Electrochemical secondary cells for high energy or high power battery applications

The development of compatible electrolytes and cathode materials for sodium-based anodes addresses the challenges of sodium metal anodes, achieving high energy density and stable cycling in electrochemical cells, surpassing the limitations of Li-ion batteries.

JP7554038B2Active Publication Date: 2024-09-19BROADBIT BATTERIES OY
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2018536345
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2015-09-30
Filing Date
2016-03-04
Publication Date
2024-09-19
Estimated Expiration
2036-03-04

AI Technical Summary

Technical Problem

Current Li-ion battery technologies for electric vehicles face high manufacturing costs, limited range, uncertain lifetime, and slow charging capabilities, with sodium-based metal anodes presenting even greater challenges due to the lack of suitable cathode materials and electrolyte systems for reversible metal deposition.

Method used

Development of electrolytes and cathode materials that support stable cycling of metallic sodium anodes, including electrolytes like NaBF4·xNH3 and NaBH4·xNH3, and cathodes such as poly-AnthraQuinonyl Sulphide (PAQS) and indanthrone blue, which enable smooth, dendrite-free sodium deposition and high energy density.

Benefits of technology

The solution provides high energy density, cost-effective, and durable electrochemical cells with stable cycling capabilities, overcoming the limitations of existing Li-ion batteries and enabling efficient sodium-based battery systems.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007554038000013
    Figure 0007554038000013
  • Figure 0007554038000007
    Figure 0007554038000007
  • Figure 0007554038000005
    Figure 0007554038000005
Patent Text Reader

Abstract

[Problem] To provide a high-performance electrochemical cell for secondary high-energy or high-power batteries based on an anode containing metallic sodium. [Solution] Preferably, an electrochemical cell for a secondary battery for use in an electric vehicle is provided. The cell includes a solid metal anode deposited on a suitable current collector substrate during the cell charging process. Several suitable modifications of electrolytes are disclosed along with suitable cathode materials for constructing a complete cell. [Selection Diagram] Figure 5
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] FIELD OF THEINVENTION In general, the present invention relates to rechargeable electrochemical cells, batteries and supercapacitors. In particular, the present invention relates to such cells that utilize metallic sodium anodes, novel cathodes that support high energy density and electrolytes that are compatible with both of these particular electrodes. [Background technology]

[0002] background Various implementations and concepts of electric vehicle (EV) batteries are known to exist, ranging from batteries based on the most widely used Li-ion vehicle technology to others such as lead-acid, nickel-cadmium (Ni-Cd), nickel-metal hydride (Ni-MH) and molten salt. Modern electric vehicle and hybrid battery production is primarily based on Li-ion battery technology. However, the technology is said to have several drawbacks. In particular, the high manufacturing cost of Li-ion batteries forces vehicle manufacturers to design vehicles with limited range. Furthermore, the uncertain life span and limited fast charging capacity of current Li-ion batteries creates hesitation for customers when choosing between battery-powered all-electric or plug-in hybrid vehicles and combustion engine vehicles. Furthermore, the high maturity of current Li-ion technology means that any significant improvement in battery performance and cost-effectiveness would require a dramatically different conceptual approach.

[0003] Intensive research has been conducted in the field of battery technology to find a cost-effective combination of sufficient specific energy, capacity and durability. Numerous compounds have been investigated as potential components for battery cells. Motivated by the high specific energy potential of EV cells containing magnesium-based metal anodes, magnesium-based metal anodes have been intensively researched. However, ambient temperature commercial devices have not yet been introduced due to the technical challenges associated with the lack of suitable cathode materials and / or challenges of electrolyte systems capable of reversible metal deposition. By general consensus of battery researchers, the challenges associated with sodium-based metal anodes are even greater than those of cells containing magnesium-based metal anodes. Thus, researchers working on metal anodes have been focusing on Mg 2+ / Mg potential is Na + Although the current study focuses mainly on magnesium-based electrode systems, sodium-based cells have been investigated by inserting them into Na-ion cell formulations, despite the fact that the potential of the anode is about 0.4 V higher than the Na / Na potential. Thus, the invention of metallic sodium anode-based battery and supercapacitor cells disclosed herein has high industrial importance and initiates a new approach for the construction of cost-effective yet high-performance batteries and supercapacitors. Summary of the Invention [Problem to be solved by the invention]

[0004] Summary of the Invention The object of the present invention is to disclose a high performance electrochemical cell for secondary high energy or high power batteries based on an anode containing metallic sodium. In a preferred embodiment, the cell is provided with a solid metal anode electrodeposited during the first charging cycle, a cathode selected from the electrode structures disclosed in the present invention, and an electrolyte selected from the electrolytes disclosed in the present invention. [Means for solving the problem]

[0005] One aspect of the present invention relates to the disclosure of electrolytes that support essentially stable cycling of metallic sodium anodes. Another aspect relates to the disclosure of current collector materials that support essentially smooth, dendrite-free, and well-adhered electrochemical deposition of sodium. In one embodiment of the present invention, electrochemical deposition of sodium is a practical prerequisite for the effective practice of the present invention. This electrochemical sodium deposition occurs either during the first charge cycle of a cell assembled in a discharged state, or during the preparation of the anode sodium thin film prior to cell assembly of a cell assembled in a charged state. The identification of a suitable current collector substrate for such sodium deposition and a suitable electrolyte for deposition on this substrate is correlated. In other words, only a subset of electrolytes that support sodium in sodium deposition support sodium deposition on the current collector substrate. Thus, the disclosure of compatible electrolyte-current collector substrate pairs is a primary objective of the present invention.

[0006] In one embodiment, the anode is essentially sodium-free in its discharged state and / or during assembly when it may be in a discharged state, where the weight percent of sodium is preferably less than 50%, and more preferably less than 30%, and more preferably less than 20%, and more preferably less than 10%, and more preferably less than 5%, and more preferably less than 3%, and more preferably less than 2%, and more preferably less than 1%, and more preferably less than 0.5%, and more preferably less than 0.3%, and more preferably less than 0.2%, and more preferably less than 0.1%, and most preferably 0%, of the total weight of the anode in its discharged state.

[0007] The anode may include a support / current collector of sodium or another conductive material. In one embodiment, the anode is pure sodium. Here, the anode is considered to be pure sodium when the weight percent of sodium is preferably greater than 50%, and more preferably greater than 70%, and more preferably greater than 80%, and more preferably less than 90%, and more preferably greater than 95%, and more preferably greater than 97%, and more preferably greater than 98%, and more preferably greater than 99%, and more preferably greater than 99.5%, and more preferably greater than 99.7%, and more preferably greater than 99.8%, and more preferably greater than 99.1%, and most preferably 100% of the total weight of the anode in its discharged state.

[0008] In one embodiment, the electrochemical deposit on the current collector material may be essentially smooth, dendrite-free, and / or well adhered. In one embodiment, the electrochemical deposit and the current collector material may be in contact. Here, smooth is defined as having a surface roughness of less than 100 microns, more preferably less than 50 microns, more preferably less than 20 microns, more preferably less than 10 microns, more preferably less than 5 microns, more preferably less than 2 microns, and most preferably less than 1 micron. Here, dendrite-free is defined as having preferably less than 90%, more preferably less than 50%, more preferably less than 20%, more preferably less than 10%, more preferably less than 5%, and most preferably less than 2% of the total mass of the sodium deposit as dendrites.

[0009] In a further aspect, the present invention relates to the disclosure of a cathode compatible with the disclosed electrolyte. Even with regard to known electrode materials, considering the thousands of electrode materials described in the literature, it is innovative to identify one that simultaneously supports good electronic conductivity, good ionic diffusion coefficient, provides high energy density, is insoluble in the novel disclosed electrolyte in reduced, oxidized or intermediate states, and is compatible with the electrochemical window of the novel disclosed electrolyte.

[0010] In further aspects, the present invention facilitates the utilization of certain disclosed cell components, for example, the use of certain disclosed cathodes in different contexts, such as those of lithium-based battery electrodes, or the use of certain disclosed electrolytes in supercapacitor cells.

[0011] In yet a further aspect, the present invention relates to the use of a secondary electrochemical battery comprising a plurality of cells according to any of the embodiments so provided in an electric vehicle.

[0012] In yet a further aspect, the invention relates to the use of the battery in an electric or electronic device, a power unit, a back-up energy unit or a grid storage or stabilization unit.

[0013] In yet a further aspect, the use of certain disclosed electrolytes for any application utilizing ionic liquids or non-aqueous liquids having high salt content.

[0014] Stable cycling is defined herein as preferably less than 50%, more preferably less than 25%, more preferably less than 10%, and most preferably less than 5% electrolyte consumption during at least 10 cycles, and more preferably at least 100 cycles, and more preferably at least 1000 cycles, and most preferably at least 10,000 cycles.

[0015] The usefulness of the present invention arises for a variety of reasons depending on its respective specific embodiment, such as high energy density per unit of mass, high power density per unit of mass, or improved durability. Cost-effective implementation of the batteries disclosed herein will positively impact many battery-powered products.

[0016] Sodium-based metal anodes offer some of the highest theoretical gravimetric capacities of any anode material: the gravimetric capacity of sodium is +For the Li / Na couple, at a potential of -2.7 V vs. the Standard Hydrogen Electrode (SHE), it is greater than 1100 mAh / g. For comparison, current graphite anodes in lithium-ion batteries have a gravimetric capacity of about 400 mAh / g. Furthermore, metal anodes do not require solid-state diffusion of ions for the transition of the material from a charged to a discharged state, but only successful deposition / dissolution of ions on / from the surface of the metal is required.

[0017] Unless otherwise indicated, the term "cell" is intended in this disclosure to refer to an electrochemical cell as a battery in its minimum packed form, and the term "battery" refers to a group of cells (e.g., a stack of cells).

[0018] Each electrochemical cell includes at least an anode, a cathode, and an electrolyte disposed between the anode and the cathode. The cell may also include a separator.

[0019] Various embodiments of the invention will become apparent by consideration of the detailed description and accompanying drawings. [Brief description of the drawings]

[0020] [Figure 0] Examples of superalkali cation formations are shown. The first two examples on the left are symmetric formations, while the last two examples on the right are asymmetric formations. [Figure 1] The electrochemical behavior of sodium deposition on sodium in various liquid ammoniates (NaI·3.3NH3, NaBF4·2.5NH3 and NaBH4·1.5NH3) is shown. The experiments were carried out in a three-electrode cell at a sweep rate of 20 mV / s using sodium metal as the reference and counter electrodes. The geometric area of ​​the working electrode is 1 cm2 for all three experiments. [Diagram 2]Cyclic voltammograms for the PAQS electrode in NaI 3.3NH3. The experiment was performed in a two-electrode split cell at a sweep rate of 20 mV / s using sodium metal as the reference and counter electrodes. Currents are shown for an active mass of PAQS, 4.8 mg, with a geometric exposed area of ​​1.1 cm2. [Diagram 3] Cyclic voltammograms for an indanthrone blue electrode in NaI 3.3NH3. The experiment was performed in a two-electrode split cell at a sweep rate of 20 mV / s using sodium metal as the reference and counter electrodes. Currents are shown for an active mass of indanthrone blue, 2 mg, with a geometric exposure area of ​​1.1 cm2. [Figure 4] The electrochemical behavior of sodium deposition on sodium in NaAlCl4·2SO2 electrolyte is shown. The experiment was carried out in a three-electrode cell at a sweep rate of 5 mV / s using sodium metal as the reference and counter electrodes. The geometric exposed area of ​​the working electrode is 1 cm2. [Diagram 5] Figure 1 shows the cell potential evolution during charge / discharge cycling of NaCl active material in NaAlCl4·2SO2 electrolyte. The capacity is shown in terms of carbon mass and the charge limit corresponds to full charging of the NaCl active material. The experiment was carried out in a coin cell using sodium metal as counter electrode. The geometric exposed area of ​​the working electrode is 1 cm2. [Figure 6] The proposed chemical process occurring during the charge / discharge cycling measurements shown in Figure 5. It should be noted that the NaCl particles do not need to completely desorb from the carbon framework. [Figure 7] Figure 1 shows the initial cell potential evolution during discharge of NaAlCl4·2SO2 catholyte when the cathode electrode already contains 4.08 mg NaCl in 3.32 mg Ketjen-Black carbon framework. The capacity is shown in terms of carbon mass. The experiment was performed in a coin cell using sodium metal as counter electrode. The geometric exposed area of ​​the working electrode is 1 cm2. [Figure 8]Ratio between capacity and initial capacity versus cycle number for an IB-based electrode in NaI 3.3NH3. The experiment was carried out in a two-electrode cell at different C-rates using sodium metal as the cathode. The active mass is 3.5 mg of indanthrone blue with a geometrical exposed area of ​​1.1 cm2. [Figure 9] FIG. 1 shows a general phase diagram for concentrated electrolytes prepared from nitrogen-based solvent precursors. [Figure 10] The electrochemical behavior of sodium deposition on sodium by 4 molar NaBF4 salt in ethylenediamine is shown. The experiment was carried out in a three-electrode cell at a sweep rate of 20 mV / s using sodium metal as the reference and counter electrodes. The geometric area of ​​the working electrode is 1 cm2. [Figure 11] 1 shows the molecular structures of some example vat dyes according to the present invention. [Figure 12] 1 shows the molecular structure of a Triazine-Quinone copolymer cathode material that can be described by the formula [C8H2N2O2Na2]n. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0021] Detailed Description of the Preferred Embodiments Detailed embodiments of the present invention are disclosed herein with reference to the accompanying drawings.

[0022] The following paragraphs first describe current collector substrate-electrolyte pairs for deposition and cycling of metallic sodium anodes. Then, for each electrolyte type, compatible cathode compositions are disclosed.

[0023] The disclosed electrochemical cells are implemented to allow for reversible redox interaction of metal ions with the cathode electrode during charge-discharge cycling. The term "reversible redox interaction" preferably refers to the ability of ions to both insert into and exit from the electrode material without causing significant degradation of the electrode material and thus adversely affecting the performance characteristics of the electrode upon repeated cycling.

[0024] According to the present invention, for carbon coated surfaces, the carbon can be in any suitable form. Preferred forms of carbon include CNT, fullerene, CNB, graphene, graphite, Ketjen-Black, mesoporous carbon, activated carbon, carbon nanohorn, carbon nanofoam, Q-carbon, T-carbon, Y-carbon, nanocarbon, carbon nanoparticles and / or porous carbon. Other forms of carbon are possible according to the present invention.

[0025] A new class of electrolytes is based on high concentration sodium salts in nitrogen-containing solvents and is disclosed in the following paragraphs.

[0026] The first class of electrolyte-substrate pairs disclosed is based on inorganic ammoniate electrolytes. Goncalves et al. [1] disclosed an electrolyte for rechargeable batteries based on sodium iodide-liquid ammoniate (NaI 3.3NH3). The NaI 3.3NH3 electrolyte was used to charge and discharge Na using nickel foil, stainless steel or carbon-coated aluminum foil as electrodes. + However, the high cost of NaI salts and the high potential window of up to 2.6 V vs. I - The heavy weight of the anion makes this known electrolyte impractical. It is therefore desirable to find a cheaper and lighter liquid ammoniate that is compatible with metallic sodium anodes. Apparently, the required quality does not depend only on the salt concentration; NaSCN·3.1NH3 room temperature liquid ammoniate has been tested as an electrolyte and found to be incompatible with metallic sodium, despite its much higher salt concentration.

[0027] Surprisingly, NaBF4·xNH3 was discovered as a previously unknown near-room temperature liquid ammoniate and was further found to be a suitable electrolyte for metallic sodium cycling. It was successfully used to cycle sodium metal using aluminum, stainless steel or carbon-coated aluminum foil as electrodes. + The potential window is up to 2.9 V vs. Na. The boiling point of NaBF4·2.5NH3 is about 10°C, and the ionic conductivity is 80 mS·cm -1 has a value of

[0028] Furthermore, NaBH4·xNH3 was found to be a suitable electrolyte for metallic sodium cycling. It was found to be a suitable electrolyte for sodium cycling using stainless steel as the electrode. + It has a potential window of up to 2.75 V vs. sodium / Na. The existence of NaBH4·1.5NH3 room temperature liquid has been known for some time, but NaBH4·xNH has never been tested as an electrolyte, probably because NaBH4 is known to be a strong and fast reducing agent in other solvents. The high potential window of this electrolyte, on the one hand, and its compatibility with metallic sodium, on the other hand, are therefore very surprising properties. The boiling point of NaBH4·1.5NH3 is about 18 °C, and the ionic conductivity is 110 mS·cm -1 has a value of

[0029] An attempt has been made to explain the properties of these newly discovered electrolyte samples. While not intending to be bound by theory, the experimental data of these electrolyte melting points versus salt content, as well as their behavior toward metallic sodium surfaces, indicate their ionic liquid or locally ordered nature. As evidenced by their high ionic conductivity, the electrolytes represent a new class of ultra-low viscosity electrolytes, with viscosities an order of magnitude lower than most currently used battery electrolytes. In these ionic liquid or locally ordered electrolytes, six nitrogen atoms are tightly bound or otherwise attracted to cations, forming super-alkaline complexes. Ni 2+For doubly charged cations such as Li, the resulting superalkali has too high a charge density to be liquid. + , Na + , K + or Cu + For singly charged cations such as Na, if the counteranion is weakly coordinating and / or there is an incompatible mix of cation sizes in the electrolyte, the resulting superalkali can be in the liquid phase. Thus, Na + X - The general formula for 3NH3 is that half of the cations are (Na 6NH3). + tend to be in a superalkaline state, while the other half is Na + There is some statistical variation between these states. The size mismatch of the cation structures and the weakly coordinating X - The combination of anion properties is sufficient to obtain a room temperature liquid in a specific stoichiometric range near a 3:1 NH3:salt ratio. The limit of the liquid range stoichiometry depends on the choice of salt cation species (Li + , Na + , K + , Cu + ), the type of amine species involved in producing the superalkaline complex, and the choice of salt anion species. Figure 9 shows the general phase diagram of these electrolytes for the described simple binary electrolytes with a NH3:salt ratio of X. According to the invention, X is preferably 0.1-10, and more preferably 0.4-5, and more preferably 0.7-4, and more preferably 0.9-3.5, and more preferably 0.95-3.2, and most preferably 0.99-3.1. According to the invention, the simple electrolytes can be combined with other electrolytes to produce electrolyte mixtures. There is a temperature-dependent concentration of free amine species in the electrolyte. As long as the concentration of these free amine species is low enough, the electrolyte is inactive towards metallic sodium. On the cathode side, the concentration of free amine species is expressed as the limiting overpotential observed for electrolyte stability relative to the oxidation potential of a given amine species.

[0030] Consistent with this conceptual discovery of the properties of ammoniate-based electrolytes, it has been found that this new class of electrolytes can be prepared not only from ammonia, but from any nitrogen-containing solvent precursor. Suitable molecules include, for example, a wide range of organic amines and nitriles. When ammonia is used, such electrolytes are called ammoniate-based electrolytes or liquid ammonia, and the electrolytes can be liquid with any stoichiometric composition near the ideal 3:1 NH3:salt ratio, preferably 0.1:1 to 100:1, and more preferably 0.5:1 to 50:1, and more preferably 1:1 to 20:1, and more preferably 1.5:1 to 10:1, and more preferably 2:1 to 5:1, and more preferably 2.5:1 to 4:1, and more preferably 2.8:1 to 3.5:1, and most preferably 2.9:1 to 3.2:1. Similarly, when a monoamine is utilized, preferably selected from the group of n-butylamine, n-propylamine, isopropylamine, ethylamine, methylamine and pyridine, the electrolyte may be liquid with some stoichiometry near the ideal 3:1 monoamine:salt ratio, preferably 0.1:1 to 100:1, and more preferably 0.5:1 to 50:1, and more preferably 1:1 to 20:1, and more preferably 1.5:1 to 10:1, and more preferably 2:1 to 5:1, and more preferably 2.5:1 to 4:1, and more preferably 2.8:1 to 3.5:1, and most preferably 2.9:1 to 3.2:1. Following this same principle, preferably when a diamine selected from the group of ethylenediamine and 1,3-diaminopropane is utilized, the electrolyte can be liquid at some stoichiometric composition near the ideal 1.5:1 diamine:salt ratio, preferably 0.1:1 to 50:1, and more preferably 0.4:1 to 20:1, and more preferably 0.6:1 to 10:1, and more preferably 0.8:1 to 6:1, and more preferably 1:1 to 3:1, and more preferably 1.2:1 to 2:1, and more preferably 1.3:1 to 1.8:1, and most preferably 1.4:1 to 1.6:1.Preferably, when triamines including diethylenetriamine are utilized, the electrolyte can be liquid with some stoichiometry near the ideal 1:1 triamine:salt ratio, preferably 0.1:1 to 20:1, and more preferably 0.2:1 to 10:1, and more preferably 0.3:1 to 5:1, and more preferably 0.4:1 to 3:1, and more preferably 0.5:1 to 2:1, and more preferably 0.6:1 to 1.4:1, and more preferably 0.8:1 to 1.2:1, and most preferably 0.9:1 to 1.1:1. The melting point of the electrolyte can be reduced due to the irregular cation shape, and therefore, according to the present invention, the melting point of the electrolyte can be varied by using a mixture of different amines. Examples include, but are not limited to, a mixture of ethylenediamine and 1,3-diaminopropane, a mixture of ammonia and amines, or a mixture of nitriles and amines, which results in a more irregular cation shape. Without being bound by theory, some examples of possible superalkali formations are illustrated in FIG. 0. The melting point of the "tailed" asymmetric cationic structure is particularly effective in lowering the melting point and viscosity of the electrolyte. Therefore, the appropriate selection of the solvent mixture is useful to achieve the lowering of the melting point and viscosity. For example, it has been found that utilizing ammonia:n-butylamine or ammonia:n-propylamine solvent mixtures in a ratio of about 5:1, preferably 0.1:1 to 100:1, and more preferably 0.5:1 to 50:1, and more preferably 1:1 to 20:1, and more preferably 2:1 to 10:1, and more preferably 3:1 to 8:1, and more preferably 4:1 to 6:1, and more preferably 4.5:1 to 5.5:1, and most preferably 4.8:1 to 5.2:1 is particularly effective in lowering the melting point of the electrolyte, possibly as a result of the cationic tail effect. The use of additional similar solvent mixtures to achieve the asymmetric "tailed" superalkaline structure is also possible in accordance with the present invention. The use of organic amines instead of ammonia has the additional utility of increasing the electrolyte boiling point and increasing the potential window.

[0031] It has been discovered that this new class of electrolytes may include nitrile-based solvents, or in the case of certain salt species such as sodium bis-(trifluoromethylsulfonyl)imide, may be nitrile-based. In accordance with the electrolyte structure disclosed above, nitriles are utilized, and although other nitriles are possible in accordance with the present invention, they may be liquid with some stoichiometric composition, preferably in the vicinity of a 3:1 nitrile:salt ratio, preferably 0.1:1 to 100:1, and more preferably 0.5:1 to 50:1, and more preferably 1:1 to 20:1, and more preferably 1.5:1 to 10:1, and more preferably 2:1 to 5:1, and more preferably 2.5:1 to 4:1, and more preferably 2.8:1 to 3.5:1, and most preferably 2.9:1 to 3.2:1. With respect to the mixed electrolytes, most preferably there is a 1 to 1 molar equivalence between the nitrile, monoamine, and ammonia, meaning that each of these compounds contributes one nitrogen atom per molecule for the superalkali formation. The use of nitriles has the advantage of further increasing the electrolyte potential window, at the cost of reducing ionic conductivity and further limiting the choice of salts resulting in a liquid electrolyte. The organic amine may be selected from ethylenediamine, 1,3-diaminopropane, diethylenetriamine, n-butylamine, n-propylamine, isopropylamine, ethylamine, methylamine, pyridine or mixtures thereof, and the nitrile may be selected from acetonitrile, propiononitrile, or a mixture containing one or more of the foregoing organic amines.

[0032] Na + The electrochemistry of the containing salts has been investigated in detail, particularly with respect to the sodium battery applications of the present invention, although other cationic species are possible in accordance with the present invention. Consistent with the conceptual discovery of this property of ammonite and amine-based electrolytes, it has been found that this new class of electrolytes, e.g., Li + , K + or Cu + It has been discovered that the electrolyte can be prepared from salts containing weakly coordinating anions. The salts utilized can contain weakly coordinating anions and are therefore generally known to be utilized to produce low viscosity electrolytes. BH4 - or BH3CN -Several additional anions, such as anions 100% Na2O3, ... + A sufficiently high oxidation potential level of at least 3 V vs. - , BH4 - , PF6 - , ClO4 - , B(CN)4 - , BF3CN - , BF2(CN)2 - , BF(CN)3 - , BH3CN - , BH2(CN)2 - , BH(CN)3 - , Al(BH4)4 - , bis-(trifluoromethylsulfonyl)imide (TFSI - ), bis(fluorosulfonyl)imide (FSI - ), trifluoromethanesulfonate (triflate - ), but other anion species are possible according to the invention. - The anion is precluded from battery applications due to its reactivity with metallic sodium, although it may be used in conjunction with other agents that reduce or negate this reactivity.

[0033] For a workable range of amine:salt or ammonia:salt ratios to support metallic sodium cycling, the preferred ratios were investigated. For example, for the NaBF4·xNH3 system, for a suitable salt:ammonia ratio for metallic sodium cycling, the x,NH3 to salt ratio can be in the range of preferably 1-6, and more preferably 1.5-5, and more preferably 2-4, and more preferably 2.25-3, and more preferably 2.3-2.7, and more preferably 2.4-2.6, and most preferably adjusted to about 2.5. An excess of solvent relative to the above ratios is desirable if melting point needs to be lowered. A higher NaBF4 salt ratio relative to the above ratios is desirable if a higher electrolyte boiling point is desired, since excess NaBF4 salt may promote super-alkaline reformation before NH3 evaporation occurs. An excess of salt relative to the above ratios is desirable if boiling point needs to be raised. For electrolyte formulations that do not contain NH3, i.e., purely organic amine-based, it is generally useful to find a salt:amine ratio that has a sufficiently high boiling point and minimizes electrolyte melting point. In the case of an excess of NH3 according to the invention, x can vary from greater than 0 to less than 0.5, more preferably greater than 0 to less than 1.0, more preferably greater than 0 to less than 2, more preferably greater than 0 to less than 2.4, most preferably greater than 0 to less than 2.5. In the case of an excess of salt according to the invention, x can vary from greater than 10 to 100, more preferably greater than 5 to 100, more preferably greater than 3 to 100, more preferably greater than 2.6 to 100, most preferably greater than 2.5 to 100.

[0034] Similarly, for the NaBH4·xNH3 system, with regard to the appropriate salt:ammonia ratio for metallic sodium cycling, x, the ratio of NH3 to salt, can range preferably from 0.5 to 6, and more preferably from 0.75 to 5, and more preferably from 1 to 3, and more preferably from 1.25 to 2, and more preferably from 1.3 to 1.7, and more preferably from 1.4 to 1.6, and is most preferably adjusted to about 1.5. An excess of solvent relative to the above ratio is desirable if the melting point needs to be lowered. An excess of salt relative to the above ratio is desirable if the boiling point needs to be raised. Compared to the NaBF4·xNH3 system, the NaBH4·xNH3 system can allow a higher salt ratio before freezing. For the excess of NH3 according to the invention, x can vary from 0 to less than 0.5, more preferably from 0 to less than 1.0, more preferably from 0 to less than 1.25, more preferably from 0 to less than 1.4, and most preferably from 0 to less than 1.5. In the case of excess salt according to the present invention, x may vary from greater than 5 to 100, more preferably from greater than 2 to 100, more preferably from greater than 1.75 to 100, more preferably from greater than 1.6 to 100, and most preferably from greater than 1.5 to 100.

[0035] Other electrolytes comprising one or more salts, at least one of which is sodium, a weakly coordinating boron, aluminum, phosphorus or chloride cored anion, and a solvent comprising a compound selected from the group of ammonia and organic amines, are possible according to the present invention. Cored means containing an element referred to herein as the molecular core element. Examples include, but are not limited to, BF4 - , BH4 - , PF6 - , ClO4 - , B(CN)4 - , BF3CN - , BF2(CN)2 - , BF(CN)3 - , BH3CN - , BH2(CN)2 - , BH(CN)3 - , Al(BH4)4 -In one embodiment of the present invention, the solvent may comprise one or more compounds selected from the group of organic amines, and preferably comprises ethylenediamine (EDA). When the electrolyte system is based on a monoamine, the appropriate salt:amine ratio for metallic sodium cycling may be such that the electrolyte system obtains the above-mentioned high concentration state; to achieve such a state, the monoamine:salt ratio x may vary preferably from 1 to 6, and more preferably from 2 to 5, and more preferably from 2.5 to 4, and more preferably from 2.75 to 2.5, and most preferably from 2.9 to 3.1. When the electrolyte system is based on a diamine, the appropriate salt:amine ratio for metallic sodium cycling may be such that the electrolyte system obtains the above-mentioned high concentration state; to achieve such a state, the monoamine:salt ratio x may vary preferably from 0.5 to 3, and more preferably from 1 to 2, and more preferably from 1.2 to 1.8, and most preferably from 1.4 to 1.6. When the electrolyte system is based on triamines, the appropriate salt:amine ratio for metallic sodium cycling may be such that the electrolyte system obtains the above-mentioned high concentration state; to achieve such a state, the monoamine:salt ratio x may vary preferably from 0.3 to 2, and more preferably from 0.5 to 1.5, and more preferably from 0.7 to 1.2, and most preferably from 0.9 to 1.1. Mixtures of the above electrolytes are possible according to the invention; the corresponding amine:salt ratios may be adjusted according to the principles described in this paragraph. (salt): xNH 3 The molar ratio x of (salt):y (organic monoamine) may be 1 to 5, the molar ratio y of (salt):z (organic diamine) may be 0.5 to 2.5, the molar ratio j of (salt):j (organic triamine) may be 0.3 to 2, or the molar ratio k of (salt):(nitrile) may be 1 to 5. The salt may be NaBF 4 and any mixtures containing one or more of the above electrolytes, (salt): xNH 3 or the molar ratio x of (salt):y (organic monoamine) may be 1 to 3.5, or the molar ratio z of (salt):z (organic diamine) may be 0.5 to 1.8, or the molar ratio j of (salt):j (organic triamine) may be 0.3 to 1.2, or the molar ratio k of (salt):(nitrile) may be 1 to 3.5. The salt may be NaBH 4 and any mixtures containing one or more of the above electrolytes, (salt): xNH 3 or the molar ratio x of (salt):y (organic monoamine) may be 2 to 3.5, or the molar ratio z of (salt):z (organic diamine) may be 1 to 1.8, or the molar ratio j of (salt):j (organic triamine) may be 0.7 to 1.2, or the molar ratio k of (salt):(nitrile) may be 2 to 3.5.

[0036] Surprisingly, it has been found that utilizing a mixture of salts can facilitate reaching the above new class of electrolytes when the solvent is completely or nearly completely in a superalkaline state. With NaBF4 salt alone, the highest possible dissolved salt concentration that can be obtained in ethylenediamine is NaBF4·3.33 ethylenediamine. With NaBr salt alone, the highest possible dissolved salt concentration that can be obtained in ethylenediamine is NaBr·3.15 ethylenediamine. However, when using a mixture of NaBF4 and NaBr salts, it is possible to obtain a more concentrated electrolyte with a composition of (yNaBF4+(1-y)NaBr)·xethylenediamine, where x<3. The preferred NaBF4:NaBr ratio is 0.1:0.9 to 0.9:0.1, more preferably 0.3:0.7 to 0.7:0.3, and even more preferably 0.4:0.6 to 0.6:0.4. Similarly, mixtures of other salts can be useful to achieve high concentration electrolytes with ethylenediamine or some other of the above nitrogen-containing solvents. In a preferred embodiment, the salt concentration is high enough to ensure that the electrolyte has essentially no free solvent molecules, hi a preferred embodiment, the electrolyte is an ionic liquid.

[0037] FIG. 1 shows comparative sodium deposition / stripping voltammograms for the above ammonia-based electrolytes.

[0038] While most current collector materials do not promote an anode substrate for smooth sodium deposits in the ammoniate electrolyte, it has been unexpectedly found that a copper current collector supports a smooth and well-adherent sodium deposit in the ammoniate electrolyte.

[0039] Surprisingly, it has been discovered that a subset of the above solvents support smooth deposition and cycling of metallic sodium on a copper current collector, even when the salt concentration is only 0.5-1.0 times the minimum concentration required for all solvent molecules involved in superalkali formation, i.e., less than that required for proper ionic liquid or local order formation. Thus, the electrolyte system may contain significant amounts of free amines or nitriles in this concentration range. Without being bound by theory, this behavior is likely caused by the thin SEI formation capacity of the utilized electrolyte, which is adequate for smooth metallic sodium deposition, and the beneficial effect of the still relatively high salt concentration on sodium dissolution or reactivity. The use of ethylenediamine solvents or mixtures of solvents mainly based on ethylenediamine are preferred in this region of operation due to the very high ionic conductivity and high sodium deposition rate capacity of the resulting electrolyte. The anode then achieves a current of nearly 10 mA / cm at 0.2 V overpotential. 2 A current of 1000 .mu.m can be achieved. The use of NaBF4 or NaBH4 salts with ethylenediamine is particularly preferred in this region of operation. This system achieves its maximum ionic conductivity at 4M salt concentration. Figure 10 shows the sodium deposition / stripping voltammogram for the above 4M ethylenediamine-based electrolyte. The salt concentration may be between 3 M and 5 M. The molar salt concentration may be at least 3.

[0040] The following table summarizes the observed qualities of the electrolyte classes disclosed in this invention. These liquid formulations, which may be, for example, ionic liquid type formulations, may also be useful for other applications beyond batteries and supercapacitors.

[0041] [Table 1]

[0042] With regard to cathode materials suitable for use in combination with the above electrolyte-substrate pairs, several high performance cathode materials are identified below for the construction of a complete electrochemical cell.

[0043] Poly-Anthraquinonyl Sulphide (PAQS) has been previously investigated as an electrode material in organic electrolytes [2]. However, this polymer has some solubility in organic solvents, which hinders its practical application in organic electrolytes. In contrast, PAQS was found to be insoluble in ammonia-based electrolytes during the cycling process and showed good electrochemical performance in terms of suitable energy density, high power density and cycling stability. The theoretical achievable capacity of this material is found to be about 210 mAh / g (referring to the active material).

[0044] Figure 2 shows the cyclic voltammograms for a PAQS-based electrode in NaI·3.3NH3 liquid ammonia.

[0045] Furthermore, it was found that previously unknown anthraquinonyl sulfide oligomers (AQS-oligomers) maintain the same insolubility as PAQS in the above liquids.

[0046] In general, vat dyes based on anthraquinone derivatives with high molecular weight, especially the anthrimidocarbazole family, as well as mixtures thereof, have been found to have good cathodic performance and, due to their insolubility in the electrolyte, allow long-term cycling with little loss of capacity. Although these materials are widely used for coloring and color development [3], their potential use as electrode materials has been unknown until now. The theoretically achievable capacity of these materials is about 240 mAh / g of active material mass. Some examples of these dyes are Indanthrone Blue (IB, also known as Pigment Blue 60, Vat Blue 4, CI 69800, CAS 81-77-6), Bisanthraquinoyl also known as Pigment Red 177 (also known as Cromophtal Red A3B, CI 65300, CAS 4051-63-2), Vat Orange 11 (Cibanoneyellow 3R, CI 70805, CAS 2172-33-0), Vat Brown 1 (Cibanon Brown, CI 70800, CAS 2475-33-4), Vat Green 8 (Indanthrene Khaki, Vat Khaki 2G, CI 71050, CAS 14999-97-4) and Vat Yellow 28 (Indanthren Yellow FFRK, CI 69000).

[0047] Other vat dyes based on anthraquinone derivatives, including but not limited to anthrimidocarbazole, are possible according to the invention. PAQS, AQS-oligomers and vat dyes are generally classified as carbonyl-based compounds. Other carbonyl-based compounds, especially those with low solubility in ammoniate and amine-based electrolytes, are possible according to the invention.

[0048] Figure 3 shows the cyclic voltammograms for an IB-based electrode in NaI·3.3NH3 liquid ammonia.

[0049] The ammoniate-based electrolyte has the additional utility of supporting simple preparation of anode sodium electrodeposition for cell assembly in the charged state. Due to the very high capacity of metallic sodium anodes, only very thin anode films are required, which are difficult to prepare by means other than electrodeposition. Electrodeposition of precise sodium thickness is also useful in preventing cell disassembly due to any excessively deep self-discharge during battery operation. The sodium on copper deposit remains non-dendritic and well adherent in the electrolyte, even at very high deposition current rates. An exemplary setup for such anode electrodeposition consists of a separator-coated flat sodium surface immersed in an ammoniate-based electrolyte. A copper film is placed on the separator, and an electrodeposition current is applied between the copper film and the sodium metal underneath. The copper film may be flipped midway through the process for uniform sodium deposition on both sides.

[0050] Sodium can also be deposited on both sides simultaneously in accordance with the present invention.

[0051] It has been found that battery cells can be assembled in a charged state by using a source of sodium without the need for uniform deposition across all anode surfaces. Sources of metallic sodium include, but are not limited to, bulk sodium, metallic sodium foil, metallic sodium powder, or mixtures thereof. This source of sodium strip is placed in electrical contact with the anode ends during assembly. For example, in the case of a pouch cell type cell assembly, a piece of sodium foil having the mass of the entire amount of sodium required in the cell can be placed on one of the anode stacks. Such an assembly has a two-fold advantage; the sodium deposition step can be omitted, and furthermore, the sodium reactivity is reduced in proportion to its complete surface area. After cell assembly, the cell can be discharged by simply connecting its ends through resistors, whereby the resistance value is adjusted to provide an appropriately slow discharge rate to ensure uniform discharge across all cathode materials without any significant potential drop gradient. As a general rule for the timing of this first discharge, the intended standard cell discharge rate is multiplied by the ratio of the longest cell dimension to the thickness of the electrode. For example, for a cell designed for a 15-minute discharge rate with 80 mm length and 0.1 mm cathode thickness, the appropriate timing for the first discharge is preferably on the order of 1 hour or more, more preferably 2 hours or more, more preferably 5 hours or more, more preferably 10 hours or more, more preferably 20 hours or more, more preferably 50 hours or more, more preferably 100 hours or more, and most preferably 200 hours. In the subsequent charge-discharge cycling, electrochemical reactions occur between the electrodes facing each other, resulting in essentially uniform metallic sodium deposition across all current collector surfaces. The assembly method of the present disclosure takes advantage of the enhanced ionic conductivity of the electrolyte formulation; in contrast, with conventional electrolyte formulations, such an assembly method would require a first discharge time several times longer.

[0052] Electrodes made from vat dye materials such as carbonyl type PAQS, AQS oligomers or IB are suitable for cell assembly in the charged state. Furthermore, for IB material-based electrodes, it was found that after being electrochemically reduced to their maximum reversible capacity, they remain stable in dry air for a long enough time to be utilized for cell assembly even in the discharged state. The ammonite-based electrolyte further supports the cost-effective electrochemical reduction of the cathode electrode, reducing it from the charged state to the discharged state. The prepared film is placed on this separator and then Na + The electrode can then be discharged at a suitable rate until a desired potential threshold (e.g., 1.4 V) is reached relative to the / Na reference. The effectiveness of this process stems from the high ionic conductivity of the ammoniate-based electrolyte and its self-infusion into the electrode porous structure. In particular, it has been found that an electrode based on indanthrone blue active material can be reduced to near its maximum reversible capacity within minutes through this method. Instead of electrochemical reduction of the cathode material, a chemical reduction route may also be utilized to obtain said cathode material in the discharged state. Such chemical reduction can be achieved, for example, by reducing the potential of the electrode relative to the Na reference, which should be less than 1.4 V to avoid degradation of the cathode material. + This can be accomplished by immersing the utilized cathode material in a liquid solution of a suitable reducing agent capable of discharging the cathode material to the desired potential threshold relative to a / Na reference, followed by filtering and drying the cathode material.

[0053] Carbonyl-type cored and based compounds are defined herein as compounds containing a carbonyl group or derivatives thereof. Other carbonyl-type / carbonyl-based compounds may be suitable for cell assembly in the charged state in accordance with the present invention in addition to vat dye materials such as PAQS, AQS oligomers or IBs.

[0054] Glass microfiber separators have been found to work with the liquid ammonia electrolytes described above, and in addition, these electrolytes wet well and are chemically compatible with separators that have hydrophilic surfaces, such as hydrophilic polypropylene separators.

[0055] In addition to the above, any other separator material is possible according to the present invention, including, but not limited to, polyethylene, polyvinyl chloride, polytetrafluoroethylene, polyvinylidene chloride, polyethylene, LDPE and HDPE. In the absence of inherent wetting, the electrolyte may be filled by application of sufficient pressure. The separator may include spandex, polypropylene, or polyethylene.

[0056] The following paragraphs describe the fabrication of energy density optimized battery cells utilizing metallic sodium anodes. High energy densities can be obtained from sodium anode-based cells using NaAlCl4·xSO2 type electrolytes. Under ambient pressure and room temperature conditions, x is preferably in the range of 1.5-2.0. The use of such electrolytes in conjunction with sodium in sodium precipitation-dissolution has been published in [4-6]. In addition to the use of pure NaAlCl4 salt for complexation with SO2, it has been found that salt mixtures consisting of NaAlCl4 and some mixtures of additional salts may also be used. Examples of suitable preferred additional salts for mixing with NaAlCl4 include NaBF4 and NaAl(BH4)4. A potential advantage of utilizing a mixture of salts is to achieve a lower salt:SO2 mass ratio at ambient temperature than is the case with NaAlCl4·xSO2. The term "SO2-based electrolyte" refers herein to the use of SO2 solvent with only NaAlCl4 salt or with a mixture of NaAlCl4 and some of the additional salts listed above.

[0057] According to the invention, x in the NaAlCl4·xSO2 electrolyte composition can vary from 0.5 to 10, more preferably from 1 to 5, more preferably from 1.25 to 3, most preferably from 1.3 to 2.5. Other salts or mixtures of salts, at least one of which contains sodium and / or boron, are possible according to the invention. (Salt): xSO 2 The molar ratio x may be 1-4.

[0058] There are several prior publications on the construction of battery cells utilizing NaAlCl4·xSO2 electrolyte [4-6]. These publications describe the construction of certain battery cell types in a charged state. However, it is more desirable to fabricate battery cells in a discharged state. Therefore, one objective of this specification is to disclose a practical solution for assembling a battery in a discharged state utilizing an SO2-based electrolyte that supports the deposition of metallic sodium. Copper foil immersed in an SO2-based electrolyte synthesized under ambient air corrodes rather rapidly, making it an unsuitable current collector substrate. Surprisingly, it has been found that by synthesizing the SO2-based electrolyte with the elimination of significant water contamination, and by ensuring that it is not subsequently exposed to air moisture, for example, copper foil immersed in this dry SO2-based electrolyte remains stable and uncorroded. Furthermore, it has been unexpectedly found that copper current collectors allow the preparation of smooth and well-adherent sodium deposits in the SO2-based electrolyte. Thereby, the combination of an essentially moisture-free SO2-based electrolyte and an anode current collector made from copper or a copper-based alloy supports the discharged state assembly of sodium-anode-based cells.

[0059] FIG. 4 shows a typical exemplary sodium deposition / stripping voltammogram of the above SO2-based electrolyte, also illustrating the time stability of the anodic operation.

[0060] Two cathode materials have been found that complement the above anode-electrolyte system, represent the discharged state of the cathode, and provide very high energy density of the entire battery cell. The first type of cathode material is NaCl. In a preferred embodiment, NaCl is deposited on a porous carbon framework. The porous carbon framework utilized has a pore size of 10 to 5000 m. 2 / g, more preferably at least 1000, more preferably at least 2000, and most preferably at least 3000m 2 / g。 Such deposition can be carried out, for example, by using anhydrous methanol as a solvent for NaCl. This is then deposited on a porous carbon framework by impregnating the carbon in the solution, evaporating the solvent, and drying.

[0061] Other solvents and precipitation techniques are possible in accordance with the present invention.

[0062] In a preferred embodiment, all or a portion of the NaCl or other sodium-containing material that makes up the cathode is not derived from the electrolyte. In a preferred embodiment, the NaCl or other sodium-containing material that makes up the cathode is precipitated into the prepared cathode prior to assembly. In one embodiment, the electrolyte salt is the source of less than 100%, more preferably less than 90%, more preferably less than 80%, more preferably less than 70%, more preferably less than 60%, and most preferably less than 50% of the NaCl or other sodium-containing material that makes up the cathode.

[0063] The resulting cathode material supports highly reversible battery cell operation and an average cell potential of about 3.2 V during the discharge sequence. 2 6 shows the cell potential evolution during charge / discharge cycling when using 1000 mA / g surface area. Without intending to be bound by theory, FIG. 6 shows the proposed chemical process during cycling of this cell system. During the charge cycle, 2Cl - +SO2 →SO2Cl2+2e- The oxidation reaction produces SO2Cl2. There are two significant properties of the carbon framework that make this charging cycle possible. First, NaCl is preferably crystallized in such a way that it does not passivate the electrode surface. In other words, a thin layer of NaCl does not significantly cover the carbon surface, and this explains why the charging potential starts at a relatively low value of 3.3-3.35 V. Second, carbon acts as a catalyst for SO2Cl2 formation, preventing the development of high Cl2 pressures [7]. Since most NaCl material is electrochemically desorbed from the carbon surface, the charging process also requires the reaction AlCl3 + NaCl → NaAlCl4, which consumes NaCl particles, as shown in Figure 6. The production of AlCl3 occurs at the carbon surface by electron transfer (2AlCl4 - +SO2→2AlCl3+SO2Cl2+2e -). The role of NaAlCl4 electrolyte salt is therefore also essential for the cell operation. The discharge operation is the reverse procedure. The downward sloping part of the discharge curve corresponds to the growth of the NaCl layer on the cathode surface along with the discharge of the electrochemical double layer of the carbon framework, while the flat part of the discharge curve corresponds to the growth of the desorbed NaCl particles. Thereby, the only limitation of the amount of NaCl that can be accommodated in the carbon pores is the condition that these pores must be completely blocked. Another prerequisite for reversible cell operation is that the SEI layer on the metal anode side must not be damaged during the discharge cycle. It was found that the SEI on the anode sodium metal remains stable up to at least 4.2V charging potential and suffers only limited damage up to 4.3V charging potential, but leads to the shuttle reaction of the cell if the charging potential exceeds the 4.3V threshold. The 3.8V at the end of charge in Figure 5 corresponds to the conversion of about half of the SO2 to SO2Cl2, and the charging potential threshold of 4.2V corresponds to the almost complete conversion of SO2 to SO2Cl2. This cell behavior is strikingly different from the Li-analogue of this cell structure, where attempts to recharge LiCl in LiAlCl4·xSO2 electrolyte fail due to the combined effects of LiCl passivation on the cathode side and SEI damage on the anode side [8]. The operating principle of this cell differs from the cell operation described in [4], which utilizes the redox reaction of the electrolyte itself. Thus, this disclosure describes a hitherto unknown battery cell chemistry.

[0064] When utilizing only NaAlCl4 salt, the energy density of the cell is optimal when it is assembled with the NaAlCl4·2SO2 electrolyte composition, i.e., utilizing the maximum possible SO2 concentration at ambient conditions. The theoretical energy density of such a cell utilizing NaCl active material can be calculated according to the following reaction: 4NaCl+NaAlCl4·2SO2⇔4Na+NaAlCl4·2SO2Cl2 This reaction corresponds to a theoretical capacity of 184 mAh / g in terms of the mass of materials and electrolyte. The corresponding energy density depends only slightly on the carbon framework surface area; the larger surface area carbon extends into the downward slope potential region compared to the plateau potential region of 3.18 V due to the larger double layer contribution. The total average discharge potential remains near the 3.2 V level with any suitable carbon framework. Thus, the corresponding theoretical energy density of this cell type is about 590 Wh / kg. It is also notable that the round trip energy efficiency has a value of about 85%. An exemplary cell was constructed by utilizing a Ketjen-Black carbon framework on an aluminum current collector on the cathode side, copper foil as the current collector on the anode side, and an essentially moisture-free NaAlCl4·2SO2 electrolyte. The internal space of the carbon framework was filled with xNaCl:NaAlCl4·2SO2 with a molar ratio x of 4:1 (i.e., a 2:1 molar ratio between NaCl:SO2) by the above-mentioned solvent evaporation-based NaCl deposition and subsequent electrolyte filling. The resulting cells can be charged, showing that this theoretical capacity can be obtained in practical cells over a very wide range.

[0065] Other molar ratios between xNaCl:NaAlCl4·2SO2 are possible according to the invention. x is preferably between 1 and 40, more preferably between 2 and 20, more preferably between 3 and 10, more preferably between 3.5 and 4, more preferably between 3.75 and 4.5, more preferably between 3.9 and 4.1. To reach as close as possible to the theoretical cell capacity, it is desirable for the molar ratio of NaCl:SO2 to be as close as possible to 2:1 (x close to 4). In practical cells, the amount of NaCl useful may be limited by the carbon morphology of the cathode or by melting point limitations in the intended operating temperature range. When an excess amount of NaAlCl4·2SO2 is desired, x / 2 may vary from greater than 0 to less than 1, more preferably greater than 0 to less than 1.5, more preferably greater than 0 to less than 1.75, more preferably greater than 0 to less than 1.9, and most preferably greater than 0 to less than 2. If an excess of NaCl is desired, x / 2 can vary from greater than 20 to 500, more preferably from greater than 10 to 400, more preferably from greater than 5 to 300, more preferably from greater than 2.5 to 200, and most preferably from greater than 2 to 100.

[0066] A second discovered cathode material for use with SO2-based electrolytes is a dehydrated Na2S2O4 (sodium dithionite):xNaAlCl4 mixture preferably utilized in a molar ratio of about 1:1 (x=1). In a preferred embodiment, the Na2S2O4:NaAlCl4 mixture is deposited onto a porous carbon framework. The porous carbon framework utilized has a pore size of 10 to 5000 m 2 / g, more preferably at least 1000, more preferably at least 2000, and most preferably at least 3000m 2 / g. Such deposition can be carried out, for example, by using anhydrous methanol, glyoxal, liquid formaldehyde or a methanol-formaldehyde mixture as a solvent for the Na2S2O4:NaAlCl4 mixture, which is then deposited onto a porous carbon framework by impregnating the carbon in the solution, evaporating the solvent, and drying.

[0067] The molar ratio x of dehydrated Na2S2O4 (sodium dithionite):NaAlCl4 may vary from 0.01 to 100, more preferably from 0.25 to 4, more preferably from 0.5 to 2, more preferably from 0.75 to 1.5, more preferably from 0.9 to 1.1, and most preferably about 1. If the cell is assembled with a highly concentrated electrolyte such as NaAlCl4·1.5SO2, an excess of Na2S2O4 is desirable, in which case x may vary from 0.01 to 100, more preferably from 0.25 to 5, more preferably from 0.5 to 1.25, and most preferably from 0.6 to 1. For example, the cell may be assembled with concentrated NaAlCl4·1.5SO2 to have a higher boiling point electrolyte during assembly, which is then diluted to a near optimal NaAlCl4·2SO2 concentration by the end of the first charge cycle by the use of excess Na2S2O4 in the cathode material.

[0068] The resulting cathode material supports highly reversible battery cell operation and provides an average cell potential of about 2.8 V during the discharge procedure. In contrast to NaCl, the Na2S2O4:NaAlCl4 mixture forms a thick layer on the carbon surface, thereby resulting in a thickness-dependent potential plateau for the recharge phase. Ketjen-Black material (1400 mm) was used as the carbon framework. 2When using 1000 mAh / g surface area, the maximum mass of rechargeable Na2S2O4:NaAlCl4 corresponds to about 10.5 g of Na2S2O4:NaAlCl4 mixture per gram of carbon, resulting in a recharge capacity of 1500 mAh / g of carbon mass. Although deposition of smaller amounts of Na2S2O4:NaAlCl4 is feasible, deposition of higher amounts of Na2S2O4:NaAlCl4 results in a recharge potential requirement exceeding the 4.2 V threshold, thereby decomposing the SEI on the anode side. Without being bound by theory, it is believed that oxidation of Na2S2O4 to SO2 occurs during the first charging phase. The subsequent discharge-recharge cycling is believed to be similar to the cell reaction process described in [4] utilizing NaAlCl4·2SO2 as the electrolyte. Although the operating principle of this cell type is similar to the cell operation described in [4], the cell composition and preparation process disclosed herein facilitates the desired discharge state preparation of a battery cell utilizing this cell chemistry.

[0069] The theoretical energy density of the above cell utilizing the Na2S2O4:NaAlCl4 cathode material can be calculated according to the following reaction: Na2S2O4+NaAlCl4→2Na+NaAlCl4·2SO2⇔2NaCl+NaAlCl2(SO2)2 This reaction corresponds to a theoretical capacity of 143 mAh / g for the deposited Na2S2O4:NaAlCl4 mass. The corresponding energy density depends on the carbon framework surface area; larger surface area carbons result in average discharge potentials closer to the initial discharge potential of 3.0 V. The Ketjen-Black carbon framework (1400 m 2When using 10.5 g / g surface area of ​​carbon, the average discharge potential is 2.8 V. This cell chemistry thereby corresponds to a theoretical energy density of about 400 Wh / kg. An exemplary cell was constructed by utilizing a Ketjen-Black carbon framework on an aluminum current collector on the cathode side, copper foil as the anode side current collector, and a dehydrated Na2S2O4:NaAlCl4 mixture. The interior space of the carbon framework is nearly completely filled after deposition of 10.5 g of Na2S2O4:NaAlCl4 mixture per gram of carbon. The cell construction is carried out by the above solvent evaporation based deposition and subsequent electrolyte filling. Since the Na2S2O4:NaAlCl4 mixture nearly fills the space in the charcoal carbon framework, the exemplary implementation shows that the theoretical capacity can be obtained in a practical cell to a very wide range.

[0070] It has been found that the two cathode compositions may be combined in a hybrid cathode and support higher energy densities than are feasible from each version on its own. The feasibility of this hybrid cathode material is based on the ability to recharge the Na2S2O4:NaAlCl4 mixture at near complete electrode space filling, i.e., it can occupy the remaining space in addition to NaCl, which is converted to NaAlCl4·2SO2 electrolyte during the recharge process. This high energy density cell is cycleable with the same reversibility as the individual compositions. The first charge cycle corresponds to the following: 4NaCl+Na2S2O4+NaAlCl4→6Na+NaAlCl4·2SO2Cl2 Without intending to be bound by theory, the improved energy density may be explained as a result of a two-step complete cell reaction: 6Na+NaAlCl4·2SO2Cl2⇔2Na+4NaCl+NaAlCl4·2SO2⇔6NaCl+NaAlCl2(SO2)2 The theoretical energy density of this optimized cell is calculated as follows: For all active materials, the capacity of the first discharge stage with SO2Cl2 reduction is 170mAh / g. As discussed above, the average potential during the first discharge stage is around 3.2V. The energy density of the first stage is 545Wh / kg. For all active materials, the capacity of the second discharge stage with SO2 reduction is 85mAh / g.

[0071] FIG. 7 shows the discharge potential evolution in the initial part of the second discharge stage (in terms of carbon mass capacity). The presence of a large amount of NaCl in the cell shifts the second stage discharge potential to about 0.6 V lower with respect to the theoretical SO2 reduction potential. Note that, unexpectedly, there is an initial increase in potential at the beginning of the discharge process, probably due to rearrangement of the electrode solid phase. Thereby, the average potential during the second discharge stage is 2.4 V. Since much of the internal space is already occupied by NaCl, the potential during SO2 reduction remains in a nearly constant region, thereby limiting the discharge capacity of this second stage to 85 mAh / g, which is in contrast to the 143 mAh / g capacity for the SO2 catholyte-based cell. As a result, this second discharge stage results in an energy density of 205 Wh / kg. Therefore, the achievable energy density of the discovered hybrid battery composition is 750 Wh / kg. This energy density is about 27% higher than what can be obtained from the NaCl active cathode material alone. An exemplary method for preparing a cell with this hybrid cathode is similar to the Na2S2O4:NaAlCl4 material-based cell preparation already described. The same solvents as described for Na2S2O4:NaAlCl4 mixture precipitation can be used, but the salt mixture used is preferably a 4:1:1 molar ratio between NaCl:Na2S2O4:NaAlCl4.

[0072] Other salt mixtures are generally possible according to the invention, where the active cathode material comprises a Na2S2O4 (sodium dithionite):xNaAlCl4 mixture, or an iNaCl:jNa2S2O4 (sodium dithionite):kNaAlCl4 mixture, where x, i, j and k define the molar ratios. Preferably, x is between 0.1 and 10, more preferably between 0.5 and 2, most preferably between 0.9 and 1.1. Preferably, i is between 1 and 50, j is between 0.2 and 5, k is between 0.2 and 5, more preferably, i is between 2 and 10, j is between 0.5 and 2, k is between 0.5 and 2, most preferably, i is between 3.9 and 4.1, j is between 0.9 and 1.1 and k is between 0.9 and 1.1. The active cathode material is iNaCl:jNa 2 S 2 O 4 (Sodium dithionite): kNaAlCl 4 It may comprise a mixture, where i is 3-5, j is 0.5-2, and k is 0.5-2.

[0073] While the cell formulations disclosed above contemplated the use of NaAlCl4 electrolyte salt, this salt can be partially replaced by a lighter salt to further increase cell-level energy density. In particular, for cells utilizing primarily only NaCl active cathode material, the NaAlCl4 salt participates only in the redox shuttle reaction described above and therefore may be replaced to a significant extent by another salt. It is desirable for the replacing salt to be lighter than NaAlCl4 and to support a sufficiently high electrolyte boiling point, preferably at least 20°C, at the preferred (sodium salt)·2SO2 solvent ratio. The additional salt may be Na / Na +It is further required that the salts have an oxidation potential higher than 4 V vs. 0 V and form a liquid electrolyte with SO2 at room temperature. Surprisingly, it has been discovered that some salts are suitable for SO2-based liquid electrolyte formulations and are miscible with NaAlCl4-containing SO2-based electrolytes in any ratio for the final electrolyte formulation. These newly discovered partial NaAlCl4 replacement salts share the common feature of being low melting salts, preferably with a melting point below 500°C, more preferably in the range of 100°C to 300°C, and are preferably sodium-containing, more preferably sodium and boron-containing, more preferably sodium, boron and carbon-containing, more preferably sodium, boron, carbon and nitrogen, or sodium, boron, carbon and aluminum-containing, and most preferably selected from the group of NaB(CN)4, NaBF3CN, NaBF2(CN)2, NaBF(CN)3 or NaAl(BH4)4. Other low melting sodium-containing salts are possible according to the invention.

[0074] Instead of assembling the cell in a fully discharged state, it is also feasible to assemble the cell in a partially charged state. One means of implementing a partially charged state is to inject NaCl into the cathode framework and deposit sodium metal on the anode side. The cell is then filled with SO2-based electrolyte and sealed. This cell preparation represents an assembly in a partially charged state, since upon assembly the cell has discharge active material on the cathode side (NaCl) and charge active material on the anode side (metallic sodium that can react with the SO2-based electrolyte). Other means of partially charged assembly are possible.

[0075] Considering a 4:1 NaCl:NaAlCl4·2SO2 cell formation, the mass of the NaAlCl4 salt represents 35% of the total electrolyte + active materials mass. With an exemplary 80% NaAlCl4 substitution, a nearly 20% reduction in the total electrolyte + active materials mass can be achieved.

[0076] In addition to the preferred discharged state assembly method, another desirable aspect of the cost-effective cell assembly according to the present invention is a simple electrolyte filling method. Good wettability of the cell structure is a useful advantage for cost-effective cell construction. With sufficient wettability, electrolyte filling is a simple process because the electrolyte self-injects into the cell and makes complete contact with all active materials. Without good wettability, cell assembly must use a more complicated filling system that first creates a vacuum and then forces the electrolyte into the cell structure by application of high pressure. With respect to the anode, the metal surface provides good wettability, which is one advantage of working with metal anode-based cells. With respect to the separator, it has been found that the porous polypropylene-type separators currently widely utilized in Li-ion cells are not wettable with SO2-based electrolytes. However, it has been found that porous polyethylene-type separators provide good wettability for SO2-based electrolytes. In addition to pure polyethylene-based separators, separators that wet well also include polyethylene containing composite separator structures, such as polypropylene-polyethylene composite separators. In addition to its good wetting properties, this separator type was found to be chemically stable during cell cycling with the respective electrolytes.

[0077] Other separator materials are possible in accordance with the present invention.

[0078] With regard to wetting of the cathode structure, it was found that the SO2-based electrolyte self-injects into the cathode electrode when the binder material is utilized in a ratio that is less than 10% by weight with respect to the carbon mass. Conventional electrode fabrication techniques require approximately 10% binder in the electrode, but it has been recently disclosed that, for example, with dry electrode processing, binder ratios of less than 10% can be utilized [9]. An exemplary electrode preparation method requires the use of 6% by weight of PTFE or heat-treated PAN binder material with respect to the carbon mass, and the preparation of the cathode electrode by a dry processing method [9]. With these findings regarding anode, separator, and cathode wetting, the electrolyte can be easily injected into the cell structure during the assembly process. The binder material may be PTFE, PVDF, styrene-butadiene rubber (SBR) or heat treated polyacrylonitrile.

[0079] Preferably, the weight percent of the binder is 1-20, more preferably 2-10, more preferably 3-8, and most preferably 4-7.

[0080] Wetting tests were carried out on electrodes made from Ketjen-Black carbon containing 6 wt. % PTFE by weight relative to the carbon mass, with or without 122 wt. % injected NaCl by weight relative to the carbon mass. The electrodes were impregnated in electrolyte, and electrolyte infusion into the electrode structure was confirmed by gravimetric measurements before and after impregnation. Wetting tests of the separator were carried out similarly.

[0081] According to one embodiment of the present invention, during the first charge of a cell containing NaCl active material, the generated SO2Cl2 may cross over onto the anode surface before being completely covered by the sodium film, thereby resulting in a continuous shuttle reaction on the anode side when the charge reaction is performed very slowly. It has been found that a cation conductive film may be advantageously utilized between the separator and the anode surface, which effectively inhibits the crossover of SO2Cl2, thereby providing greater flexibility for performing the first charge cycle. Any cation conductive film stable in a SO2-based electrolyte is suitable for this purpose, and a Nafion film of thickness in the micrometer range is found to be particularly suitable. Such a film may be deposited on the separator or anode current collector during cell preparation, or may be a free-standing film inserted between the separator and current collector. Any means of cation conductive film deposition and any sodium conductive film material are possible according to the present invention, provided that the utilized film material is compatible with the SO2-based electrolyte.

[0082] With respect to the cathode and anode of the present invention, the cathode and / or anode may be deposited on a conductive current collector / mechanical support. The current collector / mechanical support may comprise a metal or have a metallic surface. The metallic surface may comprise, for example, aluminum Al, Cu, Ni, Cr, Pd, Pt, Au, Ag and / or any other suitable metal. The metallic current collector surface may be deposited on a mechanical support, for example, a non-metallic support. The metallic current collector surface may be deposited by any means, including, but not limited to, electrochemical deposition, electrospray, thermal spray, physical vapor deposition, chemical vapor deposition, atomic layer deposition electroless deposition. According to the present invention, a material comprising carbon may be applied onto the conductive current collector / mechanical support film.

[0083] A preferred embodiment of the present invention includes an electrochemical cell for a secondary battery or supercapacitor in which the electrolyte comprises a concentrated solution of NaBF4 or NaBH4 salt in ammonia, having the approximate formulas of NaBF4·2.5NH3 and NaBH4·1.5NH3, respectively. The concentration of the electrolyte salt can vary around these indicated preferred concentration values, for example, from NaBF4·2.3NH3 to NaBF4·2.8NH3 and NaBH4·1.2NH3 to NaBH4·1.9NH3, respectively, depending on the desired melting and boiling points. In the electrochemical cell of the preferred embodiment, the anode current collector substrate is selected from copper or an alloy thereof, which allows for deposition of the metallic active material on the anode. In the preferred embodiment electrochemical cell, the active cathode material is selected from poly-anthraquinonyl-sulfide polymers, AQS-oligomers and carbonyl type compounds including indanthrone blue or similar anthrimidocarbazole compounds, utilized in the cell assembly either in their initial state or in the reduced sodium salt state. In a preferred embodiment of the cell preparation method, the metallic sodium film on the copper current collector is obtained by electrodeposition against a metallic sodium counter electrode in an electrolyte environment. In a preferred embodiment of the cell preparation method, the controlled reduction of the cathode from a charged state to a discharged state is by electrochemical reduction against a metallic sodium counter electrode in an electrolyte environment. In preferred embodiment electrochemical cells, the electrolyte comprises NaAlCl4·xSO2, ((1-y)NaBF4+yNaAlCl4)·xSO2 or ((1-y)NaAl(BH4)4+yNaAlCl4)·xSO2, preferably in the ratio of NaAlCl4·2SO2, and the anode current collector substrate is selected from copper or its alloys to enable deposition of active materials on the anode. The concentration of the electrolyte salt can vary around the preferred ·2SO2 concentration value depending on the desired melting and boiling points. In preferred embodiment electrochemical cells, the electrolyte has low water contamination to promote deposition of metallic active materials on the anode. In preferred embodiment electrochemical cells, the active cathode material comprises NaCl.In preferred embodiment electrochemical cells, the active cathode material comprises a Na2S2O4 (sodium dithionite):NaAlCl4 mixture, preferably in a 1:1 molar ratio, or NaCl:Na2S2O4 (sodium dithionite):NaAlCl4, preferably in a 4:1:1 molar ratio. In preferred embodiment electrochemical cells, the separator contains a hydrophilic surface, such as a hydrophilic type porous polypropylene separator, to support good wetting of the electrolyte. In preferred embodiment electrochemical cells, the separator includes or contains porous polyethylene in its structure to support good wetting of the electrolyte. In preferred embodiment electrochemical cells, the cathode has a binder ratio of 10% by weight or less, preferably 5-6% by weight, to support electrolyte self-injection into the electrode. In preferred embodiment electrochemical cells, the cell is prepared in a discharged state, utilizing only the anode current collector as the cathode of the assembled cell.

[0084] A novel polymeric high energy cathode material has also been discovered that is a good complement to the electrolyte formulations disclosed above. This cathode material is a copolymer of triazine and quinone rings. Its structure is shown in Figure 7. This material has the formula [C8H2N2O2Na2] n and during its synthesis it self-assembles into a microporous structure in which distinct 1-2 nm wide channels facilitate iontophoresis. This material is a Na / Na + It is reversibly cycleable to a low potential limit of 1.3 V vs. 0.05 V. Both the triazine and quinone rings contribute to its cycling capacity, resulting in a very high specific capacity measured to be in excess of 300 mAh / g.

[0085] An exemplary procedure for the synthesis of the triazine-quinone copolymer may be based on 2,5-dichloro-1,4-hydroquinone starting material. + From Na +This precursor is first stirred in an aqueous or alcohol-based NaOH solution to achieve the exchange to ions. After subsequent evaporation of the solvent, it is stirred in a hot DMSO-based solution of NaCN to achieve the ligand exchange from chloride to cyanide. The appropriate temperature range for this reaction is 100-150 °C. It is then mixed with a NaOH-NaCl salt eutectic and subjected to an io-thermal heat treatment in the temperature range of 300-400 °C. The microporous polymer structure self-assembles during this heat treatment. Then, after washing out the salt and filtration, the final polymer is obtained.

[0086] One embodiment of the present invention includes an electrochemical cell in which the active cathode material comprises a triazine-quinone copolymer. EXAMPLES

[0087] Working Example Preparation of electrolyte Example 1 Liquid ammoniate NaI·3.3NH3 was synthesized according to [1].

[0088] Example 2 Liquid ammoniate NaBF4·2.5NH3 was synthesized by condensing excess ammonia in 23 g of NaBF4 at -50°C. The reaction was carried out under magnetic stirring, resulting in a colorless solution. Once prepared, an excess of metallic sodium was used to purify the solution, which turned blue due to the generation of solvated electrons that remove impurities such as oxygen and water. Finally, the solution was allowed to approach room temperature, and the excess ammonia was evaporated to form the final ammoniate. The composition is easy to follow by continuous weighing.

[0089] Example 3 Liquid ammoniate NaBH4·1.5NH3 was synthesized according to the general procedure in Example 2. The initial amount of NaBH4 was 13 g.

[0090] Example 4 The NaAlCl4·2SO2 electrolyte was synthesized according to [4].

[0091] Its boiling point of about 20 °C was observed. The NaAlCl4:1.5SO2 electrolyte was synthesized following the same initial procedure and then heated to evaporate SO2 until NaAlCl4·1.5SO2 was reached. A boiling point of about 40 °C was observed for NaAlCl4:1.5SO2.

[0092] Preparation of active materials Example 5 PAQS active material was prepared according to [2]. Anhydrous Na2S was obtained by removing the water of hydration from Na2S·9H2O by drying in several steps: first, Na2S·9H2O was heated at 50 °C for 240 min, then the temperature was increased to 80 °C for 240 min. In the third step, the temperature was 120 °C for 2 h. Finally, the temperature was increased to 160 °C for 2 h to obtain dry Na2S.

[0093] Example 6 The active material for the indanthrone blue-based electrode was prepared by a solvothermal method. Indanthrone blue and carbon nanotubes, as a conductive carbon additive, were dispersed in N-methylpyrrolidine in a ratio of 7 / 5 at room temperature under magnetic stirring to form a slurry. The mixture is then heated in an autoclave at 180°C overnight. The product was filtered and washed with deionized water several times. Finally, it was dried in a vacuum oven at 150°C for 3 hours and then at 80°C for 8 hours.

[0094] Preparation of the anode Example 7 60 wt% of PAQS from Example 5, 30 wt% of carbon nanotubes and 10 wt% of PTFE (polytetrafluoroethylene) as a binder were mixed in a ball mill at 350 rpm for 2 hours. The homogenous mixture was then pressed onto a carbon-coated aluminum foil using a hydraulic press at 1.5 tons for 2 minutes. The final electrode was dried overnight in a vacuum oven at 60°C. The average electrode material mass was 1.1 cm 2 The substrate area covering is 8mg.

[0095] Example 8 90% by weight of the active material from Example 6 was dispersed in N-methylpyrrolidine with 10% by weight of PVDF (polyvinylidene fluoride) at room temperature under magnetic stirring to form a slurry. The slurry was then coated onto a carbon-coated aluminum foil. Finally, the electrode was dried overnight at 80°C. The average material was 1.1 cm 2 The mixture is 3.5 mg in volume.

[0096] Example 9 90 wt% of the mixture of indanthrone blue and carbon nanotubes from Example 6 and 10 wt% of PTFE were mixed in a ball mill at 350 rpm for 2 hours. The homogenous mixture was pressed onto carbon-coated aluminum using a hydraulic press at 1.5 tons for 2 minutes. Finally, the electrode was dried in a vacuum oven at 130°C for 5 hours.

[0097] Example 10 The electrode framework was prepared from a mixture of 94 wt% Ketjen-Black carbon and 6 wt% PTFE. This mixture was dry pressed onto a carbon-coated aluminum current collector following the dry pressing procedure of [9]. NaCl was dissolved in anhydrous methanol and the solution was drop cast onto the electrode in a sufficient amount to obtain a mass ratio of approximately 2.5:1 between NaCl and carbon. Finally, the electrode was dried under vacuum overnight at 80 °C.

[0098] Preparation of the cathode for state-of-charge assembly Example 11 The sodium electrode was placed on a copper substrate in the above ammonia solution at a constant potential (Na + The alloy was prepared by electrodeposition at a temperature of -0.1 V vs. Na.

[0099] Preparation of rechargeable batteries Example 12 A rechargeable sodium battery was prepared having a sodium anode, a 420 micron thick glass microfiber separator impregnated with NaI·3.3NH3 electrolyte, and the PAQS-based cathode from Example 7. The battery prepared for this example had a capacity of 150 mA·h·g -1 PAQS The maximum cathode capacity of the cell was 1.2 kcal / s. + The cells were subjected to 7 min rapid discharge / charge cycles using limits of 2.6 V to 1.2 V vs. Na. The average utilization of the active material capacity during the first 50 cycles was 64%.

[0100] Example 13 A rechargeable sodium battery was prepared having a sodium anode, a 420 micron thick glass microfiber separator impregnated with NaI·3.3NH3 electrolyte, and the indanthrone blue-based cathode from Example 8. The battery prepared for this example had a capacity of 150 mA·h·g -1 IB The cell showed a maximum cathode capacity of about 600 cycles. + The cells were subjected to 5 min rapid discharge / charge cycles using limits of 2.5 V to 1.3 V vs. Na. The average utilization of the active material capacity was 62%.

[0101] Example 14 A rechargeable sodium battery was prepared having a sodium anode, a 420 micron thick glass microfiber separator impregnated with NaBF4·1.5NH3 electrolyte, and the indanthrone blue-based cathode from Example 8. The battery prepared for this example had a capacity of 200 mA·h·g -1IB The cell showed a maximum cathode capacity of about 100 cycles. + The cells were subjected to 5 min rapid discharge / charge cycles using limits of 3 V to 1.4 V vs. Na. The average utilization of the active material capacity during the discharge / charge process was 77%.

[0102] Example 15 A rechargeable sodium battery was prepared having a sodium anode, a 420 micron thick glass microfiber separator impregnated with NaI·3.3NH3 electrolyte, and an indanthrone blue-based cathode from Example 9. The battery prepared for this example exhibited approximately 550 cycles and insignificant capacity loss. The cell contained a Na + Various C-rates were subjected using limits of 2.5 V to 1.4 V vs. / Na (Figure 8).

[0103] Example 16 A rechargeable sodium battery was prepared with a copper foil cathode, a 15 micron thick porous polyethylene separator, and a NaCl-based anode from Example 10. Both the separator and anode were impregnated in NaAlCl4·2SO2 electrolyte. The battery prepared for this example showed a capacity of 435 mAh / g of NaCl mass.

[0104] Example 17 The electrolyte was prepared from 4 molar NaBF4 dissolved in ethylenediamine. A rechargeable sodium battery was prepared with a sodium anode, a 420 micron thick glass microfiber separator impregnated with NaBF4·1.5NH3 electrolyte, and the indanthrone blue-based cathode from Example 8. The battery prepared for this example had a capacity of 200 mA·h·g -1 IB The cell capacity remained stable during cycling, and examination revealed no signs of either significant electrolyte reaction or cathode material crossover, indicating a bright sodium surface.

[0105] Example 18 A rechargeable battery was prepared according to the same procedure as in Example 16, but using a sodiated Nafion-coated polyethylene separator instead of a plain polyethylene separator. A micrometer-thick Nafion coating was deposited on the separator according to the procedure described in

[10] . The cell showed the same capacity and cycling stability as the cell in Example 16.

[0106] reference: 1. Goncalves et al. Portugaliae Electrochimica Acta (2006); 24: 117-127. 2. Deng et al. Nature Scientific Reports (2013); 3: 2671. 3. Kirk-Othmer Encyclopedia of Chemical Technology. 4. G. Jeong et al. Nature Scientific Reports (2015); 5:12827. 5.Patent number US 2014 / 0220428 A1 6.Patent number EP 2860799 A1 7. R McKee et al. Industrial and Engineering Chemistry (1924); 16:4 8. S Hossain et al. LABCOM Contract DAAL01-89-C-0939; 2nd Quarterly Report 9.Patent number DE 10 2012 203 019 A1 10. Bauer et al. Chem. Commun. (2014); 50:3208-3210.

Claims

1. a) a cathode comprising a sodium-containing cathode material and a carbon-containing cathode material; b) an electrically conductive anode current collector having essentially no metallic sodium active material on its surface in the discharged state of the cell; c) an electrolyte disposed between the cathode and the anode current collector, the electrolyte comprising a solvent and a sodium-containing electrolyte salt; and d) an electrodeposited layer of metallic sodium active material on said anode current collector in a charged state; 1. An electrochemical cell comprising:

2. a) a cathode comprising a sodium-containing cathode material, at least a portion of which is not derived from a sodium-containing electrolyte salt, and an electrically conductive anode current collector; b) an electrolyte disposed between the cathode and the anode current collector, the electrolyte comprising a solvent and a sodium-containing electrolyte salt; and c) an electrodeposited layer of metallic sodium active material on said anode current collector in a charged state; An electrochemical cell comprising: An electrochemical cell, wherein the anode current collector has essentially no metallic sodium active material on a surface thereof when the electrochemical cell is assembled and / or when the electrochemical cell is in a fully discharged state.

3. 3. The cell of claim 1 or 2, wherein the sodium-containing cathode material is inorganic.

4. The solvent of the electrolyte is sulfur dioxide (SO 2 4. The cell according to claim 1 , comprising:

5. The solvent of the electrolyte is ammonia (NH 3 5. The cell of claim 1, further comprising an organic amine, or a mixture thereof.

6. 6. The cell of claim 5, wherein the organic amine is selected from ethylenediamine, 1,3-diaminopropane, diethylenetriamine, n-butylamine, isopropylamine, ethylamine, or methylamine, including any mixtures containing one or more of said organic amines.

7. The cell of any one of claims 1 to 6, wherein the sodium-containing electrolyte salt has a melting point of less than 500°C.

8. 8. The cell of claim 7, wherein the sodium-containing electrolyte salt has a melting point of 100 to 300°C.

9. 10. The cell of claim 8, wherein the sodium-containing electrolyte salt also contains boron.

10. The cell of any one of claims 8 to 9, wherein the sodium-containing electrolyte salt also contains carbon.

11. The cell of any one of claims 8 to 10, wherein the sodium-containing electrolyte salt also contains nitrogen or aluminum.

12. The sodium-containing electrolyte salt is NaAlCl 4 , NaBF 4 , NaBH 4 , NaB(CN) 4 , NaBF 3 CN, NaBF 2 (CN) 2 , NaBF(CN) 3 or NaAl(BH 4 ) 4 or any combination thereof.

13. (Sodium-containing electrolyte salt): xSO 2 The cell according to any one of claims 1 to 12, wherein the molar ratio x is between 1 and 4.

14. The sodium-containing cathode material is 2 S 2 O 4(Sodium dithionite): xNaAlCl 4 Mixture or iNaCl:jNa 2 S 2 O 4 (Sodium dithionite): kNaAlCl 4 A cell according to any one of claims 1 to 13, comprising a mixture, wherein x, i, j and k define a molar ratio.

15. The sodium-containing cathode material is 2 S 2 O 4 (Sodium dithionite): xNaAlCl 4 The cell of claim 14, comprising a mixture, the molar ratio x being between 0.5 and 2.

16. The cell of any one of claims 1 to 15, wherein the sodium-containing cathode material comprises NaCl.

17. The cell of any one of claims 1 to 16, assembled in either a fully or partially discharged state.

18. The sodium-containing cathode material is iNaCl:jNa 2 S 2 O 4 (Sodium dithionite): kNaAlCl 4 18. The cell of any one of claims 16 to 17, comprising a mixture, wherein i is from 3 to 5, j is from 0.5 to 2, and k is from 0.5 to 2.

19. a) a cathode comprising a sodium-containing cathode material, and an electrically conductive anode current collector; b) SO 2 an electrolyte disposed between the cathode and the anode current collector, the electrolyte comprising a solvent and a sodium-containing electrolyte salt; and c) a cationically conductive film between the cathode and anode, the cationically conductive film being sodium 1. An electrochemical cell comprising:

20. 20. The cell of claim 19, wherein a porous separator film is provided between the anode current collector and the cathode.

21. the cation-conducting film is deposited on the anode current collector; or The cell of any one of claims 19 to 20, wherein the cell further comprises a separator between the anode current collector and the cathode, and the cation-conducting film is deposited on the separator.

22. The cell of any one of claims 19 to 21, wherein the cationically conductive film inhibits the migration of sulfuryl chloride.

23. a) an anode comprising a cathode and at least one anode current collector; and b) i. one or more nitrogen-containing solvent precursors; ii. at least one sodium-containing electrolyte salt comprising a sodium cation and a sulfonyl-containing anion; an electrolyte disposed between the cathode and the anode comprising:

1. An electrochemical cell comprising:

24. 24. The cell of claim 23, wherein the sodium-containing electrolyte salt molarity is at least 3 moles / liter.

25. The sodium-containing electrolyte salt is NaBF 4 , NaBH 4 , NaPF 6 , NaClO 4 , NaB(CN) 4 , NaBF 3 CN, NaBF 2 (CN) 2 , NaBF(CN) 3 , NaBH 3 CN, NaBH 2 (CN) 2 , NaBH(CN) 3 , NaAl(BH 4 ) 4, NaBr, sodium bis-(trifluoromethylsulfonyl)imide (NaTFSI), sodium bis(fluorosulfonyl)imide (NaFSI), sodium trifluoromethanesulfonate (Na triflate), or any mixture or combination thereof.

26. The nitrogen-containing solvent precursor is ammonia (NH 3 ), one or more organic amine-based liquids, one or more nitrile-based liquids, or a mixture containing one or more of said nitrogen-containing solvent precursors.

27. 27. The cell of claim 26, wherein the organic amine is selected from ethylenediamine, 1,3-diaminopropane, diethylenetriamine, n-butylamine, n-propylamine, isopropylamine, ethylamine, methylamine, pyridine or mixtures thereof, and the nitrile is selected from acetonitrile, propiononitrile, or mixtures containing one or more of the organic amines.

28. 28. The cell of any one of claims 23 to 27, wherein the sodium-containing electrolyte salt concentration is high enough to constitute an electrolyte having essentially no free solvent molecules.

29. 28. The cell of any one of claims 23 to 27, wherein the sodium-containing electrolyte salt concentration is high enough to constitute an ionic liquid type electrolyte.

30. (sodium-containing electrolyte salt): xNH 3or the molar ratio y of (sodium-containing electrolyte salt):y (organic monoamine) is 1 to 5; or the molar ratio z of (sodium-containing electrolyte salt):z (organic diamine) is 0.5 to 2.5; or the molar ratio j of (sodium-containing electrolyte salt):j (organic triamine) is 0.3 to 2; or the molar ratio k of (sodium-containing electrolyte salt):(nitrile) is 1 to 5. The cell of any one of claims 23 to 29.

31. The sodium-containing electrolyte salt is NaBF 4 and (sodium-containing electrolyte salt): xNH 3 or the molar ratio y of (sodium-containing electrolyte salt):y (organic monoamine) is 1 to 3.5; or the molar ratio z of (sodium-containing electrolyte salt):z (organic diamine) is 0.5 to 1.8; or the molar ratio j of (sodium-containing electrolyte salt):j (organic triamine) is 0.3 to 1.2; or the molar ratio k of (sodium-containing electrolyte salt):(nitrile) is 1 to 3.

5.

32. The sodium-containing electrolyte salt is NaBH 4 and (sodium-containing electrolyte salt): xNH 3 or the molar ratio y of (sodium-containing electrolyte salt):y (organic monoamine) is 2 to 3.5; or the molar ratio z of (sodium-containing electrolyte salt):z (organic diamine) is 1 to 1.8; or the molar ratio j of (sodium-containing electrolyte salt):j (organic triamine) is 0.7 to 1.2; or the molar ratio k of (sodium-containing electrolyte salt):(nitrile) is 2 to 3.

5.

33. The cell of any one of claims 23 to 30, wherein the electrolyte comprises one or more SEI-forming amine or nitrile solvents.

34. the electrolyte comprises one or more SEI-forming amine or nitrile solvents; The SEI-forming amine or nitrile solvent is ethylenediamine, and the sodium-containing electrolyte salt is NaBF 4 or NaBH 4 13. The cell of claim 12, wherein:

35. 34. The cell of claim 33, wherein the sodium-containing electrolyte salt concentration is between 3M and 5M.

36. The cell of any one of claims 23 to 30, 33 and 35, wherein a source of metallic sodium active material is provided which is electrodeposited onto the anode current collector.

37. 37. The cell of claim 36, wherein the metallic sodium active material electrodeposited on the anode current collector is provided by bringing the source of metallic sodium active material into electrical contact with an end of the anode current collector.

38. The cathode converts sodium ions (Na ions) from the sodium metal active material during a first discharge cycle of the electrochemical cell. + 38. The cell of claim 37, wherein the cell receives

39. 39. The cell of any one of claims 36 to 38, wherein the source of metallic sodium active material comprises bulk sodium, metallic sodium foil, metallic sodium powder, or a mixture thereof.

40. The cell of any one of claims 1 to 39, comprising a separator that has a higher surface energy than the electrolyte or supports good wetting of the separator by the electrolyte.

41. The cell of any one of claims 1 to 40, comprising a separator comprising spandex, polypropylene, or polyethylene.

42. The cell of any one of claims 1 to 41, wherein the sodium-containing electrolyte salt comprises boron, aluminum, fluoride, chloride and / or hydrogen.

43. The cell of any one of claims 1 to 42, wherein the cathode comprises a carbon-containing cathode material, the carbon-containing cathode material being a carbonyl or anthrimidocarbazole containing compound.

44. 44. The cell of claim 43, wherein the carbonyl or anthrimidocarbazole containing compound comprises poly-anthraquinonyl-sulfide polymer, AQS-oligomer or indanthrone blue.

45. The cell of any one of claims 1 to 22, wherein at least a portion of the sodium-containing cathode material is in its pristine state or in a reduced sodium salt state.

46. 46. ​​The cell of claim 45, wherein the cathode comprises a carbon-containing cathode material, the carbon-containing cathode material being CNT, fullerene, CNB, graphene, graphite, Ketjen-Black, mesoporous carbon, activated carbon, carbon nanohorn, carbon nanofoam, Q-carbon, T-carbon, Y-carbon, nanocarbon, carbon nanoparticles and / or porous carbon.

47. The cell of any one of claims 1 to 46, wherein the cathode comprises a binder material.

48. 48. The cell of claim 47, wherein the binder material is PTFE, PVDF, styrene-butadiene rubber (SBR), or heat-treated polyacrylonitrile.

49. The cell of any one of claims 1 to 22, wherein the sodium-containing cathode material is deposited on an electrically conductive cathode current collector / mechanical support.

50. The cell of any one of claims 1 to 49, wherein the cathode and / or anode current collector comprises a metal or has a metallic surface.

51. 51. The cell of claim 50, wherein the cathode and / or anode current collector comprises aluminum Al, Cu, Ni, Cr, Pd, Pt, Au and / or Ag, or an alloy comprising Al, Cu, Ni, Cr, Pd, Pt, Au and / or Ag.

52. A cell according to any one of claims 50 to 51, wherein the metal surface is deposited on a mechanical support to form a cathode current collector and / or a mechanical support.

53. 53. The cell of any one of claims 40 to 52, wherein the cathode comprises a carbon-containing cathode material, the carbon-containing cathode material being applied onto a conductive cathode current collector / mechanical support.

54. The cell of any one of claims 1 to 53, wherein the cathode comprises less than 10% by weight of binder.

55. 55. The cell of claim 54, wherein the cathode comprises 4 to 7 weight percent binder.

56. The cell of any one of claims 1 to 18, wherein the metallic sodium active material is electrodeposited onto the anode current collector during charging of the electrochemical cell.

57. 57. The cell of claim 56, wherein the metallic sodium active material is smooth.

58. The cell of any one of claims 1 to 57, wherein the cathode comprises a triazine-quinone copolymer.

59. A battery or supercapacitor comprising an electrochemical cell according to any one of claims 1 to 58.

60. a) providing a cathode comprising a sodium-containing cathode material, and a conductive anode current collector having essentially no metallic sodium active material on a surface thereof; b) providing an electrolyte between the cathode and the anode current collector, the electrolyte comprising a solvent and a sodium-containing electrolyte salt; and c) electrodepositing metallic sodium active material on said anode current collector during a first charge cycle. A method for manufacturing an electrochemical cell, comprising:

61. a) providing a cathode comprising a sodium-containing cathode material and an electrically conductive anode current collector; b) providing an electrolyte between the cathode and the anode current collector, the electrolyte comprising a solvent and a sodium-containing electrolyte salt; and c) electrodepositing metallic sodium active material on said anode current collector during a first charge cycle. A method for manufacturing an electrochemical cell, comprising: The method, wherein the anode current collector has essentially no metallic sodium active material on a surface thereof when the electrochemical cell is assembled and / or when the electrochemical cell is in a fully discharged state.

62. The method of any one of claims 60 to 61, wherein the sodium-containing cathode material is inorganic.

63. The solvent of the electrolyte is sulfur dioxide (SO 2 63. The method of any one of claims 60 to 62, comprising:

64. The solvent of the electrolyte is ammonia (NH 3 64. The method of any one of claims 60 to 63, comprising a tert-butyl ether or an organic amine, or any mixture thereof.

65. 65. The method of claim 64, wherein the organic amine is selected from ethylenediamine, 1,3-diaminopropane, diethylenetriamine, n-butylamine, isopropylamine, ethylamine, or methylamine, including mixtures comprising one or more of said organic amines.

66. 66. The method of any one of claims 60 to 65, wherein the sodium-containing electrolyte salt has a melting point of less than 500°C.

67. 67. The method of claim 66, wherein the sodium-containing electrolyte salt has a melting point of 100 to 300°C.

68. 68. The method of claim 67, wherein the sodium-containing electrolyte salt also contains boron.

69. 69. The method of any one of claims 67 to 68, wherein the sodium-containing electrolyte salt also comprises carbon.

70. 70. The method of any one of claims 67 to 69, wherein the sodium-containing electrolyte salt also contains nitrogen or aluminum.

71. The sodium-containing electrolyte salt is NaAlCl 4 , NaBF 4 , NaBH 4 , NaB(CN) 4 , NaBF 3 CN, NaBF 2 (CN) 2 , NaBF(CN) 3 or NaAl(BH 4 ) 4 or any mixture thereof.

72. (Sodium-containing electrolyte salt): xSO 2 The method according to any one of claims 60 to 71, wherein the molar ratio x is from 1 to 4.

73. The sodium-containing cathode material is 2 S 2 O 4(Sodium dithionite): xNaAlCl 4 Mixture or iNaCl:jNa 2 S 2 O 4 (Sodium dithionite): kNaAlCl 4 73. The method of any one of claims 60 to 72, comprising a mixture, wherein x, i, j and k define a molar ratio.

74. The sodium-containing cathode material is 2 S 2 O 4 (Sodium dithionite): xNaAlCl 4 74. The method of claim 73, comprising a mixture, the molar ratio x being from 0.5 to 2.

75. 75. The method of any one of claims 60 to 74, wherein the sodium-containing cathode material comprises NaCl and the cell is assembled in either a fully or partially discharged state.

76. The sodium-containing cathode material is iNaCl:jNa 2 S 2 O 4 (Sodium dithionite): kNaAlCl 4 74. The method of claim 73, comprising a mixture, wherein i is from 3 to 5, j is from 0.5 to 2, and k is from 0.5 to 2.

77. a) providing a cathode comprising a sodium-containing cathode material, and an electrically conductive anode current collector; b) Between the cathode and the anode current collector, SO 2 providing an electrolyte comprising a solvent and a sodium-containing electrolyte salt; and c) providing a cationically conductive film between the cathode and anode current collectors that is electrically conductive sodium A method for manufacturing an electrochemical cell, comprising:

78. 78. The method of claim 77, further comprising providing a porous separator film between the cathode and the anode current collector.

79. the cation-conducting film is deposited on the anode current collector; or 79. The method of any one of claims 77 to 78, wherein the cell further comprises a separator between the anode current collector and the cathode, and the cation-conducting film is deposited on the separator.

80. The method of any one of claims 77 to 79, wherein the cationically conductive film inhibits the migration of sulfuryl chloride.

81. a) providing a cathode and an anode current collector; and b) 1. One or more nitrogen-containing solvent precursors; 2. one or more sodium-containing electrolyte salts, at least one of which contains a sodium cation and a chloride-cored anion, or a sulfonyl-containing anion; providing an electrolyte comprising A method for manufacturing an electrochemical cell, comprising:

82. 82. The method of claim 81 , wherein the sodium-containing electrolyte salt molarity is at least 3 moles / liter.

83. The sodium-containing electrolyte salt is NaBF 4 , NaBH 4 , NaPF 6 , NaClO 4 , NaB(CN) 4 , NaBF 3 CN, NaBF 2 (CN) 2 , NaBF(CN) 3 , NaBH 3 CN, NaBH 2 (CN) 2 , NaBH(CN) 3 , NaAl(BH 4 ) 4, sodium bis-(trifluoromethylsulfonyl)imide (NaTFSI), sodium bis(fluorosulfonyl)imide (NaFSI), sodium trifluoromethanesulfonate (Na triflate), or a mixture containing one or more of the foregoing salts.

84. The nitrogen-containing solvent precursor is ammonia (NH 3 ), one or more organic amine-based liquids, one or more nitrile-based liquids, or a mixture containing one or more of said nitrogen-containing solvent precursors.

85. 85. The method of claim 84, wherein the organic amine is selected from ethylenediamine, 1,3-diaminopropane, diethylenetriamine, n-butylamine, n-propylamine, isopropylamine, ethylamine, methylamine, pyridine or mixtures thereof, and the nitrile is selected from acetonitrile, propiononitrile, or a mixture containing one or more of the organic amines.

86. 86. The method of any one of claims 81 to 85, wherein the sodium-containing electrolyte salt concentration is high enough to constitute a localized ordered liquid-type electrolyte.

87. 86. The method of any one of claims 81 to 85, wherein the sodium-containing electrolyte salt concentration is high enough to constitute an ionic liquid type electrolyte.

88. (sodium-containing electrolyte salt): xNH 3or the molar ratio y of (sodium-containing electrolyte salt):y (organic monoamine) is 1 to 5; or the molar ratio z of (sodium-containing electrolyte salt):z (organic diamine) is 0.5 to 2.5; or the molar ratio j of (sodium-containing electrolyte salt):j (organic triamine) is 0.3 to 2; or the molar ratio k of (sodium-containing electrolyte salt):(nitrile) is 1 to 5. The method of any one of claims 81 to 87.

89. The sodium-containing electrolyte salt is NaBF 4 and (sodium-containing electrolyte salt): xNH 3 or the molar ratio y of (sodium-containing electrolyte salt):y (organic monoamine) is 1 to 3.5; or the molar ratio z of (sodium-containing electrolyte salt):z (organic diamine) is 0.5 to 1.8; or the molar ratio j of (sodium-containing electrolyte salt):j (organic triamine) is 0.3 to 1.2; or the molar ratio k of (sodium-containing electrolyte salt):(nitrile) is 1 to 3.

5.

90. The sodium-containing electrolyte salt is NaBH 4 and (sodium-containing electrolyte salt): xNH 3 or the molar ratio y of (sodium-containing electrolyte salt):y (organic monoamine) is 2 to 3.5; or the molar ratio z of (sodium-containing electrolyte salt):z (organic diamine) is 1 to 1.8; or the molar ratio j of (sodium-containing electrolyte salt):j (organic triamine) is 0.7 to 1.2; or the molar ratio k of (sodium-containing electrolyte salt):(nitrile) is 2 to 3.

5.

91. The method of any one of claims 81 to 88, wherein the electrolyte comprises one or more SEI-forming amine or nitrile solvents.

92. the electrolyte comprises one or more SEI-forming amine or nitrile solvents; The SEI-forming amine or nitrile solvent is ethylenediamine, and the sodium-containing electrolyte salt is NaBF 4 or NaBH 4 72. The method of claim 71 , wherein:

93. 92. The method of claim 91, wherein the sodium-containing electrolyte salt concentration is from 3M to 5M.

94. 94. The method of any one of claims 81-88, 91 and 93, wherein a source of metallic sodium active material for the anode current collector is provided.

95. 95. The method of claim 94, wherein the metallic sodium active material is provided by bringing the source of metallic sodium active material into electrical contact with an end of the anode current collector.

96. The cathode converts sodium ions (Na ions) from the sodium metal active material during a first discharge cycle of the electrochemical cell. + 95. The method of claim 94, further comprising receiving

97. 97. The method of any one of claims 60 to 96, further comprising a separator having a higher surface energy than the electrolyte or supporting good wetting of the separator by the electrolyte.

98. The method of any one of claims 60 to 97, comprising a separator comprising spandex, polypropylene, or polyethylene.

99. 99. The method of any one of claims 60 to 98, wherein the sodium-containing electrolyte salt further comprises boron, aluminum, fluoride, chloride and / or hydrogen.

100. 100. The method of any one of claims 60 to 99, wherein the cathode comprises a carbon-containing cathode material, the carbon-containing cathode material being a carbonyl or anthrimidocarbazole containing compound.

101. 101. The method of claim 100, wherein the carbonyl or anthrimidocarbazole containing compound comprises poly-anthraquinonyl-sulfide polymer, AQS-oligomer or indanthrone blue.

102. 81. The method of any one of claims 60 to 80, wherein some or all of the sodium-containing cathode material is in its initial state or in a reduced sodium salt state.

103. The method of any one of claims 60 to 102, wherein the cathode comprises one or more carbon-containing cathode materials.

104. 104. The method of claim 103, wherein the carbon-containing cathode material is CNT, fullerene, CNB, graphene, graphite, Ketjen-Black, mesoporous carbon, activated carbon, Y-carbon, nanocarbon, carbon nanoparticles, and / or porous carbon.

105. The method of any one of claims 60 to 104, wherein the cathode comprises a binder material.

106. 106. The method of claim 105, wherein the binder material is PTFE, PVDF, styrene-butadiene rubber (SBR) or heat treated polyacrylonitrile.

107. The method of any one of claims 60 to 80, wherein the sodium-containing cathode material is deposited on a cathode conductive current collector / mechanical support.

108. The method of any one of claims 60 to 107, wherein the anode current collector is a conductive current collector / mechanical support.

109. A method according to any one of claims 107 to 108, wherein the cathode and / or anode current collector / mechanical support comprises a metal or has a metallic surface.

110. 110. The method of claim 109, wherein the cathode and / or anode current collector / mechanical support comprises aluminum Al, Cu, Ni, Cr, Pd, Pt, Au and / or Ag, or an alloy comprising Al, Cu, Ni, Cr, Pd, Pt, Au and / or Ag.

111. A method according to any one of claims 109 to 110, wherein the metal surface is deposited on a mechanical support to form an anode or cathode current collector.

112. The method of any one of claims 102 to 111, wherein the cathode comprises a carbon-containing cathode material, the carbon-containing cathode material being applied onto a cathode current collector / mechanical support.

113. The method of any one of claims 60 to 112, wherein the cathode comprises less than 10% by weight of a binder.

114. The method of claim 113, wherein the cathode comprises 4 to 7 weight percent binder.

115. The method of any one of claims 60 to 114, wherein metallic sodium active material is electrodeposited onto the anode current collector during charging of the electrochemical cell.

116. 116. The method of claim 115, wherein the metallic sodium active material is smooth.

117. a) An electric vehicle, an electric or electronic device, a power unit, a back-up energy unity, or a grid storage or stabilization unit utilizing an electrochemical cell, battery or supercapacitor according to any one of claims 1 to 59.

Citation Information

Patent Citations

  • Method for plating a metal negative electrode under a protective coating.

    JP2002504741A

  • Secondary battery and method of manufacturing the same

    JP2011159596A

  • Sodium secondary battery

    JP2012252962A

  • Positive electrode active material for sodium ion battery and process of manufacturing the same

    JP2014220203A

  • Fiber positive electrode for sodium ion secondary battery and method for manufacturing the same

    JP2015072808A