Encapsulating resin composition and semiconductor device
The encapsulating resin composition with epoxy resin, phenolic curing agent, inorganic filler, and polyfunctional silane coupling agent addresses peeling issues by improving adhesion and reducing elastic modulus, ensuring reliable semiconductor devices in harsh environments.
Patent Information
- Application Number
- JP2020165738
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-09-30
- Publication Date
- 2024-09-24
- Estimated Expiration
- 2040-09-30
AI Technical Summary
The encapsulant in semiconductor devices can peel off due to moisture absorption and thermal stress, leading to reduced reliability, especially in harsh environments such as automotive applications, where high adhesion is required.
An encapsulating resin composition comprising an epoxy resin, a phenolic curing agent, an inorganic filler, and a polyfunctional silane coupling agent with a pentaerythritol skeleton is used to enhance adhesion to metals and semiconductor elements, reducing elastic modulus at high temperatures and preventing peeling.
The composition ensures high adhesion and reliability of the encapsulant, preventing peeling during thermal cycles like reflow treatment, thus enhancing the reliability of semiconductor devices.
Smart Images

Figure 0007554996000006 
Figure 0007554996000004 
Figure 0007554996000005
Abstract
Description
[Technical field]
[0001] The present invention relates to an encapsulating resin composition and a semiconductor device, and more particularly to an encapsulating resin composition containing an epoxy resin, and a semiconductor device including an encapsulant made from the encapsulating resin composition. [Background technology]
[0002] When encapsulating semiconductor elements, resin encapsulation is sometimes performed for the purpose of improving productivity, reducing costs, etc. Resin encapsulation is performed by, for example, molding an encapsulating resin composition containing an epoxy resin, a phenol-based hardener, a hardening accelerator, and an inorganic filler to produce an encapsulant.
[0003] A semiconductor device encapsulated with an encapsulant includes, for example, a lead frame, a semiconductor element mounted on the lead frame, and wires that electrically connect the semiconductor element and the lead frame, and the encapsulant encapsulates the semiconductor element (see Patent Document 1). For this reason, the encapsulant is in contact with the lead frame and the wires.
[0004] Patent Document 1 proposes that, in order to improve the adhesion between the encapsulating material and the lead frame, an aromatic polycarboxylic acid having one nitro group in the molecule is further contained in an encapsulating epoxy resin composition containing an epoxy resin, a phenolic resin-based curing agent, a curing accelerator, and an inorganic filler. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2014-114426 A Summary of the Invention [Problem to be solved by the invention]
[0006] In particular, when a surface-mount type semiconductor device is mounted on a substrate or the like in a reflow process, the expansion of moisture absorbed by the encapsulant and thermal stress occurring in the encapsulant may cause the encapsulant to peel off from metal parts such as lead frames and semiconductor elements. Peeling of the encapsulant leads to a decrease in reliability of the semiconductor device. In recent years, high reliability is required for semiconductor devices used in harsh environments, such as semiconductor devices mounted on vehicles, and therefore it is necessary to ensure even higher adhesion between the encapsulant and metal parts such as lead frames and semiconductor elements.
[0007] An object of the present invention is to provide an encapsulating resin composition that can be used to prepare an encapsulating material having high adhesion to metals and semiconductor elements, and a semiconductor device including an encapsulating material prepared from the encapsulating resin composition. [Means for solving the problem]
[0008] An encapsulating resin composition according to one embodiment of the present invention contains an epoxy resin (A), a phenolic curing agent (B), an inorganic filler (C), and a polyfunctional silane coupling agent having a pentaerythritol skeleton (D).
[0009] A semiconductor device according to one aspect of the present invention includes a semiconductor element and an encapsulant that encapsulates the semiconductor element. The encapsulant is a cured product of the encapsulating resin composition. Effect of the Invention
[0010] According to the present invention, it is possible to provide an encapsulating resin composition that can be used to prepare an encapsulating material having high adhesion to metal, and a semiconductor device including an encapsulating material prepared from the encapsulating resin composition. [Brief description of the drawings]
[0011] [Figure 1] 1 is a schematic cross-sectional view of a semiconductor device according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] Hereinafter, one embodiment of the present invention will be described.
[0013] The encapsulating resin composition according to this embodiment (referred to as composition (X)) contains an inorganic filler (C), an epoxy resin (A), a phenol-based curing agent (B), and a polyfunctional silane coupling agent having a pentaerythritol skeleton (D).
[0014] According to this embodiment, the affinity between the sealing material made of the composition (X) and the metal is easily increased, particularly by the polyfunctional silane coupling agent (D). In addition, the elastic modulus of the sealing material at high temperatures (e.g., 260°C) can be reduced, and therefore the stress generated between the sealing material and the metal at high temperatures is easily alleviated. Therefore, the adhesion of the sealing material to the metal and the semiconductor element can be improved. Furthermore, the polyfunctional silane coupling agent (D) is unlikely to bleed out from the sealing material, so that it is unlikely to cause stains due to bleed-out, and the polyfunctional silane coupling agent (D) is unlikely to lower the glass transition temperature of the sealing material, so that it is unlikely to lower the heat resistance of the sealing material.
[0015] Therefore, even if a semiconductor device having the sealing material is heated by a reflow process or the like, peeling of the sealing material is unlikely to occur, and therefore the semiconductor device can have high reliability.
[0016] The composition of the composition (X) will be explained in more detail.
[0017] Since the composition (X) contains the epoxy resin (A) and the phenol-based curing agent (B), an encapsulant produced from the composition (X) tends to have high adhesion to metals and semiconductor elements.
[0018] The epoxy resin (A) will be described. The epoxy resin (A) may contain at least one component selected from the group consisting of, for example, glycidyl ether type epoxy resins, glycidyl amine type epoxy resins, glycidyl ester type epoxy resins, and olefin oxide type (alicyclic) epoxy resins. More specifically, the epoxy resin may be, for example, an alkylphenol novolac type epoxy resin such as a phenol novolac type epoxy resin or a cresol novolac type epoxy resin; a naphthol novolac type epoxy resin; a phenol aralkyl type epoxy resin having a skeleton such as a phenylene skeleton or a biphenylene skeleton; a biphenyl aralkyl type epoxy resin; a naphthol aralkyl type epoxy resin having a skeleton such as a phenylene skeleton or a biphenylene skeleton; a multifunctional type epoxy resin such as a triphenol methane type epoxy resin or an alkyl modified triphenol methane type epoxy resin; a triphenyl methane type epoxy resin; a tetrakisphenol ethane type epoxy resin; a disilicide type epoxy resin; The epoxy resin composition may contain one or more components selected from the group consisting of: lopentadiene-type epoxy resins; stilbene-type epoxy resins; bisphenol-type epoxy resins such as bisphenol A-type epoxy resins and bisphenol F-type epoxy resins; biphenyl-type epoxy resins; naphthalene-type epoxy resins; alicyclic epoxy resins; bromine-containing epoxy resins such as bisphenol A-type bromine-containing epoxy resins; glycidylamine-type epoxy resins obtained by reacting polyamines such as diaminodiphenylmethane and isocyanuric acid with epichlorohydrin; and glycidyl ester-type epoxy resins obtained by reacting polybasic acids such as phthalic acid and dimer acid with epichlorohydrin.
[0019] The amount of the epoxy resin (A) relative to the entire composition (X) is preferably 5% by mass or more and 35% by mass or less, in which case the fluidity of the composition (X) during molding and the physical properties of the sealing material 62 are improved.
[0020] The phenol-based curing agent (B) will be described. The phenol-based curing agent (B) can contain at least one component selected from the group consisting of novolac-type resins such as phenol novolac resins, cresol novolac resins, and naphthol novolac resins; phenol aralkyl resins having a phenylene skeleton or biphenylene skeleton; aralkyl-type resins such as naphthol aralkyl resins having a phenylene skeleton or biphenylene skeleton; polyfunctional phenol resins such as triphenol methane resins; dicyclopentadiene-type phenol resins such as dicyclopentadiene-type phenol novolac resins and dicyclopentadiene-type naphthol novolac resins; terpene-modified phenol resins; bisphenol-type resins such as bisphenol A and bisphenol F; and triazine-modified novolac resins.
[0021] The amount of epoxy resin (A) is preferably 0.9 equivalents or more and 1.5 equivalents or less per equivalent of phenol-based hardener (B). In this case, the sealing material 62 can have particularly high adhesion even at high temperatures, and the composition (X) can have good storage stability. It is more preferable that the amount of epoxy resin (A) is 1.0 equivalents or more and 1.3 equivalents or less.
[0022] The inorganic filler (C) may contain at least one component selected from the group consisting of fused silica, such as fused spherical silica, crystalline silica, alumina, and silicon nitride. When the composition (X) contains the inorganic filler (C), the thermal expansion coefficient of the sealing material 62 can be adjusted. In particular, it is preferable that the inorganic filler (C) contains fused silica. In this case, it is easy to obtain high filling property of the inorganic filler (C) in the composition (X) and high fluidity of the composition (X) during molding.
[0023] The inorganic filler (C) has an average particle size of, for example, 0.2 μm or more and 70 μm or less. The average particle size is more preferably 0.5 μm or more and 20 μm or less. The average particle size is a volume-based median diameter calculated from the measured particle size distribution by a laser diffraction / scattering method, and is obtained using a commercially available laser diffraction / scattering particle size distribution measuring device. The inorganic filler (C) may contain two or more components having different average particle sizes in order to adjust the viscosity of the composition (X) during molding, the physical properties of the sealing material 62, and the like.
[0024] The proportion of the inorganic filler (C) is preferably 60% by mass or more and 93% by mass or less with respect to the total amount of the composition (X). When the proportion of the inorganic filler (C) is 60% by mass or more, the linear expansion coefficient of the sealing material 62 is easily sufficiently reduced, and the semiconductor device 1 is less likely to warp even when heated by a reflow process or the like. When the proportion of the inorganic filler (C) is 93% by mass or less, sufficient fluidity of the composition (X) during molding is easily obtained.
[0025] The polyfunctional silane coupling agent (D) will be described. The polyfunctional silane coupling agent (D) enhances the affinity between the sealing material and the metal, and reduces the elastic modulus of the sealing material at high temperatures. The improved affinity between the sealing material and the metal is believed to be realized by the polyfunctionality of the polyfunctional silane coupling agent (D). The reduction in the elastic modulus of the sealing material at high temperatures is believed to be realized by the pentaerythritol skeleton in the polyfunctional silane coupling agent (D). The term "polyfunctional" here means that one molecule has a plurality of functional groups that react with the resin component. The functional group in the polyfunctional silane coupling agent (D) includes at least one group selected from the group consisting of, for example, an amino group, an epoxy group, a mercapto group, and an isocyanate group. It is preferable that the functional group is a mercapto group. In this case, the adhesion of the sealing material to the metal and the semiconductor element is particularly likely to be enhanced. The polyfunctional silane coupling agent (D) has at least one alkoxysilyl group in one molecule. This alkoxysilyl group is preferably a trialkoxysilyl group.
[0026] The polyfunctional silane coupling agent (D) has, for example, a pentaerythritol skeleton and four molecular chains bonded to the pentaerythritol skeleton, and each of the four molecular chain ends has an alkoxysilyl group or a functional group. In this case, the polyfunctional silane coupling agent (D) has at least one alkoxysilyl group and at least two functional groups, and the total number of the alkoxysilyl group and the functional group is 4. The alkoxysilyl group is preferably a trialkoxysilyl group, for example, a trimethoxysilyl group. For example, the polyfunctional silane coupling agent (D) has a structure in which a molecular chain is bonded to each of the four ends of the pentaerythritol skeleton having the structure shown in the following (1), and each of the four molecular chain ends preferably has an alkoxysilyl group or a functional group.
[0027] [ka]
[0028] The polyfunctional silane coupling agent (D) has, for example, a structure shown in the following formula (2).
[0029] [ka]
[0030] In formula (2), n is a number of 1 or more, for example, 1 or more and 3 or less. 1 , R 2 , R 3 and R 4 Each of R is a molecular chain having H or an alkoxysilyl group. The molecular chain having an alkoxysilyl group is, for example, a group having a structure shown in the following formula (3). For example, R 1 , R 2 , R 3 and R 4 On average, 3 to 4 of these are H.
[0031] [ka]
[0032] The above-mentioned structure of the polyfunctional silane coupling agent (D) is an example, and the polyfunctional silane coupling agent (D) may have a structure other than the above. For example, the polyfunctional silane coupling agent (D) shown in formula (2) has a mercapto group as a functional group, but as mentioned above, the polyfunctional silane coupling agent (D) may have an amino group, an epoxy group, or an isocyanate group as a functional group.
[0033] The ratio of the polyfunctional silane coupling agent (D) is preferably 0.05% by mass or more and 3% by mass or less with respect to the composition (X). If this ratio is 0.05% by mass or more, the adhesion between the encapsulant and the metal and the semiconductor element is particularly likely to be increased. Also, if this ratio is 3% by mass or less, the good moldability of the composition (X) is particularly likely to be maintained. This ratio is more preferably 0.1% by mass or more, and even more preferably 0.3% by mass or more. Also, this ratio is more preferably 2% by mass or less.
[0034] The composition (X) may contain additives other than the above components within the range that does not impair the effect of this embodiment. The additives include at least one selected from the group consisting of, for example, a curing accelerator, an ion trapping agent, a coupling agent other than the polyfunctional silane coupling agent (D), a release agent, a flame retardant, a colorant, and a stress reducing agent.
[0035] Examples of the hardening accelerator include imidazoles such as 2-methylimidazole, 2-ethylimidazole, 2-phenylimidazole, and 2-ethyl-4-methylimidazole; cycloamidines such as 1,8-diazabicyclo[5.4.0]undecene-7, 1,5-diazabicyclo[4.3.0]nonene-5, and 5,6-dibutylamino-1,8-diazabicyclo[5.4.0]undecene-7; tertiary amines such as 2-(dimethylaminomethyl)phenol, triethylenediamine, benzyldimethylamine, triethanolamine, dimethylaminoethanol, and tris(dimethylaminomethyl)phenol; tributylphosphine, methyldiphenylphosphine, and triphenylphosphine. The composition (X) may contain at least one selected from the group consisting of organic phosphines such as phenylphosphine, tris(4-methylphenyl)phosphine, diphenylphosphine, an addition product of triphenylphosphine and parabenzoquinone, and phenylphosphine; tetra-substituted phosphonium and tetra-substituted borates such as tetraphenylphosphonium·tetraphenylborate, tetraphenylphosphonium·ethyltriphenylborate, and tetrabutylphosphonium·tetrabutylborate; quaternary phosphonium salts having a counter anion other than borate; and tetraphenylboron salts such as 2-ethyl-4-methylimidazole·tetraphenylborate and N-methylmorpholine·tetraphenylborate. The ratio of the curing accelerator is, for example, 0.001% by mass or more and 0.5% by mass or less with respect to the composition (X).
[0036] The coupling agent other than the polyfunctional silane coupling agent (D) can improve the affinity between the inorganic filler (C) and the epoxy resin (A) and the phenol-based curing agent (B). The coupling agent can also further improve the adhesion of the encapsulant 62 to metal and semiconductor elements. The coupling agent preferably contains at least one component selected from the group consisting of a silane coupling agent, a titanate coupling agent, an aluminum coupling agent, and an aluminum / zirconium coupling agent. The silane coupling agent contains at least one component selected from the group consisting of glycidoxysilanes such as γ-glycidoxypropyltrimethoxysilane, γ-glycidoxypropylmethyldiethoxysilane, β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, etc.; aminosilanes such as N-β(aminoethyl)-γ-aminopropyltrimethoxysilane, γ-aminopropyltriethoxysilane, and N-phenyl-γ-aminopropyltrimethoxysilane; alkylsilanes; ureidosilanes; and vinylsilanes. The ratio of the coupling agent to the inorganic filler (C) is preferably 0.2% by mass or more and 2% by mass or less.
[0037] The release agent may contain, for example, at least one component selected from the group consisting of carnauba wax, stearic acid, montanic acid, carboxyl group-containing polyolefin, ester wax, polyethylene oxide, and metal soap.
[0038] The flame retardant may contain, for example, at least one component selected from the group consisting of magnesium hydroxide, aluminum hydroxide, and red phosphorus.
[0039] The colorant may contain, for example, at least one component selected from the group consisting of carbon black, red iron oxide, titanium oxide, phthalocyanine, and perylene black.
[0040] The stress reducing agent may contain at least one component selected from the group consisting of silicone elastomer, silicone resin, silicone oil, and butadiene-based rubber. The butadiene-based rubber may contain at least one component selected from the group consisting of methyl acrylate-butadiene-styrene copolymer and methyl methacrylate-butadiene-styrene copolymer.
[0041] The composition (X) can be prepared by mixing the components of the composition (X) as described above. More specifically, for example, raw materials including epoxy resin (A), phenolic curing agent (B), inorganic filler (C) and polyfunctional silane coupling agent (D) are mixed in a mixer, blender or the like until sufficiently uniform, and then melt-mixed in a heated state using a kneading machine such as a heat roll or kneader, and then cooled to room temperature. The mixture thus obtained is pulverized by a known means to produce a powdered composition (X). The composition (X) does not have to be in a powder form, and may be, for example, in a tablet form. When the composition (X) is in a tablet form, it is preferable that the size and mass of the composition (X) are suitable for the molding conditions.
[0042] It is preferable that the composition (X) is solid at 25° C. In this case, the sealing material 62 can be produced by molding the composition (X) by a pressure molding method such as injection molding, transfer molding, or compression molding. It is more preferable that the composition (X) is solid at any temperature in the range of 15° C. or higher and 25° C. or lower, and it is particularly preferable that the composition (X) is solid at any temperature in the range of 5° C. or higher and 35° C. or lower.
[0043] The gel time of the composition (X) is preferably 30 seconds or more and 60 seconds or less. When the gel time is 60 seconds or less, the molding cycle when producing the sealing material 62 is particularly short, and the productivity of the semiconductor device 1 is particularly high. In addition, when the gel time is 30 seconds or more, good moldability is particularly likely to be maintained. Details of the method for measuring the gel time will be described in detail in the Examples section below. In this embodiment, the amount of the multifunctional silane coupling agent (D) in the composition (X) can affect the gel time. Since the gel time tends to be shorter as the amount of the multifunctional silane coupling agent (D) increases, it is preferable to adjust the amount of the multifunctional silane coupling agent (D) so that the gel time is not excessively short.
[0044] The elastic modulus of the cured product of the composition (X) at 260°C is preferably 100 MPa or more and 1000 MPa or less. In this case, the adhesion of the encapsulant to the metal and the semiconductor element at high temperatures is more likely to be improved. This value is more preferably 150 MPa or more and 700 MPa or less, and even more preferably 200 MPa or more and 500 MPa or less. Details of the method for measuring the elastic modulus at 260°C will be described in detail in the Examples section below.
[0045] An example of a semiconductor device 1 including an encapsulant 62 made from the composition (X) and a method for producing the same will be described.
[0046] The semiconductor device 1 includes a semiconductor element and an encapsulant 62 that encapsulates the semiconductor element. The encapsulant is a cured product of a composition (X).
[0047] The semiconductor device 1 may include a conductor. The conductor is, for example, a lead frame. Note that the conductor is not limited to a lead frame and may be, for example, a conductor wiring in a printed wiring board. The conductor may have a plating layer containing nickel.
[0048] The semiconductor device 1 is, for example, a surface mount device, such as a DPAK, a D2PAK, a QFN, a quad flat package (QFP), a small outline package (SOP), or a small outline J-lead package (SOJ).
[0049] 1 shows a cross-sectional view of an example of a DPAK, which is a semiconductor device 1. This semiconductor device 1 includes a lead frame 52 made of a metal that is a conductor, a semiconductor element 50 mounted on the lead frame 52, wires 56 that electrically connect the semiconductor element 50 and the lead frame 52, and an encapsulant 62 that encapsulates the semiconductor element 50.
[0050] In this embodiment, the lead frame 52 includes a paddle 58 (also called a die pad) and a lead finger 520, and the lead finger 520 includes an inner lead 521 and an outer lead 522. The lead frame 52 is made of, for example, copper or an iron alloy such as 42 alloy. The lead frame 52 preferably includes a plating layer 54. In this case, corrosion of the lead frame 52 is suppressed. The plating layer 54 includes at least one metal of, for example, silver, nickel, and palladium. The plating layer 54 may include only one metal of silver, nickel, and palladium, or may include an alloy including at least one metal of silver, nickel, and palladium. The plating layer 54 may have a laminated structure, and specifically may have a laminated structure including, for example, a palladium layer, a nickel layer, and a gold layer. The thickness of the plating layer 54 is, for example, 1 μm or more and 20 μm or less, but is not particularly limited thereto.
[0051] The semiconductor element 50 is fixed onto the paddle 58 of the lead frame 52 with an appropriate die bond material 60. This allows the semiconductor element 50 to be mounted on the lead frame 52. The semiconductor element 50 is, for example, an integrated circuit, a large scale integrated circuit, a transistor, a thyristor, a diode, or a solid-state imaging element. The semiconductor element 50 may be a power device such as SiC or GaN.
[0052] Next, the semiconductor element 50 and the inner lead 521 of the lead frame 52 are connected by a wire 56. The wire 56 may be made of gold, or may contain at least one of copper and silver. For example, the wire 56 may be made of silver or copper. When the wire 56 contains at least one of copper and silver, the wire 56 may be coated with a thin film of a metal such as palladium. The wire may be made of aluminum. The wire 56 may be in the form of a thin line or a ribbon. A plate-shaped member (clip) may be used instead of the wire 56.
[0053] Next, the composition (X) is molded to produce an encapsulant 62 that encapsulates the semiconductor element 50. The encapsulant 62 also encapsulates the wires 56. The encapsulant 62 also encapsulates the paddle 58 and the inner lead 521, and therefore the encapsulant 62 is in contact with the lead frame 52, and in the case where the lead frame 52 has a plating layer 54, the encapsulant 62 is in contact with the plating layer 54.
[0054] It is preferable to produce the sealing material 62 by molding the composition (X) by a pressure molding method. The pressure molding method is, for example, an injection molding method, a transfer molding method, or a compression molding method.
[0055] When the composition (X) is molded by the pressure molding method, the molding pressure is preferably 3.0 MPa or more, and the molding temperature is preferably 120°C or more. In this case, it is possible to obtain a semiconductor device 1 in which the semiconductor element 50 is encapsulated with a uniform encapsulant 62 with few unfilled so-called weld voids or internal voids. In particular, in the case of the transfer molding method, the injection pressure of the composition (X) into the mold is preferably 3 MPa or more, and more preferably 4 MPa or more and 15 MPa or less. In addition, the heating temperature (mold temperature) is preferably 120°C or more, and more preferably 160°C or more and 190°C or less. In addition, the heating time is preferably 30 seconds or more and 300 seconds or less, and more preferably 60 seconds or more and 180 seconds or less.
[0056] In the transfer molding method, it is preferable to prepare the encapsulant 62 in a mold, and then heat the encapsulant 62 with the mold closed to perform post-cure, and then open the mold to remove the semiconductor device 1. The heating conditions for post-cure are, for example, a heating time of 160° C. or more and 190° C. or less, and a heating time of 2 hours or more and 8 hours or less.
[0057] In the case of compression molding, the compression pressure is preferably 3 MPa or more, more preferably 5.0 MPa or more and 10 MPa or less. The heating temperature (mold temperature) is preferably 120°C or more, more preferably 150°C or more and 185°C or less. The heating time is preferably 60 seconds or more and 300 seconds or less.
[0058] In particular, when the semiconductor device 1 is a surface mount device, when the semiconductor device 1 is mounted on a substrate or the like by a process involving heating such as a reflow process, moisture absorbed by the sealing material 62 may expand, and thermal stress may occur within the sealing material 62. However, in this embodiment, as described above, the sealing material 62 is likely to have adhesion to metal and semiconductor elements. Therefore, even if a temperature change occurs during use of the semiconductor device 1, problems such as the wire 56 being cut are unlikely to occur. Therefore, the reliability of the semiconductor device 1 can be improved.
[0059] 1, the semiconductor device 1 may include a semiconductor element 50 and a sealant 62 that seals the semiconductor element 50. For example, the semiconductor device 1 may include a substrate such as a printed wiring board, a semiconductor element 50 mounted on the substrate, and a sealant 62 that seals the semiconductor element 50 on the substrate. In this case, if the substrate includes a conductor wiring that is in contact with the sealant 62, high adhesion between the sealant 62 and the conductor wiring can be achieved. EXAMPLES
[0060] Specific examples of the present embodiment are presented below, but the present invention is not limited to these examples.
[0061] 1. Preparation of the Composition The raw materials shown in the "Raw Materials" column in Table 1 were blended and mixed uniformly in a mixer, then heated and kneaded in a kneader at 80°C to 120°C, and the resulting mixture was cooled and pulverized. The powder thus obtained was compressed into tablets to obtain a tablet-shaped composition.
[0062] The details of the raw materials shown in Table 1 are as follows. - Fused silica: manufactured by Denka Co., Ltd. Part number FB940. -Biphenyl type epoxy resin: Mitsubishi Chemical Corporation. Part number YX4000. -Biphenyl aralkyl type epoxy resin: manufactured by Nippon Kayaku Co., Ltd. Product number NC3000. -Biphenyl aralkyl type phenolic resin: manufactured by Meiwa Kasei Co., Ltd. Product number MEH7851SS. -Triphenylphosphine: Manufactured by Hokko Chemical Industry Co., Ltd. -Release agent: Carnauba wax. Manufactured by Dainichi Chemical Industry Co., Ltd. Product number F1-100. -Carbon black: Mitsubishi Chemical Corporation. Product number MA600. -Mercaptosilane: γ-mercaptopropyltrimethoxysilane. Manufactured by Shin-Etsu Chemical Co., Ltd. Product number KBM-803. - Mercapto group-containing polyfunctional silane coupling agent: a polyfunctional silane coupling agent having a pentaerythritol skeleton, a molecular chain bonded to the pentaerythritol skeleton and having a trimethoxysilyl group at its end, and a molecular chain bonded to the pentaerythritol skeleton and having a mercapto group at its end. Manufactured by Shin-Etsu Chemical Co., Ltd., product number X12-1154.
[0063] 2. Evaluation The following evaluation tests were carried out, and the results are shown in Table 1.
[0064] (1) Gel time The torque was measured while the composition was heated at 170° C. using a Curastometer VPS type manufactured by JSR Trading Co., Ltd. The time required from the start of heating until the measured torque reached 0.01 (N / m) was measured and this time was recorded as the gel time.
[0065] (2) Adhesion to SiN die (room temperature) A molded article (resin post) was formed by transferring the composition onto a silicon chip (SiN die) equipped with a passivation layer made of silicon nitride under the conditions of a mold temperature of 175°C, injection pressure of 7 MPa, and curing time of 120 seconds. The molded article was then post-cured by heating at 175°C for 6 hours. A shear test was performed at 25°C using a bond tester manufactured by Dage, and the bond strength between the SiN die and the molded article was measured.
[0066] (3) Adhesion to SiN die (260℃) Except for the shear test being carried out at 260°C, the bonding strength between the SiN die and the molded product was measured under the same conditions as in "(2) Adhesion to SiN die (room temperature)" above.
[0067] (4) Elastic modulus at high temperatures The composition was molded by transfer molding under conditions of a mold temperature of 175°C, injection pressure of 7MPa, and curing time of 120 seconds to produce a molded product with dimensions of 4 mm length, 10 mm width, and 80 mm length or more. The molded product was then post-cured by heating at 175°C for 6 hours. The elastic modulus of this molded product at 260°C was measured in a 260°C thermostatic chamber using a three-point bending test according to JIS K6911.
[0068] (5) Reflow resistance evaluation A semiconductor chip having a silicon nitride passivation film on its surface was mounted on a copper lead frame with a nickel plating layer, and the composition was transferred onto the lead frame using a multi-transfer press (Apic Yamada) under transfer molding conditions of a mold temperature of 175°C, injection pressure of 7MPa, and curing time of 120 seconds to produce an encapsulant. The encapsulant was then post-cured by heating at 175°C for 6 hours. This produced a TO-220 package for testing.
[0069] This TO-220 package was exposed to an atmosphere of 85°C and 85% RH for 168 hours to absorb moisture, and then subjected to a reflow treatment at a peak temperature of 255°C to 260°C.
[0070] Next, using an ultrasonic inspection device, we checked whether there was any peeling between the encapsulant and the die, between the encapsulant and the paddle in the lead frame, and between the encapsulant and the lead fingers in the lead frame after the test. We fabricated 100 TO-220 packages and performed the same test to check the number of TO-220 packages that had peeling.
[0071] [Table 1]
Claims
1. The encapsulating resin composition contains an epoxy resin (A), a phenol-based curing agent (B), an inorganic filler (C), and a polyfunctional silane coupling agent having a pentaerythritol skeleton (D), The polyfunctional silane coupling agent (D) has a structure represented by the following formula (2): [Formula 1] In the formula (2), n is a number of 1 or more, each of R 1 , R 2 , R 3 and R 4 is a molecular chain having H or an alkoxysilyl group, and has a plurality of mercapto groups in one molecule, The ratio of the epoxy resin (A) is 5% by mass or more and 35% by mass or less with respect to the encapsulating resin composition, the amount of the epoxy resin (A) is 0.9 equivalents or more and 1.5 equivalents or less relative to 1 equivalent of the phenol-based curing agent (B); The proportion of the inorganic filler (C) is 60% by mass or more relative to the encapsulating resin composition, The ratio of the polyfunctional silane coupling agent (D) is 0.05% by mass or more and 3% by mass or less with respect to the encapsulating resin composition. Sealing resin composition.
2. A semiconductor element; and a sealing material that seals the semiconductor element. The encapsulant is a cured product of the encapsulating resin composition according to claim 1. Semiconductor device.
3. A surface mount device, The semiconductor device according to claim 2 .
Citation Information
Patent Citations
Curing composition
JP1995062205A
Semiconductor sealing epoxy resin composition and power module using the same
JP2014114426A