Manufacturing method of electrolytic capacitor

The electrolytic capacitor design with distinct conductive polymer layers addresses the issue of increased ESR and short circuits by managing conductivity and resistance through differential boiling point dopants, maintaining stability under overvoltages.

JP7554696B2Active Publication Date: 2024-09-20NICHICON CORP
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2021045129
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-03-18
Publication Date
2024-09-20
Estimated Expiration
2041-03-18

AI Technical Summary

Technical Problem

Electrolytic capacitors coated with polyimide silicon to prevent short circuits experience increased equivalent series resistance (ESR) when subjected to overvoltages.

Method used

The electrolytic capacitor design includes a first conductive polymer layer with a larger contact area and a lower boiling point dopant, and a second conductive polymer layer with a smaller contact area and a higher boiling point dopant, to manage conductivity and resistance during overvoltages.

Benefits of technology

This configuration suppresses short circuits and maintains low ESR, ensuring stable performance under overvoltage conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007554696000004
    Figure 0007554696000004
  • Figure 0007554696000003
    Figure 0007554696000003
  • Figure 0007554696000001
    Figure 0007554696000001
Patent Text Reader

Abstract

To suppress the occurrence of a short circuit and suppress an increase in ESR when an overvoltage or the like is applied to an electrolytic capacitor.SOLUTION: A capacitor element 5 of an electrolytic capacitor includes a positive electrode 11 having a dielectric oxide film, a negative electrode 12, a separator 13, and a first conductive polymer layer and a second conductive polymer layer formed between the dielectric oxide film and the separator 13. In the dielectric oxide film, the contact area with the first conductive polymer layer is larger than the contact area with the second conductive polymer layer. The polymer contained in the first conductive polymer layer and the polymer contained in the second conductive polymer layer are the same. The boiling point of the first dopant contained in the first conductive polymer layer is lower than the boiling point of the second dopant contained in the second conductive polymer layer.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an electrolytic capacitor and a method for manufacturing the same. [Background technology]

[0002] A known electrolytic capacitor includes a capacitor element having an anode with a dielectric oxide film, a cathode, and a separator disposed between the anode and the cathode, an outer case in which the capacitor element is housed, and a sealing body (sealing means) that seals an opening of the outer case (see Patent Document 1).

[0003] In Patent Document 1, at least the round bar portion of the electrode extraction means connected to the anode for penetrating the sealing body and the welded portion are coated with polyimide silicone in advance, and then a solid electrolyte layer is formed between both electrodes of the capacitor element, which prevents a short circuit from occurring when the solid electrolyte adheres to the welded portion. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2004-296931 A Summary of the Invention [Problem to be solved by the invention]

[0005] The electrolytic capacitors mentioned above are coated with an insulating material, polyimide silicone, before the solid electrolyte layer is formed. This helps prevent short circuits when an overvoltage is applied, but the insulator acts as a resistor, increasing the equivalent series resistance (ESR) of the electrolytic capacitor.

[0006] An object of the present invention is to provide an electrolytic capacitor that can suppress the occurrence of a short circuit and an increase in ESR when an overvoltage or the like is applied to the electrolytic capacitor, and a manufacturing method thereof. [Means for solving the problem]

[0007] The electrolytic capacitor of the present invention is an electrolytic capacitor including a capacitor element having an anode with a dielectric oxide film, a cathode, and a separator arranged between the anode and the cathode, and an exterior body in which the capacitor element is housed, the capacitor element having a first conductive polymer layer and a second conductive polymer layer formed between the dielectric oxide film and the separator, the contact area of ​​the first conductive polymer layer with the dielectric oxide film being larger than the contact area of ​​the second conductive polymer layer with the dielectric oxide film, the first conductive polymer layer including a polymer and a first dopant, the second conductive polymer layer including the same polymer as the polymer contained in the first conductive polymer layer and a second dopant, and the boiling point of the first dopant being lower than the boiling point of the second dopant.

[0008] From the findings of the present inventors, the following has been found. According to the above configuration, the boiling point of the first dopant contained in the first conductive polymer layer, which has a large contact area with the dielectric oxide film, is lower than the boiling point of the second dopant contained in the second conductive polymer layer. When an overvoltage or the like is applied to the electrolytic capacitor, the first dopant contained in the first conductive polymer layer decomposes faster than the second dopant. As a result, the first conductive polymer layer, which has a large contact area with the dielectric oxide film, loses conductivity faster than the second conductive polymer layer and becomes insulated. As a result, it was found that the occurrence of short circuits is suppressed. On the other hand, the second conductive polymer layer, which has a smaller contact area with the dielectric oxide film, is less likely to become insulated than the first conductive polymer layer. Therefore, the second conductive polymer layer is less likely to become a resistor. This means that the ESR of the electrolytic capacitor is less likely to increase even when an overvoltage is applied. As described above, according to the present invention, it is possible to provide an electrolytic capacitor that can suppress the occurrence of a short circuit when an overvoltage or the like is applied, and that can suppress an increase in ESR.

[0009] In the above configuration, it is preferable that the weight of the polymer in the second conductive polymer layer is greater than the weight of the polymer in the first conductive polymer layer.

[0010] According to the above configuration, the weight of the polymer in the second conductive polymer layer, which is less likely to become insulating, is greater than the weight of the polymer in the first conductive polymer layer, which is more likely to become insulating. This indicates that the second conductive polymer layer contains a relatively large amount of polymer that is less likely to become resistor. Therefore, even if an overvoltage is applied, the ESR of the electrolytic capacitor is less likely to increase.

[0011] A method for producing an electrolytic capacitor of the present invention includes a first step of winding an anode having a dielectric oxide film and a cathode with a separator interposed therebetween to form a capacitor element; a second step of forming a first conductive polymer layer at least between the dielectric oxide film and the separator of the capacitor element; a third step of forming a second conductive polymer layer on the capacitor element with the first conductive polymer layer formed thereon; and a fourth step of housing the capacitor element with the second conductive polymer layer formed thereon in an outer casing, wherein the second step is to immerse the capacitor element in a first liquid containing at least a first monomer and a first dopant, pull it out, and then form a first conductive polymer layer by heat treatment, and the third step is to immerse the capacitor element with the first conductive polymer layer formed thereon in a second liquid containing at least a second monomer that is the same as the first monomer and a second dopant, pull it out, and then form a second conductive polymer layer by heat treatment, and the boiling point of the first dopant is lower than the boiling point of the second dopant.

[0012] According to the above configuration, the first conductive polymer layer formed first has a larger contact area with the dielectric oxide film than the second conductive polymer layer formed later. The boiling point of the first dopant contained in the first conductive polymer layer, which has a larger contact area with the dielectric oxide film, is lower than the boiling point of the second dopant contained in the second conductive polymer layer. Therefore, when an overvoltage or the like is applied to the electrolytic capacitor, the first dopant contained in the first conductive polymer layer decomposes faster than the second dopant. As a result, the first conductive polymer layer, which has a larger contact area with the dielectric oxide film, loses conductivity and becomes insulated faster than the second conductive polymer layer. As a result, it was found that the occurrence of a short circuit is suppressed. On the other hand, in the dielectric oxide film, the second conductive polymer layer, which has a smaller contact area, is less likely to become insulated than the first conductive polymer layer. Therefore, the second conductive polymer layer is less likely to become a resistor. As a result, it was found that the ESR of the electrolytic capacitor is less likely to increase even when an overvoltage is applied. As described above, according to the present invention, it is possible to provide an electrolytic capacitor that can suppress the occurrence of a short circuit when an overvoltage or the like is applied, and that can suppress an increase in ESR.

[0013] In the above configuration, it is preferable that a concentration of the second monomer in the second liquid is higher than a concentration of the first monomer in the first liquid.

[0014] According to the above configuration, the weight of the polymer in the second conductive polymer layer formed by the second liquid is greater than the weight of the polymer in the first conductive polymer layer formed by the first liquid. This results in a relatively large amount of polymer in the second conductive polymer layer that is less likely to become a resistor. Therefore, even if an overvoltage is applied, the ESR of the electrolytic capacitor is less likely to increase.

[0015] In the above configuration, it is preferable that the second liquid further contains iron ions, and a molar ratio of the second dopant to the iron ions contained in the second liquid is equal to or greater than 2.6 and equal to or less than 3.0.

[0016] With the above-described configuration, it is possible to provide an electrolytic capacitor that has a low initial ESR before an overvoltage or the like is applied.

[0017] In the above configuration, it is preferable that the first liquid further contains iron ions, and a molar ratio of the first dopant to the iron ions contained in the first liquid is equal to or greater than 2.6 and equal to or less than 3.4.

[0018] With the above configuration, it is possible to provide an electrolytic capacitor having high capacitance and low leakage current. Effect of the Invention

[0019] According to the present invention, it is possible to provide an electrolytic capacitor that can suppress the occurrence of a short circuit when an overvoltage or the like is applied to the electrolytic capacitor, and also suppresses an increase in ESR. [Brief description of the drawings]

[0020] [Figure 1] 1 is a cutaway front view of a main portion of an electrolytic capacitor according to an embodiment of the present invention; [Diagram 2] FIG. 2 is an exploded perspective view of the capacitor element shown in FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0021] Hereinafter, preferred embodiments of the present invention will be described with reference to the drawings.

[0022] As shown in FIG. 1, electrolytic capacitor 1 includes exterior body 4 having exterior case 2 and sealing body 3 that seals the opening of exterior case 2, and capacitor element 5 housed in exterior body 4.

[0023] As shown in FIG. 2, capacitor element 5 is formed by winding anode 11 and cathode 12 with separator 13 interposed therebetween into a cylindrical shape, and is secured in place by tape 14 attached to the outer circumferential surface.

[0024] Lead tabs (not shown) are connected to the anode 11 and the cathode 12, respectively. The anode 11 is connected to a lead terminal 21 via a lead tab. The cathode 12 is connected to a lead terminal 22 via a lead tab. The lead terminals 21 and 22 are led out to the outside through holes 31 and 32, respectively, formed in the sealing body 3, as shown in FIG. 1.

[0025] The anode 11 shown in Fig. 2 is a valve metal having a dielectric oxide film formed on its surface. The valve metal may be at least one selected from the group consisting of aluminum, tantalum, niobium, and titanium. The dielectric oxide film is formed, for example, by roughening the surface of a foil of the valve metal by etching, and then subjecting it to a chemical conversion treatment.

[0026] The cathode 12 is formed using a valve metal. For example, a valve metal foil whose surface is roughened by etching, or a foil whose surface is roughened and then chemically treated, is used as the cathode 12. A plain foil that is not etched may be used as the cathode 12. Furthermore, a coating foil in which a metal thin film containing at least one metal selected from the group consisting of titanium, nickel, titanium carbide, nickel carbide, titanium nitride, nickel nitride, titanium carbonitride, and nickel carbonitride is formed on the surface of the roughened foil or plain foil may be used. A coating foil in which a carbon thin film is formed on the surface of the roughened foil or plain foil may be used.

[0027] There is no particular limitation on the material of the separator 13. For example, a material mainly made of cellulose may be used as the separator 13.

[0028] Capacitor element 5 has a first conductive polymer layer and a second conductive polymer layer between at least the dielectric oxide film of anode 11 and separator 13. The contact area between the first conductive polymer layer and the dielectric oxide film is larger than the contact area between the second conductive polymer layer and the dielectric oxide film. The contact area between the second conductive polymer layer and the dielectric oxide film is preferably 50% or more of the contact area between the first conductive polymer layer and the dielectric oxide film. The first conductive polymer layer and the second conductive polymer layer may be formed in a portion other than between the dielectric oxide film of anode 11 and separator 13.

[0029] The form in which the first conductive polymer layer and the second conductive polymer layer are present is not particularly limited as long as the contact area of ​​the first conductive polymer layer with respect to the dielectric oxide film is larger than the contact area of ​​the second conductive polymer layer. For example, the first conductive polymer layer may be formed on the dielectric oxide film, and the second conductive polymer layer may be formed on the first conductive polymer layer. The first conductive polymer layer and the second conductive polymer layer may be present on the dielectric oxide film. The second conductive polymer layer may be present in the gap of the first conductive polymer layer. The "layer" here may be flat or not flat.

[0030] The first conductive polymer layer includes a polymer and a first dopant. The polymer is not limited to a specific one. Examples of the molecule include polyethylenedioxythiophene (PEDOT), polythiophene, polypyrrole, polyaniline, or derivatives thereof. The first dopant is not limited to a specific one. Examples of the first dopant include p-toluenesulfonic acid, polystyrenesulfonic acid (PSS), ethanesulfonic acid, and benzenesulfonic acid.

[0031] The first conductive polymer layer may further contain an oxidizing agent containing iron. Examples of the oxidizing agent containing iron include ferric p-toluenesulfonate and ferric benzenesulfonate. The oxidizing agent is used, for example, to chemically oxidize and polymerize the monomer when forming the first conductive polymer layer. The first conductive polymer layer may contain an oxidizing agent containing iron and a dopant separately, or may contain a compound of iron and an acid of the dopant. The compound of iron and an acid of the dopant functions as both an oxidizing agent and a dopant.

[0032] The second conductive polymer layer includes a polymer and a second dopant. The polymer included in the second conductive polymer layer is the same polymer as the polymer included in the first conductive polymer layer. Here, the "same polymer as the polymer included in the first conductive polymer layer" is a polymer obtained by polymerizing the same monomer as the monomer of the polymer included in the first conductive polymer layer. If the monomers are the same, that is, if the "monomer of the polymer included in the first conductive polymer layer" and the "monomer of the polymer included in the second conductive polymer layer" are the same, even if the "degree of polymerization of the polymer included in the first conductive polymer layer" and the "degree of polymerization of the polymer included in the second conductive polymer layer" are the same or different, the "polymer included in the first conductive polymer layer" and the "polymer included in the second conductive polymer layer" are the same.

[0033] The second dopant is not limited to a specific one, and examples of the second dopant include p-toluenesulfonic acid, polystyrenesulfonic acid (PSS), and benzenesulfonic acid.

[0034] The second conductive polymer layer may further contain an oxidizing agent containing iron. Examples of the oxidizing agent containing iron include ferric p-toluenesulfonate and ferric 1-naphthalenesulfonate. The oxidizing agent is used, for example, to chemically oxidize and polymerize the monomer when forming the second conductive polymer layer. The second conductive polymer layer may contain an oxidizing agent containing iron and a dopant separately, or may contain a compound of iron and an acid of the dopant. The compound of iron and an acid of the dopant functions as both an oxidizing agent and a dopant.

[0035] When both the first conductive polymer layer and the second conductive polymer layer contain an oxidant containing iron, the oxidant contained in the first conductive polymer layer (the oxidant containing iron) and the oxidant contained in the second conductive polymer layer may be the same as or different from each other.

[0036] The boiling point of the first dopant contained in the first conductive polymer layer is lower than the boiling point of the second dopant contained in the second conductive polymer layer, i.e., the thermal stability of the first dopant is lower than the thermal stability of the second dopant.

[0037] The boiling point of the first dopant is not particularly limited. The boiling point of the second dopant is not particularly limited. The boiling point of the first dopant is, for example, preferably 200°C or less, more preferably 150°C or less. The boiling point of the second dopant is, for example, preferably 140°C or more, more preferably 300°C or more. The difference between the boiling points of the first dopant and the second dopant is, for example, preferably 2°C or more, more preferably 15°C or more, and more preferably 150°C or more.

[0038] The weight of the polymer in the second conductive polymer layer is greater than the weight of the polymer in the first conductive polymer layer. For example, the second monomer concentration of the second liquid in which the capacitor element is immersed to form the second conductive polymer layer is made higher than the first monomer concentration of the first liquid in which the capacitor element is immersed to form the first conductive polymer layer, so that the weight of the polymer in the second conductive polymer layer can be made greater than the weight of the polymer in the first conductive polymer layer. In addition, when the first monomer concentration and the second monomer concentration are equal to or less than the same concentration, the amount of the polymer in the first conductive polymer layer can be made greater by repeating the process of immersing in the second liquid, removing the liquid, and performing heat treatment multiple times. On the other hand, since the productivity is reduced by repeating the process of immersion and heat treatment, the second monomer concentration is preferably at least twice the first monomer concentration, and more preferably at least three times the first monomer concentration.

[0039] The above-described electrolytic capacitor 1 is produced, for example, by the following method. Here, a method of chemically oxidizing and polymerizing a monomer when forming the first conductive polymer layer and the second conductive polymer layer will be described.

[0040] Lead tabs for external extraction electrodes are connected to anode 11 and cathode 12 (see FIG. 2) that have been cut to a specified width. Anode 11 and cathode 12 with the lead tabs connected are wound with separator 13 interposed therebetween to produce a main body that becomes capacitor element 5 (first step). Anode 11 is a valve metal on which a dielectric oxide film is formed.

[0041] The body is subjected to a chemical conversion treatment in order to repair the cut edge of the body that will become the capacitor element 5 and the dielectric oxide film that was lost during the preparation of the body. The chemical conversion treatment is performed by applying a voltage to the body in a chemical conversion liquid. The chemical conversion liquid used for the chemical conversion treatment can be, for example, an aqueous solution containing at least one of adipic acid and an adipate.

[0042] Next, to form a first conductive polymer layer, the main body is immersed in a first liquid containing a first monomer, a first dopant, and an oxidizing agent containing iron, and then heat-treated. The first dopant and the oxidizing agent containing iron may be different from each other, or may be the first dopant and oxidizing agent. The first monomer is polymerized to form a first conductive polymer layer at least between the dielectric oxide film and the separator 13 (second step). After the heat treatment, the main body may be dried as necessary.

[0043] Next, in order to form a second conductive polymer layer, the main body part on which the first conductive polymer layer has been formed is immersed in a second liquid containing a second monomer, a second dopant, and an oxidizing agent containing iron, and then heat-treated. The second monomer is the same monomer as the first monomer contained in the first liquid used when forming the first conductive polymer layer. The concentration of the second monomer contained in the second liquid is higher than the concentration of the first monomer contained in the first liquid. For example, the concentration of the first monomer contained in the first liquid is set to 10 wt% or more and 30 wt% or less, and the concentration of the second monomer contained in the second liquid is set to 30 wt% or more and 70 wt% or less. The concentration of the second monomer contained in the second liquid is preferably at least twice, more preferably at least three times, the concentration of the first monomer contained in the first liquid. The second monomer is polymerized to form a second conductive polymer layer (third step). After the heat treatment, the main body part may be dried as necessary. As a result, a capacitor element 5 is obtained. The capacitor element 5 is housed in a metal case (fourth step) to obtain an electrolytic capacitor 1.

[0044] By the above method, a first conductive polymer layer and a second conductive polymer layer are formed at least between the dielectric oxide film of the anode 11 and the separator. By forming the first conductive polymer layer first, the first conductive polymer layer is formed on most of the dielectric oxide film. Therefore, the contact area between the first conductive polymer layer formed first and the dielectric oxide film is larger than the contact area between the second conductive polymer layer formed later and the dielectric oxide film.

[0045] In the above-described method, the concentration of the second monomer contained in the second liquid is higher than the concentration of the first monomer contained in the first liquid, and therefore, in the obtained electrolytic capacitor, the weight of the polymer in the second conductive polymer layer is higher than the weight of the polymer in the first conductive polymer layer.

[0046] From the findings of the present inventors, it has been found that the electrolytic capacitor 1 according to this embodiment provides the following effects. In the dielectric oxide film, the boiling point of the first dopant contained in the first conductive polymer layer, which has a large contact area, is lower than the boiling point of the second dopant contained in the second conductive polymer layer. When an overvoltage or the like is applied to the electrolytic capacitor 1, the first dopant contained in the first conductive polymer layer decomposes faster than the second dopant. As a result, the first conductive polymer layer, which has a large contact area with the dielectric oxide film, loses conductivity and becomes insulated faster than the second conductive polymer layer. This suppresses the occurrence of short circuits. On the other hand, the second conductive polymer layer, which has a smaller contact area with the dielectric oxide film, is less likely to become an insulator than the first conductive polymer layer. Therefore, the second conductive polymer layer is less likely to become a resistor. As a result, it was found that the ESR of electrolytic capacitor 1 is less likely to increase even when an overvoltage is applied. According to the electrolytic capacitor 1, when an overvoltage or the like is applied, the occurrence of a short circuit can be suppressed, and an increase in ESR can also be suppressed.

[0047] In addition, the weight of the polymer in the second conductive polymer layer, which is less likely to become insulating, is greater than the weight of the polymer in the first conductive polymer layer. This means that there is more polymer in the second conductive polymer layer, which is less likely to become resistor. Therefore, even if an overvoltage is applied, the ESR of the electrolytic capacitor is less likely to increase.

[0048] In the above, in the manufacturing process of the electrolytic capacitor, the concentration of the second monomer contained in the second liquid is set higher than the concentration of the first monomer contained in the first liquid. As a result, the weight of the polymer in the second conductive polymer layer is greater than the weight of the polymer in the first conductive polymer layer. However, the concentration of the first monomer contained in the first liquid and the concentration of the second monomer contained in the second liquid may be the same, or the concentration of the first monomer contained in the first liquid may be greater than the concentration of the second monomer contained in the second liquid. In this case, for example, the main body of the capacitor element on which the first conductive polymer layer is formed is immersed in the second liquid containing the second monomer, and then pulled up and heat-treated. This process is repeated several times, so that the weight of the polymer in the second conductive polymer layer is greater than the weight of the polymer in the first conductive polymer layer in the obtained electrolytic capacitor.

[0049] In the manufacturing process of the electrolytic capacitor, when the second liquid contains iron ions, the molar ratio of the second dopant to the iron ions contained in the second liquid is preferably 2.6 to 3.0. In the second conductive polymer layer contains an oxidizing agent containing iron, the molar ratio of iron contained in the oxidizing agent to the second dopant in the second conductive polymer layer is preferably 1:2.6 to 3.0. In this case, the initial ESR of the electrolytic capacitor 1 (ESR before application of an overvoltage or the like) tends to be relatively low.

[0050] In the manufacturing process of the electrolytic capacitor, when the first liquid contains iron ions, the molar ratio of the first dopant to the iron ions contained in the first liquid is preferably 2.6 to 3.4. When the first conductive polymer layer contains an oxidizing agent containing iron, the molar ratio of iron contained in the oxidizing agent to the first dopant in the first conductive polymer layer is preferably 1:2.6 to 3.4. In this case, an electrolytic capacitor with high capacitance and low leakage current can be provided. EXAMPLES

[0051] The present invention will now be described more specifically with reference to examples.

[0052] An electrolytic capacitor was produced by the following method.

[0053] Aluminum lead tabs for external extraction electrodes were connected to the anode and cathode foils cut to a specified width. The anode aluminum foil was made by roughening the surface of the aluminum foil, which is a valve metal, by etching, and then forming a dielectric oxide film by chemical conversion treatment at 60 V. The cathode foil was aluminum foil carrying carbon. The anode aluminum foil and cathode aluminum foil were wound with cellulose-based electrolytic paper (separator) in between to create the main body that would become the capacitor element.

[0054] A chemical conversion treatment was performed to repair the dielectric oxide film that was lost on the cut edge of the anode foil and the attachment part of the lead tab. The chemical conversion treatment was performed by immersing the main body, which will become the capacitor element, in a chemical conversion solution and applying a voltage that is close to the chemical conversion voltage value of the dielectric oxide film. The chemical conversion solution used was an aqueous solution of ammonium adipate with an ammonium adipate concentration of 2 wt%.

[0055] Next, under the following conditions ([Conditions for preparing the first conductive polymer layer and the second conductive polymer layer] described below), the main body portion to become the capacitor element was immersed for 30 minutes in a first liquid prepared by mixing ethylenedioxythiophene (EDOT), the first dopant, 30 wt% of an iron salt of the first dopant (dopant and oxidizer), and ethanol, and then the main body portion was removed from the first liquid and heat-treated at 40°C for 1 hour to form a first conductive polymer layer.

[0056] Next, the main body that will become the capacitor element was immersed for 30 minutes in a second liquid that was a mixture of ethylenedioxythiophene (EDOT), a second dopant, an iron salt of the second dopant (dopant and oxidizer) of 30 wt%, and ethanol under the following conditions, and then the main body was removed from the second liquid and heat-treated at 40°C for 1 hour, and then heat-treated at 220°C for 15 minutes. The main body that will become the capacitor element was then immersed in ethylene glycol for 5 minutes to remove excess iron and dopant, and then dried at 160°C for 30 minutes. This formed a second conductive polymer layer.

[0057] The lead wires of the obtained capacitor element were inserted into the hole of the sealing body, and the capacitor element and the sealing body were housed in an aluminum case, after which the periphery of the opening of the case was curled. In a thermostatic chamber set at 150°C, the rated voltage (25V) was applied to the capacitor element housed in the case, and an aging treatment was performed to produce an electrolytic capacitor. The electrolytic capacitor produced in this experiment has a rated voltage of 25WV, a rated capacitance of 150μF, and a product size of φ8×10L (mm).

[0058] [Conditions for preparing the first conductive polymer layer and the second conductive polymer layer] <Previous conditions> Monomer (EDOT) concentration 30wt% / dopant p-toluenesulfonic acid (iron:dopant molar ratio = 1:2.8) Under conventional conditions, only one conductive polymer layer was produced. <Example 1> First conductive polymer layer: Monomer (EDOT) concentration 10 wt% / dopant p-toluenesulfonic acid (iron:dopant molar ratio = 1:2.8) Second conductive polymer layer: Monomer (EDOT) concentration 30 wt% / dopant 1-naphthalenesulfonic acid (iron:dopant molar ratio = 1:2.6) <Example 2> First conductive polymer layer: Monomer (EDOT) concentration 10 wt% / dopant ethanesulfonic acid (iron:dopant molar ratio = 1:2.6) Second conductive polymer layer: Monomer (EDOT) concentration 30 wt% / dopant p-toluenesulfonic acid (iron:dopant molar ratio = 1:2.8) <Example 3> First conductive polymer layer: Monomer (EDOT) concentration 10 wt% / dopant ethanesulfonic acid (iron:dopant molar ratio = 1:3.2) Second conductive polymer layer: Monomer (EDOT) concentration 30 wt% / dopant p-toluenesulfonic acid (iron:dopant molar ratio = 1:2.8) <Example 4> First conductive polymer layer: Monomer (EDOT) concentration 10 wt% / dopant benzenesulfonic acid (iron:dopant molar ratio = 1:2.6) Second conductive polymer layer: Monomer (EDOT) concentration 30 wt% / dopant 1-naphthalenesulfonic acid (iron:dopant molar ratio = 1:3.0) <Comparative Example 1> First conductive polymer layer: Monomer (EDOT) concentration 10 wt% / dopant benzenesulfonic acid (iron:dopant molar ratio = 1:2.6) Second conductive polymer layer: Monomer (EDOT) concentration 30 wt% / dopant benzenesulfonic acid (iron:dopant molar ratio = 1:2.6) <Comparative Example 2> First conductive polymer layer: Monomer (EDOT) concentration 10 wt% / dopant 1-naphthalenesulfonic acid (iron:dopant molar ratio = 1:2.8) Second conductive polymer layer: Monomer (EDOT) concentration 30 wt% / dopant benzenesulfonic acid (iron:dopant molar ratio = 1:2.8) <Comparative Example 3> First conductive polymer layer: Monomer (EDOT) concentration 10 wt% / dopant 1-naphthalenesulfonic acid (iron:dopant molar ratio = 1:2.8) Second conductive polymer layer: Monomer (EDOT) concentration 30 wt% / dopant p-toluenesulfonic acid (iron:dopant molar ratio = 1:2.8) <Example 5> First conductive polymer layer: Monomer (EDOT) concentration 10 wt% / dopant p-toluenesulfonic acid (iron:dopant molar ratio = 1:2.8) Second conductive polymer layer: Monomer (EDOT) concentration 30 wt% / dopant 1-naphthalenesulfonic acid (iron:dopant molar ratio = 1:3.2) <Example 6> First conductive polymer layer: Monomer (EDOT) concentration 10 wt% / dopant benzenesulfonic acid (iron:dopant molar ratio = 1:3.4) Second conductive polymer layer: Monomer (EDOT) concentration 30 wt% / dopant p-toluenesulfonic acid (iron:dopant molar ratio = 1:3.4) <Comparative Example 4> First conductive polymer layer: Monomer (EDOT) concentration 10 wt% / dopant benzenesulfonic acid (iron:dopant molar ratio = 1:3.0) Second conductive polymer layer: Monomer (EDOT) concentration 30 wt% / dopant benzenesulfonic acid (iron:dopant molar ratio = 1:3.0)

[0059] Table 1 shows the conditions for manufacturing the capacitor.

[0060] [Table 1]

[0061] (evaluation) As initial characteristics, the capacitance (Cap.), dissipation factor tangent (tan δ), equivalent series resistance (ESR), and leakage current (μA) of the capacitors were measured in an environment of 20°C. After applying 100V to each capacitor for 60 minutes (after overvoltage test), the capacitance (Cap.), dissipation factor tangent (tan δ), equivalent series resistance (ESR), and leakage current (μA) of the capacitors were measured. The evaluation results are shown in Table 2.

[0062] [Table 2]

[0063] Under conventional conditions, in which only one conductive polymer layer was formed, a short circuit occurred during the overvoltage test. A short circuit occurred during the overvoltage test also in Comparative Example 1 and Comparative Example 4. In Comparative Example 1 and Comparative Example 4, a first conductive polymer layer and a second conductive polymer layer are formed in the capacitor element, and the first conductive polymer layer and the second conductive polymer layer are formed under the same conditions (see Table 1).

[0064] As shown in Table 2, in Comparative Example 2 and Comparative Example 3, no short circuit occurred, but the ESR increased significantly after the overvoltage test. In Comparative Example 2 and Comparative Example 3, the boiling point of the second dopant contained in the second conductive polymer layer is lower than the boiling point of the first dopant contained in the first conductive polymer layer (see Table 1). It is believed that the second conductive polymer layer, which has a polymer that is relatively heavier than the polymer in the first conductive polymer layer, lost its conductivity and became insulated more quickly than the first conductive polymer layer, which is why the ESR increased significantly.

[0065] From the above experiment, the following was found. It has been found that when the boiling point of the first dopant contained in the first conductive polymer layer, which has a large contact area with the dielectric oxide film of the anode, is lower than the boiling point of the second dopant contained in the second conductive polymer layer, and the weight of the polymer in the second conductive polymer layer, which has a small contact area with the dielectric oxide film of the anode, is greater than the weight of the polymer in the first conductive polymer layer, it is possible to suppress the occurrence of a short circuit when an overvoltage is applied to the electrolytic capacitor, and also to suppress an increase in the ESR of the electrolytic capacitor.

[0066] Furthermore, in Examples 1 to 4, the initial ESR was low, as shown in Table 2. This indicates that when the molar ratio of iron contained in the oxidant:second dopant in the second conductive polymer layer is 1:2.6 to 3.0 (see Table 1), the initial ESR is low.

[0067] In the above experiment, in order to form the first conductive polymer layer and the second conductive polymer layer, a polyethylenedioxythiophene (PEDOT) polymer was obtained by polymerizing ethylenedioxythiophene (EDOT) as a monomer. However, the monomer and polymer for forming the first conductive polymer layer and the second conductive polymer layer are not limited to ethylenedioxythiophene (EDOT) and polyethylenedioxythiophene (PEDOT) used in the above experiment. Monomers and polymers other than those mentioned above may also be used. The same effect as above can be obtained by using other monomers and polymers.

[0068] The first dopant and oxidant contained in the first conductive polymer layer are not limited to the first dopant and oxidant used in the above experiment. The second dopant and oxidant contained in the second conductive polymer layer are not limited to the second dopant and oxidant used in the above experiment. The same effect as above can be obtained when other dopants and oxidants are used.

[0069] Although the embodiment of the present invention has been described above based on the examples, the specific configuration should not be considered to be limited to these embodiments. The scope of the present invention is indicated by the claims rather than the above description, and includes all modifications within the meaning and scope of the claims.

[0070] For example, in the above description, the first conductive polymer layer and the second conductive polymer layer are formed between the dielectric oxide film and the separator. However, the first conductive polymer layer and the second conductive polymer layer may be formed in a place other than between the dielectric oxide film and the separator. For example, they may be formed on the dielectric oxide film and / or the separator.

[0071] In the above, the first conductive polymer layer and the second conductive polymer layer are formed between the dielectric oxide film and the separator. However, in addition to the first conductive polymer layer and the second conductive polymer layer, another conductive polymer layer may be formed between the dielectric oxide film and the separator.

[0072] In the above experiment, electrolytic capacitors were produced with a rated voltage of 25 WV, a rated capacitance of 150 μF, and a product size of φ8×10L (mm), but the rated voltage, rated capacitance, and product size of the electrolytic capacitor of the present invention are not limited to those described above. [Explanation of symbols]

[0073] 1. Electrolytic capacitor 2 Outer case 3 Sealing body 4 Exterior body 5 Capacitor elements 11 Anode 12 Cathode 21, 22 Lead terminal

Claims

1. A first step of winding an anode having a dielectric oxide film and a cathode with a separator therebetween to form a capacitor element; a second step of forming a first conductive polymer layer between at least the dielectric oxide film and the separator of the capacitor element; a third step of forming a second conductive polymer layer on the capacitor element on which the first conductive polymer layer has been formed; and a fourth step of housing the capacitor element having the second conductive polymer layer formed thereon in an exterior body. the second step is to immerse the capacitor element in a first liquid containing at least a first monomer and a first dopant, and then to pull it out, and then to form a first conductive polymer layer by heat treatment; the third step is to immerse the capacitor element having the first conductive polymer layer formed in a second liquid containing at least a second monomer that is the same as the first monomer and a second dopant, and then to pull it out, and then to form a second conductive polymer layer by heat treatment; The method for manufacturing an electrolytic capacitor, wherein the boiling point of the first dopant is lower than the boiling point of the second dopant.

2. 2. The method for manufacturing an electrolytic capacitor according to claim 1, wherein a concentration of the second monomer in the second liquid is higher than a concentration of the first monomer in the first liquid.

3. the second liquid further contains iron ions; 2. The method for producing an electrolytic capacitor according to claim 1, wherein a molar ratio of the second dopant to the iron ions contained in the second liquid is 2.6 or more and 3.0 or less.

4. The first liquid further contains iron ions, 2. The method for producing an electrolytic capacitor according to claim 1, wherein a molar ratio of the first dopant to the iron ions contained in the first liquid is 2.6 or more and 3.4 or less.

Citation Information

Patent Citations

  • Solid electrolytic capacitor and its manufacturing method

    JP2004296931A

  • Method for manufacturing solid electrolytic capacitor

    JP2006135212A

  • Solid electrolytic capacitor

    JP2008166364A

  • Electrolytic capacitor and method for producing same

    WO2018235434A1