Method for producing cellulose-based molded body, cellulose-based molded body obtained by said method, and dental mill blank

By modifying CNF with polymerizable groups to form crosslinked structures, the molded products achieve enhanced water resistance and strength, addressing the weakness of conventional CNF products in wet environments, suitable for dental mill blanks.

JP7553897B2Active Publication Date: 2024-09-19TOKUYAMA DENTAL CORP +2
View PDF 16 Cites 0 Cited by

Patent Information

Application Number
JP2020139964
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-08-21
Publication Date
2024-09-19
Estimated Expiration
2040-08-21

Smart Images

  • Figure 0007553897000004
    Figure 0007553897000004
  • Figure 0007553897000001
    Figure 0007553897000001
  • Figure 0007553897000002
    Figure 0007553897000002
Patent Text Reader

Abstract

To provide a cellulose-based molded body having sufficient mechanical strength substantially without containing a petroleum-derived material, and having such water resistance as not showing reduction of strength even when using in an oral cavity for a long period of time.SOLUTION: A method of producing a cellulose-based molded body comprises: preliminarily modifying CNF contained in the dispersed liquid so as to substitute 0.1-1 of hydroxyl group per 1 glucose unit with a group having a polymerizable group; and closely fitting a CNF constituent onto molding surfaces under a condition of polymerizing a polymerizable group, when obtaining a molded body by feeding a dispersed liquid of cellulose nanofiber (CNF) on the molding surfaces of a female mold and / or a male mold, and closely fitting the CNF constituent onto the molding surfaces under the condition of polymerizing the polymerizable group while distilling off a dispersion medium.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a cellulose-based molded article that is substantially free of synthetic resin and that can be suitably used as a dental mill blank, and to a cellulose-based molded article produced by said method. [Background technology]

[0002] Cellulose nanofibers (hereinafter sometimes abbreviated as "CNF") are biomass materials with low environmental impact, and have excellent properties such as light weight, high strength, and low thermal expansion coefficient (see Patent Documents 1 and 2). For this reason, they are often used as reinforcing fibers for fiber-reinforced materials (see Patent Documents 3 and 4), and there are also known examples of them being incorporated into dental hardenable compositions (see Patent Document 5).

[0003] In recent years, a technique for producing a molded body substantially composed of only CNF has also been developed (see Patent Documents 6 and 7). For example, Patent Document 6 describes a method for forming a three-dimensional CNF, which is characterized by filling a mold at least partially using a steam permeation means with a slurry containing only CNFs having an average thickness of 4 to 200 nm and an average length of 0.1 μm or more as cellulose-derived fiber components, and applying a load to the slurry by the mold and / or a steam permeation means other than the mold, while heating and / or reducing the pressure, and concentrating the slurry. Patent Document 7 describes a CNF molding device that applies a load to a cellulose nanofiber (CNF)-containing slurry using a steam permeation means that allows steam to permeate the slurry, the CNF molding device being provided with a mold that forms a molding cavity with a main body and a bottom plate, and having a CNF injection means for the molding cavity, the bottom plate being capable of being fitted inside the main body, and having a pressurizing means that pressurizes the main body in the direction of the bottom plate.

[0004] Dental materials made of molded bodies obtained by such techniques are also known. For example, the above-mentioned Patent Document 7 describes a method in which a slurry of cellulose nanofibers (CNFs) containing a crosslinking agent such as isocyanate acrylate and a polymerization initiator is fed to the CNF molding device, and the molded body obtained is cut to produce a dental base for a complete denture.

[0005] Meanwhile, in dental treatment, the use of digital technology is progressing in the manufacture of dental prostheses such as inlays, onlays, crowns, bridges, and implant superstructures, and dental prosthetic devices such as dentures and denture bases. For example, as disclosed in Patent Document 8, a CAD / CAM system is being widely used, which uses a CAD / CAM device based on computer aided design (CAD) and computer aided manufacturing (CAM) technology to cut a dental mill blank (hereinafter also referred to as a "dental mill blank") made of a nonmetallic material from an image of the oral cavity to form a dental prosthesis, etc. Here, the dental mill blank means a cut object that can be attached to a cutting machine in a CAD / CAM system, and generally known examples include a (solid) block formed into a rectangular or cylindrical shape, or a (solid) disk formed into a plate or plate shape.

[0006] Various materials such as glass ceramics, zirconia, titanium, resin, etc. are used as the material to be machined in dental mill blanks. Among these, resin-based materials consisting of a hardened product of a hardening composition containing an inorganic filler such as silica, a polymerizable monomer such as methacrylate resin, and a polymerization initiator have attracted attention due to their high workability (machinability), high aesthetics, strength, etc. (see Patent Document 9). [Prior art documents] [Patent documents]

[0007] [Patent Document 1] JP 2015-142900 A [Patent Document 2] JP 2017-205683 A [Patent Document 3] JP 2005-60680 A [Patent Document 4] JP 2007-51266 A [Patent Document 5] Patent No. 6432983 [Patent Document 6] Patent No. 6460737 [Patent Document 7] International Publication No. 2018 / 207945 [Patent Document 8] Special Publication No. 2016-535610 [Patent Document 9] International Publication No. 2012 / 042911 Summary of the Invention [Problem to be solved by the invention]

[0008] In recent years, with the rise in environmental awareness, efforts to reduce the use of petroleum have been given importance. Resin-based dental materials such as those described in Patent Document 9 have problems such as not decomposing and remaining in the environment when discarded in nature, or emitting carbon dioxide and in some cases harmful gases when incinerated, and although the amount used in dental applications is small, it is required to reduce the amount of petroleum-derived resin components used as much as possible from the above perspective. As described above, cellulose nanofiber (CNF) is a biomass material with low environmental impact, and the molded body disclosed in Patent Document 7 has good mechanical properties such as bending strength, is hydrophobic and has low water absorption, so it is thought that it could be a dental material that meets such requirements. However, as described in the Comparative Example below, 2As shown in the figure, it was found that the molded body produced in the same manner as in Patent Document 7 has high strength, but the strength may decrease after immersion in water. In other words, the molded body (for producing the dental base of a complete denture) disclosed in Patent Document 7 can be said to correspond to a dental mill blank, but when considering its use in the oral cavity, there is a possibility that its strength may decrease, and it became clear that there is room for improvement in terms of water resistance.

[0009] Therefore, the present invention aims to provide a cellulose-based molded body that is substantially free of petroleum-derived materials, has sufficient mechanical strength, and has water resistance such that no decrease in strength is observed even when used for a long period of time in the oral cavity, and further to provide a dental mill blank made of such a cellulose-based molded body. [Means for solving the problem]

[0010] As a result of extensive investigations into how to improve the water resistance of the molded body disclosed in Patent Document 7, the inventors discovered that the water resistance of the resulting molded body is improved when a dispersion in which a CNF component containing modified CNF in which at least a portion of the hydroxyl groups of cellulose nanofiber (CNF) have been replaced with "groups having a polymerizable group" is dispersed in a dispersion medium is used as the cellulose nanofiber (CNF) slurry used as the raw material, and this led to the completion of the present invention.

[0011] That is, the first aspect of the present invention is a method for producing a molded body of a cellulose-based material, characterized in that it comprises a molding step of supplying a raw material slurry consisting of a dispersion in a dispersion medium containing cellulose nanofibers (CNFs) including modified CNFs in which at least a portion of the hydroxyl groups of the CNFs have been replaced with "groups having a polymerizable group", the CNF components contained in the dispersion having a degree of substitution, defined as "the average number of substituted hydroxyl groups per glucose unit", of 0.1 or more and 1.0 or less, to the molding surfaces of a female mold (concave mold) and / or a male mold (convex mold), and obtaining a molded body by adhering the CNF components to the molding surfaces under conditions in which the polymerizable groups polymerize while evaporating off the dispersion medium.

[0012] In the above-mentioned production method, it is preferable that the raw material slurry contains a polymerization initiator capable of polymerizing the polymerizable group. It is also preferable that the method further includes a raw material slurry preparation step including a CNF component preparation step in which a polymerizable group-containing hydroxyl group-reactive compound consisting of a compound having a "polymerizable group" and a "functional group capable of reacting with a hydroxyl group to form a bond" in the molecule is reacted with CNF to obtain the CNF component, and it is particularly preferable that the polymerizable group-containing hydroxyl group-reactive compound is used in an amount of 0.2 (mmol / g) or more and 7 (mmol / g) or less per unit mass of CNF in the CNF component preparation step.

[0013] A second aspect of the present invention is a molded article of a cellulosic material obtained by the production method according to the first aspect of the present invention.

[0014] In the molded article of the cellulose-based material, it is preferable that 95% or more by mass of the organic components constituting the cellulose-based material are cellulose derived from polysaccharides. Furthermore, in the molded article of the cellulose-based material, in the bending strength δ calculated by the formula: δ = 3Fl / 2bh2 {where F represents the maximum load during the bending test, l represents the distance between the supports (50.0 mm), b represents the width of the test piece (10.0 mm), and h represents the thickness of the test piece (3.0 mm)} in a three-point bending test according to ISO20795-1, when the bending strength δ0 measured using a test piece that is not in contact with water is defined as δ0, and the bending strength δ1 measured using a test piece that has been immersed in water at 37°C for one week is defined as δ1, the bending strength retention rate R defined by the formula: R = δ1 / δ0 is preferably 0.90 or more.

[0015] Further, a third aspect of the present invention is a dental mill blank comprising the molded article of the cellulose-based material according to the second aspect of the present invention. Effect of the Invention

[0016] According to the manufacturing method of the present invention, it is possible to produce a cellulose-based molded body that is substantially free of petroleum-derived materials, has sufficient mechanical strength, and has water resistance such that no decrease in strength is observed even when used in the oral cavity for a long period of time.

[0017] Furthermore, the cellulose-based molded body of the present invention obtained by the manufacturing method of the present invention is substantially free of petroleum-derived materials and not only has sufficient mechanical strength, but is also a novel molded body of a cellulose-based material that is superior in water resistance to the molded body disclosed in Patent Document 7, probably due to differences in microstructure resulting from differences in the manufacturing method, and can be suitably used as a dental mill blank. [Brief description of the drawings]

[0018] [Figure 1] This figure is a schematic diagram of a molding apparatus that can be suitably used in the manufacturing method of the present invention, and corresponds to the schematic diagram of the CNF molding apparatus shown as Figure 1 in Patent Document 7. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0019] The manufacturing method of the present invention is characterized by comprising a molding step of supplying a raw material slurry consisting of a dispersion in which a CNF component containing modified CNF in which at least a part of the hydroxyl groups of cellulose nanofibers (CNF) is substituted with a "group having a polymerizable group" is dispersed in a dispersion medium, and the CNF component contained in the dispersion has a substitution degree of 0.1 or more, defined as the "average number of hydroxyl groups substituted per glucose unit," to the molding surfaces of a female mold (concave mold) and / or a male mold (convex mold), and while evaporating off the dispersion medium, the CNF component is brought into close contact with the molding surfaces under conditions in which the polymerizable groups are polymerized, thereby obtaining a molded body. More specifically, as shown in Patent Documents 6 and 7, a molding technique such as "introducing the CNF slurry into a cavity formed between a female mold and a male mold, and molding by applying a load while concentrating the CNF by evaporating off the dispersion medium" is characterized in that a specific slurry (the raw material slurry) is used as the CNF slurry used as a raw material.

[0020] That is, in Patent Document 6, a CNF slurry in which CNF derived from natural plant polysaccharides is dispersed in water and / or an organic solvent is used as the CNF slurry used as the raw material, and in Patent Document 7, a slurry in which a metal salt such as magnesium ion, pulp, a crosslinking agent such as isocyanate acrylate, and a polymerization initiator are mixed with such a CNF slurry as necessary is used, whereas in the manufacturing method of the present invention, a raw material slurry in which CNF components including modified CNF in which a predetermined number of hydroxyl groups of CNF are substituted with "groups having polymerizable groups" are dispersed in a dispersion medium is used. And, by using such a raw material slurry, it has been successful in obtaining the effect of improving the water resistance of the obtained molded body of the cellulose-based material.

[0021] The mechanism by which such an effect is obtained is not entirely clear, but the present inventors presume that it is due to the following: In other words, in the technology of Patent Document 6, which uses a slurry in which only unmodified CNF is dispersed, when a load is applied, the fine fibers of the CNF are crosslinked with each other by the formation of hydrogen bonds between hydroxyl groups present on the CNF surface, so that in a dry state the bonds between the CNF fibers are strong and provide high mechanical strength, but after immersion in water, water molecules penetrate between the hydrogen bonds of the CNF fibers, inhibiting the bonds between the CNF fibers, and a decrease in mechanical strength is unavoidable. In addition, in the technology of Patent Document 7, which uses a slurry in which a crosslinking agent such as isocyanate acrylate and a polymerization initiator are mixed with a slurry in which unmodified CNF is dispersed, the reaction between CFN (hydroxyl group) and the crosslinking agent and the polymerization of the polymerizable group of the crosslinking agent do not occur in the slurry, and these reactions proceed all at once due to heating when a load is applied. Therefore, it is believed that although the water absorption rate of the molded body can be reduced, a crosslinking density sufficient to maintain the strength after immersion in water could not be obtained. In contrast, the CNF component contained in the raw material slurry used in the manufacturing method of the present invention has a certain percentage of its hydroxyl groups uniformly substituted with "groups having polymerizable groups" in advance, and since only the polymerization reaction of the polymerizable groups occurs during molding, crosslinks are formed uniformly and sufficiently, and water resistance is improved.

[0022] The molded article of the present invention obtained by the manufacturing method of the present invention is a novel molded article having an excellent characteristic not seen in conventional CNF molded articles, namely high water resistance, even though most of the organic components of the molded article (preferably 95% by mass or more) are made of CNF derived from polysaccharides including natural plants. Such excellent characteristics are believed to be due to the fact that it has structural characteristics (which are difficult to determine by analysis), such as a novel crosslinked structure, which are derived from the manufacturing method described above. This structural characteristic can be determined by its specific physical properties, namely, by the formula: δ=3Fl / 2bh, as determined by a three-point bending test according to ISO20795-1. 2{In the formula, F represents the maximum load during the bending test, l represents the distance between supports (50.0 mm), and b represents trial where m is the test piece width (10.0 mm), and h is the test piece thickness (3.0 mm).} where m is the test piece width (10.0 mm), and h is the test piece thickness (3.0 mm), and where m is the test piece width (10.0 mm), and h is the test piece thickness (3.0 mm), the bending strength retention rate R defined by the formula R=δ1 / δ0 is preferably 0.90 or more.

[0023] The present invention will be described in detail below. In this specification, unless otherwise specified, the expression "x to y" using numerical values ​​x and y means "greater than or equal to x and less than or equal to y." In such an expression, when a unit is added only to the numerical value y, the unit is also applied to the numerical value x.

[0024] 1. The manufacturing method of the present invention As described above, the manufacturing method of the present invention is characterized most by the use of a specific raw material slurry. The molding method in the manufacturing method of the present invention is to supply the raw material slurry to the molding surface of a female mold (concave mold) and / or a male mold (convex mold), and while evaporating off the dispersion medium, to mold the CNF component by adhering it to the molding surface under conditions in which the polymerizable group is polymerized. However, except for the requirement that molding be performed under conditions in which the polymerizable group is polymerized, a method such as that described in Patent Documents 6 and 7 in which "CNF slurry is introduced into a cavity formed between a female mold and a male mold, and a load is applied while concentrating the CNF by evaporating off the dispersion medium to mold" can also be adopted. Therefore, first, the raw material slurry will be explained, and then the molding process will be explained while citing the prior art.

[0025] 1-1 About the raw material slurry In the present invention, as the CNF slurry used as a raw material, a dispersion in which a CNF component containing a modified CNF in which at least a part of the hydroxyl groups of the CNF is substituted with a "group having a polymerizable group" is dispersed in a dispersion medium, and in the CNF component contained in the dispersion, a raw material slurry composed of a dispersion having a substitution degree of 0.1 to 1.0, defined as the "average number of substituted hydroxyl groups per glucose unit", is used.

[0026] <CNF Component Preparation Step and Raw Material Slurry Preparation Step> The above raw material slurry reacts a polymerizable group-containing hydroxyl group-reactive compound composed of a compound having a "polymerizable group" and a "functional group capable of reacting with a hydroxyl group to form a bond" in the molecule with CNF, and at least a part of the hydroxyl groups of the CNF is substituted with a "group having a polymerizable group" (hereinafter, performing such substitution is also referred to as "chemically modifying the hydroxyl groups of CNF"), and the modified CNF into which the "group having a polymerizable group" is introduced can be preferably obtained by a raw material slurry preparation step including a CNF component preparation step for obtaining the CNF component.

[0027] <Cellulose Nanofiber (CNF)> As the CNF used in the above CNF component preparation step, those available industrially or as reagents can be used without particular limitation. From the viewpoint of forming stronger bonds between CNFs and the cost and labor required for CNF fibrillation, those having an average fiber width of 3 to 200 nm and an average fiber length of 0.1 to 5.0 μm, and further, those having an average fiber width of 3 nm to 80 nm, particularly 5 nm to 50 nm, are more preferably used. Also, from the viewpoint of the rigidity and strength of the CNF fibers themselves, those having a crystallinity of 50% or more are more preferably used. Such CNFs are formed, for example, by fibrillating cellulose with high-pressure water jets. The average fiber width and average fiber length can be measured using an electron microscope or the like.

[0028] Such CNFs can be obtained by defibrating pulp to nano size. The defibrating method of pulp is not particularly limited as long as it is a known method, and examples thereof include chemical treatments such as TEMPO oxidation, enzymatic hydrolysis, and ion-selective liquid dissolution, and mechanical treatments such as underwater confrontation collision, water pressure through-pulverization, high-pressure homogenizer, microfluidizer, grinder, biaxial kneading, and ball mill grinding. These methods may also be combined for defibration. For example, a method of impinging high-pressure water of about 50 to 400 MPa against cellulose fibers suspended in 0.5 to 10% by mass of water, such as the underwater confrontation collision treatment method described in Patent Document 2, the wet pulverization method of polysaccharides described in Patent Document 7, and the nano-fine product manufacturing method described in Patent Document 1, can be suitably used.

[0029] The raw pulp of CNF is not particularly limited as long as it is a known material, and any material can be used. For example, pulp derived from polysaccharides including natural plants such as wood fiber, bamboo fiber, sugarcane fiber, seed hair fiber, leaf fiber, and seaweed can be mentioned. In addition, it may be produced from crop residues derived from leaves, flowers, stems, roots, and husks of plants such as bagasse, rice straw, used tea leaves, and squeezed fruit juice residue, and these raw materials may be used alone or in combination of two or more. As the raw pulp, it is preferable to use pulp with an α-cellulose content of 60% to 99 wt%. If the purity is 60 wt% or more of α-cellulose content, it is easy to adjust the fiber width and fiber length, and entanglement between fibers can be suppressed, and the coloring suppression effect is better than when using α-cellulose content less than 60 wt%.

[0030] <Polymerizable group-containing hydroxyl group-reactive compound> The polymerizable group-containing hydroxyl group-reactive compound used in the present invention is not particularly limited as long as it is a compound having a "polymerizable group" and a "functional group capable of reacting with a hydroxyl group to form a bond". Here, the polymerizable group means a group that causes a polymerization reaction, and from the viewpoint of high reactivity and easy densification of the cross-linked structure between CNF fibers, it is more preferably a radically polymerizable group such as an acryloxy group or a methacryloxy group. Examples of the "functional group capable of reacting with a hydroxyl group to form a bond" include an isocyanate group, an acid halogen group, a silanol group, an alkoxysilane, an acid anhydride, an ester group, and an epoxy group. From the viewpoint of high reactivity with a hydroxyl group and enabling more efficient chemical modification, an isocyanate group, an alkoxysilane, an epoxy group, or an acid halogen group is preferable.

[0031] The polymerizable group-containing hydroxyl group-reactive compound includes "a compound having a functional group capable of forming a covalent bond with PVA such as an isocyanate group and an epoxy group, and having a radically polymerizable functional group of a carbon-carbon double bond such as a (meth)acryloyl group and a vinyl group", which is used as a cross-linking agent in Patent Document 7, 2-isocyanatoethyl acrylate (manufactured by Showa Denko KK, product name: Karenz AOI); 1,1-(bisacryloyloxymethyl)ethyl isocyanate (manufactured by Showa Denko KK, Karenz BEI); a reaction product of 2-hydroxyethyl acrylate and a polymer composed of 1,6-diisocyanatohexane as constituent components (manufactured by BASF SE, product name: Laromer LR9000), etc. Examples of the polymerizable group-containing hydroxyl group-reactive compound that can be preferably used in the present invention include compounds represented by the following structural formula. In the following structural formula, n means an integer of 0 to 10.

[0032]

Chemical formula

[0033] <Reaction in the CNF component preparation process> In the CNF component preparation step, CNF is reacted with a polymerizable group-containing hydroxyl group-reactive compound to obtain a CNF component containing modified CNF in which at least a portion of the hydroxyl groups of CNF are substituted with "groups having a polymerizable group." Note that the CNF component only needs to have an overall degree of substitution (the degree of substitution will be described later) of 0.1 to 1.0, and it is not necessary that all of the individual CNFs constituting the CNF component are modified CNFs.

[0034] The reaction between CNF and a polymerizable group-containing hydroxyl group-reactive compound can be carried out by adding a predetermined amount of the polymerizable group-containing hydroxyl group-reactive compound to a slurry in which CNF is dispersed in a dispersion medium made of an organic solvent, and mixing the compound. The organic solvent that serves as the dispersion medium (which can also serve as a reaction solvent) is not particularly limited as long as it has a moderate hydrophilicity to the extent that the CNF fibers do not aggregate and does not inhibit the reaction, and for example, acetone, tetrahydrofuran, dimethylformamide, N-methylpyrrolidone, dioxane, etc. can be used. From the viewpoint of facilitating the distillation of the dispersion medium (reaction solvent) in the subsequent process, it is preferable to use acetone or tetrahydrofuran, which have a low boiling point. Since CNF is usually obtained as a slurry in which water is the dispersion medium, the dispersion medium can be changed from water to an organic solvent by performing a process of adding an organic solvent to the CNF water slurry and distilling it off using an evaporator multiple times. In addition, as a method of replacing with an organic solvent, the water slurry of CNF can also be replaced by filtering while washing with the organic solvent to be replaced, and suspending the residue on the filter paper in the organic solvent. The organic solvent may contain water to the extent that the reaction is not inhibited.

[0035] The amount of the dispersion medium (reaction solvent) is preferably selected in the range of 100 / 5 to 100 / 0.01 in terms of the ratio to the dry mass of CNF, i.e., dispersion medium mass / CNF dry mass. From the viewpoints of maintaining a viscosity that does not reduce the stirring efficiency and reaction efficiency, the amount of dispersion medium mass / CNF dry mass is more preferably in the range of 100 / 3 to 100 / 0.1, and even more preferably in the range of 100 / 2 to 100 / 0.5.

[0036] The reaction temperature of the above reaction may be below the boiling point of the organic solvent, but is preferably 40°C or higher, and more preferably 50°C or higher. In addition, the upper limit of the reaction temperature is not particularly limited as long as it is below the boiling point of the reaction solvent used. In addition, in the reaction step of CNF and the polymerizable group-containing hydroxyl group-reactive compound, a reaction catalyst that promotes the reaction of the hydroxyl group of CNF and the polymerizable group-containing hydroxyl group-reactive compound may be used. As the reaction catalyst, if the polymerizable group-containing hydroxyl group-reactive compound is an isocyanate, a tin catalyst such as dibutyltin dilaurate or an amine catalyst such as triethylamine can be used. If the polymerizable group-containing hydroxyl group-reactive compound is an epoxy, an acid catalyst such as sulfuric acid or a base catalyst such as triethylamine can be used. If the polymerizable group-containing hydroxyl group-reactive compound is an acid anhydride, an acid catalyst such as p-toluenesulfonic acid or a base catalyst such as dimethylaminopyridine can be used.

[0037] In the above reaction, the degree of substitution in the CNF component contained in the raw material slurry must be 0.1 to 1.0. Here, the degree of substitution (hereinafter sometimes abbreviated as "DS") means the average number of substituted hydroxyl groups per glucose unit. Since the number of hydroxyl groups per glucose unit in unsubstituted (unchemically modified) CNF is 3, for example, when the degree of substitution is 1.0, on average, one of these three hydroxyl groups is substituted with a "group having a polymerizable group", and when the degree of substitution is 0.1, on average, one of the 30 hydroxyl groups in 10 glucose units is substituted with a "group having a polymerizable group". In addition, it is known that if the degree of substitution of CNF becomes too large, the crystallinity of CNF is lost. Therefore, from the viewpoint of the water resistance and mechanical strength of the obtained molded body, the degree of substitution is preferably 0.2 to 1.0, more preferably 0.3 to 0.6.

[0038] The degree of substitution (DS) can be determined by quantifying the total amount (total number of moles) of “groups having a polymerizable group” introduced into the modified CNF in the CNF component and dividing it by the amount (total number of moles) of glucose units.

[0039] The total amount (total number of moles) of "groups having a polymerizable group" introduced into modified CNF in the CNF component can be determined by quantitatively hydrolyzing the ester bond using an aqueous sodium hydroxide solution, and quantifying the amount of acid produced by the hydrolysis or the amount of sodium hydroxide consumed by the hydrolysis, in the same manner as in determining the so-called "total degree of acetyl group substitution of cellulose acetate" for the CNF component containing modified CNF in which the "groups having a polymerizable group" are bonded to glucose units via ester bonds by the reaction of CNF with a polymerizable group-containing hydroxyl group-reactive compound. Alternatively, the hydroxyl groups of cellulose remaining in the CNF component can be propionylated, dissolved in deuterated chloroform, and quantified by NMR measurement.

[0040] Furthermore, for CNF components including modified CNFs in which the "groups having a polymerizable group" are bonded to glucose units through bonds that are not hydrolyzed by sodium hydroxide due to the above reaction, they may be quantified by NMR measurement in the same manner as above, but when the "groups having a polymerizable group" contain ester bonds that are quantitatively hydrolyzed by sodium hydroxide, they can be quantified by titration in the same manner as above. For example, when an isocyanate-(meth)acrylate-based polymerizable group-containing hydroxyl-reactive compound is used that has an isocyanate group as the "functional group that can react with a hydroxyl group to form a bond" and an acryloxy group or methacryloxy group as the "polymerizable group", the polymerizable group is bonded to the glucose unit through a urethane bond, but the ester bond derived from the acryloxy group or methacryloxy group is quantitatively hydrolyzed by sodium hydroxide, so the total amount (total number of moles) of the "groups having a polymerizable group" can be quantified by titration. When the titration method is employed, accurate measurement is not possible if unreacted polymerizable group-containing hydroxyl group-reactive compound remains. Therefore, it is necessary to remove unreacted polymerizable group-containing hydroxyl group-reactive compound beforehand by washing or the like prior to the titration.

[0041] The degree of substitution (DS) of the CNF component obtained using the isocyanate-(meth)acrylate polymerizable hydroxyl-reactive compound can be determined specifically as follows. That is, by repeatedly performing the operation of separating the CNF component from the slurry containing the CNF component obtained by reacting with the polymerizable hydroxyl-reactive compound and redispersing it in a washing dispersion medium, a slurry of the CNF component from which the unreacted polymerizable hydroxyl-reactive compound has been removed is obtained, and a measurement sample slurry containing 0.1 g of CNF component in dry mass is sampled from the slurry. Next, 10 ml of 0.5 N sodium hydroxide solution is added to the measurement sample slurry, and the mixture is reacted for 60 minutes to perform hydrolysis. After that, several drops of phenolphthalein solution are added, and the amount of remaining sodium hydroxide (mmol) is determined by titrating with 0.1 N hydrochloric acid, and the amount of sodium hydroxide consumed by hydrolysis (mmol) is determined by subtracting it from the amount of sodium hydroxide added (5.0 mmol). The degree of substitution (DS) can be calculated by dividing this value by the amount of glucose units (0.617 mmol) contained in 0.1 g of CNF component. In other words, if the amount of 0.1 N hydrochloric acid required to make the solution colorless after adding phenolphthalein solution is Y (ml) and the number of ester bonds contained in one molecule of isocyanate-(meth)acrylate-based polymerizable group-containing hydroxyl group reactive compound is E, the amount of sodium hydroxide consumed in hydrolysis is (0.1 × Y) (mmol), so the degree of substitution (DS) can be calculated by the formula: DS = (50-Y) / 6.17E.

[0042] The degree of substitution can be controlled by controlling the ratio of the amount of the unmodified CNF and the polymerizable group-containing hydroxyl group-reactive compound used as raw materials. In order to make the degree of substitution 0.1 or more and 1.0 or less, it is preferable to use 0.1 mmol or more of the polymerizable group-containing hydroxyl group-reactive compound per unit mass (1 g of dry mass) of the unmodified CNF used as raw material. In addition, the upper limit of the amount of the polymerizable group-containing hydroxyl group-reactive compound used is preferably 10 mmol, particularly 7 mmol, from the viewpoint of preventing excessive use. In addition, in order to further improve the degree of substitution of CNF, the amount of the polymerizable group-containing hydroxyl group-reactive compound used is more preferably 1.0 mmol or more, and even more preferably 2.0 mmol or more.

[0043] In the CNF component preparation process, after the reaction of CNF with a polymerizable group-containing hydroxyl group-reactive compound, a hydrophobizing agent consisting of another organic compound capable of reacting with the hydroxyl group of CNF is added and reacted, thereby further increasing the hydrophobicity of CNF. As the hydrophobizing agent, it is preferable to use a compound whose reaction rate with the hydroxyl group of CNF is faster than the reaction rate of the polymerizable group-containing hydroxyl group-reactive compound with the hydroxyl group of CNF, and which reacts at a rate 10 times or more, particularly 100 times or more. Examples of such compounds include phenyl isocyanate, trifluoromethylphenyl isocyanate, and bistrifluoromethylphenyl isocyanate. When using a hydrophobizing agent, the amount used is preferably 0.1 mmol to 10 mmol, particularly 0.3 mmol to 5 mmol, per unit mass (1 g dry mass) of unmodified CNF.

[0044] <Preparation of raw material slurry> For the CNF components including modified CNF obtained by carrying out these reactions in the CNF component preparation process, it is preferable to wash them after the reaction is completed in order to remove unreacted compounds. Washing can be suitably performed by repeating the operation of separating the CNF components and the dispersing medium that became the reaction solvent by a method such as centrifugation, removing the dispersing medium by decantation, adding a new organic solvent, stirring and mixing, and then removing the organic solvent in the same manner. By carrying out such washing, a slurry in which the CNF components are finally dispersed in an organic solvent that does not contain unreacted compounds is obtained, and by carrying out desolvation as necessary, a raw material slurry can be obtained. The concentration of the CNF components in the raw material slurry is preferably 5 to 35% by mass, more preferably 7 to 20% by mass, because it is easy to distill off the dispersing medium in the molding process, and further, it prevents aggregation between the CNF fibers and does not cause unevenness in the density of the obtained molded body.

[0045] In addition, in order to promote the polymerization reaction of the polymerizable group in the molding process, it is preferable to mix a polymerization initiator into the raw material slurry. The polymerization initiator is not particularly limited as long as it is an initiator that can be decomposed by heat and promote the polymerization of the polymerizable group introduced into the CNF. For example, when the polymerizable group is a radical polymerizable group, a radical polymerization initiator such as a thermal polymerization initiator, a photopolymerization initiator, or a chemical polymerization initiator may be mixed. Among these, it is preferable to use a thermal polymerization initiator that functions as a polymerization initiator by heating. Examples of suitable thermal polymerization initiators include organic peroxide initiators such as benzoyl peroxide and tert-butyl peroxide, and azo initiators such as AIBN. The amount of the polymerization initiator mixed is usually in the range of 0.001 to 0.1 g per unit mass (1 g dry mass) of the CNF component.

[0046] In addition, inorganic particles can be added to the raw material slurry for the purpose of controlling the transparency of the molded body, improving mechanical strength, improving gloss, etc. As the inorganic particles, for example, inorganic fillers consisting of inorganic oxide particles such as amorphous silica, silica-titania, silica-zirconia, silica-titania-barium oxide, quartz, alumina, etc. can be used. The particle size and shape of the inorganic filler are not particularly limited, and for example, spherical or irregular particles with an average particle size of about 0.01 μm to 100 μm can be appropriately used depending on the purpose. In addition, these inorganic fillers may be treated with a surface treatment agent represented by a silane coupling agent from the viewpoint of improving compatibility with modified CNF, etc. and improving mechanical strength and water resistance. The amount of addition of these inorganic fillers can be any blending amount depending on the purpose.

[0047] 1-2 Molding process In the molding process, the raw material slurry is supplied to the molding surface of the female mold (concave mold) and / or male mold (convex mold), and the CNF component is adhered to the molding surface under conditions in which the polymerizable group is polymerized while the dispersion medium is removed by evaporation, that is, while the dispersion medium is vaporized and removed, to obtain a molded body. Here, as a method for supplying the raw material slurry to the molding surface of the female mold (concave mold) and / or male mold (convex mold), (a) a method for introducing the raw material slurry into a cavity formed between the female mold (concave mold) and the male mold (convex mold), (b) a method for introducing the raw material slurry into the inside of the female mold (concave mold), (c) a method for spraying the raw material slurry onto the molding surface of the male mold (convex mold), or (d) a method for immersing the molding surface in the stored raw material slurry, etc. can be used. In addition, as a method for adhering the CNF component to the molding surface, a method for pressurizing the CNF component toward the molding surface to adhere it (pressure-bonding) or a method for adhering it by sucking it from the opposite side of the molding surface can be used. In this case, "close contact" means that the molding surface shape of the mold is substantially transferred to the surface shape of the molded product, and includes a state in which the molded product is in close contact directly or indirectly through a flexible, breathable or liquid-permeable sheet or film, such as a woven fabric, a nonwoven fabric, or a microporous film. From the viewpoint of obtaining a molded product with high density and excellent mechanical properties, it is preferable to adopt a method of (a) introducing the raw material slurry into a cavity formed between a female mold (concave mold) and a male mold (convex mold) and pressing the CNF component.

[0048] The method for distilling off the dispersion medium is not particularly limited as long as it can vaporize and remove the dispersion medium. For example, a method of heating the raw material slurry, a method of reducing pressure, or a method of combining heating and reducing pressure can be used. The raw material slurry can be heated by supplying the raw material slurry to a molding surface that has been heated in advance using a heater or the like. The entire system may be reduced in pressure, but it is preferable to reduce the pressure from the back side of the molding surface of the mold from the viewpoint of adhering the CNF component to the molding surface of the mold. In order to reduce the pressure from the back side of the molding surface, a flow path for degassing (for passing the vaporized dispersion medium) that communicates the front side and the back side of the molding surface is provided in the mold body, as in the case of so-called vacuum molding, and the back side is reduced in pressure. In this case, it is preferable to make the mold body out of a microporous material having air permeability (gas permeability) so that the flow path is uniformly dispersed over the entire surface of the molding surface, because the CNF component can be uniformly adhered to the molding surface of the mold.

[0049] The adhesion of the CNF component to the molding surface must be performed under conditions in which the polymerizable group is polymerized. Here, "under conditions in which the polymerizable group is polymerized" means that the conditions are such that the polymerizable groups of the "groups having a polymerizable group" introduced into the modified CNF are polymerized together to proceed with a reaction of linking them by a covalent bond, and are appropriately adopted depending on the type of polymerizable group. When the polymerizable group is a radical polymerizable group, it will polymerize when heated, but in order to polymerize more efficiently, it is preferable to use a radical polymerization initiator. A thermal (radical) polymerization initiator does not function as a polymerization initiator at room temperature, but becomes functional when a predetermined temperature is reached depending on the type, so it can be conveniently mixed in the raw material slurry in advance. For the same reason, a photopolymerization initiator may be mixed. However, when a photopolymerization initiator is used, it is necessary to irradiate the raw material slurry supplied to the molding surface with light that activates the photopolymerization initiator. It is also possible to use a chemical polymerization initiator that functions as a polymerization initiator through the coexistence of multiple components. When using a chemical polymerization initiator, however, it is preferable to premix some of the constituent components with the raw material slurry so that the polymerization reaction does not proceed during storage of the raw material slurry, and when the raw material slurry is supplied to the forming surface, to supply the remaining components separately to the forming surface, so that all of the constituent components are coexistent in the raw material slurry supplied to the forming surface.

[0050] When the raw material slurry contains a thermal (radical) polymerization initiator, it is sufficient to heat the raw material slurry to a temperature equal to or higher than the temperature at which the radical polymerization initiator starts to function. Since many thermal radical polymerization initiators function within a temperature range of 60 to 200°C, particularly within a temperature range of 80 to 160°C, the above-mentioned polymerization reaction can be promoted by heating to such a temperature. Therefore, in order to polymerize the polymerizable group while distilling off the dispersion medium when the raw material slurry contains a thermal polymerization initiator, the raw material slurry supplied to the molding surface may be heated to the above-mentioned temperature, or may be heated to the above-mentioned temperature and reduced pressure at the same time. From the viewpoint of the efficiency of removing the dispersion medium, it is preferable to heat the raw material slurry to 60 to 200°C, particularly within a temperature range of 80 to 160°C, and reduce pressure at the same time.

[0051] <Preferable embodiment of molding process> Particularly preferred embodiments of the molding step include the following: That is, it is particularly preferred that the molding step includes the following embodiments A to C. A: a molding unit is prepared, which is composed of a pair of a female mold (concave mold) and a male mold (convex mold) that are arranged so that their molding surfaces are opposed to each other and can be brought into contact with each other relatively, and a cavity for introducing a raw material slurry is formed between the two molding surfaces, and at least one of the male mold and the female mold is a decompression mold having a molding surface that is connected to its back surface and has a large number of fine hole openings that are air-permeable (allowing the vaporized gas of the dispersion medium to pass through) that are uniformly distributed on the molding surface, B: Introduce raw material slurry into the cavity; C: By heating the female mold and / or male mold, heat is transferred from the molding surface of the heated mold to heat the raw material slurry introduced into the cavity, and pressure is applied by bringing the molding surfaces of the molding die unit dies close to each other while reducing the pressure on the back side of the decompression die.

[0052] By adopting such an embodiment, a molded body can be obtained by adhering the CNF components to both molding surfaces while efficiently distilling off the raw material slurry and polymerizing the polymerizable groups.

[0053] The mold for decompression in the molding unit prepared in A above may be formed entirely from the porous material having a large number of fine holes as described above, or may be divided into a molding surface member including the molding surface and a mold body, with only the surface member being made of the porous material, and a cavity communicating with the back surface of the mold being provided inside the mold body, with the cavity communicating with the micropores of the porous material. Metal, resin, ceramics, etc. can be used as the material for the porous material and the mold body. In addition, the shapes of the female mold (concave mold) and male mold (convex mold) in the molding unit may be appropriately determined according to the shape of the desired molded product. Examples of such molding units that can be suitably used include the combination of the female mold (concave mold) and male mold (convex mold) shown in Figures 1 to 5 of Patent Document 6, and the combination of the main body part (mold part and upper plate part) and the bottom plate in the CNF molding device shown in Figure 1 of Patent Document 7.

[0054] In addition, in the above C, it is not necessarily necessary to simultaneously heat and reduce the pressure of the raw slurry and pressurize it. Rather, it is preferable to start pressurizing after the dispersion medium is reduced by heating and reducing the pressure of the raw slurry (concentrating the raw slurry) and the raw slurry becomes a highly viscous slurry or a semi-solid state.

[0055] In the above-mentioned preferred embodiment, the thickness of the molded body obtained by one cycle of B and C is almost uniquely determined by the amount of raw material slurry introduced into the cavity in B, the concentration (content) of the CNF component, and the pressure during pressurization, so the thickness of the molded body can be controlled by controlling these conditions. In addition, if the thickness of the molded body obtained by one cycle of B and C is not sufficient for the thickness of the desired molded body, a molded body of the desired thickness can be obtained by repeating the cycle of B and C. In this case, B and C may not be considered as one cycle, and the raw material slurry may be concentrated before pressurization in C, and the raw material slurry may be added at the stage of concentration, and the operation may be repeated before pressurization, or such a cycle may be repeated several times.

[0056] <Specific molding method using molding equipment> Hereinafter, with reference to FIG. 1, a preferred molding apparatus that can be used in the molding method of the present invention and a specific molding method using the molding apparatus will be described.

[0057] The molding device 1 shown in FIG. 1 is a molding device (corresponding to the CNF molding device shown in Patent Document 7 as FIG. 1) that can be suitably used in the manufacturing method of the present invention, and has a main body 2 (corresponding to a concave mold) and a bottom plate 3 (corresponding to a convex mold) that are supported in a movable state and made using a steam permeable means. The bottom plate 3 is held in an immovable state, and a molding cavity 4 is formed by the main body 2 and the bottom plate 3. Furthermore, the main body 2 is composed of a mold part 2a (corresponding to a side part of the concave mold) and an upper plate 2b (corresponding to a bottom part of the concave mold) made using a steam permeable means, and the upper plate 2b is disposed on the opposite side of the bottom plate 3 via the mold part 2a. A hydraulic actuator 5, which is a pressurizing means, is attached to the upper plate 2b, and by applying a load to this hydraulic actuator 5, the mold part 2a can be pressurized by the upper plate 2b in the direction of the bottom plate 3. Furthermore, a nozzle 6, which is a means for introducing raw material slurry into the molding cavity 4, is attached to the upper plate 2b. A far-infrared generating device 7, which is a heating means for heating the mold part 2a, is disposed near the mold part 2a. In this molding apparatus 1, the inner diameter of the mold portion 2a and the outer diameter of the bottom plate 3 are made to be approximately equal, so that the bottom plate 3 can be fitted inside the mold portion 2a. Meanwhile, the outer diameter of the upper plate 2b and the mold portion 2a are made to be approximately equal, so that when the upper plate 2b is pressurized toward the bottom plate 3 by the hydraulic actuator 5, the pressure is transmitted to the mold portion 2a, and the entire main body portion 2 supported in a movable state moves toward the bottom plate 3. Meanwhile, the bottom plate 3 held in an immovable state is held at a constant position, so that when the entire main body portion 2 moves toward the bottom plate 3, the bottom plate 3 fits inside the mold portion 2a, and the volume of the molding cavity 4 decreases.

[0058] When the molding process is performed using the molding device 1, first, the raw material slurry is poured into the inside of the molding cavity 4 from the nozzle 6 attached to the upper plate 2b in a state where the molding cavity 4 is formed by the bottom plate 3 and the main body 2. Around the same time, the heating of the mold part 2a is started by the far-infrared generating device 7. When a certain amount of raw material slurry is stored in the molding cavity 4 and the upper plate 2b is pressurized toward the bottom plate 3 by the hydraulic actuator 5, the entire main body part 2 supported in a movable state moves toward the bottom plate 3, the bottom plate 3 fits inside the mold part 2a, and the volume of the molding cavity 4 decreases. During this process, the raw material slurry inside the heated mold part 2a shrinks while discharging the vaporized dispersion medium to the outside through the upper plate 2b made of a porous body, and is molded into a predetermined shape according to the shape of the molding cavity 4, and a molded body 8 can be obtained. In this case, by appropriately refilling the raw material slurry from the nozzle 6 during the molding process, a molded body 8 having a required thickness can be obtained. In the above case, if the upper plate 2b and the bottom plate 3 are also heated in advance by the far-infrared radiation generating device 7, the time can be shortened.

[0059] 2. Molded body of the present invention and dental mill blank of the present invention The molded article of the present invention is a molded article of a cellulose-based material consisting of solid components in the raw slurry (components dispersed or dissolved in a dispersion medium), and includes a crosslinked body having a crosslinked structure in which modified CNFs in the CNF components in the raw slurry are mutually bonded via covalent bonds formed by polymerization of the polymerizable groups in the "groups having a polymerizable group" introduced into the modified CNFs. When no organic matter other than the CNF components is blended into the raw slurry, the organic component is substantially composed of only the crosslinked body. Therefore, the petroleum-derived substance contained in the organic component is only the above-mentioned "groups having a polymerizable group", and most of it, preferably 95 mass% or more, can be CNFs derived from natural products, more specifically, polysaccharides including natural plants. This point does not change even when an inorganic component is blended into the raw slurry to form a molded article made of a composite material.

[0060] In addition to the excellent characteristics of conventional CNF molded bodies, such as light weight, high strength, and low thermal expansion coefficient, the crosslinked structure described above gives it an excellent characteristic not seen in conventional CNF molded bodies, namely high water resistance. For example, in a three-point bending test according to ISO20795-1, the water resistance was calculated as follows: δ=3Fl / 2bh 2 In the bending strength δ calculated by {where F represents the maximum load during the bending test, l represents the distance between the supports (50.0 mm), b represents the test piece width (10.0 mm), and h represents the test piece thickness (3.0 mm),}, when the bending strength δ0 measured using a test piece that is not in contact with water is taken as δ0, and the bending strength δ1 measured using a test piece that has been immersed in water at 37° C. for one week is taken as δ1, the bending strength retention rate R defined by the formula R=δ1 / δ0 can be made 0.90 or more.

[0061] Therefore, in addition to the various applications in which conventional CNF molded bodies can be used, they can also be suitably used in applications such as dental materials, which require further water resistance. Furthermore, dental mill blanks made from the molded article of the present invention are not only comparable in strength and water resistance to conventional resin-based dental mill blanks, but also have the advantage of being environmentally friendly as they contain an extremely small amount of petroleum-derived components. EXAMPLES

[0062] The present invention will be described in detail below with reference to examples, but the present invention is not particularly limited to these examples.

[0063] 1. Preparation and evaluation of unmodified CNF slurry as the raw material for the raw slurry The unmodified CNF slurry was produced by the underwater counter impingement treatment method described in Patent Document 2 (JP Patent Publication 2017-205683 A) using bamboo-derived pulp as the raw material. In the underwater counter impingement method, cellulose fibers suspended in water are introduced into two nozzles facing each other in a chamber, and are sprayed from these nozzles under high pressure to cause counter impingement, which nanofibrillates the surface of the polysaccharide and peels it off, ultimately bringing it into a state close to dissolution in the carrier water. Since the cellulose is refined by cleaving only the interactions between the fibers, there is no structural change in the cellulose molecules, and cellulose nanofibers can be obtained with minimal decrease in the degree of polymerization associated with cleavage. The degree of polymerization of the resulting unmodified CNF slurry was measured. The measurement method and results are shown below.

[0064] <Measurement of polymerization degree> 0.15 g of CNF solids obtained by removing water, which is the dispersion medium of the unmodified CNF slurry, was dissolved in 30 ml of 0.5 M copper ethylenediamine solution, and after keeping at 25°C, the viscosity was measured by measuring the flow time using a Cannon-Fenske dynamic viscosity tube. The viscosity of this CNF copper ethylenediamine solution was set to η, and the viscosity of the 0.5 M copper ethylenediamine solution was set to η0, and the intrinsic viscosity: [η] was calculated by the following formula (1). Specific viscosity ηsp=(η / η0)-1 [η]=ηsp / {c(1+A×ηsp)} (1) (In the above formula (1), c represents the concentration of fibrous cellulose (g / mL) at the time of viscosity measurement, and A is a value specific to the type of solution, and in the case of a 0.5 M copper ethylenediamine solution, A = 0.28.)

[0065] Next, the degree of polymerization (DP) was calculated from the above-mentioned intrinsic viscosity [η] by the formula (2). The test was performed three times (n=3), and the average degree of polymerization, which is the average value, was 730. DP = [η] / aK (2) (K and a in the above formula (2) are values ​​determined by the type of polymer and the solvent used. In the case of cellulose dissolved in copper ethylenediamine, K=0.57 and a=1.)

[0066] 2. Production of green bodies and evaluation of the green bodies obtained Example 1 (1) Preparation of raw slurry First, 500 g of an acetone suspension (slurry) containing 1% by mass of unmodified CNF was prepared by replacing the water, which was the dispersion medium of the unmodified CNF slurry obtained in 1, with acetone. Next, 5.0 g (6.4 mmol per 1 g of dried CNF mass) of methacryloyloxyethyl isocyanate (manufactured by Showa Denko: Karenz MOI) was added dropwise to the obtained acetone slurry as a polymerizable group-containing hydroxyl group-reactive compound, and the mixture was stirred for 4 hours while refluxing at 65°C to cause a reaction, and a part of the hydroxyl groups of the unmodified CNF was replaced with a group having a polymerizable group, "group X: -OC(=O)-NH-C2H4-C(=O)CH2(Me)=CH2". The group X is bonded to the cellulose unit via a urethane bond that does not hydrolyze when contacted with an aqueous sodium hydroxide solution, and has one ester bond in the group structure that is quantitatively hydrolyzed when contacted with an aqueous sodium hydroxide solution (E=1).

[0067] After that, the reaction solution was centrifuged (5,000 rpm, 30 minutes), the supernatant was discarded, and the precipitated CFN component was suspended again in acetone and washed. This washing operation was repeated five times, and finally a slurry in which the CFN component containing the modified CNF was dispersed in acetone was obtained. Next, 0.1 g of 2,2-azobis(2,4-dimethylvaleronitrile) (Wako Pure Chemical Industries, Ltd., V-65) was added as a polymerization initiator to the obtained slurry, and then a part of the acetone was distilled off under reduced pressure to prepare a raw material slurry with a CNF component concentration of 2.4 mass%.

[0068] In addition, in order to confirm the state of crosslinking after molding during the preparation of the raw material slurry, a small amount of the slurry before the addition of the polymerization initiator was sampled, and the solvent was removed from the sample by vacuum drying to obtain a CNF component (solid component), which was subjected to IR measurement, and the amount of double bonds derived from the group X was quantified. In addition, the degree of substitution: DS in the CNF component was determined by titration. That is, 10 ml of 0.5N sodium hydroxide solution was added to a dispersion obtained by dispersing 0.1 g of the CNF component in 20 mL of distilled water, and the mixture was reacted for 60 minutes to hydrolyze the mixture, and then cooled to stop the reaction. Then, several drops of phenolphthalein solution were added, and the mixture was titrated with 0.1N hydrochloric acid solution, and the amount of the aqueous acid solution Y ml required for the titration was determined. Methacryloyloxyethyl isocyanate is an isocyanate-mono(meth)acrylate type polymerizable hydroxyl-reactive compound in which the number of ester bonds contained in one molecule of the polymerizable hydroxyl-reactive compound is 1: E. Therefore, the degree of substitution (DS) of the CNF component was determined by the formula: DS = (50-Y) / 6.17, and was found to be 0.54.

[0069] (2) Molding process Using the molding apparatus shown in FIG. 1, the raw material slurry was supplied from the nozzle 6 to the inside of the molding cavity 4 and molding was carried out under the following conditions to obtain a disk-shaped molded body A having a diameter of 150 mm and a thickness of 4.0 mm. conditions: Raw material slurry supply amount: CNF2.0% slurry 2000g Mold heating temperature: 100℃ Load capacity: 60kg Loading time: 20 hours

[0070] (3) Evaluation of the molded product The crosslinking degree of the obtained molded body A was evaluated by the following method, and the strength was evaluated before and after the water immersion test by the following method. The results are shown in Table 2.

[0071] <Evaluation of degree of cross-linking> If the unsaturated bond (C=C bond) in the group X introduced into the modified CNF in the molding process is polymerized, it can be said that crosslinks have been formed by chemical bonds between the CNF fibers (molecules). The amount of crosslinks formed can be understood as the consumption of C=C bonds. Therefore, in order to confirm whether a substantial amount of crosslinks have been formed between the CNF fibers (for example, a significant amount that affects the improvement of water resistance), IR measurements were performed on the raw material slurry (RS) and the molded body (MD), and the "double bond residual rate of the CNF molded body": X (%) was calculated from the obtained measurement chart, and the degree of crosslinking was evaluated based on this value. Specifically, first, the wave number assigned to the double bond of the group X in the above chart: 6165 cm -1 The amount of C=C bonds was evaluated based on the peak area S1 of the =CH absorption peak that appears near the center. Next, the wave number assigned to the hydroxyl group of the CNF, which serves as the internal standard, was calculated as 3500 cm. -1 The S1 was normalized by dividing the S1 by the peak area S2 of the absorption peak appearing near the S1 / S2, and this value was taken as the amount of C=C bonds per unit amount of CNF component: Q. The amount of C=C bonds per unit amount of CNF component in the molded body (MD) was Q. MD =(S1 / S2) MD The amount of C=C bonds per unit amount of CNF component in the raw slurry (RS) is Q RS =(S1 / S2) RS Then, Q RS Q in MD Percentage of:Q MD / Q RS The percentage of was evaluated as X (%). That is, in the IR measurement charts of the raw material slurry (RS) and the compact (MD), ·Wave number: 6165cm -1 The peak areas in the vicinity are S1 RS and S1 MD year, ·Wave number: 3500cm -1 The peak areas in the vicinity are S2 RS and S2 MD Then, The "residual double bond rate of the CNF molded product": X (%) can be calculated by the following formula (3). X(%)=(Q MD / Q RS ) x 100 =〔{(S1 / S2) MD} / {(S1 / S2) RS}〕×100 =〔{(S1 MD / S2 MD )} / {(S1 RS / S2 RS )}〕×100 (3)

[0072] The IR measurements were performed using a Perkin Elmer Spectrum One, with four measurements and a resolution of 4 cm. -1 The results are shown in Table 2.

[0073] <Three-point bending test after immersion in water> The CNF molded body was cut and polished to remove burrs, after which a three-point bending test was performed to measure the initial bending properties of the test pieces (Table 2). In addition, the CNF molded body was cut and polished to remove burrs, and the test pieces were immersed in water at 37°C for one week, and a three-point bending test was performed to measure the bending properties of the test pieces after immersion in water (Table 2). The three-point bending test was performed using a material testing machine (Model 5565; Instron Co., MA, USA) in accordance with ISO20795-1, with a 2kN load cell (serial no.: UK268) at a crosshead speed of 5mm / min at room temperature.

[0074] The bending strength (δ) was calculated using formula (4). δ=3Fl / 2bh 2 (4) Here, F represents the maximum load during the bending test, l represents the distance between the supports (50.0 mm), b represents the test piece width (10.0 mm), and h represents the test piece thickness (3.0 mm).

[0075] Example 2 A raw material slurry was obtained in the same manner as in Example 1, except that 6.0 g of 2-methacryloyloxy(2-ethyloxy)isocyanate (6.0 mmol per 1 g of dried CNF mass) was used instead of 5.0 g of methacryloyloxyethyl isocyanate used as the polymerizable group-containing hydroxyl group-reactive compound in Example 1. The substitution degree of the CNF component in the obtained raw material slurry was measured, and the results are shown in Table 1.

[0076] Next, the obtained raw material slurry was used to obtain a CNF molded body B in the same manner as in Example 1, and the CNF molded body B was evaluated in the same manner as in Example 1. The results are shown in Table 2.

[0077] Example 3 A raw material slurry was obtained in the same manner as in Example 1, except that 20 g (5.7 mmol per 1 g of dried CNF mass) of LR9000 (manufactured by BASF), a reaction product of a polymer containing 2-hydroxyethyl acrylate and 1,6-diisocyanatohexane, was used instead of 5.0 g of methacryloyloxyethyl isocyanate used as the polymerizable group-containing hydroxyl group-reactive compound in Example 1. The substitution degree of the CNF component in the obtained raw material slurry was measured, and the results are shown in Table 1. The molecular weight of LR9000 is expressed as H 1 The degree of substitution was calculated by measuring -NMR, and the molecular weight of LR9000 used in this example was set to 410.48 (E=1).

[0078] Next, the obtained raw material slurry was used to obtain a CNF molded body C in the same manner as in Example 1, and the CNF molded body C was evaluated in the same manner as in Example 1. The results are shown in Table 2.

[0079] Reference example 1 A thermosetting acrylic resin denture base (Acron, manufactured by GC) was cured into a rectangular parallelepiped (64.0 x 10.0 x 3.3 mm) according to the attached instructions and the method described in ISO20795-1. Both sides of the obtained cured body were polished with emery paper of #600, #800, #1000, and #1200. Next, the cured body was washed with water for 15 seconds, immersed in distilled water at room temperature (23±2°C) for 24 hours, and then subjected to a three-point bending test in the same manner as in Example 1. The results are shown in Table 2.

[0080] Comparative Example 1 In the same manner as in Example 1, 4,000 g of an acetone suspension (slurry) containing 1 mass% unmodified CNF (the same as that used as the raw material in preparing the raw material slurry in Example 1) was prepared, and without carrying out the step of functionalizing the hydroxyl groups of the unmodified CNF as in Example 1, the unmodified CNF slurry was used to obtain a CNF molded product Z in the same manner as in Example 1, and the CNF molded product Z was evaluated in the same manner as in Example 1. The results are shown in Table 2.

[0081] Comparative Example 2 In the same manner as in Example 1, 4000 g of an acetone suspension (slurry) containing 1% by mass of unmodified CNF (the same as that used as the raw material in preparing the raw material slurry in Example 1) was prepared, and concentrated by removing part of the acetone by suction filtration. The CNF residue on the filter paper was washed with acetone while suction filtration, to obtain an acetone slurry containing about 2.4% by mass of unmodified CNF. 2 g (5% by mass relative to the CNF solid content) of a reaction product of a polymer containing 2-hydroxyethyl acrylate and 1,6-diisocyanatohexane as crosslinking agents (LR9000, manufactured by BASF) and 100 mg of 2,2-azobis(2,4-dimethylvaleronitrile) (V-65, manufactured by Wako Pure Chemical Industries, Ltd.) were added to the obtained slurry, and dissolved in acetone as a dispersion medium. The degree of substitution of the CNF component in the obtained raw material slurry was measured, and the results are shown in Table 1. The molecular weight of LR9000 is H 1 The degree of substitution was calculated by measuring -NMR, and the molecular weight of LR9000 used in this example was set to 410.48 (E=1).

[0082] Next, using the obtained slurry, a molded body Y was produced in the same manner as in Example 1. The obtained molded body Y was subjected to a three-point bending test in the same manner as in Example 1 to evaluate its strength before and after a water immersion test. The results are shown in Table 2. Note that, since the degree of substitution was zero as shown in Table 1, the residual double bond rate was not measured.

[0083] [Table 1]

[0084] [Table 2] [Explanation of symbols]

[0085] 1... Molding equipment 2. Main body 2a··Mold section 2b Upper plate 3...Bottom plate 4. Molding cavity 5. Hydraulic actuator 6. Nozzle 7. Far-infrared radiation generator

Claims

1. A dispersion in which a cellulose nanofiber (CNF) component including modified CNF in which at least a portion of hydroxyl groups of CNF are substituted with a "group having a polymerizable group" is dispersed in a dispersion medium, The modified CNF is obtained by reacting a polymerizable group-containing hydroxyl group-reactive compound with cellulose nanofiber (CNF), The polymerizable group-containing hydroxyl group-reactive compound is a compound having, in the molecule, "the polymerizable group consisting of an acryloxy group or a methacryloxy group" and "a functional group capable of reacting with a hydroxyl group to form a bond," the dispersion liquid further contains a polymerization initiator capable of polymerizing the polymerizable group, and does not contain the polymerizable group-containing hydroxyl group-reactive compound, A raw material slurry preparation step of preparing a raw material slurry comprising the dispersion in which the degree of substitution, defined as the average number of substituted hydroxyl groups per glucose unit in the CNF component contained in the dispersion, is 0.1 or more and 1.0 or less; and A method for producing a molded body made of a cellulose-based material, comprising: a molding step of supplying the raw material slurry to the molding surface of a female mold (concave mold) and / or a male mold (convex mold), and obtaining a molded body by adhering the CNF component to the molding surface under conditions in which the polymerizable groups are polymerized while evaporating off the dispersion medium.

2. The method according to claim 1 , wherein the polymerizable group-containing hydroxyl group-reactive compound is used in an amount of 0.1 (mmol / g) or more and 7.0 (mmol / g) or less per unit mass of the unmodified CNF.

3. A molded article of a cellulosic material obtained by the method according to claim 1 or 2.

4. 4. The molded article of a cellulose-based material according to claim 3, wherein 95% by mass or more of the organic components constituting the cellulose-based material are cellulose derived from polysaccharides.

5. The molded article of the cellulose-based material according to claim 3 or 4, wherein the bending strength δ is calculated by a three-point bending test according to ISO20795-1 using the formula: δ = 3Fl / 2bh2 {where F represents the maximum load during the bending test, 1 represents the distance between the supports (50.0 mm), b represents the width of the test piece (10.0 mm), and h represents the thickness of the test piece (3.0 mm).}, the bending strength δ is measured using a test piece that is not in contact with water, and the bending strength δ is measured using a test piece that has been immersed in water at 37 ° C. for one week. The bending strength retention R defined by the formula: R = δ1 / δ0 is 0.90 or more.

6. A dental mill blank comprising a molded article of the cellulosic material according to any one of claims 3 to 5.

Citation Information

Patent Citations

  • Car body structure of saddling type car

    JP1989032983A

  • Electronically controlled fuel injection device for internal combustion engine

    JP1989060737A

  • Fiber-reinforced composite material, manufacturing method therefor, and wiring base

    JP2005060680A

  • Fiber-reinforced composite material and method for producing the same

    JP2007051266A

  • Resin composition containing modified microfibrillated plant fiber