Method for producing modified cellulose microfibrils

A method of chemically modifying cellulose and defibrating it under controlled conditions produces modified cellulose microfibrils with improved fiber length and aspect ratio, addressing the inefficiencies of existing methods and enhancing water retention and strength.

JP7554770B2Active Publication Date: 2024-09-20NIPPON PAPER IND CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2021562729
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-12-03
Filing Date
2020-12-03
Publication Date
2024-09-20
Estimated Expiration
2040-12-03

AI Technical Summary

Technical Problem

Existing methods for producing modified cellulose microfibrils do not provide conditions for efficient production of fibrillated cellulose fibers with a long average fiber length and large aspect ratio, which are necessary for various applications.

Method used

A method involving chemical modification of cellulose raw materials followed by mechanical defibration under specific pH and solid content conditions, including oxidation, etherification, and defibration processes, to produce modified cellulose microfibrils with desired properties.

Benefits of technology

The method efficiently produces modified cellulose microfibrils with long average fiber length and large aspect ratio, enhancing water retention and strength properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007554770000001
    Figure 0007554770000001
  • Figure 0007554770000003
    Figure 0007554770000003
  • Figure 0007554770000002
    Figure 0007554770000002
Patent Text Reader

Abstract

The purpose of the present invention is to provide a method for manufacturing modified cellulose fiber which is obtained through fibrillation and which has a long average fiber length and a large aspect ratio. The present invention provides a method for manufacturing modified cellulose microfibrils, the method including: a step (1) for subjecting a cellulosic raw material to an oxidation process and obtaining oxidized cellulose; and a step (2) for performing fiber dissociation by mechanically processing the oxidized cellulose obtained in step (1) under the conditions of a pH of 7 or less and a solid content concentration of 0.1-15 mass%. The modified cellulose microfibrils preferably have an average fiber diameter of 500 nm or more, an average fiber length of 500 μm or more, and an aspect ratio of 30 or more.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing modified cellulose microfibrils. [Background technology]

[0002] Modified cellulose microfibrils can be obtained by modifying cellulose raw materials such as pulp and then wet-pulverizing them, and are expected to be used as an additive to improve the strength and water retention of paper (Patent Documents 1 and 2). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] International Publication No. 2019 / 189588 [Patent Document 2] International Publication No. 2019 / 189611 Summary of the Invention [Problem to be solved by the invention]

[0004] However, the production conditions for modified cellulose microfibrils are not described in Patent Documents 1 and 2. Modified cellulose nanofibers have a lower viscosity than nano-order cellulose nanofibers with an average fiber diameter of less than 500 nm, and are expected to be useful in various applications, so there is a demand for the development of an efficient production method.

[0005] An object of the present invention is to provide a method for producing fibrillated modified cellulose fibers having a long average fiber length and a large aspect ratio. [Means for solving the problem]

[0006] The present invention provides the following [1] to [8]. [1] Step (1): A step of modifying a cellulosic raw material to obtain modified cellulose; and Step (2): A step of mechanically treating the modified cellulose obtained in step (1) under conditions of a pH of 7 or less and a solid content concentration of 0.1 to 15% by mass to defibrate the cellulose; A method for producing modified cellulose microfibrils, comprising: [2] The method according to [1], wherein the modified cellulose is oxidized cellulose or etherified cellulose. [3] The method according to [2], wherein the etherified cellulose is a carboxyalkylated cellulose. [4] The method according to [2] or [3], wherein the carboxyl group content of the oxidized cellulose and the carboxyalkylated cellulose is 0.1 to 2.5 mmol / g. [5] The method according to any one of [2] to [4], wherein the carboxyl substitution degree of the oxidized cellulose is 0.01 to 0.50. [6] The method according to [3] or [4], wherein the carboxyalkyl substitution degree of the carboxyalkylated cellulose is 0.01 to 0.50. [7] The method according to any one of [1] to [6], wherein the mechanical treatment is a beating or defibration treatment. [8] The method according to any one of [1] to [7], wherein the modified cellulose microfibrils have an average fiber diameter of 500 nm or more, an average fiber length of 500 μm or more, and an aspect ratio of 30 or more. Effect of the Invention

[0007] According to the method of the present invention, modified cellulose microfibrils having a long average fiber length and a large aspect ratio can be efficiently produced. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] In the present invention, modified cellulose microfibrils can be produced by a method including the following steps (1) and (2). The order of steps (1) and (2) is not particularly limited, but it is preferable to perform steps (1) and (2) in that order. Step (1): A step of modifying a cellulosic raw material to obtain modified cellulose; and Step (2): A step of defibrating the modified cellulose obtained in step (1) by mechanical treatment under conditions of pH 7 or less and a solid content concentration of 0.1 to 15 mass %.

[0009] <Step (1): Modification step> In step (1), a cellulosic raw material is modified to obtain modified cellulose.

[0010] (Cellulosic raw materials) The cellulosic raw material, which is the raw material of the modified cellulose microfibrils, is not particularly limited as long as it is a pulp containing cellulose. Examples of the cellulosic raw material include those derived from plants, animals (e.g., ascidians), algae, microorganisms (e.g., acetic acid bacteria (Acetobacter)), and microbial products. Examples of the cellulosic raw material derived from plants include wood, bamboo, hemp, jute, kenaf, agricultural waste, cloth, and pulp (e.g., softwood unbleached kraft pulp (NUKP), softwood bleached kraft pulp (NBKP), hardwood unbleached kraft pulp (LUKP), hardwood bleached kraft pulp (LBKP), softwood unbleached sulfite pulp (NUSP), softwood bleached sulfite pulp (NBSP), thermomechanical pulp (TMP), softwood dissolving pulp, hardwood dissolving pulp, recycled pulp, and waste paper). The cellulosic raw material may be any one of these, or a combination of two or more of them. Preferably, the cellulosic raw material is derived from a plant or a microorganism, more preferably, the cellulosic raw material is derived from a plant, and further preferably, pulp (eg, wood-based pulp).

[0011] The cellulose-based raw material preferably has a high cellulose I type crystallinity, more preferably 60% or more, and even more preferably 70% or more, so that the cellulose I type crystallinity of the modified cellulose microfibrils can be maintained at 50% or more.

[0012] Cellulosic raw materials usually contain cellulose fibers. In this specification, cellulose fibers means fibrous cellulose before or after chemical modification, unless otherwise specified. Cellulosic raw materials may contain fiber components other than cellulose. The average fiber diameter of the cellulose fibers is not particularly limited, but an example is as follows. The average fiber diameter of the cellulose fibers of a cellulosic raw material derived from softwood kraft pulp is usually about 30 to 60 μm, and the average fiber diameter of the cellulose fibers of a cellulosic raw material derived from hardwood kraft pulp is usually about 10 to 30 μm. The average fiber diameter of the cellulose fibers of a cellulosic raw material derived from a pulp (other than softwood kraft pulp and hardwood kraft pulp) that has undergone general refinement is usually about 50 μm.

[0013] (chemical modification) In step (1), the cellulosic raw material is subjected to a modification treatment (usually chemical modification), resulting in modified cellulose. In this specification, modification usually refers to chemical modification, and chemical modification means chemical modification, usually meaning chemical modification of the hydroxyl groups of the glucose units of cellulose. Cellulose is composed of glucose units, and has three hydroxyl groups per glucose unit. Examples of chemical modifications include oxidation, etherification, esterification such as phosphate esterification, silane coupling, fluorination, and cationization. Among these, oxidation (carboxylation), etherification (e.g., carboxyalkylation), cationization, and esterification are preferred, and oxidation (carboxylation) and carboxyalkylation are more preferred.

[0014] (Oxidation treatment (carboxylation treatment)) The oxidation treatment usually results in modification of at least one of the hydroxyl groups originally contained in cellulose to a carboxyl group, and preferably at least one of the hydroxyl groups bonded to the carbon atom at position 6 of the glucopyranose ring to a carboxyl group.

[0015] The oxidation method in the oxidation treatment is not particularly limited, but for example, a method of oxidizing a cellulose-based raw material in water using an oxidizing agent in the presence of at least one of an N-oxyl compound, a bromide, and an iodide is exemplified. According to this method, a carbon atom having a primary hydroxyl group bonded to the carbon atom at the 6-position of the glucopyranose ring on the surface of the cellulose is selectively oxidized to generate a group selected from the group consisting of an aldehyde group, a carboxyl group, and a carboxylate group. The concentration of the cellulose-based raw material during the reaction is preferably 5% by mass or less, but is not particularly limited.

[0016] The N-oxyl compound refers to a compound capable of generating a nitroxy radical. The use of the N-oxyl compound can promote the target oxidation reaction. Examples of the N-oxyl compound include, but are not limited to, 2,2,6,6-tetramethyl-1-piperidine-N-oxy radical (hereinafter also referred to as "TEMPO") and its derivatives (e.g., 4-hydroxy-2,2,6,6-tetramethyl-1-piperidine-N-oxy radical: hereinafter also referred to as "4-hydroxyTEMPO").

[0017] The amount of the N-oxyl compound used may be an amount that catalyzes the oxidation reaction of the raw cellulose. For example, the amount is preferably 0.01 mmol or more, more preferably 0.05 mmol or more, per 1 g of bone-dry cellulose. The upper limit is preferably 10 mmol or less, more preferably 1 mmol or less, and even more preferably 0.5 mmol or less. Therefore, the amount of the N-oxyl compound used is preferably 0.01 to 10 mmol, more preferably 0.01 to 1 mmol, and even more preferably 0.05 to 0.5 mmol, per 1 g of bone-dry cellulose. The amount of the N-oxyl compound used in the reaction system is usually about 0.1 to 4 mmol / L.

[0018] Bromides are compounds containing bromine, such as alkali metal bromides that can be dissociated and ionized in water. Iodides are compounds containing iodine, such as alkali metal iodides. The amount of bromide or iodide used is not particularly limited and can be selected within a range that can promote the oxidation reaction. The total amount of bromide and iodide is preferably 0.1 mmol or more, more preferably 0.5 mmol or more, per 1 g of bone dry cellulose. The upper limit of the amount is preferably 100 mmol or less, more preferably 10 mmol or less, and even more preferably 5 mmol or less. Therefore, the total amount of bromide and iodide is preferably 0.1 to 100 mmol, more preferably 0.1 to 10 mmol, and even more preferably 0.5 to 5 mmol, per 1 g of bone dry cellulose.

[0019] The oxidizing agent is not particularly limited, and examples thereof include halogen, hypohalous acid, perhalogen acid, their salts, halogen oxides, and peroxides. Among them, hypohalous acid or its salts are preferred because they are inexpensive and have a low environmental impact, hypochlorous acid or its salts are more preferred, and sodium hypochlorite is even more preferred. The amount of the oxidizing agent used is preferably 0.5 mmol or more per 1 g of bone-dry cellulose, more preferably 1 mmol or more, and even more preferably 3 mmol or more. The upper limit of the amount is preferably 500 mmol or less, more preferably 50 mmol or less, even more preferably 25 mmol or less, and even more preferably 10 mmol or less. Therefore, the amount of the oxidizing agent used is preferably 0.5 to 500 mmol, more preferably 0.5 to 50 mmol, more preferably 1 to 25 mmol, and even more preferably 3 to 10 mmol, per 1 g of bone-dry cellulose. When an N-oxyl compound is used, the amount of the oxidizing agent used is preferably 1 mol or more per 1 mol of the N-oxyl compound, and the upper limit is preferably 40 mol or less. Therefore, the amount of the oxidizing agent used per 1 mol of the N-oxyl compound is preferably 1 to 40 mol.

[0020] Conditions such as pH and temperature during the oxidation reaction are not particularly limited. In general, the oxidation reaction proceeds efficiently even under relatively mild conditions. The reaction temperature is preferably 4°C or higher, more preferably 15°C or higher. The upper limit of the temperature is preferably 40°C or lower, more preferably 30°C or lower. Therefore, the reaction temperature is preferably 4 to 40°C, and may be about 15 to 30°C, that is, room temperature. The pH of the reaction solution is preferably 8 or higher, more preferably 10 or higher. The upper limit of the pH is preferably 12 or lower, more preferably 11 or lower. Therefore, the pH of the reaction solution is preferably 8 to 12, more preferably about 10 to 11. Usually, as the oxidation reaction proceeds, carboxyl groups are generated in the cellulose, so that the pH of the reaction solution tends to decrease. Therefore, in order to efficiently proceed with the oxidation reaction, it is preferable to add an alkaline solution such as an aqueous sodium hydroxide solution to maintain the pH of the reaction solution within the above range. The reaction medium during the oxidation is preferably water for reasons such as ease of handling and the fact that side reactions are unlikely to occur. The reaction time in the oxidation can be appropriately set according to the degree of progress of the oxidation, and is usually 0.5 hours or more, with the upper limit usually being 6 hours or less, preferably 4 hours or less. Therefore, the reaction time in the oxidation is usually about 0.5 to 6 hours, preferably about 0.5 to 4 hours.

[0021] The oxidation may be carried out in two or more separate reaction stages. For example, the oxidized cellulose obtained by filtering after the completion of the first reaction stage can be oxidized again under the same or different reaction conditions, allowing efficient oxidation without reaction inhibition by table salt produced as a by-product in the first reaction stage.

[0022] Another example of oxidation is ozone oxidation, which oxidizes at least the 2- and 6-hydroxyl groups of the glucopyranose ring that constitutes cellulose, and decomposes the cellulose chain.

[0023] Ozone treatment is usually carried out by contacting a gas containing ozone with the cellulosic raw material. The ozone concentration in the gas is 50 g / m 3 More than 250 g / m is preferable. 3 Less than 220 g / m is preferred.3 Therefore, the ozone concentration in the gas is preferably 50 to 250 g / m or less. 3 is preferable, and 50 to 220 g / m 3 More preferably, the amount of ozone added is 0.1 parts by mass or more, more preferably 5 parts by mass or more, relative to 100 parts by mass of the solid content of the cellulose-based raw material. The upper limit of the amount of ozone added is usually 30 parts by mass or less. Therefore, the amount of ozone added is preferably 0.1 to 30 parts by mass, more preferably 5 to 30 parts by mass, relative to 100 parts by mass of the solid content of the cellulose-based raw material. The ozone treatment temperature is usually 0°C or more, preferably 20°C or more, and the upper limit is usually 50°C or less. Therefore, the ozone treatment temperature is preferably 0 to 50°C, more preferably 20 to 50°C. The ozone treatment time is usually 1 minute or more, preferably 30 minutes or more, and the upper limit is usually 360 minutes or less. Therefore, the ozone treatment time is usually about 1 to 360 minutes, and preferably about 30 to 360 minutes. When the ozone treatment conditions are within the above-mentioned ranges, it is possible to prevent cellulose from being excessively oxidized and decomposed, and the yield of oxidized cellulose can be improved.

[0024] The cellulose treated with ozone may be further subjected to a post-oxidation treatment using an oxidizing agent. The oxidizing agent used in the post-oxidation treatment is not particularly limited, and examples thereof include chlorine compounds such as chlorine dioxide and sodium chlorite, oxygen, hydrogen peroxide, persulfuric acid, and peracetic acid. Examples of the method of the post-oxidation treatment include a method in which an oxidizing agent is dissolved in a polar organic solvent such as water or alcohol to prepare an oxidizing agent solution, and a cellulose-based raw material is immersed in the oxidizing agent solution. The amount of carboxyl groups, carboxylate groups, and aldehyde groups contained in the oxidized cellulose can be adjusted by controlling the oxidation conditions such as the amount of oxidizing agent added and the reaction time.

[0025] (salt and acid forms) When cellulose is oxidized, the hydroxyl groups of the cellulose are modified to carboxyl groups, and the cellulose fibers after oxidation usually have a group represented by -COOH (acid type carboxyl group) and a group represented by -COO -The counter cation of the salt-type carboxyl group is not particularly limited, and examples thereof include alkali metal ions such as sodium ion and potassium ion, and other metal ions.

[0026] The amount of carboxyl groups in oxidized cellulose is preferably 0.1 mmol / g or more, 0.3 mmol / g or more, or 0.5 mmol / g or more, more preferably 0.6 mmol / g or more, and even more preferably 1.0 mmol / g or more, based on the bone dry mass. The upper limit is preferably 2.5 mmol / g or less, more preferably 2.0 mmol / g or less, or 1.5 mmol / g or less. Therefore, 0.1 to 2.5 mmol / g, 0.3 to 2.5 mmol / g, or 0.5 to 2.5 mmol / g is preferred, 0.6 to 2.5 mmol / g is more preferred, and 1.0 to 2.0 mmol / g is even more preferred. The amount of carboxyl groups in oxidized cellulose microfibrils is usually the same as that of oxidized cellulose before fibrillation. The amount of carboxyl groups can be calculated from the change in electrical conductivity.

[0027] The degree of carboxy substitution per anhydrous glucose unit of oxidized cellulose is preferably 0.01 or more, 0.02 or more, or 0.05 or more, more preferably 0.10 or more, even more preferably 0.15 or more, even more preferably 0.20 or more, and particularly preferably 0.25 or more. This ensures a degree of substitution for obtaining the effect of chemical modification. The upper limit of the degree of substitution is preferably 0.50 or less, more preferably 0.40 or less, or 0.35 or less. This makes it difficult for the cellulose fiber to dissolve in water, and allows the fiber form to be maintained in water. Therefore, the degree of carboxy substitution is preferably 0.01 to 0.50, more preferably 0.05 to 0.40, and even more preferably 0.10 to 0.35. The degree of carboxy substitution of oxidized cellulose microfibrils is usually the same as that of oxidized cellulose before fibrillation. The degree of carboxy substitution can be adjusted by reaction conditions. The degree of carboxy substitution per anhydroglucose unit is the ratio of hydroxyl groups originally possessed by each anhydroglucose (glucose residue) constituting cellulose that have been substituted with carboxyl groups (the number of carboxyl groups per glucose residue). The degree of carboxy substitution can be calculated from the amount of carboxyl groups.

[0028] (Acid-oxidized cellulose and desalting) Oxidized cellulose contains carboxyl groups as a result of oxidation, but may contain more acid-type carboxyl groups than salt-type carboxyl groups, or may contain more salt-type carboxyl groups than acid-type carboxyl groups. Oxidized cellulose may further be subjected to a desalting treatment, which converts salt-type carboxyl groups to acid-type carboxyl groups. In this specification, the term "acid type" indicates that the cellulose has been desalted, and the term "salt type" indicates that the cellulose has not been desalted. The proportion of acid-type carboxyl groups among the carboxyl groups in acid-type cellulose is preferably 40% or more, more preferably 60% or more, and even more preferably 85% or more. The proportion of acid-type carboxyl groups can be calculated by the following procedure. 1) First, 250 mL of an aqueous dispersion of acid-type oxidized cellulose before desalting treatment with a solids concentration of 0.1% by mass is prepared. A 0.1 M aqueous hydrochloric acid solution is added to the prepared aqueous dispersion to adjust the pH to 2.5, and then a 0.1 N aqueous sodium hydroxide solution is added and the electrical conductivity is measured until the pH reaches 11. The amount of acid-type carboxyl groups and the amount of salt-type carboxyl groups, i.e., the total amount of carboxyl groups, is calculated using the following formula from the amount of sodium hydroxide (a) consumed in the neutralization stage of the weak acid, where the change in electrical conductivity is gradual: Total amount of carboxyl groups (mmol / g oxidized cellulose (salt type)) = a (ml) × 0.1 / mass of oxidized cellulose (salt type) (g) 2) Prepare 250 mL of an aqueous dispersion of desalted acid-type oxidized cellulose with a solids concentration of 0.1% by mass. Add 0.1 N aqueous sodium hydroxide solution to the prepared aqueous dispersion, and measure the electrical conductivity until the pH reaches 11. Calculate the amount of acid-type carboxyl groups from the amount of sodium hydroxide (b) consumed in the neutralization stage of the weak acid, where the change in electrical conductivity is gradual, using the following formula: Amount of acid-type carboxyl groups (mmol / g acid-type oxidized cellulose) = b (ml) × 0.1 / mass of acid-type oxidized cellulose (g) 3) Calculate the proportion of acid-type carboxyl groups from the calculated total amount of carboxyl groups and the amount of acid-type carboxyl groups using the following formula. Proportion of acid-type carboxyl groups (%) = (amount of acid-type carboxyl groups / total amount of carboxyl groups) x 100

[0029] The timing of desalting may be after oxidation, and may be either before or after defibration (before or after step (2)), but is usually after oxidation, and preferably before step (2). Desalting is usually carried out by substituting salts (e.g., sodium salts) contained in the salt-type oxidized cellulose with protons. Examples of desalting methods include a method of adjusting the system to be acidic, and a method of contacting oxidized cellulose with a cation exchange resin. In the method of adjusting the system to be acidic, the pH of the system is preferably adjusted to 2 to 6, more preferably 2 to 5, and even more preferably 2.3 to 5. To adjust the system to be acidic, an acid (e.g., inorganic acids such as sulfuric acid, hydrochloric acid, nitric acid, sulfurous acid, nitrous acid, and phosphoric acid; organic acids such as acetic acid, lactic acid, oxalic acid, citric acid, and formic acid) is usually used. After the addition of the acid, a washing treatment may be carried out as appropriate. The cation exchange resin has a counter ion of H + As long as the cation exchange resin is strong acidic or weak acidic, both can be used. The ratio of the oxidized cellulose and the cation exchange resin when contacting them is not particularly limited, and can be appropriately set by a person skilled in the art from the viewpoint of efficient proton replacement. The cation exchange resin after contact can be recovered by a conventional method such as suction filtration.

[0030] (Etherification (e.g., carboxyalkylation)) Examples of the etherification include etherification by a reaction selected from carboxyalkylation, methylation, ethylation, cyanoethylation, hydroxyethylation, hydroxypropylation, ethylhydroxyethylation, and hydroxypropylmethylation, with carboxyalkylation being preferred and carboxymethylation being more preferred.

[0031] The modified cellulose (carboxyalkylated cellulose) obtained through carboxyalkylation preferably has a structure in which at least one of the hydroxyl groups of cellulose is carboxyalkylated. The degree of carboxyalkyl substitution (DS, preferably the degree of carboxymethyl substitution) per anhydrous glucose unit of the carboxyalkylated cellulose is preferably 0.01 or more, 0.02 or more, or 0.05 or more, more preferably 0.10 or more, even more preferably 0.15 or more, even more preferably 0.20 or more, and particularly preferably 0.25 or more. This ensures a degree of substitution for obtaining the effect of chemical modification. The upper limit of the degree of substitution is preferably 0.50 or less, more preferably 0.40 or less, or 0.35 or less. This makes it difficult for the cellulose fiber to dissolve in water, and allows the fiber form to be maintained in water. Therefore, the degree of carboxyalkyl substitution is preferably 0.01 to 0.50, more preferably 0.05 to 0.40, and even more preferably 0.10 to 0.35 or 0.20 to 0.35. The degree of carboxyalkyl substitution of the carboxyalkylated cellulose microfibril is usually the same as that of the carboxyalkylated cellulose before fibrillation. The degree of carboxyalkyl substitution can be adjusted by controlling any one of the amount of the carboxyalkylating agent to be reacted, the amount of the mercerizing agent, and the composition ratio of water and the organic solvent.

[0032] The degree of carboxyalkyl substitution (also called the degree of etherification) per anhydroglucose unit is the ratio of hydroxyl groups originally possessed by each anhydroglucose (glucose residue) constituting cellulose that have been substituted with carboxyalkyl ether groups (the number of carboxyalkyl ether groups per glucose residue). The degree of carboxyalkyl substitution can be calculated from the amount of carboxyalkyl groups.

[0033] The amount of carboxyl groups in the carboxyalkylated cellulose is preferably 0.1 mmol / g or more, more preferably 0.6 mmol / g or more, and even more preferably 1.0 mmol / g or more, based on the bone dry mass. The upper limit is preferably 2.5 mmol / g or less, more preferably 2.0 mmol / g or less. Therefore, it is preferably 0.1 to 2.5 mmol / g, more preferably 0.6 to 2.5 mmol / g, and even more preferably 1.0 to 2.0 mmol / g. The amount of carboxyl groups in the carboxyalkylated cellulose microfibril is usually the same as that of the carboxyalkylated cellulose before fibrillation. The amount of carboxyl groups can be calculated from the change in electrical conductivity.

[0034] The carboxyalkylation method includes, for example, a method in which the cellulosic starting material is mercerized and then etherified. Carboxymethylation will be taken as an example below.

[0035] Mercerization is usually carried out by mixing a cellulose-based raw material, a solvent and a mercerizing agent. An example of the reaction conditions is as follows. The reaction temperature is usually 0°C or higher, preferably 10°C or higher, and the upper limit is usually 70°C or lower, preferably 60°C or lower. Therefore, the reaction temperature is usually 0 to 70°C, preferably 10 to 60°C. The reaction time is usually 15 minutes or more, preferably 30 minutes or more. The upper limit of the time is usually 8 hours or less, preferably 7 hours or less. Therefore, the reaction time is usually 15 minutes to 8 hours, preferably 30 minutes to 7 hours.

[0036] Examples of the solvent include water, organic solvents (e.g., alcohols (e.g., lower alcohols), ketones, dioxane, diethyl ether, benzene, dichloromethane), and mixed solvents thereof. Examples of the lower alcohols include methanol, ethanol, N-propyl alcohol, isopropyl alcohol, N-butyl alcohol, isobutyl alcohol, and tertiary butyl alcohol. Among these, monohydric alcohols having 1 to 4 carbon atoms are preferred, and monohydric alcohols having 1 to 3 carbon atoms are more preferred, because they have good compatibility with water. Examples of the ketones include acetone, diethyl ketone, and methyl ethyl ketone. The mixing ratio of the lower alcohol in the mixed solvent is preferably 60 to 95% by mass. The amount of the solvent is usually 3 times or more by mass relative to the cellulosic raw material. The upper limit of the amount is not particularly limited, but is usually 20 times or less by mass. Therefore, the amount of the solvent is preferably 3 to 20 times by mass.

[0037] Examples of the mercerizing agent include alkali metal hydroxides such as sodium hydroxide and potassium hydroxide. The amount of the mercerizing agent used is preferably 0.5 times or more by mole, more preferably 1.0 times or more by mole, and even more preferably 1.5 times or more by mole, per anhydrous glucose residue of the starting material. The upper limit of the amount is usually 20 times or less by mole, preferably 10 times or less by mole, and even more preferably 5 times or less by mole. Therefore, the amount of the mercerizing agent used is preferably 0.5 to 20 times by mole, more preferably 1.0 to 10 times by mole, and even more preferably 1.5 to 5 times by mole.

[0038] The etherification reaction is usually carried out by adding an etherification agent (e.g., a carboxymethylation agent) to the reaction system after mercerization. The following will be explained taking carboxymethylation as an example. Examples of the carboxymethylation agent include monochloroacetic acid, sodium monochloroacetate, methyl monochloroacetate, ethyl monochloroacetate, and isopropyl monochloroacetate, and monochloroacetic acid and sodium monochloroacetate are preferred. The amount of the carboxymethylation agent used is usually 0.05 times or more by mole, or 0.5 times or more by mole, preferably 0.6 times or more by mole, and more preferably 0.7 times or more by mole, or 0.8 times or more by mole, per anhydrous glucose residue of cellulose contained in the cellulosic raw material. The upper limit of the amount is usually 10.0 times or less by mole, 5 times or less by mole, 3 times or less by mole, or 1.5 times or less by mole, preferably 1.3 times or less by mole, and more preferably 1.1 times or less by mole, and therefore the amount is preferably 0.05 to 10.0 times by mole, more preferably 0.5 to 5 times by mole, and even more preferably 0.8 to 3 times by mole. The carboxymethylating agent can be added to the reaction system as it is or in the form of an aqueous solution. The concentration of the aqueous solution of the carboxymethylating agent is usually 5 to 80% by mass, more preferably 30 to 60% by mass.

[0039] The reaction temperature for etherification is usually 30°C or higher, preferably 40°C or higher, and the upper limit is usually 90°C or lower, preferably 80°C or lower. Therefore, the reaction temperature is usually 30 to 90°C, preferably 40 to 80°C. The reaction time is usually 30 minutes or more, preferably 1 hour or more, and the upper limit is usually 10 hours or less, preferably 4 hours or less. Therefore, the reaction time is usually 30 minutes to 10 hours, preferably 1 hour to 4 hours. The reaction liquid may be stirred during the carboxymethylation reaction as necessary. The molar ratio of the mercerizing agent to the carboxymethylating agent (mercerizing agent / carboxymethylating agent) is preferably 0.90 or more when monochloroacetic acid or sodium monochloroacetate is used as the carboxymethylating agent. This allows the carboxymethylation reaction to proceed sufficiently, and the remaining unreacted monochloroacetic acid or sodium monochloroacetate can be suppressed. The upper limit is preferably 2.45 or less. This prevents the mercerizing agent from becoming excessive, suppresses the progress of side reactions caused by the mercerizing agent and monochloroacetic acid or sodium monochloroacetate, suppresses the production of glycolic acid alkali metal salt, and allows the reaction to proceed economically. Therefore, the molar ratio of the mercerizing agent to the carboxymethylating agent is generally 0.90 to 2.45.

[0040] Examples of methods for carboxymethylation include (Method 1) an aqueous medium method (a method in which both mercerization and carboxymethylation are carried out in a solvent mainly composed of water), (Method 2) a solvent method (a method in which both mercerization and carboxymethylation are carried out in a mixed solvent of water and an organic solvent), and (Method 3) a method in which a solvent mainly composed of water is used for mercerization and a mixed solvent of an organic solvent and water is used for carboxymethylation, with Method 3 being preferred. This allows carboxymethylated cellulose to be economically obtained in which the crystallinity of the cellulose is 50% or more and the carboxymethyl groups can be introduced uniformly rather than locally while maintaining the effective utilization rate of the carboxymethylating agent, and the absolute value of the degree of anionization is small.

[0041] The water content in the water-based solvent is usually more than 50% by mass, preferably 55% by mass or more, 60% by mass or more, 70% by mass or more, or 80% by mass or more, more preferably 90% by mass or more, even more preferably 95% by mass or more, and even more preferably 100% by mass. This allows the carboxymethyl group to be introduced more uniformly into the cellulose. The water-based solvent may contain a solvent other than water (e.g., the organic solvent described above). The amount of the solvent other than water is usually 45% by mass or less, preferably 40% by mass or less, 30% by mass or less, 20% by mass or less, or 10% by mass or less, more preferably 5% by mass or less, and even more preferably 0% by mass. The solvent may be prepared by preparing a predetermined amount of water and, if necessary, a solvent other than water, and mixing them.

[0042] The water content of the solvents used in the mercerization reaction and the carboxymethylation reaction is preferably less in the latter (the organic solvent content is greater in the latter) (not including the water content of cellulose). This makes it easier to maintain the crystallinity of the resulting carboxymethylated cellulose, and allows the desired modified cellulose microfibrils to be obtained efficiently. For this reason, it is preferable to add an organic solvent or an aqueous solution of an organic solvent to the reaction system between the end of the mercerization reaction and immediately after the addition of the carboxymethylating agent, or to reduce the amount of solvent other than water during the mercerization treatment (e.g., reduced pressure treatment) to form a mixed solvent of water and an organic solvent. Of these, the former is more preferable. This allows the carboxymethylation reaction to proceed efficiently by a simple means. The timing of adding or reducing the organic solvent is preferably within 30 minutes before or after the addition of the carboxymethylating agent.

[0043] The ratio of the organic solvent in the mixed solvent for carboxymethylation is preferably 20% by mass or more or 30% by mass or more, more preferably 40% by mass or more, even more preferably 45% by mass or more, and even more preferably 50% by mass or more, based on the total of water and organic solvent. This makes it easier for the substitution of carboxymethyl groups to occur uniformly, and carboxymethylated cellulose with stable quality can be obtained. The upper limit is usually 99% by mass or less, and considering the cost of the organic solvent, it is preferably 90% by mass or less, more preferably 85% by mass or less, even more preferably 80% by mass or less, and even more preferably 70% by mass or less.

[0044] The effective utilization rate (AM) of the carboxymethylating agent is preferably 15% or more, more preferably 20% or more, even more preferably 25% or more, and even more preferably 30% or more. The upper limit is not particularly limited and is substantially 80% or less. The effective utilization rate of the carboxymethylating agent means the ratio of the amount of carboxymethyl groups introduced into cellulose to the amount of carboxymethyl groups possessed by the carboxymethylating agent, and can be calculated by the following formula: AM = (DS × moles of cellulose) / moles of carboxymethylating agent DS: Degree of carboxymethyl substitution Moles of cellulose = mass of pulp / 162 The pulp mass means the dry mass when dried at 100° C. for 60 minutes, and 162 means the molecular weight per glucose unit of cellulose.

[0045] (Acid-type carboxyalkylated cellulose) The carboxyalkylated cellulose may contain more acid-type carboxyl groups than salt-type carboxyl groups, or may contain more salt-type carboxyl groups than acid-type carboxyl groups. The carboxyalkylated cellulose may further be subjected to a desalting treatment. This allows the salt-type carboxyl groups to be converted into acid-type carboxyl groups. The ratio of the amount of acid-type carboxyl groups to the amount of carboxyl groups in the acid-type carboxyalkylated cellulose is preferably 40% or more, more preferably 60% or more, and even more preferably 85% or more. The method for calculating the ratio of acid-type carboxyl groups is as described above.

[0046] The desalting is usually carried out after carboxyalkylation, preferably after etherification and before fibrillation. For example, the desalting method may be a method of contacting the carboxyalkylated cellulose with a cation exchange resin. The cation exchange resin is a cation exchange resin having a counter ion of H + As long as the cation exchange resin is strong acidic or weak acidic, both of them can be used. The ratio of the carboxyalkylated cellulose and the cation exchange resin when contacting them is not particularly limited, and a person skilled in the art can appropriately set it from the viewpoint of efficient proton replacement. As an example, the ratio can be adjusted so that the pH of the aqueous dispersion after adding the cation exchange resin to the carboxyalkylated cellulose aqueous dispersion is preferably 2 to 6, more preferably 2 to 5. The cation exchange resin after contact can be recovered by a conventional method such as suction filtration.

[0047] (Esterification (e.g., phosphate esterification)) As an example of the esterification, there is a method (phosphorylation) in which a compound having a phosphoric acid group is reacted with a cellulosic raw material. As a method of phosphate esterification, there is a method in which a powder or an aqueous solution of a compound having a phosphoric acid group is mixed with a cellulosic raw material, and a method in which an aqueous solution of a compound having a phosphoric acid group is added to an aqueous dispersion of a cellulosic raw material, and the latter is preferred. This can increase the uniformity of the reaction and the efficiency of esterification.

[0048] Examples of compounds having a phosphate group include phosphoric acid, polyphosphoric acid, phosphorous acid, phosphonic acid, polyphosphonic acid, esters thereof, and salts thereof. More specifically, examples include phosphoric acid, sodium dihydrogen phosphate, disodium hydrogen phosphate, trisodium phosphate, sodium pyrophosphate, sodium metaphosphate, potassium dihydrogen phosphate, dipotassium hydrogen phosphate, tripotassium phosphate, potassium pyrophosphate, potassium metaphosphate, ammonium dihydrogen phosphate, diammonium hydrogen phosphate, triammonium phosphate, ammonium pyrophosphate, and ammonium metaphosphate. These are low cost and easy to handle, and can be used to introduce phosphate groups into cellulose to improve defibration efficiency. The compound having a phosphate group may be one type or a combination of two or more types. Among these, from the viewpoints of high efficiency of introduction of phosphate groups, easy fibrillation, and easy industrial application, phosphoric acid, sodium salts of phosphoric acid, potassium salts of phosphoric acid, and ammonium salts of phosphoric acid are preferred, sodium salts of phosphoric acid are more preferred, and sodium dihydrogen phosphate and disodium hydrogen phosphate are even more preferred. It is preferable to use an aqueous solution of a compound having a phosphate group in the esterification because it increases the uniformity of the reaction and increases the efficiency of introduction of the phosphate group. The pH of the aqueous solution of the compound having a phosphate group is preferably 7 or less since this increases the efficiency of introducing the phosphate group, and more preferably 3 to 7 since this also suppresses hydrolysis of the fibers.

[0049] The phosphoric acid esterification method will be described below by taking an example. A compound having a phosphoric acid group is added to a suspension of a cellulose-based raw material (for example, a solid content concentration of 0.1 to 10% by mass) while stirring, and a phosphoric acid group is introduced into the cellulose. When the cellulose-based raw material is 100 parts by mass, the amount of the compound having a phosphoric acid group added is preferably 0.2 parts by mass or more, more preferably 1 part by mass or more, in terms of the amount of phosphorus atoms. This can further improve the yield of the esterified cellulose. The upper limit is preferably 500 parts by mass or less, more preferably 400 parts by mass or less. This can efficiently obtain a yield that corresponds to the amount of the compound having a phosphoric acid group used. Therefore, 0.2 to 500 parts by mass is preferable, and 1 to 400 parts by mass is more preferable.

[0050] When reacting the cellulosic raw material with the compound having a phosphoric acid group, a basic compound may be further added to the reaction system. Examples of a method for adding the basic compound to the reaction system include a method of adding the basic compound to an aqueous dispersion of the cellulosic raw material, an aqueous solution of the compound having a phosphoric acid group, or an aqueous dispersion of the cellulosic raw material and the compound having a phosphoric acid group.

[0051] The basic compound is not particularly limited, but preferably exhibits basicity, and more preferably is a nitrogen-containing compound exhibiting basicity. "Exhibits basicity" usually means that an aqueous solution of the basic compound exhibits pink to red color in the presence of a phenolphthalein indicator and / or the pH of the aqueous solution of the basic compound is greater than 7. The basic compound is preferably a compound having a nitrogen atom exhibiting basicity, and more preferably a compound having an amino group exhibiting basicity. Examples of compounds having an amino group exhibiting basicity include urea, methylamine, ethylamine, trimethylamine, triethylamine, monoethanolamine, diethanolamine, triethanolamine, pyridine, ethylenediamine, and hexamethylenediamine. Among these, urea is preferred in terms of low cost and ease of handling. The amount of the basic compound added is preferably 2 to 1000 parts by mass, more preferably 100 to 700 parts by mass. The reaction temperature is preferably 0 to 95°C, more preferably 30 to 90°C. The reaction time is not particularly limited, but is usually about 1 to 600 minutes, and preferably 30 to 480 minutes. When the esterification reaction conditions are within any of these ranges, it is possible to prevent the cellulose from being excessively esterified and becoming easily soluble, and it is possible to improve the yield of phosphated cellulose.

[0052] After reacting the cellulosic raw material with a compound having a phosphoric acid group, a suspension of cellulose phosphate is obtained. The suspension of cellulose phosphate may be dehydrated as necessary. It is preferable to carry out a heat treatment after dehydration, which can suppress hydrolysis of cellulose. The heating temperature is preferably 100 to 170°C. It is more preferable to heat the mixture at 130°C or less (preferably 110°C or less) while it contains water during the heat treatment, and then heat the mixture at 100 to 170°C after removing the water.

[0053] The degree of phosphate substitution per glucose unit of the phosphated cellulose is preferably 0.001 or more. This allows sufficient fibrillation to be performed. The upper limit is preferably less than 0.40. This allows the swelling or dissolution of the phosphated cellulose to be suppressed. Therefore, the degree of phosphate substitution is preferably 0.001 or more and less than 0.40. By the phosphate esterification reaction, a phosphate group substituent is introduced into the cellulose, and the cellulose particles repel each other electrically. Therefore, the phosphated cellulose can be easily fibrillated. After the phosphate esterification, it is preferable to perform a washing treatment such as boiling and washing with cold water. This allows efficient fibrillation.

[0054] <Step (2): Defibration (fibrillation) step> In step (2), the modified cellulose obtained in step (1) is mechanically treated and defibrated under conditions of pH 7 or less and a solid content concentration of 0.1 to 15% by mass. This produces modified cellulose microfibrils. Defibrillation (fibrillation) is usually achieved by a mechanical treatment, which is preferably a defibration or beating treatment. The mechanical treatment (preferably beating or defibration treatment) is usually carried out in a wet manner (i.e., in the form of an aqueous dispersion). Examples of equipment used for mechanical treatment include equipment capable of imparting mechanical defibration force, such as refiners (e.g., disk type, conical type, cylindrical type), high-speed defibrators, shear-type agitators, colloid mills, high-pressure jet dispersers, beaters, PFI mills, kneaders, dispersers, high-speed disintegrators (top finers), high-pressure or ultra-high-pressure homogenizers, grinders (stone-type grinders), ball mills, vibration mills, bead mills, single-axis, twin-axis, or multi-axis kneaders / extruders (homogenizers under high-speed rotation), refiners, defibrators, friction grinders, high-share defibrators, dispergers, and homogenizers (e.g., microfluidizers), among which equipment capable of imparting defibration force in a wet manner is preferred, and high-speed disintegrators and refiners are more preferred, but are not particularly limited.

[0055] When defibration is performed in a wet manner, the modified cellulose obtained in step (1) is usually dispersed in water to prepare an aqueous dispersion, and the aqueous dispersion is subjected to mechanical treatment. The solid content concentration of the modified cellulose in the aqueous dispersion obtained in step (1) is preferably 0.1% by mass or more, more preferably 0.5% by mass or more, even more preferably 1.0% by mass or more, and even more preferably 1.5% by mass or more. The upper limit of the concentration is preferably 15% by mass or less, more preferably 10% by mass or less, and even more preferably 8% by mass or less. The pH during mechanical treatment is preferably 7 or less, more preferably 6 or less, and even more preferably 5 or less. In the past, from the viewpoint of improving defibration, a pH adjuster such as an alkali was added before the mechanical treatment to adjust the pH to more than 7, but in the present invention, it has been found that the desired microfibrils can be obtained by adjusting the pH to 7 or less. The lower limit of the pH is not particularly limited, but is usually 2 or more, preferably 3 or more, and more preferably 3.5 or more. The pH can be adjusted, for example, by adding a pH adjuster such as an acid (e.g., hydrochloric acid) or an alkali (e.g., sodium hydroxide, sodium bicarbonate) to the aqueous dispersion. Prior to the preparation of the aqueous dispersion, a pretreatment such as dry pulverization of the chemically modified cellulose (e.g., pulverization after drying) may be performed. Examples of the apparatus used for dry pulverization include, but are not limited to, impact mills such as hammer mills and pin mills, media mills such as ball mills and tower mills, and jet mills. Treatments for adjusting the pH and solid content concentration may be appropriately performed after the end of step (1), but if the pH and solid content concentration are already within the above ranges at the end of step (1) (preferably during the washing treatment performed after modification as necessary), the adjustments can be omitted.

[0056] The defibration conditions can be appropriately selected so that the average fiber diameter, average fiber length, and aspect ratio after treatment are within the ranges described below. As a result, the resulting modified cellulose microfibrils can exhibit higher water retention than undefibrated cellulose fibers. Compared to finely defibrated cellulose nanofibers, even a small amount can exhibit high strength-improving effects and yield-improving effects. The defibration conditions can be appropriately selected so that the fibrillation rate or the difference Δf in the fibrillation rates of the samples before and after defibration is within the above-mentioned range. At the end of defibration, it is preferable to adjust the pH of the aqueous dispersion to near neutral (about 7.0, for example, 6.5 to 7.5) as necessary. The pH can be adjusted, for example, by adding the above-mentioned pH adjuster to the aqueous dispersion.

[0057] <Optional post-processing> The modified cellulose microfibrils may be used as a final product in the form of an aqueous dispersion obtained after the completion of step (2), or may be subjected to post-treatment as necessary. Examples of the post-treatment method include, but are not limited to, drying (e.g., freeze drying, spray drying, tray drying, drum drying, belt drying, thin spreading on a glass plate or the like and drying, fluidized bed drying, microwave drying, and heated fan-type reduced pressure drying), redispersion in water (the dispersion device is not limited), and pulverization (e.g., pulverization using equipment such as a cutter mill, hammer mill, pin mill, or jet mill).

[0058] <Modified cellulose microfibril> In the present invention, the modified cellulose microfibrils are usually fibrillated fibers of modified cellulose. By undergoing step (2), the specific surface area becomes larger than that before the treatment, and it is expected that the water retention and strength imparting effects will be improved. In addition, by undergoing step (1), the fibers are easily loosened during step (2), and fibrillation can be efficiently carried out with less power than in the case where modification is not performed. In addition, affinity with water is improved, and good water retention can be exhibited even if the fiber length is relatively long.

[0059] (Shape of modified cellulose microfibrils) The morphological features of modified cellulose microfibrils are as follows: Compared with modified cellulose that has not undergone fibrillation, fluffing of cellulose microfibrils is usually observed on the fiber surface; Compared with chemically modified cellulose nanofibers, finer fiber itself is usually suppressed, and fluffing (external fibrillation) on the fiber surface is efficiently achieved; Compared with fibrillated cellulose nanofibers that have not been chemically modified, water retention is good, and thixotropy is observed; The modified cellulose microfibrils are preferably fibrillated fibers of chemically modified cellulose. This allows the fibers to easily come apart during fibrillation, suppressing damage to the fibers.

[0060] (average fiber diameter, average fiber length, fiber length distribution and aspect ratio) The average fiber diameter of the modified cellulose microfibrils is usually 500 nm or more, preferably 1 μm or more, and more preferably 10 μm or more. This allows the microfibril to exhibit higher water retention than undefibrated cellulose fibers, and even a small amount of the microfibril can provide higher strength and yield improvement effects than finely defibrated cellulose nanofibers. The upper limit of the average fiber diameter is preferably 60 μm or less, more preferably 40 μm or less, even more preferably 30 μm or less, and even more preferably 20 μm or less, 18 μm or less, or 17 μm or less, but there is no particular limit.

[0061] The average fiber length is preferably 500 μm or more or 550 μm or more, more preferably 600 μm or more, 700 μm or more, or 800 μm or more. The upper limit of the average fiber length is not particularly limited, but is preferably 3,000 μm or less, preferably 2,500 μm or less, more preferably 2,000 μm or less, and even more preferably 1,500 μm or less.

[0062] The fiber length distribution preferably satisfies any one of the following, and it is more preferable that the fiber length of 0.6 to 1.2 mm satisfies the following range: The proportion of fiber lengths of 0 to 0.2 mm is preferably 50% or less, more preferably 45% or less (the lower limit is preferably 3% or more, more preferably 5% or more). The proportion of fibers with a fiber length of 0.2 to 0.6 mm is preferably 50% or less, more preferably 45% or less (the lower limit is preferably 10% or more, more preferably 15% or more). The proportion of fiber lengths of 0.6 to 1.2 mm is preferably 18% or more, more preferably 20% or more (the upper limit is preferably 45% or less, more preferably 40% or less). The proportion of fiber lengths of 1.2 to 2.0 mm is preferably 1% or more, more preferably 1.05% or more (the upper limit is preferably 50% or less, more preferably 45% or less). The proportion of fiber lengths of 2.0 to 3.2 mm is preferably 0.02% or more, more preferably 0.05% or more (the upper limit is preferably 20% or less, more preferably 15% or less). The proportion of fiber lengths between 3.2 and 7.6 mm is preferably 1.5% or less, more preferably 1% or less (the lower limit may be 0 or more).

[0063] The fiber length distribution of the oxidized cellulose microfibrils preferably satisfies any of the following: The proportion of fiber lengths of 0 to 0.2 mm is preferably 30% or less, more preferably 25% or less (the lower limit is preferably 3% or more, more preferably 5% or more). The proportion of fibers with a fiber length of 0.2 to 0.6 mm is preferably 50% or less, more preferably 45% or less (the lower limit is preferably 10% or more, more preferably 15% or more). The proportion of fiber lengths of 0.6 to 1.2 mm is preferably 20% or more, more preferably 25% or more (the upper limit is preferably 45% or less, more preferably 40% or less). The proportion of fiber lengths of 1.2 to 2.0 mm is preferably 3% or more, more preferably 5% or more (the upper limit is preferably 50% or less, more preferably 45% or less). The proportion of fiber lengths of 2.0 to 3.2 mm is preferably 1% or more, more preferably 2% or more (the upper limit is preferably 20% or less, more preferably 15% or less). The proportion of fiber lengths between 3.2 and 7.6 mm is preferably 1.5% or less, more preferably 1% or less (the lower limit may be 0 or more).

[0064] The fiber length distribution of the carboxyalkylated cellulose microfibrils preferably satisfies any one of the following: The proportion of fiber lengths of 0 to 0.2 mm is preferably 50% or less, more preferably 45% or less (the lower limit is preferably 20% or more, more preferably 30% or more). The proportion of fibers with a fiber length of 0.2 to 0.6 mm is preferably 50% or less, more preferably 45% or less (the lower limit is preferably 10% or more, more preferably 20% or more). The proportion of fiber lengths of 0.6 to 1.2 mm is preferably 15% or more, more preferably 20% or more (the upper limit is preferably 30% or less, more preferably 25% or less). The proportion of fiber lengths of 1.2 to 2.0 mm is preferably 1% or more, more preferably 1.05% or more (the upper limit is preferably 5% or less, more preferably 3% or less). The proportion of fiber lengths of 2.0 to 3.2 mm is preferably 0.01% or more, more preferably 0.04% or more (the upper limit is preferably 5% or less, more preferably 3% or less). The proportion of fiber lengths between 3.2 and 7.6 mm is preferably 1.5% or less, more preferably 1% or less (the lower limit may be 0 or more).

[0065] The average fiber diameter, average fiber length, and fiber length distribution can be determined using a fractionator (e.g., a fractionator manufactured by Valmet Co., Ltd.). When a fractionator is used, the average fiber diameter, average fiber length, and f1-f6(l)% (Fraction 1-6 percentage of length weighted distribution) can be determined, respectively.

[0066] The aspect ratio of the modified cellulose microfibrils is preferably 30 or more or 35 or more, more preferably 40 or more, even more preferably 50 or more, and even more preferably 60 or more. There is no particular upper limit to the aspect ratio, but it is preferably 1000 or less, more preferably 100 or less, and even more preferably 80 or less. The aspect ratio can be calculated by the following formula: Aspect ratio = average fiber length / average fiber diameter.

[0067] (transparency) The transparency (transmittance of 660 nm light) of the aqueous dispersion of modified cellulose microfibrils (solid content concentration of 1% by mass) is preferably less than 60%, more preferably 40% or less, even more preferably 30% or less, even more preferably 20% or less, and particularly preferably 13% or less. This ensures an appropriate degree of fibrillation, allowing the effects of the present invention to be fully achieved. The lower limit may be 0% or more, and is not particularly limited. The aqueous dispersion of modified cellulose microfibrils (solid content concentration of about 2% or more) is usually translucent to white, and is in the form of a gel, cream, or paste.

[0068] In this specification, unless otherwise specified, the aqueous dispersion of modified cellulose microfibrils means a dispersion obtained by dispersing the above-mentioned fibers in water as a dispersion medium.

[0069] (specific surface area) The BET specific surface area of ​​the modified cellulose microfibrils is preferably 30 m 2 / g or more, more preferably 40m 2 / g or more, more preferably 50m 2 / g or more. The upper limit is preferably 200m 2 / g or less, more preferably 150m 2 / g or less, more preferably 100m 2 The BET specific surface area can be measured by substituting t-BuOH for the aqueous dispersion and then freeze-drying the sample according to the nitrogen gas adsorption method (JIS Z 8830) using a BET specific surface area meter.

[0070] (Crystallization degree of cellulose type I) The crystallinity of cellulose type I in modified cellulose microfibrils is usually 50% or more, preferably 60% or more, 70% or more, or 75% or more, and more preferably 80% or more. There is no particular upper limit, but in reality it is thought to be about 90%. The crystallinity of cellulose can be controlled by the degree of chemical modification. The crystallinity of cellulose type I can be calculated by measuring and comparing the intensities of the (200) peak at around 22.6° and the valley between (200) and (110) (around 18.5°) by X-ray diffraction measurement.

[0071] (Degree of anionization) The degree of anionization (anion charge density) of the modified cellulose microfibrils is usually 2.50 meq / g or less, preferably 2.30 meq / g or less, more preferably 2.0 meq / g or less, and even more preferably 1.50 meq / g or less, 1.0 meq / g or less, 0.8 meq / g or less, or 0.5 meq / g or less. This is considered to make the chemical modification more uniform throughout the cellulose than chemically modified cellulose fibers having a higher degree of anionization, and it is considered to be possible to obtain the effects specific to chemically modified cellulose fibers, such as water retention, more stably. The lower limit is usually 0.08 meq / g or more, preferably 0.10 meq / g or more, or 0.20 meq / g or more, more preferably 0.30 meq / g or more, but is not particularly limited. Therefore, 0.08 meq / g or more and 2.50 meq / g or less are preferred. The degree of anionization is the equivalent of anion per unit mass of modified cellulose microfibril, and can be calculated from the equivalent of diallyldimethylammonium chloride (DADMAC) required to neutralize the anionic groups in unit mass of modified cellulose microfibril.

[0072] (Water retention capacity) The water retention capacity of the modified cellulose microfibrils is preferably 10 or more, more preferably 15 or more, or 18 or more, even more preferably 20 or more, and even more preferably 30 or more. The upper limit is thought to be about 200 or less in reality, but is not particularly limited. The water retention capacity corresponds to the mass of water in the sediment relative to the mass of the solid content of the fibers in the sediment, and is the ratio of the water content to the solid content in the precipitated gel, measured and calculated by centrifuging a 0.3 mass% aqueous dispersion of the fibers at 25,000 G. That is, it is calculated by the following formula: Water retention capacity=(B+C-0.003×A) / (0.003×AC) A: Mass of an aqueous dispersion of modified cellulose microfibrils having a solids concentration of 0.3% by mass B: Mass of sediment separated after centrifuging the aqueous dispersion of mass A at 30°C, 25,000G, and 30 minutes. C: Mass of solids in the aqueous phase separated after the centrifugation

[0073] The higher the water retention value, the stronger the fiber's ability to retain water. Water retention can be measured or calculated for fibers that have undergone fibrillation, but cannot usually be measured for fibers that have not undergone fibrillation or defibration, or for cellulose nanofibers that have been defibrated to single microfibrils. When cellulose fibers that have not been fibrillated or defibrated are centrifuged under the above conditions, a dense sediment cannot be formed, and it is difficult to separate the sediment from the aqueous phase. When cellulose nanofibers are centrifuged under the above conditions, they usually hardly settle.

[0074] (viscosity) When the modified cellulose microfibrils are dispersed in water, it is preferable that the viscosity of the dispersion is low. This allows the material to have good handleability despite being fibrillated. For example, the B-type viscosity (25°C, 60 rpm) of an aqueous dispersion with a solid content of 1% by mass is usually 3,500 mPa·s or less, preferably 3,000 mPa·s or less, more preferably 2,500 mPa·s or less, even more preferably 2,000 mPa·s or less, 1,000 mPa·s or less, 800 mPa·s or less, 500 mPa·s or less, 400 mPa·s or less, or 300 mPa·s or less. The lower limit is preferably 10 mPa·s or more, more preferably 20 mPa·s or more, even more preferably 50 mPa·s or more, 70 mPa·s or more, or 100 mPa·s or more. The B-type viscosity can be measured, for example, by the following method. After fibrillation (e.g., defibration), leave to stand for at least one day, dilute as necessary, stir with a homodisper (e.g., 3000 rpm, 5 min), and then measure the viscosity (e.g., measure the viscosity after rotating at 60 rpm for 3 minutes).

[0075] (Fibrillation rate) The fibrillation rate (Fibrillation %) of the modified cellulose microfibrils is preferably 1.0% or more, more preferably 1.2% or more, and even more preferably 1.5% or more. This confirms that the fibrillation is sufficient. The fibrillation rate can be adjusted depending on the type of cellulose-based raw material used. The fibrillation rate can be determined by an image analysis type fiber analyzer such as a fractionator manufactured by Valmet Co., Ltd.

[0076] (Electrical Conductivity) The electrical conductivity of the aqueous dispersion of modified cellulose microfibrils (solid content concentration 1.0% by mass) is preferably 500 mS / m or less, more preferably 300 mS / m or less, even more preferably 200 mS / m or less, even more preferably 100 mS / m or less, and particularly preferably 70 mS / m or less. The lower limit is preferably 5 mS / m or more, more preferably 10 mS / m or more, 13 mS / m or more, 15 mS / m or more, 18 mS / m or more, 20 mS / m or more, 30 mS / m or more, 40 mS / m or more, or 50 mS / m or more. The electrical conductivity can be measured by preparing 200 g of an aqueous dispersion of modified cellulose microfibrils having a solid content concentration of 1.0% by mass and using an electrical conductivity meter (HORIBA ES-71 type).

[0077] (Freeness) The Shopper-Riegler freeness of the modified cellulose microfibrils is preferably 1°SR or more, more preferably 10°SR or more, more preferably 25°SR or more, even more preferably 40°SR or more, and even more preferably 50°SR or more. The upper limit is not particularly limited as long as it is 100°SR or less. The Shopper-Riegler freeness is a measure of the degree of drainage of a fiber suspension, with the lower limit being 0°SR and the upper limit being 100°SR. The closer to 100°SR, the less drainage (amount of drainage) is indicated. The Shopper-Riegler freeness may be measured in accordance with JIS P 8121-1:2012. An example will be described below. The fibrillated chemically modified cellulose fibers are dispersed in water to prepare an aqueous dispersion with a solid content of 10g / L, and the mixture is stirred at 1000 rpm for 10 minutes or more using a magnetic stirrer. The obtained aqueous dispersion is diluted to 2g / L. A 60 mesh screen (wire thickness 0.17 mm) is set on a Mutec DFR-04, and the amount of liquid passing through the mesh from 1000 ml of test liquid is measured for 60 seconds. The Shopper-Riegler freeness is calculated according to the method in accordance with JIS P 8121-1:2012.

[0078] The modified cellulose microfibril in the present invention has a long fiber length, a large aspect ratio, and can exhibit a moderately low viscosity.Therefore, it can be used as a thickener, gelling agent, paste, food additive, excipient, paint additive, adhesive additive, abrasive, plastic compounding material, water retention material, shape retention agent, muddy water regulator, filter aid, overflow mud prevention agent, admixture, etc. in various fields such as food, beverage, cosmetics, medicine, papermaking, various chemical products, paint, spray, agricultural chemicals, civil engineering, construction, electronic materials, flame retardant, household goods, adhesive, detergent, fragrance, lubricant, etc. EXAMPLES

[0079] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited thereto. Unless otherwise specified, parts and % indicate parts by mass and % by mass.

[0080] <Procedure for measuring the physical properties of modified cellulose microfibrils (hereinafter sometimes referred to as MFC)> (Optical properties) Transparency: A water dispersion (solid concentration 1% (w / v), dispersion medium: water) was prepared, and the transmittance of light with a wavelength of 660 nm was measured using a UV-VIS spectrophotometer UV-1800 (Shimadzu Corporation) with a square cell with an optical path length of 10 mm (blank: ion-exchanged water).

[0081] (Chemical Properties) Carboxyl (COOH) group amount: 60 ml of a 0.5% by mass aqueous dispersion of the sample was prepared, and a 0.1 M aqueous hydrochloric acid solution was added to adjust the pH to 2.5. Then, a 0.05 N aqueous sodium hydroxide solution was added dropwise, and the electrical conductivity was measured until the pH reached 11. The amount of carboxyl (COOH) group was calculated using the following formula from the amount of sodium hydroxide (a) consumed in the neutralization stage of the weak acid, where the change in electrical conductivity is gradual: Amount of carboxyl groups [mmol / g carboxylated cellulose] = a [ml] × 0.05 / mass of carboxylated cellulose [g].

[0082] Degree of substitution: Approximately 2.0 g of sample was weighed out and placed in a 300 mL Erlenmeyer flask with a stopper. 100 mL of nitric acid methanol (a solution of 100 mL of concentrated nitric acid added to 1000 mL of methanol) was added and shaken for 3 hours to convert the salt-type carboxyl group to the acid-type. 1.5 to 2.0 g of the obtained acid-type sample (absolutely dry) was weighed out and placed in a 300 mL Erlenmeyer flask with a stopper. The sample was moistened with 15 mL of 80% methanol, 100 mL of 0.1 N-NaOH was added, and the mixture was shaken at room temperature for 3 hours. Excess NaOH was back-titrated with 0.1 N-H2SO4 using phenolphthalein as an indicator, and the degree of substitution (DS value) was calculated by the following formula. A = [(100 x F'-0.1N-H2SO4 (mL) x F) x 0.1] / (absolute dry mass of acid sample (g)) Substitution degree=0.162×A / (1-0.058×A) F': Factor of 0.1N-NaOH F: Factor of 0.1N-H2SO4.

[0083] Crystallinity of cellulose type I: A sample is placed in a glass cell and measured using an X-ray diffraction measuring device (e.g., LabX XRD-6000, manufactured by Shimadzu Corporation). The crystallinity is calculated using the method of Segal et al. For example, the diffraction intensity at 2θ=10° to 30° in the X-ray diffraction pattern is used as the baseline, and the crystallinity is calculated from the diffraction intensity of the 002 plane at 2θ=22.6° and the diffraction intensity of the amorphous part at 2θ=18.5° using the following formula. Xc = (I 002C -Ia) / I 002C ×100 Xc: Crystallinity of cellulose type I (%) I 002C : Diffraction intensity of 002 plane at 2θ=22.6° Ia: 2θ=18.5°, diffraction intensity of amorphous part The samples for measuring the crystallinity were freeze-dried samples prepared in the same manner as in the items (1) to (9) in the measurement of the specific surface area described later, and molded into tablets.

[0084] - Method for measuring the degree of anionization: The modified cellulose microfibrils were dispersed in water to prepare an aqueous dispersion with a solid content of 10 g / L, which was stirred at 1000 rpm for 10 minutes or more using a magnetic stirrer. The aqueous dispersion thus obtained was diluted to 0.1 g / L, and 10 ml of the solution was taken and titrated with 1 / 1000 normality diallyldimethylammonium chloride (DADMAC) using a streaming current detector (Mutek Particle Charge Detector 03). The amount of DADMAC added until the streaming current became zero was used to calculate the degree of anionization according to the following formula: q=(V×c) / m q: degree of anionization (meq / g) V: Amount of DADMAC added until the streaming current becomes zero (L) c: DADMAC concentration (meq / L) m: mass (g) of modified cellulose microfibrils in the measurement sample.

[0085] Electrical conductivity: 200 g of a water dispersion with a solid content of 1.0% by mass of the sample was prepared and thoroughly stirred. Then, the electrical conductivity was measured using an electrical conductivity meter (HORIBA ES-71).

[0086] (Fiber properties) Average fiber width, average fiber length, and fiber length distribution: The aqueous dispersion was diluted to a solid content concentration of 0.25% by mass and passed through a fractionator to determine the length-weighted fiber width, length-weighted average fiber length, and f1~f6(l)%: Fraction 1~6 percentage of length weighted distribution (n=2, Table 1).

[0087] [Table 1]

[0088] Aspect ratio: Calculated from the measured fiber width and fiber length using the following formula. Aspect ratio = average fiber length / average fiber diameter

[0089] · Specific surface area: (1) Approximately 2% aqueous dispersion of modified cellulose microfibrils was separated and placed in a centrifuge container so that the solid content was approximately 0.1 g, and 100 ml of ethanol was added. (2) A stirrer was added and the mixture was stirred at 500 rpm for at least 30 minutes. (3) The stirrer was removed, and the modified cellulose microfibrils were precipitated in a centrifuge at 7000 G for 30 minutes at 30°C. (4) The supernatant was removed while trying to avoid removing as much of the modified cellulose microfibrils as possible. (5) 100 ml of ethanol was added, a stir bar was added, and the mixture was stirred under the conditions of (2), centrifuged under the conditions of (3), and the supernatant was removed under the conditions of (4). This process was repeated three times. (6) The solvent in (5) was changed from ethanol to t-butanol, and the stirring, centrifugation, and removal of the supernatant were repeated three times in the same manner as in (5) at room temperature above the melting point of t-butanol. (7) After the final solvent removal, 30 ml of t-butanol was added and mixed gently, then transferred to an eggplant flask and frozen in an ice bath. (8) Cool in the freezer for at least 30 minutes. (9) The mixture was attached to a freeze-dryer and freeze-dried for 3 days. (10) BET measurements were performed (pretreatment conditions: under nitrogen flow, 105°C, 2 hours, relative pressure 0.01 to 0.30, sample amount approximately 30 mg).

[0090] Water retention capacity: 40 mL of an aqueous dispersion of modified cellulose microfibrils with a solids concentration of 0.3% by mass was prepared. The mass of the aqueous dispersion at this time was designated A. Next, the entire amount of the aqueous dispersion was centrifuged at 30°C and 25,000G for 30 minutes in a high-speed refrigerated centrifuge to separate the aqueous phase from the sediment. The mass of the sediment at this time was designated B. The aqueous phase was placed in an aluminum cup and dried overnight at 105°C to remove the water, and the mass of the solids in the aqueous phase was measured. The mass of the solids in this aqueous phase was designated C. The water retention capacity was calculated using the following formula: Water retention capacity=(B+C-0.003×A) / (0.003×AC).

[0091] Fibrillation rate: Measured using a Valmet fractionator.

[0092] (viscosity) B-type viscosity (25°C, 60 rpm): After leaving to stand for at least one day after defibration, it was measured using one of the following methods: After diluting to a solid content of 1%, it was stirred in a Homo Disper at 3000 rpm for 5 minutes, and then the viscosity measurement (60 rpm) was started and the viscosity value after 3 minutes was recorded.

[0093] Example 1 (TEMPO oxidation MFC (H-type, long)) <TEMPO oxidation of pulp> 5.00 kg (bone-dry) of bleached unbeaten kraft pulp derived from coniferous trees (NBKP, Nippon Paper Industries Co., Ltd., brightness 85%) was added to 500 L of an aqueous solution containing 39 g (0.05 mmol per 1 g of bone-dry cellulose) of TEMPO (Sigma Aldrich) and 514 g (1.0 mmol per 1 g of bone-dry cellulose) of sodium bromide, and the mixture was stirred until the pulp was uniformly dispersed. An aqueous solution of sodium hypochlorite was added to the reaction system so that the sodium hypochlorite concentration was 5.5 mmol / g per 1 g of bone-dry cellulose, and the oxidation reaction was started at room temperature. The pH of the system decreased during the reaction, but 3 M aqueous sodium hydroxide was added successively to adjust the pH to 10. The reaction was terminated when the sodium hypochlorite was consumed and the pH of the system no longer changed. After the reaction, the mixture was adjusted to pH 2 by adding hydrochloric acid, filtered through a glass filter, and the pulp was separated. The separated pulp was thoroughly washed with water to obtain TEMPO-oxidized pulp. The pulp yield was 90%, the time required for the oxidation reaction was 90 minutes, and the amount of carboxyl groups was 1.37 mmol / g.

[0094] <Microfibrillation> An aqueous dispersion (pH 4.5) of the obtained TEMPO oxidized pulp with a solids concentration of 4.0% by mass was prepared and treated for 10 minutes using a B-type Top Finer (manufactured by Aikawa Iron Works Co., Ltd.). After completion of microfibrillation, a 5% NaOH aqueous solution was added to adjust the pH to 7.4 to prepare oxidized cellulose microfibrils (TEMPO oxidized MFC). The physical properties of the obtained oxidized cellulose microfibrils are shown in Table 2.

[0095] Example 2 <TEMPO oxidation of pulp> 5.00 kg (bone-dry) of bleached unbeaten kraft pulp derived from conifers (NBKP, Nippon Paper Industries Co., Ltd., brightness 85%) was added to 500 L of an aqueous solution containing 39 g (0.05 mmol per 1 g of bone-dry cellulose) of TEMPO (Sigma Aldrich) and 514 g (1.0 mmol per 1 g of bone-dry cellulose) of sodium bromide, and the mixture was stirred until the pulp was uniformly dispersed. An aqueous solution of sodium hypochlorite was added to the reaction system so that the sodium hypochlorite concentration was 2.2 mmol / g per 1 g of bone-dry cellulose, and the oxidation reaction was started at room temperature. The pH of the system decreased during the reaction, but 3 M aqueous solution of sodium hydroxide was added successively to adjust the pH to 10. The reaction was terminated when the sodium hypochlorite was consumed and the pH of the system no longer changed. After the reaction, the mixture was adjusted to pH 2 by adding hydrochloric acid, filtered through a glass filter, and the pulp was separated. The separated pulp was thoroughly washed with water to obtain TEMPO-oxidized pulp. The pulp yield was 90%, the time required for the oxidation reaction was 90 minutes, and the amount of carboxyl groups was 0.56 mmol / g.

[0096] <Microfibrillation> An aqueous dispersion (pH 4.6) with a solids concentration of 3.8% by mass of the obtained TEMPO oxidized pulp was prepared and treated for 10 minutes using a B-type Top Finer (manufactured by Aikawa Iron Works Co., Ltd.). After completion of microfibrillation, a 5% NaOH aqueous solution was added to adjust the pH to 7.5 to prepare oxidized cellulose microfibrils (TEMPO oxidized MFC). The physical properties of the obtained oxidized cellulose microfibrils are shown in Table 2.

[0097] Example 3 <TEMPO oxidation of pulp> 5.00 kg (bone-dry) of bleached unbeaten kraft pulp derived from conifers (NBKP, Nippon Paper Industries Co., Ltd., brightness 85%) was added to 500 L of an aqueous solution containing 19.6 g (0.05 mmol per 1 g of bone-dry cellulose) of TEMPO (Sigma Aldrich) and 514 g (1.0 mmol per 1 g of bone-dry cellulose) of sodium bromide, and the mixture was stirred until the pulp was uniformly dispersed. An aqueous solution of sodium hypochlorite was added to the reaction system so that the sodium hypochlorite concentration was 5.6 mmol / g per 1 g of bone-dry cellulose, and the oxidation reaction was started at room temperature. The pH of the system decreased during the reaction, but 3 M aqueous sodium hydroxide was added successively to adjust the pH to 10. The reaction was terminated when the sodium hypochlorite was consumed and the pH of the system no longer changed. After the reaction, the mixture was adjusted to pH 2 by adding hydrochloric acid, filtered through a glass filter, and the pulp was separated. The separated pulp was thoroughly washed with water to obtain TEMPO-oxidized pulp. The pulp yield was 90%, the time required for the oxidation reaction was 90 minutes, and the amount of carboxyl groups was 1.42 mmol / g.

[0098] <Microfibrillation> Water, 5% NaOH, and sodium bicarbonate were added to the obtained TEMPO oxidized pulp to prepare an aqueous dispersion (pH 5.5) with a solids concentration of 4.2% by mass, and the dispersion was treated for 10 minutes using a B-type Topfiner (manufactured by Aikawa Iron Works Co., Ltd.). After completion of microfibrillation, a 5% aqueous NaOH solution was further added to adjust the pH to 7.5, and oxidized cellulose microfibrils (TEMPO oxidized MFC) were prepared. The physical properties of the obtained oxidized cellulose microfibrils are shown in Table 2.

[0099] Example 4 The microfibrillation was carried out in the same manner as in Example 1, except that the solid content concentration of the TEMPO oxidized pulp in the aqueous dispersion was changed to 2.0 mass % (Table 2).

[0100] Example 5 The microfibrillation was carried out in the same manner as in Example 1, except that the solids concentration of the TEMPO oxidized pulp in the aqueous dispersion was changed to 3.8 mass%, the pH of the aqueous dispersion was 4.6, and treatment using a 14-inch Lab Refiner (manufactured by Aikawa Iron Works Co., Ltd.) was performed for 22 minutes instead of the Top Refiner treatment (Table 2).

[0101] Example 6 <Carboxymethylation of pulp> In a twin-shaft kneader adjusted to a rotation speed of 100 rpm, 130 parts of water and 20 parts of sodium hydroxide dissolved in 100 parts of water were added, and 100 parts of hardwood pulp (LBKP, manufactured by Nippon Paper Industries Co., Ltd.) was added based on the dry mass when dried at 100°C for 60 minutes. The mixture was stirred and mixed at 30°C for 90 minutes to prepare a mercerized cellulose raw material. Further, 100 parts of isopropanol (IPA) and 60 parts of sodium monochloroacetate were added while stirring, and after stirring for 30 minutes, the mixture was heated to 70°C and carboxymethylation reaction was carried out for 90 minutes. The concentration of IPA in the reaction medium during the carboxymethylation reaction was 30%. After the reaction was completed, the mixture was neutralized with acetic acid to obtain a carboxymethylated cellulose raw material (sodium salt) with a carboxymethyl substitution degree of 0.21 and a crystallinity of cellulose type I of 72%.

[0102] <Microfibrillation> The obtained carboxymethylated pulp was dispersed in water (pH 6.9) with a solid content of 4.0% by mass, and treated for 10 minutes using a 14-inch lab refiner (manufactured by Aikawa Iron Works Co., Ltd.) to prepare cellulose microfibrils (carboxymethylated MFC). The physical properties of the obtained cellulose microfibrils are shown in Table 2.

[0103] Comparative Example 1 (TEMPO oxidized MFC (high viscosity)) Microfibrillation was performed in the same manner as in Example 1, except that the solids concentration of TEMPO oxidized pulp in the aqueous dispersion was changed to 2.0 mass%, 5% NaOH and sodium bicarbonate were added before the top finer treatment to adjust the pH to 8.0, and no pH adjustment treatment was performed after microfibrillation was completed (Table 3).

[0104] Comparative example 2 (TEMPO oxidized MFC (H type / high concentration)) Microfibrillation was carried out in the same manner as in Example 1, except that the solids concentration of the TEMPO oxidized pulp in the aqueous dispersion was changed to 30 mass%, and treatment using a 14-inch Lab Refiner (manufactured by Aikawa Iron Works Co., Ltd.) was performed twice instead of the Top Finer treatment (Table 3).

[0105] Comparative Example 3 Microfibrillation was performed in the same manner as in Example 1, except that 5% NaOH and sodium bicarbonate were added before the top finer treatment to adjust the pH of the aqueous dispersion of TEMPO oxidized pulp to 8.6, and no pH adjustment treatment was performed after microfibrillation was completed (Table 3).

[0106] Comparative Example 4 <TEMPO oxidation of pulp> 5.00 kg (bone-dry) of bleached unbeaten kraft pulp derived from conifers (NBKP, Nippon Paper Industries Co., Ltd., brightness 85%) was added to 500 L of an aqueous solution containing 19.6 g (0.05 mmol per 1 g of bone-dry cellulose) of TEMPO (Sigma Aldrich) and 514 g (1.0 mmol per 1 g of bone-dry cellulose) of sodium bromide, and the mixture was stirred until the pulp was uniformly dispersed. An aqueous solution of sodium hypochlorite was added to the reaction system so that the sodium hypochlorite concentration was 5.9 mmol / g per 1 g of bone-dry cellulose, and the oxidation reaction was started at room temperature. The pH of the system decreased during the reaction, but 3 M aqueous solution of sodium hydroxide was added successively to adjust the pH to 10. The reaction was terminated when the sodium hypochlorite was consumed and the pH of the system no longer changed. After the reaction, the mixture was adjusted to pH 2 by adding hydrochloric acid, filtered through a glass filter, and the pulp was separated. The separated pulp was thoroughly washed with water to obtain TEMPO-oxidized pulp. The pulp yield was 90%, the time required for the oxidation reaction was 90 minutes, and the amount of carboxyl groups was 1.48 mmol / g.

[0107] <Microfibrillation> Water, 5% NaOH, and sodium bicarbonate were added to the obtained TEMPO oxidized pulp to prepare an aqueous dispersion (pH 8.2) with a solids concentration of 4.1% by mass, and the dispersion was treated for 24 minutes using a 14-inch lab refiner (manufactured by Aikawa Iron Works Co., Ltd.) to prepare oxidized cellulose microfibrils (TEMPO oxidized MFC). The physical properties of the obtained oxidized cellulose microfibrils are shown in Table 3.

[0108] Comparative Example 5 <Carboxymethylation of pulp> The sodium salt of carboxymethylated cellulose was obtained in the same manner as in Example 6, except that the concentration of IPA in the reaction solution during the carboxymethylation reaction was 55% by changing the amount of IPA added. The degree of carboxymethyl substitution was 0.35, and the crystallinity of cellulose type I was 68%.

[0109] <Microfibrillation> The obtained carboxymethylated pulp was dispersed in water (pH 7.5) with a solid content of 4.0% by mass, and treated for 12 minutes using a 14-inch lab refiner (manufactured by Aikawa Iron Works Co., Ltd.) to prepare cellulose microfibrils (carboxymethylated MFC). The physical properties of the obtained cellulose microfibrils are shown in Table 3.

[0110] [Table 2]

[0111] [Table 3]

[0112] From the results in Tables 2 and 3, the modified cellulose microfibrils of the Examples had longer fiber lengths and larger aspect ratios than those of the Comparative Examples. The modified cellulose microfibrils of the Examples also showed a moderately low viscosity. These results indicate that the modified cellulose microfibrils obtained by the present invention can exhibit excellent functions in a wide range of applications.

Claims

1. Step (1): A step of oxidizing a cellulosic raw material to obtain oxidized cellulose; and Step (2): A step of defibrating the oxidized cellulose obtained in step (1) by mechanical treatment under conditions of a pH of 7 or less and a solid content concentration of 0.1 to 15% by mass; A method for producing oxidized cellulose microfibrils, comprising: The oxidized cellulose microfibrils have an average fiber diameter of 500 nm or more and 60 μm or less, an average fiber length of 600 μm or more and 3000 μm or less, and an aspect ratio of 50 or more.

2. The method described in claim 1, wherein the proportion of oxidized cellulose microfibrils with fiber lengths of 2.0 to 3.2 mm is 1% or more and 20% or less.

3. 3. The method according to claim 1 or 2, wherein the carboxyl group content of the oxidized cellulose is 0.1 to 2.5 mmol / g.

4. The method according to any one of claims 1 to 3, wherein the degree of carboxyl substitution of the oxidized cellulose is from 0.01 to 0.

50.

5. The method according to any one of claims 1 to 4, wherein the mechanical treatment is a beating or defibration treatment.

Citation Information

Patent Citations

  • Composite material and molded body using same

    WO2014087767A1

  • Method for storing chemically modified cellulose fibers and method for producing chemically modified cellulose nanofibers

    WO2018173761A1

  • Oxidized microfibrillar cellulose fibers and composition thereof

    WO2019189588A1

  • Paper containing microfibril cellulose fiber

    WO2019189611A1

  • Pulverized product of carboxymethylated pulp and additive containing said pulverized product