Sputtering target member for forming non-magnetic layer
A sputtering target member with a Co, Pt, and Mo metal phase, and oxide phase dispersion addresses the high cost of Ru by maintaining the hcp structure and orientation in nonmagnetic layers for perpendicular magnetic recording media, achieving cost-effective film formation.
Patent Information
- Application Number
- JP2021534574
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-07-23
- Filing Date
- 2020-05-29
- Publication Date
- 2024-09-19
- Estimated Expiration
- 2040-05-29
AI Technical Summary
The high market price of ruthenium (Ru) has increased production costs in the production of nonmagnetic layers for perpendicular magnetic recording media, necessitating a more cost-effective alternative to maintain the hexagonal close-packed (hcp) structure and orientation of the C-axis in the magnetic recording layer.
A sputtering target member with a structure where a metal phase composed of Co, Pt, and Mo, and an oxide phase are mutually dispersed, with specific concentration ranges for each element, is used to form a nonmagnetic layer, maintaining the hcp structure and reducing the reliance on Ru.
The proposed sputtering target member allows for the formation of a nonmagnetic film with the hcp structure, ensuring proper C-axis orientation and separation of magnetic grains, while significantly reducing production costs by using more affordable materials.
Smart Images

Figure 0007554192000004 
Figure 0007554192000002 
Figure 0007554192000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a sputtering target member suitable for forming a thin film for a non-magnetic layer that constitutes a perpendicular magnetic recording medium. [Background technology]
[0002] In magnetic recording media used in magnetic recording and reproducing devices such as HDDs (hard disk drives), the perpendicular magnetic recording method, which enables higher recording density, has been attracting attention as an alternative to the in-plane magnetic recording method used up until now. In the perpendicular magnetic recording method, the axis of easy magnetization in the magnetic recording layer is oriented perpendicular to the substrate surface, and has the advantage of being able to suppress the thermal fluctuation phenomenon compared to the in-plane magnetic recording method.
[0003] Perpendicular magnetic recording media that use the perpendicular magnetic recording method generally have a layer called the magnetic recording layer, which is responsible for the magnetism, and a non-magnetic layer that is used to improve the characteristics of the magnetic recording layer. hcp-Co alloys are often used as micro-magnets for the magnetic recording layer. When the magnetic recording layer has a hcp (hexagonal close-packed) structure, the axis of easy magnetization is the C-axis, and the C-axis must be oriented in the normal direction of the substrate.
[0004] In order to improve the orientation of the C-axis, it is effective to provide a non-magnetic layer (also called an "orientation control layer") with an hcp structure under the magnetic recording layer. Known materials for the non-magnetic layer include CoCr alloy, Ti, V, Zr, and Hf, and it is known that Ru (ruthenium) in particular can effectively improve the crystal orientation of the magnetic recording layer and increase the coercive force Hc (JP 2012-2088992 A, JP 2009-245484 A, WO 2010 / 038448 A, and JP 2004-310910 A). [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2012-208992 A [Patent Document 2] JP 2009-245484 A [Patent Document 3] International Publication No. 2010 / 038448 [Patent Document 4] JP 2004-310910 A Summary of the Invention [Problem to be solved by the invention]
[0006] In recent years, the market price of Ru has been rising, and there is a problem that the use of Ru increases production costs. Therefore, it would be advantageous if a non-magnetic layer with an hcp structure could be formed while reducing the amount of Ru used. The present invention has been created in view of such circumstances, and in one embodiment, the object of the present invention is to provide a sputtering target member that is advantageous for forming a non-magnetic layer with an hcp structure that constitutes a perpendicular magnetic recording medium and has excellent economical properties. In another embodiment, the object of the present invention is to provide a film formation method using such a sputtering target member. [Means for solving the problem]
[0007] The present inventors have conducted extensive research to solve the above problems and have found that a sputtering target member having a structure in which a metal phase containing Co, Pt, and Mo as main components and an oxide phase are dispersed in each other is suitable for forming a nonmagnetic layer.
[0008] [1] A sputtering target member for forming a nonmagnetic layer having a structure in which a metal phase and an oxide phase are mutually dispersed, the metal phase contains, based on the overall composition of the target member, 20 to 60 mol % Co, 5 to 30 mol % Pt, 1 to 40 mol % Mo, and contains Mo, Cr, Ru, and B in a total concentration of 25 mol % or more; The volume fraction of the oxide phase is 10 to 45%. A sputtering target member for forming a non-magnetic layer. [2] The sputtering target member for forming a nonmagnetic layer according to [1], wherein the metal phase contains 25 to 30 mol % of Mo based on the overall composition of the target member. [3] The sputtering target member for forming a nonmagnetic layer according to [1] or [2], wherein the concentration of Cr in the metal phase is 5 mol % or less based on the total composition of the target member. [4] The sputtering target member for forming a nonmagnetic layer according to any one of [1] to [3], wherein the concentration of Ru in the metal phase is 5 mol % or less based on the overall composition of the target member. [5] The sputtering target member for forming a nonmagnetic layer according to any one of [1] to [4], wherein the concentration of B in the metal phase is 5 mol % or less based on the overall composition of the target member. [6] The sputtering target member for forming a nonmagnetic layer according to any one of [1] to [5], wherein the oxide phase contains an oxide of one or more metals selected from the group consisting of Ti, Si, B, Co, Cr, Ta, Mn, Zr, and Nb. [7] The sputtering target member for forming a nonmagnetic layer according to any one of [1] to [6], which has a relative density of 90% or more. [8] A sputtering target having a structure in which the sputtering target member for forming a nonmagnetic layer according to any one of [1] to [7] and a backing plate or a backing tube are laminated via a brazing material layer. [9] A film forming method comprising a step of sputtering using the sputtering target member for forming a nonmagnetic layer according to any one of [1] to [7]. Effect of the Invention
[0009] A non-magnetic film can be easily obtained by sputtering the sputtering target member according to one embodiment of the present invention. Since the non-magnetic film maintains the hcp structure of the metal phase, when the magnetic recording layer in the perpendicular magnetic recording medium has a hcp (hexagonal close-packed) structure, the effect of orienting the C axis in the normal direction of the substrate can be obtained. In addition, since the metal phase and the oxide phase of the film are neatly separated, it is expected to contribute to the separation between magnetic grains in the magnetic layer formed on the upper layer. In addition, Mo used in the sputtering target member according to one embodiment of the present invention is available at a lower price than Ru. Therefore, the sputtering target member according to one embodiment of the present invention can be expected to be used in the formation of a non-magnetic layer that constitutes a perpendicular magnetic recording medium. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] In one embodiment, the sputtering target member for forming a nonmagnetic layer according to the present invention has a structure in which a metal phase and an oxide phase are mutually dispersed. The mutual dispersion of the metal phase and the oxide phase in the sputtering target member is advantageous for forming a homogeneous film.
[0011] (1. Metallic phase) In one embodiment of the sputtering target member for forming a nonmagnetic layer according to the present invention, the metal phase contains, based on the overall composition of the target member, 20 to 60 mol % Co, 5 to 30 mol % Pt, and 1 to 40 mol % Mo. Co, Pt, and Mo may each be present as a simple metal, or may be present as a CoPt alloy, a CoPtMo alloy, a CoMo alloy, a PtMo alloy, or an alloy of any of these with one or more of Cr, Ru, and B.
[0012] The reason why the lower limit of the Co concentration in the metal phase is set to 20 mol% or more is due to the ease of forming a Co alloy. If the amount of Co is small, it becomes difficult to maintain the hcp structure of Co and the Co alloy. The lower limit of the Co concentration is preferably 30 mol% or more, more preferably 35 mol% or more, and even more preferably 40 mol% or more. The reason why the upper limit of the Co concentration in the metal phase is set to 60 mol% or less is for the purpose of demagnetization. If the amount of Co is large, it becomes difficult to demagnetize even if other metals are used. The upper limit of the Co concentration is preferably 55 mol% or less, more preferably 50 mol% or less, and even more preferably 45 mol% or less.
[0013] The Pt concentration in the metal phase is set to 5 mol% or more and 30 mol% or less because it affects the stability of the magnetic layer formed on the upper layer. At most, the amount of Pt at least deteriorates the stability of the hcp structure in the magnetic layer. The lower limit of the Pt concentration is preferably 10 mol% or more, more preferably 15 mol% or more. The upper limit of the Pt concentration is preferably 28 mol% or less, more preferably 25 mol% or less.
[0014] The reason why the lower limit of the Mo concentration in the metal phase is set to 1 mol% or more is that Mo is available at a lower cost than Ru, and it is found to contribute to the non-magnetization of the sputtered film (in other words, the reduction of the saturation magnetization), and furthermore, it is found to be highly effective in maintaining the hcp structure of the metal phase in the sputtered film. Furthermore, Mo is chemically stable and is not easily oxidized, so there is a characteristic that there is little risk of unintentionally reducing oxides such as CoO contained in the oxide phase. This characteristic is advantageous in that the constituent phases of the sputtered film can be easily adjusted. The lower limit of the Mo concentration is preferably 5 mol% or more, more preferably 15 mol% or more, and even more preferably 25 mol% or more.
[0015] The reason why the upper limit of the Mo concentration in the metal phase is set to 40 mol% or less is to prevent the occurrence of cracks, since if the Mo concentration is too high, the sputtering target member becomes prone to cracks. The upper limit of the Mo concentration is preferably 40 mol% or less, more preferably 35 mol% or less, and even more preferably 30 mol% or less.
[0016] Therefore, in a preferred embodiment of the sputtering target member for forming a nonmagnetic layer according to the present invention, the metal phase contains 35 to 50 mol % Co, 10 to 28 mol % Pt, and 15 to 35 mol % Mo, based on the overall composition of the target member, and in a more preferred embodiment, the metal phase contains 40 to 45 mol % Co, 15 to 25 mol % Pt, and 25 to 30 mol % Mo, based on the overall composition of the target member.
[0017] The metal phase contains Mo, Cr, Ru and B in a total concentration of 25 mol% or more based on the overall composition of the target member. These metal elements contribute to the non-magnetization of the sputtered film, so it is desirable to contain them in a total concentration of 25 mol% or more. However, if the total concentration of these metal elements is too high, the hcp structure of the sputtered film may collapse, so the upper limit of the total concentration of these metal elements is preferably 40 mol% or less, more preferably 35 mol% or less, and even more preferably 30 mol% or less based on the overall composition of the target member. In addition, from the viewpoint of not bringing about unexpected changes in characteristics, it is preferable that the amount of metal components other than Mo is small.
[0018] Cr has a negative effect on maintaining the hcp structure of the metal phase, and also tends to reduce oxides such as CoO, which may result in the formation of unintended constituent phases in the sputtered film. Therefore, the concentration of Cr in the metal phase is preferably 20 mol% or less, more preferably 10 mol% or less, even more preferably 5 mol% or less, and even more preferably 1 mol% or less, based on the overall composition of the target member.
[0019] As mentioned above, Ru increases production costs, so it is desirable to add a small amount of Ru. Therefore, the Ru concentration in the metal phase is preferably 20 mol % or less, more preferably 10 mol % or less, even more preferably 5 mol % or less, and even more preferably 1 mol % or less, based on the overall composition of the target member.
[0020] Like Cr, B also easily reduces oxides such as CoO, and may generate unintended constituent phases in the sputtered film. Therefore, the concentration of B in the metal phase is preferably 20 mol% or less, more preferably 10 mol% or less, even more preferably 5 mol% or less, and even more preferably 1 mol% or less, based on the overall composition of the target member.
[0021] The total concentration of Cr, Ru and B in the metal phase is preferably 20 mol % or less, more preferably 10 mol % or less, even more preferably 5 mol % or less, and even more preferably 1 mol % or less, based on the overall composition of the target member.
[0022] (2. Oxide Phase) In one embodiment of the sputtering target member for forming a nonmagnetic layer according to the present invention, the volume fraction of the oxide phase is 10 to 45%. By setting the lower limit of the volume fraction of the oxide phase to 10% or more, the effect of blocking magnetic interactions can be enhanced. The lower limit of the volume fraction of the oxide phase is preferably 20% or more, more preferably 30% or more. The reason why the upper limit of the volume fraction of the oxide phase is set to 45% or less is that if the volume fraction of the oxide phase is greater than this, it becomes difficult to discharge during sputtering. The upper limit of the volume fraction of the oxide phase is preferably 40% or less, more preferably 35% or less.
[0023] The volume fraction of the oxide phase in the sputtering target material is measured by the following procedure. Metal particle parts and oxide parts can be distinguished by the shade of color when observing the structure. For example, in the results of structure observation using a SEM (scanning electron microscope), the intensity of secondary electrons appears as shades in the image, so generally, metal parts appear bright because the intensity of secondary electrons is strong, and oxides appear dark because the intensity is low. Using this, the average area fraction of the dark parts in the image is taken as the volume fraction of the oxide phase of the target. Here, we use the fact that the following relationship holds between the average area fraction and volume fraction of uniformly dispersed phases (Fundamentals and Applications of 3D Material Structure and Property Analysis, edited by Shinya Mitsuo, Appendix A1, Uchida Rokakuho, June 2014).
[0024] The oxides constituting the oxide phase include, but are not limited to, oxides of one or more metals selected from the group consisting of Ti, Si, B, Co, Cr, Ta, Mn, Zr and Nb. The oxides constituting the oxide phase may be one type or two or more types may be mixed.
[0025] As the oxide of titanium, TiO2, TiO, etc. can be used. As the oxide of silicon, SiO2, SiO, etc. can be used. As the oxide of boron, B2O3, BO, B2O, BO, etc. can be used. As the oxide of cobalt, CoO, Co2O3, Co3O4, etc. can be used. As the oxide of chromium, Cr2O3, etc. can be used. As the oxide of tantalum, TaO2, Ta2O5, etc. can be used. As the oxide of manganese, MnO, MnO2, Mn3O4, etc. can be used. As the oxide of zirconium, Zr2O3, etc. can be used. As the oxide of niobium, NbO, NbO2, Nb2O3, Nb2O5, etc. can be used. Other oxides can also be used.
[0026] The oxide may be a composite oxide containing two or more metal components. As the composite oxide, composite oxides having a relatively high melting point, such as CrBO3, Co2B2O5, Co3B2O6, Mn3B2O6, TiBO3, etc., can be suitably used.
[0027] Among the above oxides, from the viewpoint of increasing the separation between the metal phase and the oxide phase in the sputtered film, the oxide of cobalt, which has excellent wettability with Co constituting the metal phase, is preferred, and CoO is optimal. Therefore, the concentration of cobalt oxide in the oxide phase is preferably 50 mol% or more, and more preferably 70 mol% or more. Furthermore, the concentration of CoO in the oxide phase is preferably 50 mol% or more, and more preferably 70 mol% or more.
[0028] (3. Relative Density) A high relative density of the sputtering target member is preferable for performing stable sputtering with less arcing. In one embodiment, the sputtering target member for forming a nonmagnetic layer according to the present invention has a relative density of 90% or more. The relative density is preferably 95% or more, and more preferably 99% or more. The relative density is determined as the ratio of the Archimedes density to the theoretical density determined by the composition. The theoretical density determined by the composition may exceed 100% because it does not take into account the density of compounds that actually exist.
[0029] The theoretical density is calculated from the mass concentration and the elemental density of each component obtained by performing a component analysis of the sputtering target material. Specifically, it is the density when it is assumed that the constituent components of the target are mixed together without diffusing or reacting with each other, and is calculated by the following formula. Formula: Theoretical density (g / cm 3 ) = Σ (molecular weight of component × molar ratio of component) / Σ (molecular weight of component × molar ratio of component / literature density of component) Here, Σ means taking the sum over all of the constituent components of the target.
[0030] (4. Manufacturing Method) The sputtering target member for forming a nonmagnetic layer according to the present invention can be produced by a powder sintering method, for example, by the following procedure.
[0031] First, one or more kinds of metal powders are prepared according to the composition of the desired metal phase. The metal powder may be a simple metal powder such as Co powder, Pt powder, Mo powder, Cr powder, Ru powder, or B powder, or an alloy powder such as Co-Pt alloy powder. The metal powder may be prepared by pulverizing a melted and cast ingot, or by gas atomization.
[0032] The median diameter of each metal powder is preferably 0.1 μm or more, more preferably 0.5 μm or more, and even more preferably 1 μm or more. If the metal powder is too small, the powders will aggregate with each other, making it difficult to obtain a uniform structure. However, if the median diameter of each metal powder is too large, it is difficult to mix uniformly with the oxide powder and there is a concern that it may cause particles during sputtering, so it is preferably 150 μm or less, more preferably 30 μm or less, and even more preferably 10 μm or less. The median diameter can be adjusted by crushing or sieving.
[0033] Also, one or more kinds of oxide powders are prepared according to the composition of the desired oxide phase. From the viewpoint of easy uniform dispersion, the median diameter is preferably 30 μm or less, more preferably 10 μm or less, and even more preferably 5 μm or less. From the viewpoint of preventing aggregation of the powders, the oxide powder preferably has a median diameter of 0.1 μm or more, more preferably 1 μm or more, and even more preferably 2 μm or more.
[0034] In this specification, the median diameter of a powder means the particle size at 50% cumulative volume (D50) in the particle size distribution determined by a laser diffraction / scattering method. In the examples, a particle size distribution measuring device (Model LA-920, manufactured by HORIBA) was used, and the powder was dispersed in an ethanol solvent and measured by a wet method. The refractive index used was that of metallic cobalt.
[0035] Next, the raw powders (metal powder and oxide powder) are weighed to obtain a desired composition, and mixed while being pulverized using a known method such as a ball mill. At this time, it is preferable to seal an inert gas in the pulverization container to suppress oxidation of the raw powder as much as possible. Examples of the inert gas include Ar and N2 gas. At this time, in order to realize a uniform structure, it is preferable to pulverize the mixed powder until the median diameter is 20 μm or less, and more preferably 10 μm or less, and it can be pulverized until it is in the range of, for example, 0.1 to 10 μm. The mixed powder thus obtained is molded and sintered in a vacuum atmosphere or an inert gas atmosphere by a hot press method. In addition to the hot press method, various pressure sintering methods such as a plasma discharge sintering method can be used. In particular, hot isostatic sintering (HIP) is effective in increasing the density of the sintered body, and it is preferable to carry out the hot press method and the hot isostatic sintering method in this order from the viewpoint of increasing the density of the sintered body.
[0036] The holding temperature during sintering depends on the composition of the metal phase in order to avoid melting of the metal powder, but is preferably lower than the melting point of the metal used, more preferably at least 20° C. lower than the melting point, and even more preferably at least 50° C. lower than the melting point. In addition, the holding temperature during sintering is preferably 650° C. or higher, more preferably 700° C. or higher, and even more preferably 750° C. or higher in order to avoid a decrease in the density of the sintered body.
[0037] The pressure in the hot press is preferably 20 to 70 MPa in order to promote sintering, and the pressure in the hot isostatic sintering (HIP) is preferably 100 to 200 MPa in order to improve the density of the sintered body.
[0038] The sintering time is preferably 0.3 hours or more, more preferably 0.5 hours or more, and even more preferably 1.0 hour or more in order to improve the density of the sintered body, and is preferably 3.0 hours or less, more preferably 2.0 hours or less, and even more preferably 1.5 hours or less in order to prevent the crystal grains from becoming coarse.
[0039] The sputtering target member according to the present invention can be produced by forming the obtained sintered body into a desired shape using a lathe, etc. There are no particular limitations on the target shape, but examples of the target shape include a flat plate shape (including a disk shape and a rectangular plate shape) and a cylindrical shape.
[0040] The thickness of the sputtering target member is not particularly limited and may be appropriately set depending on the sputtering device used and the film formation time, but is usually about 3 to 25 mm, typically about 6 to 18 mm.
[0041] The sputtering target member may be used as a sputtering target as it is, or may be bonded to a backing plate or backing tube with brazing material as necessary. In this case, a sputtering target having a structure in which the sputtering target member and the backing plate or backing tube are laminated via a brazing material layer is provided. The material constituting the brazing material layer is not limited, but is preferably one or more selected from the group consisting of pure In, InSn alloy, and InZn alloy, since the melting point of In is lower than that of indium.
[0042] The thickness of the brazing material layer is not limited, but from the viewpoint of the efficiency of use of the sputtering target and the prevention of cracks based on the thermal expansion buffering effect of the brazing material, it is preferably 0.1 mm to 2 mm, more preferably 0.1 mm to 1 mm, and even more preferably 0.3 mm to 0.8 mm.
[0043] (5. Film formation) In one aspect, the present invention provides a film formation method including a step of sputtering using the sputtering target member for forming a nonmagnetic layer according to the present invention. The sputtering conditions can be appropriately set.
[0044] In one embodiment, the sputtered film obtained by carrying out the above-mentioned film forming method has a saturation magnetization of 200 emu / cc or less, preferably 150 emu / cc or less, and more preferably 100 emu / cc or less. The saturation magnetization is a value measured by a vibrating sample magnetometer (VSM). In one embodiment, when the sputtered film obtained by carrying out the above-mentioned film forming method is analyzed by XRD (X-ray diffraction method), the full width at half maximum (FWHM) of the peak due to the (002) plane of the hcp CoPt alloy, which appears between 2θ=42° and 44°, is 5 or less, preferably 4 or less, and typically in the range of 3 to 5. This means that the hcp structure of the metal phase is maintained in the sputtered film. EXAMPLES
[0045] Examples of the present invention will be described below together with comparative examples. These examples are provided for a better understanding of the present invention and its advantages, and are not intended to limit the invention.
[0046] <1. Raw material powder> (1) The following metal raw powders were prepared: Co powder (median diameter: 3 μm), Cr powder (median diameter: 10 μm), Pt powder (median diameter: 1 μm), Mo powder (median diameter: 5 μm), B powder (median diameter: 5 μm) (2) The following metal oxide powders were prepared: TiO2 powder (median diameter: 1 μm), SiO2 powder (median diameter: 1 μm), CoO powder (median diameter: 2 μm)
[0047] Next, each raw material powder was weighed so as to have the raw material composition according to the test number shown in Table 1, and was put into a ball mill pot with a capacity of 10 liters together with SUS balls as a grinding medium, and mixed and ground by rotating in an Ar atmosphere for 8 hours. The median diameter of the powder after mixing and grinding was measured and found to be about 3 μm. Next, the powder taken out of the pot was filled into a carbon mold, molded and sintered using a hot press device. The hot press conditions were a vacuum atmosphere, a heating rate of 300°C / hour, a holding temperature of 1000°C, and a holding time of 2 hours, and the material was pressurized at 30 MPa from the start of heating to the end of holding the temperature. After the holding time was ended, the material was allowed to cool naturally in the chamber. Next, the sintered body taken out of the hot press mold was subjected to hot isostatic sintering (HIP). The hot isostatic sintering conditions were a heating temperature of 300°C / hour, a holding temperature of 950°C, and a holding time of 2 hours, and the Ar gas pressure was gradually increased from the start of heating, and the material was pressurized at 150 MPa while holding at 950°C. After the temperature was maintained, the sintered bodies were naturally cooled in the furnace. Next, each sintered body was cut into a shape of 180.0 mm in diameter and 5.0 mm in thickness using a lathe to obtain a disk-shaped sputtering target member. A sufficient number of sputtering target members for each test example were prepared to carry out the following tests.
[0048] [Table 1]
[0049] <2. Tissue analysis> For each sputtering target member obtained by the above procedure, a cut surface parallel to the sputtering surface was cut and mirror-polished. The mirror-polished cut surface was analyzed using elemental mapping images by FE-EPMA. As a result, it was confirmed that each sputtering target member had a structure in which the metal phase and the oxide phase were mutually dispersed. From the elemental mapping images by FE-EPMA, it was confirmed that for both the metal phase and the oxide phase, a particle phase with a composition corresponding to the raw material composition was present. The compositions of the metal phase and the oxide phase are shown in Table 2.
[0050] [Table 2]
[0051] <3. Volume ratio of oxide phase> The mirror-polished cut surface that had been subjected to the structural analysis was imaged at 3000x magnification using a Hitachi S-3700N SEM (scanning electron microscope). The SEM image was then binarized to black and white using software called ImageJ from the National Institutes of Health to identify the oxide phase (black area) and determine the ratio of the area of the oxide phase to the area of the entire SEM image. The measurement was performed three times, and the average value was used as the measured value for the volume fraction of the oxide phase. The binarization procedure is as follows: Select File→Open to load the image. Select 8-bit from Image→Type. Select the excluding scaled portion of the image and cut out the scaled portion with Image→Crop. Select Process→Filters→Gaussian Blur, enter 2 for Sigma, and click OK. Select Process→Binary→Make Binary. The image will be binarized using the above steps.
[0052] <4. Relative density> The density of each sputtering target member according to the test example obtained by the above manufacturing method was measured by Archimedes' method, and the ratio (%) to the theoretical density determined by the composition was calculated as the relative density. The results are shown in Table 3.
[0053] <5.Strength> The sputtering target members according to the respective test examples obtained by the above manufacturing method were visually inspected for the presence or absence of cracks. The results are shown in Table 3.
[0054] <6. Film formation test> The sputtering target members according to the respective test examples obtained by the above manufacturing procedure were attached to a magnetron sputtering device (Canon Anelva C-3010 sputtering system) and sputtering was carried out. The sputtering conditions were an input power of 1 kW, an Ar gas pressure of 1.7 Pa, and a film was formed on a silicon substrate for 20 seconds.
[0055] <7.XRD analysis> The sputtered films of each test example obtained in the film formation test were analyzed by XRD (X-ray diffraction method) under the following measurement conditions. The diffraction peak positions were measured by high-angle XRD measurement, and the full width at half maximum (FWHM) was measured by rocking curve measurement. Analytical equipment: Rigaku Corporation's high-resolution X-ray thin film evaluation equipment Superlab High angle XRD measurement Tube: Cu (measured with CuKα) Tube voltage: 40kV Tube current: 20mA Optical system: Two-dimensional focusing multilayer mirror Scan mode: 2θ / θ Scanning range (2θ): 10°~100° Measurement step (2θ): 0.1° Measurement sample size: approx. 10mm x 10mm Rocking curve measurement Tube: Cu (measured with CuKα) Tube voltage: 40kV Tube current: 20mA Optical system: Two-dimensional focusing multilayer mirror Scan mode: θ alone Scanning range (θ): ±10° peak position of (002) plane identified by high-angle XRD Measurement step (2θ): 0.2° Measurement sample size: approx. 10mm x 10mm
[0056] The obtained XRD profile was analyzed using PDXL, an integrated powder X-ray analysis software manufactured by Rigaku Corporation. BG removal, Kα2 removal, and peak search were performed in automatic mode on the obtained measurement data to identify the position of the diffraction peak due to the (002) plane of the hcp CoPt alloy, which appears between 2θ = 42° and 44°, and the full width at half maximum (FWHM) of the peak was measured. The presence of the peak means that the (002) plane appears parallel to the measurement surface, that is, the C-axis of the hcp structure is perpendicular to the sputtered film. The results are shown in Table 3.
[0057] <8. Magnetic Measurement> For the sputtered films of each test example obtained in the film formation test, magnetic measurements were performed using a VSM (Tamagawa Seisakusho, model TM-VSM261483-HGC) to measure the saturation magnetization. The results are shown in Table 3. If the saturation magnetization of the sputtered film is 200 emu / cc or less, it can be expected to be used as a non-magnetic layer.
[0058] [Table 3]
[0059] <9. TEM Observation> The sputtered films of Example 1, Comparative Example 8, and Comparative Example 9 obtained in the film formation test were subjected to structure observation (magnification: ×40,000) using a JEOL transmission electron microscope (TEM). Then, the average particle size and standard deviation of the metal phase particles were measured by image analysis. The results are shown in Table 4. It can be seen from Table 4 that sputtered films having a fine structure that compares favorably with those obtained when Mo was used instead of Ru.
[0060] [Table 4]
[0061] <10. Discussion> In Comparative Example 1, the metal phase was composed of Co, Cr, and Pt, and did not contain Mo, so that it was not possible to form a film while maintaining the hcp structure with good crystallinity (this can be confirmed by the large half-value width). In Comparative Example 2, the metal phase was composed of Co, Pt and Ru, the sputtered film was made nonmagnetic, and the hcp structure was maintained; however, the raw material cost of Ru was high, which raised economical problems. In Comparative Example 3, the metal phase was composed of Co, B, and Pt, and did not contain Mo, so that it was not possible to form a film while maintaining the hcp structure with good crystallinity (this can be confirmed by the large half-value width). Comparative Examples 4 to 7 contained Mo, but the total concentration of Mo, Cr, Ru, and B was insufficient, and therefore the saturation magnetization of the sputtered films was high. In Comparative Example 8, the Mo concentration in the metal phase was too high, so that the sputtering target member became embrittled and cracked. In Comparative Example 9, the metal phase was composed of Co, Cr, and Pt, and Mo was not included. Also, Cr and CoO were used simultaneously, which resulted in the formation of Cr2O3 instead of CoO. As a result, the metal phase could not be separated well in the oxide phase, and some of the metal phase particles became coarse. This can be confirmed by the large standard deviation of the particle size of the metal phase after the film formation. In Comparative Example 10, the metal phase was composed of Co, Pt and Ru, the sputtered film was made nonmagnetic, and the hcp structure was maintained, but the raw material cost of Ru was high, which raised economical problems. In Comparative Example 11, the metal phase was composed of Co, Pt, and B, and Mo was not included. Also, B and CoO were used simultaneously, which resulted in the formation of B2O3 instead of CoO. As a result, the metal phase could not be separated well in the oxide phase, and some of the metal phase particles became coarse. This can be confirmed by the large standard deviation of the particle size of the metal phase after the film formation. On the other hand, in Examples 1 to 10, the composition in the metal phase was more appropriate than in the comparative examples, so the sputtered film was nonmagnetic and the hcp structure was maintained. In addition, the economical efficiency was improved by reducing the Ru concentration in the metal phase.
Claims
1. A sputtering target member for forming a nonmagnetic layer having a structure in which a metal phase and an oxide phase are mutually dispersed, the metal phase contains, based on the overall composition of the target member, 20 to 60 mol % Co, 5 to 30 mol % Pt, 1 to 40 mol % Mo, and contains Mo, Cr, Ru, and B in a total concentration of 25 mol % or more; The volume fraction of the oxide phase is 10 to 45%. A sputtering target member for forming a non-magnetic layer.
2. 2. The sputtering target member for forming a nonmagnetic layer according to claim 1, wherein the metal phase contains 15 to 40 mol % of Mo based on the overall composition of the target member.
3. 3. The sputtering target member for forming a nonmagnetic layer according to claim 1, wherein the concentration of Cr in the metal phase is 10 mol % or less based on the total composition of the target member.
4. 4. The sputtering target member for forming a nonmagnetic layer according to claim 1, wherein the concentration of Ru in the metal phase is 5 mol % or less based on the overall composition of the target member.
5. 5. The sputtering target member for forming a nonmagnetic layer according to claim 1, wherein the concentration of B in the metal phase is 5 mol % or less based on the overall composition of the target member.
6. The sputtering target member for forming a nonmagnetic layer according to any one of claims 1 to 5, wherein the oxide phase contains an oxide of one or more metals selected from the group consisting of Ti, Si, B, Co, Cr, Ta, Mn, Zr, and Nb.
7. 7. The sputtering target member for forming a nonmagnetic layer according to claim 1, which has a relative density of 90% or more.
8. A sputtering target member for forming a non-magnetic layer as described in claim 1, wherein the metal phase contains 15 to 30 mol % Pt based on the overall composition of the target member.
9. A sputtering target member for forming a non-magnetic layer as described in claim 1, wherein the metal phase contains 25 to 30 mol % Mo based on the overall composition of the target member.
10. A sputtering target member for forming a non-magnetic layer as described in any one of claims 1 to 9, wherein the concentration of Cr in the metal phase is 5 mol % or less based on the overall composition of the target member.
11. A sputtering target member for forming a non-magnetic layer described in any one of claims 1 to 10, wherein the total concentration of Cr, Ru and B in the metal phase is 10 mol % or less based on the overall composition of the target member.
12. 12. A sputtering target having a structure in which the sputtering target member for forming a nonmagnetic layer according to claim 1 and a backing plate or a backing tube are laminated via a brazing material layer.
13. A film forming method comprising a step of sputtering using the sputtering target member for forming a nonmagnetic layer according to any one of claims 1 to 11.
Citation Information
Patent Citations
Bonding method for sputtering target
JP1988020154A
Magnetic recording medium, its manufacturing method, and magnetic recording and reproducing device
JP2004310910A
Vertical magnetic recording medium and manufacturing method of same
JP2009245484A
METHOD OF MANUFACTURING Co-BASED SINTERED ALLOY SPUTTERING TARGET FOR FORMING MAGNETIC RECORDING FILM HAVING LOW MAGNETIC PERMEABILITY
JP2010222639A
Magnetic recording medium and magnetic recording and reproducing device
JP2011003260A