Reflective mask blank and reflective mask
A phase shift film with Ir, O, and N, and additional elements like Ta, Cr, Mo, W, or Si, addresses crystallization issues in EUV lithography, enhancing patterning precision by maintaining optical properties and reducing sidewall roughness.
Patent Information
- Application Number
- JP2023192035
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2022-11-09
- Filing Date
- 2023-11-10
- Publication Date
- 2024-09-18
- Estimated Expiration
- 2043-06-23
AI Technical Summary
Ir-based phase shift films in EUV lithography tend to crystallize, leading to increased sidewall roughness of opening patterns due to etching along grain boundaries, and alloying with elements like Nb or Zr deteriorates optical properties.
A phase shift film composed of Ir, O, and N, with additional elements like Ta, Cr, Mo, W, or Si, is used, with controlled XRD peak intensity and extinction coefficient to suppress crystallization and maintain optical properties.
The solution effectively suppresses crystallization and maintains optical properties, reducing sidewall roughness and improving patterning precision in EUV lithography.
Smart Images

Figure 0007552830000008 
Figure 0007552830000014 
Figure 0007552830000011
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a reflective mask blank and a reflective mask. [Background technology]
[0002] In recent years, with the miniaturization of semiconductor devices, EUV lithography (EUVL), an exposure technology using extreme ultraviolet (EUV) light, has been developed. EUV includes soft X-rays and vacuum ultraviolet light, and specifically refers to light with a wavelength of about 0.2 nm to 100 nm. At present, EUV with a wavelength of about 13.5 nm is mainly being considered.
[0003] In EUVL, a reflective mask is used. The reflective mask has, in this order, a substrate such as a glass substrate, a multilayer reflective film that reflects EUV light, a protective film that protects the multilayer reflective film, and a phase shift film that shifts the phase of the EUV light. An opening pattern is formed in the phase shift film. In EUVL, the opening pattern in the phase shift film is transferred to a target substrate such as a semiconductor substrate. Transferring includes reducing and transferring.
[0004] The phase shift film of Patent Document 1 is made of an alloy containing elements selected from Group A and Group B in order to suppress the variation in phase difference caused by the variation in the film thickness of the phase shift film. Group A consists of Pd, Ag, Pt, Au, Ir, W, Cr, Mn, Sn, Ta, V, Fe, and Hf. Group B consists of Rh, Ru, Mo, Nb, Zr, and Y.
[0005] The phase shift film of Patent Document 2 has a top layer and other layers below. The top layer contains at least one metal element selected from Rh, Pd, Ag, Pt, Ru, Au, Ir, Co, Sn, Ni, Re, Mo, and Nb, and further contains hydrogen or deuterium. The top layer has a microcrystalline structure or an amorphous structure by containing hydrogen or deuterium. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Japanese Patent Application Publication No. 2018-146945 [Patent Document 2] Japanese Patent Application Publication No. 2021-128247 Summary of the Invention [Problem to be solved by the invention]
[0007] The phase shift film may be made of an Ir-based material. An Ir-based material is a material that contains Ir as a main component. Ir has a small refractive index for EUV light and a large extinction coefficient for EUV light. Therefore, by using an Ir-based material as the phase shift film material, the phase shift film can be made thin while maintaining the desired phase difference.
[0008] However, when Ir is used alone, it has the problem of being prone to crystallization. The larger the crystal size, the rougher the sidewalls of the opening pattern become. This is because etching tends to proceed along the crystal grain boundaries when the opening pattern is formed.
[0009] Patent Document 1 describes that the phase shift film contains Ir, but does not describe the crystallization of Ir. Although it is possible to suppress the crystallization of Ir by alloying Ir with Nb, Zr, or Y, the optical properties (refractive index and extinction coefficient) of the phase shift film will deteriorate.
[0010] Patent Document 2 describes that the phase shift film contains Ir, but does not describe experimental data on the phase shift film containing Ir. According to the knowledge of the present inventors, Ir is difficult to bond with hydrogen or deuterium, and it is difficult to suppress the crystallization of Ir using hydrogen or deuterium.
[0011] One aspect of the present disclosure provides a technique for suppressing crystallization of a phase shift film while suppressing degradation of optical properties of the phase shift film when the phase shift film contains Ir as a main component. [Means for solving the problem]
[0012] A reflective mask blank according to an embodiment of the present disclosure includes, in this order, a substrate, a multilayer reflective film that reflects EUV light, a protective film that protects the multilayer reflective film, and a phase shift film that shifts the phase of the EUV light. The phase shift film is mainly made of Ir, and has a ratio (Ip / Ia) of a maximum peak intensity Ip in a range of 35° to 45° of 2θ to an average intensity Ia in a range of 55° to 60° in an XRD method using CuKα radiation of 1.0 to 30, a refractive index n for the EUV light of 0.925 or less, and an extinction coefficient k for the EUV light of 0.030 or more. The phase shift film contains 50 at% or more of Ir, O and N, and at least one second element X2 selected from a second group consisting of Ta, Cr, Mo, W, Re, and Si. A grayscale image of the phase shift film is obtained by imaging a cross section of the phase shift film with a scanning transmission electron microscope (STEM), and a luminance profile of the grayscale image is created. The skewness (Rsk) in the luminance profile is negative. Effect of the Invention
[0013] According to one embodiment of the present disclosure, when the phase shift film contains Ir as a main component, it is possible to suppress the crystallization of the phase shift film while suppressing the deterioration of the optical properties of the phase shift film. [Brief description of the drawings]
[0014] [Figure 1] FIG. 1 is a cross-sectional view showing a reflective mask blank according to one embodiment. [Diagram 2] FIG. 2 is a cross-sectional view showing a reflective mask according to an embodiment. [Diagram 3] FIG. 3 is a cross-sectional view showing an example of EUV light reflected by the reflective mask of FIG. [Figure 4] FIG. 4 is a flowchart showing a method for manufacturing a reflective mask blank according to one embodiment. [Diagram 5] FIG. 5 is a flowchart showing a method for manufacturing a reflective mask according to an embodiment. [Figure 6]FIG. 6 is a diagram showing the optical properties of the phase shift films according to Examples 1 to 5. In FIG. [Figure 7] FIG. 7 is a diagram showing X-ray diffraction spectra of the phase shift films according to Examples 1 to 5. As shown in FIG. [Figure 8] FIG. 8 is an enlarged view of a portion of FIG. [Figure 9] FIG. 9 is a diagram showing X-ray diffraction spectra of the phase shift films according to Examples 6 to 10. As shown in FIG. [Figure 10] FIG. 10 is a diagram showing X-ray diffraction spectra of the phase shift films of Examples 11, 12, 19 and 20. [Figure 11] FIG. 11 is a diagram showing an example of dispersed particles and a matrix. [Figure 12] FIG. 12 is a STEM image of the phase shift film according to Example 1. [Figure 13] FIG. 13 is a STEM image of the phase shift film according to Example 6. [Figure 14] FIG. 14 is a STEM image of the phase shift film of Example 19. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] Hereinafter, the embodiments of the present disclosure will be described with reference to the drawings. In each drawing, the same or corresponding configurations are denoted by the same reference numerals, and the description may be omitted. In the specification, the symbol "~" indicating a range of values means that the values before and after the symbol are included as the lower and upper limits.
[0016] 1 to 3, the X-axis direction, the Y-axis direction, and the Z-axis direction are perpendicular to each other. The Z-axis direction is perpendicular to the first main surface 10a of the substrate 10. The X-axis direction is perpendicular to the incidence surface of the EUV light (the surface including the incident light beam and the reflected light beam). As shown in FIG. 3, when viewed from the X-axis direction, the incident light beam is inclined toward the positive Y-axis direction as it moves toward the negative Z-axis direction, and the reflected light beam is inclined toward the positive Y-axis direction as it moves toward the positive Z-axis direction.
[0017] A reflective mask blank 1 according to one embodiment will be described with reference to Fig. 1. The reflective mask blank 1 has, for example, a substrate 10, a multilayer reflective film 11, a protective film 12, a phase shift film 13, and an etching mask film 14, in this order. The multilayer reflective film 11, the protective film 12, the phase shift film 13, and the etching mask film 14 are formed, in this order, on a first main surface 10a of the substrate 10. It should be noted that the reflective mask blank 1 only needs to have at least the substrate 10, the multilayer reflective film 11, the protective film 12, and the phase shift film 13.
[0018] The reflective mask blank 1 may further have a functional film not shown in Fig. 1. For example, the reflective mask blank 1 may have a conductive film on the opposite side of the substrate 10 to the multilayer reflective film 11. The conductive film is formed on the second main surface 10b of the substrate 10. The second main surface 10b is the surface facing opposite to the first main surface 10a. The conductive film is used, for example, to attach the reflective mask 2 to an electrostatic chuck of an exposure device.
[0019] Although not shown, the reflective mask blank 1 may have a buffer film between the protective film 12 and the phase shift film 13. The buffer film protects the protective film 12 from an etching gas that forms an opening pattern 13a in the phase shift film 13. The buffer film is etched more slowly than the phase shift film 13. Unlike the protective film 12, the buffer film will ultimately have the same opening pattern as the opening pattern 13a of the phase shift film 13.
[0020] Next, a reflective mask 2 according to one embodiment will be described with reference to Figures 2 and 3. The reflective mask 2 is produced, for example, by using the reflective mask blank 1 shown in Figure 1, and includes an opening pattern 13a in a phase shift film 13. Note that the etching mask film 14 shown in Figure 1 is removed after the opening pattern 13a is formed in the phase shift film 13.
[0021] In EUVL, the opening pattern 13a of the phase shift film 13 is transferred to a target substrate such as a semiconductor substrate. The transfer includes reducing and transferring. The substrate 10, the multilayer reflective film 11, the protective film 12, the phase shift film 13, and the etching mask film 14 will be described below in this order.
[0022] The substrate 10 is, for example, a glass substrate. The material of the substrate 10 is TiO 2 Quartz glass containing SiO is preferred. Quartz glass has a smaller linear expansion coefficient and smaller dimensional change due to temperature change than general soda-lime glass. 2 80% to 95% by mass, TiO 2 It may contain 4% by mass to 17% by mass of TiO 2 When the content is 4% by mass to 17% by mass, the linear expansion coefficient at room temperature is approximately zero, and almost no dimensional change occurs at room temperature. 2 and TiO 2 The material of the substrate 10 may be crystallized glass in which a β-quartz solid solution is precipitated, silicon, a metal, or the like.
[0023] The substrate 10 has a first main surface 10a and a second main surface 10b facing opposite to the first main surface 10a. A multilayer reflective film 11 and the like are formed on the first main surface 10a. The size of the substrate 10 in plan view (viewed in the Z-axis direction) is, for example, 152 mm long and 152 mm wide. The vertical and horizontal dimensions may be 152 mm or more. The first main surface 10a and the second main surface 10b each have, for example, a square quality assurance area in the center. The size of the quality assurance area is, for example, 142 mm long and 142 mm wide. The quality assurance area of the first main surface 10a preferably has a root-mean-square roughness (Rq) of 0.150 nm or less and a flatness of 100 nm or less. In addition, it is preferable that the quality assurance area of the first main surface 10a does not have a defect that causes a phase defect.
[0024] The multilayer reflective film 11 reflects EUV light. The multilayer reflective film 11 is, for example, formed by alternately laminating a high refractive index layer and a low refractive index layer. The material of the high refractive index layer is, for example, silicon (Si), and the material of the low refractive index layer is, for example, molybdenum (Mo), and a Mo / Si multilayer reflective film is used. Note that a Ru / Si multilayer reflective film, a Mo / Be multilayer reflective film, a Mo compound / Si compound multilayer reflective film, a Si / Mo / Ru multilayer reflective film, a Si / Mo / Ru / Mo multilayer reflective film, a Si / Ru / Mo / Ru multilayer reflective film, a MoRu / Si multilayer reflective film, a Si / Ru / Mo multilayer reflective film, etc. can also be used as the multilayer reflective film 11.
[0025] The film thickness of each layer constituting the multilayer reflective film 11 and the number of repeating units of the layer can be appropriately selected according to the material of each layer and the reflectivity with respect to EUV light. When the multilayer reflective film 11 is a Mo / Si multilayer reflective film, in order to achieve a reflectivity of 60% or more with respect to EUV light with an incident angle θ (see Fig. 3) of 6°, a Mo film with a film thickness of 2.3 ± 0.1 nm and a Si film with a film thickness of 4.5 ± 0.1 nm may be laminated so that the number of repeating units is 30 or more and 60 or less. The multilayer reflective film 11 preferably has a reflectivity of 60% or more with respect to EUV light with an incident angle θ of 6°. More preferably, the reflectivity is 65% or more.
[0026] The film formation method of each layer constituting the multilayer reflective film 11 is, for example, a DC sputtering method, a magnetron sputtering method, or an ion beam sputtering method. When forming a Mo / Si multilayer reflective film using the ion beam sputtering method, an example of the film formation conditions for each of the Mo film and the Si film is as follows. <Film formation conditions for Si film> Target: Si target, Sputtering gas: Ar gas, Gas pressure: 0.013 Pa to 0.027 Pa, Ion acceleration voltage: 300 V to 1500 V, Film formation rate: 0.030 nm / sec to 0.300 nm / sec, Film thickness of Si film: 4.5 ± 0.1 nm, <Film formation conditions for Mo film> Target: Mo target, Sputtering gas: Ar gas, Gas pressure: 0.013 Pa to 0.027 Pa, Ion acceleration voltage: 300 V to 1500 V, Film deposition rate: 0.030 nm / sec to 0.300 nm / sec, Thickness of Mo film: 2.3 ± 0.1 nm, <Repeating unit of Si film and Mo film> Number of repeating units: 30 to 60 (preferably 40 to 50).
[0027] The protective film 12 is formed between the multilayer reflective film 11 and the phase shift film 13 and protects the multilayer reflective film 11. The protective film 12 protects the multilayer reflective film 11 from the etching gas that forms the opening pattern 13a (see FIG. 2) in the phase shift film 13. The protective film 12 remains on the multilayer reflective film 11 without being removed even when exposed to the etching gas.
[0028] The etching gas is, for example, a halogen-based gas, an oxygen-based gas, or a mixed gas thereof. Examples of the halogen-based gas include a chlorine-based gas and a fluorine-based gas. Examples of the chlorine-based gas include Cl 2 gas, SiCl 4 gas, CHCl 3 gas, CCl 4 gas, BCl 3 gas or a mixed gas thereof. Examples of the fluorine-based gas include CF 4 gas, CHF 3 gas, SF 6 gas, BF 3 gas, XeF 2 gas or a mixed gas thereof. Examples of the oxygen-based gas include O 2 gas, O 3 gas or a mixed gas thereof.
[0029] The ratio (ER2 / ER1) of the etching rate ER2 of the phase shift film 13 to the etching rate ER1 of the protective film 12 is also called the selectivity (ER2 / ER1). The larger the selectivity (ER2 / ER1), the better the processability of the phase shift film 13. The selectivity (ER2 / ER1) is preferably 5.0 or more, more preferably 10 or more, and further preferably 30 or more. The selectivity (ER2 / ER1) is preferably 200 or less, and more preferably 100 or less.
[0030] The protective film 12 contains at least one element selected from, for example, Ru, Rh, and Si. When the protective film 12 contains Rh, it may contain only Rh, but it is preferable that the protective film 12 contains an Rh compound. The Rh compound may contain, in addition to Rh, at least one element Z1 selected from the group consisting of Ru, Nb, Mo, Ta, Ir, Pd, Zr, Y, and Ti.
[0031] By adding Ru, Nb, Mo, Zr, Y or Ti to Rh, the extinction coefficient can be reduced while suppressing an increase in the refractive index, and the reflectance to EUV light can be improved. Furthermore, by adding Ru, Ta, Ir, Pd or Y to Rh, the durability to etching gas and / or sulfuric acid / hydrogen peroxide can be improved. Sulfuric acid / hydrogen peroxide is used for removing the resist film or cleaning the reflective mask 2, which will be described later.
[0032] The element ratio (Z1:Rh) of Z1 (all Z1) to Rh is preferably 1:99 to 1:1. In this specification, the element ratio means a molar ratio. If the ratio value (Z1 / Rh) is 1 / 99 or more, the reflectance to EUV light is good. If the ratio value (Z1 / Rh) is 1 or less, the durability of the protective film 12 to the etching gas is good. The element ratio (Z1:Rh) of Z1 to Rh is more preferably 3:10 to 1:1.
[0033] The Rh compound may contain, in addition to Rh, at least one element Z2 selected from the group consisting of N, O, C, and B. The element Z2 reduces the durability of the protective film 12 against etching gas, but can suppress crystallization of the protective film 12, allowing the surface of the protective film 12 to be formed smoothly. The Rh compound containing the element Z2 has an amorphous structure or a microcrystalline structure. When the Rh compound has an amorphous structure or a microcrystalline structure, the X-ray diffraction profile of the Rh compound does not have a clear peak.
[0034] When the Rh compound contains Z2 in addition to Rh, the content of Rh or the total content of Rh and Z1 is preferably 40 at% to 99 at% and the total content of Z2 is preferably 1.0 at% to 60 at%. When the Rh compound contains Z2 in addition to Rh, the content of Rh or the total content of Rh and Z1 is more preferably 80 at% to 99 at% and the total content of Z2 is more preferably 1.0 at% to 20 at%.
[0035] The Rh compound contains 90 at % or more of Rh, at least one of Z1 and Z2, and has a concentration of 10.0 g / cm 3 ~14.0g / cm 3 When the protective film 12 has a film density of 11.0 g / cm3, the protective film 12 has an amorphous structure or a microcrystalline structure. 3 ~13.0g / cm 3 The protective film 12 contains 100 at % Rh and has a density of 11.0 g / cm 3 ~12.0g / cm 3 When the film density of the protective film 12 is 0.05 to 0.15, the protective film 12 has an amorphous structure or a microcrystalline structure. The film density of the protective film 12 is measured by X-ray reflectivity.
[0036] In this embodiment, the protective film 12 is a single layer, but may be a multilayer film having a lower layer and an upper layer. The lower layer of the protective film 12 is a layer formed in contact with the uppermost surface of the multilayer reflective film 11. The upper layer of the protective film 12 is in contact with the lowermost surface of the phase shift film 13. By forming the protective film 12 into a multilayer structure, a material having a predetermined excellent function can be used for each layer, so that the protective film 12 as a whole can be multifunctional. When the protective film 12 contains 50 at % or more of Rh as a whole, the protective film 12 may have a layer that does not contain Rh. When the protective film 12 is a multilayer film, the thickness of the protective film 12 described below means the total thickness of the multilayer film.
[0037] The thickness of the protective film 12 is preferably 1.5 nm to 4.0 nm, more preferably 2.0 nm to 3.5 nm. If the thickness of the protective film 12 is 1.5 nm or more, the etching resistance is good. If the thickness of the protective film 12 is 4.0 nm or less, the decrease in reflectance to EUV light can be suppressed.
[0038] The film density of the protective film 12 is preferably 10.0 g / cm 3 More than 14.0g / cm 3 The film density of the protective film 12 is 10.0 g / cm or less. 3 If the film density of the protective film 12 is 14.0 g / cm or more, the etching resistance is good. 3 If it is equal to or less than this, a decrease in reflectance for EUV light can be suppressed.
[0039] The upper surface of the protective film 12, i.e., the surface of the protective film 12 on which the phase shift film 13 is formed, preferably has a root-mean-square roughness (Rq) of 0.300 nm or less, more preferably 0.150 nm or less. If the root-mean-square roughness (Rq) is 0.300 nm or less, the phase shift film 13 and the like can be formed smoothly on the protective film 12. In addition, scattering of EUV light can be suppressed, and the reflectance for EUV light can be improved. The root-mean-square roughness (Rq) is preferably 0.050 nm or more.
[0040] The method for forming the protective film 12 is, for example, a DC sputtering method, a magnetron sputtering method, an ion beam sputtering method, or the like. When forming the Rh film using the DC sputtering method, an example of the film formation conditions is as follows. <Film formation conditions of Rh film> Target: Rh target, Sputtering gas: Ar gas, Gas pressure: 1.0×10 -2 Pa~1.0×10 0 Pa, Output density of target: 1.0 W / cm 2 ~8.5 W / cm 2 , Film formation rate: 0.020 nm / sec~1.000 nm / sec, Film thickness of Rh film: 1 nm~10 nm.
[0041] When forming the Rh film, as the sputtering gas, N 2 gas or a mixed gas of Ar gas and N 2 may be used. The volume ratio of N 2 gas in the sputtering gas (N 2 / (Ar + N 2 )) is 0.05 or more and 1.0 or less.
[0042] When forming the RhO film using the DC sputtering method, an example of the film formation conditions is as follows. <Film formation conditions of RhO film> Target: Rh target, Sputtering gas: O 2 gas or a mixed gas of Ar gas and O 2 is used. Volume ratio of O 2 gas in the sputtering gas (O 2 / (Ar + O 2 )): 0.05~1.0, Gas pressure: 1.0×10 -2 Pa~1.0×10 0 Pa, Output density of target: 1.0 W / cm 2 ~8.5 W / cm 2 , Film formation rate: 0.020 nm / sec to 1.000 nm / sec, Film thickness of RhO film: 1 nm to 10 nm.
[0043] When forming a RhRu film using the DC sputtering method, an example of the film formation conditions is as follows. <Film formation conditions of RhRu film> Targets: Rh target and Ru target (or RhRu target), Sputtering gas: Ar gas, Gas pressure: 1.0×10 -2 Pa to 1.0×10 0 Pa, Output density of the target: 1.0 W / cm 2 ~8.5 W / cm 2 、 Film formation rate: 0.020 nm / sec to 1.000 nm / sec, Film thickness of RhRu film: 1 nm to 10 nm.
[0044] The phase shift film 13 is a film on which the opening pattern 13a is formed. The opening pattern 13a is not formed in the manufacturing process of the reflective mask blank 1, but is formed in the manufacturing process of the reflective mask 2. The phase shift film 13 not only absorbs EUV light but also shifts the phase of the EUV light. The phase shift film shifts the phase of the second EUV light L2 with respect to the first EUV light L1 shown in FIG. 3.
[0045] The first EUV light L1 passes through the opening pattern 13a without passing through the phase shift film 13, is reflected by the multilayer reflective film 11, and then passes through the opening pattern 13a without passing through the phase shift film 13 again. The second EUV light L2 passes through the phase shift film 13 while being absorbed by the phase shift film 13, is reflected by the multilayer reflective film 11, and then passes through the phase shift film 13 while being absorbed by the phase shift film 13 again.
[0046] The phase difference (≧0) between the first EUV light L1 and the second EUV light L2 is, for example, 170° to 250°. The phase of the first EUV light L1 may be ahead of or behind the phase of the second EUV light L2. The phase shift film 13 improves the contrast of the transferred image by utilizing the interference between the first EUV light L1 and the second EUV light L2. The transferred image is an image obtained by transferring the opening pattern 13a of the phase shift film 13 onto the target substrate.
[0047] In EUVL, a so-called projection effect (shadowing effect) occurs. The shadowing effect refers to a region in which the sidewall of the opening pattern 13a blocks the EUV light due to the incident angle θ of the EUV light being not 0° (for example, 6°), resulting in a positional or dimensional shift of the transferred image. In order to reduce the shadowing effect, it is effective to reduce the height of the sidewall of the opening pattern 13a, and it is also effective to thin the phase shift film 13.
[0048] The thickness of the phase shift film 13 is, for example, 60 nm or less, and preferably 50 nm or less, in order to reduce the shadowing effect. The thickness of the phase shift film 13 is preferably 20 nm or more, and more preferably 30 nm or more, in order to ensure a phase difference between the first EUV light L1 and the second EUV light L2.
[0049] In order to reduce the thickness of the phase shift film 13 to reduce the shadowing effect while ensuring the phase difference between the first EUV light L1 and the second EUV light L2, it is effective to reduce the refractive index n of the phase shift film 13. Therefore, the phase shift film 13 of this embodiment is made of an Ir-based material. The Ir-based material is a material whose main component is Ir and contains 50 at % to 100 at % of Ir. In other words, the phase shift film 13 contains 50 at % to 100 at % of Ir.
[0050] Ir-based materials have a small refractive index n and a large extinction coefficient k. Therefore, the phase shift film 13 can be made thinner while maintaining a desired phase difference. The higher the Ir content, the smaller the refractive index n and the larger the extinction coefficient k. The Ir content is preferably 70 at% or more, and more preferably 80 at% or more.
[0051] The refractive index n of the phase shift film 13 is preferably 0.925 or less, more preferably 0.920 or less, even more preferably 0.918 or less, particularly preferably 0.910 or less, and even more particularly preferably 0.900 or less. The smaller the refractive index n of the phase shift film 13, the thinner the phase shift film 13 can be. The refractive index n of the phase shift film 13 is preferably 0.885 or more. In this specification, the refractive index is the refractive index for EUV light (for example, light with a wavelength of 13.5 nm).
[0052] The extinction coefficient k of the phase shift film 13 is preferably 0.030 or more, more preferably 0.034 or more, even more preferably 0.036 or more, and particularly preferably 0.038 or more. The larger the extinction coefficient k of the phase shift film 13, the easier it is to obtain a desired reflectance with a thin film thickness. The extinction coefficient k of the phase shift film 13 is preferably 0.065 or less. In this specification, the extinction coefficient is the extinction coefficient for EUV light (e.g., light with a wavelength of 13.5 nm).
[0053] In the phase shift film 13, the ratio (Ip / Ia) of the maximum peak intensity Ip in the range of 35° to 45° of 2θ to the average intensity (diffraction intensity) Ia in the range of 55° to 60° of 2θ is preferably 30 or less, more preferably 20 or less, and further preferably 10 or less, as measured by XRD using CuKα radiation. As the XRD method, an out of plane method is used. Hereinafter, Ip / Ia is also referred to as a peak intensity ratio. If the peak intensity ratio Ip / Ia is 30 or less, the crystallinity of the phase shift film 13 is low, and the roughness of the sidewall of the opening pattern 13a can be reduced. The smaller the peak intensity ratio Ip / Ia, the more preferable. The smaller Ip / Ia is, the lower the crystallinity is, but Ip / Ia is preferably 1.0 or more, and more preferably 2.0 or more.
[0054] In the phase shift film 13, the full width at half maximum FWHM of the most intense peak in the 2θ range of 35° to 60° is preferably 1.2° or more in an XRD method using CuKα radiation. As the XRD method, an out of plane method is used. The most intense peak in the 2θ range of 35° to 60° appears in the 2θ range of 35° to 45°. If the full width at half maximum FWHM is 1.2° or more, the crystallinity of the phase shift film 13 is low, and the roughness of the sidewall of the opening pattern 13a can be reduced. The full width at half maximum FWHM is preferably 1.5° or more, and more preferably 2.0° or more. The larger the full width at half maximum FWHM, the more preferable it is, and it is preferable that there is no clear peak.
[0055] In addition to Ir, the phase shift film 13 preferably contains at least one first element X1 selected from a first group consisting of O, B, C, and N. The first element X1 is a nonmetallic element. By adding the first element X1 to Ir, it is possible to suppress crystallization while suppressing deterioration of optical properties, and to reduce roughness of the sidewall of the opening pattern 13a.
[0056] The first element X1 preferably contains oxygen, and more preferably contains oxygen and nitrogen. A small amount of oxygen added can suppress the crystallization of the phase shift film 13, and can suppress the deterioration of the optical properties of the phase shift film 13.
[0057] The total content of the first element X1 is preferably 1.0 at% to 49 at%, more preferably 5.0 at% to 30 at%, further preferably 7.0 at% to 30 at%, and particularly preferably 15 at% to 25 at%. When the total content of the first element X1 is 1.0 at% or more, crystallization of the phase shift film 13 can be suppressed. When the total content of the first element X1 is 49 at% or less, the hydrogen resistance described below and the optical properties are good.
[0058] Incidentally, inside the EUV exposure tool, the reflective mask 2 may be exposed to hydrogen gas. Hydrogen gas is used, for example, for the purpose of reducing carbon contamination. Therefore, the phase shift film 13 may be exposed to hydrogen gas. In general, hydrogen gas and the first element X1 form a hydride (for example, H 2 O).
[0059] When the phase shift film 13 contains the first element X1, the 4f of Ir observed by X-ray photoelectron spectroscopy (XPS) is 7 / 2 It is preferable that the chemical shift ΔE1 of the peak is less than 0.3 eV. If ΔE1 is less than 0.3 eV, Ir contained in the phase shift film 13 is hardly bonded to the first element X1.
[0060] If Ir and the first element X1 are not bonded, the bond will not be broken by hydrogen gas, and a hydride of the first element X1 will not be generated. If a hydride of the first element X1 is generated, the hydride is highly volatile, and the first element X1 is desorbed from the phase shift film 13, causing the phase shift film 13 to be reduced. The film thickness after reduction is smaller than the film thickness before reduction. The change in film thickness leads to a change in the phase difference.
[0061] The electron binding energy observed by X-ray photoelectron spectroscopy represents the amount of energy consumed when an electron is ejected. When Ir is bonded to the first element X1, Ir becomes positively charged, so a large amount of energy is consumed for the electron to shake off Ir and be ejected. Therefore, when Ir is bonded to the first element X1, the peak binding energy is higher than when Ir exists alone.
[0062] The chemical shift ΔE1 of the Ir peak observed by X-ray photoelectron spectroscopy is the magnitude (absolute value) of the difference between the binding energy of the Ir peak actually observed and the binding energy of the Ir peak when it is not bound to the first element X1 and exists alone (reference binding energy) (ΔE1≧0.0 eV). The binding energy of the Ir peak actually observed is basically equal to or greater than the reference binding energy. The reference binding energy for each element is taken from literature values such as those listed in HANDBOOK OF X-RAY PHOTOELECTRON SPECTROSCOPY (1979) (authors: D. Wagner, WM Riggs, LE Davis, JF Maulder, GE Muilenberg).
[0063] ΔE1 can be adjusted by, for example, multi-target sputtering using a target containing Ir, a target containing the first element X1, and a target containing the second element X2, or reactive sputtering using a target containing Ir and a target containing the second element X2. By selectively bonding the second element X2 contained in the phase shift film 13 with the first element X1 by multi-target sputtering or reactive sputtering, the bond between Ir and the first element X1 is suppressed, and the bond is also suppressed from being broken by hydrogen gas, so that the generation of hydrides of the first element X1 can be suppressed. Therefore, ΔE1 can be adjusted to less than 0.3 eV. The method of supplying the first element X1 is not particularly limited, but it is preferable to supply it from a gas or a target, and more preferably to supply it as a gas. As the gas, oxygen, nitrogen, or methane is preferably used. When the first element X1 is supplied as a gas, in multi-target sputtering using a target containing Ir and a target containing the second element X2, the gas of the first element X1 is preferably supplied from the vicinity of the target containing the second element X2. By doing so, ΔE2, which will be described later, can be made larger than ΔE1.
[0064] Also, ΔE1 can be adjusted by multi-sputtering of a target containing Ir and a compound target containing the first element X1 and the second element X2. By using a compound target containing the first element X1 and the second element X2, the bond between Ir and the first element X1 is suppressed, and the bond is also suppressed from being broken by hydrogen gas, so that the generation of hydrides of the first element X1 can be suppressed. Therefore, ΔE1 can be adjusted to less than 0.3 eV.
[0065] In the present invention, the analysis of the phase shift film by XPS is carried out as follows. For the analysis by XPS, an analyzer "PHI 5000 VersaProbe" manufactured by ULVAC-PHI, Inc. is used. The above-mentioned apparatus is calibrated in accordance with JIS K0145. First, a measurement sample of about 1 cm square is cut out from a reflective mask blank, and the measurement sample is set in a measurement holder so that the phase shift film becomes the measurement surface. After the measurement holder is loaded into the above-mentioned apparatus, a portion of the phase shift film is removed with an argon ion beam until the peak observed from the outermost surface becomes constant. After removing the surface of the phase shift film, the removed area is irradiated with X-rays (monochromated AlKα rays) and analyzed with a photoelectron take-off angle (the angle between the surface of the measurement sample and the direction of the detector) of 45°. During the analysis, a neutralizing gun is used to suppress charge-up. The analysis involves a wide scan in the binding energy range of 0eV to 1000eV to confirm the elements present, followed by a narrow scan depending on the elements present. Narrow scans are performed with, for example, a pass energy of 58.7eV, an energy step of 0.1eV, a time / step of 50ms, and five accumulations. Wide scans are performed with a pass energy of 58.7eV, an energy step of 1eV, a time / step of 50ms, and two accumulations. Here, the bond energy is calibrated using the peak of the C1s orbital derived from carbon present on the measurement sample. Specifically, first, the bond energy value indicating the peak of the C1s orbital in the measurement sample is obtained from the narrow scan analysis result, and the value obtained by subtracting this bond energy value from 284.8 eV is used as the shift value. The above shift value is added to the bond energy value indicating the peak of each orbital obtained from the narrow scan analysis result, and the bond energy value of the peak corresponding to each orbital defined above is calculated. The bond energy may be calibrated using Au whose surface has been cleaned in ultra-high vacuum. In this case, the shift value is calculated by subtracting Au4f 7 / 2 The binding energy value of the orbital is obtained from the narrow scan analysis results and is calculated by subtracting the binding energy value from 83.96 eV. When reading the binding energy value indicating the peak of each orbital from the narrow scan analysis results, the value indicating the peak top is read as the binding energy value.
[0066] If the chemical shift ΔE1 of the Ir peak observed by X-ray photoelectron spectroscopy is less than 0.3 eV, the Ir contained in the phase shift film 13 is hardly bonded to the first element X1. Therefore, a hydride of the first element X1 is not generated, and the first element X1 is not desorbed from the phase shift film 13. Therefore, the hydrogen resistance of the phase shift film 13 can be improved, and the change in the film thickness of the phase shift film 13 can be suppressed. ΔE1 is preferably less than 0.3 eV, more preferably 0.2 eV or less, and further preferably 0.1 eV or less.
[0067] The phase shift film 13 preferably contains a second element X2, at least one of an oxide, a boride, a carbide, and a nitride, whose standard Gibbs energy of formation is -130 kJ / mol or less. In other words, the phase shift film 13 preferably contains a compound of Ir, X1, and X2. The standard Gibbs energy of formation is the free energy required to synthesize a substance from a certain element, based on a state in which the element is stable as a single element under standard conditions (25°C, 1 atm). The lower the standard Gibbs energy of formation, the more stable the substance.
[0068] If the standard Gibbs energy of formation of the oxide, boride, carbide or nitride, which is a compound of the second element X2 and the first element X1, is -130 kJ / mol or less, the stability of the compound is sufficiently high, the second element X2 and the first element X1 are strongly bonded, and the bond is not broken by hydrogen gas. Therefore, the generation of a hydride of the first element X1 can be suppressed, and the first element X1 can be suppressed from being detached from the phase shift film 13. Therefore, the hydrogen resistance of the phase shift film 13 can be improved. The above standard Gibbs energy of formation is more preferably -500 kJ / mol or less.
[0069] The second element X2 is at least one selected from a second group consisting of Ta, Cr, Mo, W, Re, and Si. The standard Gibbs energy of formation of the second group elements is −500 kJ / mol or less. Therefore, Ta, Cr, Mo, W, Re, and Si can all suppress the generation of hydrides of the first element X1 and suppress the first element X1 from being desorbed from the phase shift film 13. In addition, Ta, Cr, Mo, W, Re, and Si can all improve the selectivity (ER2 / ER1). Furthermore, among the elements of the second group, Ta, Cr, W, and Re can improve the hydrogen resistance of the phase shift film 13 while suppressing the deterioration of the optical properties of the phase shift film 13. Furthermore, among the elements of the second group, Mo and Si can further improve the hydrogen resistance of the phase shift film 13.
[0070] In the phase shift film 13, the chemical shift ΔE2 of the peak of the second element X2 observed by X-ray photoelectron spectroscopy is preferably larger than the chemical shift ΔE1 of the peak of Ir. 7 / 2 peak or Cr 2p 3 / 2 peak or Mo 3d 5 / 2 or the Si 2p peak 3 / 2 This is the peak.
[0071] The binding energy of electrons observed by X-ray photoelectron spectroscopy represents the amount of energy consumed when an electron is ejected. When the second element X2 is bonded to the first element X1, the second element X2 becomes positively charged, so a large amount of energy is consumed for the electron to shake off the second element X2 and be ejected. Therefore, when the second element X2 is bonded to the first element X1, the peak binding energy becomes higher than when the second element X2 exists alone.
[0072] The chemical shift ΔE2 of the peak of the second element X2 observed by X-ray photoelectron spectroscopy is the magnitude (absolute value) of the difference between the binding energy of the peak of the second element X2 actually observed and the binding energy of the peak of the second element X2 when it exists alone without being bound to the first element X1 (reference binding energy). The binding energy of the peak of the second element X2 actually observed is basically higher than the reference binding energy.
[0073] The chemical shift ΔE2 of the peak of the second element X2 is preferably larger than the chemical shift ΔE1 of the peak of Ir. The second element X2 bonds more strongly with the first element X1 than Ir (the bond between X2 and X1 is stronger than the bond between Ir and X1), and the bond (the bond between X2 and X1) is not broken by hydrogen gas. Therefore, the generation of hydrides of the first element X1 can be suppressed, and the first element X1 can be suppressed from being desorbed from the phase shift film 13. Therefore, the hydrogen resistance of the phase shift film 13 can be improved.
[0074] The chemical shift ΔE2 of the peak of the second element X2 observed by X-ray photoelectron spectroscopy is preferably 0.2 eV or more, more preferably 0.3 eV or more, even more preferably 0.5 eV or more, still more preferably 2.0 eV or more, and particularly preferably 2.5 eV or more. The larger ΔE2 is, the more preferable, but it may be 5.0 eV or less.
[0075] The phase shift film 13 preferably contains 50 at% to 98 at% Ir, 1.0 at% to 49 at% of the first element X1 in total, and 1.0 at% to 49 at% of the second element X2 in total. When the contents of Ir, the first element X1, and the second element X2 are within the above ranges, crystallization of the phase shift film 13 is suppressed, and the hydrogen resistance of the phase shift film 13 is effectively improved.
[0076] More preferably, the phase shift film 13 contains 60 at% to 89 at% Ir, 1.0 at% to 10 at% of the first element X1 in total, and 10 at% to 30 at% of the second element X2 in total, or 60 at% to 85 at% Ir, 10 at% to 30 at% of the first element X1 in total, and 5.0 at% to 20 at% of the second element X2 in total. If the contents of Ir, the first element X1, and the second element X2 are within the above ranges, crystallization of the phase shift film 13 is suppressed, and the hydrogen resistance of the phase shift film 13 is improved, resulting in a high level of optical properties.
[0077] Preferably, the phase shift film 13 has a total content of the first element X1 of 1.0 at% to 45 at% or a total content of the second element X2 of 5.0 at% to 49 at%. If the phase shift film 13 has a total content of the first element X1 greater than 45 at% and a total content of the second element X2 less than 5.0 at%, then iridium oxide that is unstable to hydrogen is generated, and the hydrogen resistance of the reflective mask blank 1 deteriorates.
[0078] When the second element X2 of the phase shift film 13 is Ta, the ratio (Ir / Ta) of the Ir content (at%) to the Ta content (at%) is, for example, 1 to 190. When the ratio (Ir / Ta) of the Ir content to the Ta content is 1 or more, the optical properties of the phase shift film 13 are good. When the ratio (Ir / Ta) of the Ir content to the Ta content is 190 or less, the processability of the phase shift film 13 is good. The ratio (Ir / Ta) of the Ir content to the Ta content is preferably 1 to 100, more preferably 1 to 40, further preferably 2 to 30, particularly preferably 2 to 20, and most preferably 2 to 12.
[0079] When the second element X2 of the phase shift film 13 is Cr, the ratio (Ir / Cr) of the Ir content (at%) to the Cr content (at%) is, for example, 1 to 105. When the ratio (Ir / Cr) of the Ir content to the Cr content is 1 or more, the optical properties of the phase shift film 13 are good. When the ratio (Ir / Cr) of the Ir content to the Cr content is 105 or less, the selectivity (ER2 / ER1) is large and the processability of the phase shift film 13 is good. The ratio (Ir / Cr) of the Ir content to the Cr content is preferably 1 to 105, more preferably 2 to 105, further preferably 3 to 105, and particularly preferably 4 to 105.
[0080] When the second element X2 of the phase shift film 13 is W, the ratio (Ir / W) of the Ir content (at%) to the W content (at%) is, for example, 1 to 100. When the ratio (Ir / W) of the Ir content to the W content is 1 or more, the optical properties of the phase shift film 13 are good. When the ratio (Ir / W) of the Ir content to the W content is 100 or less, the selectivity (ER2 / ER1) is large and the processability of the phase shift film 13 is good. The ratio (Ir / W) of the Ir content to the W content is preferably 1 to 90, more preferably 2 to 80, further preferably 3 to 70, and particularly preferably 4 to 30.
[0081] The etching rate of phase shift film 13 by sulfuric acid / hydrogen peroxide is 0 nm / min to 0.05 nm / min. Sulfuric acid / hydrogen peroxide is used for removing a resist film, which will be described later, or for cleaning reflective mask 2. If the etching rate of phase shift film 13 by sulfuric acid / hydrogen peroxide is 0.05 nm / min or less, damage to phase shift film 13 during cleaning can be suppressed.
[0082] The phase shift film 13 preferably contains N as the first element X1 in addition to at least one element selected from O, C, and B. By adding N to at least one element selected from O, C, and B, crystallization can be suppressed. The total content of O, C, and B is preferably 15 at% or less. The N content is preferably 10 at% or less. The smaller the total content of the first element X1, the higher the density and the better the optical properties.
[0083] The phase shift film 13 preferably contains 1.0 at% to 10 at% of N as the first element X1. If the N content is 1.0 at% or more, crystallization can be suppressed even if the O content is small. From the viewpoint of optical properties, the N content is preferably 10 at% or less, and more preferably 5.0 at% or less.
[0084] The phase shift film 13 preferably contains 1.0 at % to 15 at % of O as the first element X1. If the O content is 1.0 at % or more, crystallization can be suppressed. From the viewpoints of optical properties and patterning properties, the O content is preferably 15 at % or less. If the O content exceeds 15 at %, the density decreases and the optical properties deteriorate. Furthermore, if the O content exceeds 15 at %, large dispersed particles are generated, and the patterning properties deteriorate.
[0085] When the first element X1 of the phase shift film 13 contains O, the ratio (Ir / O) of the Ir content (at%) to the O content (at%) is, for example, 1 to 40. When the ratio (Ir / O) of the Ir content to the O content is 1 or more, the hydrogen resistance of the phase shift film 13 can be improved. When the ratio (Ir / O) of the Ir content to the O content is 40 or less, the crystallization of the phase shift film 13 can be suppressed, and the roughness of the sidewall of the opening pattern 13a can be reduced. The ratio (Ir / O) of the Ir content to the O content is preferably 1 to 40, more preferably 2 to 35, further preferably 2 to 30, particularly preferably 2 to 20, and most preferably 3 to 15.
[0086] When the first element X1 of the phase shift film 13 contains N, the ratio (Ir / N) of the Ir content (at%) to the N content (at%) is, for example, 10 to 105. If the ratio (Ir / N) of the Ir content to the N content is 10 or more, the hydrogen resistance of the phase shift film 13 can be improved. If the ratio (Ir / N) of the Ir content to the N content is 105 or less, the crystallization of the phase shift film 13 can be suppressed, and the sidewall roughness of the opening pattern 13a can be reduced. The ratio (Ir / N) of the Ir content to the N content is preferably 10 to 105, more preferably 10 to 70, even more preferably 10 to 45, particularly preferably 11 to 36, and most preferably 12 to 30.
[0087] In the phase shift film 13, when the first element X1 contains O and N, the ratio (Ir / (O+N)) of the Ir content (at%) to the total of the O content (at%) and the N content (at%) is, for example, 1 to 45. If the ratio (Ir / (O+N)) of the Ir content to the total of the O content and the N content is 1 or more, the hydrogen resistance of the phase shift film 13 can be improved. If the ratio (Ir / (O+N)) of the Ir content to the total of the O content and the N content is 45 or less, the crystallization of the phase shift film 13 can be suppressed, and the sidewall roughness of the opening pattern 13a can be reduced. The ratio (Ir / (O+N)) of the Ir content to the total of the O content and the N content is preferably 1 to 45, more preferably 2 to 30, further preferably 2.5 to 20, particularly preferably 4 to 17, and most preferably 6 to 16.
[0088] 11, the dispersed particles 131 are particles dispersed in a matrix 132. The dispersed particles 131 are rich in a first element X1 and a second element X2, and the matrix 132 is rich in Ir. The larger the dispersed particles 131, the greater the roughness of the sidewalls of the opening pattern 13a, and the worse the patterning properties. This is because etching tends to proceed along the interface between the dispersed particles 131 and the matrix 132 when the opening pattern 13a is formed.
[0089] The size of the dispersed particles 131 can be evaluated from the grayscale image. The dispersed particles 131 have a lower density because they are richer in the first element X1 and the second element X2 than the matrix 132. Therefore, in the grayscale image, the dispersed particles 131 appear darker than the matrix 132.
[0090] The grayscale image is obtained by imaging a cross section of the phase shift film 13 with a scanning transmission electron microscope (STEM). The grayscale image has, for example, 256 levels of gray scale, a magnification of 2.5 million times, and a resolution of 0.10 nm / pixel.
[0091] The size of the dispersed particle 131 can be evaluated from the brightness profile of the grayscale image. The region for creating the brightness profile has, for example, a vertical dimension of 25 nm and a horizontal dimension of 60 nm. Here, the vertical direction is the Z-axis direction. The horizontal direction is the X-axis direction or the Y-axis direction.
[0092] The intensity profile is created using SurfCharJ, a plug-in tool for ImageJ (version 1.53e) distributed by the National Institutes of Health (NIH). ImageJ is an open source, public domain image processing software. By using SurfCharJ, the roughness parameters of the intensity profile of the image, specifically the skewness (Rsk), can be obtained.
[0093] The skewness (Rsk) in the luminance profile is preferably negative. If Rsk is negative, there are many fine valleys when the average line is the center, the size of the dispersed particles 131 is small, and the structure of the phase shift film 13 is uniform. Therefore, if Rsk is negative, the patterning property is good. Rsk is more preferably -0.01 or less. Rsk is calculated in accordance with JIS B0601:2013.
[0094] The method for forming the phase shift film 13 is, for example, the DC sputtering method, the magnetron sputtering method, or the ion beam sputtering method, etc. The O 2 content in the sputtering gas can control the oxygen content of the phase shift film 13. Also, the N 2 content in the sputtering gas can control the nitrogen content of the phase shift film 13.
[0095] When forming the IrTaON film using the reactive sputtering method, an example of the film formation conditions is as follows. <Film formation conditions of IrTaON film> Targets: Ir target and Ta target (or IrTa target), Output density of Ir target: 1.0 W / cm 2 ~8.5 W / cm 2 , Output density of Ta target: 1.0 W / cm 2 ~8.5 W / cm 2 , Sputtering gas: Mixed gas of Ar gas, O 2 gas and N 2 gas, Volume ratio of O 2 gas in the sputtering gas (O 2 / (Ar + O 2 + N 2 )): 0.01 to 0.25, Volume ratio of N 2 gas in the sputtering gas (N 2 / (Ar + O 2 + N 2 )): 0.01 to 0.25, Film formation rate: 0.020 nm / sec to 0.060 nm / sec, Film thickness: 20 nm to 60 nm.
[0096] In this embodiment, the phase shift film 13 is a single layer, but may be a multi-layer film. The phase shift film 13 may have a layer that does not contain Ir. The phase shift film 13 as a whole only needs to contain 50 at % or more of Ir. When the phase shift film 13 includes a first layer and a second layer, the refractive index n of the phase shift film 13 is calculated from the following formula (1).
[0097]
number
[0098] When the phase shift film 13 includes a first layer and a second layer, the extinction coefficient k of the phase shift film 13 is calculated from the following formula (2).
[0099]
number
[0100] In addition to the first and second layers, the phase shift film 13 may include a third layer having a chemical composition different from those of the first and second layers. Even when the third layer is included, the refractive index n and the extinction coefficient k can be calculated using the same formulas as the above formulas (1) and (2).
[0101] The etching mask film 14 is formed on the opposite side of the protective film 12 with respect to the phase shift film 13, and is used to form an opening pattern 13a in the phase shift film 13. A resist film (not shown) is provided on the etching mask film 14. In the manufacturing process of the reflective mask 2, a first opening pattern is first formed in the resist film, then a second opening pattern is formed in the etching mask film 14 using the first opening pattern, and then a third opening pattern 13a is formed in the phase shift film 13 using the second opening pattern. The first opening pattern, the second opening pattern, and the third opening pattern 13a have the same dimensions and the same shape in a plan view (Z-axis direction view). The etching mask film 14 enables the resist film to be made thinner.
[0102] The etching mask film 14 preferably contains at least one element selected from Al, Hf, Y, Cr, Nb, Ti, Mo, Ta, and Si. The etching mask film 14 may further contain at least one element selected from O, N, and B.
[0103] The thickness of the etching mask film 14 is preferably 2 nm or more and 30 nm or less, more preferably 2 nm or more and 25 nm or less, and further preferably 2 nm or more and 10 nm or less.
[0104] The etching mask film 14 may be formed by, for example, DC sputtering, magnetron sputtering, or ion beam sputtering.
[0105] Next, a method for manufacturing a reflective mask blank 1 according to one embodiment will be described with reference to Fig. 4. The method for manufacturing the reflective mask blank 1 includes, for example, steps S101 to S105 shown in Fig. 4. In step S101, a substrate 10 is prepared. In step S102, a multilayer reflective film 11 is formed on a first main surface 10a of the substrate 10. In step S103, a protective film 12 is formed on the multilayer reflective film 11. In step S104, a phase shift film 13 is formed on the protective film 12. In step S105, an etching mask film 14 is formed on the phase shift film 13.
[0106] The method for manufacturing the reflective mask blank 1 only needs to include at least steps S101 to S104. The method for manufacturing the reflective mask blank 1 may further include a step of forming a functional film not shown in FIG.
[0107] Next, a method for manufacturing a reflective mask 2 according to an embodiment will be described with reference to FIG. 5. The method for manufacturing a reflective mask 2 includes steps S201 to S204 shown in FIG. 5. In step S201, a reflective mask blank 1 is prepared. In step S202, an etching mask film 14 is processed. A resist film (not shown) is provided on the etching mask film 14. First, a first opening pattern is formed in the resist film, and then a second opening pattern is formed in the etching mask film 14 using the first opening pattern. In step S203, a third opening pattern 13a is formed in the phase shift film 13 using the second opening pattern. In step S203, the phase shift film 13 is etched using an etching gas. In step S204, the resist film and the etching mask film 14 are removed. For example, sulfuric acid / hydrogen peroxide is used to remove the resist film. For example, an etching gas is used to remove the etching mask film 14. The etching gas used in step S204 (removing the etching mask film 14) may be the same as the etching gas used in step S203 (etching the phase shift film 13). The method for manufacturing the reflective mask 2 only needs to include at least steps S201 and S203. EXAMPLES
[0108] The experimental data will be explained below.
[0109] <Examples 1 to 12, 19 and 20> In Examples 1 to 12, 19, and 20, EUVL reflective mask blanks were produced under the same conditions except for the type of phase shift film and its deposition conditions. Each reflective mask blank was composed of a substrate, a multilayer reflective film, a protective film, and a phase shift film. Example 1 is a comparative example, and Examples 2 to 12, 19, and 20 are working examples.
[0110] The substrate is SiO 2 -TiO 2 A glass substrate (6-inch (152 mm) square, 6.3 mm thick) was prepared. The thermal expansion coefficient of this glass substrate at 20° C. was 0.02×10 -7 / °C, Young's modulus is 67 GPa, Poisson's ratio is 0.17, and specific stiffness is 3.07 × 10 7 m 2 / s 2 The quality assurance area of the first main surface of the substrate was polished to a root-mean-square roughness (Rq) of 0.15 nm or less and a flatness of 100 nm or less. A 100 nm-thick Cr film was formed on the second main surface of the substrate by magnetron sputtering. The sheet resistance of the Cr film was 100 Ω / □.
[0111] The multilayer reflective film was a Mo / Si multilayer reflective film. The Mo / Si multilayer reflective film was formed by repeating the deposition of a Si layer (thickness 4.5 nm) and a Mo layer (thickness 2.3 nm) 40 times using the ion beam sputtering method. The total thickness of the Mo / Si multilayer reflective film was 272 nm ((4.5 nm + 2.3 nm) x 40).
[0112] As a protective film, a Rh film (thickness: 2.5 nm) was formed by using a DC sputtering method.
[0113] As the phase shift film, an Ir film, an IrTaON film, or an IrCrON film was formed. In Example 1, an Ir film was formed by using a DC sputtering method. In Examples 2 to 4, 6 to 9, 11, and 12, an IrTaON film was formed by using a reactive sputtering method. In Examples 5 and 10, an IrCrON film was formed by using a reactive sputtering method.
[0114] Table 1 shows the film types and characteristics of the phase shift films obtained in Examples 1 to 12, 19 and 20.
[0115] [Table 1] The composition of the phase shift film was measured using an X-ray photoelectron spectrometer (PHI 5000 manufactured by ULVAC-PHI) The composition of the phase shift film shown in Table 1 was measured before the phase shift film was exposed to hydrogen gas.
[0116] The optical properties of the phase shift film (refractive index n and extinction coefficient k) were taken from the database of the Center for X-Ray Optics, Lawrence Berkeley National Laboratory, or values calculated from the "incident angle dependence" of reflectance described below.
[0117] The incident angle θ of the EUV light, the reflectance R for the EUV light, the refractive index n of the phase shift film, and the extinction coefficient k of the phase shift film satisfy the following formula (3). R = |(sinθ-((n+ik) 2 -cos 2 θ) 1 / 2 ) / (sinθ+((n+ik) 2 -cos 2 θ) 1 / 2 )|···(3) Multiple combinations of the incident angle θ and the reflectance R were measured, and the refractive index n and the extinction coefficient k were calculated by the least squares method so that the error between the multiple measurement data and equation (3) was minimized.
[0118] The crystallinity (full width at half maximum and crystallite size) of the phase shift film was measured using an X-ray diffraction analyzer (MiniFlexII) manufactured by Rigaku Corporation. The X-ray diffraction spectra of the phase shift film are shown in Figures 7 to 10. The FWHM shown in Table 1 is the full width at half maximum of the peak with the highest intensity in the 2θ range of 35° to 60°. The crystallite size was calculated from the FWHM and other data using Scherrer's equation.
[0119] The peak intensity ratio Ip / Ia was calculated by determining the average intensity Ia when 2θ is in the range of 55° to 60° and the maximum peak intensity Ip when 2θ is in the range of 35° to 45°, and dividing Ip by Ia.
[0120] The density of the phase shift film was measured by X-ray reflectometry (XRR).
[0121] As shown in Figs. 7 to 10 and Table 1, in Examples 2 to 12, 19 and 20, unlike Example 1, the phase shift film contains at least one first element X1 selected from a first group consisting of O, B, C and N in addition to Ir. As a result, in Examples 2 to 12, 19 and 20, the peak intensity ratio Ip / Ia is 30 or less, and the crystallinity is lower than that of Example 1. The lower the crystallinity, the smaller the roughness of the sidewall of the opening pattern 13a can be. Also, from Fig. 6 and Table 1, it can be seen that by adding the first element X1 to Ir, crystallization can be suppressed while suppressing deterioration of optical properties.
[0122] Furthermore, in Examples 2 to 10 and 19, unlike Example 1, the full width at half maximum FWHM was 1.2° or more and the crystallite size was smaller than that of Example 1. The smaller the crystallite size, the lower the crystallinity, and the smaller the roughness of the sidewall of the opening pattern 13a can be.
[0123] In FIG. 6, IrNb has an Ir content of 50 at%, an Nb content of 50 at%, a refractive index n of 0.919, and an extinction coefficient k of 0.025. In FIG. 6, IrY has an Ir content of 50 at%, an Y content of 50 at%, a refractive index n of 0.931, and an extinction coefficient k of 0.024. In FIG. 6, IrZr has an Ir content of 50 at%, an Zr content of 50 at%, a refractive index n of 0.939, and an extinction coefficient k of 0.023. Although Ir may be able to suppress the crystallization of Ir by alloying it with Nb, Zr, or Y, the optical properties (refractive index n and extinction coefficient k) of the phase shift film 13 are degraded.
[0124] <Example 13 to Example 18> In Examples 13 to 18, reflective mask blanks for EUVL including a substrate, a multilayer reflective film, a protective film, and a phase shift film were produced under the same conditions as in Examples 2 to 12, except for the type of film of the phase shift film and its film formation conditions. Examples 13 to 18 are working examples.
[0125] Table 2 shows the film types and characteristics of the phase shift films obtained in Examples 13 to 18.
[0126] [Table 2] The composition and optical properties of the phase shift film were measured in the same manner as in Table 1. In Table 2, the contents in parentheses are values measured after hydrogen exposure. Hydrogen exposure was performed by cutting the test sample into 2.5 cm square test pieces, attaching them to Si dummy substrates, setting them in a hydrogen irradiation test apparatus, and irradiating them with hydrogen (including hydrogen ions).
[0127] The chemical shifts ΔE1 and ΔE2 of the phase shift film were measured using an X-ray photoelectron spectrometer (PHI 5000 VersaProbe) manufactured by ULVAC-PHI. ΔE1 is the 4f 7 / 2 ΔE2 is the chemical shift of the peak of Ta 4f 7 / 2 peak or Cr 2p 3 / 2 is the chemical shift of the peak.
[0128] As shown in Table 2, in Examples 13 to 15, unlike Examples 16 to 17, the total content of the second elements X2 (Ta and Cr) of the phase shift film was 1.0 at% or more before hydrogen exposure. As a result, the desorption of O from the phase shift film could be suppressed. It is considered that this is because O is strongly bonded to Ta and the bond is not broken by hydrogen exposure.
[0129] <Analysis results of STEM images>
[0130] In Examples 3, 6, 9, 11, 12, and 19, a grayscale image was obtained by imaging the cross-section of the obtained phase shift film with STEM, and a luminance profile of the grayscale image was created. Table 3 shows the analysis results of the luminance profile and the composition.
[0131]
Table 3
[0132] A line-and-space pattern was created for the fabricated EUVL reflective mask blanks of Examples 1 and 6, and then an etching test was carried out under the following conditions. The etching test was performed using an inductively coupled plasma (ICP) etching apparatus. As the etching gas, a mixed gas of CF 4 gas and O 2 gas was used. The specific conditions for inductively coupled plasma etching were as follows. ICP antenna bias: 1200 W, Substrate bias: 50 W, Etching pressure: 2.0×10-1 Pa, Etching gas: CF 4 Gas and O 2 Gas mixtures, CF 4 Gas flow rate: 28sccm, O 2 Gas flow rate: 7sccm, Etching time: 285 seconds.
[0133] After the etching test, a SEM image of the surface of the EUVL reflective mask blank was obtained, and the LER (Line Edge Roughness) was calculated. The results are shown in Table 4.
[0134] [Table 4]
[0135] As shown in Table 4, Example 1, which has a large Ip / Ia value and high crystallinity, had a large LER value and poor pattern roughness compared to Example 6, which has a small Ip / Ia value and low crystallinity.
[0136] The reflective mask blank, the reflective mask, the manufacturing method of the reflective mask blank, and the manufacturing method of the reflective mask according to the present disclosure have been described above, but the present disclosure is not limited to the above-mentioned embodiments. Various changes, modifications, substitutions, additions, deletions, and combinations are possible within the scope of the claims. These naturally fall within the technical scope of the present disclosure.
[0137] This application claims priority based on Patent Application No. 2022-108642 filed with the Japan Patent Office on July 5, 2022, and Patent Application No. 2022-179622 filed with the Japan Patent Office on November 9, 2022, and the entire contents of Patent Application No. 2022-108642 and Patent Application No. 2022-179622 are incorporated by reference into this application. [Explanation of symbols]
[0138] 1 Reflective mask blank 2 Reflective mask 10 Substrate 11 Multilayer reflective film 12 Protective film 13 Phase shift film
Claims
1. A reflective mask blank having, in this order, a substrate, a multilayer reflective film that reflects EUV light, a protective film that protects the multilayer reflective film, and a phase shift film that shifts the phase of the EUV light, The phase shift film is mainly made of Ir, and has a ratio (Ip / Ia) of a maximum peak intensity Ip at 2θ of 35° to 45° to an average intensity Ia at 2θ of 55° to 60°, which is measured by an XRD method using CuKα radiation, of 1.0 to 30, a refractive index n for the EUV light of 0.925 or less, and an extinction coefficient k for the EUV light of 0.030 or more, The phase shift film contains Ir at 50 at % or more, O and N, and at least one second element X2 selected from a second group consisting of Ta, Cr, Mo, W, Re and Si; a reflective mask blank, wherein a grayscale image of the phase shift film is obtained by imaging a cross section of the phase shift film with a scanning transmission electron microscope (STEM), and a luminance profile of the grayscale image is created, the skewness (Rsk) in the luminance profile being negative.
2. The phase shift film has a 4f Ir phase as observed by X-ray photoelectron spectroscopy. 7/2 The chemical shift of the peak of the second element X2 observed by X-ray photoelectron spectroscopy is less than 0.3 eV, and the chemical shift of the peak of the second element X2 observed by X-ray photoelectron spectroscopy is less than 4f 7/2 The reflective mask blank according to claim 1 , wherein the chemical shift of the peak is greater than that of the peak of
3. 2. The reflective mask blank according to claim 1, wherein the phase shift film contains 50 at% to 98 at% of Ir, 1.0 at% to 49 at% in total of O and N, and 1.0 at% to 49 at% in total of the second element X2.
4. 4. The reflective mask blank according to claim 3, wherein the phase shift film contains 60 at% to 89 at% Ir, 1.0 at% to 10 at% in total of O and N, and 10 at% to 30 at% of the second element X2, or 60 at% to 85 at% Ir, 10 at% to 30 at% in total of O and N, and 5.0 at% to 20 at% of the second element X2.
5. 4. The reflective mask blank according to claim 3, wherein the phase shift film has a total content of O and N of 1.0 at % to 45 at %, or a total content of the second element X2 of 5.0 at % to 49 at %.
6. 4. The reflective mask blank according to claim 3, wherein in the phase shift film, when the second element X2 is Ta, a ratio (Ir / Ta) of the Ir content (at %) to the Ta content (at %) is 1 to 190.
7. 4. The reflective mask blank according to claim 3, wherein in the phase shift film, when the second element X2 is Cr, a ratio (Ir / Cr) of the Ir content (at %) to the Cr content (at %) is 1 to 105.
8. 2. The reflective mask blank according to claim 1, wherein the phase shift film has a ratio (Ir / N) of the Ir content (at %) to the N content (at %) of 10 to 70.
9. 2. The reflective mask blank according to claim 1, wherein the phase shift film has a ratio (Ir / (O+N)) of the Ir content (at %) to the sum of the O content (at %) and the N content (at %) of 4 to 17.
10. 2. The reflective mask blank according to claim 1, wherein the phase shift film has an extinction coefficient k for the EUV light of 0.034 or more.
11. 2. The reflective mask blank according to claim 1, wherein the phase shift film has a full width at half maximum of the most intense peak in the 2θ range of 35° to 60° of 1.2° or more when measured by XRD using CuKα radiation.
12. 2. The reflective mask blank according to claim 1, wherein the phase shift film has a thickness of 20 nm to 60 nm.
13. The reflective mask blank according to claim 1 , wherein the protective film contains at least one element selected from the group consisting of Ru, Rh and Si.
14. an etching mask film is provided on the opposite side of the protective film with respect to the phase shift film; 2. The reflective mask blank according to claim 1, wherein the etching mask film contains at least one element selected from Al, Hf, Y, Cr, Nb, Ti, Mo, Ta and Si.
15. The reflective mask blank according to claim 14 , wherein the etching mask film further contains at least one element selected from O, N, and B.
16. 2. The reflective mask blank according to claim 1, wherein the phase shift film has a refractive index n of 0.918 or less for the EUV light.
17. A reflective mask blank according to any one of claims 1 to 16, A reflective mask including an opening pattern in the phase shift film.
Citation Information
Patent Citations
Reflection type mask blank, reflection type mask, and manufacturing method for semiconductor device
JP2018146945A
Reflection type mask blank, reflection type mask, substrate with conductive film, and method for manufacturing semiconductor device
JP2021128247A
Reflective mask blank for EUV lithography, reflective mask for EUV lithography and their manufacturing method
JP2022024617A
Reflective mask blank, reflective mask, reflective mask manufacturing method, and semiconductor device manufacturing method
WO2022138170A1
Reflective mask blank, reflective mask, and method for manufacturing semiconductor device