Etching Method
By strategically controlling the distribution of noble metal catalysts through a dual-layered coating on the substrate, the method addresses processing defects in etching, ensuring uniform etching and improved semiconductor device manufacturing.
Patent Information
- Application Number
- JP2021044887
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-03-18
- Publication Date
- 2024-09-25
- Estimated Expiration
- 2041-03-18
AI Technical Summary
Existing etching methods using a catalyst are prone to processing defects, particularly due to uneven distribution of noble metal catalysts, leading to inefficient and non-uniform etching.
A method involving a substrate with distinct regions coated with a first layer having openings and a second continuous layer, where a noble metal catalyst layer is formed within the openings, and a second layer is applied to control the catalyst distribution, followed by etching with an oxidizing agent and hydrogen fluoride.
This approach minimizes processing defects by ensuring uniform etching, allowing for precise formation of recesses and structures with high aspect ratios, thereby enhancing the manufacturing yield and quality of semiconductor devices.
Smart Images

Figure 0007555860000001 
Figure 0007555860000002 
Figure 0007555860000003
Abstract
Description
[Technical field]
[0001] An embodiment of the present invention relates to an etching method. [Background technology]
[0002] The Metal-Assisted Chemical Etching (MacEtch) method is a method for etching a semiconductor surface using a precious metal as a catalyst, and can form, for example, a recess with a high aspect ratio in a semiconductor substrate. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Special Publication No. 2013-527103 [Patent Document 2] JP 2011-101009 A Summary of the Invention [Problem to be solved by the invention]
[0004] The problem to be solved by the present invention is to prevent processing defects from occurring in etching using a catalyst. [Means for solving the problem]
[0005] According to one aspect, there is provided an etching method including: forming a first layer on a substrate including a semiconductor material and having a first region and a second region adjacent to each other on one main surface, the first layer covering the first region and the second region, the first layer having a plurality of openings or one or more openings defining a plurality of island-shaped portions in a portion covering the first region and being a continuous film; forming a catalyst layer including a precious metal by a plating method on portions of the main surface exposed within the plurality of openings or the one or more openings; forming a second layer covering a portion of the catalyst layer adjacent to a boundary between the first region and the second region and exposing a portion of the catalyst layer spaced from the boundary; and etching the substrate with an etching agent including an oxidant and hydrogen fluoride in the presence of the catalyst layer and the second layer.
[0006] According to another aspect, there is provided an etching method including: forming, on a substrate including a semiconductor material and having a first region and a second region adjacent to each other on one main surface, a mask layer including a first portion covering the first region and having a plurality of openings or one or more openings defining a plurality of island-shaped portions, and a second portion which is a continuous film covering the second region, wherein a height of the second portion relative to the main surface at a position adjacent to a boundary between the first region and the second region is greater than a height of the first portion relative to the main surface; forming a catalyst layer containing a precious metal on portions of the main surface exposed in the plurality of openings or the one or more openings by a plating method; and etching the substrate with an etching agent containing an oxidant and hydrogen fluoride in the presence of the catalyst layer and the mask layer. [Brief description of the drawings]
[0007] [Figure 1] FIG. 2 is a top view showing an example of a capacitor that can be manufactured by the methods according to the first and second embodiments. [Diagram 2] 2 is a cross-sectional view of the capacitor taken along line II-II in FIG. 1. [Diagram 3] 3 is a cross-sectional view showing a step in the method for manufacturing the capacitor according to the first embodiment. [Figure 4] 5 is a cross-sectional view showing another step in the method for manufacturing the capacitor according to the first embodiment. [Diagram 5] FIG. 5 is a top view showing the structure obtained by the process of FIG. [Figure 6] 5 is a cross-sectional view showing still another step in the method for manufacturing the capacitor according to the first embodiment. [Figure 7] 5 is a cross-sectional view showing still another step in the method for manufacturing the capacitor according to the first embodiment. [Figure 8] FIG. 8 is a top view showing the structure obtained by the process of FIG. 7. [Figure 9] 5 is a cross-sectional view showing still another step in the method for manufacturing the capacitor according to the first embodiment. [Figure 10] 5 is a cross-sectional view showing still another step in the method for manufacturing the capacitor according to the first embodiment. [Figure 11] 11 is a cross-sectional view showing a structure obtained by the steps of FIGS. 9 and 10. FIG. [Figure 12] An electron microscope photograph showing an example of the structure obtained when the second layer is omitted. [Figure 13] Electron microscope photograph showing an example of a structure obtained when a second layer is provided. [Figure 14] 10 is a cross-sectional view showing a step in a method for manufacturing a capacitor according to a second embodiment. [Figure 15] FIG. 15 is a top view showing the structure obtained by the process of FIG. 14. [Figure 16] 10 is a cross-sectional view showing another step in the method for manufacturing a capacitor according to the second embodiment. [Figure 17] 13 is a cross-sectional view showing still another step in the method for manufacturing a capacitor according to the second embodiment. [Figure 18] 10A to 10C are cross-sectional views showing a modified example of the method for manufacturing a capacitor according to the second embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] Hereinafter, the embodiments will be described in detail with reference to the drawings. Note that components that perform the same or similar functions are given the same reference numerals throughout the drawings, and duplicated descriptions will be omitted.
[0009] First Embodiment The etching method according to the first embodiment includes the steps of: forming a first layer on a substrate including a semiconductor material and having a first region and a second region adjacent to each other on one main surface, the first layer covering the first region and the second region, the first region having a plurality of openings or one or more openings defining a plurality of island-shaped portions in the portion covering the first region, and the second region being a continuous film; forming a catalytic layer including a precious metal by a plating method on the portions of the main surface exposed within the plurality of openings or the one or more openings; forming a second layer covering a portion of the catalytic layer adjacent to a boundary between the first region and the second region and exposing a portion of the catalytic layer spaced from the boundary; and etching the substrate with an etching agent including an oxidant and hydrogen fluoride in the presence of the catalytic layer and the second layer.
[0010] The method for producing a structure according to the first embodiment includes forming one or more recesses in the substrate by the above-mentioned etching method.
[0011] The method for manufacturing the semiconductor device according to the first embodiment includes forming one or more recesses in the substrate by the above-mentioned etching method, forming a lower electrode on a sidewall of the one or more recesses, forming a dielectric layer on the lower electrode, and forming an upper electrode on the dielectric layer.
[0012] Hereinafter, a method for manufacturing a capacitor, which is an example of a semiconductor device, as a structure using the above-mentioned etching method will be described.
[0013] 1 and 2 show an example of a capacitor that can be manufactured by the method according to the first embodiment. The capacitor 1 shown in FIGS. 1 and 2 includes a conductive substrate CS, a conductive layer 20b, and a dielectric layer 30, as shown in FIG.
[0014] In each figure, the X direction is parallel to the main surface of the conductive substrate CS, the Y direction is parallel to the main surface of the conductive substrate CS and perpendicular to the X direction, and the Z direction is the thickness direction of the conductive substrate CS, i.e., perpendicular to the X and Y directions.
[0015] The conductive substrate CS includes a semiconductor material such as silicon. At least the surface of the conductive substrate CS facing the conductive layer 20b has electrical conductivity. At least a portion of the conductive substrate CS serves as the lower electrode of the capacitor.
[0016] The conductive substrate CS has a first main surface S1, a second main surface S2, and an end surface extending from an edge of the first main surface S1 to an edge of the second main surface S2. Here, the conductive substrate CS has a flattened, substantially rectangular parallelepiped shape. The conductive substrate CS may have another shape.
[0017] The first main surface S1, here the upper surface of the conductive substrate CS, includes a first region A1 and a second region A2. The first region A1 corresponds to a portion of the conductive substrate CS where a recess TR, which will be described later, is provided. The second region A2 has the same height as the first region A1. The second region A2 is adjacent to the first region A1. Here, the first region A1 has a rectangular shape, and the second region A2 surrounds the first region A1.
[0018] A portion of the conductive substrate CS corresponding to the first region A1 is provided with a plurality of recesses TR, each having a shape extending in one direction and arranged in the width direction. The recesses TR are open in the first region A1. The recesses TR are spaced apart from each other. Here, the recesses TR are a plurality of trenches, each extending in the Y direction and arranged in the X direction.
[0019] The conductive substrate CS has a portion sandwiched between adjacent recesses TR that is a protrusion. The protrusions each have a shape extending in the Y direction and are arranged in the X direction. That is, the conductive substrate CS has a portion corresponding to the first region A1 that is provided with a plurality of wall portions that each have a shape extending in the Y and Z directions and are arranged in the X direction as a protrusion.
[0020] The "length direction" of the recess or protrusion is the length direction of the orthogonal projection of the recess or protrusion onto a plane perpendicular to the thickness direction of the conductive substrate.
[0021] The length of the opening of the recess TR is, according to one example, in the range of 10 to 500 μm, and according to another example, in the range of 50 to 100 μm.
[0022] The width of the opening of the recess TR, i.e., the distance between adjacent protrusions in the width direction, is preferably 0.3 μm or more. By reducing this width or distance, a larger electric capacity can be achieved. However, by reducing this width or distance, it becomes difficult to form a laminated structure including the dielectric layer 30 and the conductive layer 20b in the recess TR.
[0023] According to one example, the depth of the recess TR or the height of the projection is in the range of 10 to 300 μm, and according to another example, in the range of 50 to 100 μm.
[0024] The distance between adjacent recesses TR in the width direction, i.e., the thickness of the protrusions, is preferably 0.1 μm or more. By reducing this distance or thickness, a larger electric capacity can be achieved. However, by reducing this distance or thickness, the protrusions become more susceptible to breakage.
[0025] In this embodiment, the cross sections perpendicular to the longitudinal direction of the recess TR are rectangular. These cross sections do not have to be rectangular. For example, these cross sections may have a tapered shape.
[0026] The conductive substrate CS includes a substrate 10 and a conductive layer 20a. The substrate 10 has a shape similar to that of the conductive substrate CS. The substrate 10 is a substrate containing a semiconductor material, for example, a semiconductor substrate. The substrate 10 is preferably a substrate containing silicon, such as a silicon substrate. Such a substrate can be processed using a semiconductor process.
[0027] The conductive layer 20a is provided on the substrate 10. Here, the conductive layer 20a serves as a lower electrode of a capacitor. The conductive layer 20a is made of, for example, polysilicon doped with impurities to enhance conductivity, or a metal or alloy such as molybdenum, aluminum, gold, tungsten, platinum, nickel, and copper. The conductive layer 20a may have a single-layer structure or a multi-layer structure.
[0028] The thickness of the conductive layer 20a is preferably in the range of 0.05 μm to 1 μm, and more preferably in the range of 0.1 μm to 0.3 μm. If the conductive layer 20a is too thin, discontinuities may occur in the conductive layer 20a or the sheet resistance of the conductive layer 20a may be excessively large. If the conductive layer 20a is made thicker, the manufacturing cost increases.
[0029] Here, as an example, the substrate 10 is a semiconductor substrate such as a silicon substrate, and the conductive layer 20a is a highly doped layer in which the surface region of the semiconductor substrate is highly doped with impurities. In this case, if the protrusions are sufficiently thin, they can be entirely doped with impurities at a high concentration.
[0030] Furthermore, when the substrate 10 has a high conductivity, the conductive layer 20a may be omitted and the substrate 10 may be used as the conductive substrate CS. For example, when the substrate 10 is a semiconductor substrate made of a semiconductor doped with P-type or N-type impurities or a metal substrate, the conductive layer 20a may be omitted. In this case, at least the surface region of the substrate 10, for example, the entire substrate 10, serves as the conductive layer 20a.
[0031] The conductive layer 20b serves as an upper electrode of the capacitor. The conductive layer 20b is provided on the first region A1 and covers the sidewalls and the bottom surface of the recess TR.
[0032] The conductive layer 20b is made of, for example, polysilicon doped with impurities to enhance conductivity, or a metal or alloy such as molybdenum, aluminum, gold, tungsten, platinum, nickel, copper, etc. The conductive layer 20b may have a single-layer structure or a multi-layer structure.
[0033] The thickness of the conductive layer 20b is preferably in the range of 0.05 μm to 1 μm, and more preferably in the range of 0.1 μm to 0.3 μm. If the conductive layer 20b is too thin, discontinuities may occur in the conductive layer 20b, or the sheet resistance of the conductive layer 20b may be excessively large. If the conductive layer 20b is too thick, it may be difficult to form the conductive layer 20a and the dielectric layer 30 to a sufficient thickness.
[0034] 2, the conductive layer 20b is provided such that the recess TR is completely filled with the conductive layer 20b and the dielectric layer 30. The conductive layer 20b may be a layer conformal to the surface of the conductive substrate CS. That is, the conductive layer 20b may be a layer having a substantially uniform thickness. In this case, the recess TR is not completely filled with the conductive layer 20b and the dielectric layer 30.
[0035] The dielectric layer 30 is interposed between the conductive substrate CS and the conductive layer 20b. The dielectric layer 30 is a layer conformal to the surface of the conductive substrate CS. The dielectric layer 30 electrically insulates the conductive substrate CS and the conductive layer 20b from each other.
[0036] The dielectric layer 30 is made of, for example, an organic dielectric or an inorganic dielectric. For example, polyimide can be used as the organic dielectric. For example, a ferroelectric can be used as the inorganic dielectric, but paraelectrics such as silicon nitride, silicon oxide, silicon oxynitride, titanium oxide, and tantalum oxide are preferable. These paraelectrics have a small change in dielectric constant due to temperature. Therefore, the use of a paraelectric for the dielectric layer 30 can increase the heat resistance of the capacitor 1.
[0037] The thickness of the dielectric layer 30 is preferably in the range of 0.005 μm to 0.5 μm, and more preferably in the range of 0.01 μm to 0.1 μm. If the dielectric layer 30 is thin, discontinuities may occur in the dielectric layer 30, which may cause a short circuit between the conductive substrate CS and the conductive layer 20b. Furthermore, if the dielectric layer 30 is thin, the withstand voltage decreases even if there is no short circuit, and the possibility of a short circuit when a voltage is applied increases. If the dielectric layer 30 is thickened, the withstand voltage increases, but the electric capacity decreases.
[0038] The portion of the dielectric layer 30 located on the second region A2 is opened so as to surround the first region A1. That is, the conductive layer 20a is exposed at this position of the dielectric layer 30. Here, the portion of the dielectric layer 30 provided on the first main surface S1 is opened in a frame shape.
[0039] The capacitor 1 further includes an insulating layer 60, a first internal electrode 70a, a second internal electrode 70b, a first external electrode 70c, and a second external electrode 70d.
[0040] The first internal electrode 70a is provided on the first region A1. The first internal electrode 70a is electrically connected to the conductive layer 20b. Here, the first internal electrode 70a is a rectangular electrode located at the center of the first main surface S1.
[0041] The second internal electrode 70b is provided on the second region A2. The second internal electrode 70b is in contact with the conductive substrate CS at the position of an opening provided in the dielectric layer 30. As a result, the second internal electrode 70b is electrically connected to the conductive substrate CS. Here, the second internal electrode 70b is a frame-shaped electrode disposed so as to surround the first internal electrode 70a.
[0042] The first internal electrode 70a and the second internal electrode 70b may have a single-layer structure or a multi-layer structure. Each layer constituting the first internal electrode 70a and the second internal electrode 70b is made of a metal such as molybdenum, aluminum, gold, tungsten, platinum, copper, nickel, or an alloy containing one or more of these metals.
[0043] The insulating layer 60 covers the conductive layer 20b and the portions of the dielectric layer 30 located on the first main surface S1, the first internal electrode 70a, and the second internal electrode 70b. The insulating layer 60 is partially opened at the position of a part of the first internal electrode 70a and the position of a part of the second internal electrode 70b.
[0044] The insulating layer 60 may have a single-layer structure or a multi-layer structure. Each layer constituting the insulating layer 60 is made of an inorganic insulator such as silicon nitride and silicon oxide, or an organic insulator such as polyimide and novolac resin.
[0045] The first external electrode 70c is provided on the insulating layer 60. The first external electrode 70c is in contact with the first internal electrode 70a at the positions of one or more openings provided in the insulating layer 60. As a result, the first external electrode 70c is electrically connected to the first internal electrode 70a. In FIG. 1, a region 70R1 is a region where the first external electrode 70c and the first internal electrode 70a are in contact with each other.
[0046] The second external electrode 70d is provided on the insulating layer 60. The second external electrode 70d is in contact with the second internal electrode 70b at the remaining openings provided in the insulating layer 60. As a result, the second external electrode 70d is electrically connected to the second internal electrode 70b. In FIG. 1, the region 70R2 is the region where the second external electrode 70d and the second internal electrode 70b are in contact with each other.
[0047] The first external electrode 70c has a layered structure including a first metal layer 70c1 and a second metal layer 70c2. The second external electrode 70d has a layered structure including a first metal layer 70d1 and a second metal layer 70d2.
[0048] The first metal layers 70c1 and 70d1 are made of, for example, copper. The second metal layers 70c2 and 70d2 cover the top and end surfaces of the first metal layers 70c1 and 70d1, respectively. The second metal layers 70c2 and 70d2 are made of, for example, a laminated film of a nickel or nickel alloy layer and a gold layer. The second metal layers 70c2 and 70d2 can be omitted.
[0049] The first external electrode 70c or the first internal electrode 70a may further include a barrier layer adjacent to the interface therebetween. The second external electrode 70d or the second internal electrode 70b may further include a barrier layer adjacent to the interface therebetween. The material of the barrier layer may be, for example, titanium.
[0050] The capacitor 1 is manufactured, for example, by the following method. An example of the method for manufacturing the capacitor 1 will be described below with reference to FIGS.
[0051] In this method, first, the substrate 10 shown in Fig. 3 is prepared. As described later, here, as an example, the conductive layer 20a is formed by doping impurities at a high concentration into the surface region of the substrate 10. Therefore, one main surface and the other main surface of the substrate 10 correspond to the first main surface S1 and the second main surface S2 described with reference to Fig. 2, respectively.
[0052] The first main surface S1 has the first region A1 and the second region A2 described with reference to FIG.
[0053] Here, as an example, the substrate 10 is a single crystal silicon wafer. Although the surface orientation of the single crystal silicon wafer is not particularly important, in this example, a silicon wafer having a first main surface S1 of a (100) plane is used. The substrate 10 may also be a silicon wafer having a first main surface S1 of a (110) plane.
[0054] Next, recesses are formed in the substrate 10 by MacEtch (Metal-Assisted Chemical Etching).
[0055] That is, first, a first layer 90 is formed on a first main surface S1 of a substrate 10 as shown in FIG. A plurality of openings are provided in the portion of the first layer 90 covering the first region A1. Here, the plurality of openings are a plurality of slits 90S arranged in the width direction. The length direction of the slits 90S is parallel to the Y direction and arranged in the X direction. In addition, the portion of the first layer 90 covering the second region A2 is a continuous film. The first layer 90 is a first mask layer that prevents the portion of the first main surface S1 covered by the first layer 90 from contacting a precious metal described later.
[0056] The multiple openings provided in the first layer 90 may have a shape other than slits. For example, the first layer 90 may be provided with a multiple number of through holes arranged in two intersecting directions, each of which has a circular, elliptical, or polygonal shape as the multiple openings.
[0057] Alternatively, instead of providing a plurality of openings, one or more openings defining a plurality of island-shaped portions may be provided in the first layer 90. In this case, pillar-shaped protrusions can be formed at positions corresponding to the island-shaped portions by etching, which will be described later.
[0058] Examples of materials for the first layer 90 include organic materials such as polyimide, fluororesin, phenolic resin, acrylic resin, and novolac resin, and inorganic materials such as silicon oxide and silicon nitride.
[0059] The first layer 90 can be formed, for example, by an existing semiconductor process. The first layer 90 made of an organic material can be formed, for example, by photolithography. The first layer 90 made of an inorganic material can be formed, for example, by forming an inorganic material layer by vapor deposition, forming a mask by photolithography, and patterning the inorganic material layer by etching. Alternatively, the first layer 90 made of an inorganic material can be formed by oxidizing or nitriding the surface region of the substrate 10, forming a mask by photolithography, and patterning the oxide or nitride layer by etching.
[0060] Next, as shown in FIGS. 4 and 5, a catalyst layer 80 containing a precious metal is formed by plating on the portion of the first main surface S1 exposed within the slit 90S.
[0061] The catalyst layer 80 is, for example, a discontinuous layer containing a precious metal. In this example, the catalyst layer 80 is a granular layer made of catalyst particles 81 containing a precious metal.
[0062] The precious metal is, for example, one or more of gold, silver, platinum, rhodium, palladium, and ruthenium. The catalyst layer 80 and the catalyst particles 81 may further contain metals other than the precious metal, such as titanium.
[0063] The plating method used to form the catalyst layer 80 is, for example, electrolytic plating, reduction plating, or displacement plating. Among these methods, displacement plating is particularly preferable because it allows metal to be deposited directly and almost uniformly on the area of the first main surface S1 that is not covered by the first layer 90.
[0064] However, in any plating method, the balance between the supply of metal from the plating solution and the consumption of metal due to its deposition is different between the region near the boundary between the first region A1 and the second region A2 and the region sufficiently separated from this boundary. Specifically, the region near the boundary between the first region A1 and the second region A2 is more likely to have metal deposited in the slit 90S than the region sufficiently separated from this boundary. Therefore, the catalyst layer 80 includes a first catalyst portion 80a where metal is deposited at an appropriate density and a second catalyst portion 80b where metal is deposited at a high density. As described later, the second catalyst portion 80b makes it easier for processing defects to occur.
[0065] 6 to 8, a second layer 95 is formed. Here, the second layer 95 includes a portion 95A extending along the length direction of the slits 90S and a portion 95B extending along the arrangement direction of the slits 90S.
[0066] The second layer 95 is a second mask layer that prevents an etching agent 100, which will be described later, from reaching the second catalyst portion 80b. The second layer 95 is formed so as to cover a portion of the catalyst layer 80 adjacent to the boundary between the first region A1 and the second region A2, and to expose a portion of the catalyst layer 80 away from the boundary. As a result, the second layer 95 covers the second catalyst portion 80b without covering at least a portion of the first catalyst portion 80a.
[0067] The second layer 95 is formed so that the width of the portion located on the first region A1, i.e., widths D1 and D2 in Fig. 8, is preferably within a range of 20 to 100 µm, more preferably within a range of 20 to 50 µm. Increasing this width ensures that the entire second catalyst portion 80b is covered with the second layer 95. However, increasing this width increases the portion of the first catalyst portion 80a that is covered with the second layer 95.
[0068] It should be noted that the widths D1 and D2 may be equal to each other. Alternatively, the widths D1 and D2 may be different. For example, the width D1 may be larger than the width D2.
[0069] The second layer 95 is preferably formed to have a thickness in the range of 0.1 to 10 μm, more preferably in the range of 0.5 to 1 μm. By making the second layer 95 thicker, the second catalyst portion 80b can be entirely covered with the second layer 95. However, making the second layer 95 thicker increases costs.
[0070] Examples of materials for the second layer 95 include organic materials such as polyimide, fluororesin, phenolic resin, acrylic resin, and novolac resin, and inorganic materials such as silicon oxide and silicon nitride.
[0071] The second layer 95 can be formed, for example, by an existing semiconductor process. The second layer 95 made of an organic material can be formed, for example, by photolithography. The second layer 95 made of an inorganic material can be formed, for example, by forming an inorganic material layer by a vapor phase deposition method, forming a mask by photolithography, and patterning the inorganic material layer by etching. The material of the second layer 95 is preferably an organic material.
[0072] During the formation of the second layer 95, the material of the second layer 95 may adhere to the portion of the first catalyst portion 80a that should not be covered by the second layer 95. Such adhesion reduces the catalytic activity. Therefore, after the formation of the second layer 95, it is preferable to remove the adhesion from the exposed portion of the first catalyst portion 80a, for example, by etching. For example, when an organic material is used as the material of the second layer 95, it is preferable to perform ashing. Note that when this treatment is performed on the structure of FIG. 6, the second layer 95 becomes thin, as shown in FIG. 7.
[0073] Next, the substrate 10 is etched under the catalytic action of the noble metal to form a recess in the first main surface S1.
[0074] 9, the substrate 10 is etched with an etching agent 100. For example, the substrate 10 is immersed in the liquid etching agent 100, and the etching agent 100 is brought into contact with the substrate 10.
[0075] The etchant 100 includes an oxidizer and hydrogen fluoride. The concentration of hydrogen fluoride in the etching agent 100 is preferably in the range of 1 mol / L to 20 mol / L, more preferably in the range of 5 mol / L to 10 mol / L, and even more preferably in the range of 3 mol / L to 7 mol / L. If the hydrogen fluoride concentration is low, it is difficult to achieve a high etching rate. If the hydrogen fluoride concentration is high, excessive side etching may occur.
[0076] The oxidizing agent may be selected from, for example, hydrogen peroxide, nitric acid, AgNO3, KAuCl4, HAuCl4, K2PtCl6, HPtCl6, Fe(NO3)3, Ni(NO3)2, Mg(NO3)2, Na2S2O8, K2S2O8, KMnO4, and K2Cr2O7. Hydrogen peroxide is preferred as the oxidizing agent because it does not generate harmful by-products and does not contaminate semiconductor elements.
[0077] The concentration of the oxidizing agent in the etching agent 100 is preferably in the range of 0.2 mol / L to 8 mol / L, more preferably in the range of 2 mol / L to 4 mol / L, and even more preferably in the range of 3 mol / L to 4 mol / L.
[0078] The etching agent 100 may further include a buffering agent, such as at least one of ammonium fluoride and ammonia. In one embodiment, the buffering agent is ammonium fluoride. In another embodiment, the buffering agent is a mixture of ammonium fluoride and ammonia. The etching agent 100 may further include other components, such as water.
[0079] When such an etching agent 100 is used, the material of the substrate 10, silicon in this case, is oxidized in the region of the substrate 10 where the etching agent 100 can reach and where the catalyst particles 81 are close to the substrate 10. The oxides thus produced are dissolved and removed by hydrofluoric acid. In contrast, the above reaction does not occur in the region of the substrate 10 where the catalyst particles 81 are not present nearby. Moreover, the above reaction does not occur in the region of the substrate 10 where the catalyst particles 81 are present nearby but where the etching agent 100 cannot reach due to the second layer 95. Therefore, only the portion where the etching agent 100 can reach and where the catalyst particles 81 are close to the substrate 10 is selectively etched.
[0080] As the etching proceeds, the catalyst particles 81 move toward the second main surface S2, where the same etching as described above occurs. As a result, as shown in Fig. 10, at the positions of the portions of the first catalyst portions 80a that are not covered by the second layer 95, etching proceeds in a direction perpendicular to the first main surface S1, from the first main surface S1 toward the second main surface S2.
[0081] In this manner, the recesses TR shown in FIG. 11 are formed in the first main surface S1.
[0082] Thereafter, the first layer 90, the second layer 95, and the catalyst layer 80 are removed from the substrate 10. Note that the first layer 90 may be removed from the substrate 10 after the catalyst layer 80 is formed and before the second layer 95 is formed.
[0083] Next, a conductive layer 20a shown in FIG. 2 is formed on the substrate 10 to obtain a conductive substrate CS. As described above, the conductive layer 20a is the lower electrode of the capacitor. The conductive layer 20a can be formed, for example, by doping the surface region of the substrate 10 with a high concentration of impurities. The conductive layer 20a made of polysilicon can be formed, for example, by LPCVD (low pressure chemical vapor deposition). The conductive layer 20a made of metal can be formed, for example, by electrolytic plating, reduction plating, or displacement plating.
[0084] The plating solution is a liquid containing a salt of the metal to be plated. As the plating solution, a common plating solution such as a copper sulfate plating solution containing copper sulfate pentahydrate and sulfuric acid, a copper pyrophosphate plating solution containing copper pyrophosphate and potassium pyrophosphate, and a nickel sulfamate plating solution containing nickel sulfamate and boron can be used.
[0085] The conductive layer 20a is preferably formed by a plating method using a plating solution containing a salt of the metal to be plated, a surfactant, and carbon dioxide in a supercritical or subcritical state. In this plating method, the surfactant is interposed between particles of supercritical carbon dioxide and a continuous phase of a solution containing the salt of the metal to be plated. That is, the surfactant is caused to form micelles in the plating solution, and the supercritical carbon dioxide is incorporated into these micelles.
[0086] In conventional plating methods, the supply of the plated metal to the vicinity of the bottom of the recess may be insufficient, especially when the ratio D / W of the depth D to the width or diameter W of the recess is large.
[0087] Micelles that incorporate supercritical carbon dioxide can easily enter narrow gaps. As these micelles move, the solution containing the salt of the metal to be plated also moves. Therefore, a plating method using a plating solution containing the salt of the metal to be plated, a surfactant, and carbon dioxide in a supercritical or subcritical state can easily form a conductive layer 20a with a uniform thickness.
[0088] As described above, here, as an example, the conductive layer 20a is formed by doping impurities at a high concentration into the surface region of the substrate 10. That is, here, the surface region on the first main surface S1 side of the substrate 10 is used as the conductive layer 20a.
[0089] Next, the dielectric layer 30 is formed on the conductive layer 20a. The dielectric layer 30 can be formed by, for example, chemical vapor deposition (CVD). Alternatively, the dielectric layer 30 can be formed by oxidizing, nitriding, or oxynitriding the surface of the conductive layer 20a.
[0090] Next, the conductive layer 20b is formed on the dielectric layer 30. As described above, the conductive layer 20b is the upper electrode of the capacitor. As the conductive layer 20b, for example, a conductive layer made of polysilicon or metal is formed. Such a conductive layer 20b can be formed, for example, by the same method as described above for the conductive layer 20a.
[0091] Next, an opening is formed in the dielectric layer 30. Here, a frame-shaped opening is formed in a portion of the dielectric layer 30 located on the first main surface S1. This opening can be formed, for example, by forming a mask by photolithography and patterning by etching.
[0092] Next, a metal layer is formed and patterned to obtain the first internal electrode 70a and the second internal electrode 70b. The first internal electrode 70a and the second internal electrode 70b can be formed, for example, by a combination of film formation by sputtering or plating and photolithography.
[0093] Thereafter, the insulating layer 60 is formed. The insulating layer 60 is opened at positions corresponding to parts of the first internal electrodes 70a and the second internal electrodes 70b. The insulating layer 60 can be formed, for example, by a combination of film formation by CVD and photolithography.
[0094] Next, the first external electrode 70c and the second external electrode 70d are formed on the insulating layer 60. Specifically, first, the first metal layers 70c1 and 70d1 are formed. Next, the second metal layers 70c2 and 70d2 are formed. The first metal layers 70c1 and 70d1 and the second metal layers 70c2 and 70d2 can be formed, for example, by a combination of film formation by sputtering or plating and photolithography.
[0095] The structure thus obtained is then diced, thus obtaining the capacitor 1 shown in Figs.
[0096] In this capacitor 1, a recess TR is provided in the first main surface S1, and a laminate structure including the dielectric layer 30 and the conductive layer 20b is provided not only on the first main surface S1 but also in the recess TR. Therefore, this capacitor 1 can achieve a large electric capacitance.
[0097] The above-mentioned method is less likely to cause processing defects in etching using a catalyst, as will be described below.
[0098] 4 and 5, the precious metal is more likely to be deposited in the slits 90S in the region near the boundary between the first region A1 and the second region A2 than in a region sufficiently away from the boundary. As a result, the catalyst layer 80 includes a first catalyst portion 80a in which the precious metal is deposited at an appropriate density and a second catalyst portion 80b in which the precious metal is deposited at a high density.
[0099] This is because the balance between the supply of metal from the plating solution and the consumption of metal due to its precipitation is different between the region near the boundary between the first region A1 and the second region A2 and the region sufficiently separated from this boundary. More specifically, this is because the first layer 90 does not have a slit 90S at the position of the second region A2, and therefore the area of the region to which the plating solution located near the boundary between the first region A1 and the second region A2 should supply metal is smaller than the area of the region to which the plating solution located sufficiently separated from this boundary should supply metal.
[0100] 9 and 10 is performed without forming the second layer 95, the etching proceeds in a direction perpendicular to the first main surface S1 in the region where the first catalyst portion 80a is formed. However, in this case, in the region where the second catalyst portion 80b is formed, the etching proceeds in a direction inclined with respect to the first main surface S1, the etching proceeds in a non-uniform direction, and etching in a direction perpendicular to the first main surface S1 is not efficiently performed, resulting in processing defects. As a result, for example, the structure shown in FIG. 12 is obtained.
[0101] When the second layer 95 is formed, the supply of the etching agent 100 to the second catalyst portion 80b is prevented. Therefore, etching does not proceed at the position corresponding to the second layer 95, and the above-mentioned processing defect does not occur. Therefore, for example, the structure shown in FIG. 13 is obtained.
[0102] <Second embodiment> An etching method according to a second embodiment includes the steps of: forming a mask layer on a substrate including a semiconductor material and having a first region and a second region adjacent to each other on one main surface; the mask layer including a first portion covering the first region and having a plurality of openings or one or more openings defining a plurality of island-shaped portions, and a second portion which is a continuous film covering the second region, the mask layer including a first portion having a plurality of openings or one or more openings defining a plurality of island-shaped portions, the second portion being a greater height based on the main surface of the second portion at a position adjacent to a boundary between the first region and the second region than a height based on the main surface of the first portion; forming a catalyst layer including a precious metal by a plating method on portions of the main surface exposed within the plurality of openings or the one or more openings; and etching the substrate with an etching agent including an oxidizing agent and hydrogen fluoride in the presence of the catalyst layer and the mask layer.
[0103] The method for producing a structure according to the second embodiment includes forming one or more recesses in the substrate by the above-mentioned etching method.
[0104] A method for manufacturing a semiconductor device according to the second embodiment includes forming one or more recesses in the substrate by the above-mentioned etching method, forming a lower electrode on a sidewall of the one or more recesses, forming a dielectric layer on the lower electrode, and forming an upper electrode on the dielectric layer.
[0105] Hereinafter, a method for manufacturing a capacitor, which is an example of a semiconductor device, as a structure using the above-mentioned etching method will be described.
[0106] According to the method of the second embodiment, for example, it is possible to manufacture the capacitor 1 exemplified in the first embodiment. In the second embodiment, this capacitor 1 is manufactured by the following method.
[0107] 14, a mask layer 98 is formed on the first main surface S1 of the substrate 10. The substrate 10 is similar to that described in the first embodiment.
[0108] The mask layer 98 includes a first portion 98a and a second portion 98b. The first portion 98a is a portion of the mask layer 98 that covers the first region A1. The first portion 98a has a plurality of openings. Here, the plurality of openings are a plurality of slits 90S arranged in the width direction. The length direction of the slits 90S is parallel to the Y direction, and the slits 90S are arranged in the X direction.
[0109] The multiple openings provided in the first portion 98a may have a shape other than slits. For example, the multiple openings in the first portion 98a may be multiple through holes arranged in two intersecting directions, each of which has a circular, elliptical, or polygonal shape.
[0110] Alternatively, instead of providing a plurality of openings in the first portion 98a, one or more openings defining a plurality of island-shaped portions may be provided, in which case pillar-shaped protrusions can be formed at positions corresponding to the island-shaped portions by etching, which will be described later.
[0111] The second portion 98b is a portion of the mask layer 98 that covers the second region A2. The second portion 98b is a continuous film. The height H2 of the second portion 98b at a position adjacent to the boundary between the first region A1 and the second region A2 with respect to the first main surface S1 is A or H2 B is larger than the height H1 of the first portion 98a measured from the first main surface S1.
[0112] The mask layer 98 here is a laminate of a first layer 90 and a second layer 96 shown in Figures 14 and 15. The first portion 98a is a portion of the first layer 90 that covers the first region A1. The second portion 98b is a combination of the second layer 96 and a portion of the first layer 90 that covers the second region A2.
[0113] The first layer 90 is formed on the first main surface S1. The first layer 90 is similar to that described in the first embodiment. That is, the first layer 90 plays a role similar to that described in the first embodiment.
[0114] The first layer 90 covers the first region A1 and the second region A2. A plurality of openings are provided in the portion of the first layer 90 covering the first region A1. Here, the plurality of openings are a plurality of slits 90S arranged in the width direction. The length direction of the slits 90S is parallel to the Y direction and arranged in the X direction.
[0115] The multiple openings provided in the first layer 90 may have a shape other than slits. For example, the first layer 90 may be provided with multiple through holes arranged in two intersecting directions, each of which has a circular, elliptical, or polygonal shape as the multiple openings. Alternatively, instead of providing multiple openings in the first layer 90, one or more openings that define multiple island-shaped portions may be provided.
[0116] The portion of the first layer 90 that covers the second region A2 is a continuous film. The portion of the first layer 90 that covers the second region A2 has the same height as the portion of the first layer 90 that covers the first region A1.
[0117] The materials exemplified in the first embodiment can be used for the first layer 90. The first layer 90 can be formed by, for example, the same method as that described in the first embodiment.
[0118] The second layer 96 is formed on the first layer 90. The second layer 96 exposes the portion of the first layer 90 that covers the first region A1. The second layer 96 covers the second region A2 of the first layer 90 at least at a position adjacent to the boundary between the first region A1 and the second region A2. Here, the second layer 96 has a frame shape that surrounds the first region A1.
[0119] The material of the second layer 96 may be, for example, the material exemplified for the second layer 95 in the first embodiment. The second layer 96 may be formed, for example, by the same method as that described for the second layer 95 in the first embodiment.
[0120] As described later, the second layer 96 prevents an excessive supply of metal from the plating solution to the first main surface S1 in the region near the boundary between the first region A1 and the second region A2 during plating to form the catalytic layer 80. This makes it possible to make the density of the catalytic metal approximately equal in the slits 90S near the boundary between the first region A1 and the second region A2 and in the slits 90S sufficiently separated from this boundary.
[0121] The mask layer 98 may be formed integrally. For example, first, a photosensitive resin layer is formed on the first layer 90. For example, a positive photoresist is used as the photosensitive resin. Next, the photosensitive resin layer is exposed to light using, for example, a grating mask, or exposed two or more times. This causes first and second exposed portions with different amounts of exposure and an unexposed portion to be generated in the photosensitive resin layer. Thereafter, development or the like is performed to obtain the mask layer 98 formed integrally.
[0122] A height H2 of the second portion 98b at a position adjacent to the boundary with respect to a height H1 of the first portion 98a with respect to a first main surface S1. A or H2 B The ratio is preferably in the range of 2 to 5, and more preferably in the range of 2 to 3.
[0123] Here, the height H1 is the thickness of the first layer 90. Also, the height H2 A is the height of the second portion 98b at a position adjacent to the portion of the boundary extending along the length direction of the slit 90S, with the first main surface S1 of the second portion 98b as the reference. A is the height of the portion 96A of the second layer 96 extending along the length direction of the slit 90S, based on the first main surface S1. B is a height based on the first main surface S1 of the second portion 98b at a position adjacent to a portion of the boundary extending along the arrangement direction of the slits 90S. B is the height of a portion 96B of the second layer 96 extending along the arrangement direction of the slits 90S, with respect to the first main surface S1.
[0124] In addition, the distance D in the direction parallel to the first main surface S1 from the part of the second portion 98b that has the greatest height relative to the first main surface S1 to the multiple openings or one or more openings is A Or D B The height H of the second portion 98b relative to the first portion 98a A Or H B The ratio is preferably in the range of 1 to 4, and more preferably in the range of 2 to 4).
[0125] Here, the distance D A is the distance in the arrangement direction of the slits 90S from a portion 96A of the second layer 96 extending along the length direction of the slits 90S to the slits 90S. Bis the distance in the longitudinal direction of the slits 90S from a portion 96B of the second layer 96 extending along the arrangement direction of the slits 90S to the slits 90S.
[0126] Here, the height H A is the height of the second portion 98b with respect to the first portion 98a at a position adjacent to the portion of the boundary extending along the length direction of the slit 90S. That is, here, the height H A is the thickness of the portion of the second layer 96 extending along the length of the slit 90S. B is the height of the second portion 98b with respect to the first portion 98a at a position adjacent to the portion of the boundary extending along the arrangement direction of the slits 90S. B is the thickness of the portion of the second layer 96 extending along the arrangement direction of the slits 90S.
[0127] If these ratios are increased, in the plating process for forming the catalyst layer 80, the amount of metal supplied from the plating solution to the first main surface S1 in the region near the boundary between the first region A1 and the second region A2 decreases.
[0128] The height H1 is preferably in the range of 0.1 to 10 μm, and more preferably in the range of 0.5 to 1 μm.
[0129] Height H2 A and H2 B The height H2 is preferably in the range of 0.2 to 20 μm, and more preferably in the range of 1 to 3 μm. A and H2 B may be equal to each other or may be different.
[0130] Height H A and H B is preferably in the range of 0.1 to 10 μm, and more preferably in the range of 0.5 to 2 μm. A and H B may be equal to each other or may be different.
[0131] Distance D A and D. B The distance D is preferably in the range of 0.05 to 0.5 μm, and more preferably in the range of 0.1 to 0.2 μm. A and D. B may be equal to each other or may be different.
[0132] After the mask layer 98 is formed as described above, the catalyst layer 80 is formed on the portion of the first main surface S1 exposed in the slit 90S, as shown in Fig. 16. The catalyst layer 80 may be made of the material exemplified in the first embodiment. The catalyst layer 80 may be formed by the same method as that described in the first embodiment.
[0133] 17, the substrate 10 is etched with an etching agent 100 containing an oxidizing agent and hydrogen fluoride in the presence of the catalyst layer 80 and the mask layer 98. As a result, recesses TR are formed in the first main surface S1.
[0134] For example, the etching agent 100 exemplified in the first embodiment can be used. This etching is performed, for example, by the same method as that described in the first embodiment.
[0135] Next, the mask layer 98 and the catalyst layer 80 are removed from the substrate 10. Thereafter, as described in the first embodiment, the conductive layer 20a, the dielectric layer 30, and the conductive layer 20b are formed. Furthermore, as described in the first embodiment, the first internal electrode 70a, the second internal electrode 70b, the insulating layer 60, the first external electrode 70c, and the second external electrode 70d are formed, and dicing is performed. In this manner, the capacitor 1 shown in FIGS. 1 and 2 is obtained.
[0136] In this capacitor 1, a recess TR is provided in the first main surface S1, and a laminate structure including the dielectric layer 30 and the conductive layer 20b is provided not only on the first main surface S1 but also in the recess TR. Therefore, this capacitor 1 can achieve a large electric capacitance.
[0137] As described above, in this method, the second layer 96 prevents an excessive supply of metal from the plating solution to the first main surface S1 in the region near the boundary between the first region A1 and the second region A2 during plating to form the catalytic layer 80. This makes it possible to make the density of the catalytic metal substantially equal in the slits 90S near the boundary between the first region A1 and the second region A2 and in the slits 90S sufficiently separated from this boundary. Therefore, similar to the first embodiment, it is possible to make it difficult for processing defects to occur in etching using a catalyst.
[0138] The methods described in the first and second embodiments can be modified in various ways. For example, in the first and second embodiments, a capacitor has been described as an example of a structure, but the techniques described above regarding a capacitor can also be applied to other structures.
[0139] In the methods described in the first and second embodiments, prior to forming the catalyst layer 80, the height of the portion of the first region A1 corresponding to the slit 90S may be made higher than the height of the remaining portion of the first region A1. For example, the height of the portion of the first region A1 not covered with the first layer 90 may be reduced by etching. Alternatively, the height of the portion of the first region A1 corresponding to the slit 90S may be increased by epitaxial growth. In this way, variation in the etching progress direction is less likely to occur.
[0140] In the method described in the second embodiment, the second layer 96 is formed so as to extend along the entire boundary between the first region A1 and the second region A2. A portion 96B of the second layer 96 extending along the arrangement direction of the slits 90S may be provided only in the vicinity of a portion 96A of the second layer 96 extending along the length direction of the slits 90S, as shown in FIG.
[0141] When the recesses TR are trenches, the protrusions between adjacent recesses TR have a partition wall shape. In this case, if processing defects occur over the entire length of a certain recess TR during etching to form the recesses TR, the protrusions adjacent to that recess TR may collapse. On the other hand, even if processing defects occur only at the end of a certain recess TR during etching to form the recesses TR, the protrusions adjacent to that recess TR are unlikely to collapse.
[0142] Therefore, even when the structure shown in FIG. 18 is adopted, it is possible to make it difficult for the convex portions sandwiched between adjacent concave portions TR to collapse during etching for forming the concave portions TR.
[0143] The present invention is not limited to the above-described embodiment as it is, and the components can be modified and embodied in the implementation stage without departing from the gist of the invention. In addition, various inventions can be formed by appropriately combining the multiple components disclosed in the above-described embodiment. For example, some components may be deleted from all the components shown in the embodiment. Furthermore, components from different embodiments may be appropriately combined. [Explanation of symbols]
[0144] Reference Signs List 1...capacitor, 10...substrate, 20a...conductive layer, 20b...conductive layer, 30...dielectric layer, 60...insulating layer, 70a...first internal electrode, 70b...second internal electrode, 70c...first external electrode, 70c1...first metal layer, 70c2...second metal layer, 70d...second external electrode, 70d1...first metal layer, 70d2...second metal layer, 80...catalyst layer, 80a...first catalyst portion , 80b...second catalyst portion, 81...catalyst particle, 90...first layer, 90S...slit, 95...second layer, 95A...portion, 95B...portion, 96...second layer, 96A...portion, 96B...portion, 98...mask layer, 98a...first portion, 98b...second portion, 100...etching agent, A1...first region, A2...second region, CS...conductive substrate, D1...width, D2...width, D A …distance, D B …distance, H1…height, H2 A …height, H2 B …Height, HA …Height, H B ...height, S1...first main surface, S2...second main surface, TR...recess.
Claims
1. forming a first layer on a substrate including a semiconductor material and having a first region and a second region adjacent to each other on one main surface, the first region and the second region being covered, the first layer having a plurality of openings or one or more openings defining a plurality of island-shaped portions in a portion covering the first region, and the second region being a continuous film; forming a catalytic layer including a precious metal on the plurality of openings or on a portion of the main surface exposed in the one or more openings by a plating method; forming a second layer that covers a portion of the catalyst layer adjacent to the boundary between the first region and the second region and exposes a portion of the catalyst layer away from the boundary; Etching the substrate in the presence of the catalyst layer and the second layer with an etching agent comprising an oxidizing agent and hydrogen fluoride; An etching method comprising:
2. The etching method according to claim 1 , wherein the first layer is provided with a plurality of slits arranged in a width direction as the plurality of openings.
3. 3. The etching method according to claim 1, wherein the substrate is etched in the presence of the first layer in addition to the catalyst layer and the second layer.
4. 4. The etching method according to claim 1, wherein the second layer is formed so that a width of a portion located on the first region is within a range of 20 to 100 [mu]m.
5. forming a mask layer on a substrate including a semiconductor material and having a first region and a second region adjacent to each other on one main surface, the mask layer including a first portion covering the first region and having a plurality of openings or one or more openings defining a plurality of island-shaped portions, and a second portion being a continuous film covering the second region, the mask layer having a height of the second portion relative to the main surface at a position adjacent to a boundary between the first region and the second region that is greater than a height of the first portion relative to the main surface; forming a catalytic layer including a precious metal on the plurality of openings or on a portion of the main surface exposed in the one or more openings by a plating method; Etching the substrate with an etching agent including an oxidizing agent and hydrogen fluoride in the presence of the catalyst layer and the mask layer. An etching method comprising:
6. The etching method according to claim 5 , wherein the mask layer is provided with a plurality of slits arranged in a width direction as the plurality of openings.
7. The formation of the mask layer includes: forming a first layer on the substrate, the first layer covering the first region and the second region, the first layer being provided with the plurality of openings or the one or more openings defining the plurality of island-shaped portions in the portion covering the first region, and the second layer being a continuous film in the portion covering the second region; exposing the portion of the first layer that covers the first region, and forming a second layer that covers the second region of the first layer at least at a position adjacent to the boundary; The etching method according to claim 5 or 6, comprising:
8. 8. The etching method according to claim 5, wherein a ratio of the height of the second portion from the main surface at a position adjacent to the boundary to the height of the first portion from the main surface is in the range of 2 to 5.
9. 9. The etching method according to claim 5, wherein a ratio of a height of the second portion relative to the first portion to a distance in a direction parallel to the main surface from a part of the second portion that has the greatest height relative to the main surface to the multiple openings or the one or more openings is within a range of 1 to 4.
10. 10. The etching method according to claim 1, wherein a granular layer made of particles containing the noble metal is formed as the catalyst layer.
11. A method for manufacturing a structure, comprising forming one or more recesses in the substrate by the etching method according to claim 1 .
12. forming one or more recesses in the substrate by the etching method according to any one of claims 1 to 10; forming a bottom electrode on a sidewall of the one or more recesses; forming a dielectric layer on the lower electrode; forming a top electrode on the dielectric layer; A method for manufacturing a semiconductor device comprising the steps of:
Citation Information
Patent Citations
Single-crystal substrate
JP2011101009A
Porous and non-porous nanostructures
JP2013527103A
Capacitor
JP2020119936A
Etching method, manufacturing method of semiconductor chip and manufacturing method of article
JP2021002689A
Self-Anchored Catalyst Metal-Assisted Chemical Etching
US20170243751A1