Electrode laminate and all-solid-state battery

By controlling the surface roughness of the base layer to 0.1-0.2 μm and pore diameter to 0.215-0.240 μm, the method addresses bubble generation and adhesion issues in all-solid-state battery manufacturing, resulting in improved interlayer adhesion and reduced bubble density for enhanced battery performance.

JP7553503B2Active Publication Date: 2024-09-18TOYOTA JIDOSHA KK +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2022075975
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2022-05-02
Publication Date
2024-09-18
Estimated Expiration
2042-05-02

AI Technical Summary

Technical Problem

In the manufacturing process of all-solid-state batteries, increasing the surface roughness of the base layer to enhance interlayer adhesion leads to the generation of air bubbles, which negatively affect battery performance.

Method used

Control the arithmetic mean height (Sa) of the first layer to be between 0.1 and 0.2 μm, allowing the slurry to penetrate deeply into the voids of the base layer, reducing bubble formation while maintaining sufficient interlayer adhesion by ensuring the maximum pore diameter is between 0.215 and 0.240 μm.

Benefits of technology

This approach reduces bubble density to less than 6 pieces/cm², thereby improving interlayer adhesive strength and enhancing battery performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007553503000004
    Figure 0007553503000004
  • Figure 0007553503000002
    Figure 0007553503000002
  • Figure 0007553503000003
    Figure 0007553503000003
Patent Text Reader

Abstract

To reduce air bubbles and increase the adhesion between layers.SOLUTION: A first layer is formed. A second layer is formed by applying a slurry on the surface of the first layer. The second layer is subjected to pressing processing so that an electrode laminate body is manufactured. The first layer is formed so that the relation of 0.1<Sa<0.2 is satisfied, in which Sa[μm] denotes the arithmetic average height of the surface of the first layer.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a method for producing an electrode laminate, a method for producing an all-solid-state battery, an electrode laminate, and an all-solid-state battery. [Background technology]

[0002] JP 2017-062938 A (Patent Document 1) discloses a solid electrolyte layer formed by applying a slurry onto an active material layer having a surface roughness Ra of 0.29 to 0.98 μm. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2017-062938 A Summary of the Invention [Problem to be solved by the invention]

[0004] For example, in the manufacturing process of an all-solid-state battery, an electrode laminate may be formed by repeatedly applying a slurry. The electrode laminate is subjected to a press process. If the interlayer adhesion is low, delamination may occur during the press process.

[0005] Conventionally, the anchor effect has been used to prevent delamination. That is, the surface roughness of the base layer (first layer) is increased. Part of the slurry is allowed to penetrate into the voids on the surface of the first layer. The upper layer (second layer) is formed as the slurry solidifies. An anchor part is formed as the slurry that has penetrated into the voids on the surface of the first layer solidifies. The formation of the anchor part is expected to improve the interlayer adhesion between the first and second layers.

[0006] However, it was recently discovered that increasing the surface roughness of the first layer can lead to the formation of air bubbles in the second layer, which can potentially reduce battery performance.

[0007] An object of the present disclosure is to reduce air bubbles while increasing interlayer adhesion. [Means for solving the problem]

[0008] The technical configuration and effects of the present disclosure will be described below. However, the mechanism of action in this specification includes assumptions. The mechanism of action does not limit the technical scope of the present disclosure.

[0009] 1. A method for producing an electrode laminate includes the following steps (a) to (c): (a) Form the first layer. (b) forming a second layer by applying a slurry onto the surface of the first layer; (c) The second layer is pressed to produce an electrode laminate. The first layer is represented by the following formula (1): 0.1 <Sa<0.2…(1) In the above formula (1), Sa represents the arithmetic mean height of the surface of the first layer. The unit of Sa is μm.

[0010] The arithmetic mean height (Sa) represents the three-dimensional surface roughness. When Sa becomes large, the slurry can penetrate deeply into the voids of the base layer (first layer). The penetration of the slurry causes gas to be pushed out of the voids. It is believed that the pushed out gas forms bubbles in the upper layer (second layer).

[0011] According to the new findings of the present disclosure, when Sa is less than 0.2 μm, it is expected that the number of bubbles will be reduced, and when Sa is more than 0.1 μm, it is expected that the interlayer adhesive strength will be improved.

[0012] 2. In the method for producing an electrode laminate described in "1." above, the first layer is represented by the following formula (2): 0.13≦Sa≦0.16…(2) The above relationship may be satisfied.

[0013] 3. In the method for producing an electrode laminate described in "1." or "2." above, the first layer may be, for example, an active material layer, and the second layer may be, for example, a solid electrolyte layer.

[0014] 4. A method for producing an all-solid-state battery includes the following (d): (d) A power generating element is formed, the power generating element including the electrode laminate produced by the method for producing an electrode laminate according to any one of "1." to "3.".

[0015] 5. The electrode laminate includes a first layer and a second layer. The second layer is laminated on the first layer. The first layer has a maximum pore size of 0.215 to 0.240 μm. The second layer has a pore size of 6 pores / cm. 2 has a bubble density of less than

[0016] The electrode laminate described in "5." above can be manufactured by, for example, the manufacturing method of the electrode laminate described in "1." above. The maximum pore size reflects the contact area at the interface between the first layer and the second layer. The larger the maximum pore size, the larger the contact area. By having a maximum pore size of 0.215 μm or more, improvement of interlayer adhesion is expected. By having a maximum pore size of 0.240 μm or less, reduction of air bubbles is expected. This allows for a pore size of 6 bubbles / cm. 2 A bubble density of less than 1000 nm can be achieved.

[0017] 6. In the electrode laminate described in "5." above, the first layer may be, for example, an active material layer, and the second layer may be, for example, a solid electrolyte layer.

[0018] 7. The all-solid-state battery includes a power generating element. The power generating element includes the electrode laminate described in "5." or "6."

[0019] Hereinafter, an embodiment of the present disclosure (hereinafter may be abbreviated as "the present embodiment") and an example of the present disclosure (hereinafter may be abbreviated as "the present embodiment") will be described. However, the present embodiment and the example do not limit the technical scope of the present disclosure. [Brief description of the drawings]

[0020] [Figure 1] Figure 1 shows an example of a second layer with bubbles. [Diagram 2] FIG. 2 is a schematic flow chart of the manufacturing method according to this embodiment. [Diagram 3] FIG. 3 is a conceptual diagram of an electrode laminate in this embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0021] <Terms and definitions> The words "comprise," "include," "have," and variations thereof (e.g., "consisting of") are open-ended. The open-ended form may or may not include additional elements in addition to the required elements. The words "consisting of" are closed-ended. However, the closed form does not exclude additional elements that are normally associated with the technology or that are unrelated to the technology disclosed. The words "consisting essentially of..." are semi-closed. The semi-closed form allows for the addition of elements that do not substantially affect the basic and novel characteristics of the technology disclosed.

[0022] Expressions such as "may" and "may" are used in the permissive sense, meaning "to have the possibility," rather than in the obligatory sense, meaning "to have to."

[0023] Elements expressed in the singular form include the plural form unless otherwise specified. For example, a "particle" can mean not only "one particle" but also "an aggregate of particles (powder, powder, particle group)."

[0024] For example, a numerical range such as "m to n%" includes the upper limit and the lower limit unless otherwise specified. That is, "m to n%" indicates a numerical range of "m% or more and n% or less". Furthermore, "m% or more and n% or less" includes "more than m% and less than n%". Furthermore, a numerical value arbitrarily selected from within the numerical range may be set as a new upper limit or lower limit. For example, a new numerical range may be set by arbitrarily combining a numerical value within the numerical range with a numerical value described in another part of this specification, in a table, in a figure, or the like.

[0025] All numerical values ​​are modified by the term "about." The term "about" may mean, for example, ±5%, ±3%, ±1%, etc. All numerical values ​​may be approximations that may vary depending on the application of the disclosed technology. All numerical values ​​may be expressed with significant figures. Measurements may be average values ​​of multiple measurements. The number of measurements may be three or more, five or more, or ten or more. In general, the more measurements are taken, the more reliable the average value is expected to be. Measurements may be rounded off based on the number of significant figures. Measurements may include errors associated with, for example, the detection limits of the measuring device.

[0026] Geometric terms (e.g., "parallel," "perpendicular," "orthogonal," etc.) should not be interpreted in a strict sense. For example, "parallel" may deviate slightly from the strict meaning of "parallel." Geometric terms may include, for example, tolerances, errors, etc. in design, work, manufacturing, etc. The dimensional relationships in each drawing may not match the actual dimensional relationships. In order to facilitate understanding of the disclosed technology, the dimensional relationships (length, width, thickness, etc.) in each drawing may be changed. Furthermore, some configurations may be omitted.

[0027] The term "principal surface" refers to the surface having the largest area among the outer surfaces of an object (e.g., a hexahedron).

[0028] If the compound has a stoichiometric formula (e.g., LiCoO 2When a stoichiometric formula is expressed by a formula such as "LiCoO ", the stoichiometric formula is merely a representative example of the compound. The compound may have a non-stoichiometric composition. For example, lithium cobalt oxide may be expressed by a formula such as "LiCoO 2 ", unless otherwise specified, the lithium cobalt oxide is not limited to the composition ratio of "Li / Co / O=1 / 1 / 2" and may contain Li, Co, and O in any composition ratio. Furthermore, doping or substitution with trace elements may also be permitted.

[0029] "D50" refers to the particle size at which the cumulative frequency from the smaller particle size side reaches 50% in the volume-based particle size distribution. D50 can be measured by a laser diffraction method.

[0030] The "arithmetic mean height (Sa)" is a value defined in ISO25178. Sa is measured in accordance with the standard. Sa can be measured by a laser microscope. For example, a laser microscope "VK-X3000" manufactured by Keyence Corporation may be used. The laser microscope may be substituted with a product equivalent to the "VK-X3000."

[0031] The "maximum pore diameter" is measured by the following procedure. The pore diameter distribution of the first layer is measured by mercury intrusion porosimetry. The pore diameter distribution is fitted to a normal distribution. The maximum pore diameter is calculated by the following formula (3). D max =μ+3σ…(3) D max indicates the maximum pore diameter. μ indicates the mean value of the normal distribution. σ indicates the standard deviation of the normal distribution.

[0032] The "cell density" is measured by the following procedure. The cells having a maximum Feret's diameter of 30 μm or more are counted on the main surface of the second layer after pressing. The number of cells is divided by the area of ​​the main surface of the second layer to obtain the cell density [cells / cm 2 Figure 1 shows an example of the second layer in which bubbles have occurred. A number of bubbles can be seen on the main surface of the second layer (the upper surface of the electrode laminate).

[0033] <Manufacturing method> FIG. 2 is a schematic flow chart of the manufacturing method in this embodiment. Hereinafter, the "manufacturing method in this embodiment" may be abbreviated as "this manufacturing method". This manufacturing method includes a "manufacturing method of an electrode laminate" and a "manufacturing method of an all-solid-state battery". The manufacturing method of an electrode laminate includes "(a) formation of a first layer", "(b) formation of a second layer", and "(c) press processing". The manufacturing method of an all-solid-state battery includes (a) to (c), and further includes "(d) formation of a power generating element".

[0034] (a) Formation of the first layer 3 is a conceptual diagram of an electrode laminate in this embodiment. This manufacturing method includes forming a first layer 10. The first layer 10 can be formed by any method. The first layer 10 may be formed, for example, by coating a first slurry.

[0035] For example, a substrate 11 may be prepared. The substrate 11 may be, for example, in the form of a sheet. The substrate 11 may have a thickness of, for example, 5 to 50 μm. The substrate 11 may be, for example, conductive. The substrate 11 may function as a current collector. The substrate 11 may include, for example, a metal foil. The substrate 11 may include, for example, at least one selected from the group consisting of aluminum (Al), nickel (Ni), chromium (Cr), copper (Cu), and iron (Fe).

[0036] For example, the first slurry may be prepared by mixing an active material, a conductive material, a solid electrolyte, a binder, and a dispersion medium. In this manufacturing method, any mixing device may be used. The first slurry is applied to the surface of the substrate 11. The first slurry is dried to form the first layer 10. That is, the first layer 10 may be an active material layer. In this manufacturing method, any coating device and drying device may be used.

[0037] After the first layer 10 is formed (after the first slurry is dried), the first layer 10 may be subjected to a press process. For example, a roll press machine may be used. The first layer 10 may have any thickness. After the press process, the first layer 10 may have a thickness of, for example, 10 to 200 μm.

[0038] <Three-dimensional surface height (Sa)> In this manufacturing method, the first layer 10 can be formed to have Sa greater than 0.1 μm and less than 0.2 μm. This is expected to improve interlayer adhesion and reduce air bubbles. Sa may be, for example, 0.13 μm or more, or 0.14 μm or more. Sa may be, for example, 0.16 μm or less, or 0.14 μm or less.

[0039] Sa may be adjusted by any method. For example, Sa may be adjusted by the particle size distribution of the constituent material of the first layer 10. For example, Sa may be adjusted by the roll linear pressure during press working. The roll linear pressure may be, for example, 0.2 t / cm or more, or 0.25 t / cm or more. The roll linear pressure may be, for example, 0.3 t / cm or less, or 0.25 t / cm or less.

[0040] <Active material> The active material is particulate. The active material may have a D50 of, for example, 1 to 30 μm. The active material may be, for example, a negative electrode active material. The negative electrode active material may be, for example, graphite, Si, SiO x (0 <x<2)、およびLi 4 Ti 5 O 12 may contain at least one selected from the group consisting of:

[0041] The active material may be, for example, a positive electrode active material. The positive electrode active material may be, for example, LiCoO 2 , LiNiO 2 , LiMnO 2 , LiMn 2 O 4 , Li(NiCoMn)O 2 , Li(NiCoAl)O 2 , and LiFePO 4 For example, "Li(NiCoMn)O 2"(NiCoMn)" in "Li(NiCoMn)O" indicates that the sum of the composition ratios in the parentheses is 1. As long as the sum is 1, the amount of each component is arbitrary. 2 For example, LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O 2 , LiNi 0.5 Co 0.2 Mn 0.3 O 2 , LiNi 0.8 Co 0.1 Mn 0.1 O 2 Li(NiCoAl)O 2 For example, LiNi 0.8 Co 0.15 Al 0.05 O 2 etc. may be included.

[0042] Conductive material The conductive material can form an electron conduction path. The amount of the conductive material may be, for example, 0.1 to 10 parts by mass with respect to 100 parts by mass of the active material. The conductive material may contain any component. The conductive material may contain, for example, at least one selected from the group consisting of carbon black (CB), vapor grown carbon fiber (VGCF), carbon nanotube (CNT) and graphene flake (GF).

[0043] <Solid electrolyte> The solid electrolyte can form an ion conduction path. The solid electrolyte is particulate. The solid electrolyte may have a D50 of, for example, 0.5 to 5 μm. The amount of the solid electrolyte may be, for example, 1 to 200 parts by volume per 100 parts by volume of the active material. The solid electrolyte may contain, for example, at least one selected from the group consisting of sulfides, oxides, and hydrides. The solid electrolyte may be, for example, LiI-LiBr-Li 3 P.S. 4 , Li 2 S-SiS 2 , LiI-Li 2 S-SiS 2 , LiI-Li 2 SP 2S 5 , LiI-Li 2 O-Li 2 SP 2 S 5 , LiI-Li 2 SP 2 O 5 , LiI-Li 3 PO 4 -P 2 S 5 , Li 2 SP 2 S 5 , and Li 3 P.S. 4 may contain at least one selected from the group consisting of:

[0044] For example, "LiI-LiBr-Li 3 P.S. 4 " is LiI, LiBr and Li 3 P.S. 4 The term "Li" refers to a solid electrolyte produced by mixing Li and Li in any molar ratio. For example, the solid electrolyte may be produced by a mechanochemical method. 2 SP 2 S 5 " is Li 3 P.S. 4 Includes: 3 P.S. 4 For example, Li 2 S and P 2 S 5 And "Li 2 S / P 2 S 5 =75 / 25 (molar ratio)". The solid electrolyte may be of the glass ceramic type or the argyrodite type.

[0045] <Binder> The binder can bind solid materials together. The amount of the binder may be, for example, 0.1 to 10 parts by mass with respect to 100 parts by mass of the active material. The binder may contain any component. The binder may contain, for example, at least one selected from the group consisting of polyvinylidene fluoride (PVdF), vinylidene fluoride-hexafluoropropylene copolymer (PVdF-HFP), styrene butadiene rubber (SBR), butadiene rubber (BR), and polytetrafluoroethylene (PTFE).

[0046] <Dispersion medium> The dispersion medium is a liquid. The dispersion medium may contain, for example, water, an organic solvent, etc. The dispersion medium may contain, for example, water, N-methyl-2-pyrrolidone, butyl butyrate, etc.

[0047] (b) Formation of the second layer The method includes forming a second layer 20 by applying a second slurry to a surface of the first layer 10 .

[0048] For example, the second slurry may be prepared by mixing a solid electrolyte, a binder, and a dispersion medium. The details of the solid electrolyte and the like are as described above. The solid electrolyte, binder, and dispersion medium of the first layer 10 and the second layer 20 may be the same or different.

[0049] The second slurry is applied to the surface of the first layer 10. The second slurry is dried to form the second layer 20. That is, the second layer 20 may be a solid electrolyte layer. The solid electrolyte layer may function as a separator in an all-solid-state battery.

[0050] In this manufacturing method, since Sa of the first layer 10 is more than 0.1 μm and less than 0.2 μm, it is expected that the second slurry will adequately soak into the surface of the first layer 10. In other words, it is expected that the interlayer adhesive strength will be improved and air bubbles will be reduced.

[0051] (c) Press processing The present manufacturing method includes manufacturing the electrode laminate 50 by applying press processing to the second layer 20. For example, a roll press machine may be used. The roll linear pressure may be lower when pressing the second layer 20 than when pressing the first layer 10. The roll linear pressure may be, for example, less than 0.2 t / cm or 0.1 t / cm or less. The roll linear pressure may be, for example, 0.01 t / cm or more.

[0052] The second layer 20 may have any thickness. After press working, the second layer 20 may be thinner than the first layer 10, for example. After press working, the second layer 20 may have a thickness of, for example, 5 to 50 μm.

[0053] (d) Formation of power generating elements The manufacturing method may include forming a power generating element 100 including an electrode laminate 50. For example, a third slurry may be applied to a surface of the second layer 20 to form a third layer 30. The third layer 30 may be, for example, an active material layer. The third layer 30 may have a polarity different from that of the first layer 10. For example, the first layer 10 may be a negative electrode active material layer, and the third layer 30 may be a positive electrode active material layer. For example, the first layer 10 may be a positive electrode active material layer, and the third layer 30 may be a negative electrode active material layer.

[0054] For example, the surface of the second layer 20 may also have an Sa of more than 0.1 μm and less than 0.2 μm. This is expected to improve the interlayer adhesive strength and reduce air bubbles between the second layer 20 and the third layer 30.

[0055] The number of layers in the electrode laminate 50 is arbitrary. For example, a fourth layer, a fifth layer (not shown), etc. may be further laminated on the third layer 30. After the formation of the third layer 30, each layer may be formed so that its surface has Sa of more than 0.1 μm and less than 0.2 μm.

[0056] The power generating element 100 may further include a current collector 31. The current collector 31 may include, for example, a metal foil or the like, similar to the substrate 11. For example, the current collector 31 may be attached to the outermost layer by an adhesive. Furthermore, an external terminal (not shown) may be connected to the current collector 31 and the substrate 11.

[0057] The power generating element 100 may be housed in an exterior body (not shown). The exterior body may have any shape. The exterior body may be, for example, a metal case or the like. The exterior body may be, for example, a pouch made of a metal foil laminate film or the like. In this manner, an all-solid-state battery can be manufactured.

[0058] In the present manufacturing method, as an example, a configuration in which the first layer 10 is an active material layer and the second layer 20 is a solid electrolyte layer is described. That is, the first layer 10 and the second layer 20 may be combined in any manner. For example, the first layer 10 may be a solid electrolyte layer and the second layer 20 may be an active material layer.

[0059] <All-solid-state battery> The all-solid-state battery includes a power generating element 100 (see FIG. 3). The all-solid-state battery may include a single power generating element 100, or may include two or more power generating elements. The multiple power generating elements 100 may form a parallel circuit or a series circuit.

[0060] The power generating element 100 may be housed in an exterior body (not shown). The power generating element 100 includes an electrode laminate 50. The power generating element 100 may further include a current collector 31 and the like. The electrode laminate 50 includes a first layer 10 and a second layer 20. The second layer 20 is laminated on the first layer 10. The electrode laminate 50 may further include a substrate 11, a third layer 30 and the like.

[0061] The first layer 10 has a maximum pore size of 0.215 to 0.240 μm. The second layer 20 has a maximum pore size of 6 pores / cm. 2 The bubble density is, for example, less than 3 bubbles / cm 2 May be less than 1 piece / cm 2May be less than or equal to 0 pieces / cm 2 The lower the bubble density, the more improved the battery performance (for example, output characteristics, etc.) is expected. EXAMPLES

[0062] <Sample preparation> Electrode laminates were produced according to the following Production Examples 1 to 5, respectively.

[0063] Example 1 Negative electrode active material (Li 4 Ti 5 O 12 A first slurry was prepared by mixing a powder of 0.1% by weight (D50=1.1 μm), a conductive material, a solid electrolyte, a binder, and a dispersion medium.

[0064] The first slurry was applied to the surface of a substrate (Al foil) and dried to form a first layer. The first layer was pressed using a roll press. The roll linear pressure was 0.1 t / cm. After pressing, the first layer had a thickness of 100 μm. After pressing, the Sa and maximum pore size of the first layer were measured.

[0065] Solid electrolyte (Li 3 P.S. 4 A second slurry was prepared by mixing a sintered body (sintered body, D50=2.2 μm) with a binder and a dispersion medium. The second slurry was applied to the surface of the first layer and dried to form the second layer. The second layer was pressed using a roll press. The roll linear pressure was 0.1 t / cm. After pressing, the presence or absence of delamination was confirmed. Furthermore, the bubble density of the second layer was measured. In this manner, an electrode laminate was manufactured.

[0066] <Production Examples 2-5> As shown in Table 1 below, an electrode laminate was produced in the same manner as in Production Example 1, except that the roll line pressure during press working of the first layer was changed.

[0067] [Table 1]

[0068] <Result> As shown in Table 1 above, when the Sa of the first layer exceeds 0.1 μm, delamination tends to be less likely to occur, and when the Sa of the first layer is less than 0.2 μm, the bubble density tends to decrease.

[0069] The present embodiment and the present embodiment are illustrative in all respects. The present embodiment and the present embodiment are not restrictive. The technical scope of the present disclosure includes all modifications within the meaning and scope equivalent to the description of the claims. For example, it is also intended from the beginning that any configuration may be extracted from the present embodiment and the present embodiment, and that they may be arbitrarily combined. [Explanation of symbols]

[0070] 10 first layer, 11 substrate, 20 second layer, 30 third layer, 31 current collector, 50 electrode laminate, 100 power generating element.

Claims

1. A first layer; A second layer; and Including, the second layer is laminated to the first layer; the first layer is an active material layer, the second layer is a solid electrolyte layer; The first layer has a maximum pore size of 0.215 to 0.240 μm; the arithmetic mean height of the surface of the first layer is 0.13 to 0.16 μm; In the second layer, the density of bubbles having a maximum Feret's diameter of 30 μm or more is 0 bubbles / cm2. Electrode stack.

2. Including a power generating element, The power generating element includes the electrode stack according to claim 1. All-solid-state battery.

Citation Information

Patent Citations

  • Methods for manufacturing electrode laminate and all-solid battery

    JP2017062938A

  • Method for manufacturing all-solid battery

    JP2019140042A

  • Positive electrode and lithium ion secondary battery

    JP2020140808A

  • All-solid-state lithium cell

    WO2015151566A1

  • Underground resource searching device and underground resource searching system

    WO2017002234A1