Carbon dioxide fixation method

The method efficiently immobilizes CO2 in cement hydrate by controlled CO2 injection and stirring, addressing the inefficiencies of existing methods, achieving rapid fixation and increased cement strength.

JP7555296B2Active Publication Date: 2024-09-24TAIHEIYO CEMENT CORP

Patent Information

Application Number
JP2021060238
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-03-31
Publication Date
2024-09-24
Estimated Expiration
2041-03-31

AI Technical Summary

Technical Problem

Existing methods for immobilizing CO2 in cement hydrate lack efficient manufacturing conditions suitable for mass production, particularly in terms of time and efficiency.

Method used

A method involving the injection of CO2 into a mixture of cement hydrate and water in a controlled manner, using a specific liquid-solid ratio, bubble diameter, and stirring, with a blowing speed over 3600 kg/t·h and a blowing time of 10-30 minutes, to achieve efficient immobilization.

Benefits of technology

CO2 is immobilized in a short time, producing carbonate with a large specific surface area, enhancing cement strength when mixed, and allowing for efficient fixation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007555296000005
    Figure 0007555296000005
  • Figure 0007555296000006
    Figure 0007555296000006
  • Figure 0007555296000004
    Figure 0007555296000004
Patent Text Reader

Abstract

To provide an efficient production method that fixes CO2 to cement hydrate in a short time.SOLUTION: The present invention discloses a method for fixing cement hydrate to CO2, the method including a CO2 blowing step in which cement hydrate 11 and water 12 are put into a container 10, and the liquid mixture of the cement hydrate 11 and the water 12 are stirred while CO2 14 is blown into the container 10. In the CO2 blowing step, the CO2 blowing speed is 3600 kg / t h or more and the CO2 blowing amount is 600 kg / t or more.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for fixing carbon dioxide in cement hydrate. [Background technology]

[0002] Conventionally, in order to prevent global warming, there has been a demand for reducing CO2 emissions into the atmosphere. As one method, Patent Document 1 discloses a technology for immobilizing CO2 using alkaline earth metal-containing substances. Examples of alkaline earth metal-containing substances include concrete waste generated by demolishing concrete buildings, and steel slag, a by-product generated in the steelmaking process. Conventionally, these substances have been used as aggregates, etc., but they can be used more effectively by immobilizing CO2.

[0003] In the method disclosed in the above document, water is added to ready-mixed concrete generated at ready-mixed concrete factories and construction sites to create a slurry-like ready-mixed concrete, and CO2 is then mixed into it to generate CaCO3 and fix the CO2. The generated CaCO3 is used as a concrete material. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2007-190538 A Summary of the Invention [Problem to be solved by the invention]

[0005] Although methods for fixing CO2 in cement hydrate and methods for using the material have been developed, there is still no knowledge of highly efficient manufacturing conditions for mass production. In particular, when mass production is assumed, it is necessary to fix a certain amount of CO2 within a certain time.

[0006] The present invention has been made to solve the above problems, and an object of the present invention is to provide a highly efficient production method for fixing CO2 in cement hydrate in a short period of time. [Means for solving the problem]

[0007] The method of the present invention for fixing CO2 in cement hydrate includes a CO2 injection step of placing cement hydrate and water in a container, and injecting CO2 into the container while stirring the mixture of cement hydrate and water, and in the CO2 injection step, the CO2 injection rate is 3600 kg / t h or more and the CO2 injection amount is 600 kg / t or more. , CO 2 The blowing time is between 10 and 30 minutes. It is characterized in that:

[0008] According to the method of fixing CO2 in cement hydrate of the present invention, CO2 can be fixed in cement hydrate in a short time. In addition, the specific surface area of ​​the carbonate generated by fixing CO2 in cement hydrate is large, so that it is expected to increase the strength when mixed with cement.

[0009] In addition, in the CO2 injection step of the method of fixing CO2 in cement hydrate of the present invention, the liquid-solid ratio of water to cement hydrate is 4 to 8, and the ratio of the injection depth in the CO2 mixed liquid to the maximum bubble diameter of CO2 at the water depth is 400 or more.

[0010] According to the CO2 injection process of the present invention, the liquid-solid ratio and the ratio of the injection depth of the CO2 mixture to the maximum bubble diameter of the CO2 at the water depth can be set within a suitable range. Therefore, the CO2 can be efficiently fixed in the cement hydrate. [Brief description of the drawings]

[0011] [Figure 1] FIG. 1 is a schematic diagram of an apparatus 100 for fixing CO2 in cement hydrate, which is one embodiment for carrying out the present invention. [Diagram 2] FIG. 1 is a schematic diagram of a test device embodying the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] <Embodiment Mode> The present embodiment of the manufacturing method for immobilizing CO2 in cement hydrate will be described with reference to Fig. 1. The CO2 immobilization apparatus 100 used in the above method includes a container 10, a CO2 supplying device 20, and a stirring device 30. The CO2 immobilization apparatus 100 is an apparatus for mass-production of cement hydrate in which CO2 is immobilized efficiently.

[0013] The vessel 10 is a device into which water and waste concrete are put to fix CO2. The waste concrete includes waste concrete from demolished concrete buildings, waste sludge from concrete production, waste lightweight aerated concrete (waste ALC), and the like. The waste concrete may contain aggregates other than cement hydrate, and the amount of cement hydrate may be within a specified range. The waste concrete is crushed finely by a crusher (not shown) and then put into the vessel in order to fix CO2 efficiently. Materials other than cement hydrate, such as aggregates, may be separated and selected. The finely crushed concrete powder 11 is unlikely to settle even when put into water, and the fixation reaction of CO2 can be efficiently carried out. The water 12 put into the vessel 10 together with the concrete powder 11 is, for example, industrial water.

[0014] Water 12 and concrete powder 11 are put into the container 10 and mixed to generate sludge slurry 13. The liquid-solid ratio, which is the mixing ratio of the water 12 and the concrete powder 11, is preferably in the range of 4 to 8. If the liquid-solid ratio is less than 4, i.e., if the solid content is relatively high, the CO2 supply device 20 may become clogged and may not be able to supply the required CO2. Also, if the liquid-solid ratio is 8 or more, i.e., if the solid content is relatively low, the amount of water is in excess of the amount of concrete powder 11, and the container 10 becomes too large. Therefore, the liquid-solid ratio is preferably in the above range.

[0015] The CO2 supplying device 20 supplies CO214 to the container 10. The CO2 supplying device 20 has a supply pipe 21, a flow rate adjusting device 22, and an aeration device 23. One end of the supply pipe 21 is connected to a supply source of CO214 (not shown). The supply pipe 21 has one or more branches in the middle of the supply pipe 21, and the other end of each of the supply pipes 21 is connected to a plurality of aeration devices 23. The gas to be supplied does not need to be 100% CO2 gas, and factory exhaust gas containing N2 or O2 may be used, as long as the actual supply amount of CO2 is within a specified range.

[0016] The CO2 supply device 20 has at least one of a plurality of flow rate regulators 22 capable of adjusting the amount of CO2 supplied to each of the plurality of air diffusers 23, or a single flow rate regulator 22 capable of adjusting the amount of CO2 supplied to all of the plurality of air diffusers 23, at the intermediate portion of the supply pipe 21. Each of the one or more flow rate regulators 22 may have an electromagnetic valve and be electrically controllable. In addition, the surplus of the supplied CO2 14 is discharged from the container 10 as exhaust gas 15.

[0017] The air diffuser 23 includes a porous structure and is a device that releases the introduced CO2 14 as fine bubbles. One or more air diffusers 23 are arranged in the container 10 so that the entire air diffuser 23 is immersed in the sludge slurry 13 contained in the container 10. The porous structure of the air diffuser 23 is formed of a porous material containing many holes. The porous structure may be covered with other materials except for the surface on which the CO2 release surface is formed. Alternatively, the porous structure may be formed of a material that does not have holes formed therein except for the surface on which the CO2 release surface is formed. Alternatively, the porous structure may be a material such as a hollow material with many holes processed and opened on the surface. For example, it may be a hollow tube with many holes opened on the surface. Alternatively, a device that uses blades or the like to finely disperse CO2 may be used. In addition, it is desirable that the water depth at which the air diffuser 23 is arranged is arranged close to the bottom side of the container 10 so that CO2 can be efficiently fixed. For example, the water depth of the aeration device 23 is at least 50% or more, preferably 60% or more, and more preferably 70% or more of the maximum design water depth of the vessel 10. In addition, there may be multiple CO2 fixation devices, and any shape of device is possible as long as the total contact time of CO2 and sludge slurry is the same.

[0018] The CO214 introduced into the diffuser 23 is released into the sludge slurry 13 as bubbles with a diameter of 1 mm or less. When the CO214 injection depth, i.e., the water depth of the CO2 release surface of the diffuser 23 where the CO214 bubbles are generated, is L, and the diameter of the CO214 bubbles at that water depth is M, the diffuser 23 is installed so that L / M≧400. When multiple diffusers 23 are installed at positions with different heights, the CO214 injection depth is defined as L, which is the maximum water depth of the CO2 release surface of the diffuser 23 where the CO214 bubbles are generated. Although the diffuser 23 is configured to release CO214 from the top, the CO2 release surface of the diffuser 23 may be configured not only as the top surface, but also as the side surface, the bottom surface, or any combination of the two. When the CO2 release surface of the diffuser 23 is the side surface or the bottom surface, clogging due to the concrete powder 11 in the sludge slurry 13 falling down is less likely to occur than when the CO2 release surface is the top surface. Therefore, the periodic maintenance period of the diffuser 23 can be extended. The diffuser 23 may be one or more, as long as it can release the specified amount of CO214. In addition, when there are more than one diffuser 23, it is more efficient to arrange them at approximately equal intervals around the periphery along the wall of the container 10.

[0019] The agitator 30 is a device that agitates the sludge slurry 13 so that the fixation of CO214 can be efficiently performed. The agitator 30 continues to rotate at a constant rotation speed by an electric motor (not shown) to agitate the sludge slurry 13. The agitator 30 is disposed near the approximate center of the vessel 10 so that the agitator 30 can efficiently agitate the sludge slurry 13. The agitator 30 has a rotating shaft 31 that is rotated by the electric motor, and an agitator blade 32 that is connected to the lower end of the rotating shaft 31.

[0020] The agitator 32 is formed to be 30% or more of the inner diameter of the container 10 or the inner dimension such as the cross dimension of the maximum part. The water depth of the agitator 32 is 50% or more of the design maximum water depth of the sludge slurry 13 to be put into the container 10, that is, half the water depth or deeper. The water depth at which the agitator 32 is placed is preferably as close to the bottom side of the container 10 as possible so that the concrete powder 11 contained in the sludge slurry 13 can be easily scooped up even when it sinks to the bottom of the container 10. For example, it is good to set it to at least 50% or more, preferably 60% or more, and more preferably 70% or more of the design maximum water depth of the container 10. The agitator 32 is placed at approximately the same water depth position with respect to the air diffuser 23 in the water depth direction. The position of the stirring blade 32 relative to the aeration device 23 in the water depth direction may be above the aeration device 23, within the range of the water depth direction dimension of the aeration device 23, or below the aeration device 23. A plurality of stirring blades 32 may be arranged, and they may be installed so that their total length is 30% or more of the inside diameter of the vessel 10 or the inside dimension such as the span dimension of the maximum part.

[0021] It should be noted that a circulation device for the sludge slurry 13 (not shown) can be provided together with the agitation device 30 or instead of the agitation device 30. The circulation device has a pump and pipes before and after the pump, with the end of the pipe before the pump being disposed on the bottom surface of the container 10 or near the bottom surface, and the end of the pipe after the pump being disposed at an upper portion inside the container 10. The sludge slurry 13 on the bottom surface of the container 10 or near the bottom surface is sucked by the pump and circulated to the upper portion of the sludge slurry 13 inside the container 10. This allows for efficient fixation of CO2.

[0022] In the above apparatus, water 12 and concrete powder 11 are put into the container 10 so as to have a predetermined liquid-solid ratio, and the mixing degree is made uniform by the agitator 30 to generate sludge slurry 13. The predetermined liquid-solid ratio is 4 to 8. In this state, the CO2 supply device 20 starts supplying CO2 at a predetermined CO2 injection rate. The predetermined CO2 injection rate is 3600 kg / t·h or more. The injection of CO2 is continued for a predetermined CO2 injection time, and a predetermined CO2 injection amount is injected into the sludge slurry 13. The predetermined CO2 injection time is 35 minutes or less, and the predetermined CO2 injection amount is 600 kg / t or more. By the above method, CO2 is efficiently fixed in the concrete powder 11. When one CO2 fixation operation is completed, the sludge slurry 13 is discharged from the container 10. Water 12 and concrete powder 11 are put into the container 10 again. The discharged sludge slurry 13 is used as is or after dehydration and drying, and the concrete powder 11 with the CO2 immobilized therein is used as a cement raw material, etc.

[0023] Although the supply of CO214 to the container 10 has been described as being supplied from a pressure container filled with CO214, other forms are also possible. CO2 derived from exhaust gas from the factory in which the container 10 is located or an adjacent factory may be supplied via piping installed in the factory. For example, CO2 emitted from a cement factory may be continuously supplied via a supply pipe. This reduces the amount of CO2 emitted from the factory.

[0024] In this invention, the goal is to develop a method for fixing a certain amount of CO2 in cement hydrate in a short period of time, which can fix more than 200 kg / t-cem of CO2 in cement hydrate within 35 minutes.

[0025] Next, the test apparatus and the results of the test performed on this embodiment will be described with reference to FIG. 2. The test apparatus was basically configured in accordance with the above apparatus. In the test apparatus in FIG. 2, the same or corresponding members are denoted by the same reference numerals and their description will be omitted. The test apparatus includes a container 10, a CO2 supply device 20, and an agitator 30, and is basically configured the same as the CO2 fixation device 100 in FIG. 1. The container 10 was placed in a thermo-hygrostat 40, and the test was started at 20°C. The agitator 30 has a rotating shaft 31 rotated by an electric motor and an agitator blade 32 connected to the lower end of the rotating shaft 31. The position of the CO2 release surface of the aeration device 23 and the agitator blade 32 are arranged so as to be about 70% of the water depth.

[0026] The agitator 32 is formed to be 30% or more of the inner diameter of the container 10 or the inner dimension such as the cross dimension of the maximum part. The water depth of the agitator 32 is 50% or more of the design maximum water depth of the sludge slurry 13 to be put into the container 10, that is, half the water depth or deeper. The water depth at which the agitator 32 is placed is desirably as close as possible to the bottom side of the container 10 so that the concrete powder 11 contained in the sludge slurry 13 can be easily scooped up even when it sinks to the bottom of the container 10. For example, it is good to set it to 60% or more, preferably 70% or more of the design maximum water depth of the container 10.

[0027] [Preparation of ingredients] Powdered ready-mixed concrete sludge supplied from a ready-mixed concrete factory was placed in container 10. The ready-mixed concrete sludge provided was selected from those that had been produced a short time ago, and drying was started 24 hours after it was provided. The provided ready-mixed concrete sludge was crushed and then thoroughly dried in a drying oven to obtain dried sludge. The Blaine specific surface area of ​​the dried sludge at this time was Bl' = 14230 cm 2 / g(ρ=2.61g / cm 3 , e = 0.74). The dried sludge was then crushed. For the crushing process, a 10 kg sample was pulverized in a ball mill for 30 seconds. The chemical composition of the dried sludge used is shown in Table 1. As is clear from Table 1, the chemical composition of the dried sludge used in this test is similar to that of commercially available cement, and it can be treated as cement hydrate that does not contain aggregate.

[0028] [Table 1]

[0029] [Carbonation process] The sludge slurry 13 was prepared by adding the dried sludge prepared as described above to 1000 mL of ion-exchanged water to obtain a predetermined liquid-solid ratio. Thereafter, while stirring the sludge slurry 13 in a thermo-hygrostat (incubator), CO2 was injected at a predetermined flow rate and time using an air diffuser 23. The flow rate of CO2 was controlled using a float flowmeter connected to a gas cylinder. After the injection, the slurry 13 was subjected to suction filtration to separate the solid and liquid phases. The separated solid phase was dried at 105°C to obtain carbonated sludge. The carbonated sludge was pulverized and passed through a 600 μm sieve, after which various analyses were performed.

[0030] The calculation method for each characteristic value is as follows.

[0031] 1. Amount of CO2 injected (amount of CO2 supplied to sludge) (kg-CO2 / t-sludge) CO2 / Sludge = (QCO2×t) / Msludge QCO2: CO2 flow rate (kg-CO2 / h) measured by a flow meter connected to a CO2 gas cylinder t: Time from start to finish of blowing (h) Msludge: Mass of sludge added (kg)

[0032] 2. Amount of CO2 fixed in sludge (kg / t-sludge') CO2cap=CO2TG×(100 / (100-ig.lossTG) CO2cap: The amount of CO2 contained in the ignited carbonated sludge (%) CO2TG: CO2 amount calculated by TG-DTA (%) ig.lossTG: Weight loss up to 1000℃ in TG-DTA (%)

[0033] TG-DTA was performed using a simultaneous thermogravimetry and differential thermal analyzer TG-DTA6300 manufactured by Seiko Instruments Inc. under the following conditions: temperature range: room temperature to 1000° C., heating rate: 10° C. / min, atmosphere: 20° C. In addition, the following unit correction was performed.

[0034] CO2(kg / t-sludge')=CO2cap×1000 / 100

[0035] The results of the tests conducted using the above test equipment are shown in Table 2. The results of tests conducted by changing the liquid-solid ratio are shown in Table 3. The results of tests conducted by changing the injection depth / maximum bubble diameter are shown in Table 4.

[0036] [Table 2]

[0037] [Table 3]

[0038] [Table 4]

[0039] [result] (1) From Table 2, it was confirmed that in Examples 1 to 10, the amount of CO2 fixed in the sludge was 200 (kg / t-cem) or more. From this, it was found that if the liquid-solid ratio of water to cement hydrate was 4 to 8, the CO2 injection rate was 3600 kg / t·h or more, the CO2 injection amount was 600 kg / t or more, and the ratio of the injection depth of CO2 in the mixed liquid to the maximum bubble diameter of CO2 at the water depth was a predetermined value or more, the target amount of CO2 fixed in the cement hydrate of 200 kg / t-cem or more could be achieved within 30 minutes. In addition, the specific surface area of ​​the generated carbonate was large, and when it was added to cement concrete, it was expected to increase the strength when mixed with cement. For reference, tests in which the CO2 injection time was set to 40 minutes, which was longer than the target, were conducted as Reference Examples 1 to 3. These are for reference because they are longer than the target CO2 injection time. (2) Table 3 shows that the amount of CO2 fixed in sludge is highest when the liquid-solid ratio is 6, and is slightly lower when the liquid-solid ratio is 4 or 8 compared to when the liquid-solid ratio is 6. (3) Table 4 shows that the amount of CO2 fixed in the sludge varies depending on the injection depth / maximum bubble diameter.

[0040] According to the method of the present invention for fixing CO2 in cement hydrate, it is possible to fix CO2 in the cement hydrate in a short period of time. [Explanation of symbols]

[0041] 10 container, 11 concrete powder 11, 12 water.

Claims

1. CO 2 A method for fixing a hydrate of a sulphuric acid to a cement hydrate, comprising the steps of: Cement hydrate and water are placed in a container, and while stirring the mixture of cement hydrate and water, CO is added to the container. 2 CO 2 It includes a blowing process, The CO 2 In the blowing process, CO 2 The blowing speed is 3600 kg / t・h or more. CO 2 Injection rate is 600 kg / t or more. The CO 2 blowing time is 10 minutes or more and 30 minutes or less. CO 2 A method of fixing the above in cement hydrate.

2. The CO 2 In the blowing process, The liquid-solid ratio of water to cement hydrate is 4 to 8. CO 2 The injection depth in the mixed liquid of 2 2. The CO according to claim 1, wherein the ratio of the maximum bubble diameter to the maximum bubble diameter is 400 or more. 2 A method of fixing the above in cement hydrate.

Citation Information

Patent Citations

  • Treatment method of ready-mixed concrete using carbon dioxide

    JP2007190538A

  • Method for using cement-containing waste material

    JP2014117636A

  • Method for producing inorganic carbonate

    JP2018039696A

  • Mice that make heavy chain antibodies

    US20150197557A1

Cited By

  • Method for immobilizing carbon dioxide

    JP2023147117A