Recycled polyethylene stand-up pouches
A laminate structure with HDPE, LLDPE, and MDPE layers, combined with a two-layer sealant system, addresses the recyclability and sealing effectiveness issues of SUPs, enhancing stiffness and impact resistance while incorporating recycled polyethylene.
Patent Information
- Application Number
- JP2022517340
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-09-20
- Filing Date
- 2020-09-14
- Publication Date
- 2024-09-20
- Estimated Expiration
- 2040-09-14
AI Technical Summary
Stand-up pouches (SUPs) made from a laminate of polyethylene terephthalate (PET) and polyethylene (PE) are difficult to recycle due to the different materials they are made of, and the inclusion of recycled polyethylene (r.PE) can reduce the effectiveness of the sealant layer.
A laminate structure comprising an outer web with layers of HDPE, LLDPE, and MDPE, and an inner web with recycled polyethylene (r.PE) and a two-layer sealant system, where the density of the adjacent layer is higher than the sealant layer but lower than the core layer, forming at least 95% of the polymeric material.
The laminate structure enhances sealing effectiveness and allows for the use of recycled polyethylene while maintaining recyclability, improving stiffness and impact resistance.
Smart Images

Figure 0007554822000011 
Figure 0007554822000012 
Figure 0007554822000009
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a laminate structure prepared by laminating a first polyethylene web to a second polyethylene web, the laminate structure being suitable for preparing, for example, a stand up pouch (SUP), the SUP being made from recycled polyethylene and therefore recyclable. [Background technology]
[0002] Stand-up pouch ("SUP") packaging is in widespread commercial use as packaging for consumer goods. These pouches are attractive to consumers and, if properly designed, can be very efficient in using minimal amounts of polymeric material to prepare the packaging.
[0003] SUP packaging was first produced over 30 years ago. Early designs used a laminate of layers of polyethylene terephthalate (PET) and polyethylene (PE). This type of design is still in commercial use today, with a typical structure having a thin layer (about 0.5 mil, or 0.12 mm thick) of PET and a thicker layer of PE (about 3 mil, or 0.75 mm).
[0004] The problem with this SUP design is that the pouches are difficult to recycle due to the different materials they are made from.
[0005] It is known to prepare "recyclable" SUPs that are prepared using only polyethylene (or at least 95% PE, since many recycling facilities can recycle coextruded or laminated films that contain at least 95% PE as "pure" PE material). For example, U.S. Patent Application Publication No. 2016 / 0229,157 (to NOVA Chemicals) describes SUPs that contain at least 95% PE by weight and are therefore recyclable.
[0006] A further need is to use recycled polyethylene ("r.PE") in new pouches. The inventors have observed that the inclusion of r.PE in the SUP can reduce the effectiveness of the sealant layer of the film structure used to prepare the SUP. The inventors have discovered that a two-layer sealant system mitigates this problem and enhances the sealing effectiveness. Summary of the Invention
[0007] Disclosed herein is a laminate structure made from a polymeric material, the laminate structure comprising: A) An outer web comprising: A.1) Layer 1-A comprising an HDPE composition; A.2) a layer 2-A comprising a polyethylene selected from LLDPE, MDPE, and HDPE; and B) An inner web, which includes: B.1) a 1-B layer in contact with the outer web, wherein the 1-B layer comprises a polyethylene selected from LLDPE and MDPE; B.2) Layer 2-B comprising recycled polyethylene; B.3) A sealant structure including: B.3.1) A sealant skin layer comprising a polyethylene sealant; B.3.2) a layer adjacent to the sealant skin layer comprising polyethylene, the density of the polyethylene being a) higher than the density of the polyethylene sealant and b) lower than the density of the core layer in contact with the layer adjacent to the sealant skin layer; and I) the outer web is laminated to the inner web; II) the HDPE, MDPE, LLDPE, recycled polyethylene, and polyethylene sealant together form at least 95% by weight of the polymeric materials used to prepare the laminate structure.
[0008] Disclosed herein is a laminate structure made from a polymeric material, the laminate structure comprising: A) Web sites that include: A.1) Layer 1-A comprising an HDPE composition; A.2) Layer 2-A comprising a polyethylene selected from LLDPE, MDPE, and HDPE; A.3) a layer 3-A comprising a polyethylene selected from LLDPE, MDPE, and HDPE; and B) Inner web containing: B.1) a 1-B layer in contact with the outer web, wherein the 1-B layer comprises a polyethylene selected from HDPE, LLDPE and MDPE; B.2) Layer 2-B comprising recycled polyethylene; B.3) A sealant structure including: B.3.1) A sealant skin layer comprising a polyethylene sealant; B.3.2) a layer adjacent to the sealant skin layer comprising polyethylene, the density of the polyethylene being a) higher than the density of the polyethylene sealant and b) lower than the density of the core layer in contact with the layer adjacent to the sealant skin layer; and I) each of the outer web and the inner web optionally comprises at least one additional polyethylene layer between A.1 and A.3 and between B.1 and B.3; II) the outer web is laminated to the inner web; III) the HDPE, MDPE, LLDPE, recycled polyethylene, and polyethylene sealant together form at least 95% by weight of the polymeric materials used to prepare the laminate structure. [Brief description of the drawings]
[0009] [Figure 1] FIG. 1 shows the properties of seals prepared using different inner webs. [Diagram 2] FIG. 2 shows the properties of seals prepared using different inner webs. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] In one embodiment, the polymeric material used to make the SUP (stand up pouch) comprises different types of polyethylene. In one embodiment, the polymeric material used to make the SUP consists essentially of different types of polyethylene, i.e., the only polymeric material used to make the SUP of this embodiment is polyethylene. The term polyethylene refers to a polymer that includes ethylene and may include optional comonomers.
[0011] Suitable examples of polyethylene include: 1) High density polyethylene (HDPE): a polyethylene homopolymer or copolymer having a density of about 0.95 to about 0.97 g / cc; 2) Medium Density Polyethylene (MDPE): a polyethylene copolymer having a density of about 0.93 to about 0.95 g / cc; 3) Linear low density polyethylene (LLDPE): a polyethylene copolymer having a density of about 0.915 to about 0.93 g / cc; 4) Polyethylene Sealant: A polyethylene material suitable for the preparation of thermoformed seals, or polyethylenes selected from, for example, 1) polyethylene copolymers having a density of about 0.88 to 0.915 g / cc ("VLDPE"); and 2) High Pressure Low Density Polyethylene (LD): polyethylene homopolymers prepared with free radical initiators in a high pressure process and having a density of about 0.91 to about 0.93 g / cc.
[0012] In some embodiments, only the outer webs include a layer of HDPE. In another embodiment, both the inner and outer webs of the laminate structure include HDPE in at least one layer. The HDPE layer provides stiffness / rigidity to the SUP. In one embodiment, these HDPE layers are separated by at least one layer of low density polyethylene (such as LLDPE), which provides impact and puncture resistance. Additionally, by separating the layers of rigid HDPE, the overall stiffness and torsional strength of the SUP is improved compared to structures that include a comparable amount / thickness of HDPE in a single layer, sometimes referred to as the "I-beam" effect (as it resembles the steel I-beams that are widely used in building construction).
[0013] An "adjacent" layer is in contact with a sealant skin layer on one side and with a core layer on the other side of the adjacent layer. The adjacent layer comprises a polyethylene composition having a higher density than the density of the sealant skin layer it contacts but a lower density than the density of the core layer it contacts. In one embodiment, the polyethylene composition is a blend of polyethylenes, and in another embodiment, the polyethylene composition comprises a single type of polyethylene.
[0014] In embodiments where the outer and inner webs optionally include at least one additional polyethylene layer between A.1 and A.3 and B.1 and B.3, the additional layer comprises a polyethylene composition comprising HDPE, MDPE, LLDPE, or a combination thereof. In additional embodiments, the layers comprise HDPE, MDPE, LLDPE, or a combination thereof. In additional embodiments, the layers comprise recycled polyethylene. In additional embodiments, the layers comprise recycled polyethylene.
[0015] When preparing blown multilayer films using multi-line equipment, those skilled in the art will understand that each layer may be produced by a single line, or the "layers" may result from multiple successive lines producing layers of the same composition in successive layers. As an example, a five-layer line may produce a structure of composition A / B / C / D / E, producing a five-layer film. Alternatively, the same five-layer line may be used to make a five-layer film of composition A / A / B / C / C, effectively producing a three-layer film.
[0016] In some embodiments, the laminate structures of the present disclosure are suitable for the preparation of stand-up pouches (SUPs).
[0017] SUP packages are well known. They are typically prepared from "roll stock" (i.e., films or laminated structures as disclosed herein) using a variety of well-known techniques and machinery.
[0018] SUPs are manufactured in many sizes and are typically used to package small volumes (e.g., about 25 mils to 2 liters) of consumer goods. The contents of a SUP package are typically described as "flowable," the term being intended to encompass particulate solids (such as candy, nuts, and breakfast cereals); liquids (e.g., beverages); and pastes / emulsions / purees (such as yogurt and baby food). In one embodiment, the SUP is designed such that the contents of an opened package can easily flow from the SUP (and / or can be consumed directly from the SUP). For example, the top of the SUP may be provided with an integral straw (for beverages) or a spout for pastes, emulsions, purees, etc. Such designs are well known, and one example is disclosed in Canadian Patent Application No. 2,612,940 (Rogers).
[0019] In some embodiments, the SUP is typically opened at the top of the package. The SUP can be opened using a tear strip, or a fitment (or cap) that can reseal the package, or other cap / closure known to those of skill in the art.
[0020] In one embodiment, the laminate structure is printed at the interface between two webs, either on the inner surface of the first web or on the outer surface of the second web.
[0021] This is followed by a detailed description of various embodiments of the first (outer) web, various embodiments of the second (inner) web, various embodiments of the adhesive, and various embodiments of the printing.
[0022] In one embodiment, the first (outer) web forms the outer wall of the laminate structure.
[0023] In one embodiment, the laminate structure is printed at the interface between a first web and a second (inner) web.
[0024] Since people "look through" the outer web to see the print, in some embodiments it may be desirable for the outer web to have a low haze value. Additionally, in some embodiments a high "gloss" may be desirable, since many consumers perceive a high gloss finish as an indicator of higher quality.
[0025] Additionally, in some embodiments, it is desirable for an exterior layer to provide stiffness / rigidity to the laminate structure so that a SUP made from the laminate structure is self-supporting.
[0026] Thus, a balance of good optical properties and stiffness may be desired for the outer web. HDPE is known to provide the desired stiffness, but it is also known that HDPE can have poor optical properties. Thus, in one embodiment, a very thin layer of HDPE is used as a skin layer of the outer web, along with a layer of low density polyethylene. These embodiments are further described below.
[0027] <Multi-layer outer web, or web A> Generally, the use of a thick monolayer HDPE film to form the outer web of a SUP can provide a structure with adequate stiffness. However, a drawback of the thick HDPE layer is that it has poor optical properties. This drawback can be overcome by printing the outer surface (skin) side of the outer web to form an opaque SUP. However, this design can be less tolerant of rough handling as the printing can easily be rubbed off or damaged during shipping and handling of the SUP.
[0028] In one embodiment, the structure disclosed herein mitigates these problems by providing the outer web with a coextruded multilayer film in which at least one layer ("Layer A.1") is prepared from HDPE and at least one layer ("Layer A.2") is prepared from low density polyethylene (LLDPE, LD, VLDPE, etc.).
[0029] In one embodiment, the HDPE is further characterized by having a melt index, I2, from 0.1 to 10 (or, such as, from 0.3 to 3) grams / 10 minutes.
[0030] In one embodiment, Layer 1-A is a HDPE composition that includes a nucleating agent.
[0031] In one embodiment, the LLDPE is further characterized by having a melt index, I2, from 0.1 to 5 (or, such as, from 0.3 to 3) grams / 10 minutes.
[0032] In one embodiment, the LLDPE is prepared using a single-site catalyst (such as a metallocene catalyst) and is further characterized by having a molecular weight distribution (Mw / Mn) (i.e., the weight average molecular weight divided by the number average molecular weight) of about 2 to about 4. This type of LLDPE is typically referred to as sLLDPE.
[0033] In one embodiment, very low density polyethylene (VLDPE) is an ethylene copolymer having a density of about 0.88-0.915 g / cc and a melt index (I2) of about 0.5-10 g / cc. All of the above materials are well known and commercially available.
[0034] Low density polyethylene can be used to improve the optics of the multilayer web. In one embodiment, the multilayer structure is a three-layer A / B / A type coextruded film, where A is an LLDPE (e.g., single-site catalyzed LLDPE) and B is an HDPE composition. This type of film provides superior optical properties, and in some embodiments, some of these films have been observed to have better optical properties than monolayer films made with the same LLDPE.
[0035] In another embodiment, the LLDPE used in web A is blended with a small amount (0.2-10 wt%) of LD polyethylene having a melt index I2 of 0.2 to 5, or such as 0.2 to 0.8. These LLDPEs and certain blends of LLDPE and LD have been observed to have superior optical properties and superior stiffness compared to LLDPE alone (especially when the LLDPE is sLLDPE).
[0036] In some embodiments, the use of LD resins having a melt index of about 0.2-0.8 grams / 10 minutes has been observed to be effective for this purpose (those skilled in the art commonly refer to this type of LD resin as "fractional melt LD").
[0037] In another embodiment, the LLDPE used in Web A is blended with small amounts (0.2-10% by weight) of HDPE resin and a nucleating agent.
[0038] The term "nucleating agent" as used herein is meant to convey its conventional meaning to those skilled in the art of preparing nucleated polyolefin compositions, i.e., an additive that alters the crystallization behavior of a polymer as the polymer melt cools.
[0039] Examples of conventional nucleating agents that are commercially available and widely used as polypropylene additives include dibenzylidene sorbital esters (such as products sold under the trademark MILLAD® 3988 by Milliken Chemical and IRGACLEAR® by Ciba Specialty Chemicals).
[0040] In some embodiments, the nucleating agent should be well dispersed in the polyethylene. In some embodiments, the amount of nucleating agent used is relatively small, between 200 and 10,000 ppm by weight (based on the weight of the polyethylene), so one skilled in the art will appreciate that some care must be taken to ensure that the nucleating agent is well dispersed. In some embodiments, the nucleating agent is used in finely divided form (less than 50 microns, or, for example, less than 10 microns) in the polyethylene to facilitate mixing.
[0041] Examples of nucleating agents that may be suitable for use include cyclic organic structures disclosed in U.S. Pat. No. 5,981,636 (and salts thereof, such as bicyclodisodium [2.2.1]heptene dicarboxylate); saturated versions of the structures disclosed in U.S. Pat. No. 5,981,636 (such as those disclosed in U.S. Pat. No. 6,465,551; Zhao et al. to Milliken); salts of certain cyclic dicarboxylic acids having a hexahydrophthalic acid structure (or "HHPA" structure) as disclosed in U.S. Pat. No. 6,599,971 (Dotson et al. to Milliken); metal salts of phosphate esters and glycerol (or, for example, zinc glycerolate), such as those disclosed in U.S. Pat. No. 5,342,868 and sold under the trade names NA-11 and NA-21 by Asahi Denka Kogyo. Calcium salt of 1,2-cyclohexanedicarboxylic acid, calcium salt (CAS Registry Number 491589-22-1) typically gives good results for nucleation of HDPE. The above nucleating agents are sometimes described as "organic" (meaning that they contain carbon and hydrogen atoms) to distinguish them from inorganic additives such as talc and zinc oxide. Talc and zinc oxide are usually added to polyethylene (to provide antiblocking and acid scavenging functions, respectively) and they provide some limited nucleation function.
[0042] The "organic" nucleating agents mentioned above may be better (but more expensive) nucleating agents than inorganic nucleating agents. In one embodiment, the amount of organic nucleating agent is 200-2000 ppm (based on the total weight of polyethylene in the layer containing the nucleating agent).
[0043] In some embodiments, these LLDPE / HDPE / nucleating agent blends have also been found to provide better optical properties and higher modulus (higher stiffness) than 100% LLDPE.
[0044] In another embodiment, the outer web is a three-layer A / B / A type coextruded film, where A is HDPE and B is low density polyethylene, for example, the above LLDPE compositions (including the LLDPE composition blended with LD and the LLDPE composition blended with HD and a nucleating agent). These films provide excellent rigidity.
[0045] <B. Inner web (using recycled polyethylene); also called the "B" web; also called the "sealant" web> The inner web forms the inside of the SUP made from the laminated structure. B.1) A first-B layer in contact with the outer web, where the first-B layer comprises a polyethylene selected from HDPE, LLDPE, and MDPE. B.2) A second-B layer containing recycled polyethylene. B.3) A sealant structure comprising: B.3.1) A sealant skin layer containing a polyethylene sealant. B.3.2) A layer adjacent to the sealant skin layer containing polyethylene, where the density of the polyethylene is a) higher than the density of the polyethylene sealant and b) lower than the density of the core layer in contact with the layer adjacent to the sealant skin layer.
[0046] <B.1 Interface skin layer> One skin layer of the inner web is prepared from a polyethylene composition having a density lower than that of HDPE, resulting in a layer with enhanced impact resistance and tear strength characteristics compared to the layer prepared from HDPE. In one embodiment, this layer is mainly made from LLDPE (including sLLDPE) having a melt index of 0.3 to 3 grams / 10 minutes. This layer may also be prepared using a large amount of LLDPE (or sLLDPE) and a small amount of LD (for example, the fractional melt LD as described above) or the LLDPE+HDPE+nucleating agent blend as described above.
[0047] In another embodiment, this skin layer may be prepared using MDPE (or a blend of MDPE with a small amount of another polyethylene, such as a blend with LD, and a blend of HDPE and the above-mentioned nucleating agent).
[0048] In one embodiment, this skin layer is printed. Thus, it is within the scope of the present disclosure to incorporate any of the well-known film modification means that facilitate the printing process. For example, the skin layer can be corona treated to improve the adhesion of the ink. In another embodiment, the skin layer may contain an opacifying agent (such as talc, titanium oxide, or zinc oxide) to improve the appearance of the printed surface.
[0049] <B.2 Core Layer Containing Recycled Polyethylene (r.PE)> The inner web contains at least one layer containing r.PE. The inner web contains a core layer containing r.PE. In one embodiment, the core layer consists essentially of r.PE (i.e., all the polymers used in this layer are r.PE).
[0050] Recycled polyethylene has many sources and types, which are useful for the various embodiments disclosed herein. As used herein, the term recycled polyethylene (or r.PE) refers to recycled polyethylene that is independent of its source.
[0051] In one example, the recycled polyethylene is polyethylene that has been subjected to at least one "thermal history", i.e., polyethylene that has been melted, molded, or extruded at least once. In one embodiment, the r.PE may be post-industrial recycle (PIR), which generally refers to polyethylene that has been used in the manufacturing process but not sold to the end consumer (such PIR polyethylene is typically manufactured as scrap, trimming, or off-spec parts in the manufacturing process and is either recovered for reuse in the same process or sold to other manufacturers / converters for use in another process).
[0052] In one embodiment, the r.PE is polyethylene after consumer recycling (or "PCR"). PCR is recovered from the waste stream and washed before reuse.
[0053] In certain embodiments, the PCR is prepared from recycled containers for liquids (such as milk or juice).
[0054] The r.PE has a density of 0.910 - 0.97 g / cc and a melt index I2 of 0.2 - 20.
[0055] In one embodiment, the r.PE has a density of 0.93 - 0.95 g / cc and a melt index I2 of 0.2 - 10.
[0056] In other embodiments, the density is 0.910 - 0.930, or 0.930 - 0.950, or 0.950 - 0.960.
[0057] <B.3 Sealant Structure - Sealant Layer (B.3.1) and "Adjacent to" or "Next to" Layer (B.3.2)> The inner web has two outer layers, or two "skin" layers (i.e., the boundary skin layer (layer B.1 above) and the inner skin layer (also referred to herein as the sealant layer (B.3.1))). The sealant layer is prepared from "polyethylene sealant" (i.e., a type of polyethylene that easily melts to form a seal when exposed to sealing conditions). Those skilled in the art will recognize that two types of polyethylene (i.e., a polyethylene copolymer having a density of about 0.88 - 0.915 g / cc and LD polyethylene (as described above)) are preferred for use as a sealant.
[0058] In some embodiments, it is preferred to use a low density polyethylene copolymer. In principle, the cost of these low density polyethylenes increases as the density decreases, so the "optimal" polyethylene sealant resin will typically be the highest density polyethylene that provides sufficient seal strength. Polyethylene sealants with a density of about 0.900 - 0.914 g / cc provide satisfactory results in many applications.
[0059] Other examples of polyethylene sealants include ethylene - vinyl acetate (EVA) and "ionomers" (e.g., copolymers of ethylene and an acidic comonomer, where the resulting acidic comonomer is neutralized by, for example, sodium, zinc, or lithium; ionomers are commercially available under the trademark SURLYN®).
[0060] Using EVA and / or ionomers may cause problems when recycling SUP, so it is less preferred (however, as mentioned above, many recycling facilities accept SUP containing up to 5% EVA or ionomers for recycling).
[0061] <B.3.2 "Next to" or "Adjacent to" Layer> The inventors have observed that the use of r.PE in the inner web reduces the effectiveness of the sealing layer (compared to an inner web made with virgin HDPE instead of r.PE). The reasons for this are not fully understood. However, the inventors have observed that the use of select polyethylenes in layers in contact (or "adjacent") with the sealant layer improves sealing performance. For clarity, the sealant layer (above) is the skin layer used to seal the SUP, and the "adjacent" layer is the core layer adjacent / in contact with the sealant layer, which is also in contact with another core layer. In one embodiment, the "adjacent" layer has a density of 0.917-0.921 g / cc. In some embodiments, the B.3.2 sealant layer (adjacent layer) may comprise recycled polyethylene alone or a blend of recycled and virgin polyethylene. In these embodiments, the density of the selected polyethylene, recycled polyethylene, or blend of the two satisfies the relative density requirement to allow the layer adjacent to the sealant skin layer having polyethylene to have a density that is a) higher than the density of the polyethylene sealant and b) lower than the density of the core layer in contact with the layer adjacent to the sealant skin layer.
[0062] In one embodiment, the rLLDPE has a viscosity of 0.927 g / cm 3 and has a density of 0.914 g / cm 3 It is blended with VLDPE having a density of 1000 .mu.m to 1000 .mu.m.
[0063] In one embodiment, the rLLDPE has a viscosity of 0.928 g / cm 3 and has a density of 0.912 g / cm 3 It is blended with VLDPE having a density of 1000 .mu.m to 1000 .mu.m.
[0064] <B.5 HDPE> In one embodiment, the inner web also includes at least a layer prepared from an HDPE composition, optionally including a nucleating agent.
[0065] In one embodiment, the second-B layer comprises an HDPE composition containing a nucleating agent.
[0066] HDPE is a common commercial item. Most commercially available HDPEs are prepared from catalysts containing at least a metal (e.g., chromium or a Group IV transition metal (Ti, Zr, or Hf)).
[0067] HDPE made from Cr catalysts typically contains some long-chain branching (LCB). HDPE made from Group IV metals generally contains less LCB than HDPE made from Cr catalysts.
[0068] As used herein, the term HDPE refers to polyethylene (or a polyethylene blend composition as required by the context) having a density of about 0.95 to 0.97 grams per cubic centimeter (g / cc). In one embodiment, the melt index (“I2”) of the HDPE is about 0.2 to 10 grams per 10 minutes.
[0069] In one embodiment, the HDPE is provided as a blend composition comprising two HDPEs whose melt indices are at least 10 times apart. This HDPE blend composition will be described in further detail subsequently.
[0070] <HDPE Blend Composition> <Blend Components>
[0071] <Blend Component a)> The blend component a) of the polyethylene composition used in this embodiment comprises HDPE having a relatively high melt index. As used herein, the term "melt index" is meant to refer to the value obtained by ASTM D1238 (when carried out at 190°C with a weight of 2.16 kg). This term is also referred to herein as "I2" (expressed as grams of polyethylene flowing during a 10 minute test period, or "grams / 10 minutes"). As will be recognized by those skilled in the art, the melt index I2 is generally inversely proportional to the molecular weight. In one embodiment, blend component a) has a relatively high melt index (or, in other words, a relatively low molecular weight) compared to blend component b).
[0072] The absolute value of I2 of blend component a) in these blends is generally greater than 5 grams / 10 minutes. However, the "relative value" of I2 of blend component a) is more important and generally should be at least 10 times higher than the I2 value of blend component b) [the I2 value of blend component b) is referred to herein as I2']. Thus, for illustrative purposes, if blend component b) has an I2' value of 1 gram / 10 minutes, the I2 value of blend component a) is, for example, at least 10 grams / 10 minutes.
[0073] In one embodiment, blend component a) may be further characterized by i) having a density of 0.95-0.97 g / cc, ii) being present in an amount of 5-60 wt% of the total HDPE blend composition (wherein blend component b) forms the balance of the total composition), being present in an amount of 10-40 wt%, or such as being present in an amount of 20-40 wt%. It is permissible to use multiple high density polyethylenes to form blend component a).
[0074] The molecular weight distribution is determined by dividing the weight average molecular weight (Mw) by the number average molecular weight (Mn), where Mw and Mn are determined by gel permeation chromatography according to ASTM D6474-99. The Mw / Mn of component a) is, for example, from 2 to 20, or for example, from 2 to 4. Without wishing to be bound by theory, it is believed that the low Mw / Mn value (2-4) of component a) may improve the crystallization rate and overall barrier performance of blown film and web structures prepared according to the present disclosure.
[0075] <Blend component b)> Blend component b) is also a high density polyethylene having a density of 0.95 to 0.97 g / cc (eg, 0.955 to 0.968 g / cc).
[0076] The melt index of blend component b) is also determined by ASTM D1238 using a load of 2.16 kg at 190° C. The melt index value of blend component b) (referred to herein as I2′) is lower than the melt index value of blend component a), indicating that blend component b) has a relatively high molecular weight. The absolute value of I2′ is, for example, 0.1 to 2 grams / 10 minutes.
[0077] Although the molecular weight distribution (Mw / Mn) of component b) is not necessarily critical to successful performance, examples of component b) include those having an Mw / Mn of 2-4.
[0078] Finally, the ratio of the melt index of component b) divided by the melt index of component a) is, for example, greater than 10 / 1.
[0079] Blend component b) may also contain multiple HDPE resins.
[0080] Overall HDPE Blend Composition An overall high density blend composition is formed by blending blend component a) and blend component b) together. In one embodiment, the overall HDPE composition has a melt index (measured according to ASTM D 1238 at 190° C. with a 2.16 kg load) of 0.5 to 10 grams / 10 minutes (e.g., 0.8 to 8 grams / 10 minutes).
[0081] The blends can be made by any blending process; for example, 1) physical blending of particulate resins; 2) co-feeding different HDPE resins into a common extruder; 3) melt mixing (in any conventional polymer mixing equipment); 4) solution blending; or 5) a polymerization process utilizing two or more reactors.
[0082] A suitable HDPE blend composition can be prepared by melt blending in an extruder the following two blend components: 10-30% by weight of component a): Component a) is an HDPE resin having a melt index I2 of 15-30 grams / 10 minutes and a density of 0.95-0.97 g / cc; 90-70% by weight of component b): Component b) is a HDPE resin having a melt index I2 of 0.8-2 grams / 10 minutes and a density of 0.95-0.97 g / cc.
[0083] An example of a commercially available HDPE resin suitable for component a) is sold under the trademark SCLAIR® 79F. This is an HDPE resin prepared by homopolymerizing ethylene with a conventional Ziegler-Natta catalyst. It has a typical melt index (18 grams / 10 minutes), a typical density (0.963 g / cc), and a typical molecular weight distribution (about 2.7).
[0084] Examples of commercially available HDPE resins suitable for blend component b) include (typical melt index and density values are given in brackets): SCLAIR® 19G (Melt Index = 1.2 grams / 10 minutes, Density = 0.962 g / cc); MARFLEX® 9659 (available from Chevron Phillips, melt index = 1 gram / 10 minutes, density = 0.962 g / cc); and ALATHON® L5885 (available from Equistar, melt index = 0.9 grams / 10 minutes, density = 0.958 g / cc).
[0085] In some embodiments, the HDPE blend composition is prepared by a solution polymerization process using two reactors operating under different polymerization conditions, which provides a homogeneous in situ blend of the HDPE blend components. An example of this process is described in U.S. Patent No. 7,737,220 (Swabey et al.).
[0086] In one embodiment, the HDPE composition is prepared using only ethylene homopolymer. This type of composition is suitable when it is desired to optimize (maximize) the barrier properties of the structure.
[0087] In another embodiment, the HDPE composition can be prepared using copolymers, as this allows for some improvement in physical properties, such as impact resistance. In yet another embodiment, a small amount (less than 30% by weight) of low density polyethylene can be blended into the HDPE composition, which can also allow for some improvement in impact resistance.
[0088] In one embodiment, the above HDPE blend composition is combined with an organic nucleating agent (as described above) in an amount of about 300 to 3000 ppm by weight based on the weight of the HDPE blend composition. The calcium salt of 1-2 cyclohexanedicarboxylic acid (as described above), calcium salt (CAS 491589-22-1), is suitable for use. In some embodiments, when the HDPE composition includes a nucleating agent, it is preferred to use an HDPE composition prepared with a Group IV transition metal (e.g., Ti).
[0089] This type of "nucleated" core layer has been observed to provide superior barrier properties (i.e., reduced permeability to water, gas, and grease), which are desirable for many packaging applications.
[0090] In some embodiments, the presence of a nucleating agent has been observed to improve the elastic modulus of the HDPE layer (compared to a non-nucleated layer of comparable thickness).
[0091] The use of nucleated HDPE blend compositions of the above type provides a "barrier" against oxygen and water permeation. This barrier layer performance is adequate for many commercial products. However, those skilled in the art will recognize that improved "barrier" performance can be achieved by using certain "barrier" polymers such as ethylene-vinyl alcohol (EVOH), ionomers and polyamides. The use of such non-polyethylene barrier resins in large quantities can make it very difficult to recycle films / structures / SUPs made with a combination of polyethylene and non-polyethylene materials. However, it is still possible to recycle such structures when the non-polyethylene materials are present in small amounts (less than 10% by weight, especially less than 5% by weight).
[0092] Those skilled in the art will also recognize that in some embodiments, the use of certain non-polyethylene barrier resins may require the use of a "tie layer" to enable adhesion between the non-polyethylene barrier layer and the remaining layer of polyethylene.
[0093] <Printing process> As mentioned above, in some embodiments, the laminated structures of the present disclosure are printed at the interface between two webs. Suitable processes include well-known flexographic and gravure printing techniques, which typically use nitrocellulose or water-based inks.
[0094] The outer web (described above) forms the outside of the SUP and the inner web forms the inside of the SUP. Those skilled in the art typically refer to the outer web as the "print" web and the inner web as the "sealant" web.
[0095] <Lamination / assembly process> One step in the assembly of a laminate structure requires laminating a first web to a second web. There are many commercially available techniques for the lamination process, including the use of liquid adhesives (which may be solvent-based, solvent-free, or water-based), hot melt adhesives, and thermal bonding.
[0096] The above SUP packaging container is laminated. It will be understood by those skilled in the art that a similar SUP can be prepared by coextrusion (using the same materials in the same layers as the laminated SUP). However, the laminated SUP can be printed at the web interface (whereas the coex SUP is printed on the skin layer). Therefore, the laminated SUP has better print quality (and scratch resistance).
[0097] In one embodiment, the inner web B has a total thickness equal to the thickness of web A. In other embodiments, web B may be from about twice as thick as the outer web A to up to five times as thick as the outer web A.
[0098] In one embodiment, the total thickness of the inner web is from 1.3 to 6.0 mils, from 1.8 to 2.6 mils, or such as from 2.0 to 2.5 mils.
[0099] In one embodiment, the first layer is up to 10-20% thick (of the total thickness of the three layers), the second layer is 40-70%, the third layer is 10-15%, the fourth layer is 10-20%, and the fifth layer is 10-20%. However, those skilled in the art will recognize that with equipment up to 9 layers, further division of the structure can be achieved because more layers are available. It is noted that the first and second layers can be further divided into multiple layers with the addition of ingredients to modify properties of the sealant web that are not directly related to the sealing properties. Such properties may include moisture barrier or a desire to increase the PCR content of the entire sealant web. The maximum number of total layers is limited by the number of layers possible in the extrusion units (known as coextrusion blown film lines). Furthermore, those skilled in the art will recognize that each extrusion unit capable of making, for example, 9 layers, can be used to make films consisting of fewer layers.
[0100] In another embodiment, the inner web further comprises a barrier layer, the barrier layer being located between the 1-B layer and the 2-B layer. In some embodiments, the barrier layer comprises EVOH, with the further proviso that the total weight of the barrier layer is less than 5% by weight, based on the total weight of the EVOH and the total weight of the polyethylene used in the complete structure. In another embodiment, two tie layers are included, such that a first tie layer is located on one side of the barrier layer and a second tie layer is located on the other side of the barrier layer.
[0101] In other embodiments, the outer web A may have a thickness of from about 1 to about 1.4 mils and the inner web may have a thickness of from about 2 to about 3 mils.
[0102] In another embodiment, the outer web includes an outer skin layer made of HDPE (e.g., having a thickness of about 0.8 mils) and a layer of LLDPE, e.g., having a thickness of about 0.4 mils. In this embodiment, the inner layer may be an A / B / C structure, where layer A is made of LLDPE (e.g., having a thickness of about 0.4 mils), layer B is nucleated HDPE (e.g., having a thickness of about 1.5 mils), and layer C is a sealant resin (such as VLDPE) having a thickness of about 0.3 mils.
[0103] It will be appreciated by those skilled in the art that the above thicknesses may be readily altered to modify the physical properties of the SUP, for example, the thickness of the HDPE layer may be increased (if it is desired to produce a stiffer SUP) or the thickness of the LLDPE layer may be increased to improve impact resistance.
[0104] The combined thickness of the laminated structure (i.e., outer and inner webs) is, in one embodiment, about 3 to about 4 mils. A SUP is then prepared from the laminated structure using techniques and machinery known to those skilled in the art. In one embodiment, the laminated structure is sealed using heat sealing to form the SUP. In another embodiment, the seal can be formed using ultrasonic sealing. EXAMPLES
[0105] The test procedures for evaluating the properties of SUP packages are briefly described below. 1. Melt Index: "I2" was determined in accordance with ASTM D1238. [Note: I2 measurements are made at 190°C using a 2.16 kg weight.] Test results are reported in grams / 10 minutes or, alternatively, in decigrams / minute (dg / min). 2. Density was determined using the displacement method according to ASTM D792. 3. Gloss was determined by ASTM D2457. 4. Haze was determined by ASTM D1003.
[0106] <Materials List> The following polyethylenes were used in the examples: [Table 1]
[0107] The prefix ZN indicates that the polyethylene was prepared using a Ziegler-Natta catalyst system. The prefix SSC indicates that the polyethylene was prepared using a single-site catalyst system. The term (nuc) indicates that the resin contains a nucleating agent (target point 1200 ppm by weight of a commercial nucleating agent sold under the trademark HYPERFORM® 20E by Milliken Chemicals).
[0108] <Outer web> Four blown films were prepared as potential outer webs for stand-up pouches. The films were prepared on a conventional blown film line. The total thickness of all films was 2.35 mils (0.059 mm). Films 1.1 and 1.4 were made from only one resin. Films 1.2, 1.3, and 1.5 were multi-layer constructions containing HDPE and either MDPE or LLDPE. The machine direction (MD) and transverse direction (TD) stiffness values (in g / cm) for each of these films are shown in Table 1. The thickness of the ZN-1 layer in the multi-layer films was 1.15 mils.
[0109] The seal test was completed by pressing two pieces of film together (sealant layer to sealant layer) at a set pressure and temperature for a set period of time. The temperature was varied to determine the minimum seal temperature required to provide a specified / minimum seal strength (reported as the seal initiation temperature). The seal temperature was increased until the seal strength began to decrease (due to melting / breakage of the polymer). The results were plotted on a diagram.
[0110] Seal strength is determined by an instrument that pulls the seal apart and records the force required to do so. Test methods for determining some seal properties are given below.
[0111] <Seal strength> The seal strength tests were performed on an instrument designed for that purpose and sold under the trade name INSTRUME™ 5-Head Universal Tester. The tests were performed generally according to the procedures recommended by the instrument manufacturer.
[0112] <Hot Tack> Hot tack is a measure of the ability of a seal to withstand a load before completely cooling, a feature that is important for form-fill and seal packaging.
[0113] The tests were performed using equipment designed for that purpose and sold under the trade name J&B Hot Tack Tester. The tests were performed generally in accordance with the procedures recommended by the equipment manufacturer. The specific conditions are summarized below. Sealing pressure: 0.27N / mm 2 Sealing time: 0.5 seconds Cooling time: 0.5 seconds Clamp separation speed: 200mm / sec Peel offset: 5mm Sample width: 25mm Sample length: 8mm
[0114] [Table 2]
[0115] The (comparative) inner web having a single sealant layer is shown in Table 3. [Table 3]
[0116] An inner web of the present invention with a two layer sealant system (layers 3 and 4) is shown in Table 4. Layer 4 is the sealant layer (skin layer) and layer 3 is the "adjacent" layer. [Table 4]
[0117] Another four layer film suitable for the inner web is shown in Table 5. Again, layer 4 is the sealant layer and layer 3 is the "adjacent" layer. [Table 5]
[0118] A suitable five layer film for the inner web is shown in Table 6. Layer 5 is the sealant layer and layer 4 is the "adjacent" layer. [Table 6]
[0119] An example of a seven layer film for the inner web is shown in Tables 7-9. Layer 7 is the sealant layer and layer 6 is the "adjacent" layer.
[0120] [Table 7]
[0121] [Table 8]
[0122] [Table 9]
[0123] The structure shown in Table 8 has a very good balance of sealing and hot tack properties, optical properties and hardness. It is possible to improve the optical properties (reducing haze) by replacing SSC-1 with ZN-1, but this comes at the expense of reduced hardness and MVTR.
[0124] The structure shown in Table 9 has a very good balance of sealing and hot tack properties, optical properties and hardness. It is possible to improve the optical properties (reducing haze) by replacing SSC-1 with ZN-1, but this comes at the expense of reduced hardness and MVTR.
[0125] FIG. 1 graphically illustrates the enhancement of the cold seal profile.
[0126] [Table 10]
[0127] <Completed laminated structure> The completed laminate structure is prepared by laminating a first (outer) web to a second (inner) web. Table 10 shows representative data for two completed constructs. [Industrial Applicability]
[0128] Stand-up pouches (SUPs) made from polyethylene incorporate sealing structures to improve the manufacturing and use of SUPs. SUPs are useful for packaging a wide variety of consumer goods.
Claims
1. A laminate structure made of a polymeric material, the laminate structure comprising: A) an outer web comprising: A. 1) Layer 1-A comprising a HDPE composition; A. 2) a layer 2-A comprising a polyethylene selected from LLDPE, MDPE, and HDPE; and B) an inner web comprising, in order: B. 1) a 1-B layer in contact with the outer web, wherein the 1-B layer comprises a polyethylene selected from LLDPE and MDPE; B. 2) A core layer, Layer 2-B, comprising recycled polyethylene; B.3) A sealant construction comprising: B.3.1) A sealant skin layer comprising a polyethylene sealant, wherein the polyethylene sealant is selected from a polyethylene copolymer having a density of 0.88 to 0.915 g / cc and a polyethylene homopolymer having a density of 0.91 to 0.93 g / cc; B.3.2) a layer adjacent to and in contact with the sealant skin layer comprising polyethylene, the density of the polyethylene being a) greater than the density of the polyethylene sealant and b) less than the density of the core layer in contact with the layer adjacent to and in contact with the sealant skin layer; and I) the outer web is laminated to the inner web; II) the HDPE, MDPE, LLDPE, recycled polyethylene, and polyethylene sealant together form at least 95% by weight of the polymeric materials used to prepare the laminate structure; The laminated structure.
2. A laminate structure made of a polymeric material, the laminate structure comprising: A) an outer web comprising: A. 1) Layer 1-A comprising a HDPE composition; A.2) Layer 2-A comprising a polyethylene selected from LLDPE, MDPE, and HDPE; A.3) a 3-A layer comprising a polyethylene selected from LLDPE, MDPE, and HDPE; and B) an inner web comprising, in order: B. 1) a 1-B layer in contact with the outer web, wherein the 1-B layer comprises a polyethylene selected from HDPE, LLDPE, and MDPE; B. 2) A core layer, Layer 2-B, comprising recycled polyethylene; B.3) A sealant construction comprising: B.3.1) A sealant skin layer comprising a polyethylene sealant, wherein the polyethylene sealant is selected from a polyethylene copolymer having a density of 0.88 to 0.915 g / cc and a polyethylene homopolymer having a density of 0.91 to 0.93 g / cc; B.3.2) a layer adjacent to and in contact with the sealant skin layer comprising polyethylene, the density of the polyethylene being a) greater than the density of the polyethylene sealant and b) less than the density of the core layer in contact with the layer adjacent to and in contact with the sealant skin layer; and I) each of the outer web and the inner web comprises at least one additional layer between A.1 and A.3 and at least one additional layer between B.1 and B.3, wherein the additional layer comprises a polyethylene composition comprising HDPE, MDPE, LLDPE, or a combination thereof; II) the outer web is laminated to the inner web; III) the HDPE, MDPE, LLDPE, recycled polyethylene, and polyethylene sealant together form at least 95% by weight of the polymeric materials used to prepare the laminate structure; The laminated structure.
3. 3. The construction of claim 1 or 2, wherein the layer adjacent to the sealant skin layer has a density of 0.917 to 0.921 g / cc and the polyethylene sealant has a density of 0.88 to 0.915 g / cc.
4. The structure of any one of claims 1 to 3, wherein the polyethylene sealant has a density of 0.900 to 0.914 g / cc.
5. 5. The structure of any one of claims 1 to 4, wherein the inner web further comprises an additional layer between B.1 and B.3 comprising HDPE containing a nucleating agent.
6. The structure of any one of claims 1 to 5, wherein said 2-B layer comprises HDPE containing a nucleating agent.
7. 7. The structure of any one of claims 2 to 6, wherein the outer web further comprises an additional layer between A.1 and A.3 comprising HDPE containing a nucleating agent.
8. The structure of any one of claims 1 to 7, wherein the inner web further comprises a barrier layer, the barrier layer being located between the 1-B layer and the 2-B layer.
9. The structure of any one of claims 1 to 8, wherein the inner web further comprises at least one layer comprising recycled polyethylene.
10. 10. The structure of any one of claims 1 to 9, wherein the inner web further comprises at least one layer comprising a blend of HDPE, MDPE, or LLDPE with recycled polyethylene.
11. 9. The structure of claim 8, further providing that said barrier layers comprise EVOH, the total weight of said barrier layers being less than 5 weight percent based on the total weight of said EVOH and the total weight of polyethylene used in said structure.
12. 9. The structure of claim 8, wherein a first tie layer is on one side of the barrier layer and a second tie layer is on the other side of the barrier layer.
13. A stand-up pouch prepared from the structure of any one of claims 1 to 12.
Citation Information
Patent Citations
Self-supporting bag
JP2002120849A
Multi-layer container made of resin
JP2012229037A
Laminated structure and stand-up pouch produced therefrom
JP2018511504A
JPP3555279B
Film structures for use in recylcable packaging
US20160339663A1