Semiconductor device, power conversion device, and method for manufacturing the same
By incorporating a metal film with higher hardness than the wire and maintaining an average crystal grain size of 5 μm or less, the semiconductor device enhances durability and extends its reliable life through effective crack management.
Patent Information
- Application Number
- JP2022578443
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-01-28
- Filing Date
- 2022-01-26
- Publication Date
- 2024-09-24
- Estimated Expiration
- 2042-01-26
Smart Images

Figure 0007555435000017 
Figure 0007555435000011 
Figure 0007555435000025
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a semiconductor device, a power conversion device, and a method for manufacturing a semiconductor device. [Background technology]
[0002] Conventionally, a semiconductor module equipped with a semiconductor element such as a power semiconductor element is known. The power semiconductor element is a semiconductor element for generating electric power. An electrode is disposed on the semiconductor element. The electrode is made of, for example, aluminum (Al). A wiring member such as a wire is bonded to the electrode. The wiring member electrically connects a plurality of semiconductor elements to each other. The wiring member also electrically connects the semiconductor element to a circuit pattern. For example, a semiconductor device described in Japanese Patent No. 6132014 (Patent Document 1) includes a semiconductor element, a metal film, and a wire. The metal film covers the electrode of the semiconductor element. The metal film has a higher hardness than the wire. The wire is bonded to the metal film. The bonding interface of the wire contains only crystal grains having a grain size of 15 μm or less. A portion of the wire away from the bonding interface contains crystals having a grain size larger than 15 μm. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Patent No. 6132014 Summary of the Invention [Problem to be solved by the invention]
[0004] As semiconductor devices such as semiconductor modules become smaller and denser, the current density of the current flowing through the wires increases. This causes a problem that the guaranteed reliability life of the bonded semiconductor element and wire is more limited than before. The life of the bonded portion of the bonded semiconductor element and wire is evaluated, for example, by a power cycle test.
[0005] The present disclosure has been made in view of the above-mentioned problems, and has an object to provide a semiconductor device, a power conversion device, and a method for manufacturing a semiconductor device that have a longer reliable life span than conventional devices. [Means for solving the problem]
[0006] The semiconductor device of the present disclosure includes a semiconductor element, a metal film, and a wire. The semiconductor element includes an electrode. The metal film covers the electrode of the semiconductor element. The wire is bonded to the metal film. The metal film has a higher hardness than the wire. The inside of the wire has a bond with the metal film. Throughout the wire, the average crystal grain size in a circular cross section of the wire is 5 μm or less. The wire diameter is 300 μm or more and 500 μm or less. The grain size at the joint is smaller than the average grain size in the circular cross section of the wire. Effect of the Invention
[0007] According to the semiconductor device of the present disclosure, the average crystal grain size in the circular cross section of the wire is 5 μm or less throughout the entire wire, which improves the power cycle resistance of the semiconductor device and provides a longer reliable lifespan than conventional devices. [Brief description of the drawings]
[0008] [Figure 1] 1 is a cross-sectional view illustrating a schematic configuration of a semiconductor device according to a first embodiment. [Diagram 2] 1 is a cross-sectional view roughly showing a configuration of a semiconductor device according to a first modification of the first embodiment. [Diagram 3] 11 is a cross-sectional view roughly showing a configuration of a semiconductor device according to a second modification of the first embodiment. FIG. [Figure 4] FIG. 2 is an enlarged view of region IV in FIG. [Diagram 5] 2 is an enlarged view that roughly illustrates the crystals of the wires of the semiconductor device according to the first embodiment, and corresponds to region IV in FIG. 1. [Figure 6] 3 is a flowchart illustrating an outline of a method for manufacturing a semiconductor device according to the first embodiment. [Figure 7]5 is a cross-sectional view corresponding to FIG. 4 and illustrating a schematic view of a crack occurring in the semiconductor device according to the first embodiment. [Figure 8] 6 is a cross-sectional view corresponding to FIG. 5 and illustrating a schematic view of a crack occurring in the semiconductor device according to the first embodiment. [Figure 9] 1 is a cross-sectional view illustrating a semiconductor device and a crack according to a first comparative example. [Figure 10] 1 is a graph showing the relationship between the average crystal grain size and the power cycle life. [Figure 11] FIG. 11 is a cross-sectional view illustrating a semiconductor device and a crack according to a second comparative example. [Figure 12] FIG. 11 is a cross-sectional view illustrating a semiconductor device and a crack according to a third comparative example. [Figure 13] FIG. 13 is a cross-sectional view illustrating a semiconductor device and a crack according to a fourth comparative example. [Figure 14] 11 is a cross-sectional view illustrating a schematic configuration of a crystal of a wire in a semiconductor device according to a second embodiment. FIG. [Figure 15] 11 is a crystal orientation map that roughly illustrates crystals of a wire of a first structure of a semiconductor device according to an embodiment before a power cycle test. [Figure 16] 13 is a crystal orientation map that roughly illustrates crystals of a wire of a second structure of the semiconductor device according to the embodiment before a power cycle test. [Figure 17] 11 is a crystal orientation map that roughly illustrates crystals of wires in the semiconductor device according to the first comparative example before a power cycle test. [Figure 18] 11 is a crystal orientation map that roughly illustrates crystals of a wire of a first structure of the semiconductor device according to the embodiment after a power cycle test. [Figure 19] 11 is a first cross-sectional photograph that roughly shows crystals and cracks in a wire of a first structure of a semiconductor device according to an embodiment after a power cycle test. [Figure 20] 13 is a second cross-sectional photograph that roughly illustrates crystals and cracks in the wire of the first structure of the semiconductor device according to the embodiment after a power cycle test. [Figure 21]13 is a third cross-sectional photograph that roughly illustrates crystals and cracks in the wire of the first structure of the semiconductor device according to the embodiment after a power cycle test. [Figure 22] 13 is a crystal orientation map that roughly illustrates crystals of a wire of a second structure of the semiconductor device according to the embodiment after a power cycle test. [Figure 23] 13 is a crystal orientation map that roughly illustrates crystals of a wire of the semiconductor device according to the first comparative example after a power cycle test. [Figure 24] 11 is a cross-sectional photograph that illustrates schematic crystals and cracks in the wire of the semiconductor device according to the first comparative example after a power cycle test. [Diagram 25] FIG. 25 is an enlarged view of area XXV of FIG. 24. [Figure 26] FIG. 11 is a block diagram illustrating a schematic configuration of a power conversion device according to a third embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] Hereinafter, an embodiment will be described with reference to the drawings. In the following, the same or corresponding parts are denoted by the same reference characters, and overlapping descriptions will not be repeated.
[0010] Embodiment 1 The configuration of a semiconductor device 100 according to the first embodiment will be described with reference to FIGS.
[0011] 1, the semiconductor device 100 includes a semiconductor element 1, a metal film 2, and a wire 3. The semiconductor device 100 may further include a circuit pattern 41, a metal pattern 42, an insulating member 43, a heat dissipation member 5, a first bonding material 61, a second bonding material 62, a case 7, a terminal 8, and a sealing material 9.
[0012] In this embodiment, the semiconductor element 1 is a power semiconductor element. A power semiconductor element may be called a power semiconductor element. The semiconductor element 1 is, for example, a metal oxide semiconductor field effect transistor (MOSFET), an insulated gate bipolar transistor (IGBT), or the like.
[0013] The semiconductor element 1 includes an electrode 11. The electrode 11 is, for example, an aluminum (Al)-silicon (Si) electrode. In this embodiment, the electrode 11 has a hardness lower than that of the wire 3 and the metal film 2. In this embodiment, the hardness may be, for example, the Vickers hardness defined in JIS B 7725 or the Rockwell hardness defined in JIS G 0202. The semiconductor element 1 according to this embodiment further includes a back electrode 12 and a substrate portion 13. The back electrode 12 and the electrode 11 sandwich the substrate portion 13. The substrate portion 13 is, for example, a silicon (Si) substrate, a silicon carbide (SiC) substrate, a gallium nitride (GaN) substrate, or the like.
[0014] In this embodiment, the semiconductor element 1 includes a first element portion 1a and a second element portion 1b. The first element portion 1a and the second element portion 1b are arranged with a gap therebetween. In this embodiment, the direction in which the first element portion 1a and the second element portion 1b are arranged is a first direction DR1. The direction in which the electrode 11 is superimposed on the substrate portion 13 is a second direction DR2. The first direction DR1 and the second direction DR2 intersect. In this embodiment, the first direction DR1 and the second direction DR2 are perpendicular to each other.
[0015] The metal film 2 covers the electrodes 11 of the semiconductor element 1. The metal film 2 is disposed on the opposite side of the electrodes 11 from the substrate portion 13. The metal film 2 has a higher hardness than the wires 3. The detailed configuration of the metal film 2, such as the material thereof, will be described later.
[0016] In this embodiment, the metal film 2 includes a first metal film portion 2a and a second metal film portion 2b. The first metal film portion 2a covers the electrode 11 of the first element portion 1a. The second metal film portion 2b covers the electrode 11 of the second element portion 1b.
[0017] The wire 3 is, for example, a wire made of aluminum (Al). The wire 3 is bonded to the metal film 2. The wire 3 is bonded to the terminal 8 and the circuit pattern 41. The wire 3 is provided with a first end E1, a second end E2, and a bent portion B. The first end E1 of the wire 3 is bonded to the metal film 2. The second end E2 of the wire 3 is bonded to the terminal 8. The bent portion B is provided between the first end E1 and the second end E2. The bent portion B is bent. The bent portion B is bonded to either the metal film 2 or the circuit pattern 41.
[0018] In this embodiment, the wire 3 includes a first wire portion 3a and a second wire portion 3b. The first end E1, the second end E2, the first bent portion B1, and the second bent portion B2 of the first wire portion 3a are respectively joined to the terminal 8, the second metal film portion 2b, the circuit pattern 41, and the first metal film portion 2a. The first end E1, the second end E2, and the bent portion B3 of the second wire portion 3b are respectively joined to the second metal film portion 2b, the terminal 8, and the circuit pattern 41.
[0019] The wire diameter of the wire 3 is, for example, 100 μm or more and 500 μm or less. When a current flows through the wire 3, the larger the wire diameter of the wire 3, the less heat is generated by the wire 3. For this reason, it is desirable that the wire diameter of the wire 3 is, for example, 400 μm or more and 500 μm or less. Furthermore, when the wire diameter of the wire 3 is thick, the heat generated by the wire 3 is reduced, and therefore the wires 3 can be highly integrated. Furthermore, when the wire diameter of the wire 3 is thick, the number of wires 3 is reduced, and therefore the time required for wiring the wires 3 can be shortened.
[0020] The average crystal grain size in the circular cross section of the wire 3 is 5 μm or less throughout the entire wire 3. In this embodiment, the crystal grain size of the wire 3 is evaluated by electron backscatter diffraction (EBSD). The crystal grain size of the wire 3 is evaluated based on the grain boundary between adjacent crystals. The grain boundary between adjacent crystals is defined as a boundary where the crystal orientation of adjacent crystals is shifted by 5° or more. The average crystal grain size of the entire wire 3 is evaluated based on a crystal orientation map in a circular cross section of the wire 3 having a diameter equal to the wire diameter of the wire. The strict average crystal grain size is calculated by averaging the crystal grain sizes of multiple crystals measured by an analysis method capable of observing crystal grains, such as cross-sectional SIM (Scanning Ion Microscope) observation. The detailed structure of the crystal of the wire 3 will be described later.
[0021] It is known that the smaller the crystal grain size, the greater the yield strength of the metal, according to the Hall-Petch relationship. Therefore, the smaller the average crystal grain size of the wire 3, the greater the strength and hardness of the wire 3. If the hardness of the wire 3 is greater than that of the metal film 2, when a crack occurs in the wire 3, the crack will progress into the metal film 2, resulting in a short life and resulting in lift-off, which will be described later. The crack that progresses into the metal film 2 may further progress into the electrode 11, resulting in an unexpectedly short life. In contrast, in the present disclosure, the hardness of the wire 3 is made smaller than that of the metal film 2, so that when a crack occurs in the wire 3, the crack will progress only into the wire 3. The wire 3 has a small crystal grain size as described above, which has the effect of suppressing the speed of crack progression and improving the power cycle life. This effect will be described in detail in paragraphs 0094 to 0097.
[0022] The semiconductor element 1 is bonded to the circuit pattern 41. Specifically, the back electrode 12 of the semiconductor element 1 is bonded to the circuit pattern 41 by a first bonding material 61. The first bonding material 61 is, for example, solder, silver (Ag), or the like. The circuit pattern 41 and the metal pattern 42 sandwich an insulating member 43. Each of the circuit pattern 41 and the metal pattern 42 is provided on the insulating member 43. The metal pattern 42 is bonded to the heat dissipation member 5 by a second bonding material 62. The insulating member 43 is configured as an insulating substrate.
[0023] The case 7 surrounds the semiconductor element 1, the metal film 2, the wire 3, the circuit pattern 41, the metal pattern 42, the insulating member 43, the first bonding material 61, the second bonding material 62, and the sealing material 9. The case 7 has an internal space. The internal space contains the semiconductor element 1, the metal film 2, the wire 3, the circuit pattern 41, the metal pattern 42, the insulating member 43, the first bonding material 61, the second bonding material 62, and the sealing material 9. The case 7 is bonded to the side and upper surface of the heat dissipation member 5. The lower surface of the heat dissipation member 5 is exposed from the case 7. Although not shown, the case 7 has a ring shape surrounding the heat dissipation member 5 when viewed from below.
[0024] A terminal 8 is disposed in the case 7. A first end of the terminal 8 is disposed in the internal space of the case 7. The first end of the terminal 8 is exposed from the case 7 in the internal space of the case 7. A second end of the terminal 8 is disposed in an area outside the case 7. The second end of the terminal 8 protrudes from the case 7.
[0025] The terminal 8 includes a first terminal terminal 81 and a second terminal terminal 82. The first terminal terminal 81 is connected to the first wire portion 3a. The second terminal terminal 82 is connected to the second wire portion 3b. Each of the first terminal terminal 81 and the second terminal terminal 82 may be configured as a main terminal or as a power supply terminal.
[0026] The internal space of the case 7 is filled with a sealing material 9. The sealing material 9 seals the semiconductor element 1, the metal film 2, the wires 3, the circuit pattern 41, the metal pattern 42, the insulating member 43, the first bonding material 61, and the second bonding material 62 in the internal space. The sealing material 9 may be a gel-like sealing resin or a molded resin.
[0027] As shown in Fig. 2, the semiconductor device 100 may further include a lead frame LF. When the semiconductor device 100 includes the lead frame LF, the semiconductor device 100 may not include the case 7. The lead frame LF is joined to the insulating member 43. Although the lead frame LF and the insulating member 43 are in contact with each other in Fig. 2, a metal plate (not shown) may be disposed between the lead frame LF and the insulating member 43.
[0028] The lead frame LF is partially sealed with a sealing material 9. An end of the lead frame LF protrudes outside the sealing material 9. The end of the lead frame LF is configured as a terminal 8 for connection to an external device of the semiconductor device 100.
[0029] The lead frame LF forms an electric circuit. A first end E1 of the wire 3 is joined to the semiconductor element 1. A second end E2 of the wire 3 is joined to the lead frame LF. The semiconductor element 1 joined to the wire 3 can be connected to an external device of the semiconductor device 100 via the wire 3 and the lead frame LF.
[0030] When the semiconductor device 100 includes a lead frame LF, the heat dissipation member 5 may be a metal layer, and the insulating member 43 may be an insulating sheet. The insulating sheet is laminated on the metal layer. The insulating sheet is fixed to the metal layer. The insulating sheet may have an uncured insulating resin layer.
[0031] 3, the metal film 2 disposed on the electrode 11 may be formed only on the portion where the wire 3 is connected to the metal film 2. In other words, the metal film 2 may cover only a portion of the electrode 11.
[0032] Next, the configuration of the semiconductor element 1, the metal film 2, and the wires 3 of the semiconductor device 100 according to the first embodiment will be described in detail with reference to Figures 4 and 5. Figure 4 is an enlarged view of region IV in Figure 1. For ease of explanation, the sealing material 9 (see Figure 1) is not shown in the enlarged views of Figures 4 and 5. Similarly to Figures 4 and 5, the sealing material (see Figure 1) is not shown in Figures 7 to 9 and Figures 11 to 14 described later.
[0033] As shown in FIG. 4 and FIG. 5, the wire 3 is directly bonded to the metal film 2. The wire 3 is bonded to the metal film 2 by ultrasonic bonding, for example. Therefore, the wire 3 is provided with a bonded portion 31 with the metal film 2. In this embodiment, the bonded portion 31 of the wire 3 refers to a range from the bonded interface BI of the wire 3 with the metal film 2 to a position that has advanced into the wire 3 by the average crystal grain size of the wire 3. The bonded portion 31 is provided along the first direction DR1. In this embodiment, since the average crystal grain size is 5 μm or less, the bonded portion 31 of the wire 3 refers to a range from the bonded interface BI of the wire 3 with the metal film 2 to a position that has advanced, for example, 5 μm or less into the wire 3. In addition, for example, when the average crystal grain size of the wire 3 is 10 μm, the bonded portion 31 of the wire 3 refers to a range from the bonded interface BI of the wire 3 with the metal film 2 to a position that has advanced, for example, 10 μm into the wire 3. Although not shown, the metal film 2 may include multiple film portions and multiple undercoat films. The film portions and the base films are alternately laminated, which improves the adhesion of the metal film 2. In this case, the film portions are bonded to the wires 3.
[0034] 5, the wire 3 includes a plurality of crystals 30. In this embodiment, the crystals 30 of the wire 3 are finely divided.
[0035] Preferably, the metal film 2 may be either a nickel (Ni) film or a copper (Cu) film. When the metal film 2 is a nickel (Ni) plating film, the thickness of the metal film 2 is preferably 3 μm or more and 5 μm or less. When the thickness of the nickel (Ni) plating film is less than 3 μm, the nickel (Ni) plating film may be damaged when the wire 3 is joined to the nickel (Ni) plating film. When the thickness of the nickel (Ni) plating film is more than 5 μm, it takes time to form the nickel (Ni) plating film, which is economically disadvantageous.
[0036] Also, preferably, the metal film 2 may be an electroless nickel (Ni)-phosphorus (P) plating film that does not contain sulfur (S). In this case, the phosphorus (P) content of the metal film 2 is 8 mass % or less.
[0037] Also, preferably, the metal film 2 may be an electroless nickel (Ni)-boron (B) plating film.
[0038] Also, preferably, the metal film 2 may be either a nickel (Ni) film or a copper (Cu) film formed by electroplating.
[0039] Also, preferably, the metal film 2 may be any one of a nickel (Ni) film, a copper (Cu) film, a titanium (Ti) film, and a tungsten (W) film formed by either a vapor deposition method or a sputtering method.
[0040] 1, when the semiconductor element 1 has a plurality of element portions such as a first element portion 1a and a second element portion 1b, a separate metal film portion is formed on each of the plurality of element portions. In this case, the metal film 2 is desirably formed by plating such as electroless plating and electroplating.
[0041] Next, a manufacturing method of the semiconductor device 100 according to the first embodiment will be described with reference to FIGS.
[0042] As shown in FIG. 6, the method for manufacturing the semiconductor device 100 includes a preparation step S101 and a bonding step S102.
[0043] 1, in preparation step S101 (see FIG. 6), a semiconductor element 1, a metal film 2, and a wire 3 are prepared. In this embodiment, a circuit pattern 41, a metal pattern 42, an insulating member 43, a heat dissipation member 5, a bonding material (first bonding material 61), a second bonding material 62, a case 7, a terminal 8, and a sealing material 9 are further prepared.
[0044] The electrode 11 is covered with the metal film 2. The electrode 11 may be covered with the metal film 2 by being plated by electroplating. Alternatively, the electrode 11 may be covered with the metal film 2 by being plated by electroless plating.
[0045] Next, in a bonding step S102 (see FIG. 6), the wire 3 is bonded to the metal film 2 covering the electrode 11. In the present embodiment, the wire 3 is bonded to the metal film 2 by ultrasonic bonding. The method for bonding the wire 3 and the metal film 2 may be determined appropriately.
[0046] Furthermore, the first bonding material 61 is heated, thereby bonding the semiconductor element 1 and the circuit pattern 41 together. In this embodiment, the semiconductor element 1 is bonded to the circuit pattern 41 via a bonding material (first bonding material 61) heated to 270° C. or higher. The second bonding material 62 is heated, thereby bonding the metal pattern 42 and the heat dissipation member 5 together. Furthermore, the sealing material 9 seals the internal space formed by the case 7 surrounding the semiconductor element 1, the metal film 2, the wires 3, etc., and the upper surface of the heat dissipation member 5.
[0047] Also, as shown in FIG. 2, when the semiconductor device 100 includes a lead frame LF, in the bonding step S102 (see FIG. 6), an insulating member 43, which is an insulating sheet in an uncured state, is placed in a molding die (not shown). Also, the lower surface of the metal pattern 42, which is a metal layer, is placed so as to be in surface contact with the bottom surface of the cavity of the molding die. Then, the lead frame LF is placed so as to be in surface contact with the insulating sheet in an uncured state. Then, pressure is applied to the insulating sheet via the lead frame LF. Also, with the pressure applied, a sealing material 9, which is a molding resin, is injected into the cavity of the molding die. Then, after the molding resin has filled the entire cavity, the application of pressure is stopped. Then, the molding resin and the insulating sheet in an uncured state are cured.
[0048] Next, a power cycle test for evaluating the life of the semiconductor device 100 according to the first embodiment will be described with reference to Figures 7 and 8. In this embodiment, the life of the semiconductor device 100 refers to a power cycle life evaluated by a power cycle test.
[0049] In the power cycle test, an ON state in which a current flows through the semiconductor element 1 and an OFF state in which no current flows through the semiconductor element 1 are alternately and repeatedly switched. As a result, the semiconductor element 1 is alternately and repeatedly switched between a state in which it is heated by a current and a state in which it is naturally cooled. As a result, stress is repeatedly generated in the joints 31 between the components of the semiconductor device 100 according to the difference in linear expansion coefficient between the components. In other words, the power cycle test is a fatigue test in which small deformations due to stress are repeatedly applied to the evaluation object. As a result, cracks CR may occur in the semiconductor device 100 being evaluated, as shown in Figs. 7 and 8.
[0050] When the sealing material 9 (see FIG. 1) is a gel-like sealing resin, the crack CR caused by the power cycle test propagates along the joint 31 between the wire 3 and the metal film 2. That is, the crack CR propagates mainly along the first direction DR1. Note that the propagated crack CR causes the wire 3 to separate (lift off) from the electrode 11, resulting in failure of the semiconductor device 100. The crack CR tends to propagate through portions with low strength and hardness. The crack CR also tends to propagate in the joint 31. Specifically, the crack CR tends to propagate toward crystals with large grain sizes.
[0051] Next, the effects of this embodiment will be described. 5, in the semiconductor device 100 according to the first embodiment, the average crystal grain size in the circular cross section of the wire 3 is 5 μm or less throughout the entire wire 3. This extends the life of the wire 3. Thus, the semiconductor device 100 has a long life.
[0052] The semiconductor device 100 according to the present embodiment will be compared with a semiconductor device 101 (see FIG. 9) according to a first comparative example, and the effects of the semiconductor device 100 according to the present embodiment will be described in detail.
[0053] As shown in Fig. 5, the average crystal grain size of the wires 3 of the semiconductor device 100 according to the present embodiment is 5 µm or less. In contrast, as shown in Fig. 9, the average crystal grain size of the wires 3 of the semiconductor device 101 according to the first comparative example is greater than 7 µm.
[0054] The lifetimes of the semiconductor device 100 according to the present embodiment and the semiconductor device 101 according to the first comparative example were evaluated by a power cycle test. The test conditions for the power cycle test according to the present embodiment are as follows. The current value and the time for which the current flows were determined so that the junction temperature of the semiconductor element 1 in the on state was 100° C. higher than in the off state. When the voltage between the emitter and collector of the semiconductor element 1 became 5% higher than the value before the test, the semiconductor device 100 was determined to have failed.
[0055] 8 shows a state in which a crack CR generated by a power cycle test propagates inside the wire 3 of the semiconductor device 100 according to this embodiment. When the wire 3 is joined to the semiconductor element 1 by ultrasonic bonding, the wire 3 is plastically deformed. This causes the crystals in the joint 31 of the wire 3 to become finer.
[0056] The crack CR propagates inside the wire 3. In this embodiment, the crystals of the joint 31 and the crystals at a position away from the joint 31 are finely divided. Therefore, the crack CR is suppressed from propagating from the crystals of the joint 31 toward the crystals at a position away from the joint 31. Therefore, the crack CR propagates along the joint 31 between the wire 3 and the metal film 2. Also, since the crystals at a position away from the joint 31 are finely divided, even if the crack CR propagates toward the crystals at a position away from the joint 31, the propagation speed of the crack CR is small. Therefore, the power cycle life is extended. That is, the life of the semiconductor device 100 is extended.
[0057] FIG. 9 shows how the crack CR generated by the power cycle test has progressed inside the wire 3 of the semiconductor device 101 according to this embodiment. The crack CR progresses inside the wire 3. The crystals at a position away from the joint 31 have lower strength and hardness than the finely refined crystals of the joint 31. Therefore, the crack CR progresses inside the wire 3 from the crystals of the joint 31 toward the crystals at a position away from the joint 31. Therefore, in the first comparative example, even if the crystals of the joint 31 are finely refined, the power cycle life is not sufficiently improved. In addition, the deformation amount of the wire 3 plastically deformed in the first comparative example is larger than the deformation amount of the wire 3 plastically deformed in the first embodiment. This is because the wire 3 according to this embodiment is joined to the metal film 2 in a state where the crystals of the wire 3 are finely refined, whereas the wire 3 according to the first comparative example is joined to the metal film 2 in a state where the crystals of the wire 3 are not finely refined.
[0058] 10 is a graph showing the relationship between the average crystal grain size of the wire 3 and the power cycle life when a power cycle test is performed on the semiconductor device 100 according to the present embodiment and the semiconductor device 101 according to the first comparative example. The vertical axis shows the power cycle life. The horizontal axis shows the average crystal grain size of the wire 3.
[0059] When the average crystal grain size of the wire 3 of the semiconductor device 100 according to the present embodiment is 2.7 μm, the power cycle life is 278,400 times. When the average crystal grain size of the wire 3 of the semiconductor device 100 according to the present embodiment is 5 μm, the power cycle life is 104,900 times.
[0060] When the average crystal grain size of the wire 3 of the semiconductor device 101 according to the first comparative example is 7.1 μm, the power cycle life is 40100 times. When the average crystal grain size of the wire 3 of the semiconductor device 101 according to the first comparative example is 9.3 μm, the power cycle life is 60500 times. When the average crystal grain size of the wire 3 of the semiconductor device 101 according to the first comparative example is 10.6 μm, the power cycle life is 59600 times. When the average crystal grain size of the wire 3 of the semiconductor device 101 according to the first comparative example is 13.9 μm, the power cycle life is 77300 times. When the average crystal grain size of the wire 3 of the semiconductor device 101 according to the first comparative example is 14.9 μm, the power cycle life is 77600 times. When the average crystal grain size of the wire 3 of the semiconductor device 101 according to the first comparative example is 35.8 μm, the power cycle life is 33900 times.
[0061] That is, the power cycle life of the semiconductor device 100 according to the present embodiment was approximately eight times longer than that of the semiconductor device 101 according to the first comparative example.
[0062] From the above, compared to the semiconductor device 101 of the first comparative example having wire 3 with an average crystal grain size larger than 7 μm, the semiconductor device 100 of this embodiment having wire 3 with an average crystal grain size of 5 μm or less clearly showed a different tendency, and a significant increase in power cycle life was observed.
[0063] Note that, this time, the experimental results were shown for a case where the conditions were set so that the junction temperature of semiconductor element 1 was 100°C higher in the on state than in the off state. However, even when the difference in the junction temperature of semiconductor element 1 between the on state and the off state was smaller than 100°C, for example, when the conditions were set so that the junction temperature of semiconductor element 1 was 80°C higher in the on state than in the off state, it was confirmed that the power cycle life was significantly increased in the region where the average crystal grain size was 5 μm or less.
[0064] Next, the semiconductor device 100 according to the present embodiment will be compared with a semiconductor device 102 according to a second comparative example (see FIG. 11) and a semiconductor device 103 according to a third comparative example (see FIG. 12) to describe in detail the action and effect of the semiconductor device 100 according to the present embodiment.
[0065] 5, the semiconductor device 100 according to the present embodiment includes a metal film 2. Moreover, the average crystal grain size of the wire 3 as a whole is 5 μm or less.
[0066] In contrast, as shown in FIG. 11, the semiconductor device 102 according to the second comparative example does not include the metal film 2. The average crystal grain size of the wire 3 of the semiconductor device 102 according to the second comparative example is greater than 7 μm. The wire 3 according to the second comparative example contains, for example, high-purity aluminum (Al). The aluminum (Al) content of the wire 3 according to the second comparative example is, for example, 99.99 mass % or more. The wire 3 of the semiconductor device 102 according to the second comparative example has a lower hardness than the electrode 11. Therefore, the crack CR generated in the semiconductor device 102 according to the second comparative example propagates inside the wire 3. Specifically, the crack CR propagates along the joint portion 31 inside the wire 3. Furthermore, since the average crystal grain size of the wire 3 is large, the propagation speed of the crack CR is high. Therefore, the power cycle life of the semiconductor device 102 according to the second comparative example is short.
[0067] In addition, as shown in FIG. 12, the semiconductor device 103 according to the third comparative example does not include the metal film 2, unlike the semiconductor device 100 according to the present embodiment. The average crystal grain size of the wire 3 of the semiconductor device 103 according to the third comparative example is 5 μm or less. The wire 3 of the semiconductor device 103 according to the third comparative example has a higher hardness than the electrode 11. Therefore, the crack CR generated in the semiconductor device 103 according to the third comparative example propagates inside the electrode 11. When the crack CR propagates inside the electrode 11, the chip structure of the semiconductor element 1 may be destroyed by the crack CR. Therefore, the power cycle life of the semiconductor device 103 according to the third comparative example is short.
[0068] From the above, the power cycle life of the semiconductor device 100 of this embodiment, which includes a metal film 2 and a wire 3 having an average crystal grain size of 5 μm or less, is longer than that of the semiconductor device 102 of the second comparative example and the semiconductor device 103 of the third comparative example, which do not include the metal film 2.
[0069] Next, the effect of the metal film 2 will be described. As shown in FIG. 4 and FIG. 5, when the life of the joint 31 between the wire 3 and the metal film 2 is long, it is desirable that the life of other components of the semiconductor device 100 is long. Specifically, as shown in FIG. 1, it is desirable that the life of the first bonding material 61 is long. The life of the first bonding material 61 is improved by improving the heat resistance of the first bonding material 61. By improving the heat resistance of the first bonding material 61, the heat resistance of the joint 31 (see FIG. 5) between the semiconductor element 1 and the circuit pattern 41 is improved. Specifically, the first bonding material 61 is preferably a high-temperature solder. Examples of the high-temperature solder include lead (Pb)-based solder, tin (Sn)-antimony (Sb)-based solder, gold (Au)-based solder, bismuth (Bi)-based solder, copper (Cu)-based solder, and zinc (Zn)-based solder. When the high-temperature solder melts, the liquidus temperature of the high-temperature solder is high. The liquidus temperature of the high-temperature solder is, for example, 270°C. Therefore, when the metal film 2 is a nickel (Ni) film formed by electroless plating and contains amorphous matter, as in the semiconductor device 104 according to the fourth comparative example shown in FIG. 13, the volume of the metal film 2 is reduced by crystallization. This may cause the metal film 2 to crack. As shown in FIG. 13, when the metal film 2 cracks, a crack CR may progress through the crack in the metal film 2 into the electrode 11. For example, when the metal film 2 contains phosphorus (P), the metal film 2 contains amorphous matter. When the content of phosphorus (P) is large, the metal film 2 has a single amorphous phase. Also, when the content of phosphorus (P) is small, the metal phase has a crystalline structure containing microcrystals.
[0070] According to the semiconductor device 100 of this embodiment, the metal film 2 may be an electroless nickel (Ni)-phosphorus (P) plating film that does not contain sulfur (S). In this case, the phosphorus (P) content of the metal film 2 is 5 mass % or less. When the phosphorus (P) content is 5 mass % or less, the metal phase has a crystalline structure. Therefore, it is possible to suppress metal cracking caused by amorphous. In addition, since it does not contain sulfur (S), it is possible to suppress segregation of sulfur (S) at grain boundaries during heat treatment. This makes it possible to suppress embrittlement of the grain boundaries, and therefore it is possible to suppress cracking of the metal film 2 during heat treatment. As a result, the heat resistance of the metal film 2 is improved. Therefore, for example, even if the temperature exceeds 270° C. during the manufacture of the semiconductor device 100, it is possible to suppress cracking of the metal film 2.
[0071] The metal film 2 may be an electroless nickel (Ni)-boron (B) plating film. In this case, the metal film 2 has a crystalline structure. Furthermore, the purity of nickel (Ni) contained in the metal film 2 is high. Therefore, cracking of the metal film 2 during heat treatment can be suppressed.
[0072] The metal film 2 may be either a nickel (Ni) film or a copper (Cu) film formed by electroplating. In this case, the metal film 2 has a crystalline structure. Furthermore, the purity of the nickel (Ni) contained in the metal film 2 is high. Therefore, cracking of the metal film 2 during heat treatment can be suppressed.
[0073] The metal film 2 may be any one of a nickel (Ni) film, a copper (Cu) film, and a tungsten (W) film formed by either a vapor deposition method or a sputtering method. In this case, the metal film 2 has a crystalline structure. Furthermore, the purity of the nickel (Ni) contained in the metal film 2 is high. Therefore, cracking of the metal film 2 during heat treatment can be suppressed.
[0074] 5, in the bonding step S102 (see FIG. 6), the wire 3 is bonded to the metal film 2. The average crystal grain size in the circular cross section of the wire 3 is 5 μm or less throughout the entire wire 3. This extends the life of the semiconductor device 100.
[0075] The semiconductor element 1 is bonded to the circuit pattern 41 via a bonding material (first bonding material 61) heated to 270°C or higher. For this reason, a bonding material (first bonding material 61) having high heat resistance can be used as a bonding material for bonding the semiconductor element 1 and the circuit pattern 41. Specifically, the semiconductor element 1 and the circuit pattern 41 can be bonded by a bonding material (first bonding material 61) having a melting point of 270°C or higher. For example, when the first bonding material 61 has a high lead (Pb) content, the melting point of the first bonding material 61 is 270°C or higher. Therefore, the heat resistance of the semiconductor device 100 is improved. For example, high heat resistance is required for the semiconductor device 100, which operates at a high temperature due to the high integration of the semiconductor element 1.
[0076] Embodiment 2 Next, the configuration of the semiconductor device 100 according to the second embodiment will be described with reference to Fig. 14. Unless otherwise specified, the second embodiment has the same configuration, manufacturing method, and effects as the first embodiment. Therefore, the same components as the first embodiment are denoted by the same reference numerals, and the description will not be repeated.
[0077] 14, the wire 3 according to the present embodiment contains iron (Fe) and aluminum (Al). The iron content of the wire 3 is 0.2 mass% or more and 2.0 mass% or less. The aluminum content of the remainder, excluding iron, of the wire 3 is 99.99 mass% or more.
[0078] Elements other than aluminum (Al) contained in the wire 3 exist either in a solid solution state in aluminum (Al) or in a precipitated state. For this reason, in this embodiment, iron (Fe) exists either in a solid solution state in aluminum (Al) or in a precipitated state. When elements other than aluminum (Al) are in a solid solution state in aluminum (Al), the electrical conductivity of the wire 3 is significantly reduced. When elements other than aluminum (Al) are precipitated from aluminum (Al), the reduction in the electrical conductivity of the wire 3 is suppressed. The maximum solid solubility limit in aluminum (Al) differs depending on the element. Also, the rate of reduction in the electrical conductivity of the wire 3 per amount of solid solution of the element differs depending on the element.
[0079] The maximum solid solubility limit of iron (Fe) in aluminum (Al) is, for example, 0.05 mass%. Therefore, even if the iron (Fe) content of the wire 3 is 0.2 mass% or more and 2.0 mass% or less, most of the iron (Fe) is precipitated. Therefore, the decrease in the electrical conductivity of the wire 3 due to the iron (Fe) is suppressed.
[0080] Preferably, the electrical conductivity of the wire 3 according to the present embodiment is 29×10 5 S / m (50% IACS) or more. More preferably, the electrical conductivity of the wire 3 is 32×10 5 S / m(55%IACS) or more.
[0081] The wire 3 according to the modified example of the second embodiment contains iron (Fe), an additive element, and aluminum. The iron and additive element contents of the wire 3 are 0.2% by mass or more and 2.0% by mass or less. The aluminum content of the wire 3 excluding the iron and additive element is 99.99% by mass or more.
[0082] The additive element is, for example, magnesium (Mg), silicon (Si), copper (Cu), nickel (Ni), zinc (Zn), chromium (Cr), manganese (Mn), titanium (Ti), zirconium (Zr), tungsten (W), etc. The additive element is an element different from iron (Fe).
[0083] Next, the effects of this embodiment will be described. According to the semiconductor device 100 of the second embodiment, as shown in FIG. 14, the wire 3 contains iron (Fe) and aluminum (Al). Therefore, the average crystal grain size of aluminum (Al) can be reduced by iron (Fe). That is, the average crystal grain size of the wire 3 can be reduced. In addition, the recrystallization temperature of the wire 3 can be increased. Specifically, the recrystallization temperature of the wire 3 becomes 175° C. or higher. This makes it possible to suppress the recrystallization of the fine crystals even if the wire 3 is heated by the current flowing through the wire 3 during the power cycle test. Therefore, it is possible to suppress the coarsening of the fine crystals. Therefore, it is possible to achieve both the promotion of the fine crystals and the suppression of the coarsening of the fine crystals.
[0084] The iron content of the wire 3 is 0.2 mass % or more and 2.0 mass % or less. The aluminum content of the remainder of the wire 3 excluding the iron is 99.99 mass % or more. Therefore, the solid solubility limit of iron (Fe) in aluminum (Al) is small. This makes it possible to suppress a decrease in the electrical conductivity of the wire 3. Therefore, the wire 3 according to this embodiment can be used even when a large current flows through the semiconductor device 100.
[0085] Next, the effect of the semiconductor device 100 according to this embodiment will be described in more detail with reference to Fig. 15 to Fig. 25. Fig. 15 is a crystal orientation map showing an evaluation of the wire 3 by electron backscatter diffraction (EBSD) before and after a power cycle test. Note that the crystal orientation map in Fig. 15 etc. is a crystal orientation map of a part of the semiconductor device 100, but for convenience of explanation, the four sides are illustrated by straight lines instead of ellipsis lines.
[0086] The effect of the semiconductor device 100 according to the present embodiment will be explained by comparing a wire 3 of a first configuration of the semiconductor device 100 according to the present embodiment (see FIG. 15), a wire 3 of a second configuration of the semiconductor device 100 according to the present embodiment (see FIG. 16), and a wire 3 according to a first comparative example (see FIG. 17).
[0087] As shown in FIG. 15, the average crystal grain size of the wire 3 of the first structure of the semiconductor device 100 according to the present embodiment is 2.7 μm. The content of elements other than aluminum (Al) in the wire 3 of the first structure is 0.4 mass %. As shown in FIG. 16, the average crystal grain size of the wire 3 of the second structure of the semiconductor device 100 according to the present embodiment is 5 μm. The content of elements other than aluminum (Al) in the wire 3 of the second structure is 1.5 mass %. As shown in FIG. 17, the average crystal grain size of the semiconductor device 101 according to the first comparative example is 35 μm.
[0088] The above-mentioned power cycle test was carried out on the wire 3 of the first configuration of the semiconductor device 100 according to the present embodiment, the wire 3 of the second configuration, and the wire 3 according to the first comparative example.
[0089] The power cycle life of the wire 3 of the first structure of the semiconductor device 100 according to the present embodiment was 277,000 times. As shown in FIG. 15, the wire 3 of the first structure of the semiconductor device 100 according to the present embodiment had a small difference between the crystal grain size at the bonding interface BI and the crystal grain size inside the bonding interface BI in the bonding portion 31 before the power cycle test. Specifically, the crystal grain size at the bonding interface BI and the crystal grain size inside the bonding interface BI in the bonding portion 31 before the power cycle test of the wire 3 of the first structure of the semiconductor device 100 according to the second embodiment were each about 1 μm. Also, as shown in FIG. 18, the crystal grain size at the bonding interface BI and the crystal grain size inside the bonding interface BI in the bonding portion 31 after the power cycle test of the wire 3 of the first structure of the semiconductor device 100 according to the present embodiment were each about 3 μm. As shown in FIGS. 19 to 21, the crack CR had progressed inside the wire 3 along the bonding portion 31 of the wire 3 with the metal film 2.
[0090] The power cycle life of the second structure of the semiconductor device 100 according to the present embodiment was 353,000 times. As shown in FIG. 16, the wire 3 of the second structure of the semiconductor device 100 according to the present embodiment had a small difference between the crystal grain size at the bonding interface BI and the crystal grain size inside the bonding interface BI in the bonding portion 31 before the power cycle test. Specifically, the crystal grain size at the bonding interface BI and the crystal grain size inside the bonding interface BI in the bonding portion 31 before the power cycle test of the wire 3 of the second structure of the semiconductor device 100 according to the second embodiment were each about 1 μm or more and 2 μm or less. Also, as shown in FIG. 22, the crystal grain size at the bonding interface BI and the crystal grain size inside the bonding interface BI in the bonding portion 31 after the power cycle test of the wire 3 of the second structure of the semiconductor device 100 according to the second embodiment were each about 3 μm.
[0091] As shown in FIG. 17, the wire 3 of the semiconductor device 101 according to the first comparative example includes a joint 31 having an average crystal grain size of about 1 μm before the power cycle test, and an internal region that is inside the wire 3 from the joint 31. The internal region had a crystal grain size of 2 μm or more and 5 μm or less. As shown in FIG. 20, the area of the joint 31 after the power cycle test was smaller than the area of the joint 31 after the power cycle test. The grain size of many crystals in the internal region was larger than 5 μm. Therefore, the wire 3 of the semiconductor device 101 according to the first comparative example was coarsened. As shown in FIG. 23, a crack CR was generated. Also, as shown in FIG. 24 and FIG. 25, the crack CR progressed inside the wire so as to move away from the metal film 2.
[0092] As described above, in the present disclosure, a wire 3 having a crystal grain size of 5 μm or less by adding alloy elements is bonded onto a metal film 2 that is harder than the wire 3, so that cracks during the power cycle test selectively propagate only within the wire 3, and coarsening of the crystal grain size of the wire 3 is suppressed during the test period, resulting in a characteristically long life.
[0093] The wires 3 contain iron (Fe), which improves the heat resistance of the wires 3. As a result, the heat resistance of the semiconductor device 100 improves.
[0094] The wire 3 contains an additive element. The additive element improves the strength, recrystallization temperature, corrosion resistance, etc. of the wire 3. For example, when the additive element is magnesium (Mg) or silicon (Si), the tensile strength of the wire 3 improves. When the additive element is zirconium (Zr), the recrystallization temperature of the wire 3 improves. When the additive element is manganese (Mn), the corrosion resistance of the wire 3 improves. Thus, the strength, recrystallization temperature, corrosion resistance, etc. of the semiconductor device 100 are improved.
[0095] In the above description, the iron or iron and additive element content of the wire 3 is 0.2% by mass or more and 2.0% by mass or less, and the aluminum content of the remainder after excluding the iron or iron and additive elements from the wire 3 is 99.99% by mass or more. However, the same effect can be obtained even if the iron or iron and additive element content of the wire 3 is 0.01% by mass or more and 2.0% by mass or less, and the aluminum content of the remainder after excluding the iron or iron and additive elements from the wire 3 is 99% by mass or more.
[0096] Embodiment 3 In this embodiment, the semiconductor device 100 according to the above-mentioned embodiments 1 and 2 is applied to a power conversion device. Although the present disclosure is not limited to a specific power conversion device, a case in which the present disclosure is applied to a three-phase inverter will be described below as embodiment 3.
[0097] FIG. 26 is a block diagram showing a configuration of a power conversion system to which the power conversion device according to this embodiment is applied.
[0098] The power conversion system shown in Fig. 26 is composed of a power source PW, a power conversion device 200, and a load L. The power source PW is a DC power source and supplies DC power to the power conversion device 200. The power source PW can be composed of various things, for example, a DC system, a solar cell, or a storage battery, or it may be composed of a rectifier circuit connected to an AC system or an AC / DC converter. The power source PW may also be composed of a DC / DC converter that converts DC power output from the DC system into a predetermined power.
[0099] The power conversion device 200 is a three-phase inverter connected between a power source PW and a load L, which converts DC power supplied from the power source PW into AC power and supplies the AC power to the load L. As shown in Fig. 26, the power conversion device 200 includes a main conversion circuit 201 that converts DC power into AC power and outputs it, and a control circuit 202 that outputs a control signal for controlling the main conversion circuit 201 to the main conversion circuit 201.
[0100] The load L is a three-phase motor driven by AC power supplied from the power conversion device 200. The load L is not limited to a specific application, but is a motor mounted on various electric devices, and is used as, for example, a motor for a hybrid car, an electric car, a railroad car, an elevator, or an air conditioner.
[0101] The power conversion device 200 will be described in detail below. The main conversion circuit 201 includes switching elements and free wheel diodes (not shown), and converts DC power supplied from the power source PW into AC power by switching the switching elements, and supplies the AC power to the load L. There are various specific circuit configurations of the main conversion circuit 201, but the main conversion circuit 201 according to this embodiment is a two-level three-phase full bridge circuit, and can be configured with six switching elements and six free wheel diodes connected in reverse parallel to each switching element. At least one of the switching elements and free wheel diodes of the main conversion circuit 201 is a switching element or free wheel diode of the semiconductor device 100 corresponding to the semiconductor device 100 of any of the above-mentioned first and second embodiments. The six switching elements are connected in series with every two switching elements to form upper and lower arms, and each upper and lower arm forms each phase (U phase, V phase, W phase) of the full bridge circuit. The output terminals of each upper and lower arm, i.e., the three output terminals of the main conversion circuit 201, are connected to the load L.
[0102] The main conversion circuit 201 also includes a drive circuit (not shown) for driving each switching element, but the drive circuit may be built into the semiconductor device 100, or the semiconductor device 100 may include a drive circuit separately. The drive circuit generates drive signals for driving the switching elements of the main conversion circuit 201 and supplies them to control electrodes of the switching elements of the main conversion circuit 201. Specifically, in accordance with a control signal from a control circuit 202 (described later), the drive signal for turning the switching element on and the drive signal for turning the switching element off are output to the electrodes 11 of the switching elements. When the switching element is to be maintained in the on state, the drive signal is a voltage signal (on signal) equal to or higher than the threshold voltage of the switching element, and when the switching element is to be maintained in the off state, the drive signal is a voltage signal (off signal) equal to or lower than the threshold voltage of the switching element.
[0103] The control circuit 202 controls the switching elements of the main conversion circuit 201 so that a desired power is supplied to the load L. Specifically, the control circuit 202 calculates the time (on time) for each switching element of the main conversion circuit 201 to be in the on state based on the power to be supplied to the load L. For example, the main conversion circuit 201 can be controlled by PWM control that modulates the on time of the switching elements according to the voltage to be output. Then, a control command (control signal) is output to a drive circuit provided in the main conversion circuit 201 so that an on signal is output to a switching element that should be in the on state at each time point, and an off signal is output to a switching element that should be in the off state. The drive circuit outputs an on signal or an off signal as a drive signal to the electrode 11 of each switching element according to this control signal.
[0104] In the power conversion device of this embodiment, the semiconductor device 100 of embodiments 1 and 2 is applied as the semiconductor device 100 that constitutes the main conversion circuit 201, so that a power conversion device 200 having a long life can be realized.
[0105] In the present embodiment, an example of applying the present disclosure to a two-level three-phase inverter has been described, but the present disclosure is not limited thereto and can be applied to various power conversion devices. In the present embodiment, a two-level power conversion device is described, but a three-level or multi-level power conversion device may be used. In addition, when power is supplied to a single-phase load, the present disclosure may be applied to a single-phase inverter. In addition, when power is supplied to a DC load or the like, the present disclosure may be applied to a DC / DC converter or an AC / DC converter.
[0106] Furthermore, the power conversion device to which the present disclosure is applied is not limited to the case where the above-mentioned load is an electric motor, but can also be used, for example, as a power supply device for an electric discharge machine, a laser processing machine, an induction heating cooker, or a non-contact power supply system, and can also be used as a power conditioner for a solar power generation system, a power storage system, etc.
[0107] The embodiments disclosed herein should be considered to be illustrative and not restrictive in all respects. The scope of the present disclosure is defined by the claims, not the above description, and is intended to include all modifications within the meaning and scope of the claims. [Explanation of symbols]
[0108] 1 semiconductor element, 2 metal film, 3 wire, 100 semiconductor device, 20 power conversion device, 201 main conversion circuit, 202 control circuit, L load, PW power supply.
Claims
1. A semiconductor element including an electrode; a metal film covering the electrodes of the semiconductor element; a wire bonded to the metal film; the metal film has a higher hardness than the wire; The inside of the wire has a joint with the metal film, The average crystal grain size in the circular cross section of the wire is 3 μm or less throughout the wire; The wire diameter is 300 μm or more and 500 μm or less, A semiconductor device, wherein the grain size of the joint is smaller than the average grain size in a circular cross section of the wire.
2. an insulating member on which the semiconductor element is mounted; a heat dissipation member disposed below the insulating member; a case that accommodates the insulating member and the heat dissipation member; a terminal disposed inside the case and to which the wire is connected; A sealant that seals an internal space of the case; The semiconductor device according to claim 1 , comprising:
3. the wire comprises iron and aluminum; The iron content of the wire is 0.01% by mass or more and 2.0% by mass or less, 3. The semiconductor device according to claim 1, wherein the aluminum content of the remainder, excluding the iron, of the wire is 99 mass % or more.
4. The wire comprises iron, an additive element, and aluminum; The content of the iron and the additive element in the wire is 0.01% by mass or more and 2.0% by mass or less, 3. The semiconductor device according to claim 1, wherein the aluminum content in the wire excluding the iron and the additive element is 99 mass % or more.
5. 5. The semiconductor device according to claim 1, wherein the metal film is either a nickel film or a copper film.
6. The metal film is a sulfur-free electroless nickel-phosphorus plating film, 5. The semiconductor device according to claim 1, wherein the metal film has a phosphorus content of 5 mass % or less.
7. 5. The semiconductor device according to claim 1, wherein the metal film is an electroless nickel-boron plating film.
8. 5. The semiconductor device according to claim 1, wherein the metal film is either a nickel film or a copper film formed by electroplating.
9. 5. The semiconductor device according to claim 1, wherein the metal film is any one of a nickel film, a copper film, a titanium film and a tungsten film formed by either a vapor deposition method or a sputtering method.
10. A circuit pattern; a bonding material disposed between the circuit pattern and the semiconductor element, 10. The semiconductor device according to claim 1, wherein the liquidus temperature of the bonding material is 270° C. or higher.
11. A main conversion circuit having the semiconductor device according to any one of claims 1 to 10, which converts input power and outputs the converted power; a control circuit that outputs a control signal for controlling the main conversion circuit to the main conversion circuit.
12. A step of preparing a semiconductor element having electrodes, a metal film covering the electrodes, and wires; forming a joint between the wire and the metal film inside the wire, the metal film has a higher hardness than the wire; a first conductive layer formed on the first metal film and a second conductive layer formed on the second metal film, the first conductive layer being connected to the first conductive layer and the second conductive layer being connected to the second conductive layer;
13. A circuit pattern and a bonding material are further provided; The method for manufacturing a semiconductor device according to claim 12, wherein the semiconductor element is bonded to the circuit pattern via a bonding material heated to 270° C. or higher.
Citation Information
Patent Citations
Multiple core optical fiber unit
JP1986032014A
Board laminated with metal, and semiconductor device
JP2000286289A
Power module
JP2014143406A
Al BONDING WIRE
JP2020059886A
Semiconductor device and method for manufacturing semiconductor device
WO2014175343A1