Optical fiber manufacturing method and optical fiber manufacturing device

By controlling tension and speed using a quadratic function and constant power in the optical fiber manufacturing process, the method stabilizes the tension-to-speed ratio, addressing inefficiencies and improving productivity.

JP7554355B2Active Publication Date: 2024-09-19FUJIKURA LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2023522317
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-05-18
Filing Date
2022-03-31
Publication Date
2024-09-19
Estimated Expiration
2042-03-31

AI Technical Summary

Technical Problem

Existing optical fiber manufacturing methods fail to account for the pretreatment process from when the optical fiber preform starts being heated in the spinning furnace until the tension-to-speed ratio reaches the target value, leading to deviations and inefficiencies.

Method used

A method and apparatus that control the tension and drawing speed of the optical fiber during heating and drawing, using a quadratic function to stabilize the tension-to-speed ratio by supplying constant power to the spinning furnace, reducing control load and improving productivity.

Benefits of technology

Stabilizes the tension-to-speed ratio more efficiently, reducing the time required to reach target values and enhancing the productivity of optical fiber production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007554355000001
    Figure 0007554355000001
  • Figure 0007554355000002
    Figure 0007554355000002
  • Figure 0007554355000004
    Figure 0007554355000004
Patent Text Reader

Abstract

This optical fiber manufacturing method includes a pre-treatment step (P2) of supplying electricity to a spinning furnace (110) to cause T / V to decrease over time along a quadratic function in which the maximum value is Ttarget / Vtarget so that T / V becomes Ttarget / Vtarget, in a case where: T and V are taken to be, respectively, the tension added to an optical fiber (1) and the speed at which the optical fiber (1) is withdrawn, when heating an optical fiber preform (1P) using the spinning furnace (110) and drawing the optical fiber (1); Ttarget is taken to be the tension target value; and Vtarget is taken to be the speed target value.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method and an apparatus for manufacturing an optical fiber. [Background technology]

[0002] An optical fiber is manufactured by heating an optical fiber preform in a spinning furnace and drawing it into an optical fiber. When manufacturing an optical fiber, it is known that the power supplied to the spinning furnace is adjusted according to the speed at which the optical fiber is drawn, the tension applied to the optical fiber, and the like.

[0003] The following Patent Document 1 describes that in order to prevent unnecessary adjustment of the power supplied to the spinning furnace in response to temporary fluctuations in the tension applied to the optical fiber due to temporary fluctuations in the speed at which the optical fiber is pulled, the power supplied to the spinning furnace is adjusted so that the ratio of the tension applied to the optical fiber divided by the speed at which the optical fiber is pulled is maintained at a target value.

[0004] [Patent Document 1] Japanese Patent Application Publication No. 5-139771 Summary of the Invention

[0005] However, the above-mentioned Patent Document 1 does not take into consideration the pre-processing process from when the optical fiber preform starts to be heated by the spinning furnace until the above ratio reaches the target value. For example, even if the ratio is set to the target value by adjusting the power supplied to the spinning furnace, the ratio may deviate from the target value and the power may need to be adjusted again. For this reason, there is a demand for shortening the time required for the pre-processing process to improve the productivity of optical fibers.

[0006] SUMMARY OF THE PRESENT EMBODIMENTS Accordingly, an object of the present invention is to provide an optical fiber manufacturing method and an optical fiber manufacturing apparatus that can improve the productivity of optical fibers.

[0007] In order to achieve the above object, the present invention provides a method for producing an optical fiber, comprising the steps of: heating an optical fiber preform in a spinning furnace to draw an optical fiber; defining a tension applied to the optical fiber and a speed at which the optical fiber is drawn as T and V, respectively; setting a target value of the tension as T target The target value of the speed is V target If T / V is the time course, the value of the vertex becomes T target / V target The T target / V target The present invention is characterized in that it includes a pretreatment step of supplying power to the spinning furnace so that the

[0008] In order to achieve the above object, the optical fiber manufacturing apparatus of the present invention includes a spinning furnace for heating an optical fiber preform to draw an optical fiber, a power supply unit for supplying power to the spinning furnace, and a control unit, the control unit defining a tension applied to the optical fiber when drawing the optical fiber and a speed at which the optical fiber is taken out as T and V, respectively, and a target value of the tension as T. target The target value of the speed is V target If T / V is the time course, the value of the vertex becomes T target / V target The T target / V target The power supply unit is controlled so as to

[0009] The tension may be applied to a bare optical fiber that is not covered with a coating layer. The T / V ratio corresponds to the diameter of the optical fiber to be drawn. target / V target is the value corresponding to the target diameter of the optical fiber, and this T target / V target is determined depending on, for example, the material of the optical fiber base material, the spinning furnace, etc.

[0010] As a result of intensive research, the inventors have found that T / V decreases along the above quadratic function, and T target / V targetBy setting the value as above, the T / V decreases linearly, i.e., the rate of decrease of the T / V is roughly constant. target / V target After that, the T target / V target Therefore, it was found that T / V is less likely to deviate from T target / V target Therefore, according to the optical fiber manufacturing method and the optical fiber manufacturing apparatus, the time required for T / V to stabilize at the target value, that is, the time required for the tension T and the velocity V to stabilize at the target values, can be shortened, thereby improving the productivity of the optical fiber.

[0011] The quadratic function expressing the change over time T(t) / V(t) of the T / V is target / V target The time when 0 A constant determined in advance according to the optical fiber preform is a 0 In this case, the following formula T(t) / V(t)=a 0 (tt 0 ) 2 +(T target / V target ) It may be expressed as:

[0012] The present inventors have conducted extensive research into the change in T / V over time from when heating of the optical fiber preform begins until the T / V becomes approximately constant. As a result, the present inventors have found that when a constant power is supplied to a spinning furnace, T / V decreases over time in a manner similar to a quadratic function whose peak value is a minimum value until a certain point in time, at which point T / V reaches the peak of this quadratic function, and from that point in time T / V becomes approximately constant at the value at the peak, and the value of this approximately constant T / V corresponds to the value of the constant power. For this reason, for example, when the above constant a 0 , and time t 0can be obtained in advance by experiment, and the constant power at which T / V decreases according to the above formula can also be known in advance. Therefore, by supplying this constant power to the spinning furnace, the peak value of T / V will decrease over time. target / V target Therefore, the control load can be reduced.

[0013] Alternatively, in the above-mentioned method for producing an optical fiber, in the pretreatment step, a constant power is supplied to the spinning furnace for a predetermined period of time to obtain a quadratic function representing a change in the T / V over time, and the T / V value at the apex of the quadratic function and the T target / V target The constant power supplied to the spinning furnace may be changed based on the difference between the

[0014] The inventor has found that, when the power is kept constant as described above, T / V decreases over time in a quadratic function whose peak value is the minimum value up to a certain point. target / V target Even if the quadratic function T / V is not determined in advance by experiment, the value of the peak will be T target / V target It decreases along the quadratic function T target / V target It can be made to be as follows.

[0015] In the above-described method for producing an optical fiber, it is preferable that the pretreatment step is performed after a positioning step of inserting the neck-down portion of the optical fiber preform up to the position of a heater in the spinning furnace.

[0016] The change in T / V over time until the neck-down portion of the optical fiber preform reaches the heater position in the spinning furnace tends to deviate from a quadratic function. Therefore, it is difficult to reduce the T / V to conform to a quadratic function until the neck-down portion of the optical fiber preform reaches the heater position, which may impose a control load. Therefore, by performing a pre-processing process after the positioning process, such a control load can be reduced.

[0017] The tension is preferably a tension applied to a bare optical fiber.

[0018] In this case, the value of tension T does not include the tension component caused by the coating layer, so T / V can be calculated more accurately than when the value of tension T includes the tension component caused by the coating layer.

[0019] In this case, the tension applied to the bare optical fiber is Tg, the cross-sectional area of ​​the bare optical fiber is Sg, and the target value of the cross-sectional area of ​​the bare optical fiber is S target In this case, the following formula T = Tg × (S target / Sg) It is more preferable that the value be calculated by the following formula:

[0020] The tension Tg applied to the bare optical fiber is actually affected by the fluctuation of the cross-sectional area Sg of the bare optical fiber. Therefore, as in the above formula, the value of T / V can be calculated more accurately by adding the ratio of the actual cross-sectional area of ​​the bare optical fiber to the target cross-sectional area of ​​the bare optical fiber to the tension Tg.

[0021] As described above, according to the present invention, it is possible to provide an optical fiber manufacturing method and an optical fiber manufacturing apparatus that can improve the productivity of optical fibers. [Brief description of the drawings]

[0022] [Figure 1] 1 is a diagram illustrating a cross section perpendicular to the longitudinal direction of an optical fiber according to an embodiment of the present invention. [Diagram 2] 2 is a diagram illustrating a schematic cross section perpendicular to the longitudinal direction of an optical fiber preform for producing the optical fiber illustrated in FIG. 1. [Diagram 3] 1 is a schematic diagram illustrating an optical fiber manufacturing apparatus according to an embodiment of the present invention. [Figure 4] 2 is a flow chart showing steps of a method for manufacturing an optical fiber according to an embodiment of the present invention. [Diagram 5] 1 is a graph showing the change over time in T / V according to an embodiment of the present invention. [Figure 6] 10 is a graph showing a schematic change in T / V over time according to a modified example of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0023] Hereinafter, embodiments for carrying out the optical fiber manufacturing method and optical fiber manufacturing apparatus according to the present invention will be illustrated with reference to the accompanying drawings. The embodiments illustrated below are intended to facilitate understanding of the present invention, and are not intended to limit the present invention. The present invention can be modified and improved from the following embodiments without departing from the spirit of the present invention. In addition, in this specification, the dimensions of each member may be exaggerated in some cases to facilitate understanding.

[0024] Fig. 1 is a schematic diagram showing a cross section perpendicular to the longitudinal direction of an optical fiber according to an embodiment of the present invention. As shown in Fig. 1, the optical fiber 1 of this embodiment mainly comprises a core 10, a cladding 11 surrounding the outer peripheral surface of the core 10, and a coating layer 12 coating the outer peripheral surface of the cladding 11. The outer shape of the core 10 in the cross section is circular, and the core 10 is disposed at the center of the cladding 11. The outer shape of the cladding 11 in the cross section may be non-circular, such as elliptical or polygonal. Fig. 1 shows the optical fiber 1 in which the outer shape of the cladding 11 is circular.

[0025] The refractive index of the core 10 is set higher than that of the clad 11. In this embodiment, the core 10 is made of silica glass without any additives, and the clad 11 is made of silica glass with a dopant such as fluorine (F) that lowers the refractive index. The core 10 may be made of silica glass with a dopant such as germanium (Ge) that increases the refractive index, and the clad 11 may be made of silica glass without any additives. The core 10 may be made of silica glass with a dopant that increases the refractive index, and the clad 11 may be made of silica glass with a dopant that decreases the refractive index. The dopant that increases the refractive index and the dopant that decreases the refractive index are not particularly limited.

[0026] The coating layer 12 is made of a resin. Examples of the resin constituting the coating layer 12 include a thermosetting resin and an ultraviolet-curable resin. The coating layer 12 may have a single-layer structure made of one resin layer surrounding the cladding 11, or may have a multilayer structure made of multiple resin layers.

[0027] Fig. 2 is a schematic diagram showing a cross section perpendicular to the longitudinal direction of an optical fiber preform for manufacturing the optical fiber 1 shown in Fig. 1. As shown in Fig. 2, the optical fiber preform 1P is composed of a rod-shaped core glass body 10P that becomes the core 10, and a cladding glass body 11P that surrounds the outer peripheral surface of the core glass body 10P and becomes the cladding 11. In this embodiment, the outer shape of the cladding glass body 11P in the cross section is circular, and the core glass body 10P is disposed at the center of the cladding glass body 11P. The outer shape of the core glass body 10P in the cross section is also circular.

[0028] Fig. 3 is a schematic diagram of an optical fiber manufacturing apparatus according to the present embodiment. As shown in Fig. 1, the optical fiber manufacturing apparatus 100 mainly includes a spinning furnace 110, a delivery section 115, a first outer diameter measuring section 121, a cooling device 130, a coating section 140, a hardening section 145, a second outer diameter measuring section 122, a turn pulley 150, a tension meter 151, a take-up device 160, a speed meter 161, a winding device 170, a calculation section 180, a memory 190, a power supply section 200, and a control section CO.

[0029] The control unit CO is composed of, for example, an integrated circuit such as a microcontroller, an integrated circuit (IC), a large-scale integrated circuit (LSI), or an application specific integrated circuit (ASIC), or an NC (Numerical Control) device. When an NC device is used, the control unit CO may or may not use a machine learning device. As described below, some components of the optical fiber manufacturing apparatus 100 are controlled by the control unit CO.

[0030] The spinning furnace 110 includes a furnace tube 111 and a heater 112 arranged to surround the furnace tube 111 so as to heat the furnace tube 111. The heater 112 generates heat in response to power supplied from a power supply unit 200. The power supply unit 200 adjusts the power supplied to the heater 112 according to a control signal from the control unit CO. The delivery unit 115 is attached to the upper end of the optical fiber preform 1P and is configured to deliver the optical fiber preform 1P from the lower end side into the accommodation space of the furnace tube 111. The delivery unit 115 adjusts the delivery speed of the optical fiber preform 1P according to a control signal from the control unit CO.

[0031] Heater 112 generates heat to heat core tube 111. Optical fiber preform 1P is inserted into the accommodation space of core tube 111 from the lower end side, and the lower end of optical fiber preform 1P is heated. The lower end of optical fiber preform 1P heated by heater 112 is in a molten state, and as a result, a neck-down portion ND that tapers downward is formed at the lower end of optical fiber preform 1P, and a glass wire is drawn from the neck-down portion ND. When this drawn glass wire comes out of the lower opening of core tube 111, it immediately solidifies, and core glass body 10P becomes core 10, cladding glass body 11P becomes cladding 11, and the core 10 and cladding 11 constitute bare optical fiber 1N.

[0032] The first outer diameter measuring unit 121 is disposed below the spinning furnace 110, measures the outer diameter of the bare optical fiber 1N drawn in the spinning furnace 110, and outputs a signal indicating the measured diameter value of the bare optical fiber 1N to the calculation unit 180. The first outer diameter measuring unit 121 may, for example, have a light irradiating unit that emits laser light and a light receiving unit that receives the laser light emitted from the light irradiating unit, and the light irradiating unit and the light receiving unit may be disposed to sandwich the bare optical fiber 1N.

[0033] The cooling device 130 is disposed below the first outer diameter measurement unit 121, and cools the bare optical fiber 1N to an appropriate temperature. The coating unit 140 is disposed below the cooling device 130, and the curing unit 145 is disposed below the coating unit 140. The coating unit 140 coats the bare optical fiber 1N with uncured resin that will become the coating layer 12, and the curing unit 145 cures this resin to form the coating layer 12. In this way, the bare optical fiber 1N becomes the optical fiber 1. When the coating layer 12 is made of a thermosetting resin, the curing unit 145 is configured to apply heat to the resin, and when the coating layer 12 is made of an ultraviolet-curable resin, the curing unit 145 is configured to irradiate the resin with ultraviolet light.

[0034] The second outer diameter measuring unit 122 is disposed below the hardening unit 145, and measures the outer diameter of the coating layer 12, which is the outer diameter of the optical fiber 1. The second outer diameter measuring unit 122 outputs a signal indicating the measured value of the outer diameter of the optical fiber 1 to the calculation unit 180 and the control unit CO. The second outer diameter measuring unit 122 may have a similar configuration to the first outer diameter measuring unit 121, for example.

[0035] The turn pulley 150 is disposed below the second outer diameter measurement unit 122. The optical fiber 1 has its direction changed by the turn pulley 150, and is taken up by the rotation of the take-up device 160. This applies tension to the optical fiber 1. The take-up device 160 adjusts the speed at which it takes up the optical fiber 1 based on a control signal from the control unit CO. Since the optical fiber 1 is the bare optical fiber 1N coated with the coating layer 12, this speed can be understood to also be the speed at which the bare optical fiber 1N is taken up. The optical fiber 1 that has passed through the take-up device 160 that takes up the optical fiber 1 is sent to the take-up device 170, and is taken up by the take-up device 170.

[0036] The tension meter 151 is provided on the turn pulley 150, measures the tension, and outputs a signal indicating the value of the tension to the calculation unit 180. As the tension meter 151, for example, a configuration using a strain gauge can be given.

[0037] The speedometer 161 is provided on the take-up device 160, and measures the speed at which the optical fiber 1 is taken up based on the number of rotations per unit time of the take-up device 160, and outputs a signal indicating the value of the speed to the calculation unit 180 and the control unit CO. As the speedometer 161, for example, a configuration using a magnetic sensor can be mentioned.

[0038] The memory 190 is connected to the calculation unit 180 and the control unit CO. The memory 190 is configured to store information and to be able to read the stored information. The memory 190 is, for example, a non-transitory recording medium, and is preferably a semiconductor recording medium such as a random access memory (RAM) or a read only memory (ROM), but may include any type of recording medium such as an optical recording medium or a magnetic recording medium. Note that the term "non-transitory" recording medium includes a recording medium from which all data can be read except for a transient, propagating signal, and does not exclude a volatile recording medium. The memory 190 stores information necessary for calculation by the calculation unit 180, which will be described later, information necessary for control of each component by the control unit CO, and the like.

[0039] The calculation unit 180 performs various calculations based on the input information. For example, the calculation unit 180 has a configuration similar to that of the control unit CO. In this embodiment, when the diameter of the bare optical fiber 1N is Dn and the cross-sectional area of ​​the bare optical fiber 1N is Sg, the calculation unit 180 calculates the cross-sectional area Sg of the bare optical fiber 1N based on the signal input from the first outer diameter measurement unit 121 by the following formula (1). Sg = π(Dn / 2) 2 (1) In addition, when the diameter of the optical fiber 1 is Dc and the cross-sectional area of ​​the coating layer 12 is Sc, the calculation unit 180 calculates the cross-sectional area Sc of the coating layer 12 based on the signal input from the first outer diameter measurement unit 121 and the signal input from the second outer diameter measurement unit 122 using the following formula (2). Sc=π{(Dc / 2)-(Dn / 2)} 2 (2)

[0040] Incidentally, the tension measured by the tension meter 151 is the tension applied to the optical fiber 1, and therefore this tension can be considered as the sum of the tension applied to the bare optical fiber 1N and the tension applied to the coating layer 12. Here, if the tension applied to the coating layer 12 is Tc and the speed at which the optical fiber 1 is pulled out is V, the tension Tc can be calculated by the following formula (3). Tc = α β V Sc (3) Here, α is the tension per unit area of ​​the coating layer 12, and β is a proportionality constant, and these values ​​are stored in the memory 190. In the present embodiment, when the tension measured by the tension meter 151 is Tf and the tension applied to the bare optical fiber 1N is Tg, the calculation unit 180 calculates the tension Tg by the following formula (4). Tg = Tf - α β V Sc (4)

[0041] In addition, in this embodiment, the calculation unit 180 calculates T expressed by the following formula (5) based on the cross-sectional area Sg of the bare optical fiber 1N calculated by formula (2) and the tension Tg calculated by formula (4), and outputs a signal indicating the calculated value to the control unit CO. T = Tg × (S target / Sg) (5) In addition, S target is the target cross-sectional area of ​​the bare optical fiber 1N, and this value is stored in the memory 190. Here, the tension Tg applied to the bare optical fiber 1N is actually affected by the fluctuation of the cross-sectional area Sg of the bare optical fiber 1N. Therefore, T expressed by the above formula (5) is the ratio of the cross-sectional area of ​​the bare optical fiber 1N to the target value S target This is the tension Tg that takes into account the ratio of the cross-sectional area Sg of the bare optical fiber 1N.

[0042] In this embodiment, the calculation unit 180 outputs a signal indicating the value of T to the control unit CO as the tension applied to the optical fiber 1. The calculation unit 180 also outputs a signal indicating the value of the speed at which the optical fiber 1 is withdrawn, which is input from the speedometer 161, to the control unit CO.

[0043] Next, a method for producing the optical fiber 1 using the optical fiber production apparatus 100 will be described.

[0044] Fig. 4 is a flow chart showing steps of a method for manufacturing the optical fiber 1 according to this embodiment. As shown in Fig. 4, this manufacturing method includes a positioning step P1, a pretreatment step P2, and a drawing step P3.

[0045] (Positioning process P1) First, as a preparation stage for carrying out this process, the optical fiber preform 1P shown in FIG. 2 is prepared by purchase or the like, and is fixed to the delivery unit 115 of the optical fiber manufacturing apparatus 100. The control unit CO controls the power supply unit 200 to supply power from the power supply unit 200 to the heater 112, thereby heating the furnace tube 111. In this embodiment, the power supplied from the power supply unit 200 to the heater 112 is constant. Then, while the furnace tube 111 is in a heated state, the control unit CO controls the delivery unit 115 to cause the delivery unit 115 to deliver the optical fiber preform 1P, and the optical fiber preform 1P is delivered from the lower end side into the accommodation space of the furnace tube 111. The lower end of the optical fiber preform 1P is in a molten state, and as a result, a neck-down portion ND that tapers downward is formed at the lower end of the optical fiber preform 1P. The optical fiber preform 1P is fed by the feed unit 115, thereby lowering the neck-down portion ND to the position of the heater 112. The position of the heater 112 is a position along the central axis of the furnace tube 111 that overlaps with the section from the upper end to the lower end of the heater 112. In this embodiment, the optical fiber preform 1P is fed into the accommodation space until the position of the upper end of the neck-down portion ND is a specific position that is above the center of the heater 112 and a predetermined distance below the upper end of the heater 112. In this manner, the optical fiber preform 1P is positioned.

[0046] In this embodiment, even when the optical fiber preform 1P is lowered, the optical fiber 1 is drawn from the neck-down portion ND of the optical fiber preform 1P. The control unit CO controls the take-up device 160 based on the value of the outer diameter of the optical fiber 1 measured by the second outer diameter measuring unit 122, and adjusts the speed at which the optical fiber 1 is taken out, so that the outer diameter of the optical fiber 1 becomes the target value. However, during this process, the temperature of the molten portion of the optical fiber preform 1P is elevated, so that the outer diameter of the optical fiber 1 to be drawn is not stable. Note that after the optical fiber preform 1P is positioned, power may be supplied from the power supply unit 200 to the heater 112, and the power supplied to the heater 112 may not be constant. The control unit CO may also control the take-up device 160 based on the value of the outer diameter of the bare optical fiber 1N measured by the first outer diameter measuring unit 121, and adjust the speed at which the optical fiber 1 is taken out, so that the outer diameter of the bare optical fiber 1N becomes the target value.

[0047] (Pretreatment process P2) Next, the main process is performed. In general, the tension applied to the optical fiber 1 to be drawn and the speed at which the optical fiber 1 is taken out have values ​​at which the outer diameter of the drawn optical fiber 1 is stabilized. Such values ​​are determined, for example, according to the material of the optical fiber preform 1P and the spinning furnace, and can be obtained by experiments or the like. Such values ​​for each of the tension and speed are stored in the memory 190 as target values. In this process, the control unit CO controls the take-up device 160 based on the value of the outer diameter of the optical fiber 1 input from the second outer diameter measurement unit 122 and the value of the speed at which the optical fiber 1 is taken out measured by the speedometer 161 so that the speed increases to the target value and the outer diameter of the optical fiber 1 becomes a predetermined value. The control unit CO may also control the take-up device 160 based on the value of the outer diameter of the bare optical fiber 1N measured by the first outer diameter measurement unit 121 and the value of the speed at which the optical fiber 1 is taken out measured by the speedometer 161. The control unit CO also controls the power supply unit 200 based on the value of the tension T applied to the optical fiber 1 calculated by the calculation unit 180 and the value of the speed measured by the speedometer 161. Specifically, the control unit CO sets the speed at which the optical fiber 1 is pulled out as V and the target value of the tension as T targetLet the target speed be V target If T / V is the time course, the value of the vertex becomes T target / V target It decreases along the quadratic function T target / V target The power supply unit 200 is controlled to adjust the heating temperature of the optical fiber preform 1P so as to satisfy the above condition.

[0048] In this embodiment, the quadratic function expressing the change over time T(t) / V(t) of T / V is expressed as follows: target / V target The time when 0 , a constant determined in advance according to the optical fiber preform 1P is a 0 In this case, it is assumed that the following formula (6) is used. T(t) / V(t)=a 0 (tt 0 ) 2 +(T target / V target ) ···(6) Here, the inventors have conducted extensive research into the change in T / V over time during the period from when heating of the optical fiber preform 1P begins until the above T / V becomes approximately constant. As a result, the inventors have found that when a constant power is supplied to the spinning furnace 110, T / V decreases over time in a manner similar to a quadratic function whose peak value is a minimum value until a certain point in time, at which point T / V reaches the peak of this quadratic function, and from that point in time T / V becomes approximately constant at the value at the peak, and this approximately constant value corresponds to the value of the constant power. For this reason, the above constant a 0 , and time t 0 can be obtained in advance by experiment or the like, and the constant power at which T / V decreases according to equation (6) can also be known in advance. In this embodiment, these values ​​obtained in advance by experiment are stored in memory 190. Also, in this embodiment, the constant power supplied to heater 112 in positioning step P1 is set to a constant power at which T / V decreases according to equation (6). Therefore, the power supplied to heater 112 at the beginning of pre-processing step P2 is this constant power. Therefore, as T / V increases over time, the peak value becomes Ttarget / V target Since the output voltage Vcc decreases approximately in accordance with a quadratic function, the control load of the control unit CO can be reduced.

[0049] FIG. 5 is a graph showing the change over time of T / V in this embodiment. In the graph of FIG. 5, the part shown by the thin line is the change over time of T / V during the positioning step P1. Meanwhile, the part shown by the thick line is the change over time of T / V during the pre-processing step P2. Furthermore, FIG. 5 shows the above formula (6) by the dashed line. As shown in FIG. 5, in the pre-processing step P2, the peak value of T / V becomes T target / V target It decreases along the quadratic function T target / V target And the speed V becomes V target The tension T is T target Then, the outer diameter of the bare optical fiber 1N becomes stable, and the outer diameter of the optical fiber 1 becomes stable.

[0050] (Drawing process P3) This step is a step of drawing the optical fiber 1 after the pretreatment step P2, that is, in a state where the outer diameter of the optical fiber 1 is stable. In this embodiment, the control unit CO controls the delivery unit 115 so that the position of the neck-down portion ND of the optical fiber preform 1P relative to the heater 112 does not change, and the delivery amount of the optical fiber preform 1P is adjusted. In addition, the control unit CO determines whether the speed V is V based on the value of the speed V measured by the speedometer 161. target The control unit CO controls the take-off device 160 so that the T / V is maintained at T target / V target The power supply unit 200 is controlled to adjust the heating temperature of the optical fiber preform 1P so that the outer diameter is maintained at the target value. Therefore, the optical fiber 1 having the target outer diameter can be stably drawn.

[0051] As described above, the method for producing an optical fiber in this embodiment includes a pretreatment step P2. In the pretreatment step P2, the tension applied to the optical fiber 1 when the optical fiber preform 1P is heated in the spinning furnace 110 and the optical fiber 1 is drawn and the speed at which the optical fiber 1 is drawn are defined as T and V, respectively, and the target value of the tension is set to T target Let the target speed be V target If T / V is the time course, the value of the vertex becomes T target / V target It decreases along the quadratic function T target / V target Power is supplied to the spinning furnace 110 so that

[0052] The optical fiber manufacturing apparatus 100 in this embodiment includes a spinning furnace 110 for heating the optical fiber preform 1P to draw the optical fiber 1, a power supply unit 200 for supplying power to the spinning furnace 110, and a control unit CO. The control unit CO is configured to detect when the peak value of T / V becomes T target / V target It decreases along the quadratic function T target / V target The power supply unit 200 is controlled so as to satisfy the above.

[0053] As a result of intensive research, the inventors have found that T / V decreases along the above quadratic function, and T target / V target By setting the value as above, the T / V decreases linearly, i.e., the rate of decrease of the T / V is roughly constant. target / V target After that, the T target / V target Therefore, it was found that T / V is less likely to deviate from T target / V target After this, adjustment of the power supplied to the spinning furnace 110 is suppressed. Therefore, according to the optical fiber manufacturing method and the optical fiber manufacturing apparatus 100 of the present embodiment, the time required for T / V to stabilize at the target value, that is, the time required for the tension T and the velocity V to stabilize at the target values, can be shortened, thereby improving the productivity of the optical fiber 1.

[0054] In the optical fiber manufacturing method and the optical fiber manufacturing apparatus 100 of the present embodiment, the tension T is defined as Tg, the tension applied to the bare optical fiber 1N is defined as Sg, the cross-sectional area of ​​the bare optical fiber 1N is defined as Sg, and the target value of the cross-sectional area of ​​the bare optical fiber 1N is defined as S target is calculated by the above formula (5). Therefore, the tension T in this embodiment is the tension applied to the bare optical fiber 1N, and the value of the tension T does not include a tension component caused by the coating layer 12. Therefore, the value of T / V can be calculated more accurately than when the value of the tension T includes a tension component caused by the coating layer 12.

[0055] Furthermore, the tension Tg applied to the bare optical fiber 1N is actually affected by fluctuations in the cross-sectional area Sg of the bare optical fiber 1N. Therefore, as in this embodiment, by adding the ratio between the actual measured cross-sectional area of ​​the bare optical fiber 1N and the target cross-sectional area of ​​the bare optical fiber 1N to the tension Tg using formula (5), the value of T / V can be calculated more accurately.

[0056] 5, it can be seen that the change in T / V over time in the positioning step P1, which is the period until the tip of the optical fiber preform 1P reaches the position of the heater 112, tends to deviate from a quadratic function. For this reason, it is difficult to reduce T / V to follow a quadratic function until the neck-down portion ND of the optical fiber preform 1P reaches the position of the heater 112, which may result in a control load. In this embodiment, the pre-processing step P2 is performed after the positioning step P1, so that such a control load can be reduced. However, the pre-processing step P2 may be performed during the positioning step P1.

[0057] Although the present invention has been described above by taking the above embodiment as an example, the present invention is not limited to this.

[0058] For example, in the above embodiment, the pre-treatment process P2 is described as an example in which power is supplied to the spinning furnace 110 so that T / V decreases according to the above formula (6). However, in the pre-treatment process P2, the peak value of T / V decreases with time.target / V target It decreases along the quadratic function T target / V target Electric power may be supplied to the spinning furnace 110 so that the

[0059] For example, the following modified pretreatment step may be performed.

[0060] In this modification, after the optical fiber preform 1P is positioned by the positioning step P1, a constant power EP1 is supplied to the spinning furnace 110. In this modification, the constant power EP1 is the same as the constant power supplied in the positioning step P1, but may be different. Since the power supplied to the spinning furnace 110 is constant, T / V decreases along a quadratic function during the period in which the constant power EP1 is supplied. FIG. 6 is a graph that shows an outline of the change in T / V over time in this modification, and the change in T / V over time is shown by a solid line. The calculation unit 180 calculates a quadratic function that represents the change in T / V over time by approximation based on a plurality of T / V values ​​during the period in which the constant power EP1 is supplied. In FIG. 6, the calculated quadratic function is shown by a dashed line. Note that the quadratic function is shown slightly shifted from the change in T / V over time. As an approximation method, for example, the least square method can be mentioned. The calculation unit 180 calculates the value of T / V at the vertex of the quadratic function and T target / V target The control unit 10 calculates the difference d between the T / V value and the T / V value, and outputs a signal indicating the difference d to the control unit 10. In this modification, the difference d is calculated by subtracting T target / V target It has positive and negative values.

[0061] The control unit CO controls the power supply unit 200 based on this difference d. Specifically, when the difference d is positive and the absolute value of the difference d is greater than a predetermined value, the control unit CO controls the power supply unit 200 so that the power supplied to the spinning furnace 110 becomes a constant power higher than the constant power EP1 from time t1. Therefore, the viscosity of the optical fiber preform 1P in the molten state decreases, and the tension T decreases, so that T / V decreases. On the other hand, when the difference d is negative and the absolute value of the difference d is greater than a predetermined value, the control unit CO controls the power supply unit 200 so that the power supplied to the spinning furnace 110 becomes a constant power lower than the constant power EP1 from time t1. Therefore, the viscosity of the optical fiber preform 1P in the molten state increases, and the tension T increases, so that T / V increases. In addition, when the absolute value of the difference d is equal to or less than a predetermined value, the control unit CO controls the power supply unit 200 so that the power supplied to the spinning furnace 110 is maintained at the constant power EP1 even after time t1. FIG. 6 shows a case where the power supplied to the spinning furnace 110 becomes a constant power EP2 higher than the constant power EP1 from time t1.

[0062] The calculation unit 180 calculates, by approximation, a quadratic function that represents the change in T / V over time, based on a number of values ​​of T / V after time t1. In Fig. 6, the calculated quadratic function is shown by a two-dot chain line. Note that the quadratic function is shown slightly shifted from the change in T / V over time. The calculation unit 180 also calculates the relationship between the value of T / V at the apex of the quadratic function and T target / V target The control unit CO calculates the difference d between T / V and T target / V target In the same manner as when the difference d between the power supply voltage Vcc and the power supply voltage Vcc is calculated, the power supply unit 200 is controlled based on this difference d.

[0063] Then, a quadratic function that represents the change in T / V over time is calculated, and the T / V value at the peak of the quadratic function and T target / V target The change in constant power based on the difference d between T and V is target / V targetThis is repeated until the constant power EP2 is reached. Fig. 6 shows a case where a constant power EP3 higher than the constant power EP2 is supplied to the spinning furnace 110 from time t2, a predetermined period of time after time t1. A quadratic function calculated based on a plurality of values ​​of T / V during the period in which the constant power EP3 is supplied is shown by a dashed line. In the example shown in Fig. 6, the value of T / V at the apex of this quadratic function and T target / V target When the absolute value of the difference between T and V becomes less than the above-mentioned predetermined value, the value of T / V at time t3 becomes T target / V target It is as follows.

[0064] As described above, in the pretreatment process of this modified example, a constant power is supplied to the spinning furnace 110 for a predetermined period of time, and a quadratic function that represents the change in T / V over time is calculated. The T / V value at the apex of the quadratic function and the T target / V target The constant power supplied to the spinning furnace 110 is changed based on the difference d between T target / V target Even if the quadratic function with the vertex at is not determined in advance by experiment, it is possible to determine the relationship between T / V and T target / V target It decreases along a quadratic function with a peak at T target / V target It can be made to be as follows.

[0065] In the above embodiment, the tension T is calculated by the formula (5), but the tension T may be calculated by the formula (4). Even in this case, the tension T is the tension applied to the bare optical fiber 1N, and the value of the tension T does not include the tension component caused by the coating layer 12. Therefore, the value of T / V in the bare optical fiber 1N can be calculated more accurately than when the value of the tension T includes the tension component caused by the coating layer 12. In addition, since there is no need to calculate the formula (5), the control load can be reduced. Alternatively, the tension T may be a value measured by the tension meter 151. In this case, there is no need to calculate the formula (4) or (5), so the control load can be reduced.

[0066] According to the present invention, an optical fiber manufacturing method and an optical fiber manufacturing apparatus capable of improving the productivity of optical fibers are provided, and can be used in various fields related to optical fibers.

Claims

1. The tension applied to the optical fiber when the optical fiber preform is heated in a spinning furnace and the optical fiber is drawn is defined as T and the speed at which the optical fiber is drawn is defined as V. The target value of the tension is defined as T. target The target value of the speed is V target In this case, the value at the apex of T / V becomes T target / V target The T target / V target A pretreatment step of supplying power to the spinning furnace so that 2. A method for producing an optical fiber comprising the steps of:

2. The quadratic function expressing the change over time T(t) / V(t) of the T / V is target / V target The time when 0 A constant determined in advance according to the optical fiber preform is a 0 In this case, the following formula T(t) / V(t)=a 0 (t-t 0 ) 2 + (T target / V target ) Represented by 2. The method for producing an optical fiber according to claim 1.

3. In the pretreatment step, a quadratic function expressing the change in T / V over time is obtained by supplying a constant power to the spinning furnace for a predetermined period of time, and the value of T / V at the apex of the quadratic function and the value of T target / V target The constant power supplied to the spinning furnace is changed based on the difference between the 2. The method for producing an optical fiber according to claim 1.

4. The pretreatment step is performed after a positioning step of inserting the neck-down portion of the optical fiber preform to the position of a heater in the spinning furnace.

4. The method for producing an optical fiber according to claim 1,

5. The tension is the tension applied to the bare optical fiber.

5. The method for producing an optical fiber according to claim 1.

6. The tension is Tg, the cross-sectional area of ​​the bare optical fiber is Sg, and the target value of the cross-sectional area of ​​the bare optical fiber is S target In this case, the following formula T = Tg × (S target / Sg) The value is calculated as follows:

6. The method for producing an optical fiber according to claim 5.

7. a spinning furnace for heating an optical fiber preform to draw an optical fiber; A power supply unit that supplies power to the spinning furnace; A control unit; Equipped with The control unit defines the tension applied to the optical fiber when drawing the optical fiber and the speed at which the optical fiber is drawn as T and V, respectively, and sets a target value of the tension as T target The target value of the speed is V target In this case, the value at the apex of T / V becomes T target / V target The T target / V target The power supply unit is controlled so that 1. An optical fiber manufacturing apparatus comprising:

Citation Information

Patent Citations

  • Fiber drawing for optical fiber

    JP1999255534A

  • Method of drawing optical fiber

    JP2009126755A

  • Method for manufacturing optical fiber

    JP2010269971A

  • Manufacturing method and manufacturing apparatus of optical fiber element wire

    JP2017043528A

  • Apparatus & method for drawing optical fiber having desired waveguide parameters and fiber produced thereby

    WO2008062465A2