Non-aqueous electrolyte, semi-solid electrolyte layer, sheet for secondary battery, and secondary battery
A non-aqueous electrolyte with sulfolane derivatives and low-viscosity organic solvents addresses the discharge capacity retention issue at high temperatures in lithium ion secondary batteries, enhancing their performance and stability.
Patent Information
- Application Number
- JP2020082631
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-05-08
- Publication Date
- 2024-09-18
- Estimated Expiration
- 2040-05-08
AI Technical Summary
The electrolytic solution in lithium ion secondary batteries fails to maintain a high discharge capacity retention rate when operated at relatively high temperatures, necessitating improvements.
A non-aqueous electrolyte containing specific solvents and electrolyte salts, including sulfolane derivatives and low-viscosity organic solvents, with a concentration range of 1.06 mol/L to 3.46 mol/L and a dielectric constant of 63 or less, is used to enhance discharge capacity retention at elevated temperatures.
The non-aqueous electrolyte maintains a high discharge capacity retention rate of secondary batteries even at high temperatures, improving their performance and stability.
Smart Images

Figure 0007553044000003 
Figure 0007553044000005 
Figure 0007553044000004
Abstract
Description
[Technical field]
[0001] The present invention relates to a non-aqueous electrolyte, a semi-solid electrolyte layer, a sheet for a secondary battery, and a secondary battery. [Background technology]
[0002] As a conventional technique relating to non-aqueous electrolytes used in various secondary batteries, Patent Document 1 discloses a liquid or gel-like non-aqueous electrolyte that contains a non-aqueous solvent, an electrolyte salt, and an overcharge controller that causes an oxidation-reduction reaction at a predetermined potential, as well as at least one of a thermally stable salt that has high thermal stability and remains stably in the non-aqueous electrolyte, a protective film-forming agent that forms a protective film on the positive electrode and the negative electrode to suppress decomposition of the overcharge controller, or a complex-forming agent that forms a complex with a transition metal. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2012-256502 A Summary of the Invention [Problem to be solved by the invention]
[0004] The electrolyte in the lithium ion secondary battery of Patent Document 1 is insufficient for maintaining a high discharge capacity retention rate of the secondary battery when the secondary battery is operated at a relatively high temperature, and there is still room for improvement.
[0005] The present invention aims to provide a non-aqueous electrolyte solution that can maintain a high discharge capacity retention rate of a secondary battery even when the secondary battery is operated at a relatively high temperature, and also aims to provide a semi-solid electrolyte layer, a sheet for a secondary battery, and a secondary battery that use the non-aqueous electrolyte solution. [Means for solving the problem]
[0006] In order to achieve the above object, the nonaqueous electrolyte solution of the present invention comprises an electrolyte salt and an organic solvent, the organic solvent comprising at least one main solvent selected from the group consisting of sulfolane and its derivatives, and a low-viscosity organic solvent, the concentration of the electrolyte salt relative to the main solvent being 1.06 mol / L to 3.46 mol / L, and the relative dielectric constant of the organic solvent being 63 or less. Effect of the Invention
[0007] The nonaqueous electrolyte of the present invention provides a nonaqueous electrolyte that can maintain a high discharge capacity retention rate of a secondary battery even when the secondary battery is operated at a relatively high temperature. Other objects, configurations, and effects will become apparent from the following description of the embodiments. [Brief description of the drawings]
[0008] [Figure 1] 1 is a cross-sectional view showing an embodiment of a secondary battery of the present invention. [Diagram 2] 1 is a graph showing the relationship between the lithium salt concentration (mol / L) in a main solvent and the discharge capacity retention rate (%) at 45° C. in Examples and Comparative Examples. [Diagram 3] 1 is a graph showing the relationship between the relative dielectric constant of organic solvents (mixed solvents) and the discharge capacity retention rate (%) at 45° C. in Examples and Comparative Examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] Hereinafter, an embodiment of the present invention will be described with reference to the drawings. The following description shows a specific example of the contents of the present invention, and the present invention is not limited to these descriptions. Various changes and modifications are possible by those skilled in the art within the scope of the technical ideas disclosed in this specification. In addition, in all the drawings for explaining the present invention, parts having the same functions are given the same reference numerals, and repeated explanations thereof may be omitted.
[0010] In this specification, the symbol "~" is used to mean that the numerical values before and after it are the upper and lower limits. When the upper or lower limit is 0, the upper or lower limit is not included. In the numerical ranges described in stages in this specification, the upper or lower limit described in one numerical range may be replaced with the upper or lower limit described in another stage. The upper or lower limit of the numerical ranges described in this specification may be replaced with the values shown in the examples.
[0011] As an embodiment of the secondary battery according to the present invention, a lithium ion secondary battery will be described below as an example. A lithium ion secondary battery is an electrochemical device that stores or utilizes electrical energy by absorbing and releasing lithium ions into and from an electrode in an electrolyte. Lithium ion secondary batteries are also called lithium ion batteries, nonaqueous electrolyte secondary batteries, nonaqueous electrolyte secondary batteries, and the like, and all of these batteries are within the scope of the present invention. The technical concept of the present invention can also be applied to sodium ion secondary batteries, magnesium ion secondary batteries, calcium ion secondary batteries, zinc secondary batteries, aluminum ion secondary batteries, and the like.
[0012] When selecting a material from the group of materials exemplified below, a single material may be selected or a combination of multiple materials may be selected within the scope of the disclosure of this specification. Also, a material other than the group of materials exemplified below may be selected within the scope of the disclosure of this specification.
[0013] Fig. 1 is a cross-sectional view of a lithium ion secondary battery according to one embodiment of the present invention. Fig. 1 shows a laminated lithium ion secondary battery, and the lithium ion secondary battery 1000 has a positive electrode 100, a negative electrode 200, an exterior body 500, and an insulating layer 300. The exterior body 500 houses the insulating layer 300, the positive electrode 100, and the negative electrode 200. The exterior body 500 is selected from a group of materials that are corrosion-resistant to non-aqueous electrolytes, such as aluminum, stainless steel, and nickel-plated steel. The lithium ion secondary battery can also be configured as a wound type.
[0014] In the lithium-ion secondary battery 1000, an electrode assembly is formed by stacking an electrode body 400 composed of a positive electrode 100, an insulating layer 300, and a negative electrode 200. Hereinafter, the positive electrode 100 or the negative electrode 200 may be referred to as an electrode. Also, a stack of the positive electrode 100 or the negative electrode 200, or both, and the insulating layer 300 may be referred to as a sheet for a secondary battery. When the insulating layer 300 and the electrode are integrally formed, an electrode assembly can be produced by simply stacking the sheets for a secondary battery.
[0015] The positive electrode 100 has a positive electrode current collector 120 and a positive electrode mixture layer 110. The positive electrode mixture layer 110 is formed on both sides of the positive electrode current collector 120. The negative electrode 200 has a negative electrode current collector 220 and a negative electrode mixture layer 210. The negative electrode mixture layer 210 is formed on both sides of the negative electrode current collector 220. The positive electrode mixture layer 110 or the negative electrode mixture layer 210 may be referred to as an electrode mixture layer, and the positive electrode current collector 120 or the negative electrode current collector 220 may be referred to as an electrode current collector.
[0016] The positive electrode current collector 120 has a positive electrode tab 130. The negative electrode current collector 220 has a negative electrode tab 230. The positive electrode tab 130 or the negative electrode tab 230 may be referred to as an electrode tab. An electrode mixture layer is not formed on the electrode tab. However, an electrode mixture layer may be formed on the electrode tab as long as it does not adversely affect the performance of the lithium ion secondary battery 1000. The positive electrode tab 130 and the negative electrode tab 230 protrude to the outside of the exterior body 500, and a parallel connection is formed in the lithium ion secondary battery 1000 by bonding a plurality of protruding positive electrode tabs 130 and a plurality of protruding negative electrode tabs 230 to each other, for example, by ultrasonic bonding or the like. The lithium ion secondary battery according to the present invention may also be configured as a bipolar type having an electrical series connection in the secondary battery.
[0017] The positive electrode mixture layer 110 includes a positive electrode active material, a positive electrode conductive agent, and a positive electrode binder. The negative electrode mixture layer 210 includes a negative electrode active material, a negative electrode conductive agent, and a negative electrode binder. The positive electrode active material or the negative electrode active material may be referred to as an electrode active material, the positive electrode conductive agent or the negative electrode conductive agent as an electrode conductive agent, and the positive electrode binder or the negative electrode binder as an electrode binder.
[0018] <Electrode conductive agent> The electrode conductive agent improves the electrical conductivity of the electrode mixture layer, and can be appropriately selected from a group of materials such as ketjen black, acetylene black, and graphite.
[0019] <Electrode binder> The electrode binder binds the electrode active material, the electrode conductive agent, etc. in the electrode. The electrode binder can be appropriately selected from a group of materials such as styrene-butadiene rubber (SBR), carboxymethyl cellulose (CMC), polyvinylidene fluoride (PVDF), and a copolymer of vinylidene fluoride (VDF) and hexafluoropropylene (HFP) (P(VdF-HFP)).
[0020] <Cathode active material> In the positive electrode active material exhibiting a noble potential, lithium ions are released during the charging process, and lithium ions released from the negative electrode active material are inserted during the discharging process. As the positive electrode active material, a lithium composite oxide having a transition metal is preferable. Specifically, LiMO2, Li[LiM]O2 with Li-excess composition, LiM2O4, LiMPO4, LiMVO4, LiMBO3, Li2MSiO4 (wherein M is at least one selected from Co, Ni, Mn, Fe, Cr, Zn, Ta, Al, Mg, Cu, Cd, Mo, Nb, W, Ru, etc.) can be mentioned. In addition, a part of the oxygen in these materials may be replaced with other elements such as fluorine. Furthermore, the positive electrode active material can include at least one selected from a group of materials such as chalcogenides such as TiS2, MoS2, Mo6S8, and TiSe2, vanadium-based oxides such as V2O5, halides such as FeF3, quinone-based organic crystals such as Fe(MoO4)3, Fe2(SO4)3, and Li3Fe2(PO4)3 that constitute polyanions, and oxygen.
[0021] <Positive electrode current collector 120> The positive electrode current collector 120 can be appropriately selected from a group of materials such as aluminum foil having a thickness of 1 μm to 100 μm, aluminum perforated foil having a thickness of 10 μm to 100 μm and holes with a diameter of 0.1 mm to 10 mm, expanded metal, foam metal plate, stainless steel, titanium, etc.
[0022] <Negative electrode active material> A negative electrode active material exhibiting a lower potential releases lithium ions during the discharge process, and inserts lithium ions released from the positive electrode active material in the positive electrode mixture layer 110 during the charge process. Examples of negative electrode active materials include carbon-based materials (graphite, easily graphitized carbon materials, amorphous carbon materials, organic crystals, activated carbon, etc.), conductive polymer materials (polyacene, polyparaphenylene, polyaniline, polyacetylene, etc.), lithium composite oxides (lithium titanate: Li4Ti5O 12 The material can be appropriately selected from a group of materials such as lithium carbide, lithium carbide alloys (such as Li2TiO4, Li2TiO4, etc.), metallic lithium, metals that are alloyed with lithium (such as at least one of aluminum, silicon, tin, etc.), and oxides of these metals.
[0023] <Negative electrode current collector 220> The negative electrode current collector 220 can be appropriately selected from a group of materials such as copper foil having a thickness of 1 μm to 100 μm, perforated copper foil having a thickness of 1 μm to 100 μm and a pore size of 0.1 mm to 10 mm, expanded metal, foamed metal plate, stainless steel, titanium, nickel, etc.
[0024] <Electrode> An electrode mixture layer is produced by attaching an electrode slurry, which is a mixture of an electrode active material, an electrode conductive agent, an electrode binder, and a solvent, to an electrode current collector by a coating method such as a doctor blade method, a dipping method, a spray method, etc. The solvent is selected from a group of materials such as N-methylpyrrolidone (NMP) and water. Thereafter, the electrode mixture layer is dried to remove the solvent, and the electrode mixture layer is pressure-molded by a roll press to produce an electrode.
[0025] When the electrode mixture layer contains a non-aqueous electrolyte, the content of the non-aqueous electrolyte in the electrode mixture layer is preferably 20% by volume to 40% by volume. When the content of the non-aqueous electrolyte is small, the ion conduction path inside the electrode mixture layer may not be sufficiently formed, and the rate characteristics may be deteriorated. When the content of the non-aqueous electrolyte is large, the non-aqueous electrolyte may leak from the electrode mixture layer, and the relative amount of the electrode active material may be insufficient, resulting in a decrease in energy density.
[0026] In order to make the electrode mixture layer contain the nonaqueous electrolyte, the nonaqueous electrolyte can be injected into the lithium ion secondary battery 1000 from one open side or an inlet of the exterior body 500, and the pores of the electrode mixture layer can be filled with the nonaqueous electrolyte. Alternatively, a slurry containing the nonaqueous electrolyte, the electrode active material, the electrode conductive agent, and the electrode binder may be prepared, and the prepared slurry may be applied together onto the electrode current collector to fill the pores of the electrode mixture layer with the nonaqueous electrolyte. This eliminates the need for support particles contained in a semi-solid electrolyte, and particles such as the electrode active material and the electrode conductive agent in the electrode mixture layer function as support particles, allowing the particles to hold the nonaqueous electrolyte.
[0027] The thickness of the electrode mixture layer is preferably equal to or larger than the average particle size of the electrode active material. If the thickness of the electrode mixture layer is small, the electronic conductivity between adjacent electrode active materials may deteriorate. If there are coarse particles having an average particle size equal to or larger than the thickness of the electrode mixture layer in the electrode active material powder, it is preferable to remove the coarse particles in advance by sieve classification, air flow classification, etc., to obtain particles having a size equal to or smaller than the thickness of the electrode mixture layer.
[0028] <Insulating layer 300> The insulating layer 300 serves as a medium for transmitting ions between the positive electrode 100 and the negative electrode 200. The insulating layer 300 also acts as an electronic insulator, preventing short-circuiting between the positive electrode 100 and the negative electrode 200. The insulating layer 300 may have a semi-solid electrolyte layer. As the insulating layer 300, a separator and a semi-solid electrolyte layer may be used in combination.
[0029] <separator> A porous sheet can be used as the separator. The porous sheet can be selected from a group of materials such as cellulose, modified cellulose (carboxymethyl cellulose (CMC), hydroxypropyl cellulose (HPC), etc.), polyolefin (polypropylene (PP), propylene copolymer, etc.), polyester (polyethylene terephthalate (PET), polyethylene naphthalate (PEN), polybutylene terephthalate (PBT), etc.), polyacrylonitrile (PAN), polyaramid, polyamide-imide, polyimide, and other resins, glass, etc. By making the separator larger in area than the positive electrode 100 or the negative electrode 200, a short circuit between the positive electrode 100 and the negative electrode 200 can be prevented.
[0030] The separator may be formed by applying a separator-forming mixture having separator particles, a separator binder, and a solvent to the electrode mixture layer, or the separator-forming mixture may be applied to the porous sheet.
[0031] The separator particles are selected from a group of materials such as γ-alumina (Al2O3), silica (SiO2), and zirconia (ZrO2). The average particle size of the separator particles is preferably 1 / 100 to 1 / 2 the thickness of the separator. The separator binder can be appropriately selected from materials such as polyethylene (PE), PP, polytetrafluoroethylene (PTFE), PVDF, P(VdF-HFP), styrene butadiene rubber (SBR), polyalginic acid, and polyacrylic acid.
[0032] When insulating layer 300 includes a separator, the separator can be filled with the nonaqueous electrolyte by injecting the nonaqueous electrolyte into lithium ion secondary battery 1000 through an open side of exterior body 500 or an injection hole.
[0033] <Semi-solid electrolyte layer> The semi-solid electrolyte layer includes a semi-solid electrolyte binder and a semi-solid electrolyte. The semi-solid electrolyte includes support particles and a non-aqueous electrolyte. The semi-solid electrolyte has pores formed by an aggregate of support particles, and a non-aqueous electrolyte is held therein. By holding the non-aqueous electrolyte in the semi-solid electrolyte, the semi-solid electrolyte allows lithium ions to pass through. When a semi-solid electrolyte layer is used as the insulating layer 300 and the electrode mixture layer is filled with a non-aqueous electrolyte, it is not necessary to inject a non-aqueous electrolyte into the lithium ion secondary battery 1000.
[0034] A semi-solid electrolyte layer can be a semi-transparent free-standing membrane that can be handled like a solid, even though it contains liquid components such as a non-aqueous electrolyte. Locally, the liquid components such as the non-aqueous electrolyte are responsible for lithium ion conduction, so the layer exhibits high ionic conductivity. In other words, the semi-solid electrolyte layer combines the advantages of both the high safety of a solid and the high ionic conductivity of a liquid.
[0035] Methods for producing a semi-solid electrolyte layer include a method of compressing and molding a powder of a semi-solid electrolyte into a pellet shape using a molding die, and a method of adding and mixing a semi-solid electrolyte binder with a powder of a semi-solid electrolyte to form a sheet. By adding and mixing a semi-solid electrolyte binder with a powder of a semi-solid electrolyte, a highly flexible sheet-shaped semi-solid electrolyte layer can be produced. A semi-solid electrolyte layer may also be produced by adding and mixing a binder solution in which a semi-solid electrolyte binder is dissolved in a dispersion solvent to a semi-solid electrolyte, applying the mixture to a substrate such as an electrode, and distilling off the dispersion solvent by drying.
[0036] <Support particles> From the viewpoint of electrochemical stability, the support particles are preferably insulating particles that are insoluble in the non-aqueous electrolyte. The support particles can be appropriately selected from a group of materials such as inorganic oxide particles, such as SiO2 particles, Al2O3 particles, ceria (CeO2) particles, and ZrO2 particles, and solid electrolytes. By using inorganic oxide particles as the support particles, the non-aqueous electrolyte can be maintained at a high concentration in the semi-solid electrolyte layer. In addition, since gas is not generated from the inorganic oxide particles, the semi-solid electrolyte layer can be produced by a roll-to-roll process in the atmosphere. The solid electrolyte can be an oxide-based solid electrolyte, such as Li-La-Zr-O, or Li 10 Ge2PS 12 The material can be appropriately selected from a group of sulfide-based solid electrolytes and the like.
[0037] Since the amount of non-aqueous electrolyte held is considered to be proportional to the specific surface area of the support particles, the average particle size of the primary particles of the support particles is preferably 1 nm to 10 μm. If the average particle size of the primary particles of the support particles is large, the support particles may not be able to hold a sufficient amount of non-aqueous electrolyte properly, which may make it difficult to form a semi-solid electrolyte. If the average particle size of the primary particles of the support particles is small, the inter-surface force between the support particles increases, which may make the support particles more likely to aggregate, which may make it difficult to form a semi-solid electrolyte. The average particle size of the primary particles of the support particles is more preferably in the range of 1 nm to 50 nm, and even more preferably in the range of 1 nm to 10 nm. The average particle size of the primary particles of the support particles can be measured using a TEM.
[0038] <Nonaqueous electrolyte> The non-aqueous electrolyte includes a main solvent, a low-viscosity organic solvent having a relative dielectric constant different from that of the main solvent, an electrolyte salt, and an optional negative electrode interface stabilizer. The main solvent has a high relative dielectric constant and has the effect of increasing the concentration of lithium ions by dissociation of a lithium salt. The main solvent is at least one selected from the group consisting of sulfolane and its derivatives (also referred to as "sulfolane and / or its derivatives"). Therefore, the main solvent may contain two or more solvents, for example, two, three, or four solvents, selected from the group consisting of sulfolane and its derivatives. The sulfolane and / or its derivatives constitute a solvated ionic liquid together with the electrolyte salt. In the following description, the sulfolane and / or its derivatives may be referred to as the main solvent. The components contained in the non-aqueous electrolyte can be measured by NMR or the like. The relative dielectric constants of the main solvent and the low-viscosity organic solvent can be measured by a relative dielectric constant measuring device.
[0039] The content of the non-aqueous electrolyte in the semi-solid electrolyte layer is not particularly limited, but is preferably 40% by volume to 90% by volume. If the content of the non-aqueous electrolyte is small, the interface resistance between the electrode and the semi-solid electrolyte layer may increase. If the content of the non-aqueous electrolyte is large, the non-aqueous electrolyte may leak out of the semi-solid electrolyte layer. When the semi-solid electrolyte layer is in a sheet form, the content of the non-aqueous electrolyte in the semi-solid electrolyte layer is preferably 50% by volume to 80% by volume, more preferably 60% by volume to 80% by volume. When the semi-solid electrolyte layer is formed by applying a mixture of a semi-solid electrolyte and a solution in which a semi-solid electrolyte binder is dissolved in a dispersion solvent onto an electrode, the content of the non-aqueous electrolyte in the semi-solid electrolyte layer is preferably 40% by volume to 60% by volume.
[0040] The weight ratio of the main solvent in the non-aqueous electrolyte is not particularly limited, but from the viewpoint of the stability of the lithium ion secondary battery and to enable high-speed charging and discharging, it is desirable that the weight ratio of the main solvent in the non-aqueous electrolyte be 30 weight % (wt%) to 70 wt%, particularly 40 wt% to 60 wt%, and further 45 wt% to 55 wt%.
[0041] <Solvated ionic liquid> The solvated ionic liquid contains sulfolane and / or a derivative thereof and an electrolyte salt. When a solvated ionic liquid containing sulfolane and / or a derivative thereof is used, a specific coordination structure is formed between the sulfolane and / or a derivative thereof and the lithium ion, so that the transport rate of the lithium ion in the semi-solid electrolyte layer is increased. Therefore, unlike a solvated ionic liquid containing an ether solvent and an electrolyte salt, in which the input / output characteristics of a secondary battery decrease as the viscosity increases, the solvated ionic liquid can suppress the decrease in the input / output characteristics of a secondary battery containing the solvated ionic liquid even if the viscosity of the solvated ionic liquid is increased.
[0042] Examples of the derivatives of sulfolane include those in which the hydrogen atoms bonded to the carbon atoms constituting the sulfolane ring are substituted with fluorine atoms, alkyl groups, etc. Specific examples thereof can be appropriately selected from a group of materials such as fluorosulfolane, difluorosulfolane, and methylsulfolane.
[0043] <Electrolyte salt> The electrolyte salt is preferably one that can be uniformly dispersed in a low-viscosity organic solvent, and when the cation is lithium, various lithium salts can be used. As the electrolyte salt, a material that satisfies the above conditions can be appropriately selected from a group of materials such as lithium tetrafluoroborate (LiBF4), lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), lithium bis(fluorosulfonyl)imide (LiFSI), LiClO4, lithium bis(fluorosulfonyl)amide (LiFSA), lithium bis(trifluoromethanesulfonyl)amide (LiTFSA), and mixtures of two or more of them. It is preferable to use LiBF4 as the electrolyte salt. LiBF4 is stable against negative electrode active materials such as graphite, and can increase the capacity of a secondary battery.
[0044] A solvated ionic liquid having sulfolane and / or its derivatives and an electrolyte salt can be expressed as a single entity in terms of its apparent composition. For example, a solvated ionic liquid consisting of sulfolane and LiTFSI can be expressed as Li(SL) xIt is expressed as TFSI (x = 2 to 6), and the number of moles is calculated as a single substance having this composition.
[0045] The concentration of the electrolyte salt in the main solvent is preferably 1.06 mol / L to 3.46 mol / L. If the concentration is too high, the viscosity increases, the resistance increases, and the capacity tends to decrease. If the concentration is too low, the solvent becomes unstable, and the life characteristics tend to decrease.
[0046] <Low viscosity organic solvent> The low-viscosity organic solvent is an organic solvent having a different relative dielectric constant from the main solvent and a lower viscosity than the solvated ionic liquid. Therefore, by mixing the low-viscosity organic solvent with the solvated ionic liquid, the viscosity of the solvated ionic liquid can be reduced and the ionic conductivity can be improved. In addition, when the internal resistance of the non-aqueous electrolyte is large, the internal resistance of the non-aqueous electrolyte can be reduced by adding a low-viscosity organic solvent to increase the ionic conductivity of the non-aqueous electrolyte.
[0047] The low-viscosity solvent can be appropriately selected from a group of materials such as cyclic carbonates, such as ethylene carbonate (EC), propylene carbonate (PC), 1,2-butylene carbonate (BC), and fluoroethylene carbonate (FEC); non-cyclic esters, such as methyl ethyl carbonate (EMC), dimethyl carbonate (DMC), and diethyl carbonate (DEC); phosphates, such as trimethyl phosphate (TMP), triethyl phosphate (TEP), tris(2,2,2-trifluoroethyl) phosphite (TFP), and dimethyl methylphosphonate (DMMP); lactones, such as γ-butyrolactone (GBL); and mixtures of two or more of these.
[0048] When a nonaqueous electrolyte contains one or more main solvents and one or more low-viscosity organic solvents, the relative dielectric constant Z of the mixed solvent (main solvent + low-viscosity organic solvent) is expressed as p i , the molar ratio of the i-th main solvent in the mixed solvent is q i , the dielectric constant of the i-th low-viscosity organic solvent is p' i , the molar ratio of the i-th low-viscosity organic solvent in the mixed solvent is q' i When
number
[0049] For example, when a nonaqueous electrolyte contains one main solvent and one low-viscosity organic solvent, the relative dielectric constant Z of the mixed solvent (main solvent + low-viscosity organic solvent) is expressed as follows, where p is the relative dielectric constant of the main solvent, q is the molar ratio of the main solvent in the mixed solvent, p' is the relative dielectric constant of the low-viscosity organic solvent, and q' is the molar ratio of the low-viscosity organic solvent in the mixed solvent: Z=p×q+p'×q'...Equation (2) It is desirable for Z to be 63 or less.
[0050] By adding a low-viscosity organic solvent with a low relative dielectric constant to the solvated ionic liquid, the viscosity of the solvated ionic liquid can be reduced. On the other hand, if too much low-viscosity organic solvent is added to the solvated ionic liquid, the degree of dissociation of the lithium salt decreases, making it impossible to form a good quality SEI (Solid Electrolyte Interphase), and the life characteristics at high temperatures (45°C) decrease. Therefore, by making Z 63 or less, it is possible to reduce the viscosity of the solvated ionic liquid while suppressing the decrease in the degree of dissociation of the lithium salt, and to improve the life characteristics at high temperatures (45°C). The molar ratio of the main solvent in the mixed solvent and the molar ratio of the low-viscosity organic solvent in the mixed solvent can be measured by NMR.
[0051] <Negative electrode interface stabilizing material> The non-aqueous electrolyte solution contains a negative electrode interface stabilizer, which can improve the rate characteristics and battery life of the secondary battery. The negative electrode interface stabilizer can be appropriately selected from a group of materials such as vinylene carbonate (VC) and fluoroethylene carbonate (FEC).
[0052] <Corrosion inhibitor> The non-aqueous electrolyte may contain a corrosion inhibitor as necessary. The corrosion inhibitor forms a film that is less likely to dissolve metal even when the positive electrode current collector 120 is exposed to a high electrochemical potential. As the corrosion inhibitor, a material that contains an anion species such as PF6 or BF4 and a cation species having a strong chemical bond to form a stable compound in a humid atmosphere is preferable.
[0053] Indicators of whether a compound is stable in air include its solubility in water and whether it undergoes hydrolysis. If the corrosion inhibitor is solid, it is desirable for its solubility in water to be less than 1%. Furthermore, whether it undergoes hydrolysis can be evaluated by analyzing the molecular structure of a sample after mixing with water. Here, "not undergoing hydrolysis" means that after the corrosion inhibitor absorbs moisture or is mixed with water, it is heated at 100°C or higher to remove the moisture, and 95% of the residue shows the same molecular structure as the original corrosion inhibitor.
[0054] Corrosion inhibitors include (MR) + An - It is expressed as follows. (MR) + An - The cation of (MR) + M is selected from nitrogen (N), boron (B), phosphorus (P) or sulfur (S). R consists of a hydrocarbon group.
[0055] (M.R.) + An - The anion of is An - It is. - As for BF4, - or PF6 - is preferably used. The anion of the corrosion inhibitor is BF4 - or PF6 - By using BF4, the elution of the positive electrode current collector 120 can be effectively suppressed. - or PF6 - This is thought to be because the F anions react with the SUS or aluminum of the electrode current collector, forming a passive film.
[0056] The corrosion inhibitor can be appropriately selected from a group of materials such as quaternary ammonium salts, such as tetrabutylammonium hexafluorophosphate (TBAPF6) and tetrabutylammonium tetrafluoroborate (TBABF4), and imidazolium salts, such as 1-ethyl-3-methylimidazolium tetrafluoroborate (EMI-BF4), 1-ethyl-3-methylimidazolium hexafluorophosphate (EMI-PF6), 1-butyl-3-methylimidazolium tetrafluoroborate (BMI-BF4), and 1-butyl-3-methylimidazolium hexafluorophosphate (BMI-PF6). In particular, the anion of PF6 - In this case, elution of the positive electrode current collector 120 can be suitably suppressed.
[0057] The content of the corrosion inhibitor is preferably 0.5% by weight to 20% by weight, more preferably 1% by weight to 10% by weight, based on the total weight of the non-aqueous electrolyte. If the content of the corrosion inhibitor is low, the effect of suppressing the elution of the electrode current collector is reduced, and the battery capacity may decrease with charging and discharging. If the content of the corrosion inhibitor is high, the lithium ion conductivity decreases, and moreover, a lot of storage energy is consumed to decompose the corrosion inhibitor, which may result in a decrease in battery capacity.
[0058] <Semi-solid electrolyte binder> As the semi-solid electrolyte binder, a fluorine-based resin is preferably used. The fluorine-based resin can be appropriately selected from a group of materials such as PTFE, PVDF, and P(VdF-HFP). By using PVDF or P(VdF-HFP), the adhesion between the insulating layer 300 and the electrode current collector is improved, thereby improving the battery performance.
[0059] <Semi-solid electrolyte> A semi-solid electrolyte is formed by supporting or retaining a non-aqueous electrolyte on support particles. Examples of methods for producing a semi-solid electrolyte include a method in which a non-aqueous electrolyte and support particles are mixed in a specific volume ratio, an organic solvent such as methanol is added and mixed to prepare a slurry of the semi-solid electrolyte, the slurry is spread on a petri dish, and the organic solvent is distilled off to obtain a powder of the semi-solid electrolyte. EXAMPLES
[0060] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to these examples.
[0061] <Example 1> <Preparation of non-aqueous electrolyte> The electrolyte salt was lithium bis(trifluoromethanesulfonyl)amide (LiTFSA), a lithium salt (Li salt), the main solvent was sulfolane (SL), the low-viscosity solvent was propylene carbonate (PC), the negative electrode interface stabilizer was vinylene carbonate (VC), a graphite film forming material, and the corrosion inhibitor was tetrabutylammonium hexafluorophosphate (TBA-PF6), an additive for suppressing Al current collector foils. These were weighed and mixed to prepare a non-aqueous electrolyte. The components contained in the prepared non-aqueous electrolyte were quantified by NMR. As a result, the molar ratio of the main solvent (SL) to the low-viscosity solvent (PC) was 65.4:34.6, and the lithium salt concentration was 2.37 mol / L.
[0062] <Preparation of positive electrode> LiNi as the positive electrode active material 1 / 3 Co 1 / 3 Mn 1 / 3O2-based oxide, acetylene black as a positive electrode conductive agent, and PVDF dissolved in N-methylpyrrolidone as a positive electrode binder were weighed out so that the weight ratio of solids was 94:4:2, and these were uniformly mixed in a kneader. The obtained mixture was made into a slurry by adding NMP and adjusted to a predetermined solid concentration. Next, the slurry with the adjusted concentration was applied to both sides of aluminum foil, which is a positive electrode current collector foil, using a tabletop coater, and passed through a drying oven at 120°C to obtain a positive electrode. The coating amount of the positive electrode mixture (positive electrode active material + positive electrode conductive agent + positive electrode binder) was 30.1 mg / cm2 in total on both sides. 2 The obtained positive electrode was roll-pressed to an electrode density of 3.15 g / cm 3 was adjusted to.
[0063] <Preparation of negative electrode> Graphite was used as the negative electrode active material, and styrene-butadiene rubber and carboxyl methyl cellulose were used as the negative electrode binder. They were weighed out so that the weight ratio of the solids was 98:1:1, and were mixed uniformly in a kneader. Water was added to the resulting mixture to make it into a slurry, and the solids concentration was adjusted to a predetermined value. The slurry with the adjusted concentration was then applied to both sides of a copper foil, which was the negative electrode current collector foil, using a tabletop coater, and the mixture was passed through a drying oven at 100°C to obtain a negative electrode. The coating amount of the negative electrode mixture (negative electrode active material + negative electrode binder) was 18.1 mg / cm2 in total on both sides. 2 The obtained negative electrode was roll-pressed to an electrode density of 1.55 g / cm 3 was adjusted to.
[0064] <Separator formation> The separator was formed by applying a non-volatile electrolyte to the surface of the electrode mixture layer. First, SiO2 with an average particle size of 1 μm as the supporting particles and vinylidene fluoride-hexafluoropropylene copolymer (P(VdF-HFP)) as the binder were weighed to a weight ratio of 89.3:10.7, and these were uniformly mixed in a kneader. The obtained mixture was made into a slurry by adding NMP and adjusted to a predetermined solid content concentration. Next, the slurry with the adjusted concentration was applied to both sides of the positive electrode and the negative electrode with a tabletop coater, and passed through a drying oven at 100 ° C to obtain a positive electrode and a negative electrode with a non-volatile electrolyte layer formed thereon.
[0065] <Preparation of secondary battery> <Assembly> The prepared positive and negative electrodes were punched out with an air punching machine so that the positive electrode mixture layer was 45 mm x 70 mm and the negative electrode mixture layer was 47 mm x 74 mm, and tabs were formed on the positive and negative electrodes. The positive and negative electrodes were then dried at 100°C for 2 hours to remove the NMP in the electrodes. The dried positive electrode was sandwiched between a resin microporous membrane having a thickness of 30 μm and a three-layer structure of PP / PE / PP, and the three sides other than the side on which the tab was formed were heat-welded.
[0066] The positive electrode covered with a microporous membrane and the punched negative electrode were laminated in the order of negative electrode / positive electrode / negative electrode, and then a 50 μm thick PTFE sheet was placed on the negative electrode. The tabs on the positive and negative electrodes were welded to an aluminum positive electrode terminal and a nickel negative electrode terminal by ultrasonic welding, respectively. The obtained electrode body was sandwiched between laminate films, and the three sides including the side on which the tabs were formed were heat sealed at 200 ° C. by a laminating and sealing device, leaving one side for injection, and then vacuum dried at 50 ° C. for 20 hours. Next, a nonaqueous electrolyte was injected from one side for injection, and the one side for injection was vacuum sealed to obtain a secondary battery.
[0067] <Discharge capacity measurement> (1) Measurement of initial discharge capacity The secondary battery thus fabricated was kept at 25°C and charged at a constant current (CC) at a charge rate of 0.05 C to an upper limit voltage of 4.2 V, and then charged at a constant voltage (CV) until the current value decreased to 0.005 C while maintaining the voltage at 4.2 V. Thereafter, the secondary battery was discharged at a constant current at a discharge rate of 0.05 C to a lower limit voltage of 2.7 V, and the initial discharge capacity of the secondary battery was measured.
[0068] (2) Cycle test at 45℃ After measuring the initial discharge capacity, the secondary battery was heated to 45° C. and charged and discharged at 0.3 C for 100 cycles.
[0069] (3) Measurement of discharge capacity after cycle test The temperature of the secondary battery after the cycle test was lowered to 25°C and maintained at that temperature. It was then CC charged to an upper limit voltage of 4.2 V at a charge rate of 0.05 C, and then CV charged until the current value decreased to 0.005 C while maintaining the voltage at 4.2 V. It was then CC discharged to a lower limit voltage of 2.7 V at a discharge rate of 0.05 C, and the discharge capacity of the secondary battery after the cycle test was measured.
[0070] (4) Calculation of 45℃ discharge capacity retention rate The 45° C. discharge capacity retention rate, which was calculated from the ratio of the discharge capacity after the cycle test measured in (3) to the initial discharge capacity measured in (1), was evaluated as the 100 cycle life. 45°C discharge capacity retention rate (%) (100 cycle life) = (discharge capacity after cycle test / initial discharge capacity) × 100 Formula (3)
[0071] <Examples 2 to 12, Comparative Examples 1 to 2> A secondary battery was produced in the same manner as in Example 1 except that the composition of the non-aqueous electrolyte was changed as shown in Table 1, and the components contained in the non-aqueous electrolyte were quantified and the discharge capacity was measured.
[0072] Table 1 shows the compositions and 45° C. discharge capacity retention rates of the secondary batteries of Examples 1 to 12 and Comparative Examples 1 and 2. Fig. 2 shows the relationship between the lithium salt concentration (mol / L) in the main solvent and the 45° C. discharge capacity retention rate (%) in the Examples and Comparative Examples, and Fig. 3 shows the relationship between the relative dielectric constant of the mixed solvent and the 45° C. discharge capacity retention rate (%) in the Examples and Comparative Examples.
[0073] [Table 1]
[0074] <Results and Discussion> In FIG. 2, the 45° C. discharge capacity retention rate of the secondary battery is plotted against the lithium salt concentration. As shown in FIG. 2, in compositions with a lithium salt concentration of less than 2.21 mol / L, the 45° C. discharge capacity retention rate is small, and in compositions with a lithium salt concentration of 2.21 mol / L or more, the 45° C. discharge capacity retention rate is large. This result is believed to be due to the fact that the viscosity of the non-aqueous electrolyte is reduced and the ionic conductivity of the non-aqueous electrolyte is increased by mixing a low-viscosity organic solvent with a low viscosity and a solvated ionic liquid. In addition, in compositions with a lithium salt concentration of more than 2.21 mol / L, the lower the concentration, the higher the 45° C. discharge capacity retention rate was observed. This is believed to be due to the fact that the solvent is coordinated to the lithium ions and stabilized at a lower concentration.
[0075] From FIG. 2, it was confirmed that the 45° C. discharge capacity retention rate Y of the secondary battery is expressed by the following formula (4) using the lithium salt concentration X when the lithium salt concentration is in the range of 0.8 mol / L to 3.8 mol / L. Y=-4.0167X 2 +18.13X+73.074...Equation (4)
[0076] According to formula (4), the range of the lithium salt concentration X where the 45°C discharge capacity retention rate was greater than that of Comparative Example 1 (lithium salt concentration X=1) (87.7%) was 1.06 mol / L to 3.46 mol / L. The range of the lithium salt concentration X where the 45°C discharge capacity retention rate of the secondary battery was 89.5% or more was 1.25 mol / L to 3.26 mol / L. Moreover, the range of the lithium salt concentration X where the 45°C discharge capacity retention rate of the secondary battery was 90% or more was 1.32 mol / L to 3.18 mol / L. Moreover, the range of the lithium salt concentration X where the 45°C discharge capacity retention rate of the secondary battery was 92% or more was 1.64 mol / L to 2.86 mol / L. Therefore, the range of the lithium salt concentration X is 1.06 mol / L to 3.46 mol / L, preferably 1.25 mol / L to 3.26 mol / L, and more preferably 1.32 mol / L to 3.18 mol / L.
[0077] In FIG. 3, the 45° C. discharge capacity retention rate of the secondary battery is plotted against the relative dielectric constant of the mixed solvent in the nonaqueous electrolyte. As shown in FIG. 3, in compositions with a relative dielectric constant smaller than about 31.5, the 45° C. discharge capacity retention rate increases as the relative dielectric constant increases. On the other hand, in compositions with a relative dielectric constant larger than about 31.5, the 45° C. discharge capacity retention rate increases as the relative dielectric constant decreases. It is considered that the higher the relative dielectric constant that affects the dissociation of the electrolyte salt, the more prominent the reductive decomposition of the solvent on the graphite surface becomes when the electrolyte salt is added at a high concentration, and therefore the 45° C. discharge capacity retention rate decreases.
[0078] Here, when the relative dielectric constant of the main solvent is A, the molar ratio of the main solvent in the mixed solvent is M, the relative dielectric constant of the low-viscosity organic solvent is B, and the molar ratio of the low-viscosity organic solvent in the mixed solvent is N, the relative dielectric constant T of the mixed solvent can be defined by the following formula (5). T=A×M+B×N...Formula (5)
[0079] Therefore, it was confirmed from FIG. 3 that the 45° C. discharge capacity retention rate Y of the secondary battery is expressed by the following formula (6) using the relative dielectric constant T of the mixed solvent. Y=-0.0065T 2 +0.41T+88...Equation (6)
[0080] According to formula (6), the range of the relative dielectric constant T of the mixed solvent in which the 45°C discharge capacity retention rate was greater than that of the secondary battery of Comparative Example 1 (87.7%) was 63 or less. The range of the relative dielectric constant T of the mixed solvent in which the 45°C discharge capacity retention rate Z of the secondary battery was 89.5% or more was 3.9 to 59. The range of the relative dielectric constant T of the mixed solvent in which the 45°C discharge capacity retention rate of the secondary battery was 90% or more was 5.5 to 58. Furthermore, the range of the relative dielectric constant T of the mixed solvent in which the 45°C discharge capacity retention rate of the secondary battery was 92% or more was 12.5 to 51.0. Therefore, the range of the relative dielectric constant T of the mixed solvent is 63 or less, preferably 3.9 to 59, and more preferably 5.5 to 58. [Explanation of symbols]
[0081] 100 positive electrode 110 Positive electrode mixture layer 120 Positive electrode current collector 130 Positive electrode tab 200 negative electrode 210 Negative electrode mixture layer 220 Negative electrode current collector 230 Negative electrode tab 300 Insulation layer 400 Electrode body 500 Exterior 1000 Lithium-ion secondary battery
Claims
1. A non-aqueous electrolyte solution containing an electrolyte salt and an organic solvent, The organic solvent comprises at least one main solvent selected from the group consisting of sulfolane and its derivatives, and a low-viscosity organic solvent; The mixing molar ratio of the main solvent in the organic solvent is 51.1 mol% to 68.6 mol%, The concentration of the electrolyte salt relative to the main solvent is 1.32 mol / L to 3.18 mol / L; The dielectric constant of the organic solvent is 63 or less. Non-aqueous electrolyte.
2. The non-aqueous electrolyte solution according to claim 1, wherein the concentration of the electrolyte salt relative to the main solvent is 1.64 mol / L to 2.86 mol / L.
3. 2. The nonaqueous electrolyte according to claim 1, wherein the low-viscosity organic solvent comprises at least one selected from the group consisting of ethylene carbonate, propylene carbonate, 1,2-butylene carbonate, fluoroethylene carbonate, methyl ethyl carbonate, dimethyl carbonate, diethyl carbonate, trimethyl phosphate, triethyl phosphate, tris(2,2,2-trifluoroethyl) phosphite, dimethyl methylphosphonate, and γ-butyrolactone.
4. 2. The nonaqueous electrolyte solution according to claim 1, wherein the electrolyte salt comprises at least one selected from the group consisting of lithium tetrafluoroborate and lithium bis(trifluoromethanesulfonyl)amide.
5. A semi-solid electrolyte layer comprising the non-aqueous electrolyte according to claim 1, support particles, and a semi-solid electrolyte binder.
6. A sheet for a secondary battery, comprising a positive electrode and / or a negative electrode and the semi-solid electrolyte layer according to claim 5 laminated thereon.
7. A positive electrode and A negative electrode; The semi-solid electrolyte layer according to claim 5 , which is disposed between the positive electrode and the negative electrode; A secondary battery comprising:
Citation Information
Patent Citations
Secondary lithium battery
JP2003045485A
Nonaqueous electrolyte secondary battery
JP2007328978A
Nonaqueous electrolyte and nonaqueous electrolyte battery, and battery pack, electronic apparatus, electric vehicle, electricity storage device and electric power system including nonaqueous electrolyte battery
JP2012256502A
Secondary battery and method for manufacturing the same
JP2019016430A
Non-aqueous solvent and non-aqueous electrolytic solution for electrical storage devices, and electrical storage device, lithium secondary battery and electric double-layer capacitor each utilizing said non-aqueous solvent and said non-aqueous electrolytic solution
WO2012172723A1