chloride solution, etc.).

[0039] The first carrier layer 11 constituting the clad plate material 3S is directly pressed against one side (Z1 side) of the base layer 10. The second carrier layer 12 constituting the clad plate material 3S is directly pressed against the other side (Z2 side) of the base layer 10. The first carrier layer 11 and the second carrier layer 12 are effective in reinforcing the thinned base layer 10 which is the main body of the metal mask, and are effective in increasing the mechanical strength of the thin clad plate material 2S. The first carrier layer 11 and the second carrier layer 12 become carriers for the thinned base layer 10, making it easier to handle the thinned base layer 10 and contributing to stabilizing the etching of the clad plate material 2S including the base layer 10. The first carrier layer 11 and the second carrier layer 12 can be the main body of the metal mask, just like the base layer 10. In this case, it is possible to obtain a metal mask having a single layer structure made of the first carrier layer 11, a metal mask having a single layer structure made of the second carrier layer 12, a metal mask having a two-layer structure made of the first carrier layer 11 and the base layer 10, a metal mask having a two-layer structure made of the second carrier layer 12 and the base layer 10, or a metal mask having a three-layer structure made of the first carrier layer 11, the base layer 10, and the second carrier layer 12. When the purpose is to reinforce the base layer 10 from the viewpoint of facilitating handling, the thickness t1 of the first carrier layer 11 and the thickness t2 of the second carrier layer 12 are each preferably 5 μm or more and 100 μm or less, more preferably 20 μm or more and 100 μm or less. When the first carrier layer 11 portion or the second carrier layer 12 portion is used as the main part of the metal mask, the upper limit value of the thickness t1 of the first carrier layer 11 and the upper limit value of the thickness t2 of the second carrier layer 12 are preferably 20 μm or less, more preferably 15 μm or less, and even more preferably 10 μm or less, respectively.

[0040] Both the first carrier layer 11 and the second carrier layer 12 can be etched with a ferric chloride solution capable of etching the base layer 10. That is, the base layer 10 and the first carrier layer 11, the base layer 10 and the second carrier layer 12, and the first carrier layer 11 and the second carrier layer 12 can be simultaneously etched with the same ferric chloride solution in each combination. In this invention, when the base layer 10 and the first carrier layer 11 can be simultaneously etched, when the base layer 10 and the second carrier layer 12 can be simultaneously etched, and when the first carrier layer 11 and the second carrier layer 12 can be simultaneously etched, the base layer 10 may have higher corrosion resistance to the ferric chloride solution than the first carrier layer 11 and the second carrier layer 12. Note that the first carrier layer 11 may have higher corrosion resistance to the same ferric chloride solution than the second carrier layer 12, or the second carrier layer 12 may have higher corrosion resistance to the same ferric chloride solution than the first carrier layer 11. As a result, for example, by simultaneously half-etching the first carrier layer 11 and the second carrier layer 12 having different thicknesses (for example, t1>t2), a part of the first carrier layer 11 and the whole of the second carrier layer 12 are simultaneously removed to expose only the surface on one side (Z2 side) of the base layer 10, and a two-layer clad plate material can be obtained in which the first carrier layer 11 is provided with a predetermined thickness on the other side (Z1 side) of the base layer 10. In addition, such a two-layer clad plate material can also be obtained by, for example, configuring the first carrier layer 11 and the second carrier layer 12 with different materials and leaving only one of the first carrier layer 11 or the second carrier layer 12, which has higher corrosion resistance against ferric chloride solution, with a predetermined thickness. In such a case, by adjusting the half-etching conditions, it is also possible to obtain a three-layer clad plate material in which the first carrier layer 11 and the second carrier layer 12 are provided on both sides of the base layer 10 with a predetermined thickness.

[0041] The base layer 10 has higher corrosion resistance to this ferric chloride solution than the first carrier layer 11 and the second carrier layer 12. As a result, when etching of the above-mentioned two-layer clad plate material is started with this ferric chloride solution, the base layer 10 is less likely to be etched than the first carrier layer 11 (or the second carrier layer 12), so the etching rate of the base layer 10 can be slower than the etching rate of the first carrier layer 11 (or the second carrier layer 12). Therefore, for example, when etching holes are simultaneously formed in a two-layer clad plate material having the base layer 10 and the first carrier layer 11, the depth of the etching hole formed from the surface (Z2 side) of the base layer 10 toward the Z1 side is shallower than the depth of the etching hole formed from the surface (Z1 side) of the first carrier layer 11 toward the Z2 side. Alternatively, when etching holes are simultaneously formed in a two-layer clad plate material having a base layer 10 and a second carrier layer 12, the depth of the etching holes formed from the surface (Z1 side) of the base layer 10 toward the Z2 side is shallower than the depth of the etching holes formed from the surface (Z2 side) of the second carrier layer 12 toward the Z1 side. By using a metal mask plate material (clad plate material 3S) that can achieve such a difference in etching hole depth, it is possible to configure a metal mask having a mask pattern in which the depth of the holes arranged on one side differs from the depth of the holes arranged on the other side.

[0042] In addition, the clad plate material 3S was etched using the same ferric chloride solution under the same environment to measure the corrosion loss of the base layer 10. b The corrosion loss of the first carrier layer 11 is M C1 The corrosion loss of the second carrier layer 12 is M C2 In this case, the base layer 10, the first carrier layer 11 and the second carrier layer 12 are M b / M c1 ≦0.9 and M b / M c2It is preferable that the relationship of ≦0.9 is satisfied. In the clad plate material 3S satisfying this relationship, when the base material layer 10 and the first carrier layer 11 are etched simultaneously, the etching rate of the base material layer 10 can be reliably slower than the etching rate of the first carrier layer 11, or when the base material layer 10 and the second carrier layer 12 are etched simultaneously, the etching rate of the base material layer 10 can be reliably slower than the etching rate of the second carrier layer 12. As a result, when etching holes are to be formed simultaneously, for example, the depth of the etching hole formed from the surface (Z2 side) of the base material layer 10 toward the Z1 side can be reliably made shallower than the depth of the etching hole formed from the surface (Z1 side) of the first carrier layer 11 toward the Z2 side, or the depth of the etching hole formed from the surface (Z1 side) of the base material layer 10 toward the Z2 side can be reliably made shallower than the depth of the etching hole formed from the surface (Z2 side) of the second carrier layer 12 toward the Z1 side. Note that the base material layer 10 and the first carrier layer 11, which are etched simultaneously, are M b / M c1 >0(M b >0, M c1 >0), or the substrate layer 10 and the second carrier layer 12 that are etched simultaneously satisfy the relationship M b / M c2 >0(M b >0, M c2 >0). The first carrier layer 11 and the second carrier layer 12 satisfy the relationship of M c1 / M c2 ≦0.9, or M c2 / M c1 ≦0.9.

[0043] The clad plate material 3S preferably has mechanical strength and various properties suitable for a metal mask, such as 0.2% proof stress, tensile strength, elongation, Young's modulus, hardness, and linear expansion coefficient. For example, from the viewpoint of facilitating handling, the clad plate material 3S having a large tensile strength and a large Young's modulus is preferable. In this case, the clad plate material 3S, particularly the base layer 10 which is the main part of the metal mask, preferably has a tensile strength of 700 MPa or more and a Young's modulus of 100 GPa or more. Also, for example, from the viewpoint of suppressing thermal deformation (distortion) during deposition when using a metal mask for an organic EL element, the clad plate material 3S is preferable to have a small warp caused by heating, and it is preferable that the difference between the linear expansion coefficient of the base layer 10, the linear expansion coefficient of the first carrier layer 11, and the linear expansion coefficient of the second carrier layer 12 constituting the clad plate material 3S is small. In this case, it is preferable that the linear expansion coefficient of the base layer 10 is 5 ppm / °C or less, and the linear expansion coefficients of the first carrier layer 11 and the second carrier layer 12 are each within ±2 ppm / °C of the linear expansion coefficient of the base layer 10.

[0044] Specific embodiments (product examples) of the metal mask according to the present invention that can be manufactured using the above-mentioned clad plate material for metal masks (first embodiment, second embodiment, and third embodiment) will be described below.

[0045] <First product example> A first example of a metal mask product according to the present invention is shown in FIG. 6. FIG. 6 is a cross-sectional view of a metal mask 1M cut in the thickness direction (Z direction). The metal mask 1M has, for example, etching holes 1f as a mask pattern. In the cross-sectional view cut in the thickness direction, the metal mask 1M has a single-layer structure. The main part of the metal mask 1M is a substrate portion 10M. The substrate portion 10M is made up of, for example, the substrate layer 10 portion constituting the clad plate material 1S shown in FIG. 3, the substrate layer 10 portion constituting the clad plate material 2S shown in FIG. 4, or the substrate layer 10 portion constituting the clad plate material 3S shown in FIG. 5. The metal mask 1M is thinned to a thickness T 1MThe thickness T of the metal mask 1M is 20 μm or less (preferably 15 μm or less). The metal mask 1M having such a thin thickness has high dimensional accuracy of the mask pattern such as the etching holes 1f formed by etching, and has a more precise mask pattern. 1M may be equal to, for example, the thickness of the base layer 10 constituting the clad plate material 1S, the thickness of the base layer 10 constituting the clad plate material 2S, or the thickness of the base layer 10 constituting the clad plate material 3S (T 1M =t0), it may be thinned to the same level or less by half etching, etc. (T 1M <t0)。

[0046] <Modification of the first product example> FIG. 7 shows a modified example of the first product example of the metal mask according to the present invention. FIG. 7 is a cross-sectional view of the metal mask 1Ma cut in the thickness direction (Z direction). The metal mask 1Ma has, for example, etching holes 1f as a mask pattern. In the cross-sectional view cut in the thickness direction, the metal mask 1Ma consists of a single-layer structure portion and a two-layer structure portion. The single-layer structure portion is the main body of the metal mask 1Ma and is made of a base material portion 10M. The two-layer structure portion consists of the base material portion 10M and a frame portion 11f for reinforcing the main body of the metal mask 1Ma. The base material portion 10M consists of, for example, the base material layer 10 portion constituting the clad plate material 1S shown in FIG. 3, the base material layer 10 portion constituting the clad plate material 2S shown in FIG. 4, or the base material layer 10 portion constituting the clad plate material 3S shown in FIG. 5. The frame portion 11f is, for example, the first carrier layer 11 portion constituting the clad plate material 1S shown in FIG. 3, the first carrier layer 11 portion constituting the clad plate material 2S shown in FIG. 4, or the first carrier layer 11 portion constituting the clad plate material 3S shown in FIG. 5. The frame portion 11f is arranged in a ring shape on the edge portion of the base layer 10. The metal mask 1Ma having such a frame portion 11 is easier to handle than the metal mask 1M shown in FIG. 6 because the mechanical strength is improved when the thickness of the main body of the metal mask is approximately the same. The frame portion 11f is arranged in a ring shape on the edge portion of the base portion 10M, but it does not have to be arranged in a ring shape on the edge portion of the base portion 10M, and may be arranged on the opposite side of the base portion 10M. The configuration of the frame portion 11f is not limited to the above. For example, the frame portion 11f can be composed of the base layer 10 of the clad plate material 1S shown in Fig. 3, the base layer 10 of the clad plate material 2S shown in Fig. 4, or the base layer 10 of the clad plate material 3S shown in Fig. 5. When the frame portion 11f is composed of the base layer 10, the metal mask has a single-layer structure. Also, the frame portion 11f can be composed of the second carrier layer 12 of the clad plate material 2S shown in Fig. 4, or the second carrier layer 12 of the clad plate material 2S shown in Fig. 5.

[0047] The metal mask 1Ma is thinned to a thickness of T 1Mais 20 μm or less (preferably 15 μm or less). The metal mask 1Ma, which is thinned in this way, has high dimensional accuracy of mask patterns such as the etching holes 1f formed by etching, and has a higher definition mask pattern. The thickness T of the metal mask 1Ma 1Ma may be equivalent to, for example, the thickness of the base material layer 10 constituting the clad plate material 1S, the thickness of the base material layer 10 constituting the clad plate material 2S, or the thickness of the base material layer 10 constituting the clad plate material 3S (T 1Ma = t0), and may be made thinner than or equal to that by half etching or the like (T 1Ma < t0). The thickness T of the frame portion 11f X may be equivalent to, for example, the thickness of the first carrier layer 11 constituting the clad plate material 1S, the thickness of the first carrier layer 11 constituting the clad plate material 2S, or the thickness of the first carrier layer 11 constituting the clad plate material 3S (T X = t1), and may be made thinner than or equal to that by half etching or the like (T X < t1). Incidentally, the total thickness of the above-mentioned thickness T 1Ma and the thickness T X (T 1Ma + T X ) can also be regarded as the thickness of the metal mask 1Ma.

[0048] <Second Product Example> A second product example of the metal mask according to the present invention is shown in FIG. 8. FIG. 8 is a cross-sectional view of the metal mask 2M cut in the thickness direction (Z direction). The metal mask 2M has, for example, etching holes 2f as a mask pattern. In the cross-sectional view cut in the thickness direction, the metal mask 2M has a two-layer structure. The main body of the metal mask 2M consists of a base material part 10M and a carrier part 12M. The base material part 10M consists of, for example, the base material layer 10 part constituting the clad plate material 1S shown in FIG. 3, the base material layer 10 part constituting the clad plate material 2S shown in FIG. 4, or the base material layer 10 part constituting the clad plate material 3S shown in FIG. 5. The carrier part 12M consists of, for example, the second carrier layer 12 part constituting the clad plate material 1S shown in FIG. 3, the second carrier layer 12 part constituting the clad plate material 2S shown in FIG. 4, or the second carrier layer 12 part constituting the clad plate material 3S shown in FIG. 5. Note that the configuration of the carrier part 12M is not limited to the above. For example, the carrier part 12M can be composed of any of the first carrier layer 11 parts of the clad plate material 1S shown in FIG. 3, the first carrier layer 11 parts of the clad plate material 2S shown in FIG. 4, or the first carrier layer 11 of the clad plate material 3S shown in FIG. 5.

[0049] The metal mask 2M is thinned, and its thickness T 2M is 20 μm or less (preferably 15 μm or less). The metal mask 2M thinned in this way has high dimensional accuracy of mask patterns such as the etching holes 2f formed by etching, and has a higher-definition mask pattern. The thickness T of the metal mask 2M 2M can be, for example, equivalent to the total thickness of the base material layer 10 and the second carrier layer 12 constituting the clad plate material 1S, the total thickness of the base material layer 10 and the second carrier layer 12 constituting the clad plate material 2S, or the total thickness of the base material layer 10 and the second carrier layer 12 constituting the clad plate material 3S (T 2M =t0 + t2), and may be thinned to be equivalent or less by, for example, half etching (T 2M <t0 + t2). The thickness T of the carrier part 12M Ymay be equal to, for example, the thickness of the second carrier layer 12 constituting the clad plate material 1S, the thickness of the second carrier layer 12 constituting the clad plate material 2S, or the thickness of the second carrier layer 12 constituting the clad plate material 3S (T Y =t2), it may be thinned to the same level or less by half etching, etc. (T Y <t2)。

[0050] <Modification of the second product example> FIG. 9 shows a modified example of the second product example of the metal mask according to the present invention. FIG. 9 is a cross-sectional view of the metal mask 2Ma cut in the thickness direction (Z direction). The metal mask 2Ma has, for example, etching holes 2f as a mask pattern. In the cross-sectional view cut in the thickness direction, the metal mask 2Ma is composed of a two-layer structure portion and a three-layer structure portion. The two-layer structure portion is the main body of the metal mask 2Ma and is composed of a base material portion 10M and a carrier layer 12M. The three-layer structure portion is composed of the base material portion 10M, the carrier layer 12M, and a frame portion 11f for reinforcing the main body of the metal mask 2Ma. The base material portion 10M is composed of, for example, the base material layer 10 portion constituting the clad plate material 1S shown in FIG. 3, the base material layer 10 portion constituting the clad plate material 2S shown in FIG. 4, or the base material layer 10 portion constituting the clad plate material 3S shown in FIG. 5. The carrier portion 12M is, for example, the second carrier layer 12 portion constituting the clad plate material 1S shown in FIG. 3, the second carrier layer 12 portion constituting the clad plate material 2S shown in FIG. 4, or the second carrier layer 12 portion constituting the clad plate material 3S shown in FIG. 5. The frame portion 11f is, for example, the first carrier layer 11 portion constituting the clad plate material 1S shown in FIG. 3, the first carrier layer 11 portion constituting the clad plate material 2S shown in FIG. 4, or the first carrier layer 11 portion constituting the clad plate material 3S shown in FIG. 5. The frame portion 11f is arranged in a ring shape on the edge portion of the base layer 10. The metal mask 2Ma having such a frame portion 11 is easier to handle than the metal mask 2M shown in FIG. 8 because the mechanical strength is improved when the thickness of the main body of the metal mask is approximately the same. The frame portion 11f is arranged in a ring shape on the edge portion of the base portion 10M, but it does not have to be arranged in a ring shape on the edge portion of the base portion 10M, and may be arranged on the opposite side of the base portion 10M. The configuration of the frame portion 11f is not limited to the above. For example, the frame portion 11f can be composed of the base layer 10 portion of the clad plate material 1S shown in Fig. 3, the base layer 10 portion of the clad plate material 2S shown in Fig. 4, or the base layer 10 portion of the clad plate material 3S shown in Fig. 5. When the frame portion 11f is composed of the base layer 10 portion, the metal mask has a two-layer structure of the base layer 10 and the carrier portion 12M.Moreover, the configuration of the carrier portion 12M is not limited to the above. For example, the carrier portion 12M can be composed of any of the first carrier layer 11 portions constituting the clad plate material 1S shown in FIG. 3, the first carrier layer 11 portions constituting the clad plate material 2S shown in FIG. 4, or the first carrier layer 11 portions constituting the clad plate material 3S shown in FIG. 5.

[0051] The metal mask 2Ma is thinned, and its thickness T 2Ma is 20 μm or less (preferably 15 μm or less). Such a thinned metal mask 2Ma has high dimensional accuracy of mask patterns such as the etching holes 2f formed by etching and has a higher-definition mask pattern. The thickness T of the metal mask 2Ma 2Ma may be equivalent to, for example, the total thickness of the base material layer 10 and the second carrier layer 12 constituting the clad plate material 1S, the total thickness of the base material layer 10 and the second carrier layer 12 constituting the clad plate material 2S, or the total thickness of the base material layer 10 and the second carrier layer 12 constituting the clad plate material 3S (T 2Ma = t0 + t2), and may be made thinner than or equal to this by means such as half etching (T 2Ma < t0 + t2). The thickness T of the carrier portion 12M Y may be equivalent to, for example, the thickness of the second carrier layer 12 constituting the clad plate material 1S, the thickness of the second carrier layer 12 constituting the clad plate material 2S, or the thickness of the second carrier layer 12 constituting the clad plate material 3S (T Y = t2), and may be made thinner than or equal to this by means such as half etching (T Y < t2). The thickness T of the frame portion 11f X may be equivalent to, for example, the thickness of the first carrier layer 11 constituting the clad plate material 1S, the thickness of the first carrier layer 11 constituting the clad plate material 2S, or the thickness of the first carrier layer 11 constituting the clad plate material 3S (T X = t1), and may be made thinner than or equal to this by means such as half etching (T X < t1). Note that the total thickness of the above-mentioned thickness T 2Ma and the thickness T X (T2Ma +T X ) can also be considered as the thickness of the metal mask 2Ma.

[0052] <Third product example> A third example of a metal mask product according to the present invention is shown in FIG. 10. FIG. 10 is a cross-sectional view of a metal mask 3M cut in the thickness direction (Z direction). The metal mask 3M has, for example, etching holes 3f as a mask pattern. In the cross-sectional view cut in the thickness direction, the metal mask 3M has a three-layer structure. The main body of the metal mask 3M is composed of a base material portion 10M, a first carrier portion 11M, and a second carrier portion 12M. The base material portion 10M is composed of, for example, a base material layer 10 portion constituting the clad plate material 1S shown in FIG. 3, a base material layer 10 portion constituting the clad plate material 2S shown in FIG. 4, or a base material layer 10 portion constituting the clad plate material 3S shown in FIG. 5. The first carrier portion 11M is composed of, for example, a first carrier layer 11 portion constituting the clad plate material 1S shown in FIG. 3, a first carrier layer 11 portion constituting the clad plate material 2S shown in FIG. 4, or a first carrier layer 11 portion constituting the clad plate material 3S shown in FIG. 5. The second carrier part 12M is, for example, the second carrier layer 12 part constituting the clad plate material 1S shown in FIG. 3, the second carrier layer 12 part constituting the clad plate material 2S shown in FIG. 4, or the second carrier layer 12 part constituting the clad plate material 3S shown in FIG. 5. The configurations of the first carrier part 11M and the second carrier part 12M are not limited to the above. For example, the first carrier part 11M can be composed of the second carrier layer 12 part of the clad plate material 1S shown in FIG. 3, and the second carrier part 12M can be composed of the first carrier layer 11 part of the clad plate material 1S shown in FIG. 3. Also, the first carrier part 11M can be composed of the second carrier layer 12 part of the clad plate material 2S shown in FIG. 4, and the second carrier part 12M can be composed of the first carrier layer 11 part of the clad plate material 2S shown in FIG. 4. It is also possible for the first carrier portion 11M to be formed from the second carrier layer 12 portion of the clad plate material 3S shown in FIG. 5, and for the second carrier portion 12M to be formed from the first carrier layer 11 portion of the clad plate material 3S shown in FIG.

[0053] The metal mask 3M is thinned, and its thickness T 3M is 20 μm or less (preferably 15 μm or less). The metal mask 3M thinned in this way has high dimensional accuracy of mask patterns such as the etching holes 3f formed by etching and has a finer mask pattern. The thickness T of the metal mask 3M 3M may be equal to, for example, the total thickness of the base material layer 10, the first carrier layer 11, and the second carrier layer 12 that make up the clad plate material 1S, the total thickness of the base material layer 10, the first carrier layer 11, and the second carrier layer 12 that make up the clad plate material 2S, or the total thickness of the base material layer 10, the first carrier layer 11, and the second carrier layer 12 that make up the clad plate material 3S (T 3M =t0 + t1 + t2), and may be made thinner than or equal to that by half etching or the like (T 3M <t0 + t1 + t2). The thickness T of the first carrier portion 11M Y1 may be equal to, for example, the thickness of the first carrier layer 11 that makes up the clad plate material 1S, the thickness of the first carrier layer 11 that makes up the clad plate material 2S, or the thickness of the first carrier layer 11 that makes up the clad plate material 3S (T Y1 =t1), and may be made thinner than or equal to that by half etching or the like (T Y1 <t1). The thickness T of the second carrier portion 12M Y2 may be equal to, for example, the thickness of the second carrier layer 12 that makes up the clad plate material 1S, the thickness of the second carrier layer 12 that makes up the clad plate material 2S, or the thickness of the second carrier layer 12 that makes up the clad plate material 3S (T Y2 =t2), and may be made thinner than or equal to that by half etching or the like (T Y2 <t2).

[0054] <Modification of the Third Product Example> FIG. 11 shows a modified example of the third product example of the metal mask according to the present invention. FIG. 11 is a cross-sectional view of the metal mask 3Ma cut in the thickness direction (Z direction). The metal mask 3Ma has, for example, etching holes 3f as a mask pattern. In the cross-sectional view cut in the thickness direction, the metal mask 3Ma has a three-layer structure. The main body of the metal mask 3Ma is made up of a base material portion 10M, a first carrier portion 11M, and a second carrier portion 12M. The first carrier portion 11M has a frame portion 11f for reinforcing the metal mask 3Ma. The base material portion 10M is made up of, for example, the base material layer 10 portion constituting the clad plate material 1S shown in FIG. 3, the base material layer 10 portion constituting the clad plate material 2S shown in FIG. 4, or the base material layer 10 portion constituting the clad plate material 3S shown in FIG. 5. The first carrier portion 11M and the frame portion 11f are, for example, the first carrier layer 11 portion constituting the clad plate material 1S shown in FIG. 3, the first carrier layer 11 portion constituting the clad plate material 2S shown in FIG. 4, or the first carrier layer 11 portion constituting the clad plate material 3S shown in FIG. 5. The second carrier portion 12M is, for example, the second carrier layer 12 portion constituting the clad plate material 1S shown in FIG. 3, the second carrier layer 12 portion constituting the clad plate material 2S shown in FIG. 4, or the second carrier layer 12 portion constituting the clad plate material 3S shown in FIG. 5. The frame portion 11f can be formed when the first carrier portion 11M is formed. The frame portion 11f is arranged in a ring shape at the edge portion of the base layer 10. The metal mask 3Ma having such a frame portion 11 is easier to handle than the metal mask 3M shown in FIG. 10, because the mechanical strength is improved when the thickness of the main body of the metal mask is approximately the same. The frame portion 11f is arranged in a ring shape on the edge portion of the first carrier portion 11M, but it does not have to be arranged in a ring shape on the edge portion of the first carrier portion 11M, and may be arranged on the second carrier portion 12M on the opposite side of the first carrier portion 11M. The configuration of the frame portion 11f is not limited to the above. For example, the frame portion 11f can be composed of any of the second carrier layer 12 portion of the clad plate material 1S shown in FIG. 3, the second carrier layer 12 portion of the clad plate material 2S shown in FIG. 4, or the second carrier layer 12 portion of the clad plate material 3S shown in FIG. 5.

[0055] The metal mask 3Ma is thinned, and its thickness T 3Ma is 20 μm or less (preferably 15 μm or less). The thus thinned metal mask 3Ma has high dimensional accuracy of mask patterns such as the etching holes 3f formed by etching, and has a finer mask pattern. The thickness T of the metal mask 3Ma 3Ma may be equal to, for example, the total thickness of the base material layer 10, the first carrier layer 11, and the second carrier layer 12 constituting the clad plate material 1S, the total thickness of the base material layer 10, the first carrier layer 11, and the second carrier layer 12 constituting the clad plate material 2S, or the total thickness of the base material layer 10, the first carrier layer 11, and the second carrier layer 12 constituting the clad plate material 3S (T 3Ma =t0 + t1 + t2), and may be thinned to be equal to or less than that by means of half etching or the like (T 3Ma <t0 + t1 + t2). The thickness T of the first carrier portion 11M Y1 may be equal to, for example, the thickness of the first carrier layer 11 constituting the clad plate material 1S, the thickness of the first carrier layer 11 constituting the clad plate material 2S, or the thickness of the first carrier layer 11 constituting the clad plate material 3S (T Y1 =t1), and may be thinned to be equal to or less than that by means of half etching or the like (T Y1 <t1). The thickness T of the second carrier portion 12M Y2 may be equal to, for example, the thickness of the second carrier layer 12 constituting the clad plate material 1S, the thickness of the second carrier layer 12 constituting the clad plate material 2S, or the thickness of the second carrier layer 12 constituting the clad plate material 3S (T Y2 =t2), and may be thinned to be equal to or less than that by means of half etching or the like (T Y2 <t2). The thickness T of the frame portion 11f X may be equal to, for example, the thickness obtained by subtracting the thickness of the first carrier portion 11M from the thickness of the first carrier layer 11 constituting the clad plate material 1S, from the thickness of the first carrier layer 11 constituting the clad plate material 2S, or from the thickness of the first carrier layer 11 constituting the clad plate material 3S (T X =t1 - TY1 ), it may be thinned to the same degree or less by half etching or the like (T X <t1-T Y1 ) Note that the thickness T 3Ma and thickness T X The total thickness (T 3Ma +T X ) can also be considered as the thickness of the metal mask 3Ma.

[0056] Hereinafter, a method for manufacturing an embodiment (product example) of a metal mask according to the present invention using a clad plate material for a metal mask (first, second and third examples) according to the present invention will be described with reference to Figures 12 to 20. Note that an example of a method for manufacturing a metal mask using a clad plate material 1S (first embodiment) shown in Figure 3 will be described with reference to Figures 12 to 16, and an example of a method for manufacturing a metal mask using a clad plate material 2S (second embodiment) shown in Figure 4 and a clad plate material 3S (third embodiment) shown in Figure 5 will be described with reference to Figures 17 to 20.

[0057] <First product example> <Second product example> According to the method for manufacturing a metal mask shown in FIGS. 12 and 13, a metal mask 1M (first product example) shown in FIG. 6 and a metal mask 2M (second product example) shown in FIG. 8 can be manufactured.

[0058] In FIG. 12, step (a) is a material preparation step. In this material preparation step, for example, a clad plate material 1S shown in FIG. 3 is prepared. 1S) comprises a base layer 10 (thickness t0) and a first carrier layer 11 (thickness t1). The base layer 10 has a thickness of 1 μm or more and 20 μm or less (preferably 5 μm or more and 15 μm or less). The base layer 10 and the first carrier layer 11 are pressure welded together. The base layer 10 is made of an Fe-based alloy A containing, for example, about 32 mass% Ni and about 5.5 mass% Co. The first carrier layer 11 is made of an Fe-based alloy B containing, for example, about 36 mass% Ni. The base layer 10 made of the Fe-based alloy A and the first carrier layer 11 made of the Fe-based alloy B can be etched with a ferric chloride solution of the same quality (for example, a ferric chloride solution of a concentration of 40 mass%). The base layer 10 made of the Fe-based alloy A has higher corrosion resistance to the ferric chloride solution than the first carrier layer 11 made of the Fe-based alloy B.

[0059] 12, step (b) is a coating step in which a protective film 13 is formed on the surface 10a of the base layer 10, and a protective film 14 is formed on the surface 11a of the first carrier layer 11 in order to form a predetermined etching pattern.

[0060] In FIG. 12, step (c) is an etching step. In this etching step, the clad plate material 1S is etched using a ferric chloride solution suitable for both the Fe-based alloy A constituting the base layer 10 and the Fe-based alloy B constituting the first carrier layer 11. For example, a ferric chloride solution (aqueous solution) with a concentration of 40% by mass is used as the ferric chloride solution. By this etching, the surface 10a of the base layer 10 not having the protective film 13 and the surface 11a of the first carrier layer 11 not having the protective film 14 are simultaneously etched, and for example, etching holes 10b and etching holes 11b are formed approximately simultaneously. At this time, since the base layer 10 made of the Fe-based alloy A has a higher corrosion resistance to the ferric chloride solution than the first carrier layer 11 made of the Fe-based alloy B, the etching rate of the first carrier layer 11 side is higher than the etching rate of the base layer 10 side. Therefore, the corrosion weight loss is larger on the first carrier layer 11 side than on the base material layer 10 side, and the size (depth from the surface, opening diameter to the surface, volume inside the hole, etc.) of the etching holes 11b on the first carrier layer 11 side can be made larger than the etching holes 10b on the base material layer 10 side. Note that the sizes of the etching holes 10b and 11b can be adjusted by appropriately selecting the thicknesses, materials, etc. of the base material layer 10 and the first carrier layer 11.

[0061] In FIG. 12, step (d) is a finishing step. In this finishing step, the protective film 13 and the protective film 14 are removed from the clad plate material 1S, and the entire surface is cleaned. This allows a metal mask to be manufactured. This metal mask is composed of a substrate portion 10M made of Fe-based alloy A and a carrier portion 11M made of Fe-based alloy B. This metal mask is, for example, a metal mask 2M as shown in FIG. 8, and has, for example, a mask pattern 2f and a thickness T 2M This is a two-layered metal mask, 2M (second product example).

[0062] Next, a method for manufacturing a metal mask using the manufacturing process shown in Fig. 13 will be described. The manufacturing process shown in Fig. 13 is a process that continues from step (a) to step (c) shown in Fig. 12. By going through steps (c1) and (d1) shown in Fig. 13 following steps (a) to (c) shown in Fig. 12, it is possible to manufacture a metal mask 1M (first product example) as shown in Fig. 6, for example.

[0063] In FIG. 13, step (c1) is a half-etching step. In this half-etching step, half-etching is performed after the protective film 13 is removed from the clad plate material 1S. The half-etching is performed approximately uniformly from the surface 10a side (Z2 side) of the base layer 10 toward the first carrier layer 11 side (Z1 side) using a ferric chloride solution suitable for the Fe-based alloy A constituting the base layer 10. For example, a ferric chloride solution (aqueous solution) with a concentration of 40 mass % is used as the ferric chloride solution. This half-etching removes approximately the entire base layer 10. It is also possible to perform half-etching toward the Z1 side on the first carrier layer 11 after the base layer 10 is removed by adjusting the half-etching conditions. This allows the metal mask to be made thinner.

[0064] In FIG. 13, step (d1) is a finishing step. In this finishing step, the protective film 14 is removed from the clad plate material 1S, and the entire surface of the clad plate material 1S is cleaned, so that a metal mask can be manufactured. This metal mask is composed of a carrier portion 11M made of an Fe-based alloy B. This metal mask is, for example, a metal mask 1M as shown in FIG. 6, and has, for example, a mask pattern 1f and a thickness T 1M This is a single-layered metal mask 1M (first product example).

[0065] <First modified example of the first product example> According to the manufacturing method of the metal mask shown in Figures 12 and 14, or Figures 12 and 15, it is possible to manufacture the metal mask 1Ma (first modified example of the first product example) shown in Figure 14 or Figure 15, which has a similar configuration to the metal mask shown in Figure 7 (modified example of the first product example).

[0066] The metal mask 1Ma (first modified example of the first product example) shown in Fig. 14 or Fig. 15 can be manufactured by the manufacturing process shown in Fig. 13 or Fig. 14 following steps (a) to (c) shown in Fig. 12. In the material preparation step corresponding to step (a) shown in Fig. 12, for example, a clad plate material 1S shown in Fig. 3 is prepared. This clad plate material 1S may be similar to that in the case of the above-mentioned metal mask 1M. The coating step corresponding to step (b) and the etching step corresponding to step (c) shown in Fig. 12 may be performed in the same manner as in the case of the above-mentioned metal mask 1M.

[0067] A method for manufacturing a metal mask using the manufacturing process shown in Fig. 14 will be described. The manufacturing process shown in Fig. 14 is a process continuing from step (a) to step (c) shown in Fig. 12. In Fig. 14, step (e) is a coating step. In this coating step, in order to form a frame portion 11f (see step (h)) of a predetermined shape on the Z1 side, a protective film 15 is formed on the surface 11a of the first carrier layer 11, a protective film 16 is formed in the etching holes 11b (see Fig. 12), and a protective film 17 is formed on the surface 10a and the etching holes 10b of the base material layer 10.

[0068] In FIG. 14, step (f) is an etching step. In this etching step, the first carrier layer 11 is etched using a ferric chloride solution suitable for the Fe-based alloy B constituting the first carrier layer 11. For example, a ferric chloride solution (aqueous solution) with a concentration of 40 mass % is used as the ferric chloride solution. By this etching, the surface 11a of the first carrier layer 11 not having the protective film 15 and the protective film 16 is etched, and for example, an etching hole 11c is formed. The depth (etching amount) of the etching hole 11c can be adjusted by adjusting the etching conditions, etc.

[0069] In FIG. 14, step (g) is a half-etching step. In this half-etching step, first, the protective film 17 is removed from the base layer 10. Next, a protective film 18 is formed on the surface 11a of the first carrier layer 11 including the etching holes 11b and 11c, and a protective film 19 is formed in the etching holes 10b (see FIG. 12). After that, half-etching is performed. The half-etching is performed approximately uniformly from the surface 10a side (Z2 side) of the base layer 10 toward the first carrier layer 11 side (Z1 side). The half-etching removes approximately the entire base layer 10. It is also possible to perform half-etching toward the Z1 side on the first carrier layer 11 after the base layer 10 has been removed by adjusting the half-etching conditions. This allows the metal mask to be thinned.

[0070] In FIG. 14, step (h) is a finishing step. In this finishing step, the protective film 18 and the protective film 19 are removed from the clad plate material 1S, and the entire surface is cleaned. This allows a metal mask to be manufactured. This metal mask is composed of a carrier portion 11M made of an Fe-based alloy B, and a frame portion 11f is arranged in an annular shape on the peripheral portion on the Z1 side of the carrier portion 11M. This frame portion 11f is made of the first carrier layer 11 portion. This metal mask has a similar structure to the metal mask shown in FIG. 7, for example, and is a metal mask having a thickness T 1Ma 1 is a metal mask 1Ma having a single-layer structure (a first modified example of the first product example).

[0071] Next, a method for manufacturing a metal mask using the manufacturing process shown in FIG. 15 will be described. The manufacturing process shown in FIG. 15 is a process that continues from step (a) to step (c) shown in FIG. 12. In FIG. 15, step (e1) is a coating step. In this coating step, in order to form a frame portion 11f (see step (h1)) of a predetermined shape on the Z1 side, a protective film 15 is formed on the surface 11a of the first carrier layer 11, a protective film 16 is formed in the etching hole 11b (see FIG. 12), and a protective film 19 is formed in the etching hole 10b (see FIG. 12). Note that no protective film is formed on the surface 10a of the base material layer 10.

[0072] In FIG. 15, step (f1) is an etching and half-etching step. In this etching and half-etching step, the first carrier layer 11 side (Z1 side) and the base layer 10 side (Z2 side) are simultaneously etched using a ferric chloride solution suitable for both the Fe-based alloy A constituting the base layer 10 and the Fe-based alloy B constituting the first carrier layer 11. For example, a ferric chloride solution (aqueous solution) with a concentration of 40 mass % is used as this ferric chloride solution. By this etching, the surface 11a of the first carrier layer 11 not having the protective film 15 and the protective film 16 is etched, and for example, an etching hole 11c is formed. The depth (etching amount) of this etching hole 11c can be adjusted by adjusting the etching conditions. At the same time, the surface 10a of the base layer 10 not having the protective film 19 is almost uniformly half-etched toward the first carrier layer 11 side (Z1 side), and almost the entire base layer 10 is removed. By adjusting the half-etching conditions, it is also possible to perform half-etching toward the Z1 side on the first carrier layer 11 after the base layer 10 has been removed. This makes it possible to thin the metal mask.

[0073] In FIG. 15, step (h1) is a finishing step. In this finishing step, the protective film 15, the protective film 16 and the protective film 19 are removed from the clad plate material 1S, and the entire surface is cleaned. This makes it possible to manufacture a metal mask. This metal mask is composed of a carrier part 11M made of an Fe-based alloy B, and a frame part 11f is arranged in an annular shape on the peripheral part on the Z1 side of the carrier part 11M. This frame part 11f is made of the first carrier layer 11 part. This metal mask has a similar structure to the metal mask shown in FIG. 7, for example, and is a metal mask having a thickness T 1Ma 1 is a metal mask 1Ma having a single-layer structure (a first modified example of the first product example).

[0074] <Second modified example of the first product example> According to the manufacturing method of the metal mask shown in Figures 12 and 16, it is possible to manufacture a metal mask 1Mb (second modified example of the first product example) shown in Figure 16, which has a similar configuration to the metal mask shown in Figure 7 (modified example of the first product example) and in which the frame portion 11f is arranged on the Z2 side.

[0075] Metal mask 1Mb (second modified example of the first product example) shown in Fig. 16 can be manufactured by the manufacturing process shown in Fig. 16 following steps (a) to (c) shown in Fig. 12. In the material preparation step corresponding to step (a) shown in Fig. 12, for example, clad plate material 1S shown in Fig. 3 is prepared. This clad plate material 1S may be similar to that in the case of metal mask 1M described above. The coating step corresponding to step (b) and the etching step corresponding to step (c) shown in Fig. 12 may be performed in the same manner as in the case of metal mask 1M described above.

[0076] The manufacturing process shown in Fig. 16 is a process continuing from step (a) to step (c) shown in Fig. 12. In Fig. 16, step (e2) is a coating step. In this coating step, in order to form a frame portion 10f (see step (h2)) of a predetermined shape on the Z2 side, a protective film 17 is formed on the surface 10a of the base material layer 10, a protective film 19 is formed in the etching holes 10b, and a protective film 20 is formed on the surface 11a and the etching holes 11b (see Fig. 12) of the first carrier layer 11.

[0077] In FIG. 16, step (f2) is an etching step. In this etching step, the base layer 10 is etched using a ferric chloride solution suitable for the Fe-based alloy A constituting the base layer 10. For example, a ferric chloride solution (aqueous solution) with a concentration of 40% by mass is used as the ferric chloride solution. By this etching, the surface 10a of the base layer 10 not having the protective film 17 and the protective film 19 is etched, and substantially the entire base layer 10 is removed, and for example, an etching hole 10c is formed. The depth (etching amount) of the etching hole 10c can be adjusted by adjusting the etching conditions. It is also possible to etch the first carrier layer 11 from which the base layer 10 has been removed toward the Z1 side by adjusting the etching conditions. This allows the metal mask to be made thinner.

[0078] In FIG. 16, step (h2) is a finishing step. In this finishing step, the protective film 17, the protective film 19, and the protective film 20 are removed, and the entire surface is cleaned. This allows the manufacture of a metal mask. This metal mask is composed of a carrier part 11M made of an Fe-based alloy B, and a frame part 10f is arranged in an annular shape on the peripheral part on the Z2 side of the carrier part 11M. This frame part 10f is made of a base material layer 10 part. This metal mask has a similar structure to the metal mask shown in FIG. 7, for example, and the frame part 10f is arranged on the Z2 side. This frame part 10f is made of a second carrier layer 12 part. This metal mask is, for example, a mask having a thickness T 1Mb This metal mask 1Mb is a second modified example of the first product example. The main body of this metal mask 1Mb has a single-layer structure.

[0079] <Third product example> According to the metal mask manufacturing method shown in FIG. 17, the metal mask 3M (third product example) shown in FIG. 10 can be manufactured.

[0080] In Fig. 17, step (i) is a material preparation step. In this material preparation step, for example, the clad plate material 2S shown in Fig. 4 or the clad plate material 3S shown in Fig. 5 is prepared. In Fig. 16, the clad plate material 2S shown in Fig. 4 is given as a representative example. The clad plate material 2S (thickness T 2S ) comprises a base layer 10 (thickness t0), a first carrier layer 11 (thickness t1), and a second carrier layer 12 (thickness t2). The base layer 10 has a thickness of 1 μm or more and 20 μm or less (preferably 5 μm or more and 15 μm or less). The base layer 10 and the first carrier layer 11 are directly pressed together. The base layer 10 and the second carrier layer 12 are directly pressed together. The base layer 10 is made of an Fe-based alloy A containing, for example, about 32 mass% Ni and about 5.5 mass% Co. The first carrier layer 11 is made of an Fe-based alloy B containing, for example, about 36 mass% Ni. The second carrier layer 12 is made of an Fe-based alloy C, which can be etched with a ferric chloride solution of the same quality as the Fe-based alloy B, and has higher corrosion resistance to the ferric chloride solution than the Fe-based alloy B. The base layer 10 made of Fe-based alloy A, the first carrier layer 11 made of Fe-based alloy B, and the second carrier layer 12 made of Fe-based alloy C can all be etched with the same ferric chloride solution (e.g., ferric chloride solution with a concentration of 40 mass %). The base layer 10 made of Fe-based alloy A has higher corrosion resistance to the ferric chloride solution than the first carrier layer 11 made of Fe-based alloy B, and has higher corrosion resistance than the second carrier layer 12 made of Fe-based alloy C.

[0081] 17, step (j) is a coating step in which a protective film 13 is formed on the surface 11a of the first carrier layer 11, and a protective film 14 is formed on the surface 12a of the second carrier layer 12 in order to form a predetermined etching pattern.

[0082] In FIG. 17, step (k) is an etching step. In this etching step, the clad plate material 2S is etched using a ferric chloride solution suitable for both the Fe-based alloy B constituting the first carrier layer 11 and the Fe-based alloy C constituting the second carrier layer 12. For example, a ferric chloride solution (aqueous solution) with a concentration of 40% by mass is used as the ferric chloride solution. By this etching, the surface 11a of the first carrier layer 11 not having the protective film 13 and the surface 12a of the second carrier layer 12 not having the protective film 14 are simultaneously etched, and for example, the etching holes 11b and the etching holes 12b are formed almost simultaneously. At this time, since the second carrier layer 12 made of the Fe-based alloy C has higher corrosion resistance to the ferric chloride solution than the first carrier layer 11 made of the Fe-based alloy B, the etching rate on the first carrier layer 11 side is higher than the etching rate on the second carrier layer 12 side. Therefore, the corrosion weight loss is larger on the first carrier layer 11 side than on the base material layer 10 side, and the formation of the etching holes from the Z1 side to the Z2 side proceeds more quickly. As a result, since etching of the base layer 10 progresses from the Z1 side, the size (depth from the surface, opening diameter to the surface, volume inside the hole, etc.) of the etching hole 11b on the first carrier layer 11 side (Z1 side) can be made larger than the etching hole 12b on the second carrier layer 12 side (Z2 side). Note that the size of the etching hole 11b and the etching hole 12b can be adjusted by appropriately selecting the thickness, material, etc. of the first carrier layer 11 and the second carrier layer 12.

[0083] In Fig. 17, step (m) is a finishing step. In this finishing step, the protective film 13 and the protective film 14 are removed from the clad plate material 2S, and the entire surface is cleaned. This allows a metal mask to be manufactured. This metal mask is composed of a substrate part 10M made of Fe-based alloy A, a first carrier part 11M made of Fe-based alloy B, and a second carrier part 12M made of Fe-based alloy C. This metal mask is, for example, a metal mask 3M as shown in Fig. 10, and has, for example, a mask pattern 3f and a thickness T 3M This is a three-layer metal mask from 3M (third product example).

[0084] <Modification of the third product example> According to the manufacturing process shown in FIGS. 17 and 18, the metal mask 3Ma (a modified example of the third product example) shown in FIG. 11 can be manufactured.

[0085] The metal mask 3Ma shown in FIG. 11 (a modified example of the third product example) can be manufactured by the manufacturing process shown in FIG. 18 following the steps (i) to (k) shown in FIG. 17. In the material preparation step corresponding to the step (a) shown in FIG. 17, for example, the clad plate material 3S shown in FIG. 5 is prepared. The clad plate material 3S (thickness T 3S ) comprises a base layer 10 (thickness t0), a first carrier layer 11 (thickness t1), and a second carrier layer 12 (thickness t2, t1>t2). The thickness of the base layer 10 is 1 μm or more and 20 μm or less (preferably 5 μm or more and 15 μm or less). The thickness t1 of the first carrier layer 11 is made thicker than the thickness t2 of the second carrier layer 12 (see FIG. 5, t1>t2) in order to provide a frame portion 11f (see FIG. 18) using the first carrier layer 11 portion. The base layer 10 and the first carrier layer 11 are directly pressure-welded. The base layer 10 and the second carrier layer 12 are directly pressure-welded. The base layer 10 is made of, for example, an Fe-based alloy A containing about 32 mass % Ni and about 5.5 mass % Co. The first carrier layer 11 is made of, for example, an Fe-based alloy B containing about 36 mass % Ni. The second carrier layer 12 is made of Fe-based alloy C, can be etched with a ferric chloride solution of the same quality as that of the Fe-based alloy B, and has higher corrosion resistance to the ferric chloride solution than the Fe-based alloy B. The base layer 10 made of Fe-based alloy A, the first carrier layer 11 made of Fe-based alloy B, and the second carrier layer 12 made of Fe-based alloy C can all be etched with a ferric chloride solution of the same quality (e.g., a ferric chloride solution of 40 mass% concentration). The base layer 10 made of Fe-based alloy A has higher corrosion resistance to the ferric chloride solution than the first carrier layer 11 made of Fe-based alloy B, and has higher corrosion resistance than the second carrier layer 12 made of Fe-based alloy C. The coating step corresponding to step (j) and the etching step corresponding to step (k) shown in FIG. 17 may be performed in the same manner as in the case of the metal mask 3M described above.

[0086] The manufacturing process shown in Fig. 18 is a process continuing from step (i) to step (k) shown in Fig. 17. In Fig. 18, step (n) is a coating step. In this coating step, in order to form a frame portion 11f (see step (q)) of a predetermined shape on the Z1 side, a protective film 15 is formed on the surface 11a of the first carrier layer 11, a protective film 16 is formed in the etching hole 11b (see Fig. 17), and a protective film 17 is formed on the surface 12a and the etching hole 12b (see Fig. 17) of the second carrier layer 12.

[0087] In FIG. 18, step (p) is an etching step. In this etching step, the first carrier layer 11 is etched using a ferric chloride solution suitable for the Fe-based alloy B constituting the first carrier layer 11. For example, a ferric chloride solution (aqueous solution) with a concentration of 40 mass % is used as the ferric chloride solution. By this etching, the surface 11a of the first carrier layer 11 not having the protective film 15 is etched, and for example, an etching hole 11c is formed. The depth of the etching hole 11c can be adjusted by adjusting conditions such as the etching time.

[0088] In FIG. 18, step (q) is a finishing step. In this finishing step, the protective film 15, the protective film 16 and the protective film 17 are removed from the clad plate material 3S, and the entire surface is cleaned. This allows a metal mask to be manufactured. This metal mask is composed of a substrate portion 10M made of Fe-based alloy A, a first carrier portion 11M made of Fe-based alloy B, and a second carrier portion 12M made of Fe-based alloy C, and a frame portion 11f is arranged in an annular shape on the peripheral portion on the Z1 side of the first carrier portion 11M. This frame portion 11f is composed of the first carrier layer 11 portion. This metal mask is, for example, a metal mask 3Ma as shown in FIG. 11, and is, for example, a metal mask having a thickness T 3Ma This is a three-layered metal mask, 3Ma (third product example).

[0089] <Modification of the second product example> According to the manufacturing process shown in FIGS. 17 and 19, the metal mask 2Ma (a modified example of the second product example) shown in FIG. 9 can be manufactured.

[0090] The metal mask 2Ma (a modified example of the second product example) shown in FIG. 9 can be manufactured by the manufacturing process shown in FIG. 19 following the steps (i) to (k) shown in FIG. 17. In the material preparation step corresponding to the step (a) shown in FIG. 17, for example, the clad plate material 2S shown in FIG. 4 or the clad plate material 3S shown in FIG. 5 is prepared. In FIG. 19, the clad plate material 2S shown in FIG. 4 is shown as a representative. This clad plate material 2S may be similar to the case of the above-mentioned metal mask 3M. The thickness t1 of the first carrier layer 11 may be approximately equal to the thickness t2 of the second carrier layer 12 (see FIG. 4, t1=t2) in order to provide the frame portion 11f (see FIG. 18) by etching the first carrier layer 11 portion. The covering step corresponding to the step (b) and the etching step corresponding to the step (c) shown in FIG. 17 may be performed in the same manner as the case of the above-mentioned metal mask 3M.

[0091] The manufacturing process shown in Fig. 19 is a process continuing from step (i) to step (k) shown in Fig. 17. In Fig. 19, step (n1) is a coating step. In this coating step, in order to form a frame portion 11f (see step (q1)) of a predetermined shape on the Z1 side, a protective film 15 is formed on the surface 11a of the first carrier layer 11, a protective film 16 is formed in the etching hole 11b (see Fig. 17), and a protective film 17 is formed on the surface 12a and the etching hole 12b (see Fig. 17) of the second carrier layer 12.

[0092] In FIG. 19, step (p1) is an etching step. In this etching step, the first carrier layer 11 is etched using a ferric chloride solution suitable for the Fe-based alloy B constituting the first carrier layer 11. For example, a ferric chloride solution (aqueous solution) with a concentration of 40% by mass is used as the ferric chloride solution. By this etching, the surface 11a of the first carrier layer 11 not having the protective film 15 is etched, and substantially the entire first carrier layer 11 is removed, and for example, an etching hole 11c is formed. Note that the depth of the etching hole 11c can be adjusted by adjusting the conditions such as the etching time. In addition, by adjusting the etching conditions, it is also possible to etch the base layer 10 from which the first carrier layer 11 has been removed toward the Z2 side. This allows the metal mask to be made thinner.

[0093] In FIG. 19, step (q1) is a finishing step. In this finishing step, the protective film 15, the protective film 16, and the protective film 17 are removed from the clad plate material 2S, and the entire surface is cleaned. This allows a metal mask to be manufactured. The main body of this metal mask is composed of a base material portion 10M made of Fe-based alloy A and a second carrier portion 12M made of Fe-based alloy C. This metal mask has a ring-shaped frame portion 11f arranged on the peripheral portion on the Z1 side of the first carrier portion 11M made of Fe-based alloy B. This frame portion 11f is composed of the first carrier layer 11 portion. This metal mask is, for example, a metal mask 2Ma as shown in FIG. 9, and is, for example, a metal mask having a thickness T 2Ma 1 is a metal mask 2Ma (a modified example of the second product example). The main body of this metal mask 2Ma has a two-layer structure.

[0094] <Third modified example of the first product example> 17 and 20, it is possible to manufacture the metal mask 1Ma (a modified example of the first product example) shown in Fig. 7. For convenience, the metal mask 1Ma shown in Fig. 20 obtained by this manufacturing process is referred to as the third modified example of the first product example.

[0095] The metal mask 1Ma (the third modification example of the first product example) shown in FIG. 7 can be manufactured by the manufacturing process shown in FIG. 20 following the processes (i) to (k) shown in FIG. 17. In the material preparation process corresponding to the process (a) shown in FIG. 17, for example, a clad sheet similar to the clad sheet 2S shown in FIG. 4 or the clad sheet 3S shown in FIG. 5 is prepared. This clad sheet 3S may be the same as that in the case of the above-described metal mask 3Ma (see FIG. 18), but may not be the same as that in the case of the above-described metal mask 3Ma (see FIG. 18). The clad sheet 3S may have, for example, a thickness t2 of the second carrier layer 12 thicker than a thickness t1 of the first carrier layer 11 (t1 < t2). In FIG. 20, a three-layer clad sheet (hereinafter referred to as the clad sheet 3S) similar to the clad sheet 3S shown in FIG. 5 is exemplarily shown. The base material layer 10 is made of, for example, the above-described Fe-based alloy A. The first carrier layer 11 is made of, for example, the above-described Fe-based alloy C, which is more easily etched with ferric chloride solution of the same quality as the above-described Fe-based alloy A. The second carrier layer 12 is made of, for example, the above-described Fe-based alloy B, which is more easily etched with ferric chloride solution of the same quality as the above-described Fe-based alloy C. Therefore, the base material layer 10, the first carrier layer 11, and the second carrier layer 12 can be etched simultaneously. Also, with respect to the ferric chloride solution, the base material layer 10 has higher corrosion resistance than the first carrier layer 11 and the second carrier layer 12, and the first carrier layer 11 has higher corrosion resistance than the second carrier layer 12. The coating process corresponding to the process (b) shown in FIG. 17 may be performed in the same manner as in the case of the above-described metal mask 3M. Also, in the etching process corresponding to the process (c), since the first carrier layer 11 has higher corrosion resistance than the second carrier layer 12, the etching rate of the second carrier layer 12 becomes larger than the etching rate of the first carrier layer 11. Therefore, it may be adjusted in consideration of the fact that the etching amount (depth) from the second carrier layer 12 side (Z2 side) toward the Z1 side becomes larger than the etching amount (depth) from the first carrier layer 11 side (Z1 side) toward the Z1 side.

[0096] The manufacturing process shown in FIG. 20 is a process continuing from step (i) to step (k) shown in FIG. 17. In FIG. 20, step (n2) is a coating step. In this coating step, in order to form a frame portion 11f (see step (q2)) of a predetermined shape on the Z1 side, a protective film 15 is formed on the surface 11a of the first carrier layer 11, a protective film 16 is formed in the etching hole 11b (see FIG. 17), and a protective film 19 is formed in the etching hole 12b (see FIG. 17). Note that no protective film is formed on the surface 11a of the second carrier layer 11.

[0097] In FIG. 20, step (p2) is an etching and half-etching step. In this etching and half-etching step, the first carrier layer 11 and the second carrier layer 12 are simultaneously etched using a ferric chloride solution suitable for the Fe-based alloy B constituting the first carrier layer 11 and the Fe-based alloy C constituting the second carrier layer 12. For example, a ferric chloride solution (aqueous solution) with a concentration of 40 mass % is used as the ferric chloride solution. By this etching, the surface 11a of the first carrier layer 11 not having the protective film 15 is etched, and substantially the entire first carrier layer 11 is removed, and for example, an etching hole 11c is formed. At the same time, the surface 12a of the second carrier layer 12 not having the protective film 19 is substantially uniformly half-etched toward the base layer 10 side (Z1 side), and substantially the entire second carrier layer 11 is removed. In this case, the etching rate of the second carrier layer 12 is higher than the etching rate of the first carrier layer 11, which is more corrosion-resistant than the second carrier layer 12. Therefore, the amount (depth) of etching from the second carrier layer 12 side (Z2 side) toward the Z1 side is larger than the amount (depth) of etching from the first carrier layer 11 side (Z1 side) toward the Z1 side. Therefore, taking into consideration the difference in thickness and corrosion resistance between the first carrier layer 11 and the second carrier layer 12, it is possible to adjust so that the second carrier layer 12 is substantially removed at substantially the same time as the formation of the etching hole 11C. The depth of the etching hole 11c can be adjusted by adjusting the etching conditions. In addition, by adjusting the etching conditions, it is also possible to perform half etching toward the Z1 side on the base layer 10 after the second carrier layer 12 has been removed. This allows the metal mask to be made thinner.

[0098] In FIG. 20, step (q2) is a finishing step. In this finishing step, the protective film 15, the protective film 16 and the protective film 19 are removed from the clad plate material 2S, and the entire surface is cleaned. This allows a metal mask to be manufactured. The main part of this metal mask is composed of a substrate 10M made of an Fe-based alloy A. This metal mask has a ring-shaped frame portion 11f disposed on the peripheral portion on the Z1 side of the substrate 10M. This frame portion 11f is composed of a first carrier layer 11 portion. This metal mask is, for example, a metal mask 1Ma as shown in FIG. 7, and is, for example, a metal mask having a thickness T 1Ma 17 and 20, a metal mask using the clad plate material 3S can be manufactured, which is sufficiently easy to handle, and has a high possibility of enabling the metal mask to be sufficiently thin-walled. Also, according to a method for manufacturing a metal mask using the clad plate material 3S as shown in FIG. 17 and FIG. 20, which is sufficiently easy to handle, a metal mask with a sufficiently thin wall can be manufactured, and a sufficient improvement in productivity can be expected. [Explanation of symbols]

[0099] <Fig. 1, Fig. 2> 100, 200. Metal mask 100a. Metal plate material 100b.1st surface 100c.2nd surface 100d, 100e, 201b, 202b. Etching holes 100f. Mask pattern 101~104.Protective film 200. Metal Mask 200a. Clad plate material 200f. Mask pattern 201.1st layer 201a, 202a.Surface 202.Second layer 203, 204.Protective film <Fig. 3~Fig. 5> 1S. Clad plate material (first embodiment) 2S. Clad plate material (second embodiment) 3S. Clad plate material (third embodiment) 10.Base material layer 11. First carrier layer 12. Second carrier layer <Figures 6 to 11> 1M. Metal mask (first product example) 1Ma. Metal mask (a variation of the first product example) 1f, 2f, 3f. Mask pattern 2M. Metal mask (second product example) 2Ma. Metal mask (variation of the second product example) 3M. Metal mask (third product example) 3Ma. Metal mask (variation of the third product example) 10M.Base material part 11M. Carrier section (first carrier section) 11f. Frame section 12M. Carrier section (second carrier section) <Fig. 12, Fig. 13> 1M. Metal mask 1S. Clad plate material 1f, 2f. Mask pattern 2M. Metal Mask 10.Base material layer 10M.Base material part 10a, 11a.Surface 10b, 11b. Etching holes 11. First carrier layer 11M. Carrier Section 13, 14.Protective film <Fig. 14~Fig. 16> 1Ma, 1Mb. Metal mask 1f, 1fa. Mask pattern 10.Base material layer 10a, 11a.Surface 10c, 11c. Etching holes 10f, 11f. Frame section 11. First carrier layer 11M. Carrier Section 15~20.Protective film <Figures 17 to 20> 1Ma, 2Ma, 3M, 3Ma. Metal mask 1f, 2f, 3f. Mask pattern 2S, 3S. Clad plate material 10.Base material layer 10M.Base material part 11. First carrier layer 11M. First Carrier Section 11a, 12a.Surface 11b, 12b. Etching holes 12. Second carrier layer 12M. First Carrier Section 13~17, 19.Protective film

Claims

1. A substrate layer is made of an Fe-based alloy containing at least one of Ni and Co in a range of 30 mass% to 50 mass% in a cross-sectional view cut in a thickness direction, and a first carrier layer is directly pressed against one side of the substrate layer, the base layer and the first carrier layer can be etched with a ferric chloride solution of the same quality, and the base layer has higher corrosion resistance to the ferric chloride solution than the first carrier layer; Etching was performed using the same ferric chloride solution under the same environment, and the corrosion loss of the substrate layer was measured. b The corrosion loss of the first carrier layer is M C1 When the base layer and the first carrier layer are b / M c1 A clad sheet material for metal masks that satisfies the relationship of ≦0.

9.

2. In a cross-sectional view cut in the thickness direction, the magnet comprises a base layer made of an Fe-based alloy containing at least one of Ni and Co in a range of 30 mass % to 50 mass %, a first carrier layer directly pressed onto one side of the base layer, and a second carrier layer directly pressed onto the other side of the base layer, the base layer, the first carrier layer, and the second carrier layer can be etched with a homogeneous ferric chloride solution, and the base layer has higher corrosion resistance to the ferric chloride solution than the first carrier layer and the second carrier layer; Etching was performed using the same ferric chloride solution under the same environment, and the corrosion loss of the substrate layer was measured. b The corrosion loss of the first carrier layer is M C1 The corrosion loss of the second carrier layer is M C2 wherein the base layer, the first carrier layer and the second carrier layer are M b / M c1 ≦0.9 and M b / M c2 A clad sheet material for metal masks that satisfies the relationship of ≦0.

9.

3. A metal mask formed using the clad plate material for metal masks according to claim 1 or 2, A metal mask comprising: a first metal layer made of the Fe-based alloy constituting the base layer; and a second metal layer made of the metal constituting the first carrier layer, wherein the first metal layer and the second metal layer are directly bonded to each other.

4. A metal mask formed using the clad material plate for metal masks according to claim 2, A metal mask comprising: a first metal layer made of the Fe-based alloy constituting the base layer; a second metal layer made of a metal constituting the first carrier layer; and a third metal layer made of a metal constituting the second carrier layer, wherein the second metal layer, the first metal layer, and the third metal layer are directly bonded in this order.

Citation Information

Patent Citations

  • Automatic seed bag feeding device

    JP1987021629A

  • Shadowmask member

    JP1987082630A

  • Portable multipurpose precise length measuring method

    JP1988019505A

  • - Production of silicon carbide and carbon composite material

    JP1989003072A

  • Metal mask

    JP2004039319A