Water-based resin composition for paint and paint

The aqueous resin composition with incompatible water dispersion resins and carbon black particles addresses the challenge of achieving ultra-low gloss and reflection in paint films for electronic devices and models, enhancing design aesthetics and light-shielding capabilities.

JP7555321B2Active Publication Date: 2024-09-24SOMAR CORP
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2021159584
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-09-29
Publication Date
2024-09-24
Estimated Expiration
2041-09-29

AI Technical Summary

Technical Problem

Existing paint technologies struggle to achieve a highly designed film with ultra-low gloss, reflection, and L value for electronic device casings and model parts, which are essential for improved design aesthetics.

Method used

Aqueous resin compositions comprising incompatible water dispersion resins, such as acrylic and polyester emulsions, combined with a black material containing specific particle-sized carbon black, form a film with low gloss and ultra-low reflection by creating an incompatible region in the film structure.

Benefits of technology

The composition achieves a film with glossiness less than 1.0%, reflectance less than 1.5%, and L value less than 15%, providing enhanced designability and light-shielding properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007555321000003
    Figure 0007555321000003
  • Figure 0007555321000002
    Figure 0007555321000002
  • Figure 0007555321000001
    Figure 0007555321000001
Patent Text Reader

Abstract

To provide an aqueous resin composition for a coating material which enables formation of a film having high designability.SOLUTION: An aqueous resin composition for a coating material is (A) a resin component, (A1) an emulsion of an acrylic resin, (A2) an emulsion of a polyester-based resin, (B) a black material, and (B1) a composite of a black pigment and a resin having a particle diameter of 2 μm or more and 4 μm or less. (A) contains 90 mass% or more of (A1) and (A2), and a mass ratio of a resin solid content of (A2) to a resin solid content of (A1) is 1.8 or more and 4.4 or less. (B) contains 90 mass% or more of (B1), and a mass ratio of (B) to a resin solid content of (A): 1 is 1.3 or more and 4.0 or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an aqueous resin composition for use in a paint and a paint containing the same. [Background technology]

[0002] Smartphones and tablets to In electronic devices such as personal computers, a black coating is sometimes applied to part or all of the housing (either the outer or inner surface) or to part of the non-visible surface (e.g., the frame portion) of a cover glass that is placed and fixed on the visible surface side of a touch panel, for the purposes of improving the design, concealing internal wiring, blocking light, etc. In recent years, this demand has also been applied to part or all of electronic device parts such as lenses attached to various camera units (e.g., the outer edge of the lens), assembly models such as plastic models, or parts of assembly models in such model kits.

[0003] For example, Patent Document 1 discloses a technology for forming a membrane by directly screen-printing an insulating material onto the housing of a portable electronic device such as a smartphone, or by in-mold molding a membrane-forming film that has been screen-printed. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2007-285093 A Summary of the Invention [Problem to be solved by the invention]

[0005] However, in response to the recent demand for improved design of industrial products, there is an increasing demand to apply a black coating (eg, a concave-convex coating) with a more stylish design to such products.

[0006] The present invention has been made in view of the above circumstances. An object of the present invention is to provide an aqueous resin composition for coating that can form a film with excellent designability, and a coating material thereof. [Means for solving the problem]

[0007] As a result of extensive research, the present inventors have found that by satisfying the following requirements, it is possible to effectively form a film with a highly designable appearance that not only has low gloss (less than 1.0%) but also exhibits ultra-low reflectance (less than 1.5%) and an ultra-low L value (less than 15) that are lower than ever before.

[0008] · Incompatible with each other Multiple water dispersion resin Mixed A resin composition having a specific composition is used, which contains a resin component including a specific compound and a black material including a specific compound having a specific particle size range in a specific ratio (mass ratio range). Included in resin components The above As an example of the mixture, a mixture containing an acrylic resin emulsion and a polyester resin emulsion in a predetermined mass ratio range is used.

[0009] Based on these new findings, the present inventors have completed the invention provided below and have solved the above-mentioned problems. In the following, (A) Film forming property The resin components are (A1) an emulsion of an acrylic resin, (A2) an emulsion of a polyester resin, (A3) a water-soluble polymer, (B) a black material, (B1) a composite of a black pigment and a resin, and (C) a dilution solvent.

[0010] According to the present invention, An aqueous resin composition for paint, comprising: At least (A) and (B), (A) are incompatible with each other Multiple water dispersion resin Mixed Compounds, (B) contains 90 mass% or more of (B1) having a particle size of 2 μm or more and 4 μm or less, and the mass ratio of (B) to the resin solid content of (A): 1 is 1.3 or more and 4.0 or less. is provided.

[0011] The above composition may include the following aspects. Included in (A) Mixed As one water-dispersible resin in the mixture, a resin that increases the haze value of the film formed from the mixture with one or more other water-dispersible resins as the blending amount increases can be used. (A) preferably contains 90% by mass or more of (A1) and (A2), and the mass ratio of the resin solid content of (A2) to the resin solid content of (A1):1 is 1.8 or more and 4.4 or less. (B1) preferably contains acrylic resin particles containing carbon black therein. (A) may further contain (A3), in which case the mass ratio of (A3) to the resin solid content of (A1):1 can be 1.2 or more and 1.7 or less.

[0012] According to the present invention, The composition includes the above composition, and (C), Paint with a viscosity of 1 mPa·s or more and 300 mPa·s or less at 25°C measured with a B-type viscometer. is provided.

[0013] The above paint may include the following aspects. May be used for coating model parts. May be used for coating camera parts. May be for application by spray coating method. It may be for application by a pen-type applicator method. May be for application by brush painting method. May be for application by dip coating method. May be for application by dispenser method.

[0014] According to the present invention, A pen-type applicator filled with the above paint is provided.

[0015] According to the present invention, A film formed from the above paint, A film having a glossiness (hereinafter also simply referred to as "glossiness") of less than 1.0% for incident light at an angle of 60°, a reflectance (hereinafter also simply referred to as "reflectance") of less than 1.5% for light with a wavelength of 550 nm, and an L value of less than 15 in the CIELAB color system according to the SCE method on the outermost surface on which the film is formed. is provided.

[0016] The above membrane may include the following features. When the film is required to have light-shielding properties in transmission, the optical density of the outermost surface on which the film is formed may be 2.0 or more. Effect of the Invention

[0017] According to the present invention, there are provided an aqueous resin composition for coating capable of forming a film with excellent designability, and a coating material thereof. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] The best mode for carrying out the present invention will be described below. However, the present invention is not limited to the following embodiment. Appropriate modifications and improvements to the following embodiment based on the ordinary knowledge of a person skilled in the art are also within the scope of the present invention, provided they do not deviate from the spirit of the present invention.

[0019] In the numerical ranges described in this specification, the upper or lower limit value described in a certain numerical range may be replaced with a value shown in the examples. In this specification, the content or amount of each component in a composition means, when multiple substances corresponding to each component are present in the composition, the total content or amount of those multiple substances present in the composition, unless otherwise specified.

[0020] <Aqueous resin composition for paint> The aqueous resin composition for paint according to one embodiment of the present invention (hereinafter also simply referred to as the "composition") comprises: (A) Film forming property (A) is a resin component and (B) a black material. (A) is not compatible with (B) a black material. MultipleWater-dispersed resin (hereinafter also referred to simply as "emulsion particles") Mixed Includes compounds. The film formed from the composition containing (A) and (B) has a low gloss (less than 1.0%) compared to the film formed from the conventional aqueous resin composition for paint, and also exhibits an ultra-low reflectance (less than 1.5%) and an ultra-low L value (less than 15). Although the reason is unclear, the presence of (A) Multiple water dispersion resin of When a mixture is included, incompatible regions are formed in the film after film formation, resulting in film The latter film is an incompatible film. It is believed that the action of this incompatible film and (B) blended in the film effectively contributes to the realization of low gloss, extremely low reflectance, and extremely low L value.

[0021] -(A)- The component (A) used in forming the composition is a fixing agent for the coating surface and also a binder for the component (B). Multiple (2 or more types) Water-dispersed resin (emulsion particles) Mixed For example, when the number of water-dispersible resins to be combined is two, one water-dispersible resin is designated as resin A and the other water-dispersible resin is designated as resin B, a resin having low compatibility with resin A is used as resin B. In this case, the resin B must be such that the haze value of the film formed from the mixture with the resin A increases according to the mixing amount. Specifically, the resin B that has a haze value of 3.5% or more (preferably 4.5% or more) of the film (thickness 12 μm) formed from the mixture of the resin B and the resin A in a mass ratio of 1:1 can be defined as a resin that is incompatible with the resin A (i.e., a resin that is incompatible with the resin A). The haze value can be measured by the method described later.

[0022] Whether or not the combined water-dispersed resins form "incompatible regions" (immiscible regions) in the film after film formation can also be confirmed by whether or not separate solid phases can be detected when a cut surface of the film after film formation is observed under a microscope.

[0023] Multiple water dispersion resin of By including the mixture, an incompatible region is formed in the film after film formation, and as a result, the film after film formation becomes an incompatible film. In addition, in combination with the incorporation of (B) into the incompatible film, the film surface has low gloss. In addition, it is possible to realize an even lower level of ultra-low reflectivity, and the blackness is further increased (the L value becomes even lower. Ultra-low L value). These were discovered by the present inventors.

[0024] In one embodiment, so long as the two types of water-dispersed resins form an incompatible region in the film after film formation, it is also within the scope of the present invention that a part of one resin A is dissolved in the other resin B. When three or more types (four or more types) of water-dispersed resins are used, the respective water-dispersed resins may all be incompatible with each other, but it is sufficient that one water-dispersed resin is incompatible with a mixed resin consisting of two or more (three or more) water-dispersed resins that are mutually compatible with each other.

[0025] The combination of water-dispersible resins is There are no particular limitations as long as they are mutually compatible. For example, two or more types are selected from the group consisting of acrylic resin emulsion, polyester resin emulsion, urethane resin emulsion, polyvinyl acetate resin emulsion, polyvinyl chloride resin emulsion, polybutadiene resin emulsion, polyolefin resin emulsion, etc. Among these, a combination including two types of acrylic resin emulsion and polyester resin emulsion is preferred from the viewpoint of realizing low gloss, ultra-low reflection, and ultra-low L value of the film surface after film formation, and from the viewpoint of film strength.

[0026] In one embodiment, the water-dispersible resin of The minimum film-forming temperature of the mixture is, for example, less than 40°C, and may be less than 0°C, from the viewpoint of forming a film at room temperature and providing the necessary adhesion to the coating surface.

[0027] below, As an example, when the number of water-dispersible resins to be combined is two (i.e., the combination of resin A and resin B as mentioned above),As an example, the acrylic resin emulsion is abbreviated as (A1) and the polyester resin emulsion is abbreviated as (A2). Note that the combination of (A1) and (A2) is merely a preferred example (one embodiment). Therefore, the present invention is not limited to this embodiment.

[0028] (A1) Include in (A) Multiple water dispersion resin of By including (A1) in the mixture, a film having excellent water resistance and adhesion to the coating surface can be formed. In addition, the formed film has the advantages of high strength and light resistance. (A1), which constitutes a part of (A), contains an acrylic resin and is further contained in the composition of the present invention in an emulsion state. Here, the emulsion state refers to a state in which the resin, etc. contained in the resin emulsion are dispersed in the composition as fine particles. Resins in an emulsion state generally have the property of thickening and coagulating when the aqueous solvent, which is the continuous phase, is reduced by evaporation or penetration, and can promote adhesion to the coating surface.

[0029] Examples of the acrylic resin in (A1) include polymers obtained by polymerizing one or more radical polymerizable monomers. For example, (A1) can be obtained by polymerizing one or more monomers selected from functional group-containing monomers such as (meth)acrylic acid, hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, hydroxybutyl (meth)acrylate, and an adduct of hydroxyethyl acrylate and ε-caprolactone, and further, as (meth)acrylic acid alkyl esters, methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, octyl (meth)acrylate, nonyl (meth)acrylate, decyl (meth)acrylate, dodecyl (meth)acrylate, stearyl (meth)acrylate, isobornyl (meth)acrylate, and lauryl (meth)acrylate to form an aqueous emulsion.

[0030] Examples of aqueous emulsification include a method in which solvent polymerization is followed by emulsification in water with forced stirring or using an emulsifier, and an emulsion polymerization method in which copolymerization is carried out in water using an emulsifier.

[0031] In one embodiment, (A1) includes an acrylic resin having at least one of a hydroxyl group and a carboxyl group, for example, an acrylic resin having a hydroxyl group and a carboxyl group. In one embodiment, the acrylic resin in (A1) may be a crosslinkable resin particle, for example an acrylic resin particle having crosslinkability and further having at least one of a hydroxyl group and a carboxyl group.

[0032] In one embodiment, the acrylic resin having a hydroxyl group and a carboxyl group can be obtained by emulsion polymerization of a monomer mixture containing (meth)acrylic acid alkyl ester (i), a carboxyl group-containing ethylenically unsaturated monomer (ii), and a hydroxyl group-containing ethylenically unsaturated monomer (iii). The compounds exemplified below as components of the monomer mixture may be used alone or in appropriate combination of two or more. The term "meth(acrylic)" refers to both acrylic and methacrylic.

[0033] The (meth)acrylic acid alkyl ester (i) is used to form the main skeleton of (A1).

[0034] Specific examples of the (meth)acrylic acid alkyl ester (i) include those exemplified above as the (meth)acrylic acid alkyl ester.

[0035] The carboxyl group-containing ethylenically unsaturated monomer (ii) can be used to improve the storage stability, mechanical stability, and other stabilities of the resulting (A1).

[0036] Examples of carboxyl group-containing ethylenically unsaturated monomers include acrylic acid, methacrylic acid, crotonic acid, isocrotonic acid, ethacrylic acid, propylacrylic acid, isopropylacrylic acid, itaconic acid, maleic anhydride, and fumaric acid.

[0037] The hydroxyl group-containing ethylenically unsaturated monomer (iii) imparts hydrophilicity based on the hydroxyl group to (A1), and can be used to improve the workability, etc., when this is used as a coating material.

[0038] Examples of the hydroxyl group-containing ethylenically unsaturated monomer (iii) include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, N-methylol acrylamide, allyl alcohol, and ε-caprolactone-modified (meth)acrylic monomers.

[0039] A specific example of an ε-caprolactone modified acrylic monomer is dice. ru company Examples of such products include "Placcel FA-1", "Placcel FA-2", "Placcel FA-3", "Placcel FA-4", "Placcel FA-5", "Placcel FM-1", "Placcel FM-2", "Placcel FM-3", "Placcel FM-4" and "Placcel FM-5" manufactured by Pharmaceuticals & Medical Devices, Inc.

[0040] The monomer mixture may contain at least one monomer selected from the group consisting of styrene-based monomers, (meth)acrylonitrile, and (meth)acrylamide as an optional component, and examples of the styrene-based monomer include α-methylstyrene in addition to styrene. Examples of the crosslinking monomer include ethylene glycol di(meth)acrylic acid and divinylbenzene.

[0041] The emulsion polymerization can be carried out by heating the monomer mixture in an aqueous liquid under stirring in the presence of a radical polymerization initiator and an emulsifier. The reaction temperature is preferably about 30 to 100°C, and the reaction time is preferably about 1 to 10 hours. The reaction temperature can be adjusted by adding the monomer mixture or the monomer pre-emulsion all at once or gradually dropping it into a reaction vessel containing water and an emulsifier.

[0042] As the radical polymerization initiator, known initiators that are usually used in emulsion polymerization of acrylic resins can be used. Specifically, as the water-soluble free radical polymerization initiator, for example, persulfates such as potassium persulfate, sodium persulfate, and ammonium persulfate are used in the form of an aqueous solution. In addition, so-called redox initiators, which are combinations of oxidizing agents such as potassium persulfate, sodium persulfate, ammonium persulfate, and hydrogen peroxide with reducing agents such as sodium hydrogen sulfite, sodium thiosulfate, Rongalite, and ascorbic acid, are used in the form of an aqueous solution.

[0043] The emulsifier may be an anionic or nonionic emulsifier selected from micellar compounds having a hydrocarbon group with 6 or more carbon atoms and a hydrophilic portion such as a carboxylate, a sulfonate, or a sulfate partial ester in the same molecule. Among these, anionic emulsifiers include alkali metal salts or ammonium salts of sulfuric acid half esters of alkylphenols or higher alcohols; alkali metal salts or ammonium salts of alkyl or aryl sulfonates; alkali metal salts or ammonium salts of sulfuric acid half esters of polyoxyethylene alkylphenyl ethers, polyoxyethylene alkyl ethers, or polyoxyethylene allyl ethers. Nonionic emulsifiers include polyoxyethylene alkylphenyl ethers, polyoxyethylene alkyl ethers, or polyoxyethylene allyl ethers. In addition to these general-purpose anionic and nonionic emulsifiers, various anionic and nonionic reactive emulsifiers having a radically polymerizable unsaturated double bond in the molecule, i.e., an acrylic, methacrylic, propenyl, allyl, allyl ether, maleic acid, or other group, may also be used alone or in combination of two or more kinds as appropriate.

[0044] During emulsion polymerization, the use of an auxiliary agent (chain transfer agent) for adjusting the molecular weight, such as a mercaptan compound or a lower alcohol, in combination is often preferable from the viewpoint of advancing the emulsion polymerization and promoting the smooth and uniform formation of a film and improving adhesion to the substrate, and is carried out as appropriate depending on the situation.

[0045] Any polymerization method can be used for emulsion polymerization, including the usual one-stage continuous uniform monomer dropping method, the core-shell polymerization method which is a multi-stage monomer feed method, and the power feed polymerization method which continuously changes the monomer composition fed during polymerization.

[0046] In addition, a basic compound may be added to the obtained (A1) in order to neutralize a part or all of the carboxylic acid and maintain the stability of (A1). As the basic compound, ammonia, various amines, alkali metals, etc. can be appropriately used.

[0047] The molecular weight of the acrylic resin in (A1) is not particularly limited, but may be, for example, 50,000 or more and 1,000,000 or less, or 100,000 or more and 800,000 or less, in terms of weight average molecular weight (Mw).

[0048] The glass transition temperature (Tg) of the acrylic resin in (A1) may be, for example, from −10° C. to 100° C., or from 0° C. to 80° C. In addition, the glass transition temperature (Tg) of the acrylic resin may be from 10° C. to 80° C. When the glass transition temperature (Tg) is within such a range, the acrylic resin can be dispersed in the film and exhibit higher hiding power.

[0049] The acid value of the acrylic resin in (A1) may be, for example, 2 mgKOH / g or more and 20 mgKOH / g or less, or 5 mgKOH / g or more and 10 mgKOH / g or less. When the acid value is within such a range, the compatibility with the solvent can be improved. The acid value is defined as the mass (mg) of potassium hydroxide (KOH) required to neutralize the acidic components in 1 g of the sample (solid content of the resin) (hereinafter the same). Such an acid value can be adjusted by the type and content of the monomer constituting the resin. The acid value can be adjusted, for example, by the content of the constituent unit derived from the acid group-containing monomer such as (meth)acrylic acid in the acrylic resin.

[0050] The hydroxyl value of the acrylic resin in (A1) may be, for example, 5 mgKOH / g or more and 20 mgKOH / g or more and 10 mgKOH / g or more and 20 mgKOH / g or less. When the hydroxyl value is within such a range, the advantages of dispersibility and self-crosslinking can be enjoyed. The hydroxyl value is defined as the mass (mg) of KOH required to acetylate the hydroxyl groups (hydroxyl groups) in 1 g of sample (solid resin content) (hereinafter the same).

[0051] The particle size of the acrylic resin in (A1) may be, for example, 100 nm or more and 900 nm or less, or 200 nm or more and 500 nm or less.

[0052] The medium (dispersion medium) in which the acrylic resin is dispersed in (A1) is water or a mixed solvent of water and a water-soluble organic solvent. The water-soluble organic solvent is not particularly limited as long as it is miscible with water, and examples thereof include monoalcohols, polyhydric alcohols, lower alkyl ethers of polyhydric alcohols, ketones, ethers, esters, and nitrogen-containing compounds. These may be used alone or in combination of two or more. Examples of monoalcohols include methanol, ethanol, n-propanol, n-butanol, isobutanol, n-pentanol, n-hexanol, n-heptanol, n-octanol, n-nonyl alcohol, n-decanol, or isomers thereof, cyclopentanol, cyclohexanol, etc., and preferably, alcohols having an alkyl group with 1 to 6 carbon atoms can be used. Examples of polyhydric alcohols that can be used include ethylene glycol, propylene glycol, 1,3-butylene glycol, 1,4-butylene glycol, 1,2-pentanediol, 1,5-pentanediol, neopentyl glycol, 1,2-hexanediol, 1,6-hexanediol, 1,2-cyclohexanediol, heptanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, glycerin, pentaerythritol, diethylene glycol, dipropylene glycol, triethylene glycol, tetraethylene glycol, polyethylene glycol, polypropylene glycol, and thiodiglycol. Examples of lower alkyl ethers of polyhydric alcohols that can be used include ethylene glycol monomethyl ether, ethylene glycol dimethyl ether, ethylene glycol monoethyl ether, ethylene glycol diethyl ether, ethylene glycol monopropyl ether, ethylene glycol isopropyl ether, ethylene glycol monobutyl ether, ethylene glycol isobutyl ether, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol-n-propyl ether, propylene glycol monobutyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, dipropylene glycol mono-n-propyl ether, and dipropylene glycol mono-n-butyl ether. The content of the water-soluble organic solvent is preferably as small as possible, and may not be blended at all. When blended, the content is preferably 0 to 10.0% by mass, more preferably 0 to 5.0% by mass, based on 100% by mass of the mixed solvent. If it exceeds 10.0% by mass, drying failure and blocking resistance decrease.

[0053] The resin solid content of (A1) (also simply referred to as "solid content") may be, for example, 10% by mass or more, preferably 15% by mass or more, more preferably 25% by mass or more, and preferably 50% by mass or less, more preferably 35% by mass or less.

[0054] The pH value of (A1) may be, for example, from 4 to 8, or from 4 to 7. When the pH value is within such a range, the adhesion between the formed film and the substrate can be further improved.

[0055] (A1) can be a commercially available product. For example, EM57DOC (Daicel Miraizu Company), Mowinyl 7471, Mowinyl 7540, Mowinyl DM774, Mowinyl 6520 (above, Mitsubishi ChemicalExamples of the resins include NeoCryl A-639 and NeoCryl A-1127 (both manufactured by Kusumoto Chemical Industry Co., Ltd.); Vinybran 278 and Vinybran 690 (both manufactured by Nissin Chemical Industry Co., Ltd.); and the like. These may be used alone or in combination of two or more.

[0056] (A2) Include in (A) Multiple water dispersion resin of The mixture containing (A2) has the advantage of improving the strength of the formed film. (A2), which constitutes a part of (A), contains a polyester resin and is contained in the composition of the present invention in an emulsion state, in the same manner as (A1).

[0057] The polyester resin in (A2) may be, for example, a condensate of a polybasic acid and a polyhydric alcohol. Examples of the polybasic acid include phthalic anhydride, isophthalic acid, terephthalic acid, adipic acid, and succinic anhydride. Examples of the polyhydric alcohol include ethylene glycol, propylene glycol, 1,3-butylene glycol, 1,6-hexanediol, polyethylene glycol, and polypropylene glycol.

[0058] In one embodiment, the polyester resin in (A2) preferably has a carboxy group and / or a sulfonic acid group. The polyester resin has these hydrophilic groups, which improves dispersibility in water, and as a result, a more uniform film can be formed from a coating material containing the composition, and the adhesion between the film and the substrate can be further improved.

[0059] The molecular weight of the polyester resin in (A2) is not particularly limited, but may be, for example, 6,000 or more and 20,000 or less, or 8,500 or more and 20,000 or less, in number average molecular weight (Mn).

[0060] The glass transition temperature (Tg) of the polyester resin in (A2) may be, for example, from 40° C. to 80° C., or from 55° C. to 75° C. When the glass transition temperature (Tg) is within such a range, a film having excellent water resistance and adhesion to the substrate can be formed.

[0061] The acid value of the polyester resin in (A2) may be, for example, 1 mgKOH / g or more and 10 mgKOH / g or 1 mgKOH / g or more and 8 mgKOH / g or more. When the acid value is within such a range, the compatibility with the solvent can be improved.

[0062] The hydroxyl value of the polyester resin in (A2) may be, for example, 1 mgKOH / g or more and 20 mgKOH / g or less, or 1 mgKOH / g or more and 10 mgKOH / g or less. When the hydroxyl value is within such a range, the advantages of dispersibility and self-crosslinking can be enjoyed.

[0063] The particle size of the polyester resin in (A2) may be, for example, from 10 nm to 300 nm, or from 50 nm to 150 nm.

[0064] As the dispersion medium for the polyester resin in (A2), water or a mixture of water and an organic solvent can be used, similar to the dispersion medium in (A1) described above.

[0065] The solid content of (A2) may be, for example, 50% by mass or more, preferably 60% by mass or more, more preferably 70% by mass or more, and preferably 90% by mass or less, more preferably 80% by mass or less.

[0066] Commercially available products can be used as (A2). For example, KA-5071S, KZT-8803, KT-8701, KZT-9204 (Unitika Co., Ltd.); Vylonal MD1200, MD1245, MD1480, MD1930, MD2000, MD1500 (Toyobo Co., Ltd.); High Tech PE series such as PES-H001 (Toho Chemical Industry Co., Ltd.); New Track 2010 (Kao Corporation); Super Flex 210 (Daiichi Kogyo Seiyaku Co., Ltd.); Plus Coat Z730, Z760, Z592, Z687, Z690 (Go-o Chemical Industry Co., Ltd.); and the like can be mentioned. These may be used alone or in combination of two or more.

[0067] In one embodiment, the mass ratio of the resin solid content of (A2) in (A) is preferably 1.8 or more, more preferably 2.0 or more, and preferably 4.4 or less, more preferably 3.0 or less, relative to the resin solid content of (A1) : 1. By blending (A2) within this resin solid content mass ratio range, it is possible to enjoy stable film strength (no peeling off of the film from the coating surface or poor adhesion to the coating surface).

[0068] The combined content (total amount) of (A1) and (A2) in (A) is preferably 90% by mass or more, more preferably 95% by mass or more. The upper limit is not particularly limited and is 100% by mass. That is, in one embodiment, (A1) and (A2) may be contained in 100% by mass of (A), preferably at 90% by mass or more.

[0069] When (A) contains another resin emulsion together with (A1) and (A2), the mass ratio of the resin solid content of the other resin emulsion in (A) to the total of (A1) and (A2):1 is, for example, 0.4 or less.

[0070] The molecular weight (Mw, Mn), glass transition temperature (Tg), acid value, hydroxyl value, and particle size of each water-dispersible resin (acrylic resin, polyester resin, or other resin), as well as the resin solids concentration (solids content) of the emulsion, may all be measured by any method known to those skilled in the art.

[0071] For example, the molecular weight (Mw, Mn) of each water-dispersed resin is measured by gel permeation chromatography (GPC). GPC is performed using HLC-8020GPC (Tosoh Corporation), three TSKgel Super Multipore HZ-H (Tosoh Corporation, 4.6 mm ID x 15 cm) columns, THF (tetrahydrofuran) as the eluent, detection with THF as the solvent, and conversion using polystyrene as the standard substance. The glass transition temperature (Tg) is measured by a differential scanning calorimeter according to the DSC method. More specifically, the glass transition temperature can be measured by a differential scanning calorimeter (DSC) (e.g., Shimadzu Corporation's differential scanning calorimeter "DSC-50"). When multiple glass transition temperatures are observed, the main transition temperature with the largest heat absorption can be used. The acid value and hydroxyl value are measured in accordance with the method (potentiometric titration method) defined in the JIS standard (JIS K0070, 1992). The particle size is the average particle size of primary particles, and is measured, for example, using a particle size distribution analyzer (FPAR-1000: Otsuka Electronics Co., Ltd.) using a dynamic light scattering method. It can also be measured (specified) using image analysis using, for example, a transmission electron microscope (TEM) or a scanning electron microscope (SEM). The solid content of the emulsion is calculated from the residue after drying at 150℃ for 2 hours.

[0072] (A3) (A) is Multiple water dispersion resin of The mixture may contain a water-soluble polymer (A3). By containing (A3) in (A), it is expected that the adhesion of the formed film to the coating surface will be improved.

[0073] The water-soluble polymer is not particularly limited as long as it is water-soluble, and examples thereof include polycarboxylic acid polymers, polyvinyl alcohol polymers, cellulose and its derivatives, gelatin, polymers having structural units derived from N-vinyl cyclic lactams, etc. These may be used alone or in combination of two or more.

[0074] When (A3) is contained in (A), it is preferable to use polyvinyl alcohol (PVA) from the viewpoint of the stability of the composition. Polyvinyl alcohol is a polymeric compound obtained by saponifying polyvinyl acetate with an alkali, acid, ammonia water, etc., and is preferably a partially saponified type having a saponification degree of about 78.5 to 89.0 mol%, which is good for the stability over time of the composition. This is the so-called polyvinyl alcohol (PVA) with a low to medium saponification degree. The average degree of polymerization is preferably about 300-2,300, and more preferably about 1,500-1,900.

[0075] Commercially available products can be used as (A3). For example, Gohsenol GH23 (degree of polymerization: about 2300, degree of saponification: 86.5 to 89.0 mol%), Gohsenol GH20 (degree of polymerization: about 2000, degree of saponification: 86.5 to 89.0 mol%), Gohsenol GH17 (degree of polymerization: about 1700, degree of saponification: 86.5 to 89.0 mol%), Gohsenol GM14 (degree of polymerization: about 1400, degree of saponification: 86.5 to 89.0 mol%), Gohsenol GL-03 (degree of polymerization: about 300, degree of saponification: 86.5 to 89.0 mol%) ...GL-03 (degree of polymerization: about 300, degree of saponification: 86.5 to 89.0 mol%), Gohsenol GL-03 (degree of polymerization: about 300, degree of saponification: 86.5 %), GL-05 (degree of polymerization about 500, degree of saponification 86.5-89.0 mol%), KH20 (degree of polymerization about 2000, degree of saponification 78.5-81.5 mol%), KH17 (degree of polymerization about 1700, degree of saponification 78.5-81.5 mol%), KL-03 (degree of polymerization about 300, degree of saponification 78.5-82.0 mol%), KL-05 (degree of polymerization about 500, degree of saponification 78.5-82.0 mol%) (all of the above, Mitsubishi ChemicalCompany: Kuraray Poval PVA-203 (degree of polymerization approx. 300, degree of saponification 86.5-89.5 mol%), PVA-204 (degree of polymerization approx. 400, degree of saponification 86.5-89.5 mol%), PVA-205 (degree of polymerization approx. 500, degree of saponification 86.5-89.5 mol%), PVA-210 (degree of polymerization approx. 1000, degree of saponification 88.0 mol%), PVA-217 (degree of polymerization approx. 1700, degree of saponification 88.0 mol%), PVA-220 (degree of polymerization approx. 2000, degree of saponification 88.0 mol%), PVA-217EE (degree of polymerization about 1700, degree of saponification 88.0 mol%), PVA-217E (degree of polymerization about 1700, degree of saponification 88.0 mol%), PVA-220E (degree of polymerization about 2000, degree of saponification 88.0 mol%), PVA-403 (degree of polymerization about 300, degree of saponification 80.0 mol%), PVA-405 (degree of polymerization about 500, degree of saponification 83.0 mol%), PVA-420 (degree of polymerization about 2000, degree of saponification 81.0 mol%) (all from Kuraray Co., Ltd.); Denka Poval B-03 (degree of polymerization about 300, degree of saponification 87-89 mol%), Denka Poval B-05 (degree of polymerization about 500, degree of saponification 87-89 mol%) (all from Kuraray Co., Ltd.); Denka Unitika Poval UP050G (polymerization degree approx. 500, saponification degree approx. 87-89 mol%, Unitika ) : etc. These may be used alone or in combination of two or more.

[0076] When (A) contains (A3), the mass ratio of (A3) in (A) is preferably 1.2 or more, more preferably 1.35 or more, and preferably 1.7 or less, more preferably 1.55 or less, relative to the resin solid content of (A1) : 1. By blending (A3) within this resin solid content mass ratio range, it is easy to improve the adhesion of the formed film to the coating surface.

[0077] The content (total amount) of the resin solids of (A) is not particularly limited, but taking into consideration the blending balance with other components, it is preferably 10 mass% or more, more preferably 20 mass% or more, even more preferably 25 mass% or more, and preferably 50 mass% or less, more preferably 40 mass% or less, and even more preferably 35 mass% or less, relative to the total amount (100 mass%) of all solids in the composition.

[0078] -(B)- (B) used to form the composition includes (B1) a composite of a black pigment and a resin. The resin constituting the composite with the black pigment is insoluble in water. Examples of such resins include epoxy resins, acrylic resins, urethane resins, styrene resins, ethylene resins, phenol resins, urea resins, amide resins, melamine resins, and benzoguanamine resins. Among these, from the viewpoint of dispersibility, acrylic resins and urethane resins are preferred, and acrylic resins are more preferred. These may be used alone or in combination of two or more. In addition, the name of the resin particles can be partially abbreviated by adding the name of the resin before the name of beads. For example, resin particles made of acrylic resin are sometimes called acrylic beads.

[0079] The black pigment constituting the composite with the resin is not particularly limited, but it is preferable to use carbon black (hereinafter, also simply referred to as "CB"), which has a large effect of blackening the composite and is advantageous in terms of cost. By using CB, the film formed is colored, so that the antireflection effect is further improved and good antistatic effect is obtained.

[0080] Examples of the composite form of the black pigment and the resin include (1) a form in which the black pigment is coated with the resin (including a form in which the black pigment is encapsulated in the resin particles), (2) a form in which the resin is bonded to the surface or inside of the black pigment, or (3) a form in which the resin is attached to the surface or inside of the black pigment, or a composite form of these.

[0081] Examples of the means for coating the surface of the black pigment with a resin include the microencapsulation method, more specifically the interfacial polymerization method, the in-situ polymerization method, the liquid curing coating method (orifice method), the phase separation method from an aqueous solution, and the liquid drying method. In addition to the microencapsulation method, there are also methods for bonding or attaching a resin to a dispersed black pigment. For example, there is a method in which the pigment is used as a core and the surface is covered with a large number of colloidal resin particles. When using a colorant in which the black pigment core is covered with colloidal resin particles, it is desirable that the size of the surrounding resin particles is sufficiently small compared to the pigment core. Furthermore, it is desirable that the colloidal resin particles cover the pigment core with almost no gaps. However, this does not exclude the pigment core being directly exposed to the outside.

[0082] (B1) may be a pigment bound to a resin having a particle size similar to that of the pigment. Alternatively, the black pigment or black dye may be kneaded into a thermoplastic or thermosetting resin and pulverized to form a composite of the black pigment and the resin.

[0083] In one embodiment, the composite form is preferably form (1), i.e., resin particles encapsulating a black pigment, from the viewpoint of improving dispersibility. In the resin particles encapsulating a black pigment, the pigment is encapsulated in resin particles having a larger diameter, so aggregates are less likely to occur in the composition compared to when a pigment having a smaller diameter is directly blended in the composition, which contributes to improving dispersibility.

[0084] The content of the pigment (particularly CB) in (B1) is preferably 1 mass% or more, more preferably 5 mass% or more, even more preferably 10 mass% or more, and preferably 50 mass% or less, more preferably 40 mass% or less, even more preferably 30 mass% or less.

[0085] The particle size of (B1) is preferably 2 μm or more, more preferably 3 μm or more, preferably 8 μm or less, more preferably 6 μm or less, and even more preferably 4 μm or less. If the particle size is too small, the amount of aggregates in the composition increases, making dispersion difficult. If the particle size is too large, the coloring power tends to decrease. The particle size of (B1) refers to the particle size (D50) value at which the integrated value expressed as an integrated (cumulative) percentage in the particle size distribution is 50%.

[0086] The shape of (B1) is not particularly limited, but from the viewpoint of matte, a perfect sphere is preferable. In order to realize a single layer of low gloss, low reflection, and low L value of the film surface to be formed, it is preferable to use particles (sharp products) with a narrow particle size distribution (CV (Coefficient of Variation) value is, for example, 15 or less). The CV value is a numerical value of the degree of spread of particle size distribution (variation of particle size) relative to the average particle size (arithmetic mean particle size). By using such particles, they are uniformly contained in the film and fine unevenness is formed on the film surface, making it easy to realize a single layer of low gloss, low reflection, and low L value of the film surface. In order to further reduce the gloss of the film surface, amorphous particles may be used as (B1). By using amorphous particles as (B1), the gloss of the film surface can be further reduced by repeating light refraction on the surface and inside of (B1) when the film is formed.

[0087] Commercially available products can be used as (B1). Examples of those containing urethane beads include Art Pearl C800 Black (particle size 6.5 μm, CB content 7.5%, Negami Chemical Industries Co., Ltd.). Examples of those containing acrylic (acrylic copolymer) beads include Art Pearl GR-004BK (particle size 3.8 μm, CB content 37%, Negami Chemical Industries Co., Ltd.); Lovecolor 224 (SMD) Black (average particle size 2 to 3 μm, CB content 18%, Dainichiseika Chemical Industries Co., Ltd.); etc.

[0088] The content of (B1) in (B) is preferably 90% by mass or more, more preferably 95% by mass or more. The upper limit is not particularly limited, and is 100% by mass. That is, in one embodiment, (B1) may be contained in 100% by mass of (B) at preferably 90% by mass or more.

[0089] In one embodiment, the mass ratio of (B) is preferably 1.3 or more, more preferably 1.9 or more, and preferably 4.0 or less, more preferably 3.0 or less, relative to the resin solid content of (A) : 1. By blending (B) within this mass ratio range, it is possible to enjoy low gloss, low reflectance, and low L value while maintaining the coating film strength.

[0090] The content (total amount) of (B) is, for example, 60% by mass or more, preferably 65% ​​by mass or more, more preferably 75% by mass or more, and for example, 90% by mass or less, preferably 85% by mass or less, more preferably 80% by mass or less, based on the total amount (100% by mass) of all solid contents of the composition. If the total amount of (B) is less than 60% by mass, problems such as increased gloss and insufficient optical density occur, and if it exceeds 90% by mass, the amount of (A) in the formed film becomes relatively small, which may result in problems such as the film falling off from the coated object.

[0091] -Optional ingredients- In addition to the above components ((A) and (B)), the composition may contain other optional components as long as they do not impede the effects of the present invention. However, the total mass of the above components ((A) and (B)) is preferably 50% by mass or more in 100% by mass of the solid content of the composition. This mass proportion varies depending on the physical properties required of the composition, but is more preferably 70% by mass or more, even more preferably 80% by mass or more, and particularly preferably 90% by mass or more.

[0092] The composition is an aqueous composition in which the above emulsions (A1, A2) are dispersed in the above dispersion medium.

[0093] The composition according to one embodiment of the present invention can be prepared (manufactured) by mixing and stirring (A1), (A2), (B), and optional components added as necessary. The order in which the components are mixed is not particularly limited as long as these components are mixed uniformly.

[0094] <Water-based paint> An aqueous paint according to one embodiment of the present invention (hereinafter also simply referred to as "paint") is used to form a film of the above composition on a coating surface, and contains the above composition and (C) a dilution solvent. The content of the above composition in the paint is preferably 90% by mass or more, more preferably 95% by mass or more, based on the total amount (100% by mass) of all solids in the paint. The upper limit is not particularly limited, and is 100% by mass.

[0095] -(C)- (C) is used in the formation of the paint, and is blended for the purpose of adjusting the viscosity of the paint. The use of (C) improves the uniformity of the paint. In addition, the viscosity of the paint can be adjusted appropriately, which makes it possible to improve the operability of the paint and the uniformity of the coating thickness when forming a film on the painted surface, and therefore can greatly contribute to improving the design of the final product.

[0096] (C) is not particularly limited as long as it is a solvent capable of adjusting the paint viscosity. As with the dispersion medium of the emulsion particles, water or a mixture of water and an organic solvent can be used. The amount of the solvent to be added may be appropriately set to adjust the solid content concentration of the paint.

[0097] The appropriate range for paint viscosity varies depending on the application method, so it is difficult to generalize, but the viscosity at 25°C measured with a B-type viscometer is approximately 1 mPa·s to 300 mPa·s. For example, if the application method is spray coating, the range is 1 mPa·s to 50 mPa·s. 、 If the application method is dip coating, the viscosity should be between 100 mPa·s and 300 mPa·s. 、If the coating method is a dispenser method, the viscosity should be between 100 mPa·s and 250 mPa·s. 、 It is preferable to apply the paint to a pen-type applicator. Mitsuru When used with a filling, it should be 80 mPa s or more and 230 mPa s or less. 、 It is preferable to set the temperature to about 100° C.

[0098] In the case of the spray coating method, if the viscosity of the paint is too low, it may not be possible to form a film thick enough to exhibit the desired performance. If the viscosity of the paint is too high, it is likely to cause inconveniences such as the liquid not coming out of the nozzle, or not being able to atomize even if it comes out. In the case of the dip coating method, if the viscosity of the paint is too low, it may cause severe dripping and unevenness, making it impossible to form a clean film. If the viscosity of the paint is too high, it may cause poor liquid cutting when the coated object is pulled out of the paint, resulting in burrs, or the surface shape of the coating film may tend to become flat, resulting in a glossy appearance. In the case of the dispenser method, if the viscosity of the paint is too low, it may cause splashing and dripping, resulting in the paint being applied to places where it is not desired to apply. If the viscosity of the paint is too high, it may cause the liquid not to come out of the nozzle, or even if it comes out, the surface shape may tend to become flat, resulting in a glossy appearance. Applying paint to a pen-type applicator Mitsuru When using the paint by filling it, if the viscosity of the paint is too low, the film thickness will be too thin, resulting in insufficient optical density, and the paint will spread out and not allow for clean lines to be drawn. If the viscosity of the paint is too high, the liquid will not come out of the pen tip, streaks will easily form, and clean lines will not be able to be drawn.

[0099] The viscosity of the paint varies depending on the components contained in the composition in the paint, i.e., the types and molecular weights of the (A) and (B) used to form the composition, and also varies depending on the type and molecular weight of any optional components added in addition to the above (A) and (B); however, it can be easily adjusted by appropriately determining the amount of (C) in the paint.

[0100] -Other additives- In addition to the above-mentioned components (composition, (C)), the coating material may contain one or more other additives, so long as they do not impair the effects of the present invention. Examples of other additives include leveling agents, thickeners, pH adjusters, lubricants, dispersants, antifoaming agents, curing agents, and reaction catalysts. When other additives are added, the amount added is preferably 0 to 100 parts by mass, and more preferably 0 to 30 parts by mass, per 100 parts by mass of the resin solid content in the coating material.

[0101] In one embodiment, the paint may be for coating parts of a model assembly. The paint according to one embodiment may be for coating camera parts. The coating material according to one embodiment may be for application by a spray coating method. The coating material according to one embodiment may be for application using a pen-type applicator, for application using a brush coating method, for application using a dip coating method, or for application using a dispenser method. The coating material according to one embodiment can be used by being contained in a pen-type coating tool.

[0102] <Application method, object to be coated> The film according to one embodiment of the present invention is formed by applying the coating material to a substrate to form a coating film, and then drying the coating film to form a film.

[0103] The coating method may be a spray coating method (e.g., air spray method, airless spray method, electrostatic spray method, etc.). By using the spray coating method, even if the surface of the object to be coated has protrusions or steps, a film having a uniform thickness and specific performance can be formed over the entire surface.

[0104] The application conditions for the spray coating method are: the diameter of the spray gun is about 0.2 to 1.2 mm, and the amount of the discharged liquid is 0.2 to 10 ( g / min ) The minimum distance between the spray gun and the workpiece surface is about 30 to 500 mm, and the coating speed is 30 to 300( mm / sec ) The preferred number of spray guns is about 1.5 to 10 mm, the overlap pitch is about 1.5 to 10 mm, and the atomizing air pressure is about 0.03 to 0.2 MPa. In addition to using a single gun, multiple guns may be arranged according to the size of the workpiece from the viewpoint of coating efficiency.

[0105] After the coating material is applied to the surface of the substrate, the solvent is removed by drying to form a film. If necessary, the coating film may be cured by irradiating it with UV light or EB light or by heating the coating film.

[0106] The coating material may be applied by a spray coating method, or may be applied by a method using a pen-type applicator such as a marking pen, a method using a brush (brush painting), a dip coating method, or a dispenser method.

[0107] In one embodiment, the configuration of the pen-type applicator is not limited, and examples include those equipped with a pen tip, a paint refilling mechanism, a pen tip extension / retraction mechanism, and a paint supply mechanism.

[0108] Examples of applicator pen tips include ballpoint pen tips in which a ball is rotatably held in a ball house (ball-holding chamber) in the tip body, as well as pen cores such as fiber tips, felt tips, and plastic tips, and metal fountain pen tips.

[0109] The paint refilling mechanism of the applicator may be configured to directly refill the paint, or may include a paint reservoir or occlusion body into which the paint can be refilled. When the paint refilling mechanism is configured to directly refill the paint, it is preferable that the paint container has a built-in agitator such as a stirring ball for stirring the paint in order to facilitate the redispersion of (B). Examples of the shape of the agitator include a sphere, a rod, etc. The material of the agitator is not particularly limited, but specific examples include metal, ceramic, resin, glass, etc. When the paint refilling mechanism includes a paint occlusion body, the paint occlusion body is preferably configured as a fiber bundle made of twisted fibers.

[0110] The pen tip extending / retracting mechanism of the applicator is not particularly limited, and examples thereof include a cap type having a cap that covers the pen tip, a knock type, a rotation type, a slide type, etc. Also, it may be a retractable type that allows the pen tip to be housed in the barrel.

[0111] The paint supply mechanism of the applicator is not particularly limited, and examples include: a mechanism that has a paint guide core made of a fiber bundle or the like as a paint flow rate adjustment member and supplies the paint to the pen tip; a mechanism that has a comb-shaped paint flow rate adjustment member and supplies the paint to the pen tip through this; a mechanism that guides the paint to the pen tip via a pen core in which a large number of disks are arranged in parallel at comb-groove intervals, with slit-shaped paint guide grooves running vertically through the disks in the axial direction and wide ventilation grooves formed beyond the grooves, and a paint guide core is arranged in the axial center for guiding paint from a paint storage section to the pen tip; a mechanism that has a paint flow rate adjustment member with a valve mechanism and supplies the paint to the pen tip; a mechanism that supplies the paint directly to the pen tip from a paint container or barrel equipped with a pen tip; and the like.

[0112] In one embodiment, the pen-type applicator is, for example, a marking pen such as an application marker for a model assembly kit, and the pen tip is not particularly limited and may be, for example, a fiber tip, a felt tip, or a plastic tip, and further, the shape may be bullet-shaped, chisel-shaped, brush-pen-shaped, or the like. In one form, the pen-type applicator may be a liquid-type pen having a cylindrical barrel, a paint container, an agitator built into the paint container for agitating the paint, and a valve mechanism for regulating the supply of the paint contained in the paint container to the pen tip, and the valve mechanism is released when the pen tip is pressed, causing the paint to flow out onto the pen tip.

[0113] When the above paints are applied by brush painting, the thickness of the film formed on the painted surface tends to vary depending on the location, but the performance of the film obtained is equivalent to that of other application methods. The reason for this is unclear, but it is thought to be because the appropriate amount of pigment is included, forming unevenness.

[0114] The object to be coated with the paint (substrate) is not particularly limited, and may be, for example, an object having a hard surface made of glass, resin, metal, ceramics, wood, etc. The shape of the substrate is also not particularly limited, and examples thereof include plate-shaped, (hollow) cylindrical, and film-shaped objects. Examples of substrates include the following: · Electrical and electronic devices such as mobile phones, smartphones, tablets, PCs, PC peripherals (keyboards, printers, external disks, etc.), watches, audio equipment, and various office automation equipment. ·Home appliances such as refrigerators, vacuum cleaners, microwave ovens, televisions, and recording devices. Stairs, floors, desks, chairs, dressers, other furniture and woodwork. - Various building materials, flooring, interior and exterior walls of buildings, etc. ·Vehicles such as automobiles and motorcycles or their parts: Specifically, vehicle bodies, interior parts (meter panels, dashboards, handlebars, etc.), bumpers, spoilers, door handles, headlights, taillights, aluminum wheels, motorcycle gas tanks, etc. Optical applications, such as lenses mounted on various camera units, the inner walls of lens barrels, inner and outer covers of lens units, lens spacers, and other camera parts. Glasses, goggles and similar products. Hobby products made of resin molded products, and their assembly parts (for example, assembly models (plastic models, etc.), parts of assembly models in model kits, etc.).

[0115] <Membrane characteristics> The properties of the film formed from the above paint are as follows:

[0116] (glossiness, reflectance, L value, optical density, adhesion) The film formed from the above coating preferably has a film surface with a gloss of less than 1.0%, a reflectance of less than 1.5%, and an L value of less than 15. When light-shielding properties in transmission are required for the film formed from the above coating, in addition to the above characteristics (film surface with a gloss of less than 1.0%, a reflectance of less than 1.5%, and an L value of less than 15), the film surface preferably has an optical density of 2.0 or more.

[0117] Here, if the film formed from the above coating material is exposed on the outermost surface, it is preferable that the gloss, reflectance, L value, and optical density, if necessary, of the film surface are literally within the above ranges. If another film is coated on the film formed from the above coating material, it is preferable that the gloss, reflectance, L value, and optical density, if necessary, of the surface of the other film, i.e., the outermost surface of the film formed on the substrate, are within the above ranges. Hereinafter, these surfaces are collectively referred to as the "outermost surface of the film."

[0118] The film formed from the above coating preferably has a gloss of less than 1.0%, a reflectance of less than 1.5%, and an L value of less than 15 on the outermost surface of the film. When light-shielding properties in transmission are required for the film formed from the above coating, in addition to the above characteristics (gloss of the outermost surface of the film less than 1.0%, reflectance of less than 1.5%, and L value of less than 15), the optical density of the outermost surface of the film is preferably 2.0 or more. By having the gloss, reflectance, L value, and optical density, as required, of the outermost surface of the film within the above ranges, it is possible to achieve low gloss, low reflectance, high blackness, and, as required, high light-shielding properties of the outermost surface of the film.

[0119] The upper limit of the glossiness is more preferably less than 0.7%, and even more preferably less than 0.5%. By adjusting the glossiness to the above range, flare and ghost phenomena caused by diffuse reflection of light can be effectively prevented. The lower limit of the glossiness is not particularly limited, and the lower the better.

[0120] The upper limit of the reflectance is more preferably less than 1.25%, and even more preferably less than 1.0%. The lower limit of the reflectance is not particularly limited, and the lower the better. By adjusting the reflectance within the above range, flare and ghost phenomena caused by diffuse reflection of light can be more effectively prevented.

[0121] The upper limit of the L value (blackness) is more preferably less than 12. Furthermore Preferably, it is less than 10. The lower limit of the L value is not particularly limited, but from the viewpoint of obtaining a blacker appearance, the lower the value, the better. By adjusting the L value to the above range, the blackness is high and the blackness stands out, resulting in excellent design, and therefore the film can be suitably used as a camera unit for mobile phones such as smartphones. The above L value refers to the lightness L* value of the outermost surface of the film in the CIE 1976 L*a*b* (CIELAB) color system according to the SCE method. The SCE method is a method of measuring color by removing specular reflected light. The definition of the SCE method is stipulated in JIS Z 8722 (2009). Since the SCE method removes specular reflected light when measuring, the color is closer to what the human eye actually sees. CIE is an abbreviation of Commission Internationale de l'Eclairage, which means International Commission on Illumination. CIELAB display color is a uniform color space recommended in 1976 and specified in JIS Z 8781 (2013) to measure color differences due to differences in perception and devices. The three coordinates of CIELAB are L* value, a* value, and b* value. L* value indicates lightness and is expressed as 0 to 100. An L* value of 0 means black, and an L* value of 100 means diffuse white color. a* value indicates a color between red and green. If the a* value is negative, it means a color leaning toward green, and if it is positive, it means a color leaning toward red. b* value indicates a color between yellow and blue. If b* is negative, it means a color leaning toward blue, and if it is positive, it means a color leaning toward yellow.

[0122] In the case where the film formed from the coating material is required to have light-shielding properties in transmission, the lower limit of the optical density is more preferably 2.5 or more, and even more preferably 3.2 or more. By adjusting the optical density to the above range, the light-shielding properties can be further improved. The upper limit of the optical density is not particularly limited, and the higher the better.

[0123] The glossiness, reflectance, L value, and optical density can be measured by the methods described below.

[0124] In addition to the above characteristics (glossiness, reflectance, L value, and optical density if necessary), the film formed from the coating material preferably has good adhesion to the coating surface. The adhesion of the film formed from the coating material to the coating surface is preferably such that 90% or more of the coating remains, as shown in the adhesion evaluation in the Examples described later. EXAMPLES

[0125] The present invention will be specifically described below based on experimental examples (including examples and comparative examples), but the present invention is not limited to these experimental examples. In the following description, "parts" refers to "parts by mass" and "%" refers to "% by mass".

[0126] [Components of water-based paints] A( Film forming property The following resin components were prepared: A1a: Acrylic resin emulsion (Movinyl 7471, Mitsubishi Chemical Corporation) (Acrylic ester copolymer, resin Tg 23°C, resin solids 44%) A2a: Polyester resin emulsion (Vylonal MD1200, Toyobo) (Resin Tg 67℃, resin solids 34%, Mn 15,000, acid value 1mgKOH / g, hydroxyl value 5mgKOH / g) A3a: Polyvinyl alcohol (Gohsenol KH17, Mitsubishi Chemical Corporation) (Resin solid content 15%, polymerization degree approx. 1700, saponification degree 78.5-81.5 mol%)

[0127] The resin solids (acrylic resin and polyester resin) in "Movinyl 7471" used in A1a and "Vylonal MD1200" used in A2a (both emulsions) were mixed at a mass ratio of 1:1 to form a film from the mixture, and the haze value of the film (thickness 12 μm) obtained was measured using a haze meter (NDH4000, Nippon Denshoku Industries Co., Ltd.) in accordance with the method of JIS K7136. The haze value of the film (film 1) is The ratio of the resin solid content of A2a to the resin solid content of A1a was then changed to 1.23, 2.94, and 12.25, respectively, and the film was formed in the same manner as above. each The haze value of the film was measured. The haze value of each film (films 2 to 4) is It was confirmed that the haze value increased as the mixing amount of A2a increased to 4.72%, 8.55%, and 15.82%, respectively. When the cut surfaces of each film (films 1 to 4) were observed under a microscope, separate solid phases were detected, confirming that incompatible regions were formed within each film (each film was an incompatible film).

[0128] The following was prepared as B (black material): B1a: Black acrylic beads (particle size 2-3μm) (Lovecolor 224 (SMD) Black, Dainichi Seika Color & Chemicals Co., Ltd., CB content 18%) B2a: Black acrylic beads (particle size 7-9μm) (Lovecolor 220 (MD) Black, Dainichi Seika Color & Chemicals Co., Ltd., CB content 5%) ·B2b: CB (particle size 150nm) (MHI Black #273, Mikuni Color Co., Ltd., CB content 9.5%) B2c: Composite silica (particle size 3μm) (Vexia ID, Fuji Silysia Chemical)

[0129] In addition, "Labcolor 224 (SMD) Black" used in B1a and "Labcolor 220 (MD) Black" used in B2a are both spherical acrylic resin particles containing CB, and are one of the composites of CB and acrylic resin. "MHI Black_#273" used in B2b (CB) is a CB dispersion, and of the total solid content of the dispersion of 18%, 9.5% is CB and the remaining 8.5% is other compounds. Of the 8.5% other compounds, 3% is copper compounds and 5.5% is acrylic resin. "Vexia ID" used in B2c (composite silica) is a composite particle of CB and silica with a CB / silica ratio of approximately 25 / 75 (mass ratio).

[0130] The following was prepared as C (dilution solvent): ·C1: Water C2: Alcohol

[0131] [Subject to be coated] A smartphone housing (plastic outer box) was prepared as the substrate.

[0132] [Experimental Examples 1 to 23 and 4a to 17a] 1. Preparation of Water-Based Paint Each component for each experimental example was added to a mixed solvent of water and alcohol in the specified amounts shown in Tables 1 and 2 so that the total solids content (mass%) and the solids content ratio of each component were the values ​​shown in Tables 1 to 3, and the components were stirred and mixed to prepare water-based paints (hereinafter simply referred to as "paints").

[0133] 2-1. Formation of Membrane 1 The paint obtained in each experimental example was sprayed onto the substrate to form a coating film using a spray coating method in the same manner as in (3-3-1) Coating Property 1 below. The coating film was then left to stand at room temperature for approximately 5 to 10 minutes to form a spray coating film 1 with an average thickness of 20 μm on the coating surface of the substrate.

[0134] 2-2. Formation of Membrane 2 The marking pen used in (3-3-2) Coating property 2 below was used to fill in the surface of the substrate in the same manner to form a coating film, and the coating film was then left to stand at room temperature for 5 to 10 minutes to form a written film 2 with an average thickness of 10 μm on the coating surface of the substrate.

[0135] 3. Evaluation The paints obtained in each experiment were evaluated for various properties (viscosity, injectability, coatability1 and Spreadability 2, dripping property) were evaluated (paint evaluation). In addition, for the films 1 and 2 formed from the paints obtained in each experimental example, various properties (characteristics) were evaluated by the methods described below (film evaluation). The results are shown in Tables 1 to 3.

[0136] [Paint evaluation] (3-1-1) Viscosity 1 The viscosity of the paint was measured using a B-type viscometer (Tokisan Co., Ltd.) Company Measurements were performed using a VISCOMETER BM2 (manufactured by VISCOMETER) under the conditions of 25° C., 60 rpm, 1 minute, and No. 1 rotor. The evaluation criteria are as follows.

[0137] ○: Viscosity is 1 mPa s or more and 50 mPa s or less (good viscosity) ×: Viscosity exceeds 50 mPa·s (too high viscosity) (3-1-2) Viscosity 2 The viscosity of the paint was measured using a B-type viscometer (Tokisan Co., Ltd.) Company Measurements were performed using a VISCOMETER BM2 (manufactured by VISCOMETER) under the conditions of 25° C., 60 rpm, 1 minute, and No. 2 rotor. The evaluation criteria are as follows.

[0138] Good: Viscosity is between 80mPa·s and 230mPa·s (good viscosity) ×: Viscosity exceeds 230 mPa·s (too high viscosity)

[0139] (3-2) Injectability The injectability of the paint was evaluated by observing the state of injection into the air spray. Using an air sprayer with an air brush (Spray Work HG Single Air Brush, Tamiya) attached to an air can (Spray Work Air Can 420D, Tamiya), the paint was visually observed as it went from the cup of the air brush into the nozzle to evaluate the pourability. The evaluation criteria were as follows:

[0140] 〇: There was no clogging at all and the liquid entered the nozzle smoothly. △: There was no clogging, but the liquid flowed into the nozzle a little slowly. ×: The liquid was clogged and did not enter the nozzle.

[0141] (3-3-1) Spreadability 1 Coating properties 1: By spray coating method Coating Each paint was poured into the air spray used in (3-2) above, and sprayed onto the outer surface of the object to be coated for 10 seconds from a distance of 10 cm from the tip of the airbrush, and the formed coating film (before drying) was visually evaluated for coating unevenness. (3-3-2) Spreadability 2 The coating properties2 of the paints were evaluated by observing the unevenness of the coating after writing with a marking pen. The paint obtained in each experiment and one stainless steel ball (diameter 5 mm) for stirring were simultaneously filled into the cylindrical barrel of a liquid-type pen (Uni-Bosca PC-1M: Mitsubishi Pencil Co., Ltd.) in which the valve is released by pressing the pen tip, and the paint flows out onto the pen tip. The paints were then assembled to produce a marking pen including a pen tip ground into a chisel shape. Using this marking pen, an area of ​​2 cm square on the workpiece was painted over by writing vertically in one direction, and the formed coating film (before drying) was visually evaluated for unevenness of the coating.

[0142] Coating ability 1 and Spreadability The evaluation criteria for both are as follows: ◎: No uneven coating (thickness unevenness) was observed 〇: A small amount of uneven paint was observed ×: Uneven coating was observed in many areas

[0143] (3-4) Dripping property The dripping property of the paint is determined by the spray coating method. Coating The coating was evaluated by observing dripping from the coated object. As in (3-3-1) above, each paint was poured into the air spray used in (3-2) above, and sprayed toward the outer surface of the object to be coated for 10 seconds from a distance of 10 cm from the tip of the airbrush, and then the dripping of the droplets adhering to the object to be coated was evaluated. The evaluation criteria were as follows:

[0144] ○: No dripping occurred even when the coated object was placed vertically after application. △: When the coated object was placed vertically after application, the liquid gradually started to drip. ×: When the coated object was placed vertically after coating, the liquid immediately started dripping.

[0145] [Film evaluation] (3-5) Characteristics -Glossiness- The glossiness (60° specular glossiness) of the surfaces of both films 1 and 2 formed on each coated object with respect to the measurement light having an incident angle of 60° was measured at nine points using a glossmeter (VG 7000: Nippon Denshoku Industries Co., Ltd.) according to the method conforming to JIS Z8741, and the average value was regarded as the glossiness. The evaluation criteria are as follows.

[0146] ◎: Glossiness is less than 0.5% (extremely low gloss) Excellent ) 〇: Glossiness is 0.5% or more and less than 0.7% (low glossiness) Excellent ) △: Glossiness is 0.7% or more and less than 1.0% (low glossiness) Good ) ×: Glossiness is 1.0% or more (insufficient low glossiness)

[0147] -Reflectance- The reflectance of the surfaces of both films 1 and 2 formed on each substrate to light with a wavelength of 550 nm (550 nm reflectance) was measured at nine points using a spectrophotometer (CM-5: Konica Minolta) in accordance with the method of JIS Z8722, and the average value was taken as the reflectance. The evaluation criteria were as follows:

[0148] ◎: Reflectance is less than 1.0 (extremely low reflectance) Excellent ) ○: Reflectance is 1.0% or more and less than 1.25% (low reflectivity Excellent ) △: Reflectance is 1.25% or more and less than 1.5% (low reflectivity) Good ) ×: Reflectance is 1.5% or more (insufficient low reflectivity)

[0149] -Blackness- The blackness of the surfaces of both films 1 and 2 formed on each substrate was evaluated by measuring the lightness L* value of the film surface in the CIE 1976 L*a*b* (CIELAB) color system according to the SCE method. The lightness L* value was measured using a spectrophotometer (CM-5: Konica Minolta) in accordance with a method conforming to JIS Z8781-4:2013. The evaluation criteria are as follows: In the measurements, the CIE standard illuminant D65 was used as the light source, and the viewing angle was set to 10°, and the L* value was obtained using the SCE method with CIELAB display colors. CIE standard illuminant D65 is specified in JIS Z 8720 (2000) "Illuminates (standard light) and standard illuminants for color measurement", and the same specification is also found in ISO 10526 (2007). CIE standard illuminant D65 is used when displaying the color of an object illuminated by daylight. The viewing angle of 10° is specified in JIS Z 8723 (2009) "Method for visual comparison of surface colors", and the same specification is also found in ISO / DIS 3668.

[0150] ◎: L value is less than 10 (extremely dark) Excellent ) 〇: L value is 10 or more and less than 12 (blackness is Excellent ) △: L value is 12 or more and less than 15 (blackness is Good ) ×: L value is 15 or more (insufficient blackness)

[0151] -Light blocking property- The light-shielding properties of the films 1 and 2 formed on each of the substrates were evaluated by calculating the optical density of the films. The optical density of the films 1 and 2 formed on each of the substrates was measured using an optical densitometer (X-rite 361T (orthofilter): Nippon Daiichi Life Sciences Co., Ltd.) edition machine Material A vertical transmitted light beam was irradiated onto the film side of the coated object using a spectrophotometer (manufactured by the company), and the ratio to the state without the film was calculated and expressed in log (logarithm). An optical density of 6.0 or more is the upper detection limit for the measurement. The evaluation criteria are as follows. Note that this evaluation is based on the assumption that the coated object itself is transparent and that the film formed on it is required to have light-blocking properties. If the film is not required to have light-blocking properties, the evaluation here does not affect the overall evaluation.

[0152] ◎: Optical density is 3.2 or more (extremely light-shielding) Excellent ) 〇: Optical density is 2.5 or more and less than 3.0 (light blocking ability Excellent ) △: Optical density is 2.0 or more and less than 2.5 (light blocking ability Good ) ×: Optical density is less than 2.0 (insufficient light blocking properties)

[0153] -Adhesion- The adhesion of both films 1 and 2 formed on each substrate to the substrate surface was evaluated by making checkerboard-shaped cuts in the film with a commercially available cutter knife, attaching cellophane tape (Cellotape, Nichiban Co., Ltd.) to the cuts, and then peeling it off, and visually checking the remaining state of the film. The evaluation criteria are as follows.

[0154] ◎: 100% of the film remains (very good adhesion) Excellent ) 〇: Film remaining is 95% or more but less than 100% (adhesion is poor) Excellent ) △: Film remaining is 90% or more but less than 95% (adhesion is poor) Good ) ×: Less than 90% of the film remains (insufficient adhesion)

[0155] -comprehensive evaluation- The glossiness, reflectance, blackness, and adhesion were evaluated comprehensively according to the following criteria. As mentioned above, light-shielding ability is not included in the overall evaluation because it may or may not be necessary.

[0156] ◎: Glossiness, reflectance, blackness, and adhesion are all excellent. ◯: At least one of the evaluations of gloss, reflectance, blackness, and adhesion is ◯, and none of them is × ×: At least one of the evaluations of gloss, reflectance, blackness, and adhesion was ×

[0157] [Table 1]

[0158] [Table 2]

[0159] [Table 3]

[0160] 4. Discussion As shown in Table 1, when one or more of (A1) and (A2) were not included as (A) in the composition contained in the paint (Experimental Examples 1 to 3), one or more of the film properties, gloss, reflectance, L value, and adhesion, could not be satisfied. On the other hand, even when both (A1) and (A2) were included in the composition as (A) (Experimental Examples 4 to 10), the film property of adhesion could not be satisfied if the mass ratio of the resin solid content of (A2) to the resin solid content of (A1):1 was less than 1.8 (Experimental Example 4) or exceeded 4.4 (Experimental Example 10). Even when both (A1) and (A2) were included and the mass ratio range of the resin solid content of (A2) to the resin solid content of (A1):1 was appropriate (1.8 or more and 4.4 or less) (Experimental Examples 6, 11 to 17), if (B) did not contain (B1) having a particle size within a predetermined range (Experimental Examples 11 to 13), or if (B) contained (B1) having a particle size within a predetermined range, then one or more of the film properties, gloss, reflectance, L value, and adhesion, could not be satisfied if the mass ratio of (B) to the resin solid content of (A1):1 was less than 1.3 (Experimental Example 14) or exceeded 4.0 (Experimental Example 17). In contrast, when the mass ratio range of the resin solid content of (A2) to the resin solid content of (A1):1 was appropriate (1.8 or more and 4.4 or less) and the mass ratio of the resin solid content of (B) to the resin solid content of (A1):1 was also appropriate (1.3 or more and 4.0 or less) (Experimental Examples 5 to 9, 15, and 16), all of the paint properties and film properties were able to be satisfied.

[0161] As shown in Table 2, even when both (A1) and (A2) were included in the composition contained in the paint as (A) (Experimental Examples 4a to 10a), if the mass ratio of the resin solid content of (A2) to the resin solid content of (A1):1 was less than 1.8 (Experimental Example 4a) or more than 4.4 (Experimental Example 10a), the film properties and adhesion could not be satisfied. Even when both (A1) and (A2) were included and the mass ratio range of the resin solid content of (A2) to the resin solid content of (A1):1 was appropriate (1.8 or more and 4.4 or less) (Experimental Examples 6a, 11a to 17a), if (B) did not contain (B1) having a particle size within a predetermined range (Experimental Examples 11a to 13a), or if (B) contained (B1) having a particle size within a predetermined range, then when the mass ratio of (B) to the resin solid content of (A1):1 was less than 1.3 (Experimental Example 14a) or exceeded 4.0 (Experimental Example 17a), one or more of the film properties, gloss, reflectance, L value, and adhesion, could not be satisfied. In contrast, when the mass ratio range of the resin solid content of (A2) to the resin solid content of (A1):1 was appropriate (1.8 or more and 4.4 or less) and the mass ratio of (B) to the resin solid content of (A1):1 was also appropriate (1.3 or more and 4.0 or less) (Experimental Examples 5a to 9a, 15a, and 16a), all of the coating properties and film properties were able to be satisfied.

[0162] As shown in Table 3, when the amounts of (B) and (A) were fixed and the ratio of (A1) to (A2) in (A) was varied (Experimental Examples 6, 18 to 23), it was confirmed that as the ratio of the resin solid content of (A2) to the resin solid content of (A1) increased, the film properties of gloss and reflectance were maintained at high performance while the L value and, although not essential, the light blocking property improved. The haze values ​​in Table 3 are the haze values ​​of a film (thickness 12 μm) obtained by forming a film from a mixture (excluding (B)) in which (A1a) and (A2a) were mixed at the mass ratio (resin solid content equivalent) shown in Table 3, and were measured using a haze meter (NDH4000: Nippon Denshoku) in the same manner as above, in accordance with JIS K7136. industry The values ​​were measured using a meter (company name: TEL).

Claims

1. An aqueous resin composition for paint, comprising: Contains at least (A) and (B), (A) contains a mixture of a plurality of mutually incompatible water-dispersed resins, and one of the water-dispersed resins in the mixture is a mixture with one or more other water-dispersed resins, and the haze value of the film formed after film formation increases with an increase in the blending amount of the water-dispersed resin, (B) contains 90 mass% or more of (B1) having a particle size of 2 μm or more and 4 μm or less, and the mass ratio of (B) to the resin solid content:1 of (A) is 1.3 or more and 4.0 or less. (A) Film-forming resin component (B) Black material (B1) Composite of black pigment and resin

2. An aqueous resin composition for paint, comprising: Contains at least (A) and (B), (A) contains 90 mass% or more of (A1) and (A2), and the mass ratio of the resin solid content of (A2) to the resin solid content of (A1) is 1.8 or more and 4.4 or less; (B) contains 90 mass% or more of (B1) having a particle size of 2 μm or more and 4 μm or less, and the mass ratio of (B) to the resin solid content:1 of (A) is 1.3 or more and 4.0 or less. (A) Film-forming resin component (A1) Acrylic resin emulsion (A2) Polyester resin emulsion (B) Black material (B1) Composite of black pigment and resin

3. The composition according to claim 1 or 2, wherein (B1) contains acrylic resin particles containing carbon black.

4. The composition according to claim 2 or 3, wherein (A) further contains (A3), and the mass ratio of (A3) to the resin solid content:1 of (A1) is 1.2 or more and 1.7 or less. (A3) Water-soluble polymer

5. A coating material comprising the composition according to any one of claims 1 to 4 and (C), and having a viscosity of 1 mPa·s or more and 300 mPa·s or less at 25°C as measured by a B-type viscometer. (C) Dilution Solvent

6. 6. A coating material according to claim 5 for coating model parts.

7. The coating material according to claim 5, which is used for coating camera parts.

8. 6. The coating material according to claim 5, which is intended for application by a spray coating method and has a viscosity at 25° C. as measured by a Brookfield viscometer of 1 mPa·s or more and 50 mPa·s or less.

9. 6. A pen-type applicator filled with the paint according to claim 5, the paint having a viscosity of 80 mPa·s or more and 230 mPa·s or less at 25° C. as measured by a Brookfield viscometer.

10. A film formed from the paint according to claim 5, wherein the outermost surface on which the film is formed has a glossiness for incident light at an incident angle of 60° of less than 1.0%, a reflectance for light with a wavelength of 550 nm of less than 1.5%, and an L value in the CIELAB color system according to the SCE method of less than 15.

11. The film according to claim 10, wherein the outermost surface on which the film is formed has an optical density of 2.0 or more when the film is required to have light-shielding properties in transmission.

Citation Information

Patent Citations

  • JP1974017896A

  • Coating material for forming dot pattern and method for forming coating film

    JP2001240807A

  • Water-based ink erasable with eraser

    JP2003268284A

  • Printing plate material, thermosensitive recording material and method for forming image in thermosensitive recording material

    JP2004122526A

  • Black composite powder particle and preparation method of the same, and coating material and resin composition using the same

    JP2004300350A