Rubber composition for tires and tires

A rubber composition for tires using vegetable globular protein effectively controls vulcanization and enhances mechanical strength, addressing the need for reduced PVI and efficient processing.

JP7553792B2Active Publication Date: 2024-09-19THE YOKOHAMA RUBBER CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2020164513
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-09-30
Publication Date
2024-09-19
Estimated Expiration
2040-09-30

AI Technical Summary

Technical Problem

The challenge is to develop a rubber composition for tires that reduces the use of N-(cyclohexylthio)phthalimide (PVI) while maintaining a suitable vulcanization rate and achieving high mechanical properties, particularly breaking strength, without compromising processing efficiency.

Method used

Incorporating a small amount of vegetable globular protein, such as zein, gluten, or soy protein, into the rubber composition, along with diene rubber and carbon black, to control the vulcanization process and enhance breaking strength.

Benefits of technology

The composition achieves an appropriate vulcanization time (T30) and high breaking strength, ensuring efficient processing and productivity, while minimizing PVI content.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007553792000002
    Figure 0007553792000002
  • Figure 0007553792000001
    Figure 0007553792000001
Patent Text Reader

Abstract

To provide a rubber composition for tires that has a T30 of proper length and shows high breaking strength after vulcanization, and a tire produced from the rubber composition for tires.SOLUTION: A rubber composition for tires contains a diene rubber, carbon black, and vegetable spherical protein. The content of the vegetable spherical protein is 0.01 pt.mass or more and less than 0.5 pt.mass relative to 100 pts.mass of the diene rubber.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a rubber composition for a tire and a tire. [Background technology]

[0002] When a tire is manufactured using a rubber composition, the rubber composition is usually vulcanized. If the vulcanization proceeds too quickly, processing becomes difficult, so a technique is known in which a vulcanization retarder is blended into the rubber composition to adjust the progress of vulcanization (for example, Patent Document 1). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2006-117781 A Summary of the Invention [Problem to be solved by the invention]

[0004] In recent years, the Chemical Substances Management Promotion Act (PRTR Act) has required a reduction in the amount of vulcanization retarder (N-(cyclohexylthio)phthalimide) (PVI) used in the examples of Patent Document 1. For this reason, there is a demand for rubber compositions for tires that contain a low amount of PVI (preferably no PVI) and that undergo vulcanization at an appropriate rate. Naturally, rubber compositions for tires are also required to have excellent mechanical properties (especially breaking strength) after vulcanization. Here, the progress of vulcanization can be evaluated, for example, by the vulcanization time (T30) (minutes) until 30% of the maximum torque is reached according to JIS K6300-2. If T30 is too short, processing becomes difficult, and conversely, if T30 is too long, productivity decreases. Therefore, it is desirable that T30 be of an appropriate length.

[0005] In view of the above circumstances, the present invention aims to provide a rubber composition for tires, which has an appropriate T30 and exhibits high breaking strength after vulcanization, and a tire manufactured using the rubber composition for tires. [Means for solving the problem]

[0006] As a result of extensive research into the above problems, the inventors discovered that the above problems could be solved by incorporating a small amount of vegetable globular protein, thereby completing the present invention. That is, the present inventors have found that the above problems can be solved by the following configuration.

[0007] (1) A rubber composition comprising a diene rubber, carbon black, and a vegetable globular protein, A rubber composition for tires, comprising the vegetable globular protein in an amount of 0.01 part by mass or more and less than 0.5 part by mass per 100 parts by mass of the diene rubber. (2) The rubber composition for a tire according to the above (1), wherein the vegetable globular protein is zein, gluten or soy protein. (3) The rubber composition for tires according to the above (1) or (2), wherein the content of the carbon black is 20 to 80 parts by mass per 100 parts by mass of the diene rubber. (4) A tire produced using the rubber composition for tires according to any one of (1) to (3) above. Effect of the Invention

[0008] As described below, according to the present invention, it is possible to provide a rubber composition for tires, which has an appropriate T30 and exhibits high breaking strength after vulcanization, and a tire manufactured using the rubber composition for tires. [Brief description of the drawings]

[0009] [Figure 1] 1 is a partial cross-sectional schematic view showing an example of an embodiment of a tire of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] The rubber composition for tires of the present invention and a tire produced using the rubber composition for tires will be described below. In this specification, a numerical range expressed using "to" means a range that includes the numerical values ​​before and after "to" as the lower and upper limits. In addition, each component contained in the rubber composition for tires of the present invention may be used alone or in combination of two or more. Here, when two or more types of each component are used in combination, the content of the component refers to the total content unless otherwise specified. The breaking strength after vulcanization is also simply called breaking strength. In addition, when T30 is of an appropriate length or when high breaking strength is exhibited, it is also said that the effects of the present invention are excellent.

[0011] [Rubber composition for tires] The rubber composition for tires of the present invention (hereinafter also simply referred to as the "composition of the present invention") has The rubber composition contains a diene rubber, carbon black, and a vegetable globular protein, The rubber composition for tires has a content of the vegetable globular protein of 0.01 part by mass or more and less than 0.5 part by mass per 100 parts by mass of the diene rubber.

[0012] It is believed that the composition of the present invention has the above-mentioned effects because of its constitution. Although the reason is not clear, it is speculated to be as follows.

[0013] As described above, the composition of the present invention contains a small amount of vegetable globular protein. The vegetable globular protein has a high proportion of amino groups present on the surface, which is believed to trap radicals during vulcanization and delay the vulcanization reaction. On the other hand, as shown in the Examples section below, the inventors' studies have shown that such a delay in the vulcanization reaction is not observed in the case of animal proteins or vegetable but fibrous proteins. This is believed to be because these proteins have a low proportion of amino groups present on the surface, have many functional groups containing sulfur atoms (which promote vulcanization), or have low compatibility with rubber components. In addition, since the content of vegetable globular protein in the present invention is small, the vulcanization time is not delayed too much. As a result, it is believed that the composition of the present invention has a moderate T30.

[0014] [Diene rubber] The diene rubber contained in the composition of the present invention is not particularly limited, and specific examples thereof include natural rubber (NR), butadiene rubber (BR), aromatic vinyl-conjugated diene copolymer rubber, isoprene rubber (IR), acrylonitrile-butadiene copolymer rubber (NBR), butyl rubber (IIR), halogenated butyl rubber (Br-IIR, Cl-IIR), and chloroprene rubber (CR). Examples of the aromatic vinyl-conjugated diene copolymer rubber include styrene-butadiene rubber (SBR) and styrene-isoprene copolymer rubber. Among these, natural rubber is preferred because the effect of the present invention is more excellent.

[0015] <Molecular weight> The weight average molecular weight (Mw) of the diene rubber is not particularly limited, but in order to obtain better effects of the present invention, it is preferably 100,000 to 5,000,000, more preferably 200,000 to 3,000,000, and even more preferably 300,000 to 2,000,000. In this specification, the weight average molecular weight (Mw) and number average molecular weight (Mn) are values ​​calculated as standard polystyrene by gel permeation chromatography (GPC).

[0016] [Carbon Black] The carbon black contained in the composition of the present invention is not particularly limited, and various grades such as SAF-HS, SAF, ISAF-HS, ISAF, ISAF-LS, IISAF-HS, HAF-HS, HAF, HAF-LS, and FEF can be used. The nitrogen adsorption specific surface area (N2SA) of the carbon black is not particularly limited, but is preferably 50 to 200 m because the effect of the present invention is more excellent. 2 / g, and 70 to 150m 2 It is more preferable that the molecular weight is / g. Here, the nitrogen adsorption specific surface area (N2SA) is the amount of nitrogen adsorbed on the surface of carbon black measured according to JIS K6217-2:2001 "Part 2: Determination of specific surface area - Nitrogen adsorption method - Single point method."

[0017] The content of the carbon black is not particularly limited, but in order to obtain better effects of the present invention, it is preferably 1 to 200 parts by mass, and more preferably 20 to 80 parts by mass, per 100 parts by mass of the diene rubber.

[0018] [Plant-derived globular proteins] The vegetable globular protein contained in the composition of the present invention is a vegetable globular protein. Here, globular protein is a general term for proteins that have a shape that approximates a sphere or a spheroid. Such proteins tend to have a spherical shape as a whole, with the polypeptide chain folded, a hydrophobic core formed by the hydrophobic amino acid side chains inside the molecule, and hydrophilic side chains on the surface of the molecule, which maintains the spherical shape. They also tend to disperse in a colloidal form in water. Whether or not a protein is globular may be judged by a method based on the translational friction coefficient, etc., as described in Biochemical Experiment Lecture 1: Protein Chemistry III: Higher-Order Structure Research Methods, p. 425 to p. 428, published by Tokyo Kagaku Dojin Co., Ltd. If the ratio of the translational friction coefficient f to the minimum translational friction coefficient f min is about f / f min = 1.1 to 1.3, the protein is judged to be globular.

[0019] The vegetable globular protein is preferably zein (corn protein), gluten or soy protein, and more preferably gluten or soy protein, because the effects of the present invention are superior.

[0020] The composition of the present invention may contain the above vegetable globular protein as a naturally derived product, for example, zein from corn (zein content: about 5% by mass), gluten from wheat (gluten content: about 6 to 15% by mass), and soy protein from soybeans or soybean flour (soy protein content: about 35% by mass).

[0021] <Content> In the composition of the present invention, the content of the vegetable globular protein is 0.01 parts by mass or more and less than 0.5 parts by mass per 100 parts by mass of the diene rubber. Among them, for the reason that the effect of the present invention is more excellent, it is preferably 0.1 parts by mass or more, more preferably more than 0.2 parts by mass, and even more preferably 0.3 parts by mass or more.

[0022] When the composition of the present invention contains a vulcanizing agent described below, the content of the vegetable globular protein is preferably 1 to 50 mass %, more preferably 5 to 30 mass %, and even more preferably 10 to 20 mass %, relative to the content of the vulcanizing agent, because this provides better effects of the present invention.

[0023] When the composition of the present invention contains a vulcanization accelerator described below, the content of the vegetable globular protein is preferably 1 to 50 mass%, more preferably 5 to 40 mass%, and even more preferably 15 to 30 mass%, based on the content of the vulcanization accelerator, because the effects of the present invention are more excellent.

[0024] [Optional ingredients] The composition of the present invention may contain components (optional components) other than the above-mentioned components, as necessary, to the extent that the effects and objects of the composition are not impaired. Examples of such components include various additives that are generally used in rubber compositions, such as silica, carbon black and fillers other than silica, silane coupling agents, terpene resins (preferably aromatic modified terpene resins), thermally expandable microcapsules, zinc oxide (zinc white), stearic acid, antioxidants, waxes, processing aids, process oils, liquid polymers, thermosetting resins, vulcanizing agents (e.g., sulfur), and vulcanization accelerators.

[0025] <Vulcanizing agent> The composition of the present invention preferably contains a vulcanizing agent (particularly sulfur) because the effect of the present invention is more excellent. In the composition of the present invention, the content of the vulcanizing agent is preferably 0.1 to 10 parts by mass, and more preferably 1 to 5 parts by mass, per 100 parts by mass of the diene rubber, because this provides better effects of the present invention.

[0026] <Vulcanization accelerator> The composition of the present invention preferably contains a vulcanization accelerator because the effect of the present invention is more excellent. The vulcanization accelerator is not particularly limited, but specific examples thereof include sulfenamide-based, thiazole-based, thiuram-based, thiourea-based, guanidine-based, dithiocarbamic acid-based, aldehyde-amine-based, aldehyde-ammonia-based, imidazoline-based, and xanthate-based vulcanization accelerators, which may be used alone or in combination of two or more. The vulcanization accelerator is preferably a sulfenamide-based (e.g., N-tert-butyl-2-benzothiazolyl sulfenamide). In the composition of the present invention, the content of the vulcanization accelerator is preferably 0.1 to 10 parts by mass, and more preferably 1 to 5 parts by mass, per 100 parts by mass of the diene rubber, because the effects of the present invention are more excellent. In addition, in the composition of the present invention, the content of the vulcanization accelerator is preferably 20 to 100 mass %, and more preferably 40 to 80 mass %, based on the content of the vulcanizing agent, because the effects of the present invention are more excellent.

[0027] [tire] The tire of the present invention is a tire manufactured using the above-mentioned composition of the present invention. The tire of the present invention is preferably a pneumatic tire, and can be filled with air, an inert gas such as nitrogen, or other gases. The tire of the present invention is preferably a studless tire.

[0028] Fig. 1 is a schematic partial cross-sectional view of a tire showing one example of an embodiment of a tire according to the present invention. However, the tire according to the present invention is not limited to the embodiment shown in Fig. 1.

[0029] In FIG. 1, reference numeral 1 denotes a bead portion, reference numeral 2 denotes a sidewall portion, and reference numeral 3 denotes a tire tread portion. Between the pair of left and right bead portions 1, a carcass layer 4 having fiber cords embedded therein is installed, and the ends of this carcass layer 4 are folded back and wrapped around the bead cores 5 and bead fillers 6 from the inside to the outside of the tire. In the tire tread portion 3, a belt layer 7 is disposed on the outer side of the carcass layer 4 over one circumference of the tire. In addition, a rim cushion 8 is disposed in the bead portion 1 at a portion that comes into contact with the rim. At least any one of the reference numerals 2 to 3, 5 to 6, and 8 is formed from the above-mentioned composition of the present invention.

[0030] The tire of the present invention can be manufactured, for example, according to a conventionally known method. The gas to be filled in the tire can be normal air or air with an adjusted oxygen partial pressure, or an inert gas such as nitrogen, argon, or helium. EXAMPLES

[0031] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.

[0032] [Preparation of rubber composition for tires] The components shown in Table 1 below were mixed in the ratios (parts by mass) shown in the same table. Specifically, the components shown in Table 1 below, excluding sulfur and a vulcanization accelerator, were first heated to about 140°C using a 1.7-liter internal Banbury mixer, mixed for 5 minutes, then discharged and cooled to room temperature to obtain a master batch. Furthermore, sulfur and a vulcanization accelerator were mixed into the obtained master batch using the Banbury mixer to obtain a rubber composition for tires.

[0033] 〔evaluation〕 The obtained rubber compositions for tires were evaluated as follows.

[0034] <t30> For the obtained rubber composition for tires, the vulcanization time (T30) (minutes) until 30% of the maximum torque was reached was measured in accordance with JIS K6300-2. The results are shown in Table 1. In practice, T30 is preferably from 2.5 to 10.0 minutes, more preferably from 3.0 to 9.0 minutes, and even more preferably from 4.0 to 8.0 minutes.

[0035] <Breaking strength> The obtained rubber composition for tires was press-vulcanized in a mold (15 cm × 15 cm × 0.2 cm) at 160°C for 15 minutes to produce a vulcanized rubber sheet. Next, a JIS No. 3 dumbbell-shaped test piece (thickness 2 mm) was punched out of the obtained vulcanized rubber sheet in accordance with JIS K6251:2010, and the breaking strength was evaluated under conditions of a temperature of 20°C and a tensile speed of 500 mm / min. The results are shown in Table 1. The results are expressed as an index with Comparative Example 1 being 100. In practice, a value of 95 or more is preferable.

[0036] [Table 1]

[0037] In Table 1, the details of each component are as follows. ·NR:TSR20 (natural rubber, glass transition temperature: -62℃) Carbon black: Show Black N339 (Cabot Japan) Stearic acid: Beads stearic acid (NOF Corporation) Zinc oxide: 3 types of zinc oxide (manufactured by Seido Chemical Industry Co., Ltd.) Sulfur: Kinkaji oil-filled fine sulfur (sulfur content 95.24% by mass, manufactured by Tsurumi Chemical Industry Co., Ltd.) Vulcanization accelerator: Sancerer NS-P (manufactured by Ouchi Shinko Chemical Industry Co., Ltd.) (N-tert-butyl-2-benzothiazolyl sulfenamide) · Vulcanization retarder: N-(cyclohexylthio)phthalimide (PVI) · Plant Globular Protein 1: Gluten · Plant-based globular protein 2: Soy protein Animal protein: casein · Plant-based fibrous protein: Coconut fiber (plant-based fibrous protein)

[0038] As can be seen from Table 1, Examples 1 to 3, which contained vegetable globular protein, had an appropriate T30 length and exhibited high breaking strength. Comparing Examples 1 and 2 (comparison between embodiments containing gluten as the vegetable globular protein), Example 2, in which the vegetable globular protein content was more than 0.2 parts by mass per 100 parts by mass of diene rubber, showed a more appropriate T30 length and higher breaking strength.

[0039] On the other hand, Comparative Example 1, which does not contain vegetable globular protein, had a short T30. Comparative Examples 3 and 4, which contain vegetable globular protein but the content is 0.5 parts by mass or more per 100 parts by mass of diene rubber, had a long T30, which was not a suitable length, and had a low breaking strength. Comparative Example 5, which contains animal protein instead of vegetable globular protein, and Comparative Example 6, which contains vegetable fibrous protein instead of vegetable globular protein, had a short T30 and a low breaking strength. [Explanation of symbols]

[0040] 1 Bead section 2 Sidewall 3 Tire tread 4 Carcass layer 5 Bead Core 6 Bead Filler 7 Belt layer 8 Rim cushion

Claims

1. Contains diene rubber, carbon black, and gluten, A rubber composition for tires, wherein the gluten content is 0.01 parts by mass or more and less than 0.5 parts by mass per 100 parts by mass of the diene rubber; The rubber composition contains a diene rubber, carbon black, and a vegetable globular protein, A rubber composition for tires (excluding compositions containing gluten), comprising the vegetable globular protein in an amount of 0.01 part by mass or more and less than 0.5 part by mass per 100 parts by mass of the diene rubber.

2. 2. The rubber composition for a tire according to claim 1, wherein the vegetable globular protein is zein or soy protein.

3. 3. The rubber composition for tires according to claim 1, wherein the content of the carbon black is 20 to 80 parts by mass based on 100 parts by mass of the diene rubber.

4. A tire produced using the rubber composition for tires according to any one of claims 1 to 3.

Citation Information

Patent Citations

  • Rubber composition

    JP1981166243A

  • Rubber composition for tire

    JP2006117781A

  • Rubber composition for tire and pneumatic tire

    JP2009114250A

  • Rubber composition for winter tire treads

    JP2011508029A

  • Method and formulation for reinforcing elastomers

    JP2014062269A