Positive electrode active material for sodium ion batteries

The development of the Na0.5-yCu0.5-zTi0.5O2 active material for sodium ion batteries addresses capacity loss issues by stabilizing performance through specific synthesis and cycling methods, resulting in enhanced cycle durability and capacity retention.

JP7555335B2Active Publication Date: 2024-09-24RENAULT SA +3
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2021519643
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2018-10-11
Filing Date
2019-10-10
Publication Date
2024-09-24
Estimated Expiration
2039-10-10

AI Technical Summary

Technical Problem

Existing positive electrode materials for sodium ion batteries face issues with capacity loss during charge and discharge cycles, particularly in polyanionic compounds like Na3V2(PO4)2F3 due to toxic vanadium presence and high molecular mass, and layered oxides like NaNi0.5Mn0.5O2 experiencing capacity degradation over cycles.

Method used

A new positive electrode active material formula Na0.5-yCu0.5-zTi0.5O2 is developed, where x varies from 0.9 to 1, y from 0.05 to 0.1, and z from 0.1 to 0.3, prepared by mixing transition metal oxides with sodium carbonate and heating to 800-1000°C, incorporating a conductive compound like carbon black, and using specific charge-discharge cycling methods.

Benefits of technology

The new material exhibits improved capacity stability and reduced deterioration over multiple cycles, maintaining higher capacity and linear voltage profiles, enhancing the performance of sodium ion batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007555335000004
    Figure 0007555335000004
  • Figure 0007555335000005
    Figure 0007555335000005
  • Figure 0007555335000008
    Figure 0007555335000008
Patent Text Reader

Abstract

The present invention relates to a compound of formula (I): Na x Ni 0.5-y Cu y Mn 0.5-z Ti z O2(I), wherein: - x varies from 0.9 to 1; - y varies from 0.05 to 0.1; - z varies from 0.1 to 0.3, it being understood that when z is equal to 0.1 and x is equal to 1, then y is not equal to 0.05.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to the general field of rechargeable sodium-ion (Na-ion) batteries.

[0002] The invention more precisely relates to a positive electrode active material for Na-ion batteries and a positive electrode comprising same.

[0003] The present invention also relates to a method for cycling a Na-ion battery. [Background technology]

[0004] Na-ion batteries represent one of the most promising alternatives to lithium-ion batteries, with sodium attracting more interest than lithium from an economic point of view, especially due to its abundance and its low cost.

[0005] However, the Na-ion battery cell assembly can currently only be considered as a prototype since it has only been tested.

[0006] Positive electrodes for Na-ion batteries have been extensively studied, leading to their classification into two main categories.

[0007] The first category contains polyanion compounds. Among these polyanion compounds, the compound Na3V2(PO4)2F3 was found to be possibly suitable for use in Na-ion batteries. Indeed, as described in document WO2014 / 009710, it is characterized as easy to synthesize and stable, especially when used in high humidity conditions or at high specific energies. However, the presence of vanadium in the electrodes can cause problems during the use of Na-ion batteries in the medium / long term, resulting in its toxic nature. Moreover, even if better results are obtained with this polyanion compound, the latter specific capacity is limited due to its relatively high molecular mass.

[0008] The second category includes the layered oxides of sodium. These particular oxides have the general formula Na b MO2 (where b is equal to or less than 1 and M represents at least one transition metal). These layered oxides are considered more promising than polyanionic compounds, in particular because they have a lower molecular mass. Furthermore, the gravimetric energy density of the layered oxides of sodium is greater than that of the compound Na3V2(PO4)2F3 (approximately 4.5 g / cm 3 For approximately 3g / cm 3 ).

[0009] Thus, much research has been done on layered oxides of sodium.

[0010] Certain substances have been found to have certain advantages. 1-x Ni 0.5 Mn 0.5 As described in "O2 for a rechargeable sodium ion battery", S. Komaba, N. Yabuuchi, T. Nakayama, A. Ogata, T. Ishikawa, I. Nakai, J. Inorg Chem. 51, 6211-6220 (2012), the material NaNi 0.5 Mn 0.5 O2 has a theoretical capacity of approximately 240 mAh / g, but the capacity of this material is found to decrease over the charge-discharge cycling of a Na-ion battery.

[0011] There is therefore a need to develop new positive electrode active materials for sodium ion batteries that can overcome the problem of capacity fading.

[0012] It has been discovered that certain positive electrode active materials can provide improved capacity that does not degrade with repeated charge / discharge cycles. Summary of the Invention

[0013] Thus, the object of the present invention is to provide a compound of formula (I): Na x Ni 0.5-y Cu y Mn 0.5-z Ti z O2(I) [In the formula, - x goes from 0.9 to 1; - y increases and decreases from 0.05 to 0.1; - z increases and decreases from 0.1 to 0.3, If z is equal to 0.1 and x is equal to 1, then y is understood to be not equal to 0.05. The positive electrode active material for a sodium ion battery has the following structure:

[0014] Another object of the invention is a method for preparing the active material according to the invention.

[0015] A subject of the invention is also a positive electrode comprising an active material according to the invention.

[0016] Another object of the invention is a Na-ion battery cell comprising an electrode according to the invention.

[0017] The invention also relates to a Na-ion battery comprising at least one cell according to the invention.

[0018] Finally, the present invention also relates to a specific charge / discharge cycling method for a Na-ion battery containing a specific positive electrode active material.

[0019] Other advantages and features of the present invention will become more apparent upon consideration of the detailed description and the accompanying drawings. [Brief description of the drawings]

[0020] [Figure 1] 1 is a graph showing the capacity of a Na-ion battery cell as a function of the number of charge / discharge cycles. [Diagram 2] 1 is a graph showing the voltage of a Na-ion battery cell as a function of capacity. [Diagram 3]1 is a graph showing the capacity of a Na-ion battery cell as a function of the number of charge / discharge cycles. [Figure 4] 1 is a graph showing the voltage of a Na-ion battery cell as a function of capacity. [Diagram 5] 1 is a graph showing the voltage of a Na-ion battery cell as a function of capacity. [Figure 6] 1 is a graph showing the voltage of a Na-ion battery cell as a function of capacity. [Figure 7] 1 is a graph showing the voltage of a Na-ion battery cell as a function of capacity. [Figure 8] 1 is a graph showing voltage of a half-cell of a Na-ion battery as a function of capacity. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0021] It is specified that the expression "from to" used in the present description of the invention must be understood as including each of the endpoints referred to.

[0022] The positive electrode active material for a Na-ion battery according to the present invention satisfies the above-mentioned formula (I).

[0023] Preferably, y varies from 0.06 to 0.1, and more preferably, y is equal to 0.1.

[0024] Advantageously, z varies from 0.2 to 0.3.

[0025] According to one particular embodiment of the invention, x varies from 0.95 to 1, and preferably x is equal to 1.

[0026] An object of the present invention is a method for preparing an active material according to the invention, comprising the following steps: (a) mixing at least one compound selected from oxides and / or salts of transition metals with at least one precursor selected from sodium carbonate, sodium nitrate, sodium acetate, sodium sulfate, caustic soda, and Na2O, and mixtures thereof; (b) heating the mixture obtained after step (a) to a temperature in the range of 800-1000°C; (c) recovering said material. The present invention is also a method including the steps of:

[0027] Preferably, the compound is selected from oxides.

[0028] Preferably, the oxide is selected from NiO, CuO, Mn2O3, MnO2, TiO2, and mixtures thereof.

[0029] Advantageously, the precursor is sodium carbonate. Thus, preferably, an oxide chosen from NiO, CuO, Mn2O3, MnO2, TiO2, and mixtures thereof is mixed with sodium carbonate.

[0030] According to one preferred embodiment, the mixture obtained after step (a) is heated to a temperature in the range of 850-950°C.

[0031] Preferably, step (b) occurs over a period of time in the range of from 6 hours to 20 hours, preferably in the range of from 9 hours to 15 hours, more preferably in the range of from 11 to 13 hours, particularly preferably over a period of 12 hours.

[0032] Advantageously, step (b) is followed by a cooling step and a drying step.

[0033] For example, the mixture may be heated in an oven to 900° C. for 12 hours, then cooled to 300° C., and then removed from the oven.

[0034] Another object of the invention is a positive electrode comprising an active material according to the invention.

[0035] Preferably, the positive electrode according to the present invention further comprises at least one conductive compound.

[0036] According to one particular embodiment, the conductive compound is selected from metal particles, carbon, and mixtures thereof, preferably carbon.

[0037] The metal particles may be silver, copper, or nickel particles.

[0038] The carbon may be in the form of graphite, carbon black, carbon fibers, carbon nanowires, carbon nanotubes, carbon nanospheres, preferably in the form of carbon black.

[0039] In particular, the positive electrode according to the invention advantageously comprises the carbon black SuperC65® sold by Timcal.

[0040] Preferably, the content of the active material according to the invention varies from 50% to 90% by weight, preferably from 70% to 90% by weight, relative to the total weight of the positive electrode.

[0041] Advantageously, the content of conductive compounds varies from 10% to 50% by weight, preferably from 10% to 30% by weight, and even more preferably from 15% to 25% by weight, relative to the total weight of the positive electrode.

[0042] The present invention also relates to a Na-ion battery cell comprising a positive electrode, a negative electrode, a separator, and an electrolyte, which comprise an active material according to the present invention.

[0043] Preferably, the battery cell includes a separator located between the electrodes and acting as an electrical insulator. Several materials can be used as the separator. Separators are generally made of porous polymers, preferably polyethylene and / or polypropylene. They may also be made of glass microfibers.

[0044] Advantageously, the separator used is a glass microfiber separator sold by Whatman, CAT No. 1823-070®.

[0045] Preferably, the electrolyte is a liquid.

[0046] The electrolyte can include one or more sodium salts and one or more solvents.

[0047] The sodium salt(s) may be selected from NaPF6, NaClO4, NaBF4, NaTFSI, NaFSI, and NaODFB.

[0048] The sodium salt(s) are preferably dissolved in one or more solvents selected from aprotic polar solvents, such as ethylene carbonate, propylene carbonate, dimethyl carbonate, diethyl carbonate, and methyl carbonate and ethyl carbonate.

[0049] Advantageously, the electrolyte comprises propylene carbonate in a mixture with the sodium salt NaPF6 at 1M.

[0050] The subject of the invention is also a Na-ion battery comprising at least one cell as previously described.

[0051] The present invention relates to a negative electrode, a separator, an electrolyte, and a cathode comprising the following formula (II): Na p Ni 0.5-r Cu r Mn 0.5-t Ti t O2(II) [In the formula, - p increases or decreases from 0.9 to 1; - r increases or decreases from 0.05 to 0.1; - t increases or decreases from 0.1 to 0.3] 1. A method for cycling a sodium ion battery comprising a positive electrode comprising an active material having using multiple charge / discharge cycles at a voltage ranging from an upper voltage limit to a lower voltage limit, the upper voltage limit being in the range of 4.2V to 4.7V, preferably in the range of 4.4V to 4.6V, more preferably equal to 4.5V, and the lower voltage limit being in the range of 0.5V to 2.5V, preferably in the range of 1.5V to 2.5V, more preferably equal to 2V; The cycles are performed at cycling rates ranging from C / 20 to C, where C indicates the cycling rate of the sodium-ion battery; It also relates to methods.

[0052] The use of an upper voltage limit of 4.2 to 4.7 in the method of cycling a Na-ion battery results in a more protective solid stable layer, called the positive electrode electrolyte interphase (CEI), relative to the use of a lower upper voltage limit, e.g., less than 4.1 V. This CEI, located between the positive electrode and the electrolyte, is a key element for the proper operation of a Na-ion battery, since it not only conducts the sodium ions very well, but also has the advantage of stopping the catalytic decomposition of the electrolyte.

[0053] Advantageously, the active material having formula (II) has formula (I).

[0054] Preferably, the cycling rate is C / 10.

[0055] The invention is illustrated, but not limited to, by the following examples. EXAMPLES

[0056] Example 1 I. Electrochemical Cell Fabrication 1.Synthesis of active material 1.1 Active material NaNi 0.5 Mn 0.5 Synthesis of O2 73.45 mg NiO3, 434.7 mg MnO2, and 529.95 mg sodium carbonate are added. The temperature is brought up to 850° C. at a rate of 3° C. per minute, and then the whole is calcined in an oven at 850° C. for 12 hours. The mixture is then cooled down to 300° C. at a rate of 1° C. per minute. This comparative active material is called material A.

[0057] 1.2 Active material NaNi 0.5 Mn 0.4 Ti 0.1 Synthesis of O2 73.45 mg NiO3, 315.74 mg Mn2O3, 79.87 mg TiO2, and 529.95 mg sodium carbonate are added. The temperature is brought up to 900° C. at a rate of 3° C. per minute, and then the whole is calcined in an oven at 900° C. for 12 hours. The mixture is then cooled down to 300° C. at a rate of 1° C. per minute. This comparative active material is called material B.

[0058] 1.3 Active material NaNi 0.44 Cu 0.06 Mn 0.4 Ti 0.1 Synthesis of O2 28.64 mg NiO3, 47.73 mg CuO, 315.74 mg Mn2O3, 79.87 mg TiO2 and 529.95 mg sodium carbonate are added. The temperature is brought up to 900°C at a rate of 3°C per minute and then the whole is calcined in an oven at 900°C for 12 hours. The mixture is then cooled down to 300°C at a rate of 1°C per minute. This active material according to the invention is called material C.

[0059] 1.4 Active material NaNi 0.4 Cu 0.1 Mn 0.4 Ti 0.1 Synthesis of O2 86.76 mg NiO2, 79.55 mg CuO, 315.74 mg Mn2O3, 79.87 mg TiO2 and 529.95 mg sodium carbonate are added. The temperature is brought up to 900°C at a rate of 3°C per minute and then the whole is calcined in an oven at 900°C for 12 hours. The mixture is then cooled down to 300°C at a rate of 1°C per minute. This active material according to the invention is called material D.

[0060] 1.5 Active material NaNi 0.45 Cu 0.05 Mn 0.3 Ti 0.2 Synthesis of O2 45.11 mg NiO3, 9.78 mg CuO3, 36.81 mg Mn2O32, 159.74 mg TiO2 and 529.95 mg sodium carbonate are added. The temperature is brought up to 900°C at a rate of 3°C per minute and then the whole is calcined in an oven at 900°C for 12 hours. The mixture is then cooled down to 300°C at a rate of 1°C per minute. This active material according to the invention is called material E.

[0061] 1.6 Active material NaNi 0.45 Cu 0.05 Mn 0.2 Ti 0.3 Synthesis of O2 45.11 mg NiO3, 9.78 mg CuO3, 157.87 mg Mn2O3, 39.61 mg TiO2 and 529.95 mg sodium carbonate are added. The temperature is brought up to 900° C. at a rate of 3° C. per minute, then the whole is calcined in an oven at 900° C. for 12 hours. The mixture is then cooled down to 300° C. at a rate of 1° C. per minute. This active material according to the invention is called material F.

[0062] 2. Preparation of Positive Electrode These materials were used to prepare six positive electrodes, designated EN-A, EN-B, EN-C, EN-D, EN-E, and EN-F, respectively. The positive electrodes EN-A and EN-B are reference electrodes. The electrodes EN-C to EN-F are electrodes according to the invention.

[0063] The positive electrode EN-A is prepared by mixing 80% by weight of active material A, which is transferred directly from the oven into the glove box without exposure to air, and 20% by weight of carbon black Super C65®, and then grinding the mixture for 30 minutes using a SPEX8000M mixer.

[0064] The other positive electrodes EN-B to EN-F are prepared by mixing 80% by weight of active materials B to F, respectively, and 20% by weight of carbon black Super C65®, and then grinding the mixture in the same manner as for the positive electrode EN-A. As in the case of active material A, active materials B to F are transferred directly from the oven to the glove box without exposure to air.

[0065] 3. Electrochemical Cell Assembly Six electrochemical cells were then fabricated, each containing a positive electrode EN-A to EN-F, and designated CE-A, CE-B, CE-C, CE-D, CE-E, and CE-F, respectively.

[0066] The assembly of the electrochemical cells is carried out in a glove box with the device consisting of button cells of type 2032. Each of the cells includes a separator, a negative electrode, and an electrolyte.

[0067] 3.1 Assembly of cell CE-A Positive electrode Then, electrode EN-A, in powder form and with a mass of 8.13 mg, is spread over an aluminium sheet placed in cell CE-A.

[0068] Separator To avoid any short circuit between the positive and negative electrodes during the charge-discharge cycle, two layers of separators made of glass microfiber, CAT No. 1823-070®, are used, which are cut according to a diameter of 16.6 mm and a thickness of 400 μm.

[0069] negative electrode 1cm 2 The electrodes are obtained by inserting a hard carbon coated disk into the aluminum current collector film. The active mass of hard carbon is approximately 5.20 mg / cm. 2 It is.

[0070] electrolyte The electrolyte used comprises a solution of 1M NaPF6 dissolved in propylene carbonate.

[0071] 3.2 Assembly of cell CE-B to cell CE-F Positive electrode Then, electrodes EN-B to EN-F in powder form with masses of 8.50 mg, 9.35 mg, 9.36 mg, 9.35 mg, and 8.75 mg, respectively, are spread over an aluminum sheet placed in cells CE-B to CE-F, respectively.

[0072] The separator, negative electrode, and electrolyte are the same as those used in cell CE-A.

[0073] II. Electrochemical Testing 1. Comparison cell CE-A Galvanostatic cycling was performed at a cycling rate of C / 20 (C denotes the capacity of the cell) using a BioLogic cycler at voltages ranging from 4.2 V to 1.5 V. The capacity of cell CE-A was measured as a function of cycle number, as shown in Figure 1. The increase and decrease in capacity are observed in curve A.

[0074] Therefore, a degradation of capacity can be observed with charge-discharge cycling. Approximately 130 mAh.g -1 The capacity was measured after 30 cycles.

[0075] 2. Comparison cell CE-B Galvanostatic cycling was performed at a cycling rate of C / 20 using a BioLogic cycler at voltages ranging from 4.4 V to 1.2 V, where C denotes the capacity of the cell. The voltage of cell CE-B was measured as a function of capacity, as shown in FIG. 2.

[0076] In this figure, curve B1 corresponds to the first charge / discharge cycle, curve B2 corresponds to the second charge / discharge cycle, and so on up to curve B5 which corresponds to the fifth charge / discharge cycle.

[0077] A very clear shoulder is observed in the region ranging from approximately 3.6 V to 3.8 V. Several plateaus corresponding to the process of phase transition can be observed in these curves B1 to B5.

[0078] Therefore, the degradation of the capacity of cell CE-B can be observed.

[0079] 3. Cell CE-C according to the present invention Galvanostatic cycling was performed at a cycling rate of C / 20 using a BioLogic cycler at voltages ranging from 4.4 V to 1.2 V. C denotes the cell capacity. The capacity of cell CE-C was measured as a function of cycle number, as shown in Figure 3. The increase and decrease in capacity are observed in curve C.

[0080] Therefore, approximately 170mAh.g -1 The capacity was measured after 20 cycles.

[0081] Compared to the capacity of the comparative cell CE-A observed in FIG. 1, the capacity of the cell CE-C according to the invention is larger and more stable over charge-discharge cycles.

[0082] Thus, the capacity of cells containing the active material according to the invention is improved.

[0083] Additionally, the voltage of cell CE-C was measured as a function of capacity, as shown in FIG.

[0084] In this FIG. 4, curve C1 corresponds to the first charge / discharge cycle, and so on up to curve C5, which corresponds to the fifth charge / discharge cycle.

[0085] Curves C1 to C5 are more linear than curves B1 to B5.

[0086] Therefore, the degradation of the capacity of cell CE-C is not observed as in the case of cell CE-B, and in fact the capacity of cell CE-C is more stable.

[0087] 4. Cell CE-D according to the present invention Galvanostatic cycling was performed at a cycling rate of C / 20 using a BioLogic cycler at voltages ranging from 4.4 V to 1.2 V, where C denotes the capacity of the cell. The voltage of cell CE-D was measured as a function of capacity, as shown in FIG. 5.

[0088] In this FIG. 5, curve D1 corresponds to the first charge / discharge cycle, and so on up to curve D5, which corresponds to the fifth charge / discharge cycle.

[0089] Curves D1 to D5 are more linear than curves B1 to B5.

[0090] Therefore, the degradation of the capacity of cell CE-D is not observed as in the case of cell CE-B, and in fact the capacity of cell CE-D is more stable.

[0091] 5. Cell CE-E according to the present invention Galvanostatic cycling was performed at a cycling rate of C / 20 using a BioLogic cycler at voltages ranging from 4.4 V to 1.2 V, where C denotes the capacity of the cell. The voltage of cells CE-E was measured as a function of capacity, as shown in FIG. 6.

[0092] In this FIG. 6, curve E1 corresponds to the first charge / discharge cycle, and so on up to curve E5, which corresponds to the fifth charge / discharge cycle.

[0093] Curves E1 to E5 are more linear than curves B1 to B5.

[0094] Therefore, the degradation of the capacity of cell CE-E is not observed as in the case of cell CE-B, and in fact the capacity of cell CE-E is more stable.

[0095] 6. Cell CE-F according to the present invention Galvanostatic cycling was performed at a cycling rate of C / 20 using a BioLogic cycler at voltages ranging from 4.4 V to 1.2 V, where C denotes the capacity of the cell. The voltage of cell CE-F was measured as a function of capacity, as shown in FIG. 7.

[0096] In this FIG. 7, curve F1 corresponds to the first charge / discharge cycle, and so on up to curve F5, which corresponds to the fifth charge / discharge cycle.

[0097] Curves F1 to F5 are more linear than curves B1 to B5.

[0098] Therefore, the degradation of the capacity of cell CE-F is not observed as in the case of cell CE-B, and in fact the capacity of cell CE-F is more stable.

[0099] Example 2 I. Fabrication of Electrochemical Half-Cell 1.Active material NaNi 0.45 Cu 0.05 Mn 0.4 Ti 0.1 Synthesis of O2 45.11 mg NiO3, 9.78 mg CuO3, 315.74 mg Mn2O3, 79.87 mg TiO2, and 529.95 mg sodium carbonate are added. The temperature is allowed to reach 900°C at a rate of 3°C per minute, and then the whole is calcined in an oven at 900°C for 12 hours. The mixture is then cooled to 300°C at a rate of 1°C per minute.

[0100] 2. Preparation of Positive Electrode The positive electrode is transferred directly from the oven to the glove box without exposure to air. The active material is NaNi 0.45 Cu 0.05 Mn 0.4 Ti 0.1 It is prepared by mixing 80% by weight of O2 and 20% by weight of carbon black Super C65®, and then grinding the mixture for 30 minutes using a SPEX 8000M mixer.

[0101] 3. Assembly of the Electrochemical Half-cell Next, a half cell containing the above positive electrode was prepared.

[0102] The assembly of the half-cell is carried out in a glove box using a device consisting of a Swagelok® connector with a diameter of 12 mm. The half-cell contains a separator, a negative electrode, and an electrolyte.

[0103] Positive electrode A mass of 10 mg of the positive electrode in powder form is spread over an aluminium piston placed in the half-cell.

[0104] Separator To avoid any short circuit between the positive and negative electrodes during the charge-discharge cycle, two layers of separators made of glass microfiber, CAT No. 1823-070®, are used, which are cut according to a diameter of 12 mm and a thickness of 500 μm.

[0105] negative electrode A pad with a diameter of 11 mm is cut from a sheet of metallic sodium. The resulting pad is pressure bonded to a stainless steel current collector. This current collector is then deposited on the separator membrane of the cell.

[0106] electrolyte The electrolyte used comprises a solution of 1M NaPF6 dissolved in propylene carbonate.

[0107] II. Electrochemical Testing A cycling method involving the use of multiple charge-discharge cycles at voltages ranging from 2 V to 4.5 V was carried out at a cycling rate of C / 10.

[0108] The voltage of the half-cell was measured as a function of capacity, as shown in FIG.

[0109] In this FIG. 8, curve G indicates a number of charge-discharge cycles that were carried out.

[0110] Therefore, the capacity of the half-cell is stable over repeated charge-discharge cycles.

Claims

1. The following formula (I) Na x Ni 0.5-y Cu y Mn 0.5-z Ti z O 2 (I) [In the formula, x increases and decreases from 0.9 to 1; y increases and decreases from 0.05 to 0.1; z increases and decreases from 0.1 to 0.3, If z is equal to 0.1 and x is equal to 1, then it is understood that y is not equal to 0.

05. A positive electrode active material for a sodium ion battery comprising:

2. 2. The material of claim 1, wherein y varies from 0.06 to 0.

1.

3. 3. A material according to claim 1 or 2, characterized in that z increases or decreases from 0.2 to 0.

3.

4. 4. A material according to any one of claims 1 to 3, characterised in that x varies from 0.95 to 1.

5. A method for producing the active material according to any one of claims 1 to 4, comprising the steps of: (a) At least one compound selected from oxides and / or salts of transition metals is dissolved in a solvent such as sodium carbonate, sodium nitrate, sodium acetate, sodium sulfate, caustic soda, and Na 2 with at least one precursor selected from O, and mixtures thereof; (b) heating the mixture obtained after step (a) to a temperature in the range of 800 to 1000° C.; (c) recovering the active material A method comprising:

6. A positive electrode comprising at least one active material according to any one of claims 1 to 4.

7. 7. The positive electrode of claim 6, further comprising at least one conductive compound.

8. 8. The positive electrode of claim 7, wherein the conductive compound is selected from metal particles, carbon, and mixtures thereof.

9. 9. The positive electrode according to claim 8, characterized in that the carbon is present in the form of graphite, carbon black, carbon fibers, carbon nanowires, carbon nanotubes or carbon nanospheres.

10. A sodium ion battery cell comprising the positive electrode of any one of claims 6 to 9, a negative electrode, a separator, and an electrolyte.

11. A sodium-ion battery comprising at least one cell according to claim 10.

12. A negative electrode, a separator, an electrolyte, and a polymer having the following formula (II): Na p Ni 0.5-r Cu r Mn 0.5-t Ti t O 2 (II) [In the formula, p increases and decreases from 0.9 to 1; r increases and decreases from 0.05 to 0.1; t increases or decreases from 0.1 to 0.

3.

1. A method for cycling a sodium ion battery comprising a positive electrode comprising an active material having using multiple charge / discharge cycles at a voltage ranging from an upper limit voltage to a lower limit voltage, the upper limit voltage being in the range of 4.2V to 4.7V and the lower limit voltage being in the range of 0.5V to 2.5V; The method, wherein the cycles are performed at cycling rates ranging from C / 20 to C, where C indicates the cycling rate of the sodium ion battery.

Citation Information

Patent Citations

  • Doped nickelate compounds

    JP2015530960A

  • Layered copper-containing oxide materials, their preparation processes, and their uses

    JP2016537294A

  • Cathode active material for sodium ion batteries