Composition for electrode mixture, electrode mixture, electrode, non-aqueous electrolyte secondary battery, and method for manufacturing electrode
By combining a vinylidene fluoride polymer with a polyisocyanate compound having blocked isocyanate groups, the adhesive strength between the current collector and electrode mixture layer is enhanced, addressing the issues of low adhesion and gelation in non-aqueous electrolyte secondary batteries.
Patent Information
- Application Number
- JP2021509251
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-03-22
- Filing Date
- 2020-03-18
- Publication Date
- 2024-09-20
- Estimated Expiration
- 2040-03-18
AI Technical Summary
Existing vinylidene fluoride polymers used in non-aqueous electrolyte secondary batteries exhibit low adhesive strength with metal foils and active materials, leading to issues such as gelation and reduced adhesion, particularly when high nickel content materials are used as positive electrode active materials.
Incorporating a vinylidene fluoride polymer with a polyisocyanate compound, where some isocyanate groups are blocked with a blocking agent, to enhance the adhesive strength between the current collector and the electrode mixture layer.
The proposed composition significantly increases the adhesive strength between the current collector and the electrode mixture layer, preventing gelation and ensuring robust bonding, thereby improving the stability and performance of the battery.
Smart Images

Figure 0007554735000002 
Figure 0007554735000001 
Figure 0007554735000006
Abstract
Description
[Technical field]
[0001] The present invention relates to a composition for an electrode mixture, an electrode mixture, and uses thereof. More specifically, the present invention relates to a composition for an electrode mixture, an electrode mixture, an electrode, a nonaqueous electrolyte secondary battery, and a method for producing an electrode. [Background technology]
[0002] In recent years, electronic technology has been developing remarkably, and small portable devices are becoming more and more sophisticated. Therefore, the power sources used in these devices are required to be smaller and lighter, i.e., have higher energy density. As batteries with high energy density, non-aqueous electrolyte secondary batteries, such as lithium ion secondary batteries, are widely used.
[0003] Furthermore, from the viewpoints of global environmental issues and energy conservation, nonaqueous electrolyte secondary batteries are also used in hybrid automobiles that combine secondary batteries with engines, and electric automobiles that use secondary batteries as their power source, and their applications are expanding.
[0004] An electrode for a non-aqueous electrolyte secondary battery has a structure having a current collector and an electrode mixture layer formed on the current collector. The electrode mixture layer is generally formed by applying an electrode mixture containing an electrode active material, a conductive assistant, and an electrode mixture composition (binder composition) in a slurry state dispersed in a suitable solvent or dispersion medium onto the current collector, and then volatilizing the solvent or dispersion medium. As the binder composition, a vinylidene fluoride polymer composition such as polyvinylidene fluoride (PVDF) is mainly used because it has excellent chemical resistance, weather resistance, and excellent electrochemical stability.
[0005] For example, Patent Document 1 describes an electrode binder for lithium ion secondary batteries that contains a vinylidene fluoride polymer dispersed in an organic diluent and a (meth)acrylic polymer dispersant.
[0006] However, vinylidene fluoride polymers sometimes have low adhesive strength to metal foils serving as battery current collectors and to active materials, and there is a demand for improving the adhesive strength.
[0007] Lithium cobalt oxide has been mainly used as a positive electrode active material (electrode active material), but in recent years, lithium nickel composite oxide and lithium iron phosphate have also been known as positive electrode active materials depending on the application. When using lithium nickel composite oxide as a positive electrode active material, if vinylidene fluoride polymer is used as a binder composition, the electrode mixture tends to thicken during storage. In some cases, gelation may occur, and there is a demand for improving the stability of the electrode mixture.
[0008] As a method for improving the adhesion of vinylidene fluoride polymers to metal foils, etc., there have been disclosed vinylidene fluoride-based copolymers obtained by copolymerizing vinylidene fluoride with a monoester of an unsaturated dibasic acid such as monomethyl maleate (see, for example, Patent Documents 2 and 3), and vinylidene fluoride-based copolymers obtained by copolymerizing vinylidene fluoride with an acrylic acid compound (see, for example, Patent Document 4).
[0009] As a method for preventing gelation of an electrode mixture, a copolymer containing vinylidene fluoride and chlorotrifluoroethylene (see, for example, Patent Document 5) has been disclosed. [Prior art documents] [Patent documents]
[0010] [Patent Document 1] Japanese Patent Publication No. 2017-510044 [Patent Document 2] Japanese Patent Publication No. 2001-19896 [Patent Document 3] Japanese Patent Publication No. 6-172452 [Patent Document 4] Japan Patent Publication No. 2010-525124 [Patent Document 5] Japanese Patent Publication No. JP11-195419A Summary of the Invention [Problem to be solved by the invention]
[0011] However, even the polymers described in Patent Documents 2 to 4 still do not have sufficient adhesiveness to metal foils, etc. In addition, as disclosed in Patent Document 5, when an electrode mixture is produced using a vinylidene fluoride polymer and a positive electrode active material, if a high-nickel positive electrode active material having a high nickel content is used as the positive electrode active material, gelation is suppressed, but there is a problem that the adhesiveness decreases.
[0012] The present invention has been made in consideration of the problems associated with the above-mentioned conventional techniques, and has an object to provide a binder composition which has superior adhesion to metal foils and the like compared to conventional vinylidene fluoride polymers. [Means for solving the problem]
[0013] The present inventors have conducted intensive research to solve the above-mentioned problems, and as a result have unexpectedly found that the adhesive strength between a current collector and an electrode mixture layer can be increased by using an electrode mixture containing a vinylidene fluoride polymer and a polyisocyanate compound, which led to the invention.
[0014] That is, an electrode mixture composition according to one embodiment of the present invention is a composition for an electrode mixture comprising a synthetic resin containing a vinylidene fluoride polymer in a proportion of 99% by mass or more, and a polyisocyanate compound in which at least a portion of the isocyanate groups are blocked with a blocking agent. Effect of the Invention
[0015] According to one aspect of the present invention, it is possible to provide a composition for an electrode mixture that can increase the adhesive strength between a current collector and an electrode mixture layer in a battery such as a lithium ion secondary battery. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] [Electrode mixture composition] The electrode mixture composition according to the present embodiment contains a synthetic resin and a polyisocyanate compound.
[0017] (Synthetic resin) The synthetic resin may contain vinylidene fluoride polymer at a ratio of 99% by mass or more, and in one embodiment, contains only vinylidene fluoride polymer. When the synthetic resin contains other polymers, there is no particular limitation as long as the desired effect of the electrode mixture composition of this embodiment is not impaired. In one embodiment, the synthetic resin may be a synthetic resin that does not contain a (meth)acrylic polymer as the other polymer. By containing vinylidene fluoride polymer at a ratio of 99% by mass or more, the adhesive strength between the current collector and the electrode mixture layer when the electrode mixture composition according to this embodiment is used can be increased. In addition, containing vinylidene fluoride polymer at a ratio of 99% by mass or more is also preferable from the viewpoint of electrochemical stability.
[0018] (Vinylidene fluoride polymer) In this specification, the term "vinylidene fluoride polymer" includes both a homopolymer of vinylidene fluoride and a copolymer of vinylidene fluoride and a monomer copolymerizable with vinylidene fluoride. The monomer copolymerizable with vinylidene fluoride can be appropriately selected from known monomers, for example. When vinylidene fluoride is copolymerized, it is preferable that the vinylidene fluoride unit is contained at 50 mol% or more, more preferably that the vinylidene fluoride unit is contained at 80 mol% or more, and particularly preferably that the vinylidene fluoride unit is contained at 90 mol% or more.
[0019] When the vinylidene fluoride polymer is a copolymer, it is preferably a vinylidene fluoride copolymer having vinylidene fluoride as a main constituent component and containing at least one structural unit selected from the structural units derived from an unsaturated dibasic acid, the structural units derived from an unsaturated dibasic acid monoester, the structural units derived from an alkyl vinyl halide compound, the structural units derived from a compound represented by the following formula (1), the structural units derived from a compound represented by the following formula (2), and the structural units derived from a compound represented by the following formula (3).
[0020] [ka]
[0021] Examples of the unsaturated dibasic acid according to this embodiment include fumaric acid, maleic acid, citraconic acid, and phthalic acid.
[0022] Examples of the unsaturated dibasic acid monoester according to this embodiment include monomethyl fumarate, monoethyl fumarate, monomethyl maleate, monoethyl maleate, monomethyl citraconate, monoethyl citraconate, monomethyl phthalate, and monoethyl phthalate.
[0023] In the compound represented by the above formula (1) according to this embodiment, 1 , R 2 , and R 3 each independently represents a hydrogen atom, a fluorine atom, a chlorine atom, or an alkyl group having 1 to 5 carbon atoms.
[0024] Examples of the alkyl group having 1 to 5 carbon atoms include a methyl group, an ethyl group, a propyl group, and an isopropyl group. 1 is preferably a hydrogen atom or a methyl group, more preferably a hydrogen atom. 2 is preferably a hydrogen atom or a methyl group, more preferably a hydrogen atom. 3is preferably a hydrogen atom, a fluorine atom, or a methyl group, and more preferably a hydrogen atom.
[0025] In formula (1), the main chain constituting X' has 1 to 19 atoms, preferably 1 to 14 atoms, and more preferably 1 to 9 atoms. Examples of atoms constituting such a main chain include carbon atoms and heteroatoms. When a heteroatom is contained, the heteroatom is preferably an oxygen atom. In this specification, the number of atoms in the main chain does not include the number of hydrogen atoms. The number of atoms in the main chain refers to the number of atoms of the carboxyl group written to the right of X' and the group (R 1 R 2 C=CR 3 This refers to the number of atoms in the backbone portion of the chain connecting the alkyl group and the alkyl group (—CO—) with the fewest number of atoms.
[0026] In formula (1), the molecular weight of the atomic group X′ may be 472 or less, and is preferably 172 or less. In the case of an atomic group, the lower limit of the molecular weight is not particularly limited, but is usually about 14.
[0027] Specific examples of the compound represented by formula (1) according to this embodiment include acryloyloxypropyl succinic acid, acryloyloxyethyl succinic acid, methacryloyloxyethyl succinic acid, methacryloyloxypropyl succinic acid, 2-carboxyethyl acrylate, 2-carboxyethyl methacrylate, acryloyloxyethyl phthalic acid, methacryloyloxyethyl phthalic acid, N-carboxyethyl (meth)acrylamide, and carboxyethyl thio (meth)acrylate. Among these, acryloyloxypropyl succinic acid and acryloyloxyethyl succinic acid are preferred.
[0028] In the compound represented by the above formula (2) according to this embodiment, 1 , R 2 , and R 3are each independently a hydrogen atom, a fluorine atom, a chlorine atom, or an alkyl group having 1 to 5 carbon atoms. 1 , R 2 , and R 3 is the same as:
[0029] In formula (2), the main chain constituting X" may have 1 to 19 atoms, preferably 1 to 14 atoms, more preferably 1 to 9 atoms, and further preferably 2 to 6 atoms. Examples of atoms constituting the main chain include carbon atoms and heteroatoms. When a heteroatom is contained, the heteroatom is preferably an oxygen atom. The number of atoms in the main chain does not include the number of hydrogen atoms. The number of atoms in the main chain refers to the number of atoms of the carboxyl group described to the right of X" and the group (R 1 R 2 C=CR 3 This refers to the number of atoms in the backbone of the chain that connects the alkyl group (–O–) with the fewest number of atoms.
[0030] In formula (2), the molecular weight of the atomic group X'' may be 484 or less, preferably 184 or less, and more preferably 156 or less. When it is an atomic group, there is no particular lower limit to the molecular weight, but it is usually about 14. X'' is preferably an atomic group having a main chain composed of 2 to 6 atoms and a molecular weight of 156 or less.
[0031] Specific examples of the compound represented by formula (2) according to this embodiment include vinyl carboxymethyl ether and vinyl carboxyethyl ether.
[0032] In the compound represented by the above formula (3) according to this embodiment, 1 , R 2 , and R 3 are each independently a hydrogen atom, a fluorine atom, a chlorine atom, or an alkyl group having 1 to 5 carbon atoms. 1 , R 2 , and R 3 is the same as:
[0033] In formula (3), X''' is a hydrogen atom or a hydrocarbon moiety having 1 to 5 carbon atoms and containing at least one hydroxyl group. Examples of the hydrocarbon moiety having 1 to 5 carbon atoms and containing a hydroxyl group include a hydroxyethyl group and a hydroxypropyl group.
[0034] Specific examples of the compound represented by formula (3) include acrylic acid, methacrylic acid, 2-hydroxyethyl acrylate, 2-hydroxypropyl acrylate, 2-hydroxyethyl methyl acrylate, 2-hydroxypropyl methacrylate, etc. Among these, 2-hydroxyethyl acrylate and acrylic acid are preferred.
[0035] Examples of the other monomers include halogenated alkylvinyl compounds copolymerizable with vinylidene fluoride, fluorine-based monomers, or hydrocarbon monomers such as ethylene and propylene, dimethacrylic acid (poly)alkylene glycol esters, diacrylic acid (poly)alkylene glycol esters, and polyvinylbenzene.
[0036] Examples of halogenated alkyl vinyl compounds include fluorinated alkyl vinyl compounds, and more specifically, examples thereof include hexafluoropropylene (HFP), chlorotrifluoroethylene (CTFE), trifluoroethylene (TFE), tetrafluoroethylene, hexafluoroethylene, and fluoroalkyl vinyl ethers, among which hexafluoropropylene and chlorotrifluoroethylene are preferred. The other monomers may be used alone or in combination of two or more.
[0037] (Example of vinylidene fluoride polymer) As the vinylidene fluoride polymer, commercially available products can be used, such as KF#7300, KF#9100, KF#9700, and KF#7500 manufactured by Kureha Corporation.
[0038] (Inherent viscosity (η i )) The inherent viscosity of the vinylidene fluoride polymer used in the present embodiment is not particularly limited, but is preferably 0.5 to 5.0 dl / g, more preferably 1.0 dl / g or more and 4.5 dl / g or less, and even more preferably 1.5 dl / g or more and 4.0 dl / g or less.
[0039] The above inherent viscosity (η i ) can be calculated from the viscosity (η) of a solution of vinylidene fluoride polymer (A) dissolved in n-methylpyrrolidone (NMP) at 30°C, the viscosity (η0) of NMP at 30°C, and the concentration (C) of vinylidene fluoride polymer (A) in the solution by the following formula:
[0040] η i =(1 / C)·ln(η / η0) (Polymerization method for vinylidene fluoride polymer) The polymerization method for vinylidene fluoride polymer is not particularly limited, and any conventionally known polymerization method can be used. Examples of the polymerization method include suspension polymerization, emulsion polymerization, solution polymerization, etc., and among them, from the viewpoint of ease of post-treatment, etc., aqueous suspension polymerization and emulsion polymerization are preferred, and aqueous suspension polymerization is particularly preferred.
[0041] (Polyisocyanate compounds) In the polyisocyanate compound contained in the electrode mixture composition of the present embodiment, at least a part of the isocyanate groups is blocked with a blocking agent. That is, the polyisocyanate compound has at least one blocked isocyanate group. In this specification, the "blocked isocyanate group" refers to an isocyanate group that is blocked (stabilized) with a blocking agent.
[0042] When the blocked isocyanate group is heated, the blocking agent dissociates (deblocking) and the isocyanate group is regenerated. From the viewpoint of improving the adhesive strength between the current collector and the electrode mixture layer, it is preferable that 60% or more of the total isocyanate groups are blocked with a blocking agent, more preferably 80% or more of the isocyanate groups are blocked with a blocking agent, and it is particularly preferable that all of the isocyanate groups of the polyisocyanate compound are blocked with a blocking agent.
[0043] The polyisocyanate compound contained in the electrode mixture composition of the present embodiment is a polymer of at least one diisocyanate selected from the group consisting of aliphatic diisocyanates, alicyclic diisocyanates, and aromatic diisocyanates, and at least a portion of the isocyanate groups are blocked (stabilized) with a blocking agent.
[0044] Examples of the aliphatic diisocyanate compound include butane diisocyanate, pentane diisocyanate, hexamethylene diisocyanate (HDI), trimethylhexamethylene diisocyanate, and lysine diisocyanate.
[0045] Examples of the alicyclic diisocyanate compound include isophorone diisocyanate (IPDI), hydrogenated xylylene diisocyanate, hydrogenated diphenylmethane diisocyanate, and 1,4-cyclohexane diisocyanate.
[0046] Examples of aromatic diisocyanates include xylylene diisocyanate (XDI), diphenylmethane diisocyanate (MDI), and tolylene diisocyanate (TDI).
[0047] These diisocyanates may be used alone or in combination of two or more.
[0048] Among these, aliphatic diisocyanates and alicyclic diisocyanates are preferred, and from the viewpoints of weather resistance and industrial availability, hexamethylene diisocyanate and isophorone diisocyanate are preferred, with hexamethylene diisocyanate being more preferred.
[0049] The polyisocyanate derived from diisocyanate includes polyisocyanates having at least one bond selected from the group consisting of isocyanurate bond, biuret bond, urethane bond, uretdione bond, urea bond, allophanate bond, oxadiazinetrione bond, and iminooxadiazinedione bond. From the viewpoint of weather resistance and heat resistance, polyisocyanates having an isocyanurate bond, biuret bond, urethane bond, or allophanate bond are preferred. Also, the polyisocyanate may contain two or more of these bonds.
[0050] The number of isocyanate groups (including blocked isocyanate groups) in the polyisocyanate is preferably 2-22, and more preferably 3-18.
[0051] The polyisocyanate may be used alone or in combination of two or more kinds.
[0052] Examples of the blocking agent include oxime compounds, active methylene compounds, pyrazole compounds, alcohol compounds, alkylphenol compounds, phenol compounds, mercaptan compounds, acid amide compounds, acid imide compounds, imidazole compounds, urea compounds, and amine compounds.
[0053] Examples of the oxime compound include formaldoxime, acetaldoxime, acetoxime, methyl ethyl ketoxime (MEK oxime), methyl isobutyl ketoxime (MIBK oxime), dimethyl ketoxime, diethyl ketoxime, and cyclohexanone oxime.
[0054] Examples of active methylene compounds include dimethyl malonate, diethyl malonate, ethyl isobutanoylacetate, methyl acetoacetate, ethyl acetoacetate, and acetylacetone.
[0055] Examples of the pyrazole compound include 3,5-dimethylpyrazole, pyrazole, and 3-methylpyrazole.
[0056] Examples of the alcohol compound include methanol, ethanol, 2-propanol, n-butanol, sec-butanol, 2-ethyl-1-hexanol, 2-methoxyethanol, 2-ethoxyethanol, and 2-butoxyethanol.
[0057] Examples of the alkylphenol compound include monoalkylphenols and dialkylphenols having an alkyl group having 4 or more carbon atoms as a substituent.
[0058] Examples of phenolic compounds include phenol, cresol, ethylphenol, styrenated phenol, and hydroxybenzoic acid esters.
[0059] Examples of the mercaptan compound include butyl mercaptan and dodecyl mercaptan.
[0060] Examples of the acid amide compound include acetanilide, acetic acid amide, ε-caprolactam, δ-valerolactam, and γ-butyrolactam.
[0061] Examples of the acid imide compound include succinimide and maleimide.
[0062] Examples of the imidazole-based compounds include imidazole and 2-methylimidazole.
[0063] Examples of the urea compound include urea, thiourea, and ethyleneurea.
[0064] Examples of the amine compounds include diphenylamine, aniline, carbazole, di-n-propylamine, diisopropylamine, and isopropylethylamine.
[0065] The isocyanate group of the polyisocyanate compound may be blocked with one type of blocking agent, or may be blocked with two or more types of blocking agents.
[0066] In the case of polyisocyanate in which the isocyanate groups are blocked with a blocking agent, the blocking agent is dissociated (deblocked) by heating, and the isocyanate groups are regenerated. It is preferable that the blocking agent is dissociated at the heating temperature in the heating and drying process in which the electrode mixture is applied to the current collector foil and then dried, or at the heating temperature in the heat treatment process in which heat treatment is then performed. From this viewpoint, the blocking agent is preferably an oxime compound, an active methylene compound, or a pyrazole compound. Among them, methyl ethyl ketoxime, dimethyl malonate, diethyl malonate, methyl acetoacetate, ethyl acetoacetate, 3,5-dimethylpyrazole, and pyrazole are preferable. In particular, when an oxime compound is used as a blocking agent, the adhesive strength between the current collector and the electrode mixture layer can be increased, and the thickening of the electrode mixture can be suppressed.
[0067] As the polyisocyanate compound in which at least a part of the isocyanate groups are blocked with a blocking agent, commercially available products can be used, such as Duranate TPA-B80E (oxime derivative blocked polyisocyanate of 1,6-hexamethylene diisocyanate), SBN-70D (pyrazole derivative blocked isocyanate of 1,6-hexamethylene diisocyanate), and MF-K60B (active methylene derivative blocked isocyanate of 1,6-hexamethylene diisocyanate) (all manufactured by Asahi Kasei Chemicals Corporation).
[0068] (Mass ratio of polyisocyanate compound to synthetic resin) In the electrode mixture composition of the present embodiment, the content of the polyisocyanate compound relative to 100 parts by mass of the synthetic resin is preferably 0.5 to 50 parts by mass, more preferably 2 to 40 parts by mass. When the mass ratio of the polyisocyanate compound to the synthetic resin is within the above range, the adhesive strength between the current collector and the electrode mixture layer can be increased. From the viewpoint of increasing the adhesive strength, the inherent viscosity of the synthetic resin is preferably high within the preferred viscosity range of the synthetic resin.
[0069] The form of the electrode mixture composition of this embodiment is not particularly limited, and may be in powder or liquid form. The electrode mixture composition may also contain a solvent. The solvent may be a non-aqueous solvent or may be water. Examples of non-aqueous solvents include N-methylpyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide, dimethylsulfoxide, hexamethylphosphoramide, dioxane, tetrahydrofuran, tetramethylurea, triethyl phosphate, trimethyl phosphate, acetone, ethyl acetate, n-butyl acetate, n-butanol, dipropylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, and cyclohexanone. Two or more of these solvents may be mixed and used.
[0070] [Electrode mixture] The electrode mixture of the present embodiment includes the above-mentioned electrode mixture composition and an active material. The electrode mixture may include a conductive assistant, a non-aqueous solvent, a pigment dispersant, a dispersion stabilizer, and the like.
[0071] The electrode mixture can be used as an electrode mixture for a positive electrode or an electrode mixture for a negative electrode by changing the type of active material depending on the type of the current collector to be applied. Since vinylidene fluoride polymers generally have excellent oxidation resistance, the electrode mixture of the present embodiment can be suitably used as an electrode mixture for a positive electrode. Furthermore, since vinylidene fluoride polymers generally have excellent reduction resistance, the electrode mixture of the present embodiment can be suitably used as an electrode mixture for a negative electrode.
[0072] (Active material) As the positive electrode active material, a lithium composite metal oxide is typically used.
[0073] Examples of the lithium composite metal oxide include, for example, LiMnO2, LiMn2O4, LiCoO2, LiNiO2, LiNi x Co 1-x O2 (0 < x < 1), LiNi x Co y Mn 1-x-y O2 (0 < x < 1, 0 < y < 1), LiNi x Co y Al Z O2 (0.55 ≤ x < 1, 0 < y2 < 0.55, 0 < z < 0.55, and x / (x + y + z) ≥ 0.55), LiFePO4, etc. can be mentioned. As specific examples of the lithium composite metal oxide, Li 1.00 Ni 0.5 Co 0.2 Mn 0.3 O2 (NCM523), Li 1.00 Ni 0.6 Co 0.2 Mn 0.2 O2 (NCM622), Li 1.00 Ni 0.83 Co 0.12 Mn 0.05 O2 (NCM811), and Li 1.00 Ni 0.85 Co 0.15 Al 0.05 O2 (NCA811) can be mentioned.
[0074] As the negative electrode active material, conventionally known materials such as carbon materials, metal / alloy materials, and metal oxides can be used. Among these, from the viewpoint of further increasing the energy density of the battery, carbon materials are preferred, and examples of the carbon materials include artificial graphite, natural graphite, graphitization-resistant carbon, and graphitization-easy carbon.
[0075] In the electrode binder, when the active material is 100 parts by mass, it is preferably contained 0.2 to 15 parts by mass of a vinylidene fluoride polymer, and more preferably contained 0.5 to 10 parts by mass.
[0076] (Conductive assistant) The conductive assistant may be added for the purpose of improving the conductivity of the electrode mixture layer when an active material with low electronic conductivity such as LiCoO2 is used. Examples of the conductive assistant include carbonaceous materials such as carbon black, carbon nanotubes, graphite fine powder and graphite fiber, and metal fine powder or metal fiber such as nickel and aluminum.
[0077] (Non-aqueous solvent) The non-aqueous solvent may be any of those exemplified as non-aqueous solvents that may be contained in the electrode mixture composition, such as N-methylpyrrolidone (NMP), etc. The non-aqueous solvent may be used alone or in combination of two or more.
[0078] (Other components of electrode mixture) The electrode mixture in this embodiment may contain other components in addition to the above-mentioned components, such as a pigment dispersant such as polyvinylpyrrolidone.
[0079] (Preparation of electrode mixture) The electrode mixture according to this embodiment may be prepared by, for example, mixing an electrode mixture composition containing a synthetic resin and a polyisocyanate compound, and an active material to form a uniform slurry, and the order of mixing is not particularly limited. Furthermore, when using an electrode mixture composition containing a solvent as the electrode mixture composition, an electrode active material or the like may be added before adding the solvent to the electrode mixture composition. For example, an electrode active material may be added to the electrode mixture composition, and then a solvent may be added and stirred and mixed to obtain an electrode mixture. Alternatively, an electrode active material may be added to an electrode mixture composition containing a solvent as the electrode mixture composition, and stirred and mixed to obtain an electrode mixture.
[0080] Alternatively, the porous polymer can be prepared by mixing a polyisocyanate compound with an active material, and then mixing the synthetic resin therewith.
[0081] 〔electrode〕 The electrode according to the present embodiment includes an electrode mixture layer formed from the electrode mixture on a current collector. In this specification and the like, unless otherwise specified, the term "electrode" refers to an electrode of a battery in which an electrode mixture layer formed from the electrode mixture in the present embodiment is formed on a current collector.
[0082] (current collector) The current collector is the base material of the electrode and is a terminal for extracting electricity. Examples of the material of the current collector include iron, stainless steel, steel, copper, aluminum, nickel, and titanium. The current collector is preferably in the form of a foil or a mesh. When the electrode is a positive electrode, the current collector is preferably an aluminum foil. The thickness of the current collector is preferably 1 μm to 100 μm, and more preferably 3 to 20 μm.
[0083] (Electrode mixture layer) The electrode mixture layer is a layer obtained by applying the above-mentioned electrode mixture to a current collector and drying it. The electrode mixture can be applied by a method known in the art, and can include a method using a bar coater, a die coater, a comma coater, or the like. The drying temperature for forming the electrode mixture layer is preferably 50°C to 200°C, and more preferably 80°C to 180°C. The electrode mixture layer may be formed on both sides of the current collector, or only on one side.
[0084] The thickness of the electrode mixture layer is usually 20 to 600 μm, preferably 20 to 350 μm per side. The electrode mixture layer may be pressed to increase its density. The basis weight of the electrode mixture layer is usually 20 to 700 g / m 2 and preferably 30 to 500 g / m 2 It is.
[0085] As described above, the electrode becomes a positive electrode when an electrode mixture layer is obtained using an electrode mixture for a positive electrode, and becomes a negative electrode when an electrode mixture layer is obtained using an electrode mixture for a negative electrode. The electrode according to this embodiment can be used as a positive electrode of a non-aqueous electrolyte secondary battery such as a lithium ion secondary battery. Alternatively, it can be used as a negative electrode of a non-aqueous electrolyte secondary battery such as a lithium ion secondary battery.
[0086] [Electrode manufacturing method] An example of a method for producing an electrode will be specifically described below, but the method for producing an electrode according to this embodiment is not limited to the method described below.
[0087] (Method of manufacturing electrodes using one-step heating) The method for producing an electrode according to this embodiment includes a coating step of coating the electrode mixture onto a current collector, and a heat-drying step of heating and drying the current collector after the coating step at a temperature of 80° C. or higher.
[0088] <Coating process> In the coating step, the electrode mixture is coated onto the current collector. The method for coating the electrode mixture may be a method known in the art, such as a method using a bar coater, a die coater, or a comma coater.
[0089] <Heat drying process> In the heat drying step, the current collector after the coating step is heat dried at a temperature of 80° C. or higher, preferably at a temperature of 110° C. or higher. Heat drying within the above temperature range allows the blocking agent to be dissociated from the blocked isocyanate groups. In addition, it is preferable that the temperature of the electrode mixture applied to the current collector is 80° C. or higher.
[0090] The temperature at which the blocking agent dissociates and the thermal stability of the blocked isocyanate group vary depending on the type of blocking agent, so the heat drying temperature may be appropriately selected depending on the type of blocking agent. For example, when the blocking agent that blocks the isocyanate group is an oxime compound, it is more preferable to heat dry at 110 to 180°C. When the blocking agent that blocks the isocyanate group is an active methylene compound, it is more preferable to heat dry at 80 to 150°C. When the blocking agent that blocks the isocyanate group is a pyrazole compound, it is more preferable to heat dry at 80 to 180°C.
[0091] The heating and drying time is not particularly limited, but is preferably 1 to 300 minutes, and may be appropriately selected depending on the heating temperature.
[0092] (Method of manufacturing electrodes by multiple heating stages) The method for producing an electrode according to this embodiment may include a coating step of coating a current collector with the electrode mixture, a drying step of heating and drying the current collector after the coating step at a temperature of 110° C. or less, and a heat treatment step of treating the current collector after the drying step at a temperature higher than the temperature in the drying step and at least 110° C. The coating step is the same as the coating step described above (method for producing an electrode by heating in one step).
[0093] <Drying process> In the drying step, the current collector after the coating step is heated and dried at a temperature of 110° C. or less. In the drying step, it is preferable to heat and dry at a temperature at which most of the blocking agent does not dissociate from the blocked isocyanate groups and at which the solvent in the electrode mixture can be removed. Specifically, it is preferable to heat and dry at a temperature of 110° C. or less, and it is more preferable to heat and dry at a temperature of 100° C. or less. In addition, it is preferable that the temperature of the electrode mixture applied to the current collector is 110° C. or less.
[0094] The drying time is not particularly limited, but is preferably 1 to 100 minutes.
[0095] <Heat treatment process> In the heat treatment step, the current collector after the drying step is heat-treated at a temperature higher than that in the drying step and at 110° C. or higher. By performing the heat treatment within the above temperature range, the blocking agent can be dissociated from most of the blocked isocyanate groups. In addition, it is preferable that the temperature of the electrode mixture applied to the current collector is 110° C. or higher.
[0096] The temperature at which the blocking agent dissociates and the thermal stability of the blocked isocyanate group vary depending on the type of blocking agent, so the heat treatment temperature may be appropriately selected depending on the type of blocking agent. For example, when the blocking agent blocking the isocyanate group is an oxime compound, it is more preferable to perform the heat treatment at 120 to 180°C. When the blocking agent blocking the isocyanate group is an active methylene compound, it is preferable to perform the heat treatment at 110 to 150°C. When the blocking agent blocking the isocyanate group is a pyrazole compound, it is preferable to perform the heat treatment at 120 to 180°C.
[0097] The heat treatment time is not particularly limited, but is preferably 1 to 300 minutes, and may be appropriately selected depending on the heating temperature.
[0098] An electrode manufactured by multiple heating stages can have a stronger adhesive strength between the current collector and the electrode mixture layer than an electrode manufactured by a single heating stage. The reason for this is believed to be as follows.
[0099] It is considered that the isocyanate group is bonded to the OH group present in the active material and the current collector (e.g., aluminum foil), thereby improving the adhesion at the interface between the active material and the vinylidene fluoride polymer and at the interface between the current collector and the electrode mixture layer. The isocyanate group reacts preferentially with amines rather than with OH groups. Therefore, when the blocking agent is dissociated from the blocked isocyanate group and the isocyanate group is regenerated, if there is a large amount of amine contained in the dispersion medium around the isocyanate group, the isocyanate group reacts with the amine rather than with the OH group present in the active material and the current collector. Therefore, first, the amount of amine present is reduced by removing the dispersion medium in the electrode mixture layer in the first heating stage. Then, it is considered that the regenerated isocyanate group is bonded to the OH group present in the active material and the current collector by dissociating the blocking agent from the blocked isocyanate group in the second and subsequent heating stages, thereby improving the adhesion. It is considered that the isocyanate group reacts more easily with amines, OH groups, and COOH groups in that order.
[0100] [Nonaqueous electrolyte secondary battery] The nonaqueous electrolyte secondary battery of this embodiment includes the above-mentioned electrode. Other components in the nonaqueous electrolyte secondary battery are not particularly limited, and for example, conventionally used components can be used.
[0101] As a method for producing a non-aqueous electrolyte secondary battery, for example, a method is available in which a negative electrode layer and a positive electrode layer are superimposed with a separator interposed therebetween, the layers are placed in a battery container, and an electrolytic solution is injected into the battery container and then sealed. In this production method, at least a part of the vinylidene fluoride polymer contained in the electrode mixture is melted by heat pressing after the injection of the electrode solution, and is bonded to the separator.
[0102] 〔summary〕 The electrode mixture composition according to this embodiment is a composition for an electrode mixture, comprising a synthetic resin containing a vinylidene fluoride polymer in a proportion of 99% by mass or more, and a polyisocyanate compound in which at least a portion of the isocyanate groups are blocked with a blocking agent.
[0103] In the electrode mixture composition according to the present embodiment, the polyisocyanate compound is preferably at least one compound selected from an isocyanurate, a biuret, and an adduct derived from hexamethylene diisocyanate.
[0104] In the electrode mixture composition according to this embodiment, the blocking agent is preferably at least one blocking agent selected from the group consisting of an oxime compound, an active methylene compound, and a pyrazole compound.
[0105] In the electrode mixture composition according to this embodiment, the blocking agent is more preferably an oxime compound.
[0106] In the electrode mixture composition according to the present embodiment, the content of the polyisocyanate compound is preferably 0.5 to 50 parts by mass with respect to 100 parts by mass of the synthetic resin.
[0107] In the electrode mixture composition according to this embodiment, the vinylidene fluoride polymer may be a homopolymer of vinylidene fluoride.
[0108] Furthermore, in the electrode mixture composition according to this embodiment, the vinylidene fluoride polymer may be a vinylidene fluoride copolymer having vinylidene fluoride as a main constituent component and containing at least one structural unit selected from the group consisting of a structural unit derived from an unsaturated dibasic acid, a structural unit derived from an unsaturated dibasic acid monoester, a structural unit derived from an alkyl vinyl halide compound, a structural unit derived from a compound represented by the following formula (1), a structural unit derived from a compound represented by the following formula (2), and a structural unit derived from a compound represented by the following formula (3).
[0109] [ka] (In formulas (1) to (3), R 1 , R 2 , R 3are each independently a hydrogen atom, a fluorine atom, a chlorine atom, or an alkyl group having 1 to 5 carbon atoms; in formula (1), X' is an atomic group having a main chain consisting of 1 to 19 atoms and a molecular weight of 472 or less; in formula (2), X'' is an atomic group having a main chain consisting of 1 to 19 atoms and a molecular weight of 484 or less; and in formula (3), X''' is hydrogen or a hydrocarbon moiety having 1 to 5 carbon atoms containing at least one hydroxyl group.
[0110] The electrode mixture according to this embodiment contains the composition for an electrode mixture and an active material.
[0111] The electrode according to this embodiment includes an electrode mixture layer formed from the electrode mixture on a current collector.
[0112] The nonaqueous electrolyte secondary battery according to this embodiment includes the above-described electrode.
[0113] The method for producing an electrode according to this embodiment includes a coating step of coating a current collector with the electrode mixture, and a heat-drying step of heating and drying the current collector after the coating step at a temperature of 80° C. or higher.
[0114] Moreover, the method for producing an electrode according to the present embodiment includes a coating step of coating a current collector with the electrode mixture, a drying step of heating and drying the current collector after the coating step at a temperature of 110°C or less, and a heat treatment step of treating the current collector after the drying step at a temperature higher than the temperature in the drying step and not less than 110°C.
[0115] The following examples are provided to further explain the embodiments of the present invention. Of course, the present invention is not limited to the following examples, and various modifications are possible in detail. Furthermore, the present invention is not limited to the above-described embodiments, and various modifications are possible within the scope of the claims. The embodiments obtained by appropriately combining the technical means disclosed herein are also included in the technical scope of the present invention. In addition, all of the documents described in this specification are incorporated by reference. EXAMPLES
[0116] [Example 1] Preparation of electrode mixture As a positive electrode active material, 100 parts by mass of Li 1.0 Ni 0.5 Co 0.2 Mn 0.3 As the conductive carbon black, 2 parts by mass of Super-P (manufactured by Timcal Japan, average particle diameter 40 nm, specific surface area 60 m) was used. 2 / g) was used. 2 parts by mass of polyvinylidene fluoride (KF#9700 manufactured by Kureha Corporation) was used as the synthetic resin. 0.38 parts by mass of polyisocyanate (Duranate (trademark) TPA-B80E manufactured by Asahi Kasei Chemicals Corporation) was used as the polyisocyanate compound. The positive electrode active material, conductive carbon black, synthetic resin, and polyisocyanate compound were dispersed in NMP to prepare a slurry-like positive electrode mixture (electrode mixture).
[0117] [Example 2] Preparation of electrode mixture An electrode mixture was prepared in the same manner as in Example 1, except that the amount of the polyisocyanate compound was 0.04 parts by mass.
[0118] [Example 3] Preparation of electrode mixture An electrode mixture was prepared in the same manner as in Example 1, except that the amount of the polyisocyanate compound was 0.16 parts by mass.
[0119] [Example 4] Preparation of electrode mixture An electrode mixture was prepared in the same manner as in Example 1, except that the amount of the polyisocyanate compound was 0.57 parts by mass.
[0120] [Example 5] Preparation of electrode mixture An electrode mixture was prepared in the same manner as in Example 1, except that the polyisocyanate compound was SBN-70D (manufactured by Asahi Kasei Chemicals Corporation).
[0121] [Example 6] Preparation of electrode mixture An electrode mixture was prepared in the same manner as in Example 1, except that the polyisocyanate compound was MF-K60B (manufactured by Asahi Kasei Chemicals Corporation).
[0122] [Comparative Example 1] Preparation of electrode mixture An electrode mixture was prepared in the same manner as in Example 1, except that the amount of the synthetic resin was 2.38 parts by mass and no polyisocyanate compound was used.
[0123] [Comparative Example 2] Preparation of electrode mixture An electrode mixture was prepared in the same manner as in Example 1, except that the amount of the synthetic resin was 3 parts by mass and no polyisocyanate compound was used.
[0124] [Comparative Example 3] Preparation of electrode mixture An electrode mixture was prepared in the same manner as in Example 1, except that the amount of the polyisocyanate compound was 2.04 parts by mass and no synthetic resin was used.
[0125] [Comparative Example 4] Preparation of electrode mixture An electrode mixture was prepared in the same manner as in Comparative Example 3, except that the polyisocyanate compound was changed to SBN-70D.
[0126] [Comparative Example 5] Preparation of electrode mixture An electrode mixture was prepared in the same manner as in Example 1, except that the polyisocyanate compound was an isocyanate compound MOI-BP (manufactured by Showa Denko KK).
[0127] [Comparative Example 6] Preparation of electrode mixture An electrode mixture was prepared in the same manner as in Example 1, except that the polyisocyanate compound was a polyisocyanate compound 24A-100 (manufactured by Asahi Kasei Corporation) in which the isocyanate group was not blocked.
[0128] [Example 7] Preparation of electrode mixture An electrode mixture was prepared in the same manner as in Example 1, except that the synthetic resin was KF#7300 (manufactured by Kureha Corporation).
[0129] [Comparative Example 7] Preparation of electrode mixture An electrode mixture was prepared in the same manner as in Comparative Example 1, except that the synthetic resin was KF#7300.
[0130] [Example 8] Preparation of electrode mixture An electrode mixture was prepared in the same manner as in Example 1, except that the synthetic resin was KF#9100 (manufactured by Kureha Corporation).
[0131] [Comparative Example 8] Preparation of electrode mixture An electrode mixture was prepared in the same manner as in Comparative Example 1, except that the synthetic resin was KF#9100.
[0132] [Example 9] Preparation of electrode mixture An electrode mixture was prepared in the same manner as in Example 1, except that the synthetic resin was KF#7500 (manufactured by Kureha Corporation).
[0133] [Comparative Example 9] Preparation of electrode mixture An electrode mixture was prepared in the same manner as in Comparative Example 1, except that the synthetic resin was KF#7500 (manufactured by Kureha Corporation).
[0134] [Example 10] Preparation of electrode mixture An electrode mixture was prepared in the same manner as in Example 1, except that the positive electrode active material was LiCoO2 (LCO Cellseed C5H, manufactured by Nippon Chemical Industry Co., Ltd., average particle diameter 5 μm).
[0135] [Comparative Example 10] Preparation of electrode mixture An electrode mixture was prepared in the same manner as in Comparative Example 1, except that LCO was used as the positive electrode active material.
[0136] [Example 11] Preparation of electrode mixture The positive electrode active material was LiFePO4 (LFP, average particle size 1.2 μm, specific surface area 14.7 m 2 An electrode mixture was prepared in the same manner as in Example 1, except that the weight ratio of the electrode mixture was changed to 1 / g.
[0137] [Comparative Example 11] Preparation of electrode mixture An electrode mixture was prepared in the same manner as in Comparative Example 1, except that LFP was used as the positive electrode active material.
[0138] [Example 12] Preparation of electrode mixture The positive electrode active material is Li 1.0 Ni 0.85 Co 0.15 Al 0.05 O2 (NCA811, average particle size 14.7μm, specific surface area 0.17m 2 An electrode mixture was prepared in the same manner as in Example 1, except that the weight ratio of the electrode mixture was changed to 1 / g.
[0139] [Example 13] Preparation of electrode mixture An electrode mixture was prepared in the same manner as in Example 12, except that the polyisocyanate compound was SBN-70D.
[0140] [Comparative Example 12] Preparation of electrode mixture An electrode mixture was prepared in the same manner as in Comparative Example 1, except that the positive electrode active material was NCA.
[0141] [Example 14] Preparation of electrode mixture As the negative electrode active material, 95 parts by mass of natural graphite (BTR NEW ENERGY MATERIALS INC., BTR (registered trademark) 918) was used. As the synthetic resin, 4.5 parts by mass of polyvinylidene fluoride (KF#9700, Kureha Corporation) was used. As the polyisocyanate compound, 0.5 parts by mass of polyisocyanate (Duranate (trademark) TPA-B80E, Asahi Kasei Chemicals Corporation) was used. The negative electrode active material, synthetic resin, and polyisocyanate compound were dispersed in NMP to prepare a slurry-like negative electrode mixture (electrode mixture).
[0142] [Comparative Example 13] Preparation of electrode mixture An electrode mixture was prepared in the same manner as in Example 14, except that the amount of the synthetic resin was 5.0 parts by mass and no polyisocyanate compound was used.
[0143] [Example 15] Preparation of electrode mixture An electrode mixture was prepared in the same manner as in Example 14, except that the synthetic resin was KF#7300 (manufactured by Kureha Corporation).
[0144] [Comparative Example 14] Preparation of electrode mixture An electrode mixture was prepared in the same manner as in Comparative Example 13, except that the synthetic resin was KF#7300 (manufactured by Kureha Corporation).
[0145] [Evaluation Example 1] Measurement of peel strength The positive electrode mixture obtained in each of the Examples and Comparative Examples was applied to an Al foil having a thickness of 15 μm using a bar coater, and then dried by heating at 110° C. for 30 minutes. The positive electrode mixture was then further heat-treated at 130° C. for 2 hours, and the coating weight on one side was 200 g / m 2 A single-sided coated electrode was prepared.
[0146] The single-sided coated electrode was cut to a length of 50 mm and a width of 20 mm, and a 90-degree peel test was performed at a head speed of 10 mm / min using a tensile tester (UNIVERSAL TESTING INSTRUMENT MODEL: STA-1150 manufactured by Orientec Co., Ltd.) in accordance with JIS K6854-1 to measure the peel strength (gf / mm). The results of the peel strength measurement are shown in Table 1.
[0147] [Evaluation Example 2] Viscosity measurement of electrode mixture The slurry viscosity of the positive electrode mixture obtained in Examples 12 and 13 and Comparative Example 12 was measured using a B-type viscometer (a digital viscometer LV DV-E manufactured by BROOKFIELD) with a spindle No. 64. After preliminary stirring at 0.5 rpm for 1 minute, the viscosity was measured at 1.0 rpm for 2 minutes, at 6.0 rpm for 2 minutes, and at 12 rpm for 2 minutes. The viscosity value after 2 minutes at 1.0 rpm was taken as the slurry viscosity.
[0148] While storing the above slurry-like positive electrode mixture in a nitrogen atmosphere at 25°C, the slurry viscosity was measured at regular intervals (the start of storage was set as 0 hours, followed by 3 hours, 6 hours, 24 hours, 48 hours, and 72 hours). When the slurry viscosity exceeded 400,000 mPa s, it was determined that the above positive electrode mixture had gelled.
[0149] If no gelation occurred after 72 hours, it was judged as "◎" (thickening of the electrode mixture was sufficiently suppressed). If no gelation occurred up to 48 hours, it was judged as "○" (thickening of the electrode mixture was suppressed). If gelation occurred within 24 hours, it was judged as "×" (thickening of the electrode mixture was not suppressed). The results of the viscosity measurements are shown in Table 1.
[0150] [Table 1]
[0151] As shown in Table 1, high peel strength was observed when the electrode mixtures of Examples 1 to 13 were used. On the other hand, the peel strength was low when the electrode mixtures of Comparative Examples 1, 2, and 7 to 12, which did not contain a polyisocyanate compound, were used. The peel strength was also low when the electrode mixtures of Comparative Examples 3 and 4, which did not contain a synthetic resin, were used.
[0152] In addition, when comparing Example 1, Comparative Examples 5 and 6, when the electrode mixture of Example 1 containing a polyisocyanate compound in which at least a part of the isocyanate group is a blocked isocyanate group was used, a sufficiently high peel strength was shown. On the other hand, when the electrode mixture of Comparative Example 5 containing an isocyanate compound having a blocked isocyanate group, which is not a polyisocyanate compound, was used, the peel strength was not sufficient. In addition, when the electrode mixture of Comparative Example 6 containing a polyisocyanate compound in which the isocyanate group is not blocked was used, the peel strength was also not sufficient. From these results, it was found that the adhesive strength between the current collector and the electrode mixture layer can be increased by using a polyisocyanate compound in which at least a part of the isocyanate group is a blocked isocyanate group for the electrode mixture.
[0153] In addition, when Examples 12 and 13 are compared with Comparative Example 12, thickening was suppressed in the electrode mixtures of Examples 12 and 13, which contained a polyisocyanate compound. In particular, thickening was sufficiently suppressed in the electrode mixture of Example 12, which contained a polyisocyanate compound in which at least a portion of the isocyanate groups were blocked by an oxime compound. On the other hand, thickening was not suppressed in the electrode mixture of Comparative Example 12, which did not contain a polyisocyanate compound.
[0154] [Evaluation Example 3] Examination of peel strength according to heating and drying temperature Except for changing the amount of the synthetic resin to 1.68 parts by mass and the amount of the polyisocyanate compound to 0.32 parts by mass, an electrode mixture was prepared in the same manner as in Example 5. Next, the peel strength was measured in the same manner as in Evaluation Example 1, except that the heating and drying temperature was set to 90° C. and no heat treatment was performed.
[0155] [Evaluation Example 4] Examination of peel strength depending on heating and drying temperature The peel strength was measured in the same manner as in Evaluation Example 3, except that the heating and drying temperature was 100°C.
[0156] [Evaluation Example 5] Examination of peel strength according to heating and drying temperature Except for changing the amount of the synthetic resin to 2 parts by mass and not using a polyisocyanate compound, an electrode mixture was prepared in the same manner as in Example 5. Next, the peel strength was measured in the same manner as in Evaluation Example 3.
[0157] [Evaluation Example 6] Examination of peel strength as a function of heat treatment temperature Except for changing the amount of the synthetic resin to 1.68 parts by mass and the amount of the polyisocyanate compound to 0.32 parts by mass, an electrode mixture was prepared in the same manner as in Example 1. Next, the peel strength was measured in the same manner as in Evaluation Example 1, except for changing the heating and drying temperature to 100°C.
[0158] [Evaluation Example 7] Examination of peel strength as a function of heat treatment temperature The peel strength was measured in the same manner as in Evaluation Example 6, except that the heating and drying temperature was 110°C.
[0159] [Evaluation Example 8] Examination of peel strength as a function of heat treatment temperature The peel strength was measured in the same manner as in Evaluation Example 6, except that the heating and drying temperature was 130°C.
[0160] [Evaluation Example 9] Examination of peel strength according to heat treatment temperature Except for changing the amount of the synthetic resin to 2 parts by mass and not using a polyisocyanate compound, an electrode mixture was prepared in the same manner as in Example 1. Next, the peel strength was measured in the same manner as in Evaluation Example 1.
[0161] The peel strength measurement results in Evaluation Examples 3 to 9 are shown in Table 2.
[0162] [Table 2]
[0163] As shown in Table 2, Evaluation Examples 3 and 4 showed high peel strength, while Evaluation Example 5, which used an electrode mixture not containing a polyisocyanate compound, showed low peel strength. In addition, when Evaluation Examples 3 and 4 are compared, Evaluation Example 4, in which the heating and drying temperature was 100°C, showed the highest peel strength.
[0164] Furthermore, as shown in Table 2, Evaluation Examples 6 to 8 exhibited high peel strength, while Evaluation Example 9, which used an electrode mixture not containing a polyisocyanate compound, exhibited low peel strength. Comparing Evaluation Examples 6 to 8, Evaluation Example 6, in which the heating and drying temperature was 100°C, exhibited the highest peel strength.
[0165] The polyisocyanate compounds used in Evaluation Examples 6 to 8 are polyisocyanate compounds in which at least a portion of the isocyanate groups are blocked with a blocking agent. When the polyisocyanate compounds are heated at around 130° C., the blocking agent dissociates from the isocyanate groups, and the isocyanate groups are regenerated.
[0166] In Evaluation Example 8, it is believed that the blocking agent was dissociated from most of the blocked isocyanate groups in the heat drying step by setting the heat drying temperature to 130° C. On the other hand, in Evaluation Examples 6 to 7, in which the heat drying temperature was set to 110° C. or lower, the blocking agent was not dissociated from the blocked isocyanate groups much in the heat drying step, and it is believed that the blocking agent was dissociated from most of the blocked isocyanate groups in the heat treatment step.
[0167] The results of Evaluation Examples 6 to 9 show that the adhesive strength between the current collector and the electrode mixture layer can be further increased by drying at a temperature below which dissociation of the blocking agent from the blocked isocyanate groups is minimal, and then drying (heat treatment) at a temperature above which most of the blocking agent dissociates from the blocked isocyanate groups.
[0168] [Evaluation Example 10] Measurement of peel strength The negative electrode mixtures obtained in Examples 14 and 15 and Comparative Examples 13 and 14 were each applied to a Cu foil having a thickness of 10 μm using a bar coater, and then dried by heating at 110° C. for 30 minutes. The negative electrode mixtures were then further heat-treated at 130° C. for 2 hours to obtain a coating weight on one side of 150 g / m 2 A single-sided coated electrode was prepared.
[0169] The single-sided coated electrode was cut to a length of 50 mm and a width of 20 mm, and a 90-degree peel test was performed at a head speed of 10 mm / min using a tensile tester (UNIVERSAL TESTING INSTRUMENT MODEL: STA-1150 manufactured by Orientec Co., Ltd.) in accordance with JIS K6854-1 to measure the peel strength (gf / mm). The results of the peel strength measurement are shown in Table 3.
[0170] [Table 3] [Industrial Applicability]
[0171] The present invention can be used as an electrode mixture to be applied to a current collector in the manufacture of electrodes for non-aqueous electrolyte secondary batteries.
Claims
1. A synthetic resin containing a vinylidene fluoride polymer in a proportion of 99% by mass or more; A composition for an electrode mixture comprising: a polyisocyanate compound in which at least a part of the isocyanate groups is blocked with a blocking agent; The vinylidene fluoride polymer is at least one selected from a vinylidene fluoride homopolymer and a vinylidene fluoride copolymer, The vinylidene fluoride copolymer has vinylidene fluoride as a main component, A composition for an electrode mixture, which is a copolymer of vinylidene fluoride and at least one structural unit selected from the group consisting of a structural unit derived from an unsaturated dibasic acid, a structural unit derived from an unsaturated dibasic acid monoester, a structural unit derived from an alkyl vinyl halide compound, a structural unit derived from a compound represented by the following formula (1), a structural unit derived from a compound represented by the following formula (2), and a structural unit derived from a compound represented by the following formula (3) (with the exception that the structural unit is a structural unit derived from an unsaturated peroxide). 【Chemistry 1】 (In formulas (1) to (3), R 1 , R 2 , R 3 each independently represents a hydrogen atom, a fluorine atom, a chlorine atom, or an alkyl group having 1 to 5 carbon atoms, In formula (1), X′ is an atomic group having a main chain composed of 1 to 19 atoms and a molecular weight of 472 or less, In formula (2), X″ is an atomic group having a main chain composed of 1 to 19 atoms and a molecular weight of 484 or less, In formula (3), X''' is hydrogen or a hydrocarbon moiety having 1 to 5 carbon atoms and containing at least one hydroxyl group.
2. 2. The electrode mixture composition according to claim 1, wherein the polyisocyanate compound is at least one compound selected from an isocyanurate, a biuret, and an adduct derived from hexamethylene diisocyanate.
3. 3. The composition for an electrode mixture according to claim 1, wherein the blocking agent is at least one blocking agent selected from the group consisting of an oxime compound, an active methylene compound, and a pyrazole compound.
4. The composition for an electrode mixture according to any one of claims 1 to 3, wherein the blocking agent is an oxime compound.
5. The electrode mixture composition according to any one of claims 1 to 4, wherein the content of the polyisocyanate compound relative to 100 parts by mass of the synthetic resin is 0.5 to 50 parts by mass.
6. An electrode mixture comprising the composition for an electrode mixture according to any one of claims 1 to 5 and an active material.
7. An electrode comprising an electrode mixture layer formed from the electrode mixture according to claim 6 on a current collector.
8. A non-aqueous electrolyte secondary battery comprising the electrode according to claim 7.
9. A coating step of coating a current collector with the electrode mixture according to claim 6; and a heat drying step of heating and drying the current collector after the coating step at a temperature of 80° C. or higher.
10. A coating step of coating a current collector with the electrode mixture according to claim 6; a drying step of heating and drying the current collector after the coating step at a temperature of 110° C. or less; The method for producing an electrode includes a heat treatment step of treating the current collector after the drying step at a temperature higher than the temperature of the drying step and not lower than 110°C.
Citation Information
Patent Citations
Vinylidene fluoride-based copolymer
JP1994172452A
Lithium secondary battery
JP1994243896A
Resin composition
JP1998330611A
Depolarizing mix for nonaqueous battery and nonaqueous battery
JP1999195419A
Decorative sheet and its manufacture
JP2000108292A