Flexographic printing plate

By integrating an oxygen barrier layer and increasing photopolymerization initiator content in the photosensitive resin layer, the flexographic printing plate effectively addresses oxygen polymerization inhibition, ensuring faithful microcell pattern reproduction and improved ink coverage in solid areas, thus improving printing quality and durability.

JP7554403B2Active Publication Date: 2024-09-20TOYOBO MC CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2023068045
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-08-23
Filing Date
2023-04-18
Publication Date
2024-09-20
Estimated Expiration
2040-07-30

AI Technical Summary

Technical Problem

Flexographic printing faces challenges in achieving adequate ink coverage in solid areas due to oxygen polymerization inhibition during exposure, which affects the faithful reproduction of microcell patterns on the printing plate, requiring special equipment or complex processes.

Method used

Incorporating an oxygen barrier layer between the photosensitive resin layer and the heat-sensitive mask layer, with an increased content of photopolymerization initiator in the photosensitive resin composition, to suppress oxygen polymerization inhibition and ensure complete crosslinking reactions during exposure, allowing faithful reproduction of microcell patterns without additional equipment or processes.

Benefits of technology

The solution enables faithful reproduction of microcell patterns and improved ink coverage in solid areas, enhancing the quality and durability of flexographic printing without the need for special equipment or additional steps.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007554403000001
    Figure 0007554403000001
  • Figure 0007554403000002
    Figure 0007554403000002
Patent Text Reader

Abstract

To provide a flexographic printing plate precursor which makes it possible to precisely reproduce a microcell pattern on the surface of a printing plate without a special device or an additional step, and thus to improve the ink laydown on a solid-printed part.SOLUTION: A flexographic printing plate precursor comprises at least a support (A), a photosensitive resin layer (B), an oxygen barrier layer (C) and a heat-sensitive mask layer (D) which are laminated in this order, wherein a photosensitive resin composition constituting the photosensitive resin layer (B) comprises (a) a polymer prepared by polymerizing a conjugated diene, (b) an ethylenically unsaturated compound and (c) a photopolymerization initiator, and wherein the content of the photopolymerization initiator (c) in the photosensitive resin composition is 2 to 9 mass%.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a flexographic printing plate precursor having good microcell reproducibility in solid areas of the printing plate and excellent ink adhesion in the solid areas. [Background technology]

[0002] Flexographic printing is a printing method in which ink is placed on the raised areas of a printing plate and then pressed against a substrate to transfer the ink from the printing plate to the substrate. The printing plate used in flexographic printing is relatively flexible and can conform to various shapes, making it possible to print on a wide range of substrates. Substrates include packaging films, label papers, beverage cartons, paper containers, envelopes, and cardboard, and flexographic printing is used exclusively for substrates with rough surfaces. Flexographic printing can also use water-based or alcohol-based inks that emit low amounts of VOCs, making it a highly environmentally friendly printing method. Due to these advantages, such as substrate adaptability and environmental adaptability, there is a shift from gravure printing and offset printing to flexographic printing.

[0003] On the other hand, flexographic printing has a problem in that the ink coverage in solid areas is inferior to that of gravure printing when printing on a film substrate. One method to improve the ink coverage in solid areas of flexographic printing is to increase the physical pressure between the printing plate and the printed material. However, in this case, the fine dots are deformed by the pressure, and the printability of the fine dots is impaired.

[0004] Another method is to provide microcells on the surface of the solid area to improve the ink adhesion of the solid area. Microcells refer to a specific minute uneven pattern formed on the surface of the solid area. By providing microcells, the ink can be given an appropriate mobility when the printing plate and the printed material are pressed against each other, and the uniformity of the ink distribution in the solid area can be improved. As a method for providing microcells on the solid area of ​​the printing plate, a method of imaging microcells on the solid area of ​​the thermal mask layer and reproducing them on the printing plate is widely used. A typical example is microcell screening made by ESKO-Graphic (see Non-Patent Document 1). Microcell screening includes the MC type that introduces rectangular cells, the GROOVY type that introduces oblique line cells, and the single pixel screen that introduces specially shaped cells. In order to effectively utilize these microcells, it is necessary to faithfully reproduce the microcell pattern depicted on the thermal mask layer on the solid area of ​​the printing plate.

[0005] In order to faithfully reproduce the microcell pattern on the surface of the printing plate, it is important to suppress the oxygen polymerization inhibition of the photosensitive resin layer. If the photosensitive resin layer is inhibited by oxygen polymerization, the crosslinking reaction in the photosensitive resin layer does not proceed sufficiently, and the surface of the photosensitive resin layer is washed out in the development process, making it impossible to faithfully reproduce the microcell pattern on the surface of the printing plate.

[0006] In response to this problem, Patent Document 1 proposes a method of faithfully reproducing a microcell pattern on the surface of a printing plate by exposing the printing plate under an inert gas atmosphere to suppress oxygen polymerization inhibition. However, there is a problem that a special device is required for exposure under an inert gas atmosphere. Patent Document 2 proposes a method of faithfully reproducing a microcell pattern on the surface of a printing plate by laminating an oxygen barrier layer after imaging on the mask layer to suppress oxygen polymerization inhibition. However, a dedicated laminator is required to laminate the oxygen barrier layer after imaging on the mask layer, and there is a problem that the plate making process becomes complicated. Patent Documents 3 and 4 propose a printing original plate in which oxygen polymerization inhibition is suppressed by providing an oxygen barrier layer between a photosensitive resin layer and a heat-sensitive mask layer. These methods have the advantage of not requiring special devices or additional processes during plate making. However, although these oxygen barrier layers can suppress oxygen polymerization inhibition to a certain extent, the progress of the crosslinking reaction is insufficient, and the microcell pattern cannot be faithfully reproduced on the surface of the printing plate. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] Patent No. 6219954 [Patent Document 2] Patent No. 5872693 [Patent Document 3] Patent No. 5573675 [Patent Document 4] Patent No. 4332865 [Non-patent literature]

[0008] [Non-Patent Document 1] Journal of the Japanese Society of Printing Science and Technology, Vol. 43, No. 4 (2006), pp. 261-271 Summary of the Invention [Problem to be solved by the invention]

[0009] The present invention has been made in consideration of the current state of the prior art described above, and an object of the present invention is to provide a flexographic printing original plate that can faithfully reproduce a microcell pattern on the surface of the printing plate without the need for special equipment or additional processes, and can improve ink adhesion in solid areas. [Means for solving the problem]

[0010] As a result of extensive research into achieving the above-mentioned object, the present inventors have discovered that by providing an oxygen barrier layer similar to those described in Patent Documents 3 and 4 between the photosensitive resin layer and the heat-sensitive mask layer, and by increasing the content of photopolymerization initiator in the photosensitive resin layer compared to conventional methods, the crosslinking reaction of the photosensitive resin can be allowed to proceed sufficiently without being affected by oxygen polymerization inhibition during exposure, particularly during main exposure, and thus the microcell pattern imaged on the heat-sensitive mask layer can be faithfully reproduced on the printing plate, thereby completing the present invention.

[0011] That is, the present invention has the following configurations (1) to (6). (1) A flexographic printing original plate comprising at least a support (A), a photosensitive resin layer (B), an oxygen barrier layer (C), and a heat-sensitive mask layer (D) laminated in that order, wherein the photosensitive resin layer (B) is formed from a photosensitive resin composition that contains (a) a polymer obtained by polymerizing a conjugated diene, (b) an ethylenically unsaturated compound, and (c) a photopolymerization initiator, and the content of the photopolymerization initiator (c) in the photosensitive resin composition is 2 to 9 mass %. (2) The flexographic printing original plate according to (1), characterized in that (b) the ethylenically unsaturated compound contains (i) a (meth)acrylate compound having a number average molecular weight of 100 or more and 600 or less, the content of (i) the (meth)acrylate compound having a number average molecular weight of 100 or more and 600 or less in the photosensitive resin composition is 5 to 16 mass %, and the ratio of the mass of (c) the photopolymerization initiator in the photosensitive resin composition to the mass of (i) the (meth)acrylate compound having a number average molecular weight of 100 or more and 600 or less is in the range of 0.20 to 0.55. (3) (b) The flexographic printing original plate according to (2), characterized in that the ethylenically unsaturated compound further comprises a (meth)acrylate compound (ii) having a number average molecular weight of more than 600 and not more than 20,000, and the content of the (meth)acrylate compound (ii) having a number average molecular weight of more than 600 and not more than 20,000 in the photosensitive resin composition is 5 to 25 mass %. (4) The flexographic printing plate precursor according to any one of (1) to (3), wherein development is carried out using an aqueous developer. (5) A flexographic printing plate obtained by exposing and developing the flexographic printing original plate of (1) to (4), characterized in that a microcell is applied to the solid portion formed on the printing plate. (6) A flexographic printing method using the flexographic printing plate according to (5). Effect of the Invention

[0012] The flexographic printing plate precursor of the present invention has an oxygen barrier layer between the photosensitive resin layer and the heat-sensitive mask layer, and the content of the photopolymerization initiator in the photosensitive resin composition is greater than that of the conventional one. Therefore, without any special equipment or additional steps, the microcell pattern can be faithfully reproduced on the surface of the printing plate without being affected by oxygen polymerization inhibition during exposure, particularly during main exposure, and the ink adhesion to the solid parts of the printing plate can be improved. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] The flexographic printing plate of the present invention is a flexographic printing plate having at least a support (A), a photosensitive resin layer (B), an oxygen barrier layer (C), and a heat-sensitive mask layer (D) laminated in sequence, and the photosensitive resin composition forming the photosensitive resin layer (B) contains (a) a polymer obtained by polymerizing a conjugated diene, (b) an ethylenically unsaturated compound, and (c) a photopolymerization initiator, and the content of the (c) photopolymerization initiator in the photosensitive resin composition is 2 to 9% by mass. By providing an oxygen barrier layer between the photosensitive resin layer and the heat-sensitive mask layer in this way and increasing the content of the photopolymerization initiator in the photosensitive resin composition compared to the conventional method, it is possible to faithfully reproduce a microcell pattern on the surface of the printing plate without being affected by oxygen polymerization inhibition during exposure, especially during main exposure, without any special equipment or additional process, and to improve the ink adhesion of the solid parts of the printing plate. In addition, the flexographic printing plate precursor of the present invention can faithfully reproduce the image of the thermal mask layer on the printing plate not only when the microcells are in the solid area, but also when the microcells are introduced into the special highlight dots or dots. Examples of the special highlight dots include SambaFlex Screen, PerfectHighlight Screens, Smooth PerfectHighlight, and Support dot, which are manufactured by ESKO, and have an adjusted number of highlight dots. Examples of the introduction of microcells into dots include Crystal Screening, manufactured by ESKO.

[0014] The support (A) used in the flexographic printing plate precursor is preferably a material that is flexible but has excellent dimensional stability, and may be, for example, a metal support such as steel, aluminum, copper, or nickel, or a thermoplastic resin support such as a polyethylene terephthalate film, a polyethylene naphthalate film, a polybutylene terephthalate film, or a polycarbonate film. Among these, a polyethylene terephthalate film having excellent dimensional stability and sufficiently high viscoelasticity is particularly preferred. The thickness of the support is desirably 50 to 350 μm, preferably 100 to 250 μm, in view of mechanical properties, shape stability, or handling during printing plate making. If necessary, an adhesive may be provided between the support (A) and the photosensitive resin layer (B) to improve the adhesion between them.

[0015] The photosensitive resin composition forming the photosensitive resin layer (B) used in the flexographic printing original plate contains (a) a polymer obtained by polymerizing a conjugated diene, (b) an ethylenically unsaturated compound, and (c) a photopolymerization initiator, and further contains additives such as a plasticizer, a hydrophilic compound, an ultraviolet absorber, a surface tension adjuster, a thermal polymerization inhibitor, a dye, a pigment, a fragrance, or an antioxidant, as necessary. In particular, the present invention is characterized in that the composition of the ethylenically unsaturated compound (b) in the photosensitive resin composition forming the photosensitive resin layer (B) is devised, and that the photopolymerization initiator (c) is used in a mass ratio greater than the amount actually used in the past.

[0016] (a) As the polymer obtained by polymerizing a conjugated diene, a conventionally known synthetic polymer compound used for a printing plate can be used. Specifically, a polymer obtained by polymerizing a conjugated diene hydrocarbon, or a copolymer obtained by copolymerizing a conjugated diene hydrocarbon with a monoolefin unsaturated compound can be used. For example, a butadiene polymer, an isoprene polymer, a chloroprene polymer, a styrene-butadiene copolymer, a styrene-butadiene-styrene copolymer, a styrene-isoprene copolymer, a styrene-isoprene-styrene copolymer, a styrene-chloroprene copolymer, an acrylonitrile-butadiene copolymer, an acrylonitrile-isoprene copolymer, a methyl methacrylate-butadiene copolymer, a methyl methacrylate-isoprene copolymer, an acrylonitrile-butadiene-styrene copolymer, an acrylonitrile-isoprene-styrene copolymer, and the like can be used. Among these, a butadiene polymer is preferably used from the viewpoint of the characteristics as a flexographic printing plate, that is, the impact resilience of the plate surface, the strength and elongation properties, the resin plate hardness, and the shape stability when not exposed, or the availability, etc. These polymers may be used alone or in combination of two or more. The proportion of the component (a) in the photosensitive resin composition forming the photosensitive resin layer (B) is preferably in the range of 40 to 70 mass %.

[0017] As the (b) ethylenically unsaturated compound, a conventionally known compound used in a printing plate can be used, but it is preferable to include a (meth)acrylate compound (i) having a number average molecular weight of 100 to 600 (hereinafter also simply referred to as a low molecular weight (meth)acrylate compound), and further, it is preferable to include a (meth)acrylate compound (ii) having a number average molecular weight of more than 600 and not more than 20,000 (hereinafter also simply referred to as a high molecular weight (meth)acrylate compound). Here, the low molecular weight (meth)acrylate compound is crosslinked and hardened by a photopolymerization initiator to form a dense crosslinked network, and the high molecular weight (meth)acrylate compound is crosslinked and hardened by a photopolymerization initiator to form a loose crosslinked network. The former is more preferably a number average molecular weight of 200 to 500, and the latter is more preferably a number average molecular weight of 2000 to 10000. As described above, by blending not only low molecular weight (meth)acrylate compounds but also high molecular weight (meth)acrylate compounds, the reproducibility of independent points and durability during printing are not impaired even when a larger amount of (c) photopolymerization initiator is blended than before. This is thought to be because the inclusion of a certain proportion of high molecular weight (meth)acrylate compounds increases the toughness of the plate. The proportion of component (b) in the photosensitive resin composition forming the photosensitive resin layer (B) is preferably in the range of 10 to 50 mass%.

[0018] The content of the high molecular weight (meth)acrylate compound in the photosensitive resin composition is preferably 5 to 25% by mass, more preferably 8 to 20% by mass. If the content is less than the above range, durability is likely to decrease when a large amount of (c) photopolymerization initiator is blended, and if the content exceeds the above range, the composite elastic modulus of the solid part is likely to be high, and the ink adhesion of the solid part may be insufficient, resulting in poor quality of the printed matter. In addition, the content of the low molecular weight (meth)acrylate compound in the photosensitive resin composition is preferably 5 to 16% by mass, more preferably 7 to 13% by mass. If the content of the low molecular weight (meth)acrylate compound is less than the above range, oxygen polymerization inhibition may not be sufficiently suppressed, and if the content exceeds the above range, the plate may become too hard, and the ink adhesion of the solid part may be insufficient, resulting in poor quality of the printed matter.

[0019] The low molecular weight (meth)acrylate compound is not particularly limited as long as the number average molecular weight is within the range of 100 or more and 600 or less, and examples thereof include linear, branched, and cyclic monofunctional monomers such as hexyl (meth)acrylate, nonane (meth)acrylate, lauryl (meth)acrylate, stearyl (meth)acrylate, 2-ethyl, 2-butylpropanediol (meth)acrylate, hydroxyethyl (meth)acrylate, 2-(meth)acryloyloxyethyl hexahydrophthalate, 2-(meth)acryloyloxyethyl phthalate, (meth)acrylic acid dimer, ECH-modified allyl acrylate, benzyl acrylate, caprolactone (meth)acrylate, dicyclopentenyl (meth)acrylate, isobornyl (meth)acrylate, and cyclohexyl (meth)acrylate. In addition, linear, branched, and cyclic polyfunctional monomers such as hexanediol di(meth)acrylate, nonanediol di(meth)acrylate, 2-butyl-2-ethylpropane di(meth)acrylate, neopentyl glycol di(meth)acrylate, hydroxypivalic acid neopentyl glycol di(meth)acrylate, ECH-modified phthalic acid di(meth)acrylate, dicyclopentadiene di(meth)acrylate, tricyclodecane dimethanol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, ECH-modified glycerol tri(meth)acrylate, trimethylolpropane benzoate (meth)acrylate, EO(PO)-modified trimethylolpropane tri(meth)acrylate, and dipentaerythritol hexa(meth)acrylate may also be used. Only one of these compounds may be used alone, or two or more may be used in combination to provide the desired resin properties.

[0020] The high molecular weight (meth)acrylate compound is not particularly limited as long as it has a number average molecular weight in the range of more than 600 and not more than 20,000, and examples thereof include butadiene oligomers or isoprene oligomers to which a (meth)acrylate group has been added, and urethane (meth)acrylates. These compounds may be used alone or in combination of two or more to provide the desired resin properties.

[0021] (c) The ratio of the mass of the photopolymerization initiator to the mass of the low molecular weight (meth)acrylate compound (i) [(mass of photopolymerization initiator) / (mass of low molecular weight (meth)acrylate compound)] is preferably 0.20 to 0.55. More preferably, it is 0.22 to 0.50, and even more preferably, it is 0.25 to 0.45. By setting such a ratio, oxygen polymerization inhibition can be suppressed and the microcell pattern can be faithfully reproduced. If this ratio is below the above range, the amount of photopolymerization initiator is too small and oxygen polymerization inhibition cannot be sufficiently suppressed, and as a result, the crosslinking reaction does not proceed, and the microcell pattern may not be faithfully reproduced on the printing plate. If it exceeds the above range, the amount of photopolymerization initiator is too large relative to the (meth)acrylate, and the amount of (meth)acrylate that undergoes the crosslinking reaction may be insufficient, and in this case, oxygen polymerization inhibition may not be sufficiently reduced.

[0022] (c) Examples of photopolymerization initiators include benzophenones, benzoins, acetophenones, benzils, benzoin alkyl ethers, benzyl alkyl ketals, anthraquinones, and thioxanthones. Specific examples include benzophenone, chlorobenzophenone, benzoin, acetophenone, benzil, benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, benzoin isobutyl ether, benzil dimethyl ketal, benzil diethyl ketal, benzil diisopropyl ketal, anthraquinone, 2-ethylanthraquinone, 2-methylanthraquinone, 2-allylanthraquinone, 2-chloroanthraquinone, thioxanthone, and 2-chlorothioxanthone.

[0023] In the present invention, the content of the (c) photopolymerization initiator in the photosensitive resin composition is preferably 2 to 9 mass%, more preferably 2.5 to 7.5 mass%, and even more preferably 3 to 7 mass%. By blending the photopolymerization initiator in an amount larger than that used in the past, the influence of oxygen polymerization inhibition during exposure can be completely eliminated and the crosslinking reaction can be sufficiently promoted, and as a result, the microcell pattern imaged on the heat-sensitive mask layer can be faithfully reproduced on the printing plate.

[0024] Usually, when manufacturing a flexographic printing plate from a flexographic printing plate, four types of exposure are performed: back exposure, main exposure, post-exposure, and exposure with a germicidal lamp. Back exposure is performed by irradiating the entire surface of the plate from the support side with light to form a floor part on the printing plate. Main exposure is performed by irradiating the flexographic printing plate with light in an image-like manner through a mask to crosslink and harden the unsaturated compounds in the photosensitive resin layer in the irradiated parts to form the image. Post-exposure is performed by developing the plate after the main exposure to form the convex dots and solid parts, and irradiating the entire surface of the plate with light. This is to complement the crosslinking hardening in the main exposure and to crosslink and harden the sides of the convex dots. Exposure with a germicidal lamp is performed to remove the surface tackiness of the plate, but it also has a role of crosslinking and hardening the sides of the dots as well as the post-exposure. Usually, main exposure and post-exposure are performed using UVA, while exposure with a germicidal lamp is performed using UVC.

[0025] These four types of exposure are usually carried out in the atmosphere, so that polymerization inhibition occurs due to oxygen in the atmosphere. For this reason, in the past, the crosslinking reaction in the photosensitive resin layer did not proceed sufficiently, and the surface of the photosensitive resin layer was washed out in the development process, making it impossible to faithfully reproduce the microcell pattern on the printing plate surface. In contrast, in the present invention, by blending a larger amount of photopolymerization initiator than in the past, the influence of polymerization inhibition due to oxygen is suppressed, the crosslinking hardening reaction is allowed to proceed sufficiently, and the imaging image (microcell pattern) of the heat-sensitive mask layer can be faithfully reproduced on the printing plate.

[0026] If the content of the photopolymerization initiator is less than the above-mentioned preferred range, the crosslinking curing reaction during exposure is insufficient, and the faithful reproduction of the imaging image (microcell pattern) on the printing plate may be insufficient. On the other hand, if the content of the photopolymerization initiator exceeds the above-mentioned preferred range, the reproducibility of the independent points and the durability of the printing plate may be reduced.

[0027] Conventionally, it was thought that increasing the content of the photopolymerization initiator would cause problems such as the light absorption by the photopolymerization initiator after the reaction blocking the light in the thickness direction of the plate, reducing the reproducibility of independent points, for which crosslinking in the thickness direction is important, and reducing durability during printing. Therefore, conventionally, the content of the photopolymerization initiator in the photosensitive resin composition was usually only about 1% by mass at most in practical use. In contrast, in the present invention, the toughness of the plate can be increased by including a certain proportion of a high molecular weight (meth)acrylate compound in the photosensitive resin composition, and the above-mentioned conventional disadvantages (reduced reproducibility of independent points and reduced durability during printing) when a large amount of photopolymerization initiator is blended are overcome, and it is possible to enjoy the advantage of increasing the content of the photopolymerization initiator (faithful reproduction of the microcell pattern on the printing plate by eliminating the effect of oxygen polymerization inhibition).

[0028] The photosensitive resin composition forming the photosensitive resin layer (B) used in the flexographic printing original plate contains (a) a polymer obtained by polymerizing a conjugated diene, (b) an ethylenically unsaturated compound, and (c) a photopolymerization initiator, and further contains additives such as a plasticizer, a hydrophilic compound, an ultraviolet absorber, a surface tension adjuster, a thermal polymerization inhibitor, a dye, a pigment, a fragrance, or an antioxidant, as necessary.

[0029] The plasticizer imparts flexibility to the photosensitive resin layer (B), and examples of the plasticizer include liquid rubber, oil, polyester, and phosphoric acid compounds. Examples of the liquid rubber include liquid polybutadiene, liquid polyisoprene, and those to which hydroxyl groups or carboxyl groups have been added. Examples of the oil include paraffin, naphthene, and aroma. Examples of the polyester include adipic acid polyester. Examples of the phosphoric acid compounds include phosphoric acid esters. Among these, liquid polybutadiene and liquid polybutadiene to which hydroxyl groups or carboxyl groups have been added are preferred from the viewpoint of compatibility with the polymer obtained by polymerizing a conjugated diene. When developing with a water-based developer, liquid polybutadiene to which hydroxyl groups or carboxyl groups have been added is particularly preferred. The content of the plasticizer in the photosensitive resin composition is preferably 5 to 15% by mass.

[0030] The hydrophilic compound enhances the developability of the photosensitive resin layer (B) in an aqueous developer. Examples of the hydrophilic compound include acrylic polymers, urethane polymers, polyamide polymers, and polyester polymers having hydrophilic groups such as carboxylic acid, carboxylate, sulfonic acid, sulfonate, hydroxyl group, amino group, phosphoric acid group, ethylene oxide, and propylene oxide. Known surfactants can also be used. Among these, urethane polymers having carboxylate are preferred from the viewpoint of developability in an aqueous developer. The content of the hydrophilic compound in the photosensitive resin composition is preferably 1 to 15% by mass.

[0031] The surface tension adjuster adjusts the surface tension of the printing plate, and by adjusting the surface tension of the printing plate, it is possible to adjust the ink transferability and ink clogging on the printing plate. Examples of the surface tension adjuster include paraffin oil, long-chain alkyl compounds, surfactants, fatty acid amides, silicone oils, modified silicone oils, fluorine compounds, and modified fluorine compounds. The content of the surface tension adjuster in the photosensitive resin composition is preferably 0.1 to 2% by mass.

[0032] The ultraviolet absorber increases the exposure latitude of the photosensitive resin layer (B), and examples of the ultraviolet absorber include benzophenone-based, salicylate-based, benzotriazole-based, acrylonitrile-based, metal complex salt-based, hindered amine-based, anthraquinone-based, azo-based, coumarin-based, and furan-based compounds. Among these, benzotriazole-based compounds are preferred from the viewpoints of availability and exposure latitude. The content of the ultraviolet absorber in the photosensitive resin composition is preferably 0.005 to 0.1% by mass.

[0033] The oxygen barrier layer (C) used in the flexographic printing plate precursor of the present invention is provided between the photosensitive resin layer (B) and the heat-sensitive mask layer (D) to suppress oxygen polymerization inhibition during the main exposure, so that a sufficient curing reaction occurs. This oxygen barrier layer (C) can eliminate the influence of oxygen polymerization inhibition during the main exposure to some extent, but the oxygen barrier layer alone is insufficient. In the present invention, in addition to the oxygen barrier layer, a larger amount of (c) photopolymerization initiator is used than in the past, and as a result, a sufficient crosslinking reaction of the photosensitive resin is achieved, and the microcell pattern can be faithfully reproduced on the printing plate. Examples of the binder polymer in the barrier layer include polyvinyl alcohol, partially saponified vinyl acetate, alkyl cellulose, cellulose-based polymer, and polyamide. These polymers are not limited to the use of one type, and two or more types of polymers can be used in combination. Examples of binder polymers that are preferable in terms of oxygen barrier properties are polyvinyl alcohol, partially saponified vinyl acetate, and polyamide. By selecting a binder polymer whose oxygen barrier properties are in a preferred range, image reproducibility can be suitably controlled.

[0034] The thickness of the oxygen barrier layer (C) is preferably 0.2 μm to 3.0 μm, more preferably 0.2 μm to 1.5 μm. If the layer thickness is less than the above range, the oxygen barrier property is insufficient, and the relief plate surface may become rough. If the layer thickness exceeds the above range, poor reproduction of fine lines may occur.

[0035] The heat-sensitive mask layer (D) used in the flexographic printing plate can be that used in the printing plate, but is preferably composed of, for example, carbon black, which is a material that has the function of absorbing infrared laser and converting it to heat and the function of blocking ultraviolet light, its dispersion binder, and a binder polymer capable of forming a film. The dispersion binder and the binder polymer capable of forming a film can be used together. In addition, as optional components other than these, pigment dispersants, fillers, surfactants, coating aids, etc. can be contained within a range that does not impair the effects of the present invention.

[0036] The heat-sensitive mask layer (D) used in the flexographic printing plate precursor of the present invention is preferably water-developable. Specific examples of the heat-sensitive mask layer (D) include a heat-sensitive mask layer combining a polar group-containing polyamide and a butyral resin (Patent No. 4200510), a heat-sensitive mask layer containing a polymer having the same structure as the polymer in the photosensitive resin layer and an acrylic resin (Patent No. 5710961), and a heat-sensitive mask layer containing an anionic polymer and a polymer having an ester bond in the side chain and a saponification degree of 0% to 90% (Patent No. 5525074).

[0037] The method for producing the flexographic printing plate precursor of the present invention is not particularly limited, but it is generally produced as follows. First, the components of the heat-sensitive mask layer (D) other than the carbon black, such as the binder, are dissolved in a suitable solvent, and the carbon black is dispersed therein to prepare a dispersion. Next, such a dispersion is applied onto a support for the heat-sensitive mask layer (e.g., a polyethylene terephthalate film), and the solvent is evaporated. Then, the oxygen barrier layer (C) components are overcoated to prepare one of the laminates. Furthermore, separately from this, a photosensitive resin layer (B) is formed on the support (A) by coating, and the other laminate is prepared. The two laminates thus obtained are laminated under pressure and / or heat so that the photosensitive resin layer (B) is adjacent to the oxygen barrier layer (C). The support for the heat-sensitive mask layer functions as a protective film for the surface of the printing original plate after completion.

[0038] In the method of producing a flexographic printing plate from the flexographic printing plate produced as described above, if a protective film is present, the protective film is first peeled off from the flexographic printing plate. Then, the thermal mask layer (D) is image-wise imaged with an IR laser to form an image on the photosensitive resin layer (B). Examples of suitable IR lasers include ND / YAG lasers (1064 nm) or diode lasers (e.g., 830 nm). Laser systems suitable for computer-assisted platemaking technology are commercially available, and for example, CDI (Esco Graphics) can be used. This laser system includes a rotating cylindrical drum that holds the printing plate, an IR laser irradiation device, and a layout computer, and image information is transferred directly from the layout computer to the laser device.

[0039] After imaging the image information on the heat-sensitive mask layer (D), the flexographic printing plate master is irradiated with active light through an image-like mask (main exposure). This can be performed while the plate is attached to the laser cylinder, or the plate can be removed from the laser device and irradiated with a conventional flat irradiation unit. As the active light, ultraviolet light having an emission peak at a wavelength of 330 to 380 nm can be used. As the light source, LED, low pressure mercury lamp, high pressure mercury lamp, ultra-high pressure mercury lamp, metal halide lamp, xenon lamp, zirconium lamp, carbon arc lamp, ultraviolet fluorescent lamp, etc. can be used. Thereafter, the irradiated plate is developed, post-exposed, and further exposed with a germicidal lamp to obtain a flexographic printing plate. The development process can be performed with a conventional development unit.

[0040] When applying a microcell to a solid portion of a printing plate, a suitable microcell can be selected from the various microcells available on a CDI (Esko Graphics), for example, and then the microcell can be applied to an image on a computer, and the image can be used to image the thermal mask layer. EXAMPLES

[0041] The effects of the printing plate precursor of the present invention will be shown by the following examples, but the present invention is not limited thereto. Note that the parts in the examples mean parts by mass, and the numerical values ​​showing the composition ratios in the tables also mean parts by mass.

[0042] The evaluations in the examples were carried out by the following methods. (1) Reproducibility of microcells on the printing plate The surface of the solid portion of the printing plate made with Pattern 1 described below was magnified 500 times with a Keyence digital microscope (VHX5000) and judged according to the following criteria. The judgment was made based on the best reproduction of the MG45 microcell pattern with boost values ​​ranging from 50 to 170 in increments of 10. ⊚: Microcells are faithfully and clearly reproduced on the surface of the solid portion of the printing plate. ◯: Microcells are reproduced on the surface of the solid area of ​​the printing plate. △: Microcells are only partially reproduced on the surface of the solid area of ​​the printing plate. ×: Microcells are not reproduced on the surface of the solid portion of the printing plate.

[0043] (2) Ink application to solid areas For the flexographic printing plate made in Pattern 1, the ink application in the solid areas was evaluated using a flexographic printing machine FPR302 (manufactured by MCK Corporation) with a 900LPI anilox. UV ink (product name: FLEXOCURE CYAN (manufactured by Flint)) was used. Polypropylene film (product name: P4256, manufactured by Toyobo) was used as the substrate. The printing speed was 50m / min. The amount of pressing during printing was defined as zero at the point where the plate contacted the substrate, and 90μm from there. The ink coverage (ink uniformity) of printed matter of normal solid areas (without microcell application) and solid areas with various microcell applications was measured using a Keyence digital microscope (VHX5000) and expressed as a percentage. The coverage of the microcell pattern with the highest coverage among the various microcells was taken as the coverage when microcell was applied. The higher the ink coverage, the more evenly the ink is applied, meaning better ink application. The difference between the coverage when microcell was applied and the coverage of normal solid areas was calculated to determine the improvement in coverage due to the application of microcell.

[0044] (3) Reproducibility of independent points The reproducibility of the smallest independent point on a printing plate made with Pattern 2 described below was measured. If the smallest independent point was 50 μm or less, it was judged as ◎, if it was between 50 μm and 100 μm, it was judged as ○, if it was between 100 μm and 200 μm, it was judged as △, and if it was more than 200 μm, it was judged as ×. The smaller the reproduced smallest independent point, the better the reproducibility of the independent points.

[0045] (4) Durability of the printing plate The durability of the flexographic printing plate made in pattern 2 was evaluated using a flexographic printing machine FPR302 (manufactured by MCK Co., Ltd.) with an anilox of 900 LPI. UV ink (product name: FLEXOCURE CYAN (manufactured by Flint Co., Ltd.)) was used. Coated paper (product name: Pearl Coat, manufactured by Oji Paper Co., Ltd.) was used as the substrate. The printing speed was 50 m / min. The amount of pressing in the printing was set to zero at the point where the plate contacted the substrate, and 150 μm from there. 5,000 m of printing was performed using this printing method. The halftone dots of 16 μm in diameter on the plate after printing were observed under a microscope. The evaluation was made as follows: ◎ if there was no change before and after printing, ○ if there was slight wear only at the edge, △ if there was partial chipping or wear, and × if there was chipping or wear all over the plate.

[0046] Example 1 Preparation of photosensitive resin composition As a polymer obtained by polymerizing a conjugated diene, 86 parts by mass of butadiene latex (Nipol LX111NF, non-volatile content 55%, manufactured by Nippon Zeon Co., Ltd.) and 24 parts by mass of acrylonitrile-butadiene latex (Nipol SX1503, non-volatile content 42%, manufactured by Nippon Zeon Co., Ltd.) were used. As an ethylenically unsaturated compound, 15 parts by mass of polybutadiene-terminated acrylate having a number average molecular weight of 10,000 (BAC45, manufactured by Osaka Organic Chemical Industry Co., Ltd.) and 10 parts by mass of trimethylolpropane trimethacrylate having a number average molecular weight of 338 (Light Ester TMP, manufactured by Kyoeisha Chemical Co., Ltd.) were used. As a photopolymerization initiator, 3 parts by mass of benzyl dimethyl ketal were used. As other components, 20 parts by mass of a hydrophilic polymer (PFT-4, non-volatile content 25%, manufactured by Kyoeisha Chemical Co., Ltd.) and butadiene oligomer (manufactured by Nippon Soda Co., Ltd.) were used. B2000) 9.9 parts by mass, heat stabilizer (4-methoxyphenol) 0.1 parts by mass, and UV absorber (Tinuvin 326) 0.01 parts by mass were mixed in a container to prepare a dope. The dope was placed in a pressure kneader, and the solvent was removed under reduced pressure at 80°C to obtain a photosensitive resin composition.

[0047] Flexographic printing plate making Carbon black dispersion (Orient Chemical Industry Co., Ltd., AMBK-8), copolymerized polyamide (PA223, Toyobo Co., Ltd.), propylene glycol, and methanol were mixed in a mass ratio of 45 / 5 / 5 / 45 to obtain a heat-sensitive mask layer coating liquid. After performing a release treatment on both sides of a PET film (Toyobo Co., Ltd., E5000, thickness 100 μm), the heat-sensitive mask layer coating liquid was applied with a bar coater so that the thickness of the coating film after drying was 2 μm, and the film laminate (I) was obtained by drying at 120 ° C. for 5 minutes. The optical density was 2.3. The optical density was measured with a black and white transmission densitometer DM-520 (Dainippon Screen Mfg. Co., Ltd.). Polyvinyl acetate (KH20, Nippon Gosei Co., Ltd.) with a saponification degree of 80% and a plasticizer (glycerin) were mixed in a mass ratio of 70 / 30 to obtain an oxygen barrier layer coating liquid. The oxygen barrier layer coating liquid was applied to the film laminate (I) with a bar coater so that the thickness of the coating film after drying was 2.0 μm, and the film laminate (II) was obtained by drying at 120 ° C for 5 minutes. The above-mentioned photosensitive resin composition was placed on a PET film support (Toyobo Co., Ltd., E5000, thickness 125 μm) coated with a copolymer polyester adhesive, and the film laminate (II) was superimposed on it. The flexographic printing original plate consisting of the PET support, adhesive layer, photosensitive resin layer, oxygen barrier layer, heat-sensitive mask layer and cover film was obtained by laminating at 100 ° C using a heat press machine. The total thickness of the plate was 1.14 mm.

[0048] Making printing plates from flexographic printing masters The printing plates were made from the flexographic printing master plate in the following two patterns, changing the images to be formed. Pattern 1 The printing plate was exposed to light from the PET support side for 10 seconds. The cover film was then peeled off. This plate was wrapped around an Esko Graphics CDI4530 and imaged at a resolution of 4000 dpi. For the image, a test chart was used with a normal solid area (without microcells) and solid areas with MG45, MG34, MG25, WSI, and MC16 microcells applied. The test charts were arranged in 10 increments with boost values ​​between 50 and 170, and the images were used as the imaging images. The main exposure was performed with an LED built into the CDI4530 at an illuminance of 22 mW / cm. 2 The plate was then removed from the CDI and developed for 8 minutes in a developing machine manufactured by A&V Corporation (Stuck System, 1% laundry soap aqueous solution, 40°C), and water droplets on the plate surface were removed with a water stripping rod. It was then dried for 10 minutes in a dryer at 60°C. Next, post-exposure was carried out for 7 minutes, and finally, a germicidal lamp was irradiated for 5 minutes to obtain a flexographic printing plate. Back exposure and post-exposure were carried out using a Philips TL-K 40W / 10R lamp (peak wavelength 370 nm, illuminance at 350 nm is 10 mW / cm 2 ) and the germicidal lamp was a Panasonic germicidal lamp GL-40 (peak wavelength 250 nm, illuminance at 250 nm is 4.5 mW / cm 2 The resulting printing plate had a relief depth of 0.6 mm.

[0049] Pattern 2 The printing plate was exposed to light from the PET support side for 10 seconds. The cover film was then peeled off. This plate was wrapped around an Esko Graphics CDI4530, and ablation was performed at a resolution of 4000 dpi with a test image having 175 lpi halftone dots at 0.3% intervals between 0 and 10%, independent points at 50 μm intervals between 0 and 300 μm, and a halftone dot gradation part (fade-out part) that transitions to zero. After ablation, the plate was taken out and returned to a flat surface, and main exposure was performed for 7 minutes. Then, it was developed for 8 minutes with an A&V Co., Ltd. developing machine (Stuck System, 1% laundry soap aqueous solution, 40 ° C.), and water droplets on the plate surface were removed with a water-squeezing rod. Then, it was dried for 10 minutes in a 60 ° C. dryer. Then, post-exposure was performed for 7 minutes, and finally, it was irradiated with a germicidal lamp for 5 minutes to obtain a flexographic printing plate. Back exposure, main exposure, and post-exposure were performed using a Philips TL-K 40W / 10R lamp (peak wavelength 370 nm, illuminance at 350 nm is 10 mW / cm 2 ) and the germicidal lamp was a Panasonic germicidal lamp GL-40 (peak wavelength 250 nm, illuminance at 250 nm is 4.5 mW / cm 2 The resulting printing plate had a relief depth of 0.6 mm, and it was confirmed that halftone dots with a diameter of 16 μm were reproduced on the printing plate.

[0050] Examples 2 to 12, Comparative Examples 1 to 5 A flexographic printing plate master was prepared in the same manner as in Example 1, except that the blending ratio of each component in the photosensitive resin composition constituting the photosensitive resin layer was changed as shown in Tables 1 and 2, and a printing plate was obtained from the master. The back exposure time was adjusted so that the relief depth was 0.6 mm.

[0051] Comparative Example 6 A flexographic printing plate precursor was obtained in the same manner as in Example 1, except that no oxygen barrier layer was formed when preparing the flexographic printing plate precursor in Example 1. Thereafter, in preparing a printing plate from the flexographic printing plate precursor, Membrane 100 was laminated as an oxygen barrier layer on the heat-sensitive mask layer after imaging using a dedicated laminator. After the main exposure, Membrane 100 was removed, and then a flexographic printing plate was obtained in the same manner as in Example 1.

[0052] The evaluation results of Examples 1 to 12 and Comparative Examples 1 to 6 are shown in Tables 1 and 2.

[0053] [Table 1]

[0054] [Table 2]

[0055] The details of the ethylenically unsaturated compounds in the above table are as follows. Light Ester TMP: Trimethylolpropane trimethacrylate, number average molecular weight 338, manufactured by Kyoeisha Chemical Co., Ltd. Light Ester 1,6HX: 1,6 hexanediol dimethacrylate, number average molecular weight 254, manufactured by Kyoeisha Chemical Co., Ltd. Light Ester 19ND: 1,9 nonanediol dimethacrylate, number average molecular weight 298, manufactured by Kyoeisha Chemical Co., Ltd. BAC45: Polybutadiene terminated acrylate, number average molecular weight 10,000, manufactured by Osaka Organic Chemical Industry Co., Ltd. TE2000: Polybutadiene with terminal methacrylic groups, urethane bond type, number average molecular weight 3,000, manufactured by Nippon Soda Co., Ltd.

[0056] As can be seen from the evaluation results in the above table, in Examples 1 to 12 in which the amount of photopolymerization initiator, the amount of low molecular weight (meth)acrylate compound, and the blending ratio of the photopolymerization initiator to the low molecular weight (meth)acrylate compound are within the range of the present invention, the reproducibility of microcells on the printing plate and the ink adhesion of solid areas are excellent. Furthermore, by blending a high molecular weight (meth)acrylate compound, the reproducibility of independent points and the durability of the printing plate are not impaired even when a large amount of photopolymerization initiator is blended (Comparison of Examples 1 to 6, 9 to 11 with Examples 7, 8, and 12).

[0057] In contrast, in Comparative Example 1, the amount of photopolymerization initiator is small and is about the same as that of the conventional one, so that the reproducibility of microcells on the printing plate and the ink adhesion of solid parts are poor. In Comparative Example 2, the amount of photopolymerization initiator is small, so that even if the mixing ratio of the photopolymerization initiator and the low molecular weight (meth)acrylate compound is appropriate, the reproducibility of microcells on the printing plate and the ink adhesion of solid parts are poor. In Comparative Example 3, the amount of photopolymerization initiator is small, and the amount of low molecular weight (meth)acrylate compound is also small, so that the reproducibility of microcells on the printing plate and the ink adhesion of solid parts are poor. In Comparative Example 4, the amount of photopolymerization initiator is too large, so that the plate hardness of the solid parts becomes too high, so that the ink adhesion of the solid parts is poor, and the reproducibility of independent points and the durability of the printing plate are also poor. In Comparative Example 5, since no oxygen barrier layer is provided, even if the amount of photopolymerization initiator, the amount of low molecular weight (meth)acrylate compound, and the ratio of the photopolymerization initiator and the low molecular weight (meth)acrylate compound are appropriate, the reproducibility of microcells on the printing plate and the ink adhesion of solid areas are poor. In Comparative Example 6, since the oxygen barrier layer is not provided between the photosensitive resin layer and the heat-sensitive mask layer, but is laminated after imaging on the heat-sensitive mask layer, the reproducibility of microcells on the printing plate and the ink adhesion of solid areas are excellent, but a dedicated laminator is required to laminate the oxygen barrier layer, and the plate-making process is complicated. [Industrial Applicability]

[0058] The flexographic printing plate precursor of the present invention has an oxygen barrier layer between the photosensitive resin layer and the heat-sensitive mask layer, and the content of the photopolymerization initiator in the photosensitive resin composition is higher than that of the conventional one, so that the microcell pattern can be faithfully reproduced on the printing plate surface without being affected by oxygen polymerization inhibition during exposure, particularly during main exposure, without any special equipment or additional process, and the ink adhesion in the solid parts of the printing plate can be improved. Therefore, the flexographic printing plate precursor of the present invention is extremely useful in the industry.

Claims

1. A flexographic printing original plate comprising at least a support (A), a photosensitive resin layer (B), an oxygen barrier layer (C), and a heat-sensitive mask layer (D) laminated in this order, the photosensitive resin layer (B) being formed from a photosensitive resin composition comprising (a) a polymer obtained by polymerizing a conjugated diene, (b) an ethylenically unsaturated compound, and (c) a photopolymerization initiator, the (c) photopolymerization initiator being benzyl dimethyl ketal, the content of the (c) photopolymerization initiator in the photosensitive resin composition being 2.5 to 7 mass %, and the (b) ethylenically unsaturated compound being a number average The photosensitive resin composition contains a (meth)acrylate compound (i) having a number average molecular weight of 100 or more and 600 or less, the content of the (meth)acrylate compound (i) having a number average molecular weight of 100 or more and 600 or less in the photosensitive resin composition is 5 to 16 mass %, the ratio of the mass of the (c) photopolymerization initiator to the mass of the (meth)acrylate compound (i) having a number average molecular weight of 100 or more and 600 or less in the photosensitive resin composition is in the range of 0.20 to 0.55, and the (b) ethylenically unsaturated compound is a (meth)acrylate compound having a number average molecular weight of more than 600 and 20,000 or less. (ii), in which the content of the (meth)acrylate compound (ii) having a number average molecular weight of more than 600 and not more than 20,000 in the photosensitive resin composition is 5 to 25 mass %, and the (meth)acrylate compound (i) having a number average molecular weight of 100 to 600 is selected from the group consisting of hexanediol di(meth)acrylate, 2-butyl-2-ethylpropane di(meth)acrylate, neopentyl glycol di(meth)acrylate, hydroxypivalic acid neopentyl glycol di(meth)acrylate, ECH-modified fluorine-containing ...

1. A flexographic printing original plate comprising a tertiary acrylate selected from the group consisting of tetraethylhexyl acrylate, ...

2. 2. The flexographic printing plate precursor according to claim 1, wherein the development is carried out using a water-based developer.

3. A flexographic printing plate obtained by exposing and developing the flexographic printing plate precursor according to claim 1, characterized in that microcells are applied to solid areas formed on the printing plate.

Citation Information

Patent Citations

  • Preparation of phthalic anhydride

    JP1980073675A

  • Axial thrust balancer device

    JP1983072693A

  • Transmission system for fault message

    JP1987019954A

  • Flexographic printing plate

    JP4332865B1

  • Relief printing original plate for rotary letterpress printing

    WO2017169572A1