Thermosetting maleimide resin composition
The thermosetting maleimide resin composition addresses separation and turbidity issues by using a styrenic elastomer and maleimide compound with organic peroxide, providing stable films with superior dielectric properties and adhesion for high-frequency applications.
Patent Information
- Application Number
- JP2021183051
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-11-10
- Publication Date
- 2024-09-25
- Estimated Expiration
- 2041-11-10
AI Technical Summary
Existing resin compositions for high-frequency applications, such as those used in 5G communication, suffer from separation and turbidity issues, leading to inadequate dielectric properties and adhesion, particularly with materials like LCP and MPI, which are unsuitable for substrates.
A thermosetting maleimide resin composition comprising a styrenic elastomer with reactive functional groups, a maleimide compound, and an organic peroxide, with specific mass ratios and optional adhesion aids, ensuring compatibility and strong adhesive strength.
The composition achieves stable, varnish-like films with excellent dielectric properties and strong adhesion to both organic resins and copper, suitable for high-frequency applications.
Smart Images

Figure 0007555684000001 
Figure 0007555684000002 
Figure 0007555684000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a thermosetting maleimide resin composition, an uncured or cured resin film made of the resin composition, an adhesive, a sealing material, and a substrate containing a cured product of the thermosetting maleimide resin composition. [Background technology]
[0002] In recent years, the next-generation mobile communication system known as 5G has become popular, aiming to realize high-speed, large-capacity, low-latency communications. To realize this, materials for high-frequency bands are required, and since reducing transmission loss is essential as a noise countermeasure, there is a demand for the development of insulating materials with excellent dielectric properties (low dielectric constant and low dielectric tangent).
[0003] Among these, insulating materials with excellent dielectric properties are in demand for circuit board applications. Insulating materials with excellent dielectric properties are required for circuit boards such as rigid and flexible circuit boards, and reactive polyphenylene ether resins (PPE) are being used for rigid circuit boards, while liquid crystal polymers (LCPs) and modified polyimides (MPIs) with improved properties are being used for flexible printed circuit boards (FPCs).
[0004] When manufacturing the above FPC, an adhesive is required to attach the base film and coverlay film to the surface having the wiring portion by using a heat press, etc. Traditionally, adhesives that mainly use epoxy resins have been used, but recently there has been a demand for adhesives with excellent dielectric properties.
[0005] In light of this background, adhesives with excellent dielectric properties have been reported (for example, Patent Documents 1 to 4), but most of them are combinations of epoxy resins, other thermosetting resins, and thermoplastic resins. These compositions have excellent dielectric properties in the frequency range of 10 GHz or less, but 5G requires them to have dielectric properties in the frequency range of 28 GHz or more, known as millimeter waves, and many of the adhesives that were previously said to have excellent dielectric properties do not currently have sufficient dielectric properties.
[0006] In addition, a resin composition containing a special maleimide compound and a thermoplastic resin has been disclosed as a composition that has excellent high-frequency characteristics and also has a high level of adhesion to conductors (Patent Document 5). [Prior art documents] [Patent documents]
[0007] [Patent Document 1] JP 2008-248141 A [Patent Document 2] JP 2011-68713 A [Patent Document 3] International Publication No. 2016-17473 [Patent Document 4] JP 2016-79354 A [Patent Document 5] International Publication No. 2018-16489 Summary of the Invention [Problem to be solved by the invention]
[0008] However, the resin composition described in Patent Document 5 is in a varnish state, and the resins are not compatible with each other, so that separation of the varnish occurs, and it has been confirmed that a resin film cannot be obtained, or even if a resin film is obtained, it does not exhibit adhesiveness, and it has been found to be unsuitable for substrate applications. Accordingly, an object of the present invention is to provide a thermosetting maleimide resin composition which is in a varnish form and which gives a cured product which is free from turbidity or separation and has excellent dielectric properties and which has strong adhesive strength even to organic resins such as LCP and MPI, and to copper, as well as an uncured or cured resin film, an adhesive, or a sealant made thereof, and a substrate including a cured product of the thermosetting maleimide resin composition. [Means for solving the problem]
[0009] Means for Solving the Problems The present inventors have conducted intensive research to solve the above problems and have found that the following thermosetting maleimide resin composition can achieve the above object, thereby completing the present invention.
[0010] <1> (A) a styrene-based elastomer having reactive functional groups at both ends, (B) A maleimide compound represented by the following formula (1): [ka] (In formula (1), R 1 represents a divalent hydrocarbon group derived from a dimer acid skeleton. and (C)Organic peroxide wherein the ratio of component (A) to component (B) (mass ratio (A) / (B)) is 2 to 20. <2> The styrene-based elastomer of component (A) is a copolymer of styrene with an alkene and / or a non-conjugated diene, and the reactive functional groups at both ends of the copolymer contain at least one of an amino group, maleic anhydride, and a vinyl group. <1> 2. The thermosetting maleimide resin composition according to claim 1 . <3> Further, the adhesive agent (D) is contained. <1> or <2> 2. The thermosetting maleimide resin composition according to claim 1 . <4> <1> ~ <3> 2. An uncured resin film comprising the thermosetting maleimide resin composition according to claim 1. <5> <1> ~ <3> 2. A cured resin film comprising a cured product of the thermosetting maleimide resin composition according to claim 1. <6> <1> ~ <3> 2. An adhesive comprising the thermosetting maleimide resin composition according to claim 1. <7> <1> ~ <3> 2. An encapsulating material comprising the thermosetting maleimide resin composition according to claim 1. <8> <1> ~ <3> 2. A substrate comprising a cured product of the thermosetting maleimide resin composition according to claim 1. Effect of the Invention
[0011] The thermosetting maleimide resin composition of the present invention does not separate or become turbid even when made into a varnish, and the cured product thereof has excellent dielectric properties and adhesive strength, and has particularly strong adhesive strength to organic resins such as LCP and MPI, as well as to copper. Therefore, the thermosetting maleimide resin composition of the present invention is particularly useful as a material for FPCs. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] The present invention will now be described in more detail.
[0013] (A) Styrene-based elastomer having reactive functional groups at both ends The styrene-based elastomer of component (A) mainly contributes to improving the dielectric properties, heat resistance, and adhesiveness of the cured product of the composition at high frequencies, as well as improving the flexibility of the composition when made into a film, and is not particularly limited as long as it is a thermoplastic elastomer having a structural unit derived from a styrene-based compound and having reactive functional groups at both ends, and may be a thermoplastic elastomer having a structural unit derived from styrene.
[0014] In the present invention, the styrene-based elastomer is preferably a copolymer of styrene and an alkene and / or a non-conjugated diene, which is partially or completely hydrogenated. That is, it is a block copolymer and / or a random copolymer with styrene as a hard segment and alkene and / or a non-conjugated diene as a soft segment. Examples of the styrene-based elastomer include styrene / butadiene / styrene block / random copolymer, styrene / isoprene / styrene block / random copolymer, styrene / ethylene / butylene / styrene block / random copolymer, styrene / ethylene / propylene / styrene block / random copolymer, and styrene / butadiene block / random copolymer. Block copolymers are preferred from the viewpoint of quality stability.
[0015] From the viewpoint of heat resistance, it is preferable to use styrene / ethylene / butylene / styrene block / random copolymer, styrene / ethylene / propylene / styrene block / random copolymer, styrene / butadiene block / random copolymer, etc., in which the double bonds of the conjugated diene component have been eliminated by a hydrogenation reaction (hydrogenation). The hydrogenation may be partial or complete, but complete hydrogenation or one with a high hydrogenation rate is more preferable from the viewpoint of heat resistance.
[0016] The mass ratio of styrene / conjugated diene and its double bond hydrogenated portion in the styrene copolymer is preferably 10 / 90 to 70 / 30, more preferably 20 / 80 to 67 / 33. If the mass ratio is within this range, a composition with excellent compatibility and dispersibility and stable quality can be obtained. That is, the styrene content by mass in the styrene-based elastomer is preferably 10 to 90%, more preferably 20 to 67%.
[0017] In addition, both ends of the styrene-based elastomer of the component (A) are modified with at least one reactive functional group selected from the group consisting of amino, carboxyl, and vinyl groups. This allows the component (A) to react with the component (B) described below, resulting in a cured product with excellent heat resistance. The modification of the styrene-based elastomer can be carried out, for example, by copolymerizing an unsaturated carboxylic acid during polymerization of the styrene-based elastomer. It can also be carried out by heating and kneading the styrene-based elastomer and the unsaturated carboxylic acid in the presence of an organic peroxide. Examples of the unsaturated carboxylic acid include acrylic acid, methacrylic acid, maleic acid, itaconic acid, fumaric acid, maleic anhydride, itaconic anhydride, and fumaric anhydride. The method of amine-modifying the styrene-based elastomer is not particularly limited, and known methods can be used. For example, it can be carried out by copolymerizing an unsaturated monomer containing an amino group with the styrene-based elastomer. It can also be carried out by polymerization using a polymerization initiator containing an amino group.
[0018] The number average molecular weight (Mn) of component (A) is preferably 10,000 to 300,000, and more preferably 10,000 to 200,000. When the number average molecular weight is within the above range, the resulting composition has excellent film properties, excellent compatibility and dispersibility with other components such as components (B) and (C), and exhibits good adhesion. The number average molecular weight referred to in this specification refers to the number average molecular weight measured by gel permeation chromatography (GPC) under the following conditions using polystyrene as a standard substance.
[0019] [Measurement conditions] Developing solvent: Tetrahydrofuran (THF) Flow rate: 0.35mL / min Detector: Refractive index detector (RI) Column: TSK Guardcolumn SuperH-L TSKgel SuperHZ4000(4.6mmI.D.×15cm×1) TSKgel SuperHZ3000(4.6mmI.D.×15cm×1) TSKgel SuperHZ2000 (4.6mmI.D.×15cm×2) (All manufactured by Tosoh Corporation) Column temperature: 40℃ Sample injection volume: 5 μL (0.2% by mass in THF solution)
[0020] The styrene-based elastomer (A) may be a commercially available product. Specific examples include the Tuftec series manufactured by Asahi Kasei Corporation and the FG series manufactured by Kraton. The composition of the present invention may contain one type of styrene-based elastomer alone or a mixture of two or more types. In the thermosetting maleimide resin composition of the present invention, the blending amount of the component (A) is preferably from 60 to 99 mass %, more preferably from 65 to 97 mass %, and further preferably from 70 to 95 mass %.
[0021] (B) Maleimide Compound The component (B) used in the present invention is a maleimide compound represented by the following formula (1), and is preferably a maleimide compound which is a reaction product of dimer diamine and maleic anhydride. The component (B) is a thermosetting resin, and since it reacts with the component (A), it has good heat resistance and mechanical properties, resulting in a highly reliable composition. In addition, the component (B) has good dielectric properties because it has a divalent hydrocarbon group derived from the dimer acid skeleton. Therefore, the composition exhibits excellent dielectric properties. [ka] (In formula (1), R 1 represents a divalent hydrocarbon group derived from a dimer acid skeleton.
[0022] Dimer acids are liquid fatty acids that are mainly composed of dicarboxylic acids with 36 carbon atoms, produced by dimerization of unsaturated fatty acids with 18 carbon atoms, which are derived from natural products such as vegetable oils. Dimer acids do not have a single skeleton, but rather have multiple structures and exist in several types of isomers. Representative dimer acids are classified as linear (a), monocyclic (b), aromatic (c), and polycyclic (d). In this specification, the dimer acid skeleton refers to a group derived from a dimer diamine having a structure in which the carboxy group of such a dimer acid is substituted with a primary aminomethyl group. Examples of the divalent hydrocarbon group derived from the dimer acid skeleton include, but are not limited to, the following structures. Furthermore, from the viewpoint of the heat resistance and reliability of the cured product, it is more preferable that the divalent hydrocarbon group derived from the dimer acid skeleton of component (B) has a structure in which the carbon-carbon double bond in the hydrocarbon group derived from the dimer acid skeleton is reduced by a hydrogenation reaction. [ka]
[0023] When a maleimide compound other than that represented by formula (1) is used as component (B), its compatibility with component (A) decreases, causing turbidity and separation when made into a varnish, which may lead to unevenness in the composition and variations in the properties of the composition.
[0024] The mass ratio ((A) / (B)) of the component (A) to the component (B) is 2 to 20, and preferably 3 to 15. If this ratio is greater than 20, the amount of liquid components will increase, which may result in poor film properties when uncured. Conversely, if it is less than 2, the amount of thermosetting components will decrease, which may result in poor heat resistance.
[0025] (C)Organic peroxide The organic peroxide, component (C), is added primarily to initiate the crosslinking reaction of the maleimide compound, component (B), and, if there is a radically polymerizable functional group in the styrene-based elastomer, component (A), to promote the reaction between the functional group and the maleimide compound, component (B). Examples of organic peroxides include dicumyl peroxide, di-tert-butyl peroxide, 2,5-dimethyl-2,5-di-(tert-butylperoxy)hexane, 2,5-dimethyl-2,5-di(tert-butylperoxy)hexyne-3, 1,3-bis(tert-butylperoxyisopropyl)benzene, 1,1-bis(tert-butylperoxy)-3,3,5-trimethylcyclohexane, n-butyl-4,4-bis(tert-butylperoxy)valerate, benzoyl peroxide, p-chlorobenzoyl peroxide, 2,4-dichlorobenzoyl peroxide, tert-butyl peroxybenzoate, tert-butylperoxyisopropyl carbonate, diacetyl peroxide, lauroyl peroxide, and tert-butylcumyl peroxide.
[0026] The amount of the (C) component is preferably 0.01 to 5.0 parts by mass, more preferably 0.1 to 3.0 parts by mass, based on 100 parts by mass of the total amount of the (A) and (B) components. If the (C) component is more than this range, the adhesive strength may decrease, and the dielectric properties may deteriorate due to the residual (C) component. On the other hand, if the (C) component is less than the above range, the curability may decrease, and therefore the dielectric properties and heat resistance may decrease.
[0027] <Other additives> The thermosetting maleimide resin composition of the present invention may further contain various additives as necessary within the range that does not impair the effects of the present invention. For example, as an adhesion aid, coupling agents such as silane coupling agents and titanate coupling agents, and monomers having a (meth)acrylic group may be blended. (D) Adhesive assistant As the adhesion promoter, a coupling agent such as a silane coupling agent or a titanate coupling agent, or a monomer having a (meth)acrylic group can be blended. Examples of the silane coupling agent include epoxy-functional alkoxysilanes such as γ-glycidoxypropyltrimethoxysilane, γ-glycidoxypropylmethyldiethoxysilane, and β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane; mercapto-functional alkoxysilanes such as γ-mercaptopropyltrimethoxysilane; amine-functional alkoxysilanes such as γ-aminopropyltrimethoxysilane and N-2-(aminoethyl)-3-aminopropyltrimethoxysilane; and methacryl-functional alkoxysilanes such as 3-methacryloxypropyltrimethoxysilane. Titanium coupling agents include isopropyl triisostearoyl titanate, isopropyl tridodecylbenzenesulfonyl titanate, isopropyl tris(dioctyl pyrophosphate) titanate, tetraisopropyl bis(dioctyl phosphite) titanate, tetraoctyl bis(ditridecyl phosphite) titanate, bis(dioctyl pyrophosphate) oxyacetate titanate, isopropyl trioctanoyl titanate, isopropyl dimethacryl isostearoyl titanate, isopropyl isostearoyl diacryl titanate, isopropyl tri(dioctyl phosphate) titanate, isopropyl tricumyl phenyl titanate, and isopropyl tri(N-aminoethyl aminoethyl) titanate. Examples of monomers having a (meth)acrylic group include 1,6-hexanediol diacrylate, neopentyl glycol diacrylate, dipropylene glycol diacrylate, tricyclodecane dimethanol diacrylate, 9,9-bis[4-(2-hydroxyethoxy)phenyl]fluorene diacrylate, bisphenol A diacrylate, trimethylolpropane triacrylate, tris(2-acryloxymethyl)isocyanurate, ditrimethylolpropane tetraacrylate, 1,6-hexanediol dimethacrylate, neopentyl glycol methacrylate, dipropylene glycol methacrylate, tricyclodecane dimethanol methacrylate, 9,9-bis[4-(2-hydroxyethoxy)phenyl]fluorene methacrylate, bisphenol A dimethacrylate, trimethylolpropane trimethacrylate, tris(2-methacryloxymethyl)isocyanurate, and ditrimethylolpropane tetramethacrylate.
[0028] Other examples of additives include inorganic fillers such as silica, alumina, and boron nitride, resin powders such as PTFE powder, metal particles such as silver, organopolysiloxanes having reactive functional groups, non-functional silicone oils, thermoplastic resins, thermoplastic elastomers other than styrene-based, organic synthetic rubbers, photosensitizers, light stabilizers, polymerization inhibitors, flame retardants, pigments, dyes, etc. In order to improve the electrical properties of the cured product of the thermosetting maleimide resin composition, an ion trapping agent or the like may be blended as other additives.
[0029] The thermosetting maleimide resin composition of the present invention can be produced by mixing the components (A), (B), and (C) and other additives that are added as necessary. The thermosetting maleimide resin composition of the present invention can also be dissolved in an organic solvent and treated as a varnish. The thermosetting maleimide resin composition can be easily molded into a sheet or film by forming it into a varnish. Any organic solvent can be used without limitation as long as it dissolves the (A) component and the (B) component. As the organic solvent, for example, toluene, xylene, anisole, cyclohexanone, cyclopentanone, etc. can be suitably used. The above organic solvents may be used alone or in combination of two or more kinds. The concentration of the thermosetting maleimide resin composition of the present invention in the varnish is preferably 5 to 80% by mass, more preferably 10 to 75% by mass.
[0030] This thermosetting maleimide resin composition can be suitably used mainly as an adhesive, a primer, a bonding film or sheet material for a substrate, a sealing material, an adhesive layer for a coverlay film for an FPC, or a flexible flat cable. There are no limitations on the method or form of use. For example, it can be used as an uncured resin film or a cured resin film, or as an adhesive. Examples of use are shown below, but are not limited thereto.
[0031] For example, a thermosetting maleimide resin composition (varnish) dissolved in an organic solvent is applied to a support sheet, and then the organic solvent is removed by heating at a temperature of usually 80° C. or higher, preferably 100° C. or higher, for 0.5 to 5 hours, to obtain an uncured film-like or sheet-like composition (uncured resin film). As the support sheet, a commonly used one may be used, for example, polyolefin resins such as polyethylene (PE) resin, polypropylene (PP) resin, and polystyrene (PS) resin, and polyester resins such as polyethylene terephthalate (PET) resin, polybutylene terephthalate (PBT) resin, and polycarbonate (PC) resin, and the surface of these support sheets may be subjected to a release treatment. In addition, the coating method is not particularly limited, and examples thereof include a gap coater, a curtain coater, a roll coater, and a laminator. In addition, the thickness of the coating layer is not particularly limited, but the thickness after distillation of the solvent is in the range of 1 to 100 μm, preferably 3 to 80 μm. Furthermore, a cover film may be used on the coating layer.
[0032] Moreover, a copper foil can be attached onto the coating layer to use it as a substrate material.
[0033] Furthermore, the organic solvent is removed by applying a varnish to the substrate and heating it at a temperature of usually 80°C or higher, preferably 100°C or higher, for 0.5 to 5 hours, and the material to be bonded to the substrate is pressed while being heated, and then heated at a temperature of 130°C or higher, preferably 150°C or higher, for 0.5 to 10 hours to bond the material.
[0034] Examples of a method for applying the thermosetting maleimide composition solution (varnish) include ordinary coating methods and printing methods. Specifically, coating methods such as air doctor coating, bar coating, blade coating, knife coating, reverse coating, transfer roll coating, gravure roll coating, kiss coating, cast coating, spray coating, slot orifice coating, calendar coating, dam coating, dip coating, and die coating, as well as printing methods such as intaglio printing such as gravure printing, and stencil printing such as screen printing can be used. EXAMPLES
[0035] The present invention will be specifically described below with reference to examples and comparative examples, but the present invention is not limited to the following examples.
[0036] The components used in the examples and comparative examples are shown below.
[0037] (A) Styrene-based elastomer having reactive functional groups at both ends (A-1) Amine-modified styrene / ethylene / butylene / styrene block copolymer, hydrogenated, styrene content 30%, number average molecular weight 33,000 (Tuftec MP10: Asahi Kasei Corporation) (A-2) Carboxylic acid modified styrene / ethylene / butylene / styrene block copolymer, styrene content 30%, number average molecular weight 90,000 (Tuftec M1913: Asahi Kasei Corporation) (A-3) Styrene / ethylene / butylene / styrene block copolymer, styrene content 30%, number average molecular weight 74,000 (Tuftec H1041: Asahi Kasei Corporation, for comparison)
[0038] (B) Maleimide Compound (B-1): A bismaleimide compound represented by the following formula (SLK-6895, manufactured by Shin-Etsu Chemical Co., Ltd.) [ka] -C36 H 70 - represents a hydrocarbon group derived from a dimer acid skeleton. (B-2): A bismaleimide compound represented by the following formula (SLK-3000, manufactured by Shin-Etsu Chemical Co., Ltd., for comparative purposes) [ka] -C 36 H 70 - represents a hydrocarbon group derived from a dimer acid skeleton. (B-3): 4,4'-diphenylmethane bismaleimide (BMI-1000: manufactured by Daiwa Chemical Industry Co., Ltd., for comparison)
[0039] (C)Organic peroxide (C-1): Dicumyl peroxide (Percumyl D: manufactured by NOF Corp.) (C-2): 2-ethyl-4-methylimidazole (2E4MZ: manufactured by Shikoku Kasei Co., Ltd., for comparison purposes)
[0040] (D) Adhesive assistant (D-1): 3-methacryloxypropyltrimethoxysilane (KBM-503: manufactured by Shin-Etsu Chemical Co., Ltd.)
[0041] <Preparation of varnish> The components according to the formulations in Tables 1 and 2 were placed in a 500 mL four-neck flask equipped with a Dimroth condenser and a stirrer, and stirred at 50° C. for 2 hours to obtain a varnish-like resin composition.
[0042] <Appearance of varnish> Regarding the varnish before being made into a film, if there was no residual dissolution or turbidity when visually observed, and if a 30 mass % xylene solution of the resin composition was placed in a quartz cell, the direct light transmittance at 740 nm with an optical path length of 1 mm was measured at 25°C using a spectrophotometer U-4100 (manufactured by Hitachi High-Tech Science Corp.), those that were 50% or more were marked as ○, and those that were less than 50% were marked as ×.
[0043] <Preparation of uncured film> The varnish-like thermosetting maleimide resin composition was applied to a PET film having a thickness of 38 μm using a roller coater so that the thickness after drying would be 50 μm, and then dried at 120° C. for 10 minutes to obtain an uncured resin film.
[0044] <Handling of uncured resin film> The uncured resin film was visually inspected for cracks or breakage when it was bent 90 degrees at 25° C. When no cracks, breaks, tackiness, or the like were observed, it was marked with an ◯, and when even a small amount of cracks, breaks, tackiness, or the like was observed, it was marked with an ×.
[0045] [Table 1]
[0046] [Table 2]
[0047] From the results in Tables 1 and 2, it was confirmed that the varnish appearance of the varnish compositions of Examples 1 to 8 was stable without separation or turbidity. The stability of the varnish compositions was also confirmed in Comparative Examples 3 to 6. On the other hand, the varnishes of Comparative Examples 1 and 2 became turbid.
[0048] From the results in Tables 1 and 2, it was confirmed that there were no cracks or breaks in the uncured resin film properties for Examples 1 to 8. Similarly to the Examples, no cracks or the like were confirmed for Comparative Examples 1, 3, 5 to 6. On the other hand, cracks and tack were observed in Comparative Examples 2 and 4. Further evaluation of Comparative Examples 2 and 4 was discontinued.
[0049] <Dielectric constant, dielectric loss tangent> The uncured resin film was cured at 180° C. for 2 hours, and the resulting resin film was cut to prepare a 60 mm×60 mm test piece. The dielectric constant and dielectric loss tangent of the obtained test piece were measured at 10 GHz and 28 GHz at 25° C. using an SPDR dielectric resonator (MS46122B, manufactured by Anritsu Corporation).
[0050] <Heat resistance> The cured resin film produced by the above process was stored at 150°C for 500 hours, and then the dielectric properties were measured at 10 GHz at 25°C using the above device. When the rate of change between the initial dielectric tangent at 10 GHz and the dielectric tangent at 10 GHz after storage was less than 100%, it was evaluated as ◯, and when it was 100% or more, it was evaluated as ×.
[0051] <Peel strength>
[0052] A slide glass having a length of 75 mm, a width of 25 mm, and a thickness of 1.0 mm was prepared, and the resin composition side of the uncured resin film with a PET film, on which the PET substrate was not attached, was placed on one surface, and lamination was performed under conditions of 120 ° C, 0.3 MPa pressure, and 60 seconds. After lamination, the PET substrate was peeled off, and a 18 μm thick copper foil (Mitsui Kinzoku Co., Ltd., Ra 0.6 μm), a 50 μm thick LCP (Chiyoda Integre Co., Ltd.) or MPI (PIXEO SR, Kaneka Co., Ltd.) was placed on the resin composition surface, and lamination was performed under conditions of 120 ° C, 0.3 MPa pressure, and 60 seconds. After lamination, the adhesive test piece was prepared by curing at 180 ° C for 2 hours.
[0053] To evaluate the adhesion, the 90° peel strength (kN / m) was measured when peeling the copper foil, LCP, or MPI of each adhesive test piece from the slide glass at a temperature of 23°C and a tensile speed of 50 mm / min in accordance with JIS-C-6481 "Test methods for copper-clad laminates for printed wiring boards."
[0054] The evaluation results are shown in Tables 3 and 4.
[0055] [Table 3]
[0056] [Table 4]
[0057] From the above results, it has been confirmed that the thermosetting maleimide resin composition of the present invention is free from separation or turbidity of the varnish, has excellent dielectric properties after curing, and exhibits high adhesive strength to metals and organic resins, and is therefore useful as an insulating material suitable for substrate applications.
Claims
1. (A) a styrene-based elastomer having reactive functional groups at both ends, (B) A maleimide compound represented by the following formula (1): 【Chemistry 1】 (In formula (1), R 1 represents a divalent hydrocarbon group derived from a dimer acid skeleton.) and (C) Organic peroxide The ratio of the component (A) to the component (B) (mass ratio (A) / (B)) is 2 to 20; The styrene-based elastomer of component (A) is a copolymer of styrene with an alkene and / or a non-conjugated diene, and reactive functional groups at both ends of the copolymer include at least one of an amino group, a carboxyl group, and a vinyl group; A thermosetting maleimide resin composition further containing an adhesive aid as component (D) (excluding the case where the thermosetting maleimide resin composition contains an inorganic filler).
2. An uncured resin film comprising the thermosetting maleimide resin composition described in claim 1.
3. A cured resin film comprising a cured product of the thermosetting maleimide resin composition described in claim 1.
4. An adhesive comprising the thermosetting maleimide resin composition described in claim 1.
5. A sealing material comprising the thermosetting maleimide resin composition described in claim 1.
6. A substrate comprising a cured product of the thermosetting maleimide resin composition described in claim 1.
Citation Information
Patent Citations
Maleimide-terminated rubber and curable composition using the same
JP2004315818A
Flame retardant curable resin composition
JP2008248141A
Coverlay film
JP2011068713A
Resin composition, insulation film and semiconductor device using the same
JP2016079354A
Resin sheet
JP2022146808A