Plastic Nut

The resin nut design with an injection gate mark on a stepped surface addresses precision and cost issues by ensuring high-precision screw holes and reducing production costs through improved dimensional stability and productivity.

JP7555226B2Active Publication Date: 2024-09-24NTN CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2020168959
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-10-07
Filing Date
2020-10-06
Publication Date
2024-09-24
Estimated Expiration
2040-10-06

AI Technical Summary

Technical Problem

Conventional resin nuts face issues with maintaining high precision in screw holes due to gate marks, leading to uneven rotation and increased inspection costs, and require manual gate cutting, which raises production costs.

Method used

The resin nut design includes an injection gate mark formed near the screw hole opening on a stepped surface, eliminating factors that cause dimensional distortion and allowing for high-precision screw holes without manual gate cutting, using a thermoplastic resin composition like polyarylene sulfide (PAS) for improved dimensional stability and reduced costs.

Benefits of technology

The solution ensures high precision in screw holes, prevents uneven rotation, reduces production costs, and enhances productivity by eliminating the need for manual gate cutting and inspection, while maintaining dimensional accuracy even in environments with oil or solvents.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007555226000008
    Figure 0007555226000008
  • Figure 0007555226000006
    Figure 0007555226000006
  • Figure 0007555226000007
    Figure 0007555226000007
Patent Text Reader

Abstract

To provide a resin nut which avoids occurrence of a failure, such as a rotation failure, to achieve reduction of costs.SOLUTION: A resin nut includes an injection molded item formed as a body formed with a screw hole. A recessed part is formed on an end surface at the screw hole opening side of the body to provide a stepped surface. A screw hole end part is opened on the stepped surface. An injection gate mark is formed on the stepped surface.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention Is, tree Regarding grease nuts. [Background technology]

[0002] Sending As described in Patent Document 1, there is a feed screw whose nut is made of synthetic resin. Figure 3 As shown in FIG. 1, the screw shaft 2 has a male thread 1, and a nut 4 has a screw hole 3 that screws into the male thread 1 of the screw shaft 2. The screw shaft 2 is made by rolling stainless steel or carbon steel, and the nut 4 is made of PPS (polyphenylene sulfide) material, which has excellent dimensional stability during molding, and is mixed with whiskers during molding.

[0003] The nut 4 was injection molded from a PPS composition containing whiskers, thereby improving the dimensional accuracy and rigidity. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2001-116102 A Summary of the Invention [Problem to be solved by the invention]

[0005] However, in the conventional nut 4 (resin nut 4), when the resin nut 4 is injection molded, there is a problem that the precision of the screw hole 3 cannot be maintained at a high level depending on the position of the gate mark. If the precision of the screw hole 3 is low, the rotation of the male screw 1 entering the screw hole 3 becomes uneven, and there is a risk of problems such as poor rotation of the male screw 1 occurring.

[0006] To address this problem, it may be proposed to screw a male thread 1 onto the resin nut 4 after injection molding, inspect the rotational irregularities of the male thread 1, and sort all of the resin nuts 4 into those that pass and those that fail in terms of rotational irregularities. However, such a proposal would require high costs for inspection and sorting, making it difficult to keep the price of the resin nuts 4 low.

[0007] In addition, when a resin nut is injection molded, a gate mark is formed in one of the locations. For this reason, a process of manually cutting the gate mark is usually required. However, when such a gate cutting process is performed manually, costs are incurred for the gate cutting process, making it difficult to keep the price of the resin nut low.

[0008] Therefore, in view of the above problems, the present invention provides a resin nut that can avoid the occurrence of defects such as poor rotation and reduce costs. [Means for solving the problem]

[0009] The resin nut of the present invention is a resin nut having an injection-molded product as a main body in which a screw hole is formed, and an injection gate mark is formed near the opening of the screw hole of the main body.

[0010] Since an injection gate mark is formed near the opening of the screw hole in the body, factors that can cause dimensional errors in the screw hole during injection molding, such as short shots, are eliminated, and the precision of the screw hole is maintained at a high level. Since the precision of the screw hole is high, uneven rotation of the male screw entering the screw hole is avoided, and rotation precision is improved.

[0011] The injection gate mark is preferably provided on a stepped surface formed as a recess in the end face of the main body on the screw hole opening side. Since the injection gate mark is formed on the stepped surface formed as a recess in the end face of the main body on the screw hole opening side, the injection gate mark is located at a position set back from the end face of the main body, and this injection gate mark can be effectively prevented from contacting other members.

[0012] In addition, the resin nut of the present invention is a resin nut having an injection-molded main body in which a screw hole is formed, and has a stepped surface formed as a recess on the end face of the main body on the screw hole opening side, with the screw hole end opening into this stepped surface, and an injection gate mark formed on this stepped surface.

[0013] Since the opening of the screw hole in the main body is located at a position set back from the end face of the main body, even if another member comes into contact with the end face of the main body on the side of the screw hole opening and causes a dent to be formed on this end face, no dent will be formed on the opening of the screw hole. Also, since the injection gate mark is formed on the stepped surface, the injection gate mark is located at a position set back from the end face of the main body, and this injection gate mark can be effectively prevented from coming into contact with other members.

[0014] The injection gate mark is preferably formed on a surface that is approximately at the end of the body and is approximately perpendicular to the axial direction of the screw hole. When the resin nut is removed from the injection mold, the injection mold opens while moving approximately along the axial direction of the screw hole. If the injection gate mark is formed on a surface that is approximately at the end of the body and is approximately perpendicular to the axial direction of the screw hole, when the resin nut is removed from the injection mold, the gate is cut at the same time as the injection mold moves approximately along the axial direction of the screw hole and opens. Therefore, the process of manually performing the gate cutting process is omitted, and productivity is improved, thereby reducing the cost of the resin nut.

[0015] It is preferable to have a plurality of the injection gate marks. If the resin nut has only one injection gate mark, the screw hole of the resin nut will be, for example, elliptical, and the screw hole of the resin nut will not be formed with high precision. In contrast, if the resin nut is molded using an injection mold having multiple gates, when the synthetic resin is filled into the cavity of the injection mold having multiple gates, the synthetic resin is filled into the cavity of the injection mold almost simultaneously and uniformly from the multiple gates. Therefore, the screw hole of the resin nut having multiple injection gate marks will be formed with high precision.

[0016] The injection gate mark is preferably a circular shape of 0.8 mm or less. By manufacturing a resin nut using an injection mold with an injection gate diameter of approximately 0.8 mm or less, when the injection mold is opened and the resin nut is removed from the injection mold, the resin nut and the sprue or runner continuing to the resin nut are easily separated. At that time, a resin nut with an injection gate mark diameter of approximately 0.8 mm or less is manufactured. In order to easily separate the resin nut and the sprue or runner continuing to the resin nut, the diameter of the injection gate mark is preferably 0.7 mm or less, or even 0.6 mm or less.

[0017] Moreover, the injection gate mark is preferably a circular shape of 0.5 mm or more. If the injection gate mark is less than 0.5 mm, the injection gate will be less than 0.5 mm, and the gate diameter of the injection molding die, which is the entrance to the molded product, will be small, and there is a risk that the resin will not flow well into the cavity that forms the molded product. For this reason, it is preferable that the injection gate mark has a circular shape with a diameter of 0.5 mm or more.

[0018] It is preferable to set the depth of the stepped surface (recess) formed as a recess on the end face of the body on the side of the screw hole opening to 0.2 mm or more and 0.8 mm or less. If the depth is less than 0.2 mm, it is too shallow, and if a dent is formed on the end face on the side of the screw hole opening of the body due to contact with another member, the screw hole opening may be affected by the dent. If the depth exceeds 0.8 mm, the axial length of the screw hole becomes too short, and the screwing of the screw shaft becomes unstable.

[0019] It is preferable to use polyarylene sulfide (PAS) as the main component of the resin composition forming the injection molded product. PAS is one of the super engineering plastics. PAS is excellent in heat resistance, cold resistance, heat shock resistance, creep resistance, fatigue properties, flame retardancy, chemical resistance, dimensional stability due to almost no water absorption, and little change in physical properties. Therefore, by using PAS as the main component of the resin composition forming the injection molded product, e.g. Water Even if the plastic nut with the body is used in an environment where it comes into contact with oil, various solvents, etc., the dimensional accuracy of the plastic nut body is maintained. Therefore, it is possible to avoid problems such as poor rotation of the plastic nut with the body due to a decrease in the dimensional accuracy of the body. In addition, since PAS is relatively inexpensive, it can contribute to lowering the price of plastic nuts with the body. Effect of the Invention

[0020] In the present invention, since an injection gate mark is formed near the opening of the screw hole in the main body, factors that may cause dimensional distortion in the screw hole during injection molding, such as short shots, can be eliminated. Therefore, it is possible to form a resin nut with a highly accurate screw hole that does not require 100% inspection of rotation unevenness using a male screw, for example, and as a result, it is possible to provide a resin nut that avoids problems such as poor rotation and is low in cost.

[0021] In addition, in the present invention, the opening of the screw hole in the main body is located at a position set back from the end face of the main body, so even if another member comes into contact with the end face of the main body on the side of the screw hole opening and causes a dent to be formed on this end face, no dent will be formed on the opening of the screw hole. Therefore, when a male screw is screwed into this resin nut, problems such as poor rotation of the male screw can be effectively prevented, and smooth screwing is possible.

[0022] In addition, the injection gate mark can be effectively prevented from contacting other components, and the rotational movement of the resin nut is not impaired even without gate cutting processing, which improves productivity and reduces costs. [Brief description of the drawings]

[0023] [Figure 1] FIG. [Diagram 2] FIG. 2 is an enlarged cross-sectional view of a main portion of a resin nut. [Diagram 3] FIG. 1 is a perspective view showing a feed screw using a conventional resin nut. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0024] The following describes an embodiment of the present invention with reference to FIGS. Figure 2 The following description will be given based on the above. FIG. 1 shows a feed screw using a resin nut 10 according to the present invention. A feed screw is a mechanical part that converts a rotational motion into a linear motion. That is, the feed screw is a mechanical part that includes the resin nut 10 according to the present invention and a screw threaded thereto. Male thread have Screw shaft It consists of:

[0025] The resin nut 10 is Figure 1 and Figure 2 As shown in FIG. 1, the device is provided with a main body 15 having a first portion 13 having a large diameter and a short cylindrical shape, and a second portion 14 having a small diameter and a short cylindrical shape protruding from a wall portion 13b that closes one opening of the first portion 13. So The wall portion 13b is provided with a hole portion 15a that communicates with the through hole 14a of the second portion 14. The through hole 14a and the hole portion 15a form a hole portion 19 that communicates with the hole portion 13a of the first portion 13.

[0026] The hole 19 formed by the through hole 14a and the hole 15a is formed into a threaded hole 20 having a female thread on the inner diameter surface. The female thread is a metric thread having a thread size of, for example, M2 or more, preferably M2.3 or more, for example, M5 or less, specifically M3 or less, and may be either coarse or fine, but the pitch is a small female thread of, for example, 0.25 or more, preferably 0.35 or more, or even 0.4 or more, for example, 0.8 or less, specifically 0.6 or less, or even 0.5 or less. Male thread The nominal thread size, pitch, etc. of the screw are small like the female thread. In this manner, since the resin nut 10 has the screw hole 20 with a small female thread in the body 15, it is necessary to form the female thread of the screw hole 20 with high precision. In addition, a large diameter portion 15a1 is formed on the hole portion 13a side of the first portion 13 of the hole portion 15a, and a tapered hole 15a2 is formed between the large diameter portion 15a1 and the through hole 14a.

[0027] Further, a recess 21 is formed in the end face 15b on the side of the screw hole opening 20a of the main body 15 to provide a stepped surface 21a. The screw hole 20 is communicated with this recess 21, and the opening 20a of the screw hole 20 on the side of the end face 15b is provided on the stepped surface 21a.

[0028] The stepped surface 21a is Figure 1 As shown in FIG. 1, the nut 10 is made up of an annular portion 21a1 and a radial protruding portion 21a2 that is connected to the annular portion 21a1. In this case, three radial protruding portions 21a2 are provided at a pitch of 120° along the circumferential direction. The resin nut 10 is formed by injection molding, and an injection gate mark G is formed on the injection molded product. Therefore, in the resin nut 10, the position of the gate (not shown) of the injection molding die (not shown) is determined so that the injection gate mark G is formed on the radial protruding portion 21a2.

[0029] This resin nut 10 is an injection molded product as a main body 15 in which a screw hole 20 is formed, and an injection gate mark G is formed in the vicinity of the screw hole opening 20a of the main body 15. Here, the vicinity of the screw hole opening 20a will be described in detail. And, Figure 1 As shown in the enlarged view of the main part of the front of the resin nut 10, for example, the injection gate mark G may be formed at a position within a radius of 5 mm from approximately the center of the screw hole opening 20a, preferably within a radius of 4 mm, more preferably within a radius of 3 mm, or even within a radius of 2.5 mm.

[0030] Since the injection gate mark G is formed near the screw hole opening 20a of the main body 15, factors that may cause the screw hole 20 to be deformed during injection molding, such as short shots, can be eliminated, and even if the main body 15 of the resin nut 10 has a small female thread screw hole 20, the precision of the screw hole 20 is maintained high. Male thread This prevents the rotation from becoming uneven, and improves the rotation accuracy. Male thread It is now possible to form a resin nut 10 having a highly accurate screw hole 20 that does not require full inspection for rotation unevenness using a screw hole 20, and as a result, it is possible to provide a resin nut 10 that avoids the occurrence of defects such as poor rotation and at low cost.

[0031] In addition, in consideration of the relationship between the diameter of the screw hole opening 20a and the diameter D of the injection gate mark G, it is preferable that the injection gate mark G is located within the range of the above-mentioned radius from approximately the center of the screw hole opening 20a and at a position that is at least a radius of 1.5 mm from approximately the center of the screw hole opening 20a.

[0032] Furthermore, the injection gate mark G is provided on a stepped surface 21a formed as a recess 21 on the end face 15b on the screw hole opening 20a side of the main body 15. Since the injection gate mark G is formed on the stepped surface 21a formed as a recess 21 on the end face 15b on the screw hole opening 20a side of the main body 15, the injection gate mark G is located at a position set back from the end face 15b of the main body 15, and this injection gate mark G can be effectively prevented from contacting other members.

[0033] During injection molding, a cavity corresponding to the shape of the body 15 of the resin nut 10 is formed in the injection mold. The molten resin composition is injected and filled into the cavity from the gate of the injection mold. In addition, since traces such as gate marks G and ejector pin marks remain on the resin molded body manufactured based on the injection molding method, it is possible to determine whether it was manufactured based on the injection molding method.

[0034] Plastic Nut 10 For example, For example, it is made of polyphenylene sulfide (PPS) which has excellent chemical resistance and low water absorption. The diameter of the gate of the injection molding die (not shown) is set so that the injection gate mark G has a circular shape with a diameter D of 0.8 mm or less and 0.5 mm or more. Furthermore, the depth T of the recessed portion 21 (the dimension from the end face 15b to the stepped face 21a) is set to, for example, 0.2 mm or more and 0.8 mm or less, preferably 0.3 mm or more and 0.5 mm or less.

[0035] In the screw hole 20 of the resin nut 10 thus configured Screw shaft of Male thread The feed screw is formed by fitting the two together. Screw shaft The material may be stainless steel, carbon steel, or steel for mechanical construction. do.

[0036] To explain in more detail, Screw shaft is formed of a molten metal base material. The molten metal material is preferably iron, aluminum, an aluminum alloy, copper, or a copper alloy. Examples of iron include general structural carbon steel (SS400, etc.), mild steel (SPCC, SPCE, etc.), and stainless steel (SUS304, SUS316, etc.), and these irons may be plated with zinc, nickel, copper, etc. Examples of aluminum include A1100 and A1050, examples of aluminum alloys include A2017 and A5052 (including anodized products), examples of copper include C1100, and examples of copper alloys include C2700 and C2801.

[0037] Further, to explain the above-mentioned resin nut 10 in more detail, the resin nut 10 is a resin nut 10 having an injection-molded main body 15 in which a screw hole 20 is formed, and a recess 21 is formed in the end face 15b on the screw hole opening 20a side of the main body 15 to provide a stepped surface 21a, the screw hole end 20b is opened in this stepped surface 21a, and an injection gate mark G is formed on this stepped surface 21a.

[0038] In the resin nut 10 configured as described above, the opening 20a of the screw hole 20 of the main body 15 is located at a position set back from the end face 15b of the main body 15, so even if another member comes into contact with the end face 15b on the side of the screw hole opening 20a of the main body 15 and a dent is formed on this end face 15b, no dent will be formed on the opening 20a of the screw hole 20. For this reason, Screw shaft This effectively prevents problems such as poor rotation of the nut 10 when the two are screwed together, thereby enabling smooth screwing.

[0039] In addition, since the injection gate mark G is formed on the stepped surface 21a, the injection gate mark G is located at a position set back from the end surface 15b of the main body 15, and the injection gate mark G can be effectively prevented from contacting other members. Therefore, even if the gate cut processing is not performed, the rotational operation of the resin nut 10 is not impaired. This makes it possible to improve productivity and reduce costs.

[0040] The injection gate mark G is formed at approximately the end 15c of the main body 15 on a surface 21a that is approximately perpendicular to the axial direction A of the screw hole 20. When the resin nut 10 is removed from the injection mold, the injection mold opens while moving approximately along the axial direction A of the screw hole 20. If the injection gate mark G is formed at approximately the end 15c of the main body 15 on a surface 21a that is approximately perpendicular to the axial direction A of the screw hole 20, when the resin nut 10 is removed from the injection mold, the gate is cut at the same time as the injection mold opens while moving approximately along the axial direction A of the screw hole 20. Therefore, the process of manually performing the gate cutting process is omitted, and the productivity is improved, so that the cost of the resin nut 10 is reduced.

[0041] The stepped surface 21a has a plurality of injection gate marks G. If the resin nut has only one injection gate mark, the screw hole of the resin nut will be, for example, elliptical, and the screw hole of the resin nut will not be formed with high precision. In contrast, if the resin nut 10 is molded using an injection mold having multiple gates, when the synthetic resin is filled into the cavity of the injection mold, the synthetic resin is filled into the cavity of the injection mold almost simultaneously and uniformly from the multiple gates. Therefore, the screw hole 20 of the resin nut 10 having multiple injection gate marks G will be formed with high precision.

[0042] The injection gate mark G is preferably a circular shape with a diameter D of 0.8 mm or less. By manufacturing the resin nut 10 using an injection mold with an injection gate diameter of approximately 0.8 mm or less, when the injection mold is opened and the resin nut 10 is removed from the injection mold, the resin nut 10 and the sprue or runner continuing to the resin nut 20 are easily separated. At that time, the resin nut 10 with the diameter D of the injection gate mark G of approximately 0.8 mm or less is manufactured. In order to easily separate the resin nut 10 and the sprue or runner continuing to the resin nut 10, the diameter D of the injection gate mark G is preferably 0.7 mm or less, or even 0.6 mm or less.

[0043] The injection gate mark G is preferably a circular shape with a diameter D of 0.5 mm or more. If the injection gate mark G is less than 0.5 mm, the injection gate will be less than 0.5 mm, and the gate diameter of the injection molding die, which is the entrance to the molded product, will be small, which may prevent the resin from flowing well into the cavity that forms the molded product. For this reason, it is preferable that the injection gate mark G is a circular shape with a diameter D of 0.5 mm or more.

[0044] It is desirable to set the depth T of the stepped surface 21a (recessed portion) formed as the recess 21 on the end face 15b on the screw hole opening 20a side of the main body 15 to, for example, 0.2 mm to 0.8 mm, preferably 0.3 mm to 0.5 mm. If the depth is, for example, less than 0.2 mm, specifically less than 0.3 mm, it is too shallow, and if a dent is formed on the end face on the screw hole opening side of the main body due to contact with another member, the screw hole opening may be affected by the dent, whereas if the depth exceeds, for example, 0.8 mm, specifically 0.5 mm, the axial length of the screw hole becomes short, and the screwing of the screw shaft becomes unstable.

[0045] The body 15 of the resin nut 10 is mainly composed of at least one of a thermoplastic resin capable of being injection molded, such as engineering plastics or super engineering plastics, and a thermoplastic resin composition.

[0046] Thermoplastic resins and thermoplastic resin compositions that can be injection molded, either engineering plastics or super engineering plastics, that are available on the market, have excellent injection moldability, so that the main body 15 of the resin nut 10 can be efficiently injection molded, thereby improving the productivity of the resin nut 10 and reducing the cost.

[0047] Examples of engineering plastics (engineering plastics) include amide-based resins such as polyamide (PA), oxymethylene-based resins such as polyacetal (POM), etc. Examples of super engineering plastics (super engineering plastics) include arylene sulfide-based resins such as polyphenylene sulfide (PPS), ketone-based resins such as polyether ether ketone (PEEK), liquid crystal resins such as liquid crystal polymer (LCP), and imide-based resins such as polyetherimide (PEI), polyamideimide (PAI), and thermoplastic polyimide (TPI).

[0048] Polyarylene sulfide (PAS) is used as the main component of the resin composition that forms the injection molded product. PAS is one of the super engineering plastics. PAS has excellent heat resistance, cold resistance, heat shock resistance, creep resistance, fatigue properties, flame retardancy, chemical resistance, dimensional stability due to almost no water absorption, and little change in physical properties. Therefore, by using PAS as the main component of the resin composition that forms the injection molded product, even Water Even if the resin nut 10 having the main body 15 is used in an environment where it comes into contact with oil, various solvents, etc., the dimensional accuracy of the main body 15 of the resin nut 10 is maintained. Therefore, it is possible to avoid problems such as poor rotation of the resin nut 10 having the main body 15 due to a decrease in the dimensional accuracy of the main body 15. In addition, since PAS is relatively inexpensive, it can contribute to reducing the price of the resin nut 10 having the main body 15.

[0049] PAS-based resins are generally synthetic resins represented by the following formula (1): Ar in the following formula (1) represents an arylene group, and examples of Ar include those represented by formulas (2) to (7) in the following formulas (2) and (3). In the following formula (5), X represents a halogen selected from F, Cl, and Br or CH3, and m represents an integer of 1 to 4. [ka]

[0050] [ka]

[0051] [ka]

[0052] As the PAS-based resin, a PPS resin in which Ar in the above formula (1) is the above formula (2) can be suitably used. In addition to having various excellent characteristics as a super engineering plastic, PPS resin is also one of the super engineering plastics that is inexpensive, which allows the main body 15 of the resin nut 10 to be further reduced in price.

[0053] The PAS resin preferably has a repeating unit (-Ar-S-) content of 70 mol % or more, and more preferably 90 mol % to 100 mol %. The repeating unit content here refers to the proportion of the repeating unit in 100% of all monomers constituting the PAS resin. When a PAS resin having a repeating unit content of less than 70 mol % is used, it tends to be difficult to obtain the effect of dimensional stability based on the low water absorption of the PAS resin.

[0054] A known method can be used to obtain PAS resins. For example, they are synthesized by the reaction of a halogen-substituted aromatic compound with an alkali sulfide (JP Patent Publication 44-27671), the condensation reaction of an aromatic compound with sulfur chloride in the presence of a Lewis acid catalyst (JP Patent Publication 46-27255), or the condensation reaction of thiophenols in the presence of an alkali catalyst or copper salt (U.S. Patent Publication 3,274,165). A specific method is to react sodium sulfide with p-dichlorobenzene in an amide solvent such as N-methylpyrrolidone or dimethylacetamide, or a sulfone solvent such as sulfolane.

[0055] Furthermore, the components shown in the following formulas (8) to (12) can be included in the PAS resin as copolymerization components within the range that does not affect the crystallinity of the PAS resin. The amount of the components shown in the following formulas (8) to (12) added can be less than 30 mol %, preferably less than 10 mol % and 1 mol % or more, relative to 100% of all monomers constituting the PAS resin. [ka]

[0056] [ka]

[0057] Here, the PPS resin is obtained, for example, by reacting sodium sulfide with p-dichlorobenzene in an amide solvent such as N-methylpyrrolidone or dimethylacetamide, or a sulfone solvent such as sulfolane, and the PPS resin at this stage is called the as-polymerized PPS resin. This as-polymerized low-molecular-weight PPS resin can be subjected to a process such as heat treatment to freely produce various polymerization degrees ranging from those with no cross-links in the resin to those with partial cross-links (cross-links). This allows the selection of any PPS resin having melt viscosity characteristics appropriate for the intended melt blend. Linear PPS resins that do not have a cross-linked structure can also be used.

[0058] The PAS resin is preferably a crosslinked PAS resin or a PAS resin having partial crosslinks, i.e., partial crosslinks. The PAS resin having partial crosslinks is also called a semi-crosslinked or semi-linear type. The crosslinked PAS resin can be obtained, for example, by heat treating in the presence of oxygen during the manufacturing process to increase the molecular weight to a required level. The crosslinked PAS resin has a two-dimensional or three-dimensional crosslinked structure in which some of the molecules are crosslinked with each other via oxygen. Therefore, compared to the linear PAS resin without crosslinks described later, it is superior in that it retains high rigidity even in a high-temperature environment, has little creep deformation, and is less susceptible to stress relaxation. In addition, the crosslinked or semi-crosslinked PAS resin is superior in heat resistance and creep resistance, etc., compared to the linear PAS resin without crosslinks, and it is easy to obtain a main body 15 with less burrs and excellent dimensional accuracy in the injection-molded body.

[0059] On the other hand, linear type PAS resins do not contain crosslinked structures in their molecules because there is no heat treatment process in the manufacturing process, and the molecules are one-dimensional and straight-chained. In general, linear type PAS resins are characterized by lower rigidity and somewhat higher toughness and elongation than crosslinked type PAS resins. In addition, linear type PAS resins have the advantage of being excellent in mechanical strength from a specific direction and having less moisture absorption, resulting in less dimensional change even in a high-temperature and humid atmosphere. In addition, linear type PAS resins can be adjusted to lower their melt viscosity, for example, by adjusting the molecular weight. For this reason, even if a resin composition is made by mixing a specified amount of filler such as carbon fiber, glass fiber, potassium titanate whisker, fibrous inorganic materials, calcium carbonate, mica, and metal powder into a linear type PAS resin, the injection moldability is not significantly impaired.

[0060] Methods for forming crosslinks or partial crosslinks in PAS resins include, for example, a method in which a polymer with a low degree of polymerization is polymerized and then heated in an air-containing atmosphere, or a method in which a crosslinking agent or a branching agent is added.

[0061] The apparent melt viscosity of the PAS resin is preferably in the range of 1000 poise to 10000 poise. If the apparent melt viscosity is less than 1000 poise, the strength of the resin molded body may decrease. On the other hand, if the apparent melt viscosity exceeds 10000 poise, the moldability may decrease. The melt viscosity of the crosslinked PAS resin may be 1000 poise to 5000 poise, and is preferably 2000 poise to 4000 poise. If the melt viscosity is low, the mechanical properties such as creep resistance may decrease in a high temperature range of 150°C or higher. Also, if the melt viscosity is high, the moldability may decrease. The melt viscosity is measured at a measurement temperature of 300°C, with an orifice having a hole diameter of 1 mm, a length of 10 mm, and a measurement load of 20 kg / cm. 2 This can be performed using a high-temperature flow tester with a preheating time of 6 minutes.

[0062] The thermal stability of the partially cross-linked PAS resin is preferably such that the rate of change in melt viscosity after 6 minutes and 30 minutes of preheating is in the range of -50% to 150% under the above melt viscosity measurement conditions. The rate of change is expressed by the following formula. [Rate of change = (P30-P6) / P6 x 100 (P6: measured value after 6 minutes of preheating, P30: measured value after 30 minutes of preheating)]

[0063] The molecular weight of the PAS resin is preferably 13,000 to 30,000 in terms of number average molecular weight in consideration of injection moldability, and more preferably 18,000 to 25,000 in terms of number average molecular weight in consideration of fatigue resistance and high molding accuracy. If the number average molecular weight is less than 13,000, the molecular weight is too low and fatigue resistance tends to be poor. On the other hand, if the number average molecular weight exceeds 30,000, fatigue resistance is improved, but mechanical strength such as required impact strength may decrease. The number average molecular weight here refers to the number average molecular weight in terms of polystyrene measured by gel permeation chromatography (GPC method) after dissolving the PAS resin in a solvent.

[0064] The melting point of the PAS resin is, for example, about 220°C to 290°C, and preferably 280°C to 290°C. In general, the melting point of PPS resin is about 285°C, so it is preferable to use PPS resin as the PAS resin. Since PAS resin has low water absorption, dimensional changes due to water absorption are reduced. Resin molded products using PAS resin such as PPS resin as the base resin have excellent creep resistance, chemical resistance, etc., and have excellent stability in that dimensional changes due to water absorption are reduced.

[0065] Moreover, the resin composition containing the PAS resin has a deflection temperature under load of, for example, 105° C. or higher, measured based on the test method of ISO 75-1, 2 (1.8 MPa).

[0066] As described above, the resin molded body made of the resin composition having the PAS-based resin as the base resin has the required properties for the main body 15 of the resin nut 10. Special It has the ability to

[0067] As solid lubricants to be added to the thermoplastic resin that is the main component of the resin composition forming the injection molded product, polytetrafluoroethylene (PTFE) resin (powder), graphite, molybdenum disulfide, tungsten disulfide, boron nitride, etc. can be used. These are, for example, granular fillers. Powdered PTFE resin, which has excellent lubricating properties, is considered to be granular organic matter, and graphite, molybdenum disulfide, tungsten disulfide, boron nitride, etc., which have excellent lubricating properties, are considered to be granular inorganic matter.

[0068] The powdered PTFE resin may be any of molding powder by suspension polymerization, fine powder by emulsion polymerization, and PTFE resin powder by heating and baking, but it is preferable to adopt PTFE resin powder by heating and baking. This is because molding powder and fine powder that have not been heated and baked have low friction properties, but are inferior in uniform dispersion and wear resistance. The PTFE resin powder by heating and baking may be a powder obtained by pulverizing molding powder or fine powder after heating and baking (material molding, heat treatment), or may be a powder obtained by irradiating this powder with gamma rays or electron beams. The particle size of the PTFE resin powder is not particularly limited, but in order to obtain stable low friction properties, it is preferable that the average particle size is 5 μm or more and 30 μm or less.

[0069] In addition, the resin composition preferably contains a predetermined amount of granular inorganic matter and fibrous inorganic matter as inorganic fillers in addition to the thermoplastic resin of the base resin described above. By using the granular inorganic matter and the fibrous inorganic matter, it is easy to achieve both the dimensional accuracy and mechanical strength required for the main body 15 of the resin nut 10. The granular inorganic matter mainly contributes to improving the dimensional accuracy, and the fibrous inorganic matter mainly contributes to improving the mechanical strength.

[0070] The granular inorganic material used in the resin composition is a non-fibrous filler such as a spherical, amorphous granular, plate-like, flat, or scaly material. In this form, the anisotropy caused by the granular inorganic material is less likely to be expressed in the injection molded product. Examples of the granular inorganic material include diatomaceous earth, glass flakes, glass beads, glass balloons, silica balloons, spherical graphite, graphite fluoride, graphite, spherical ceramics, alumina, kaolin, talc, clay, mica, silica, magnesium oxide, calcium sulfate, calcium oxide, calcium hydroxide, calcium carbonate, and other powdered calcium compounds. In addition, the granular inorganic material may be a mixture of not only one type of granular inorganic material, but also a plurality of types of granular inorganic materials.

[0071] Among the above-mentioned granular inorganic substances, graphite, glass flake, alumina, talc, clay, mica, silica, magnesium oxide, and calcium carbonate are preferable because they are relatively inexpensive.

[0072] The average particle size of the granular inorganic material is 0.5 μm or more, preferably 1 μm or more, more preferably 3 μm or more, and more preferably 5 μm or more, and 100 μm or less, preferably 80 μm or less, more preferably 50 μm or less, and more preferably 30 μm or less. If the average particle size is less than a predetermined average particle size (e.g., 0.5 μm), aggregation between particles may occur, making uniform dispersion difficult. If the average particle size exceeds a predetermined average particle size (e.g., 100 μm), the surface smoothness may be deteriorated. Here, the average particle size is the volume average particle size (MV: Mean Volume Diameter) obtained by measurement using a laser diffraction / scattering method.

[0073] Examples of fibrous inorganic materials used in the resin composition include whiskers such as calcium silicate whiskers, calcium carbonate whiskers, calcium sulfate whiskers, magnesium sulfate whiskers, magnesium nitrate whiskers, potassium titanate whiskers, titanium oxide whiskers, zinc oxide whiskers, aluminum borate whiskers, silicone carbide whiskers, sapphire whiskers, wollastonite whiskers, graphite whiskers, and the like; composite fibers such as so-called boron fibers, silicon carbide fibers, and Tyranno fibers, in which boron or silicon carbide is vapor-deposited on tungsten core wire or carbon fibers, and the like, and the like, can be mentioned. As the carbon fibers, for example, carbon fibers of any type of raw material, such as pitch-based, polyacrylonitrile-based (PAN-based), carbonaceous, graphite-based, rayon-based, and lignin-poval-based mixtures, can be used. In addition, as the fibrous inorganic materials, not only one type of fibrous inorganic material but also a mixture of multiple types of fibrous inorganic materials can be used.

[0074] Among the above-mentioned fibrous inorganic materials, carbon fibers such as PAN-based carbon fibers and pitch-based carbon fibers, and glass fibers are preferable because they are relatively inexpensive. By selecting at least one of graphite, talc, clay, mica, glass flakes, magnesium oxide, alumina, silica, and calcium carbonate as the granular inorganic material, and at least one of PAN-based carbon fibers, pitch-based carbon fibers, and glass fibers as the fibrous inorganic material, the price of the resin molded body can be kept low.

[0075] The average fiber length of the fibrous inorganic material is 10 μm or more, preferably 20 μm or more, more preferably 30 μm or more, and 40 μm or more or even 50 μm or more depending on the type of fibrous inorganic material. The upper limit is 3 mm or less, substantially 2 mm or less, more substantially 1 mm or less, and 700 μm or less or even 300 μm or less depending on the type of fibrous inorganic material. In the present invention, the average fiber length is a number average fiber length, which roughly corresponds to the cut length. The average fiber length is obtained, for example, by randomly extracting the fibrous inorganic material to be measured for the fiber length from an image obtained by observation with an optical microscope, measuring the long side of the fibrous inorganic material, and based on the measured value obtained.

[0076] The average fiber diameter of the fibrous inorganic material is 5 μm or more, preferably 6 μm or more, and 25 μm or less, preferably 15 μm or less, more preferably 13 μm or less. The average fiber diameter is measured by an electron microscope or an atomic force microscope that is commonly used in this field. The average fiber diameter can be calculated as the number average fiber diameter based on the above measurement.

[0077] If the average fiber length of the fibrous inorganic material is less than a predetermined value (e.g., 10 μm) or the average fiber diameter is less than a predetermined value (e.g., 5 μm), the mechanical strength required for the resin composition may not be expected. On the other hand, if the average fiber length of the fibrous inorganic material exceeds a predetermined value (e.g., 3 mm) or the average fiber diameter exceeds a predetermined value (e.g., 25 μm), it may be difficult to uniformly disperse the fibrous inorganic material when mixed with the resin, which may adversely affect injection molding.

[0078] The average aspect ratio of the fibrous inorganic material has a lower limit of 2 or more, preferably 3 or more, more preferably 4 or more, and depending on the type of fibrous inorganic material, it is 5 or more, or even 6 or more. The upper limit is 1000 or less, substantially 700 or less, more substantially 500 or less, and depending on the type of fibrous inorganic material, it is 300 or less, or even 50 or less. If the average aspect ratio is less than a predetermined value (e.g., 2), the reinforcing effect of the matrix itself may be impaired, and the mechanical properties may be reduced. If the average aspect ratio exceeds a predetermined value (e.g., 1000), uniform dispersion during mixing may be difficult, which may lead to a deterioration in quality.

[0079] The "average aspect ratio" means "average fiber length / average fiber diameter", and more specifically, is the value obtained by dividing the "average fiber length" by the "average fiber diameter".

[0080] Books Various additives can be mixed into the resin composition used in the main body 15 of the resin nut 10 according to the present invention in amounts that do not impair the object of the invention. Examples of various additives that can be mixed include one or more of a release agent, a lubricant, a heat stabilizer, an antioxidant, an ultraviolet absorber, a crystal nucleating agent, a rust inhibitor, an ion trapping agent, a flame retardant, a flame retardant assistant, a colorant such as a dye or pigment, and an antistatic agent.

[0081] By using such a resin composition to injection-mold the body 15 of the resin nut 10, it is possible to provide a resin nut 10 having a body 15 with improved dimensional accuracy compared to the case of injection-mold using a general resin. In addition, by using a thermoplastic resin as the base resin, the body 15 of the resin nut 10 can be produced by an injection molding method suitable for mass production, so that the unit price of the resin nut 10 can be reduced, and the price can be reduced. In addition, the resin body 15 can contribute to, for example, rust prevention and sliding characteristics more than a metal body.

[0082] As the resin nut 10 of the present invention Send In addition to the screw, a ball screw may also be used. stomach.

[0083] Although the embodiment of the present invention has been described above, the present invention is not limited to the above embodiment and can be modified in various ways. As the resin used for the resin nut 10, various resin materials generally known as the material of the resin nut 10 can be used. As the base resin constituting the resin nut 10, thermoplastic resins such as PPS (polyphenylene sulfide), TPI (thermoplastic polyimide), PEEK (polyether ether ketone), POM (polyacetal), PA (polyamide), and PE (polyethylene) can be adopted. These base resins are appropriately mixed with reinforcing agents and fillers to form resin materials.

[0084] The number of gate marks G provided on the stepped surface 21a is not limited to three and may be increased or decreased as desired. However, if there is only one, the screw hole may become elliptical, and if there are too many, the gate diameter of the injection mold, which is the entrance to the molded product, may become small, and the resin may not flow well into the cavity that forms the molded product. For this reason, the number of gate marks G is, for example, 2 to 6, preferably 3 to 5, and more preferably about 3 or 4. In addition, it is preferable to set the number of radial protrusions 21a2 on the stepped surface 21a in accordance with the number of the gate marks G. In addition, in the above embodiment, the radial protrusions 21a2 are provided on the stepped surface 21a, and the gate marks G are provided on the radial protrusions 21a2. However, such radial protrusions 21a2 may not be provided. [Explanation of symbols]

[0085] 10 Plastic nut 15 Main unit 15b End face 15c end 20 Screw holes 20a Screw hole opening (opening) 20b Screw hole end 21 Recess 21a Stepped surface (surface) A axis direction D diameter (diameter) G Injection gate mark (gate mark) T Depth

Claims

1. A resin nut having an injection molded product as a main body having a screw hole formed therein, A resin nut characterized in that an injection gate mark is formed near the screw hole opening of the body, and the injection gate mark is provided on a stepped surface formed as a recess in the end face of the body on the screw hole opening side.

2. A resin nut having an injection molded product as a main body having a screw hole formed therein, A resin nut characterized in that it has a stepped surface formed as a recess on the end face of the body on the opening side of the screw hole, the end of the screw hole is opened on this stepped surface, and an injection gate mark is formed on this stepped surface.

3. The injection gate mark is located at the end of the main body and is approximately parallel to the axial direction of the screw hole. The resin nut according to claim 1 or 2, characterized in that the resin nut is formed on orthogonal surfaces.

4. The resin nut according to any one of claims 1 to 3, characterized in that it has a plurality of the injection gate marks.

5. The resin nut according to any one of claims 1 to 4, characterized in that the injection gate mark has a circular shape of 0.8 mm or less.

6. The resin nut according to any one of claims 1 to 5, characterized in that the injection gate mark has a circular shape of 0.5 mm or more.

7. The resin nut according to any one of claims 1 to 6, characterized in that the depth of the stepped surface formed as a recess on the end surface on the screw hole opening side of the body is set to 0.2 mm or more and 0.8 mm or less.

8. The resin nut according to any one of claims 1 to 7, characterized in that polyarylene sulfide is used as a main component of the resin composition forming the injection molded product.

Citation Information

Patent Citations

  • Resin nut, manufacture thereof, and slide screw device

    JP1998281132A

  • Molding nut, manufacture of molding nut, and linear guide device using molding nut

    JP2000074172A

  • Feed screw

    JP2001116102A

  • Feeding mechanism of valve body of fluid control valve and fluid control valve using the same