Vulcanized fiber and its manufacturing method
By using a low-density vulcanized fiber with a softener and controlled zinc chloride concentration, along with physical engraving, the challenge of achieving flexibility and strength in vulcanized fibers is addressed, resulting in a flexible and durable material.
Patent Information
- Application Number
- JP2020213970
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-12-23
- Publication Date
- 2024-09-18
- Estimated Expiration
- 2040-12-23
AI Technical Summary
Existing vulcanized fibers struggle to achieve flexibility while maintaining strength, with impregnation methods like using humectants or nitrogen-containing and sulfur-containing compounds leading to issues such as moisture absorption limitations or metal corrosion.
Incorporating a softener with an apparent density of 1.1 g/cm³, achieved through low-density base paper, controlled zinc chloride concentration, and physical engraving to create voids, allowing for easy softener absorption and flexibility enhancement.
The resulting vulcanized fiber maintains strength while achieving leather-like suppleness and improved processing suitability, with enhanced flexibility and reduced metal corrosion risks.
Smart Images

Figure 0007553347000003 
Figure 0007553347000006 
Figure 0007553347000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a vulcanized fiber and a method for producing the same, and more particularly to a vulcanized fiber imparted with softness while suppressing a decrease in strength, and a method for producing the same. [Background technology]
[0002] Vulcanized fiber, also called vulcan fiber, is a tough organic industrial material produced by immersing base paper, mainly made of natural cellulose such as wood pulp and cotton pulp, in a reactive chemical that swells and gelats the pulp, such as an aqueous solution of zinc chloride, to swell and gelatinize the surface of the base paper, then removing the reactive chemical with a cleaning solution to stop the swelling and gelatinization reaction, and then drying and finishing. Vulcanized fiber is an environmentally friendly industrial material, as the main fiber is made of natural cellulose fiber, and is biodegradable and suitable for clean incineration treatment when discarded.
[0003] It is desirable for vulcanized fibers to be used in bags, wallets, hinges, etc., and therefore there is a demand for imparting flexibility to them. One proposal to achieve this is to impregnate vulcanized fibers with a moisturizing agent such as glycerin to impart moisture retention and hygroscopicity in order to improve their flexibility (see Patent Document 1). There is also a proposal to impregnate or coat vulcanized fibers with a nitrogen- and sulfur-containing water-soluble compound (see Patent Document 2).
[0004] As in Patent Document 1, there is a method of impregnating vulcanized fiber with a moisturizing agent having a high density and few voids to improve flexibility, but vulcanized fiber does not easily absorb moisturizing agents such as glycerin due to the reason above, and it is difficult to impart the desired level of flexibility to a level that satisfies the purpose by only adding a moisturizing agent. Also, vulcanized fiber impregnated or coated with a nitrogen-containing / sulfur-containing water-soluble compound as in Patent Document 2 has the problem that corrosion occurs when it comes into contact with metal. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Utility model registration No. 3099092 [Patent Document 2] Patent Publication No. 2015-89986 Summary of the Invention [Problem to be solved by the invention]
[0006] An object of the present invention is to provide a vulcanized fiber that is imparted with flexibility while suppressing a decrease in strength such as tensile strength, and a method for producing the same.
[0007] Other objects and advantages of the present invention will become readily apparent to those skilled in the art by reading the following description. [Means for solving the problem]
[0008] In order to achieve the above object, the vulcanized fiber of the present invention contains a softening agent and has an apparent density of 1.1 g / cm 3 The present invention is characterized in that:
[0009] The term "apparent density" as used herein refers to the mass per unit volume including not only the solid portion of the vulcanized fiber (the actual portion of the fibers, etc.) but also the void portion (the space such as pores, etc.).
[0010] According to this construction, the apparent density is lower than that of conventional vulcanized fibers, and therefore it is possible to obtain a vulcanized fiber having excellent flexibility and being more likely to absorb a fabric softener.
[0011] In a preferred embodiment of the present invention, the softening agent may be glycerin and / or polyethylene glycol, which results in a soft vulcanized fiber that is free from problems such as metal corrosion.
[0012] In a preferred embodiment of the present invention, the vulcanized fiber is engraved, and the reduction in basis weight before and after engraving may be in the range of 10 to 40%.
[0013] By "engraved" herein is meant that the surface of the vulcanized fiber has been cut to provide physical voids.
[0014] With this structure, the strength of the vulcanized fiber is maintained, while the apparent density can be easily reduced by providing physical voids through engraving.
[0015] The present invention can also be understood as a method for producing vulcanized fiber.
[0016] The method for producing a vulcanized fiber according to the present invention includes a base paper preparation step of preparing a vulcanized fiber base paper, a gelatinization step of immersing the vulcanized fiber base paper in a reactive chemical to swell and gelatinize the surface of the vulcanized fiber base paper, a deliquification step of immersing the vulcanized fiber base paper in a solution having a lower concentration than the reactive chemical to remove the reactive chemical, a drying and finishing step of drying the vulcanized fiber base paper after the deliquification to obtain a vulcanized fiber substrate, a softener impregnation step of impregnating the vulcanized fiber substrate with a softener, and a softener drying step of drying the vulcanized fiber substrate impregnated with the softener to obtain a vulcanized fiber, and the apparent density of the vulcanized fiber substrate is 1.1 g / cm. 3 The present invention is characterized in that:
[0017] According to this configuration, it is possible to produce a vulcanized fiber that has flexibility while maintaining its strength.
[0018] In a preferred embodiment of the present invention, an engraving step of providing engravings on the vulcanized fiber substrate may be further included between the drying / finishing step and the softener impregnation step.
[0019] According to such a configuration, the apparent density due to the engraving is reduced, and in addition, the softener is more easily impregnated in the subsequent process.
[0020] In a preferred embodiment of the present invention, the reduction rate of basis weight before and after the engraving step may be in the range of 10 to 40%.
[0021] In this configuration, the apparent density can be reduced by the physical voids provided by the engraving, while still maintaining the strength of the vulcanized fiber. Effect of the Invention
[0022] According to the present invention, it is possible to provide a vulcanized fiber that is imparted with flexibility while suppressing a decrease in strength, and a method for producing the same. The vulcanized fiber of the present invention has flexibility like leather, and, despite being a vulcanized fiber, has excellent processability such as folding and bending. [Brief description of the drawings]
[0023] [Figure 1] 1 is a general flow chart showing an example of a manufacturing process for a vulcanized fiber according to the present invention. [Diagram 2] FIG. 2 is a diagram showing an example of a cross-sectional structure of a vulcanized fiber. [Diagram 3] 1 is a table showing the composition of vulcanized fiber substrates according to examples and comparative examples. [Figure 4] 1 is a chart showing the composition of engraved vulcanized fibers according to examples and comparative examples. [Diagram 5] 1 is a table showing the evaluation results of vulcanized fibers according to Examples and Comparative Examples. [Figure 6] FIG. 1 shows an example of an engraved vulcanized fiber substrate surface. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0024] The present invention will be described below, but it should not be construed as being limited to these embodiments.
[0025] The vulcanized fiber according to the present invention contains a softening agent and has an apparent density of 1.1 g / cm 3 The vulcanized fiber according to the present invention is characterized in that it is characterized by the following. An example of the manufacturing process of the vulcanized fiber according to the present invention is shown in FIG. 1. Finishing The product at the stage where step 50 is completed is called "vulcanized fiber base material" and softener Drying The fiber after the step 70 is completed is called "vulcanized fiber." In the following description, reference will be made to FIG.
[0026] <Base paper preparation process 10> In the present invention, the vulcanized fiber base paper used for the vulcanized fiber may be produced from raw materials, or may be purchased and used according to the conditions. When producing the vulcanized fiber base paper, it is produced from natural cellulose such as wood pulp and cotton pulp. Examples of wood pulp include chemical pulps such as softwood dissolved sulfate pulp (NDSP), softwood bleached kraft pulp (NBKP), softwood unbleached kraft pulp (NUKP), hardwood bleached kraft pulp (LBKP), and hardwood unbleached kraft pulp (LUKP), mechanical pulps such as groundwood pulp (GP) and thermomechanical pulp (TMP), and waste paper pulps such as deinked pulp. One or more types selected from these pulps may be used. For example, a pulp slurry containing 15 to 55 parts by mass of NDSP, 25 to 75 parts by mass of NUKP, and 5 to 25 parts by mass of NBKP per 100 parts by mass of the total pulp slurry (Composition Example 1), or a pulp slurry containing 25 to 45 parts by mass of NDSP, 35 to 65 parts by mass of NUKP, and 10 to 20 parts by mass of NBKP per 100 parts by mass of the total pulp slurry (Composition Example 2) can be used.
[0027] In addition, it is preferable to adjust the pulp slurry for producing vulcanized fiber base paper to an appropriate freeness. For example, in the above-mentioned configuration examples 1 and 2, the freeness after beating is preferably in the range of 450 to 750 ml CSF for configuration example 1 and 550 to 650 ml CSF for configuration example 2 in terms of Canadian standard freeness (JIS P 8121:1995 "Testing method for freeness of pulp")
[0028] Furthermore, the base paper may suitably be made from cotton fibers such as cotton rag pulp and linters, papermaking pulp made from wood fibers, non-wood fibers such as kenaf and bamboo pulp, and regenerated cellulose fibers such as rayon, which are produced by wet papermaking. Organic chemical synthetic fibers and inorganic fibers may also be blended within the scope of the present invention, so long as the intended effects of the present invention are not impaired. The base paper preferably has suitable water absorption, air permeability, and uniform texture so that when immersed in a reactive chemical that has the property of swelling and gelatinizing the pulp, such as an aqueous zinc chloride solution, the aqueous zinc chloride solution can penetrate uniformly into the base paper.
[0029] <Agglomeration process 20> In the gelatinization step 20, the vulcanized fiber base paper is immersed in a reactive chemical in a conventional manner to swell and gelatinize the surface. Hereinafter, the gelatinization step may be referred to as "vulcanization". The reactive chemical used here may be a conventional one used for swelling and gelatinizing vulcanized fiber, such as an aqueous zinc chloride solution. When an aqueous zinc chloride solution is used as the reactive chemical, the concentration of zinc chloride is preferably in the range of 65 to 74 Baume (°Be), and the temperature of the aqueous solution during the immersion treatment is preferably in the range of 28 to 55°C.
[0030] As mentioned above, in the present invention, the apparent density of the vulcanized fiber is 1.1 g / cm 3By configuring the density of the vulcanized fiber base paper to be as low as 0.1 mm or less, it is possible to maintain strength while imparting flexibility. Effective methods for obtaining vulcanized fiber with a low apparent density include using vulcanized fiber base paper with a low apparent density, lowering the concentration of the zinc chloride aqueous solution in the gelatinization step 20, shortening the immersion time, and lowering the immersion temperature. The reason that the density of the vulcanized fiber base material is lowered by adjusting the concentration of the zinc chloride aqueous solution, the immersion time, and the immersion temperature is that the degree of penetration of zinc chloride into the cellulose fibers is reduced. By lowering the density of the vulcanized fiber base material, it becomes easier for the fabric softener to be absorbed, making it easier to soften the fiber.
[0031] When two or more sheets of base paper are used for the vulcanized fiber, these sheets of base paper are laminated in a gelatinization step 20. More specifically, the vulcanized fiber base paper is immersed in a reactive chemical, and then a lamination process is performed in the liquid several seconds later. The lamination step is not necessary for vulcanized fiber made of one sheet of base paper. The reactive chemical used here is not particularly limited as long as it swells and gelats the cellulose fiber, and in addition to an aqueous solution of zinc chloride, N-methylmorpholine-N-oxide, a mixed solution of N-methylmorpholine-N-oxide and a polar liquid, sulfuric acid, etc. can be used, but the method using an aqueous solution of zinc chloride is the most industrialized and is the most desirable for mass production.
[0032] <Deliquoring process 30> In the deliquor step 30, the reactive chemicals used in the gelatinization step 20 are removed with a cleaning solution. More specifically, a zinc chloride aqueous solution with a lower concentration than the zinc chloride aqueous solution used in the gelatinization step 20 is used as the cleaning solution, and the reactive solution is removed by sequentially immersing the paper in multiple cleaning tanks with gradually decreasing zinc chloride concentration, or by sequentially lowering the cleaning solution concentration in the cleaning tank. When multiple cleaning tanks are used, the cleaning tanks are provided so that the zinc chloride concentration is gradually decreased from the first tank to the final tank, and the cleaning solution in the final tank is a solution containing almost no zinc chloride component or fresh water, and the base paper after the gelatinization step 20 is sequentially immersed in these cleaning tanks to remove the zinc chloride aqueous solution. On the other hand, if processing is performed in a single tank, the reactive solution can be removed by sequentially replacing the entire amount of the cleaning solution in the cleaning tank to gradually change the concentration of the solution to a lower concentration, or by gradually pouring water into the cleaning tank to decrease the concentration of the cleaning solution.
[0033] The cleaning solution used in the deliquification step 30 is an aqueous zinc chloride solution with a lower concentration than that used in the gelatinization step 20. For example, if an aqueous zinc chloride solution with a concentration of 65 to 74 Baume is used in the gelatinization step 20, a cleaning solution with a lower concentration of zinc chloride, starting with an aqueous zinc chloride solution with a concentration of 15 to 33 Baume, is prepared so that the concentration of zinc chloride is gradually reduced to a solution containing almost no zinc chloride or water containing no zinc chloride, and deliquification is performed by the above-mentioned method. Furthermore, in the deliquification step, as disclosed in JP-A-09-302594, a device having a single-stage or multi-stage vibrating blade plate fixed non-rotatably to a vibration shaft that vibrates in the axial direction to promote the removal of reactive chemicals such as zinc chloride may be placed in the zinc dechlorination tank, i.e., in the cleaning solution in the cleaning tank, and deliquification may be performed while applying vibration to the vibration blade plate with a frequency of 10 to 60 Hz and a vibration width of 2 to 30 mm.
[0034] <Drying process 40, finishing process 50> After the deliquification step 30, the vulcanized fiber substrate is obtained through the drying step 40 and finishing step 50. The drying method used here is not particularly limited, and known drying methods such as hot air drying, microwave drying, infrared drying, and roll dryer drying can be used, and the vulcanized fiber substrate is dried until the desired moisture content is reached. In the finishing step 50, a roll winding process or cutting process to a predetermined size by flat cutting is performed. Calendaring may be performed as necessary to impart smoothness.
[0035] <Softener impregnation process 60> In the softener impregnation step 60, the vulcanized fiber substrate obtained by carrying out the base paper preparation step 10 to the finishing step 50 is impregnated with a softener. The softener used here may be glycerin, polyethylene glycol (PEG), polyacrylate, 1,2-hexanediol, 1,5-pentanediol, amino acids, hyaluronic acid, or the like. Among these, glycerin or polyethylene glycol is preferred because of its high softening effect, and glycerin is more preferred. Glycerin is easily absorbed into the vulcanized fiber substrate, and is highly effective in imparting softness. The method of imparting the softener is not particularly limited, but may be, for example, a method of immersing the vulcanized fiber substrate in an impregnation liquid containing a softener.
[0036] When glycerin is used as the softener, it is preferable to use an aqueous glycerin solution having a concentration of 20 to 90% by mass as the impregnation liquid, and more preferably an aqueous glycerin solution having a concentration of 30 to 70% by mass. If the concentration of the aqueous glycerin solution exceeds 90% by mass, the viscosity may become too high, which may make it difficult for the aqueous glycerin solution to impregnate the vulcanized fiber substrate. On the other hand, if the concentration of the aqueous glycerin solution is less than 20% by mass, the amount of glycerin imparted to the vulcanized fiber substrate may be reduced, even if the impregnation ability increases, and the desired flexibility may not be obtained. In addition, when the softener is impregnated into the vulcanized fiber substrate by impregnating the softener into the vulcanized fiber substrate, it is preferable to impregnate the vulcanized fiber substrate with water in advance. By impregnating the vulcanized fiber substrate with water in advance, the softener can be more easily penetrated. When the aqueous glycerin solution is impregnated into water in advance, the impregnation time is preferably about 30 minutes to 6 hours.
[0037] <Softener drying process 70> The vulcanized fiber substrate is impregnated with a softener and then dried to obtain the desired vulcanized fiber. The drying method used here is not particularly limited, and known drying methods such as hot air drying, heat drying, microwave drying, infrared drying, and roll dryer drying can be used, but heat drying at 60 to 100°C for about 15 minutes to 3 hours is preferred.
[0038] As mentioned above, the vulcanized fiber of the present invention has an apparent density of 1.1 g / cm 3 The apparent density is 1.0 g / cm or less. 3 It is more preferable that the apparent density is 1.1 g / cm or less. Here, the "apparent density" refers to the mass per unit volume including not only the actual part of the vulcanized fiber (the actual part of the fiber, etc.), i.e., the resin part of the porous sheet, but also the void part (the space part such as the pores). According to the findings of the present inventors, the apparent density is 1.1 g / cm 3By adjusting the density below, the flexibility of the vulcanized fiber containing the softener can be increased, and it can be made supple like leather. The apparent density of typical vulcanized fibers is 1.20 to 1.35 g / cm 3 That's about it.
[0039] In the present invention, the apparent density of the vulcanized fiber is 1.1 g / cm 3 The method described below is not particularly limited, and in addition to the degree of penetration of the reactive chemicals described above, the density of the vulcanized fiber substrate can be reduced, for example, to 1.1 g / cm. 3 This can be achieved by the following: When a vulcanized fiber base material is impregnated with a softener, the weight of the vulcanized fiber increases by the amount of the softener impregnated, but the thickness also increases accordingly, so that the apparent density of the vulcanized fiber can be controlled to some extent by the density of the vulcanized fiber base material.
[0040] In the present invention, the density of the vulcanized fiber substrate is not particularly limited, but is, for example, 0.7 to 1.4 g / cm 3 The desired effect is easily obtained by setting the density to 0.7 to 0.9 g / cm. Since the softening effect is easily obtained with a lower density, it is particularly preferable to set the density to 0.7 to 0.9 g / cm. 3 In order to keep the density of the vulcanized fiber substrate low, the vulcanization conditions may be relaxed, for example by lowering the temperature of the aqueous zinc chloride solution.
[0041] As a method for controlling the apparent density other than the vulcanization conditions, a method of physically providing voids by engraving the vulcanized fiber, as described below, may also be considered.
[0042] In the present invention, the thickness of the vulcanized fiber can be set to a desired thickness depending on the application, and for example, for general applications, a thickness of about 0.1 to 2.5 mm is considered. On the other hand, in the present invention, since a thinner thickness is more likely to achieve a softening effect, if the aim is to more significantly exert the effects of the present invention, the thickness is preferably in the range of 0.2 to 1.5 mm, and more preferably in the range of 0.3 to 1.0 mm.
[0043] The equilibrium moisture value of the vulcanized fiber conditioned under an environment of 23°C x 50% RH is not particularly limited, but is preferably in the range of 5 to 11%, and more preferably in the range of 5.5 to 10.5%. If the equilibrium moisture value is less than 5%, paper dust may be easily generated, and the paper may become brittle or easily cracked. On the other hand, if the equilibrium moisture value exceeds 11%, the degree of expansion and contraction may become large, making processing difficult. The moisture adjustment method is not particularly limited, and any known method used in the field of the present invention may be used, and the moisture can be adjusted mainly in the drying process 40. The drying temperature is preferably set appropriately in the range of 80 to 180°C.
[0044] <Engraving process> In the present invention, it is also possible to provide physical voids in the vulcanized fiber substrate or vulcanized fiber by engraving or the like. By engraving, the apparent density can be reduced, and at the same time, if engraving is performed at the vulcanized fiber substrate stage, it is possible to obtain the effect of making it easier to impregnate the softener. The timing of engraving can be between the finishing process 50 and the softener impregnation process 60, or after the softener is impregnated. Drying Although this can be done either after completion of step 70, impregnating the vulcanized fiber substrate with softener after engraving provides a greater softening effect, so it is preferable to perform this on the vulcanized fiber substrate between the finishing step 50 and the softener impregnation step 60. When voids are provided on the surface of the vulcanized fiber by engraving or the like, the apparent density can be calculated using the thickness of the portion where no voids are provided.
[0045] An example of the cross-sectional structure when engraving is applied to a vulcanized fiber substrate is shown in Figure 2. In the figure, 1 is the vulcanized fiber substrate, 2 is the surface of the vulcanized fiber substrate, 3 is the cut portion (recess), Ta is the thickness of the vulcanized fiber substrate, and Tb is the thickness of the cut portion. In the case of the example of Figure 2, the actual thickness of the engraved portion is Ta-Tb, but the apparent density is calculated using Ta.
[0046] In the present invention, the engraving technique may be any technique that produces depressions on the surface of the base material, such as laser processing, plasma etching, reactive ion etching, electron beam etching, focused ion beam processing, embossing, etc., but laser processing is preferred because of the ease of creating and modifying the engraving design.
[0047] In the present invention, the engraving pattern on the vulcanized fiber substrate is not particularly limited, and general patterns such as crosses and circles, or any other arbitrary engraving pattern can be appropriately provided. In the case of forming a cross engraving pattern, for example, a cross engraving pattern can be formed by intersecting straight lines with a line width of 0.05 mm and a length of 1.0 mm. Since the stiffness of the vulcanized fiber tends to be greater in the flow direction (MD) of the base paper than in the width direction (CD), it is preferable to engrave the vulcanized fiber so that the stiffness in the flow direction of the base paper is easily reduced in order to make all directions soft to the same degree. For example, when forming a cross engraving pattern, the length of the engraving in the width direction of the base paper is made larger than the length of the engraving in the flow direction of the base paper, making it easier to make all directions soft to the same degree. In addition, when forming a circular engraving pattern, the same effect can be obtained by making the engraving an ellipse with a long diameter in the width direction of the base paper.
[0048] In the present invention, the reduction in basis weight of the vulcanized fiber substrate before and after engraving is preferably in the range of 10 to 40%, more preferably in the range of 15 to 35%. If the reduction in basis weight is less than 10%, the softening effect of engraving may be poor. On the other hand, if the reduction in basis weight is more than 40%, the strength may decrease significantly, making it impractical.
[0049] In the present invention, the depth of the recess in the cut portion is preferably in the range of 30 to 95% of the thickness of the vulcanized fiber substrate, and more preferably in the range of 50 to 90%. If the depth of the recess is less than 30%, the reduction in the thickness of the vulcanized fiber substrate is small, and the softening effect may be poor. On the other hand, if the depth of the recess is more than 95%, the remaining portion is too small, making it easy to penetrate, and as a result, although softness is obtained, there is a risk of a large decrease in strength.
[0050] The shape of each engraving may be, for example, a cross or an L-shape, and the adjacent engraved parts are preferably not connected to each other and are spaced at a distance of 0.05 mm or more, more preferably at a distance of 0.1 mm or more. If the individual engraved parts are connected to each other, the strength may be significantly reduced. In addition, the size of each engraved pattern is preferably 2 mm or less in diameter. The diameter here means the length of the long side in the case of a shape having a long side and a short side such as an oval or a cross.
[0051] Figure 6 shows an example of the engraved surface of a vulcanized fiber substrate. In the example shown in the figure, a cross-shaped engraved pattern is formed by intersecting a straight line with a line width of 0.14 mm and a length of 0.75 mm with a straight line with a line width of 0.14 mm and a length of 0.33 mm. In addition, each pattern is spaced apart by 0.1 mm or more. Note that Figure 6 corresponds to Example 1 described later.
[0052] In the present invention, by engraving the vulcanized fiber substrate, the apparent density of the vulcanized fiber is finally set to 0.5 to 1.1 g / cm 3The surface may be scraped off by engraving to obtain the desired apparent density, or the density of the vulcanized fiber itself may be kept low to reduce the amount of engraving. 3 If the thickness is more than this, the desired softness may not be obtained. Conversely, if the thickness is less than 0.5 g / cm 3 If it exceeds this value, the strength may decrease too much. EXAMPLES
[0053] The method for producing a vulcanized fiber according to the present invention will be specifically described below using examples, but the present invention is not limited to these examples. In the examples, "parts" and "%" respectively mean "parts by mass" and "% by mass" unless otherwise specified. The number of parts added is a value calculated as a solid content.
[0054] Example 1 <Preparation of base paper> A slurry containing 70 parts by mass of cotton linters and 30 parts by mass of NBKP adjusted to 500 ml of CSF was used as a papermaking raw material and paper was made on a Fourdrinier papermaking machine to obtain a base paper. <Preparation of vulcanized fiber substrate> Ten sheets of base paper were immersed in an aqueous solution of zinc chloride (69°Be, 44°C) to swell and gelatinize the surfaces of the base paper, and the base papers were laminated. After that, the base papers were immersed in multiple baths containing cleaning solutions with gradually decreasing concentrations, from an aqueous zinc chloride solution of 23°Be to water without zinc chloride, and the base papers were subjected to a deliquification process to remove the aqueous zinc chloride solution from the base paper, a drying process using hot air and a cylinder dryer, and a calendaring process, in that order, to obtain a vulcanized fiber substrate. The thickness of the vulcanized fiber substrate was 1.0 mm. <Engraving process> One side of the obtained vulcanized fiber substrate was engraved using a small CO2 laser processing machine (HAJIME CL1: manufactured by O-Laser Co., Ltd.). The engraving was a cross pattern with a line width of 0.14 mm, and straight lines 0.75 mm long in the width direction of the vulcanized fiber substrate and 0.33 mm long in the flow direction were crossed at the center, and multiple such engravings were engraved. The spacing between each of the engravings was 1.13 mm in the width direction of the vulcanized fiber substrate and 0.38 mm in the flow direction. The laser output was 90%. <Softener impregnation and drying treatment> The engraved vulcanized fiber substrate was immersed in water for 1 hour, then immersed in a 50% glycerin aqueous solution for 1 hour using a shaker. It was then heat-dried at 80°C for 30 minutes and conditioned in an environment of 23°C x 50% RH. The basis weight of the vulcanized fiber after conditioning was 1219 g / m 2 , apparent density is 1.02g / cm 3 It was.
[0055] Example 2 A vulcanized fiber was obtained in the same manner as in Example 1, except that the pattern engraved on the vulcanized fiber substrate was changed. The engraving was a cross pattern with a line width of 0.28 mm, and consisted of straight lines with a length of 1.50 mm in the width direction of the vulcanized fiber substrate and a length of 0.65 mm in the flow direction, each of which was perpendicular to the center. The spacing between each of the engraved patterns was 2.25 mm in the width direction of the vulcanized fiber substrate and 0.75 mm in the flow direction. The basis weight of the vulcanized fiber after humidity conditioning was 1269 g / m 2 , apparent density is 1.07g / cm 3 It was.
[0056] Example 3 A vulcanized fiber was obtained in the same manner as in Example 1, except that the pattern engraved on the vulcanized fiber substrate was changed. The engraving was a cross pattern with a line width of 0.07 mm, and consisted of straight lines with a length of 0.38 mm in the width direction of the vulcanized fiber substrate and a length of 0.17 mm in the flow direction, each of which was perpendicular to the center. The spacing between each of the engraved patterns was 0.57 mm in the width direction of the vulcanized fiber substrate and 0.19 mm in the flow direction. The basis weight of the vulcanized fiber after humidity conditioning was 889 g / m 2 , apparent density is 0.86g / cm 3 It was.
[0057] Example 4 A vulcanized fiber was obtained in the same manner as in Example 1, except that the pattern engraved on the vulcanized fiber substrate was changed. The engraving was a circular pattern, and the diameter of the circle was 0.75 mm. The spacing between adjacent engraved patterns was 1.25 mm in the width direction of the vulcanized fiber substrate and 1.00 mm in the machine direction. The basis weight of the vulcanized fiber after humidity conditioning was 1289 g / m 2 , apparent density is 1.01g / cm 3 It was.
[0058] Example 5 A vulcanized fiber was obtained in the same manner as in Example 1, except that the pattern engraved on the vulcanized fiber substrate was changed. The engraving was an elliptical pattern, and the diameter of the ellipse was 1.75 mm in the width direction of the vulcanized fiber substrate and 0.60 mm in the machine direction. The spacing between adjacent engraved patterns was 2.50 mm in the width direction of the vulcanized fiber substrate and 1.25 mm in the machine direction. The basis weight of the vulcanized fiber after humidity conditioning was 1332 g / m 2 , apparent density is 1.04g / cm 3 It was.
[0059] Example 6 A vulcanized fiber was obtained in the same manner as in Example 1, except that the laser output was reduced to 30% and engraving was performed on both sides of the vulcanized fiber substrate. The basis weight of the vulcanized fiber after humidity conditioning was 1205 g / m2 , apparent density is 1.02g / cm 3 It was.
[0060] Example 7 A vulcanized fiber was obtained in the same manner as in Example 1, except that the number of base paper sheets was changed from 10 to 8, and the temperature of the aqueous zinc chloride solution was changed from 69° Be and 44° C. to 67° Be and 30° C. The basis weight of the vulcanized fiber after humidity conditioning was 853 g / m 2 , apparent density is 0.91g / cm 3 It was.
[0061] Example 8 A vulcanized fiber was obtained in the same manner as in Example 1, except that the softener was changed from a 50% aqueous solution of glycerin to a 50% aqueous solution of polyethylene glycol (reagent name: PEG400 / manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.). The basis weight of the vulcanized fiber after humidity conditioning was 1209 g / m 2 , apparent density is 1.02g / cm 3 It was.
[0062] Example 9 A vulcanized fiber was obtained in the same manner as in Example 1, except that the vulcanized fiber obtained in Example 7 was not engraved. The basis weight of the vulcanized fiber after humidity conditioning was 940 g / m 2 , apparent density is 1.04g / cm 3 It was.
[0063] Comparative Example 1 A vulcanized fiber was obtained in the same manner as in Example 1, except that engraving was not performed.
[0064] Comparative Example 2 A vulcanized fiber was obtained in the same manner as in Example 7, except that the fiber was not engraved or impregnated with glycerin. The basis weight of the vulcanized fiber after humidity conditioning was 803 g / m 2 , apparent density is 1.00g / cm 3 It was.
[0065] The compositions of the vulcanized fibers obtained in each of the Examples and Comparative Examples are shown in Figures 3 and 4, and the evaluation results are shown in Figure 5. Note that measurements and evaluations were made after the vulcanized fiber substrate was produced as described above in Figure 3, after engraving, and after softener impregnation and drying in Figure 5. The measurements and evaluations of the values shown in Figures 3 to 5 were made by the following methods.
[0066] <Thickness and density> The thickness and density of the vulcanized fiber were measured in accordance with JIS P 8118:14 Paper and paperboard-Test methods for thickness, density and specific volume.
[0067] <Basic weight> The thickness and density of the vulcanized fiber were measured in accordance with JIS P 8124:11 Paper and paperboard--Test method for basis weight.
[0068] <Measurement of Gurley stiffness> Measurements were carried out in the machine direction (MD) and cross direction (CD) of the vulcanized fiber in accordance with JAPAN TAPPI Paper and Pulp Test Method No. 40:2000 Paper and paperboard - Test method for stiffness under load bending - Gurley method.
[0069] <Measurement of tensile strength> Measurements were carried out in the machine direction (MD) and cross direction (CD) of the vulcanized fiber in accordance with JIS K7161-1 Plastics - Determination of tensile properties.
[0070] As is clear from the results shown in Fig. 5, the vulcanized fibers obtained in Examples 1 to 8 had excellent flexibility. In contrast, the vulcanized fiber obtained in Comparative Example 1 had poor flexibility, possibly due to insufficient impregnation with glycerin because it was not subjected to engraving processing with a laser processing machine. The vulcanized fiber obtained in Comparative Example 2 had poor flexibility because it was not impregnated with glycerin.
Claims
1. It contains a softener, is engraved, and has an apparent density including voids of 0.5 to 1.1 g / cm 3 and A vulcanized fiber characterized in that the rate of reduction in basis weight before and after engraving is in the range of 10 to 40%, and the depth of the depression in the cut portion by engraving is in the range of 30 to 95% of the thickness of the vulcanized fiber.
2. 2. The vulcanized fiber according to claim 1, characterized in that the softening agent is glycerin and / or polyethylene glycol.
3. a base paper preparation step of preparing a vulcanized fiber base paper; a gelatinization step of immersing the vulcanized fiber base paper in a reactive chemical to swell and gelatinize the surface of the vulcanized fiber base paper; a deliquation step of immersing the vulcanized fiber base paper in a solution having a lower concentration than the reactive chemicals to remove the reactive chemicals; a drying and finishing process for drying the vulcanized fiber base paper after the deliquor is removed to obtain a vulcanized fiber substrate; a softener impregnation step of impregnating the vulcanized fiber substrate with a softener; and a softener drying step of drying the vulcanized fiber substrate impregnated with the softener to obtain a vulcanized fiber. Further, the method includes an engraving step of providing engraving on the vulcanized fiber substrate or the vulcanized fiber, either between the drying / finishing step and the softener impregnation step, or after the softener drying step, The apparent density of the vulcanized fiber substrate, including the voids, is 0.5 to 1.1 g / cm 3 and A method for producing a vulcanized fiber, characterized in that the rate of reduction in basis weight before and after engraving is in the range of 10 to 40%, and the depth of the depression in the cut portion by engraving is in the range of 30 to 95% of the thickness of the vulcanized fiber.
4. 4. The method for producing vulcanized fiber according to claim 3, wherein the engraving step is performed between the drying / finishing step and the softening agent impregnation step.
Citation Information
Patent Citations
Carrier tape for small electronic parts and vulcanized fiber for carrier tape
JP1991084772U
Paper basket
JP1995298969A
Absorbent paper and method of manufacturing the same
JP2012152349A
Method of producing vulcanized fiber
JP2015089986A
file binder
JP3099092U