Process for removing reactive solvents from lithium bis(fluorosulfonyl)imide (LIFSI) using organic solvents that are stable towards lithium ion and lithium metal battery anodes

The use of anhydrous organic solvents and vacuum treatment effectively removes reactive solvents and impurities from LiFSI, producing ultra-high purity LiFSI that improves battery performance and cycle life by preventing anode degradation.

JP7555921B2Active Publication Date: 2024-09-25SES HLDG PTE LTD
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2021526413
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-09-13
Filing Date
2019-11-15
Publication Date
2024-09-25
Estimated Expiration
2039-11-15

AI Technical Summary

Technical Problem

Existing methods for purifying lithium bis(fluorosulfonyl)imide (LiFSI) struggle to effectively remove reactive solvents and impurities, particularly those that are reactive towards lithium metal anodes, leading to performance issues in lithium-ion and lithium metal batteries.

Method used

A method involving the use of anhydrous organic solvents to reduce reactive solvents and impurities through vacuum treatment, filtration, and solvent displacement, followed by isolation and drying under inert conditions to produce ultra-high purity LiFSI suitable for lithium-based batteries.

Benefits of technology

The method achieves LiFSI with extremely low levels of reactive solvents and impurities, enhancing the performance and cycle life of lithium-ion and lithium metal batteries by preventing adverse reactions with lithium metal anodes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007555921000006
    Figure 0007555921000006
  • Figure 0007555921000007
    Figure 0007555921000007
  • Figure 0007555921000008
    Figure 0007555921000008
Patent Text Reader

Abstract

Methods for producing high-purity LiFSI salts and intermediate products using one, the other, or both of a reactive solvent removal / replacement method and a LiFSI purification method. In some embodiments, the reactive solvent removal / replacement method comprises using a non-reactive anhydrous organic solvent to remove and / or replace one or more reactive solvents in crude LiFSI. In some embodiments, the LiFSI purification method comprises using an anhydrous organic solvent to remove impurities, such as synthetic impurities, from crude LiFSI. In some embodiments, crude LiFSI can be produced using an aqueous neutralization process. LiFSI salts and products produced using the methods of the present disclosure are also described, as are uses of such salts and products and electrochemical devices comprising such salts and products.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] Related Application Data This application is a continuation-in-part of U.S. Nonprovisional Application No. 16 / 570,262, filed September 13, 2019, and entitled "PURIFIED LITHIUM BIS(FLUOROSULFONYL)IMIDE (LiFSI) PRODUCTS, METHODS OF PURIFYING CRUDE LiFSI, AND USES OF PURIFIED LiFSI PRODUCTS," which is incorporated herein by reference in its entirety. This application also claims the benefit of priority to the following applications, each of which is incorporated herein by reference in its entirety: U.S. Provisional Patent Application No. 62 / 883,177, filed August 6, 2019, entitled “PROCESS FOR PRODUCING ULTRAPURE LITHIUM BIS(FLUOROSULFONYL)IMIDE(LiFSI) FOR LITHIUM METAL ANODE BATTERIES APPLICATIONS”; U.S. Provisional Patent Application No. 62 / 883,178, filed August 6, 2019, entitled “PROCESS FOR REMOVING REACTIVE SOLVENT FROM LITHIUM BIS(FLUOROSULFONYL)IMIDE(LIFSI) USING ORGANIC SOLVENTS THAT ARE STABLE TOWARD ANODES IN LITHIUM-ION AND LITHIUM-METAL BATTERIES”; U.S. Provisional Patent Application No. 62 / 840,949, filed April 30, 2019, entitled “PROCESS FOR REMOVING PROTIC SOLVENTS FROM LITHIUM BIS(FLUORO-SULFONYL)IMIDE (LiFSI)”; U.S. Provisional Patent Application No. 62 / 768,447, filed on November 16, 2018, entitled “PROCESS FOR THE PURIFICATION OF LITHIUM BIS(FLUOROSULFONYL)IMIDE (LiFSI).”

[0002] The present invention relates generally to the field of lithium sulfonimide salts for electrolytes for lithium-based electrochemical devices. In particular, the present invention relates to a process for removing reactive solvents from lithium bis(fluorosulfonyl)imide (LiFSI) using organic solvents that are stable towards lithium-ion and lithium metal battery anodes. [Background technology]

[0003] Lithium bis(fluorosulfonyl)imide (LiFSI) has been reported as a conductive salt for lithium-based batteries due to its desirable physicochemical and electrochemical properties. LiFSI has a melting point of 143 °C and is thermally stable up to 200 °C. LiFSI exhibits much better stability against hydrolysis compared to lithium hexafluorophosphate (LiPF6), a salt commonly used in electrolytes for lithium-ion batteries. LiFSI has attracted great interest as an electrolyte / additive for lithium-ion batteries due to its unique properties such as excellent solubility, ionic conductivity comparable to LiPF6-based electrolytes, cost-effectiveness, environmental friendliness, and good solid electrolyte interface (SEI) formation properties. The purity level of LiFSI used in battery electrolytes can be critical for the operation and cycle life of batteries using LiFSI-based electrolytes. However, many commercial processes for synthesizing LiFSI produce by-products that remain in the crude LiFSI produced by the synthesis process. The main synthetic impurities in LiFSI are lithium fluoride (LiF), lithium chloride (LiCl), lithium sulfate (Li2SO4), lithium fluorosulfonate (LiFSO3), and acid-type impurities such as hydrogen fluoride (HF). These impurities must be removed or reduced to various acceptable levels before using the LiFSI salt in batteries. However, removing them can be difficult.

[0004] Some processes for removing impurities such as the synthetic impurities listed above from crude LiFSI utilize one or more solvents that are reactive towards lithium metal, such as alcohol(s) and water. Also, crude LiFSI may contain water by means other than the solvent. Thus, even if such LiFSI is purified to a point where the levels of the target synthetic impurities are low enough that they do not interfere with the function of the electrochemical device when the purified LiFSI is placed in the electrolyte of the device, the purified LiFSI may still be unsuitable for use in a secondary lithium metal battery. This is because the purified LiFSI contains residues of the reactive solvent used to remove the target impurities and / or water that may otherwise be present, and the reactive solvent residues and / or water react with the lithium metal of the anode of the device, thereby destroying the integrity of the lithium metal and the ability of the anode to function properly. Over time, even a relatively small amount of reactive solvent(s) in the LiFSI salt used to make the electrolyte can significantly affect the performance and cycle life of a secondary lithium metal battery.

[0005] There is a need for ultra-high purity LiFSI salts that not only have very low levels of synthetic impurities, but also have very low levels of reactive solvents. Summary of the Invention

[0006] In one embodiment, the present disclosure relates to a method for producing a reduced-reactive-solvent lithium bis(fluorosulfonyl) imide (LiFSI) product. The method includes providing a first crude LiFSI containing LiFSI and one or more reactive solvents; contacting the first crude LiFSI with at least one first anhydrous organic solvent under inert conditions to produce a solution containing the first crude LiFSI and the one or more reactive solvents, wherein the solubility of LiFSI in the at least one first anhydrous organic solvent is at least about 35% at less than 25° C.; subjecting the solution to a vacuum to remove the at least one first anhydrous organic solvent and the one or more reactive solvents to obtain a solid mass; treating the solid mass with at least one second anhydrous organic solvent in which LiFSI is insoluble to produce a combination having an insoluble portion; isolating the insoluble portion in an inert atmosphere; flushing the insoluble portion with at least one dry inert gas to remove traces of the at least one second anhydrous organic solvent; and subjecting the flushed insoluble portion to a pressure of less than about 100 Torr to obtain a reactive solvent reduced LiFSI product.

[0007] For the purpose of illustrating the invention, the drawings show aspects of one or more embodiments of the invention, it being understood, however, that the invention is not limited to the precise arrangements and instrumentalities shown in the drawings. [Brief description of the drawings]

[0008] [Figure 1] 1 is a flow diagram illustrating a multi-pass method for reducing reactive solvent in lithium bis(fluorosulfonyl)imide (LiFSI) according to an embodiment of the present disclosure.

[0009] [Diagram 2] FIG. 1 is a high-level diagram illustrating an electrochemical device made according to an embodiment of the present disclosure.

[0010] [Diagram 3] 1 is a flow diagram illustrating a multi-pass method for purifying LiFSI according to an embodiment of the present disclosure.

[0011] [Figure 4A] 1 is a graph of discharge capacity versus cycle number for a non-aqueous electrolyte utilizing a LiFSI salt synthesized according to an embodiment of the present disclosure (top line) and a similar non-aqueous electrolyte utilizing a commercially available LiFSI salt (bottom line).

[0012] [Figure 4B] 1 is a graph of capacity retention versus cycle number for a non-aqueous electrolyte utilizing a LiFSI salt synthesized according to an embodiment of the present disclosure (top line) and a similar non-aqueous electrolyte utilizing a commercially available LiFSI salt (bottom line). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] In some embodiments, the present disclosure relates to a method for removing one or more reactive solvents from crude lithium bis(fluorosulfonyl)imide (LiFSI). As used herein and in the appended claims, unless otherwise specified, the use of the term "reactive" to modify "solvent" or "solvents" or the like shall mean that the solvent(s) are reactive to lithium metal in a lithium-based battery, for example, lithium metal in the anode of a lithium metal battery. As one skilled in the art will appreciate, "reactive" in this context refers to the magnitude of the reduction potential of lithium metal relative to the solvent(s). A reactive solvent has a reactive proton that has a relatively high reduction potential relative to lithium metal that has a relatively low reduction potential. Examples of reactive solvents include protic solvents, such as water, and reactive organic solvents, such as alcohols. Conversely, as used herein and in the appended claims, unless otherwise specified, the use of the term "non-reactive" to modify "solvent" or "solvents" or the like shall mean that the solvent(s) are non-reactive to lithium metal. Also, the reactive solvent(s) are not effective at passivating lithium metal, while the non-reactive solvent(s) are non-reactive with respect to lithium metal or effectively passivate lithium metal, i.e., render the electrolyte / lithium anode system kinetically stable. Examples of non-reactive solvents include dimethyl carbonate, ethyl methyl carbonate, diethyl carbonate, fluorine-containing carbonates, and glycol ethers.

[0014] As used herein and in the appended claims, the term "crude" and similar terms when referring to LiFSI refers to a synthesis product that includes at least LiFSI and one or more reactive solvents, such as reactive solvents resulting from the synthesis and / or purification of LiFSI or present in LiFSI. The presence of reactive solvent(s) in LiFSI salts used in electrolytes for lithium-ion and lithium-metal batteries can adversely affect the cycling performance, such as discharge capacity and capacity retention, of such batteries. It is therefore desirable to remove as much of the reactive solvent(s) present in the LiFSI salt as possible. Such reactive solvents may also be referred to herein and in the appended claims as "solvent residue" or "solvent residues." Crude LiFSI may contain additional impurities, such as the impurities described below in Section II.

[0015] As used herein and in the appended claims, the term "anhydrous" refers to having about 1% or less water by weight, typically about 0.5% or less water, often about 0.1% or less water by weight, more frequently about 0.01% or less water by weight, and most frequently about 0.001% or less water by weight. Within this definition, the term "substantially anhydrous" refers to having about 0.1% or less water by weight, typically about 0.01% or less water by weight, and often about 0.001% or less water by weight.

[0016] Throughout this disclosure, the term "about" when used in conjunction with a corresponding numerical value refers to ±20% of the numerical value, typically ±10% of the numerical value, often ±5% of the numerical value, and most frequently ±2% of the numerical value. In some embodiments, the term "about" can refer to the numerical value itself.

[0017] When describing a chemical reaction, such as any of the synthesis and purification reactions described herein and / or addressed in the appended claims, the terms "treating," "contacting," and "reacting" are used interchangeably and refer to the addition or mixing of two or more reagents under conditions sufficient to produce the indicated and / or desired product(s). It is understood that the reaction that produces the indicated and / or desired product does not necessarily result directly from the combination of the initially added reagent(s). That is, there may be one or more intermediates that are produced in the mixture and ultimately result in the formation of the indicated and / or desired product.

[0018] On a commercial scale, crude LiFSI usually contains one or more reactive solvent residues, such as methanol, ethanol or water, originating from the solvent source from which LiFSI is synthesized or purified. These reactive solvent residues are known to solvate very strongly with alkali metal salts and are difficult to remove by suction under vacuum without heating to high temperatures. However, LiFSI is unstable to heating at high temperatures in the presence of reactive solvents, and high heat causes defluorination of LiFSI to produce hydrogen fluoride (HF), a strong acid known to be corrosive. The following scheme illustrates the defluorination of LiFSI with protic solvents upon heating. [ka]

[0019] All protic solvents are also prone to undergo proton reduction to produce hydrogen gas, and they are generally only used for reductive electrochemistry with electrodes such as mercury or carbon where proton reduction is kinetically slow. Protic solvents also react with lithium metal present in lithium-based batteries, and in particular with the lithium metal anode of a lithium metal battery to produce hydrogen gas according to the following scheme: [ka]

[0020] While the above details relate to LiFSI, it should be noted that the same or similar issues with reactive solvents exist for crude lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), particularly crude LiTFSI produced using commercial scale processes. As a result, the general methodology for reducing the amount of each of the one or more reactive solvents described herein for crude LiFSI also relates to crude LiTFSI.

[0021] In another aspect, the present disclosure relates to a reduced-reactive-solvent LiFSI product that contains LiFSI and a relatively low level of one or more reactive solvents, such as one or more reactive solvents used in the synthesis and / or purification of crude LiFSI. Examples of reactive solvents that may be present in crude LiFSI or LiTFSI include water, methanol, ethanol, and propanol, among others, alone or in various combinations with each other. As described in more detail below, such a reduced-reactive-solvent LiFSI product can be produced using the reactive solvent reduction method of the present disclosure, which can produce a reduced-reactive-solvent LiFSI product in a single pass through one of the disclosed basic processes, or in multiple passes through one or more of the disclosed basic processes.

[0022] In yet another aspect, the present disclosure relates to the use of the LiFSI salt product of the present disclosure.For example, the LiFSI salt product of the present disclosure can be used to produce electrolytes that can be used in any suitable electrochemical device, such as batteries or supercapacitors, particularly secondary lithium ion batteries and secondary lithium metal batteries.

[0023] While in some embodiments, removal of reactive solvent(s) and / or replacement of reactive solvent(s) with non-reactive solvent(s) using the methods disclosed herein may be sufficient for certain uses of LiFSI (or LiTFSI), in other cases, it may be beneficial to apply the reactive solvent removal / replacement methods of the present disclosure to a higher purity LiFSI product than LiFSI products available by other methods. Two routes to provide such high purity LiFSI, which are specifically addressed below, are a method of removing non-solvent impurities from crude LiFSI, and a method of synthesizing crude LiFSI using an aqueous neutralization process. As a result, as described below, additional aspects of the present disclosure include these methods and processes, as well as various combinations of two or more of the methods disclosed herein, their associated intermediate and end products, and their uses, which are described immediately below.

[0024] In some additional aspects, the present disclosure relates to a method for purifying crude LiFSI to remove any one or more of various non-solvent impurities from the crude LiFSI. When used in the context of non-solvent impurity removal and in the appended claims, the term "crude LiFSI" and similar terms refer to a synthesis product that includes at least LiFSI and one or more non-solvent impurities, such as non-solvent impurities resulting from the synthesis of LiFSI. Hereinafter and in the appended claims, this type of impurity is referred to as a "synthetic impurity." Each of the targeted impurities that are removed to some degree or another using the disclosed methods is referred to herein and in the appended claims as a "target impurity." In one example, the target impurity may be a synthetic impurity that is a by-product of the synthesis of LiFSI, as described above.

[0025] On a commercial scale, crude LiFSI is generally obtained by neutralizing hydrogen bis(fluorosulfonyl)imide (HFSI), which contains various concentrations of synthetic impurities such as hydrogen fluoride (HF), fluorosulfuric acid (FSO3H), hydrogen chloride (HCl), and sulfuric acid (H2SO4), with lithium carbonate (Li2CO3) or lithium hydroxide (LiOH). Using a LiOH-based synthesis as an example, during this process of producing crude LiFSI, HFSI and impurities such as HF, FSO3H, HCl, and H2SO4 are converted to the corresponding Li salts to produce LiFSI, Li2SO4, FSO3Li, LiF, and LiCl, respectively, according to the following scheme: [ka] In this example, Li2SO4, FSO3Li, LiF, and LiCl are the target impurities (here, synthetic impurities) that are desired to be removed from crude LiFSI. In some embodiments, the purification methods of the present disclosure remove one or more synthetic impurities, such as one or more of Li2SO4, FSO3Li, LiF, and LiCl, and / or any other impurities having molecular structures and properties suitable for removal by the disclosed methods, each of which is a "target impurity" in the terminology of the present disclosure.

[0026] In another aspect, the present disclosure relates to a purified LiFSI product that contains LiFSI and relatively low levels of one or more target impurities, such as one or more synthetic impurities, such as Li2SO4, FSO3Li, LiF, and LiCl, as described in more detail below. Such purified LiFSI products can be produced using the purification methods of the present disclosure, which can produce the purified LiFSI product in a single pass through one of the disclosed basic processes, or in multiple passes through one or more of the disclosed basic processes.

[0027] In yet another aspect, the present disclosure relates to the use of the LiFSI salt product of the present disclosure.For example, the LiFSI salt product of the present disclosure can be used to produce electrolytes that can be used in any suitable electrochemical device, such as batteries or supercapacitors.

[0028] In yet another aspect, the present disclosure relates to a method for synthesizing LiFSI using an aqueous neutralization method followed by removal of impurities. As described in more detail below, one exemplary LiFSI synthesis method includes neutralizing hydrogen bis(fluorosulfonyl)imide (HFSI) (e.g., purified HFSI) with one or more lithium bases in deionized water to obtain an aqueous solution of LiFSI and one or more synthetic impurities. Additional steps may include removing at least a portion of the deionized water to obtain crude LiFSI, and then purifying the crude LiFSI to remove at least a portion of the one or more synthetic impurities.

[0029] In yet further aspects, the present disclosure relates to carrying out any one of the various combinations of the various methods disclosed herein. For example, the overall process can include synthesizing LiFSI using the aqueous neutralization synthesis method of the present disclosure, followed by carrying out either the non-reactive solvent purification process of the present disclosure or the reactive solvent reduction / replacement method of the present disclosure, or a combination of the two, using the synthesized LiFSI. If both additional methods are used, it is generally preferred to carry out the reactive solvent reduction / replacement method last, especially if any reactive solvent is used in the non-reactive solvent purification process. As another example, the overall process can include starting with already synthesized crude LiFSI, such as commercially supplied, conventionally synthesized crude LiFSI, and then carrying out one, the other, or both of the non-reactive solvent purification process of the present disclosure or the reactive solvent reduction / replacement method of the present disclosure.

[0030] In still further aspects, the present disclosure relates to purified LiFSI products containing LiFSI produced using any one of the method combinations described in the immediately preceding paragraph, electrolytes produced using the purified LiFSI salt produced using any one of the method combinations described in the immediately preceding paragraph, and uses of such electrolytes.

[0031] Details of these and other aspects of the disclosure are set forth below.

[0032] I. Removal / replacement of reactive solvent(s)

[0033] This section covers methods for removing and / or replacing reactive solvent in lithium sulfonimide salts, the reactive solvent-reduced lithium sulfonimide salts produced thereby, and uses of such reactive solvent-reduced lithium sulfonimide salts.

[0034] Exemplary Methods for Removing / Replacing Reactive Solvent(s) in IA Crude LiFSI

[0035] As noted above, crude LiFSI may contain one or more reactive solvents, for example, as residuals from the synthesis and / or purification of LiFSI. The reactive solvent removal method of the present disclosure may be used to reduce, including completely remove, one or more reactive solvents in crude LiFSI. Since the removal of the reactive solvent(s) utilizes one or more non-reactive solvents, and at least a portion of the non-reactive solvent(s) remains after completing the reactive solvent removal method, in some embodiments, the method may also be considered a solvent replacement method, in which the undesired reactive solvent(s) are replaced with a non-reactive solvent(s) that does not adversely affect the battery performance of the reactive solvent(s). As described below, in some embodiments, the remaining non-reactive solvent(s) is often about 3000 ppm or less, for example, in the range of about 100 ppm to about 3000 ppm.

[0036] In some embodiments, the reactive solvent removal method includes contacting crude LiFSI with at least one first anhydrous organic solvent under inert conditions to produce a solution containing crude LiFSI and one or more reactive solvents. Generally, this step involves replacing the coordinating reactive solvent molecules bound to the ions with the desired non-reactive molecules. In some embodiments, the solubility of LiFSI in the at least one first anhydrous organic solvent is at least about 35% to about 65% at room temperature. In some embodiments, contacting crude LiFSI with at least one first anhydrous organic solvent includes contacting crude LiFSI with an amount of at least one first anhydrous organic solvent in the range of about 35% to about 65% by weight based on the weight of the total solution.

[0037] The inert conditions during contacting of LiFSI with the at least one first anhydrous organic solvent can be generated using any suitable technique, such as using argon gas and / or nitrogen gas, and / or other inert, dry (i.e., anhydrous) gas, among others. The purification method can be carried out at any suitable pressure, such as 1 atmosphere.

[0038] Examples of anhydrous organic solvents from which each of the at least one first anhydrous organic solvent may be selected include, but are not necessarily limited to, organic carbonates such as dimethyl carbonate (DMC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), propyl methyl carbonate (PMC), ethylene carbonate (EC), fluoroethylene carbonate (FEC), and trans-butylene carbonate, nitriles such as acetonitrile, malononitrile, and adiponitrile, alkyl acetates such as methyl acetate, ethyl acetate, propyl acetate, and butyl acetate, and alkyl propionates such as methyl propionate (MP) and ethyl propionate (EP). For example, when one or more non-reactive organic solvents are used to remove one or more reactive solvents to produce LiFSI salts for lithium ion or lithium metal batteries, it is desirable that each anhydrous organic solvent selected for the at least one first anhydrous organic solvent is non-reactive with lithium metal. Such non-reactive anhydrous organic solvents include DMC, DEC, EMC, fluoroethylene carbonate, difluoroethylene carbonate, and trifluoromethylethyl carbonate.

[0039] After contacting the crude LiFSI or LiTFSI with at least one first anhydrous organic solvent, the solution is subjected to a vacuum to remove the at least one first anhydrous organic solvent and one or more reactive solvents, such as one or more of water, methanol, or ethanol, among others that may be present, to obtain a solid mass. In some embodiments, the pressure of the vacuum may be less than about 100 Torr, less than about 10 Torr, or less than about 1 Torr, less than about 0.1 Torr, or less than about 0.01 Torr. In some embodiments, the vacuum is performed at a controlled temperature, such as a temperature in the range of about 25° C. to about 40° C.

[0040] The solid mass can then be treated with at least 100% by weight of one or more second anhydrous organic solvents in which LiFSI in the solid mass is insoluble to produce a combination having an insoluble portion. This treatment can remove any coordinating or solvating solvent. Examples of anhydrous organic solvents from which each of the one or more second anhydrous organic solvents can be selected include, but are not necessarily limited to, dichloromethane, dichloroethane, chloroform, pentane, hexane, heptane, octane, nonane, decane, undecane, and dodecane.

[0041] The insoluble portion is isolated from the combination in an inert atmosphere provided by a dry inert gas, such as argon, nitrogen, another dry inert gas, or any combination thereof. The insoluble portion may be isolated by any suitable method, such as filtration using one or more filter media, centrifugation, gravity separation, hydrocyclones, or any other suitable method. Those skilled in the art will understand the appropriate filtration techniques for use in any particular embodiment of the protic solvent reduction method of the present disclosure.

[0042] The insoluble portion can be flushed with at least one inert gas (e.g., dry inert gas, i.e., less than 1 ppm water) to remove traces of at least one second anhydrous organic solvent. Examples of inert gases from which the at least one dry inert gas can each be selected include argon and nitrogen.

[0043] The flashed insoluble portion can be subjected to a pressure of less than about 100 Torr to obtain a protic solvent reduced LiFSI product or a protic solvent reduced LiTFSI product. In some embodiments, the pressure can be less than about 10 Torr, or less than about 1 Torr, or less than about 0.1 Torr, or less than about 0.01 Torr. In one example, the pressure in the vacuum is less than about 0.01 Torr. In some embodiments, the vacuum is performed at a controlled temperature, such as a temperature of less than about 40° C. (e.g., in the range of about 20° C. to about 40° C.). The resulting reactive solvent reduced LiFSI product is typically a white, free-flowing powder.

[0044] The dried, reactive solvent reduced LiFSI product can be stored in a dry, inert container, such as a dry polytetrafluoroethylene (PTFE) container or a nickel alloy that is inert to free fluoride, at a low temperature, such as about 25° C. or below, and in an inert gas, such as argon, to inhibit decomposition of the LiFSI during storage.

[0045] In a typical example, using DMC as at least one first anhydrous organic solvent and dichloromethane as at least one second anhydrous organic solvent, a typical process involves contacting crude LiFSI with various levels of one or more reactive solvents, such as water, methanol, and / or ethanol, among others, with about 30% to about 50% by weight of anhydrous dimethyl carbonate, in which LiFSI is soluble. In this example, after contacting the crude LiFSI with DMC, the DMC is removed using reactive solvent(s), such as water, methanol, and / or ethanol, under vacuum (e.g., less than about 0.01 Torr). Removal of DMC results in a solid mass. The method may further include treating the resulting solid mass with anhydrous dichloromethane, in which LiFSI is insoluble, to obtain a combination of the insoluble portion with anhydrous dichloromethane and any other non-insoluble component(s). The insoluble portion (e.g., powdered LiFSI) can be obtained by filtration, and traces of dichloromethane can be removed by flushing with dry Ar and / or dry N2. The flushed LiFSI can then be subjected to a vacuum (e.g., less than 0.01 Torr) at a temperature less than about 40°C to obtain a dry reactive solvent-reduced LiFSI product, now a free-solvent-free LiFSI product. The reactive solvent-reduced LiFSI product may not be free-solvent-free, but in practical terms, the LiFSI product typically contains at least some reactive and / or non-reactive solvent coordinated with LiFSI. The dry protic solvent-free LiFSI product may be stored under inert conditions, e.g., in a PTFE container at a temperature less than about 25°C.

[0046] Depending on the amount of reactive solvent(s) in the crude LiFSI from which the reactive solvent(s) are removed using any one of the above methods and the desired maximum amount of reactive solvent(s) in the desired LiFSI product, it may be necessary to perform a multi-pass process to sequentially reduce the amount of one or more reactive solvents with each pass. Such a multi-pass process may successively utilize any one or more of the aforementioned methods to successively reduce the level of each of the one or more reactive solvents that may initially be in the crude LiFSI and then still remain in the resulting reactive-solvent-reduced LiFSI product. An exemplary multi-pass reactive solvent reduction process 100 of the present disclosure is shown in FIG. 1.

[0047] Referring to FIG. 1, in block 105, crude LiFSI is provided that contains one or more reactive solvents present at a particular level(s). In block 110, the reactive solvent content of the crude LiFSI is reduced using any one of the methods described above. The end result of the reactive solvent reduction in block 110 is a reactive solvent-reduced LiFSI product with a reduced level of each reactive solvent. In optional block 115, the level of each of the reactive solvents in the reactive solvent-reduced LiFSI product is measured using a suitable measurement procedure. In optional block 120, each of the measured levels is compared to a maximum desired level of the reactive solvent(s) that is allowed to be present in the reactive solvent-reduced LiFSI product. In optional block 125, it is determined whether one or more of the measured levels exceed the corresponding desired maximum level. If not, i.e., if each measured level is below the corresponding desired maximum level, the reactive solvent-reduced LiFSI product meets the specification of the desired reactive solvent reduction level and does not require further reactive solvent reduction. Thus, the multi-pass reactive solvent reduction method 100 may end at block 130.

[0048] However, if at block 125 any one or more of the measured levels exceed the corresponding desired maximum level(s), then the reactive solvent reduced LiFSI product that was processed in the previous pass through reactive solvent reduction at block 110 may be processed via loop 135 at block 110. In this reactive solvent reduction pass through at block 110, the anhydrous organic solvent(s) used to generate solution and / or wash the crystallized LiFSI may be the same or different as that used in the previous pass through reactive solvent reduction at block 110. At the end of the reactive solvent reduction at block 110, at optional blocks 115 and 120, one or more measurements of the reactive solvent level(s) and a comparison of the measured level(s) with one or more corresponding desired maximum levels may be made to determine whether the method 100 may end at block 130 or whether the LiFSI in the reactive solvent reduced LiFSI product of the latest pass should be subjected to reactive solvent reduction again via loop 135.

[0049] A non-limiting, illustrative example in which the multi-pass reactive solvent reduction method may be useful is a lithium-based electrolyte, such as LiFSI for lithium-based batteries. Crude LiFSI typically has reactive solvents, such as methanol, ethanol, and / or propanol, from the crystallization process of LiFSI. These reactive solvents may be present at more than 3000 ppm. However, such reactive solvent levels are detrimental to lithium metal batteries because the reactive solvents react with lithium metal to produce hydrogen gas and lithium alkoxides. As a result, it is desirable to keep the reactive solvent levels in LiFSI-based electrolytes for lithium metal batteries low, for example, less than about 200 ppm, less than about 100 ppm, less than about 50 ppm, or less than about 10 ppm. Using a multi-pass purification method of the present disclosure, such as the multi-pass reactive solvent reduction method 100 shown in FIG. 1, for crude LiFSI used to synthesize LiFSI salts used in electrolytes may be a useful way to achieve such low reactive solvent levels.

[0050] As a non-limiting but illustrative example, the multi-pass reactive solvent reduction process 100 can be used to reduce the reactive solvent content (in the form of the target reactive alcohol) in the LiFSI product to less than 1 ppm, starting with crude LiFSI containing 3000 ppm alcohol as a synthetic impurity. At block 105, a desired amount of crude LiFSI is provided. At block 110, the crude LiFSI is purified, i.e., the amount of undesired alcohol is reduced, using any of the methods exemplified above or below.

[0051] In optional block 115, the level of alcohol in the reactive solvent reduced LiFSI product is measured to be 1000 ppm. In optional block 120, the measured level of 1000 ppm is compared to the requirement of less than 100 ppm. In optional block 125, since 1000 ppm is greater than the requirement of less than 100 ppm, the reactive solvent reduced LiFSI product is processed in block 110, via loop 135, using the same or a different reactive solvent reduction process as used to reduce the reactive solvent level in the initial crude LiFSI. In this second pass, the starting alcohol level is 1000 ppm and the final impurity level in the twice reactive solvent reduced LiFSI product, as measured in optional block 115, is now 500 ppm. After comparing this 500 ppm level with the requirement of less than 100 ppm in optional block 120, it is determined in optional block 125 that the twice reactive solvent reduced LiFSI product needs to be treated again in block 110 via loop 135 with the same or a different reactive solvent reduction methodology used in either of the previous two passes.

[0052] In this third pass, the starting alcohol level is 500 ppm and the final impurity level in the thrice reactive solvent reduced LiFSI product is now less than 100 ppm, as measured in optional block 115. After comparing this less than 100 ppm level to the less than 100 ppm requirement in optional block 120, in optional block 125 it is determined that the thrice reactive solvent reduced LiFSI product meets the requirement such that the multi-pass reactive solvent reduction method 100 can end in block 130.

[0053] IB example

[0054] The above methods are further illustrated by the following examples, it being understood that these examples are included for illustrative purposes only and are not intended to limit the scope of the present disclosure. Unless otherwise stated, all chemicals used in these examples were of high purity and obtained from reputable commercial sources. Strict precautions were taken to exclude moisture from the process and reactions were carried out using a well-ventilated hood.

[0055] IB1. Example 1

[0056] Removal of methanol from LiFSI using DMC and dichloromethane: In a 250 mL dry flask, LiFSI (200 g) containing 4000 ppm of methanol and 50 ppm of water was taken under nitrogen atmosphere and cooled to 10 °C using a water bath. Anhydrous DMC (140 g (about 41 wt%)) was added in portions with stirring to obtain a clear solution. The mixture was stirred at room temperature for 0.5 h. The clear solution was concentrated under reduced pressure of less than 0.01 Torr to obtain a solid, which was treated with anhydrous dichloromethane (150 g) under argon. The combination was stirred at room temperature for 1 h and the desired insoluble LiFSI product was isolated by filtration. Traces of dichloromethane were removed by flushing with dry Ar / N2 gas. The isolated LiFSI was dried in vacuum (less than 0.1 Torr) at 35 °C to obtain the reactive solvent reduced LiFSI product containing 0 ppm of methanol and 15.0 ppm of water in 90% yield.

[0057] IB2. Example 2

[0058] Removal of ethanol from LiFSI using DMC and dichloromethane: In a 250 mL dry flask, LiFSI (178 g) containing 2900 ppm ethanol and 15 ppm water was taken under nitrogen atmosphere and cooled to 10 °C using a water bath. Anhydrous DMC (140 g (about 44 wt%)) was added in portions with stirring to obtain a clear solution. The mixture was stirred at room temperature for 0.5 h. The clear solution was concentrated under reduced pressure of less than 0.01 Torr to obtain a solid, which was treated with anhydrous dichloromethane (150 g) under argon. The combination was stirred at room temperature for 1 h and the desired insoluble LiFSI product was isolated by filtration. Traces of dichloromethane were removed by flushing with dry Ar / N2 gas. The isolated LiFSI was dried in vacuum (less than 0.1 Torr) at 35 °C to obtain the reactive solvent reduced LiFSI product with 0 ppm ethanol and 4 ppm water in 90% yield.

[0059] IB3. Example 3

[0060] Removal of isopropanol from LiFSI using DMC and dichloromethane: In a 250 mL drying flask, LiFSI (350 g) containing 2000 ppm isopropanol and 30 ppm water was taken under nitrogen atmosphere and cooled to 10 °C using a water bath. Anhydrous DMC (200 g (about 36 wt%)) was added in portions with stirring to obtain a clear solution. The mixture was stirred at room temperature for 0.5 h. The clear solution was concentrated under reduced pressure of less than 0.01 Torr to obtain a solid, which was treated with anhydrous dichloromethane (350 g) under argon. The combination was stirred at room temperature for 1 h and the desired insoluble LiFSI product was isolated by filtration. Traces of dichloromethane were removed by flushing with dry Ar / N2 gas. The isolated LiFSI was dried in vacuum (less than 0.1 Torr) at 35 °C to obtain the reactive solvent reduced LiFSI product containing 0 ppm isopropanol and 4 ppm water in 92% yield.

[0061] IC Exemplary Reactive Solvent Reduced LiFSI Products

[0062] Using any of the aforementioned reactive solvent reduction methods, such as any of the single-pass reactive solvent reduction methods disclosed above or the multi-pass method 100 of FIG. 1, the resulting purified LiFSI product may have very low target reactivity levels of the reactive solvent(s). For example, in some embodiments particularly suitable for use in lithium metal batteries, the amount of reactive solvent(s) remaining in the final ultra-high purity LiFSI salt product (i.e., after completion of the reactive solvent reduction disclosed herein) is preferably less than about 100 ppm, more preferably less than about 50 ppm, and most preferably less than about 25 ppm. In some embodiments, the non-reactive solvent remaining in the final ultra-high purity LiFSI salt product has less adverse effect on battery performance than the reactive solvent, but in such embodiments, the amount of non-reactive solvent(s) remaining in the final ultra-high purity LiFSI salt product is typically less than about 3000 ppm, more typically less than about 1000 ppm. When purification is performed using only non-reactive solvents for all purification steps, the final ultra-pure LiFSI salt product typically has at least about 100 ppm of non-reactive solvent(s), but typically has about 100 ppm or less of reactive solvent(s). The level of reactive solvent(s) in the crude LiFSI before reactive solvent reduction according to the present disclosure may be about 500 ppm or more, about 1000 ppm or more, or about 2000 ppm or more. In one example where DMC is used in the reactive solvent removal / replacement method, the purified LiFSI of the present disclosure has about 0.2% to about 0.3% DMC and less than 100 ppm of water as the reactive solvent.

[0063] Use examples of ID reactive solvent reduced LiFSI salt products

[0064] As described above, the reactive solvent reduced LiFSI salt product can be used to produce, among other things, reactive solvent reduced LiFSI-based electrolytes for electrochemical devices, where the reactive solvent reduction of the reactive solvent reduced electrolyte results from the fact that the reactive solvent reduced LiFSI salt product has been processed by any one or more of the methods disclosed herein. Such reactive solvent reduced electrolytes can be produced using any of a variety of methods, such as by mixing the reactive solvent reduced LiFSI salt product (salt) of the present disclosure with one or more solvents, one or more diluents, and / or one or more additives, where the solvents, diluents, and additives may be known in the art.

[0065] When the electrochemical device is a lithium-based device, such as a secondary lithium-ion battery or a secondary lithium metal battery, it is desirable to minimize the amount of reactive solvent(s) in the LiFSI salt used to produce the electrolyte, so that the reactive solvent(s) do not affect the performance of the battery. For example, the more reactive solvent in the LiFSI salt, the greater the adverse effect of that reactive solvent on cycling performance, such as discharge capacity and capacity retention. Thus, for lithium-based secondary batteries, it is desirable to remove as much of the reactive solvent(s) as possible from the LiFSI salt used in the electrolyte of such batteries. Typically, as described above, this involves using one or more non-reactive solvents in the reactive solvent reduction process disclosed herein. Thus, the majority of the reactive solvent in the initial crude LiFSI is removed and / or replaced with the non-reactive solvent(s) used in the corresponding reactive solvent reduction process. In some embodiments, the reactive solvent-reduced LiFSI product produced using the techniques disclosed herein can have the reactive and / or non-reactive solvent levels shown above in the section entitled "IC Exemplary Protic Solvent-Reduced LiFSI Products."

[0066] ID1. Preparation of LiFSI salt for use in electrolytes for lithium-based electrochemical devices

[0067] As mentioned above, a key step in preparing an electrolyte for use in a lithium-based electrochemical device, such as a secondary lithium battery having a lithium metal anode, is to remove as many reactive solvent residues as possible from the LiFSI salt containing such residues, for example, from the process(es) of synthesizing and / or purifying the LiFSI salt. In some embodiments, this removal process may include a substitution aspect in which one or more reactive solvents, such as one or more alcohols and water, are at least partially replaced by one or more non-reactive solvents. As mentioned above, removing and / or substituting the reactive solvent residue(s) in the LiFSI salt prior to producing an electrolyte for a lithium-based electrochemical device results in better performance and / or improved cycle life of the electrochemical device due to the fact that there is much less (and in some cases no) reactive solvent present in the LiFSI salt to react with the lithium metal in the device. It is noted that the non-reactive solvent(s) used in the substitution / removal process may be selected based on their benefit to the lithium-based electrochemical device. For example, the non-reactive solvent selected may be of a type that can be used as a solvent in which LiFSI salt is dissolved to provide a desired concentration in the electrolyte. In this case, it would be beneficial for the final electrolyte to use the reactive solvent removal / replacement method of the present disclosure to remove the reactive solvent(s) and potentially replace the reactive solvent with a small amount of the final solvent. Alternatively, the non-reactive solvent(s) selected for the reactive solvent removal / replacement process, apart from any primary salt dissolving function, may be a desirable additive added to be particularly beneficial to the electrochemical device, such as an additive to promote the formation of a solid electrolyte interface (SEI) layer on the lithium metal anode, among others.

[0068] The method of preparing LiFSI salt for use in lithium-based electrochemical devices includes providing a LiFSI salt containing one or more reactive solvent residues that would be detrimental to the function of a lithium-based device if such solvent residues were not removed and / or replaced prior to using the LiFSI salt to prepare an electrolyte for the lithium-based device. Providing a LiFSI salt may include purchasing LiFSI salt from a commercial supplier of such salts, or synthesizing and / or purifying crude LiFSI salt in-house. This reactive solvent residue-containing LiFSI salt can then be processed by any of the methods disclosed herein, for example, by the methods described above in the section entitled "Exemplary Methods for Removing Reactive Solvent(s) from IA Crude LiFSI". The method of preparing LiFSI salt for use in lithium-based electrochemical devices may include selecting one or more non-reactive solvents for use in a reactive solvent removal / replacement method. It should be noted that the forward slash or diagonal line in "removal / replacement" and similar positions means "and / or," i.e., one, the other, or both, as is commonly understood. In some embodiments, at least one of the non-reactive solvents selected is selected based on not only being non-reactive with lithium metal, but also providing positive benefits such as promoting SEI layer growth as an electrolyte additive. The LiFSI salt, once subjected to reactive solvent removal / replacement treatment, can be used to generate electrolytes for lithium-based electrochemical devices.

[0069] ID2. Exemplary electrochemical devices utilizing LiFSI salts produced using the methods of the present disclosure

[0070] FIG. 2 illustrates an electrochemical device 200 made according to an embodiment of the present disclosure. Those skilled in the art will readily appreciate that the electrochemical device 200 may be, for example, a battery or a supercapacitor. Furthermore, those skilled in the art will readily appreciate that FIG. 2 illustrates only some basic functional components of the electrochemical device 200, and that actual implementations of electrochemical devices such as secondary batteries or supercapacitors are typically implemented using either wound or stacked structures. Furthermore, those skilled in the art will appreciate that the electrochemical device 200 includes other components, such as electrical terminals, seal(s), thermal barrier(s), and / or vent(s), among others, that are not shown in FIG. 2 for ease of illustration.

[0071] In this example, the electrochemical device 200 includes spaced apart positive and negative electrodes 204, 208 and a corresponding pair of current collectors 204A, 208A, respectively. A porous dielectric separator 212 is disposed between the positive and negative electrodes 204, 208 to electrically isolate the positive and negative electrodes but allow ions of a reactive solvent-reduced LiFSI-based electrolyte 216 produced in accordance with the present disclosure to flow therethrough. The porous dielectric separator 212 and / or one, the other, or both of the positive and negative electrodes 204, 208 are impregnated with a protic solvent-reduced LiFSI-based electrolyte or a LiTFSI-based electrolyte 216, depending on whether they are porous or not. In FIG. 2, both the positive and negative electrodes 204, 208 are shown as being porous with the reactive solvent-reduced LiFSI-based electrolyte 216 shown extending therethrough. As mentioned above, an advantage of using the reactive solvent reduced LiFSI-based electrolyte of the present disclosure for the reactive solvent reduced LiFSI-based electrolyte 216 is that reactive solvent(s) that may be present in the LiFSI-based electrolyte, such as protic solvents by synthesis or purification, can be reduced to a level acceptable for use in the electrochemical device 200 (e.g., meeting one or more protic solvent level specifications). Examples of reactive solvent reduced LiFSI products (salts) and examples of low levels of reactive solvent(s) that can be used to produce the reactive solvent reduced LiFSI-based electrolyte 216 are described above. The electrochemical device 200 includes current collectors 204A, 208A, positive and negative electrodes 204, 208, a porous dielectric separator 212, and a container 220 that contains the protic solvent reduced LiFSI-based electrolyte or LiTFSI-based electrolyte 216.

[0072] As will be appreciated by those skilled in the art, depending on the type and design of the electrochemical device, each of the positive and negative electrodes 204, 208 comprises a suitable material that is compatible with the alkali metal ions and other components in the purified LiFSI-based electrolyte 216. Each of the current collectors 204A, 208A can be made of any suitable conductive material, such as copper or aluminum or any combination thereof. The porous dielectric separator 212 can be made of any suitable porous dielectric material, such as a porous polymer, among others. Various battery and supercapacitor structures that can be used to construct the electrochemical device 200 of FIG. 2 are known in the art. When any of such known structures are used, the novelty of the electrochemical device 200 lies in the high purity reactive solvent-reduced LiFSI-based electrolyte 216 that has not been achieved by conventional methods of producing LiFSI salt and corresponding electrolytes.

[0073] In one example, the electrochemical device 200 can be made as follows: A reactive solvent reduced LiFSI-based electrolyte 216 can be produced starting from crude LiFSI, which is then purified using any one or more of the reactive solvent reduction methods described herein to produce a reactive solvent reduced LiFSI product having an appropriate low level of one or more target reactive solvents. This reactive solvent reduced LiFSI product can then be used to produce the reactive solvent reduced LiFSI-based electrolyte 216, for example, by adding one or more solvents, one or more diluents, and / or one or more additives that improve the performance of the electrochemical device 200. The reactive solvent reduced LiFSI-based electrolyte 216 can then be added to the electrochemical device 200, after which the container 220 can be sealed.

[0074] II. Removal of non-solvent impurities from crude lithium sulfonimide salts

[0075] This section covers methods for removing non-solvent impurities from crude lithium sulfonimide salts, the purified lithium sulfonimide salts produced thereby, and uses of such purified lithium sulfonimide salts.

[0076] II.A. Exemplary Methods for Purifying Crude LiFSI

[0077] Although several processes for producing LiFSI are known, each of the known methods for synthesizing LiFSI on a commercial scale produces crude LiFSI that contains various levels of impurities, such as synthetic impurities. For example, as noted above, LiFSI is often commercially produced using crude HFSI that is reacted with Li2CO3 or LiOH, and the crude HFSI contains various synthetic impurities that result in impurities in the crude LiFSI so synthesized.

[0078] For example, one method of synthesizing HFSI uses urea (NH2CONH2) and fluorosulfonic acid (FSO3H). The drawbacks of this process are the low yield of HFSI and the isolated HFSI with a large excess of fluorosulfonic acid as an impurity. The boiling points (bp) of fluorosulfonic acid (bp 165.5 °C) and bp of HFSI (bp 170 °C) are very close to each other, making it very difficult to separate them from each other by simple fractional distillation [1]. Attempts have been made to remove the fluorosulfonic acid by treating a mixture of HFSI and fluorosulfonic acid with sodium chloride. In this case, sodium chloride reacts selectively with the fluorosulfonic acid to produce sodium salt and HCl by-product. The drawbacks of this process are the low yield of purified HFSI and also that the HFSI product is contaminated with some chloride impurities (HCl and NaCl) as impurities.

[0079] Another method of synthesizing HFSI for use in LiFSI synthesis involves the fluorination of bis(chlorosulfonyl)imide (HCSI) with arsenic trifluoride (AsF3). In this reaction, HCSI is treated with AsF3. Arsenic trifluoride is particularly difficult to handle on an industrial scale due to its toxic nature and high vapor pressure. A typical reaction uses a ratio of HCSI to AsF3 of 1:8.6. HFSI produced by this method was also found to be contaminated with AsF3 and AsCl3 synthetic impurities, which were found to be good sources of chloride and fluoride impurities [2].

[0080] HFSI for use in LiFSI synthesis can also be prepared by fluorinating HCSI with antimony trifluoride (SbF3). The antimony trichloride by-product of this reaction has high solubility in HFSI, is essentially sublimable, and is very difficult to separate from the desired product. The product of this reaction is typically contaminated with antimony trichloride, which is a good source of chloride impurities [3].

[0081] Yet another method to produce HFSI for use in LiFSI synthesis involves reacting HCSI with excess anhydrous HF at high temperatures [4]. The yield of this reaction is at most 60%, and the product is contaminated with fluorosulfonic acid produced from the decomposition of HCSI. This by-product is difficult to remove because its boiling point is close to that of HFSI. This reaction to fluorinate HSCI using anhydrous HF achieved a yield of over 95% [5], but the product is still contaminated with fluorosulfonic acid, hydrogen fluoride, hydrogen chloride, and sulfuric acid as synthetic impurities.

[0082] It has been reported that the reaction of HCSI with bismuth trifluoride (BiF3) produces HFSI in the cleaner reaction product. In this reaction, BiCl3 is not sublimable, so the formed BiCl3 by-product can be easily separated from HFSI by fractional distillation [6]. However, the product has some chloride, fluoride, and fluorosulfonic acid as synthetic impurities.

[0083] Another method for synthesizing HFSI involves reacting potassium bis(fluorosulfonyl)imide (KFSI) with perchloric acid.[7] In this process, the by-product potassium perchlorate is considered explosive, and isolated HFSI is contaminated with high levels of potassium cations and some chloride impurities present in KFSI.

[0084] Hydrogen bis(fluorosulfonic acid), also known as imidobis(sulfuric acid) difluoride, having the formula FSO2NH-O2F, has a melting point (mp) of 17 °C, a bp of 170 °C, and a density of 1.892 g / cm 3 It is a colorless liquid with a pH of 1. It is very soluble in water and in many organic solvents. Its hydrolysis in water is relatively slow, resulting in the formation of HF, H2SO4, and amidosulfuric acid (H3NSO3). HFSI is a strong acid with a pKa of 1.28[8].

[0085] The purification methods of the present disclosure can be used to remove target impurities, such as synthetic impurities and / or other impurities present in crude LiFSI, e.g., crude LiFSI synthesized using crude HFSI produced using any one or more of the synthesis methods described above. In some embodiments, the purification method includes contacting the crude LiFSI with at least one first anhydrous organic solvent under inert conditions to produce a solution containing crude LiFSI and one or more target impurities. In some embodiments, the solubility of LiFSI in the at least one first anhydrous organic solvent is at least about 60%, typically in the range of about 60% to about 90%, at room temperature, and the solubility of each of the one or more target impurities is typically about 20 parts per million (ppm) or less, often, e.g., less than about 13 ppm, at room temperature. In some embodiments, the contacting of the crude LiFSI with the at least one first anhydrous organic solvent is performed using a minimal amount of the at least one first anhydrous organic solvent. A "minimal amount" in the context of the at least one first anhydrous organic solvent means that the at least one first anhydrous organic solvent is provided in an amount in which LiFSI is substantially no longer dissolved. In some embodiments, the minimum amount of the at least one anhydrous inorganic solvent is in the range of about 50% to about 75% by weight of the solution.

[0086] In some embodiments, the contacting of the crude LiFSI with the at least one first anhydrous organic solvent is carried out at a temperature lower than a temperature in the range of about 15° C. to about 25° C. The dissolution of the crude LiFSI in the at least one first anhydrous organic solvent is an exothermic reaction. As a result, in some embodiments, the temperature of the solution can be controlled using any suitable temperature control device, such as a chiller, a thermostat, a circulator, etc. In some embodiments, the temperature of the solution is controlled to maintain the temperature of the solution below about 25° C. when the at least one anhydrous organic solvent is contacted with the crude LiFSI. To achieve a minimum amount of the at least one first anhydrous organic solvent and / or to control the temperature of the solution during the contacting of the crude LiFSI with the at least one first anhydrous organic solvent, the at least one anhydrous organic solvent can be added continuously or continuously at a precisely controlled rate or in a precisely controlled amount using a suitable feeder or dosing device.

[0087] The inert conditions during contacting of LiFSI with the at least one first anhydrous organic solvent can be generated using any suitable technique, such as using argon gas and / or nitrogen gas, and / or other inert, dry (i.e., anhydrous) gas, among others. The purification method can be carried out at any suitable pressure, such as 1 atmosphere.

[0088] Examples of anhydrous organic solvents from which each of the at least one first anhydrous organic solvent may be selected include, but are not necessarily limited to, dimethyl carbonate (DMC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), propyl methyl carbonate (PMC), ethylene carbonate (EC), fluoroethylene carbonate (FEC), transbutylene carbonate, acetonitrile, malononitrile, adiponitrile, methyl acetate, ethyl acetate, propyl acetate, butyl acetate, methyl propionate (MP), ethyl propionate (EP), methanol, ethanol, propanol, and isopropanol.

[0089] After contacting the crude LiFSI with the at least one first anhydrous organic solvent, at least one second anhydrous organic solvent is added to the solution to precipitate the at least one target impurity. The at least one second anhydrous organic solvent is selected such that the LiFSI and the one or more target impurities are substantially insoluble in the at least one second anhydrous organic solvent (as described above, it is generally desirable that the target impurities should not be soluble at more than 20 ppm). In some embodiments, the at least one second anhydrous organic solvent is added in a minimal amount. By "minimal amount" in the context of the at least one second anhydrous organic solvent, it is meant that the at least one second anhydrous organic solvent is provided in an amount such that the one or more target impurities are no longer substantially precipitated out of solution. In some embodiments, the minimal amount of the at least one anhydrous inorganic solvent is in the range of greater than 0% to 10% by weight or less of the solution. The at least one second anhydrous organic solvent can be added under the same temperature, pressure and inert conditions that exist during contacting the crude LiFSI with the at least one first anhydrous organic solvent.

[0090] Examples of anhydrous organic solvents from which each of the at least one second anhydrous organic solvent may be selected include, but are not necessarily limited to, dichloromethane, dichloroethane, chloroform, pentane, hexane, heptane, octane, nonane, decane, undecane, and dodecane.

[0091] After adding at least one second anhydrous organic solvent, the insoluble portion of each of the one or more target impurities is separated from the solution, for example, by filtration or cannulation, to produce a filtrate containing LiFSI in solution. Filtration can be performed using any suitable method, such as using one or more filter media, centrifugation, gravity separation, hydrocyclones, etc. One of skill in the art will understand the appropriate filtration technique(s) for use in any particular embodiment of the purification method of the present disclosure.

[0092] After the filtrate is obtained from the filtration, the solvent in the filtrate is removed to obtain a solid mass consisting mainly of LiFSI and some reduced amount of one or more target impurities. The solvent removed is typically each of the one or more first anhydrous organic solvents and the one or more second anhydrous organic solvents from the previous treatment. The solvent can be removed using any suitable technique, for example, under suitable temperature and reduced pressure conditions. For example, removing the solvent may be performed at a pressure of about 0.5 Torr or less or about 0.1 Torr or less. The temperature during removal may be, for example, about 25°C to about 40°C or less.

[0093] After obtaining the solid mass, the solid mass can be contacted with at least one third anhydrous organic solvent in which LiFSI is substantially insoluble to further remove more of the one or more target impurities by the one or more target impurities solvated with the third solvent. Another advantage is that any ppm level of HF formed during the process is removed by aspirating the solvent, especially at reduced pressure and at a temperature slightly above room temperature. In some embodiments, the amount of the at least one third anhydrous organic solvent used to contact the solid mass can be at least 50% by weight of the mass of the solid mass. Examples of anhydrous organic solvents from which each of the at least one third anhydrous organic solvent can be selected include, but are not necessarily limited to, dichloromethane, dichloroethane, chloroform, pentane, hexane, heptane, octane, nonane, decane, undecane, dodecane.

[0094] After contacting the solid mass with at least one third anhydrous organic solvent, LiFSI is isolated from the at least one third anhydrous organic solvent to obtain a purified LiFSI product containing reduced amounts of each of one or more target impurities. Isolation of LiFSI from the at least one third anhydrous organic solvent can be performed using any one or more suitable techniques, such as filtering the solid form of LiFSI and / or drying the solid LiFSI, such as in vacuum. In some embodiments, the pressure in the vacuum is less than about 0.1 Torr or less than about 0.01 Torr. The resulting purified LiFSI product is typically a white, free-flowing powder.

[0095] The dried, purified LiFSI product can be stored in a dry, inert container, such as a dry polytetrafluoroethylene (PTFE) container or a nickel alloy that is inert to free fluoride, at a low temperature, such as about 25° C. or below, and in an inert gas, such as argon, to inhibit decomposition of the LiFSI during storage.

[0096] Table I below shows an example of the selection of each of the first, second and third anhydrous organic solvents for the LiFSI purification method of the present disclosure. As can be seen in the table, the first anhydrous organic solvent selected is dimethyl carbonate, and the second and third anhydrous organic solvents selected are dichloromethane. [Table 1]

[0097] Based on Table I above, the solubility of LiFSI in dimethyl carbonate is more than 90% and it is insoluble in dichloromethane. Meanwhile, the solubility of the target impurities such as LiF, LiCl and Li2SO4 in this example is less than 13 ppm in dimethyl carbonate under anhydrous conditions. Therefore, in this example of purifying crude LiFSI, anhydrous dimethyl carbonate and anhydrous dichloromethane solvents were selected to obtain purified LiFSI product according to the present disclosure. According to the above method embodiment, crude LiFSI containing the impurities reported in Table I above can be mixed in dimethyl carbonate at a concentration of about 40% to about 75% at about 25° C. and stirred at room temperature, followed by addition of about 2% to about 10% dichloromethane to precipitate the target impurities. The target impurities can then be removed, for example, by filtration, and the filtrate can be concentrated to dryness. The resulting solid can then be treated with anhydrous dichloromethane to remove any target HF impurities that are soluble in dichloromethane. However, LiFSI is insoluble in dichloromethane.

[0098] The purified LiFSI is collected by filtration and finally dried under reduced pressure (in one example, less than about 0.1 Torr) and less than about 40° C. to obtain a white, free-flowing powder. In this example, the white powder was stored under an argon atmosphere in a PTFE container.

[0099] Depending on the concentration of the target impurity(s) in the crude LiFSI purified using any one of the above methods and the desired maximum concentration of the target impurity(s) in the desired purified LiFSI product, it may be necessary to perform a multi-pass process to sequentially reduce the amount of the target impurity(s) with each pass. Such a multi-pass process may successively utilize one or more of any of the aforementioned methods to successively reduce the level of each of the target impurities that may be initially in the crude LiFSI and then still remain in the resulting purified LiFSI product. An exemplary multi-pass purification process 100 of the present disclosure is shown in FIG. 1.

[0100] Referring to FIG. 3, in block 305, crude LiFSI is provided that contains one or more target impurities present at a particular level(s). In block 310, the crude LiFSI is purified using any one of the methods described above. The end result of the purification in block 310 is a purified LiFSI product with reduced levels of each target impurity. In optional block 315, the level of each of one or more of the target impurities in the purified LiFSI product is measured using a suitable measurement procedure. In optional block 320, each of the measured levels is compared to a maximum desired level of the corresponding target impurity that is allowed to be present in the purified LiFSI product. In optional block 325, it is determined whether any one or more of the measured levels exceed the corresponding maximum desired level. If not, i.e., if each measured level is below the corresponding maximum desired level, the purified LiFSI product meets the desired impurity level specification and does not require further purification. Thus, the multi-pass purification method 300 can end in block 330.

[0101] However, if at block 325, any one or more of the measured levels exceed the corresponding desired maximum level(s), the purified LiFSI product purified in the previous pass-through purification at block 310 can be purified via loop 335 at block 310. In this pass-through purification at block 310, the anhydrous organic solvent(s) used to generate the solution and / or wash the crystallized LiFSI can be the same or different from those used in the previous pass-through purification at block 310. At the end of the purification at block 310, at optional blocks 315 and 320, one or more measurements of the target impurity level(s) and one or more comparisons of the measured level(s) with one or more corresponding desired maximum levels can be made to determine whether the method 300 can end at block 330 or whether the LiFSI in the purified LiFSI product of the latest pass should be subjected to purification again via loop 335.

[0102] A non-limiting but illustrative example where a multi-pass purification method may be useful is a lithium-based electrolyte, such as LiFSI for a lithium-based battery. Crude LiFSI typically has chloride impurities, e.g., on the order of 350 ppm or more of LiCl from HCl synthesis impurities in the crude HFSI used to produce LiFSI. However, such chloride levels are corrosive to lithium metal batteries. As a result, it is desirable to keep chloride levels in LiFSI-based electrolytes for lithium metal batteries low, e.g., less than about 10 ppm or less than 1 ppm. Using a multi-pass purification method of the present disclosure, such as the multi-pass purification method 300 shown in FIG. 3, for crude LiFSI used to synthesize the LiFSI salt used in the electrolyte may be a useful way to achieve such low chloride levels.

[0103] As a non-limiting but illustrative example, multi-pass purification method 300 can be used to reduce the chlorine content (in the form of target impurity LiCl) in the LiFSI product to less than 1 ppm, starting with crude LiFSI containing 200 ppm LiCl as a synthetic impurity. At block 305, a desired amount of crude HFSI is provided. At block 310, the crude LiFSI is purified using any of the purification methods exemplified above or below.

[0104] In optional block 315, the level of LiCl (or chloride) in the purified LiFSI product is measured to be 100 ppm. In optional block 320, the measured level of 300 ppm is compared to the requirement of less than 1 ppm. In optional block 325, because 100 ppm is greater than the requirement of less than 1 ppm, the purified LiFSI product is processed in block 310, via loop 335, using the same or a different purification process as was used to purify the initial crude LiFSI. In this second pass, the starting target impurity level is 100 ppm and the final impurity level in the twice purified LiFSI product, as measured in optional block 315, is now 20 ppm. After comparing this 20 ppm level with the requirement of less than 1 ppm in optional block 320, it is determined in optional block 325 that the twice purified LiFSI product needs to be purified again in block 310 via loop 335 with the same or a different purification method used in either of the previous two passes.

[0105] In this third pass, the starting target impurity level is 20 ppm and the final impurity level of the triple purified LiFSI product is now less than 1 ppm, as measured in optional block 315. After comparing this less than 1 ppm level to the less than 1 ppm requirement in optional block 320, in optional block 325 it is determined that the triple purified LiFSI product meets the requirement such that the multi-pass purification method 300 can end in block 330.

[0106] II.B. Example

[0107] The above methods are further illustrated by the following examples, it being understood that these examples are included for illustrative purposes only and are not intended to limit the scope of the present disclosure. Unless otherwise stated, all chemicals used in these examples were of high purity and obtained from reputable commercial sources. Strict precautions were taken to exclude moisture from the process and reactions were carried out using a well-ventilated hood.

[0108] II.B.1. Example 1

[0109] Purification of LiFSI using dimethyl carbonate (DMC) and dichloromethane: In a 500 mL dry flask, various levels of impurities, here FSO3 - = 400 ppm, Cl - = 50 ppm, F - =200ppm, SO4 2- Crude LiFSI (250 g) containing ZnO = 200 ppm and water = 200 ppm was taken under nitrogen atmosphere and cooled to 10 °C using a water bath. Anhydrous DMC (250 g (50 wt%)) was added portionwise to the flask with stirring, followed by 20 g (4 wt%) of anhydrous dichloromethane. The mixture was stirred at room temperature for 1 hour. Insoluble impurities were removed from the mixture by filtration. The filtrate was concentrated under reduced pressure to give a solid, which was then treated with anhydrous dichloromethane (200 g) under argon. The mixture was stirred at room temperature for 1 hour and the desired insoluble LiFSI product was isolated by filtration and finally dried in vacuum (<0.1 Torr) at 35 °C to give the purified LiFSI product in 95% yield. In this example, the purified LiFSI product was free of the following impurities: FSO3 - = 100 ppm, Cl - = 10 ppm, F - =50ppm, SO4 2- = 60 ppm, and water = 50 ppm.

[0110] II.B.2. Example 2

[0111] Purification of LiFSI using ethyl methyl carbonate (EMC) and dichloromethane: In a 500 mL dry flask, various levels of impurities, here FSO3 - = 200 ppm, Cl - = 10 ppm, F - =100ppm, SO4 2- Crude LiFSI (250 g) containing ZnO = 100 ppm and water = 100 ppm was collected under nitrogen atmosphere and cooled to 10 °C using a water bath. Anhydrous EMC (200 g (about 44 wt%)) was added portionwise to the flask with stirring, followed by 25 g anhydrous dichloromethane (about 5.6 wt%). The mixture was stirred at room temperature for 1 hour. Insoluble impurities were removed by filtration. The filtrate was concentrated under reduced pressure to give a solid, which was then treated with anhydrous dichloromethane (250 g) under argon. The mixture was stirred at room temperature for 1 hour and the desired insoluble LiFSI product was isolated by filtration and finally dried in vacuum (<0.1 Torr) at 35 °C to give the purified LiFSI product in 92% yield. In this example, the purified LiFSI was free of the following impurities: FSO3 - = 40 ppm, Cl - = 1 ppm, F - =10ppm, SO4 2- = 20 ppm, and water = 30 ppm.

[0112] II.B.3. Example 3

[0113] Purification of LiFSI using diethyl carbonate (DEC) and dichloromethane: In a 500 mL dry flask, various levels of impurities, here FSO3 - = 400 ppm, Cl - = 50 ppm, F - =200ppm, SO4 2-Crude LiFSI (250 g) containing ZnO = 200 ppm and water = 200 ppm was taken under nitrogen atmosphere and cooled to 10 °C using a water bath. Anhydrous DEC (250 g (50 wt%)) was added portionwise to the flask with stirring, followed by 20 g (4 wt%) of anhydrous dichloromethane. The mixture was stirred at room temperature for 1 hour. Insoluble impurities were removed from the mixture by filtration. The filtrate was concentrated under reduced pressure to give a solid, which was then treated with anhydrous dichloromethane (200 g) under argon. The mixture was stirred at room temperature for 1 hour and the desired insoluble LiFSI product was isolated by filtration and finally dried in vacuum (<0.1 Torr) at 35 °C to give the purified LiFSI product in 90% yield. In this example, the purified LiFSI product was free of the following impurities: FSO3 - =80ppm, Cl - = 5 ppm, F - =30ppm, SO4 2- = 50 ppm, and water = 45 ppm.

[0114] II.B.4. Example 4

[0115] Purification of LiFSI using dipropyl carbonate (DPC) and dichloromethane: In a 500 mL dry flask, various levels of impurities, here FSO3 - = 200 ppm, Cl - = 10 ppm, F - =100ppm, SO4 2-Crude LiFSI (250 g) containing ZnO = 100 ppm, and water = 100 ppm was taken under nitrogen atmosphere and cooled to 10 °C using a water bath. Anhydrous dipropyl carbonate (200 g (about 44 wt%)) was added portionwise to the flask with stirring, followed by 20 g anhydrous dichloromethane (about 4.4 wt%). The mixture was stirred at room temperature for 1 hour. Insoluble impurities were removed from the mixture by filtration. The filtrate was concentrated under reduced pressure to give a solid, which was treated with anhydrous dichloromethane (250 g) under argon. The mixture was stirred at room temperature for 1 hour and the desired insoluble LiFSI product was isolated by filtration and finally dried in vacuum (<0.1 Torr) at 35 °C to give the purified LiFSI product in 90% yield. In this example, the purified LiFSI product was free of the following impurities: FSO3 - = 30 ppm, Cl - = 1 ppm, F - =11ppm, SO4 2- = 15 ppm, and water = 30 ppm.

[0116] II.B.5. Example 5

[0117] Purification of LiFSI using methyl propyl carbonate (MPC) and dichloromethane: In a 500 mL dry flask, various levels of impurities, here FSO3 - = 200 ppm, Cl - = 10 ppm, F - =100ppm, SO4 2-Crude LiFSI (250 g) containing ZnO = 100 ppm, and water = 100 ppm was taken under nitrogen atmosphere and cooled to 10 °C using a water bath. Anhydrous methyl propyl carbonate (MPC) (200 g (about 44.4 wt%)) was added in portions to the flask with stirring, followed by 20 g (about 4.4 wt%) of anhydrous dichloromethane. The mixture was stirred at room temperature for 1 hour. Insoluble impurities were removed by filtration. The filtrate was concentrated under reduced pressure to give a solid, which was treated with anhydrous dichloromethane (250 g) under argon. The mixture was stirred at room temperature for 1 hour and the desired insoluble LiFSI product was isolated by filtration and finally dried in vacuum (<0.1 Torr) at 35 °C to give the purified LiFSI product in 91% yield. In this example, the purified LiFSI product was free of the following impurities: FSO3 - =32ppm, Cl - = 2 ppm, F - =12ppm, SO4 2- = 22 ppm, and water = 35 ppm.

[0118] II.B.6. Example 6

[0119] Purification of LiFSI using ethyl acetate and chloroform: In a 500 mL dry flask, various levels of impurities, here FSO3 - = 200 ppm, Cl - = 10 ppm, F - =100ppm, SO4 2- Crude LiFSI (250 g) containing ZnO = 100 ppm, and water = 100 ppm was collected under nitrogen atmosphere and cooled to 10 °C using a water bath. Anhydrous ethyl acetate (150 g (37.5 wt%)) is added portionwise to the flask with stirring, followed by 20 g (5 wt%) of anhydrous chloroform. The mixture was stirred at room temperature for 1 h. Insoluble impurities were removed by filtration. The filtrate was concentrated under reduced pressure to give a solid, which was treated with anhydrous chloroform (250 g) under argon. The mixture was stirred at room temperature for 1 h and the desired insoluble LiFSI product was isolated by filtration and finally dried in vacuum (<0.1 Torr) at 35 °C to give the purified LiFSI product in 88% yield. In this example, the purified LiFSI was free of the following impurities: FSO3- = 40 ppm, Cl - = 2 ppm, F - =15ppm, SO4 2- = 20 ppm, and water = 40 ppm.

[0120] II.B.7. Example 7

[0121] Purification of LiFSI using butyl acetate and dichloromethane: In a 500 mL dry flask, various levels of impurities, here FSO3 - = 200 ppm, Cl - = 10 ppm, F - =100ppm, SO4 2- Crude LiFSI (200 g) containing ZnO = 100 ppm and water = 100 ppm was taken under nitrogen atmosphere and cooled to 10 °C using a water bath. Anhydrous butyl acetate (150 g (about 43 wt%)) was added in portions to the flask with stirring, followed by 30 g anhydrous dichloromethane (about 8.6 wt%). The mixture was stirred at room temperature for 1 hour. Insoluble impurities were removed by filtration. The filtrate was concentrated under reduced pressure to give a solid, which was treated with anhydrous dichloromethane (250 g) under argon. The mixture was stirred at room temperature for 1 hour and the desired insoluble LiFSI product was isolated by filtration and finally dried in vacuum (<0.1 Torr) at 35 °C to give the purified LiFSI product in 89% yield. In this example, the purified LiFSI product was free of the following impurities: FSO3 - =38ppm, Cl - = 1 ppm, F - =15ppm, SO4 2- = 22 ppm, and water = 40 ppm.

[0122] II.B.8. Example 8

[0123] Purification of LiFSI using acetonitrile and dichloromethane: In a 500 mL dry flask, various levels of impurities, here FSO3 - = 200 ppm, Cl - = 10 ppm, F - =100ppm, SO4 2-Crude LiFSI (200 g) containing ZnO = 100 ppm, and water = 100 ppm was taken under nitrogen atmosphere and cooled to 10 °C in a water bath. Anhydrous butyl acetate (150 g (about 43 wt%)) was added portionwise with stirring, followed by 30 g anhydrous dichloromethane (about 8.6 wt%). The mixture was stirred at room temperature for 1 h. Insoluble impurities were removed by filtration. The filtrate was concentrated under reduced pressure to give a solid, which was treated with anhydrous dichloromethane (250 g) under argon. The mixture was stirred at room temperature for 1 h and the desired insoluble LiFSI product was isolated by filtration and finally dried in vacuum (<0.1 Torr) at 35 °C to give the purified LiFSI product in 90% yield. In this example, the purified LiFSI was free of the following impurities: FSO3 - = 50 ppm, Cl - = 5 ppm, F - =20ppm, SO4 2- = 22 ppm, and water = 38 ppm.

[0124] II.C. Exemplary Purified LiFSI Products

[0125] Using any of the aforementioned purification methods, such as any of the single-pass purification methods disclosed above or the multi-pass method 300 of FIG. 3, the resulting purified LiFSI product can have exceptionally low levels of target impurities removed by the purification method. For example, a purified LiFSI product of the present disclosure, where at least one of the target impurities is LiCl, can have 10 ppm or less or less than 1 ppm LiCl (Cl - As another example, at least one of the target impurities may have a LiF (F - ), FSO3Li(FSO3 - ), and LiCl (Cl - The purified LiFSI product of the present disclosure contains about 80 ppm or less of F. - , approximately 100 ppm or less FSO3 - , and less than about 100 ppm Cl - , approximately 40 ppm or less F - , approximately 250 ppm or less FSO3 - , and about 20 ppm or less of Cl -or approximately 200 ppm or less F - , approximately 100 ppm or less FSO3 - , and about 30 ppm or less of Cl - In another example, the F - , approximately 200 ppm or more of FSO3 - , and / or Cl of about 200 ppm or more - Each of the aforementioned levels of impurities and combinations thereof can be achieved starting with crude LiFSI having a concentration of 0.01% by weight, preferably 0.01% by weight, and more preferably 0.01% by weight. In yet another example, at least one of the target impurities is SO4 2- The purified LiFSI product of the present disclosure has about 280 ppm or less, or about 100 ppm or less SO4 2- In a further example, the aforementioned SO4 2- Each level is approximately 500 ppm or higher SO4 2- A useful feature of the purification methods of the present disclosure is the ability to simultaneously remove different types of target impurities in each (or only) pass through the method.

[0126] II.D. Exemplary Uses of Purified LiFSI Products

[0127] As discussed above, the purified LiFSI product can be used to produce, among other things, purified LiFSI-based electrolytes for electrochemical devices, where the purity of the purified electrolyte results from the fact that the purified LiFSI product has been purified by one or more of any of the methods disclosed herein. Such purified electrolytes can be produced using any of a variety of methods, such as by mixing the purified LiFSI product (salt) of the present disclosure with one or more solvents, one or more diluents, and / or one or more additives, where the solvents, diluents, and additives may be known in the art.

[0128] As discussed above in Section ID2, FIG. 2 illustrates an electrochemical device 200 made according to an embodiment of the present disclosure. In this example, the purified LiFSI-based electrolyte 216A produced according to the present disclosure may be used in place of the reactive solvent-reduced LiFSI-based electrolyte 216 described above. As discussed above, an advantage of using the purified LiFSI-based electrolyte of the present disclosure, which has been purified to remove non-solvent impurities, for the purified LiFSI-based electrolyte 216A is that impurities that may be present in the LiFSI-based electrolyte, such as synthetic impurities, can be reduced to levels that are acceptable for use in the electrochemical device 200 (e.g., meeting one or more impurity level specifications). Examples of purified LiFSI products (salts) and low levels of various of those impurities that can be used to produce the purified LiFSI-based electrolyte 216A are described above.

[0129] In one example, the purified LiFSI-based electrolyte 216A can be produced starting from crude LiFSI, which is then purified using any one or more of the purification methods described herein to produce a purified LiFSI product having an appropriate low level of one or more target impurities. In another example, crude HFSI can be first synthesized, for example, by any of the synthesis methods described above, and the crude HFSI can be used to synthesize crude LiFSI. The crude LiFSI can be purified using any one or more of the purification methods described herein to produce a purified LiFSI product (salt). The purified LiFSI product can then be used to produce the purified LiFSI-based electrolyte 216A, for example, by adding one or more solvents, one or more diluents, and / or one or more additives that improve the performance of the electrochemical device 200. The purified LiFSI-based electrolyte 216A can then be added to the electrochemical device 200, after which the container 220 can be sealed.

[0130] III. Synthesis of LiFSI using an aqueous neutralization process

[0131] This section covers methods for synthesizing LiFSI using an aqueous neutralization process, the LiFSI salts produced thereby, and uses of such LiFSI salts.

[0132] III.A. Exemplary Aqueous Neutralization Synthesis Methods

[0133] In the present disclosure, LiFSI products (e.g., salts) can be obtained by first neutralizing purified hydrogen bis(fluorosulfonyl)imide (HFSI) with one or more lithium bases, such as lithium carbonate (Li2CO3) or lithium hydroxide (LiOH), in deionized water to obtain an aqueous solution of LiFSI. Insoluble impurities, such as Li2SO4, LiCl, LiF, and LiFSO3 mentioned above, can be removed by filtration. Water can be removed, for example, in vacuum. Purified HFSI for use in this process can be obtained by any suitable method, such as purifying HFSI by crystallization, as described, for example, in U.S. Patent Application Serial No. 16 / 570,131, filed September 13, 2019, entitled "Purified Hydrogen Bis(fluorosulfonyl)imide (HFSI) Products, Methods of Purifying Crude HFSI, and Uses of Purified HFSI Products," which is incorporated herein by reference for its teachings of HFSI purification. Experimental examples of synthesizing LiFSI using aqueous neutralization and their corresponding resulting impurity levels are described below in Examples 1, 4, and 6 in Sections III.C.1, III.C.4, and III.C.6, respectively.

[0134] III.B. Exemplary Purification of LiFSI Salts Generated Using Aqueous Neutralization

[0135] The crude LiFSI product produced using the aqueous neutralization process of Section III.A above can be purified to remove one or more targeted impurities, such as any synthetic impurities remaining after removal of water from the synthetic LiFSI product. Additionally or alternatively, the crude LiFSI product produced using the aqueous neutralization process of Section III.A above can be purified to remove and / or replace reactive solvent(s), such as water, present in the LiFSI product. This section briefly describes examples of purification of crude LiFSI produced using an aqueous neutralization process.

[0136] III.B.1. Removal of Non-Reactive Solvent Impurities

[0137] As described above in Section II.A, crude LiFSI, including the crude LiFSI product produced using the aqueous neutralization process described above in Section III.A, can be purified to remove targeted impurities. Such targeted impurities can include any synthetic salts that may remain after filtration of such insoluble salts and removal of water, such as Li2SO4, LiCl, LiF, and LiFSO3, described above in Section III.A. As an example, after removing water from the aqueous neutralization process, the resulting LiFSI product (herein "crude LiFSI" for the context of purification according to Section II.A above) can be subjected to purification as described above in Section II.A. The resulting purified LiFSI product has reduced levels of the targeted impurity(s). Experimental examples of such purification and corresponding targeted impurity levels are described below in Examples 2, 5, and 7 in Sections III.C.2, III.C.5, and III.C.7, respectively. It is noted that when the purified LiFSI product is used to prepare an electrolyte, the solvent(s) used in the purification process may be one or more of the solvent(s) used in the final electrolyte. In this manner, the solvent(s) remaining from the purification process become part of the final electrolyte solvent(s).

[0138] III.B.2. Removal / Replacement of Reactive Solvent(s)

[0139] As described above in Section IA, crude LiFSI, including the crude LiFSI product produced using the aqueous neutralization process described above in Section III.A, can be purified to remove / replace one or more reactive solvents. Such reactive solvents can include any residual water not removed in the water removal step described above in Section III.A. Additionally, one or more reactive solvents targeted for removal and / or replacement with one or more non-reactive solvents can be present after purification to remove non-reactive solvent impurities, as described above in Sections III.B.1 and II.A. As an example, after removing water from the aqueous neutralization process, the resulting LiFSI product (herein, "crude LiFSI" in the context of purification according to Section IA above) can be subjected to purification as described in Section IA. As another example, after purification of LiFSI synthesized by the aqueous neutralization process of Section III.A (see Section III.B.1 above), the resulting purified LiFSI product (herein, "crude LiFSI" in the context of purification according to Section IA above) can be subjected to purification as described above in Section IA. In either case, the resulting purified LiFSI product will have reduced levels of the targeted reactive solvent(s). An experimental example of such purification and corresponding target impurity levels is described below in Example 3 of Section III.C.3. Note that when the purified LiFSI product is used to prepare an electrolyte, the solvent(s) used in the reactive solvent removal / replacement process may be one or more of the solvent(s) used in the final electrolyte. In this manner, the solvent(s) remaining from the removal / replacement process become part of the final electrolyte solvent(s).

[0140] The crude LiFSI thus obtained can be purified to remove one or more target impurities, such as synthetic impurities and / or other impurities present in the crude LiFSI. In some embodiments, the crude LiFSI can be mixed with a minimal amount (e.g., about 50% to about 70% by weight) of one or more first anhydrous organic solvents in which LiFSI is soluble to further insoluble impurities such as Li2SO4, LiCl, LiF, and LiFSO3. Anhydrous organic solvents that can be used for this purpose include dimethyl carbonate (DMC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), propyl methyl carbonate (PMC), ethylene carbonate (EC), fluoroethylene carbonate (FEC), transbutylene carbonate, acetonitrile, malononitrile, adiponitrile, methyl acetate, ethyl acetate, propyl acetate, butyl acetate, methyl propionate (MP), and ethyl propionate (EP).

[0141] To the above solution, one or more second anhydrous organic solvents in which LiFSI is insoluble are added (e.g., in an amount of about 2% to 10% by weight). Organic solvents that can be used for this purpose include dichloromethane, dichloroethane, chloroform, pentane, hexane, heptane, octane, nonane, decane, undecane, and dodecane.

[0142] In some embodiments, the impurities remain precipitated after the addition of one or more second anhydrous organic solvents and can be removed by filtration. The filtrate is collected and the solvent(s) can be removed therefrom to obtain a solid. In some examples, the solvent(s) can be removed at a controlled temperature (e.g., less than about 40° C.) in vacuum (e.g., less than about 0.1 Torr) to obtain a solid. The resulting solid can then be treated with at least one third anhydrous organic solvent in which LiFSI is insoluble. Organic solvents that can be used for this purpose include dichloromethane, dichloroethane, chloroform, pentane, hexane, heptane, octane, nonane, decane, undecane, dodecane. The precipitated LiFSI salt product can then be isolated by filtration under an inert environment (e.g., argon gas) and dried, for example, in vacuum (e.g., less than about 0.1 Torr) at less than about 40° C.

[0143] To illustrate, Table II below provides detailed examples of impurities and their solubilities in dimethyl carbonate and dichloromethane. [Table 2]

[0144] As seen in Table II above, the solubility of LiFSI in dimethyl carbonate is over 90% and it is insoluble in dichloromethane, whereas the solubility of impurities such as LiF, LiCl, Li2SO4 is less than 13 ppm in dimethyl carbonate under anhydrous conditions.

[0145] Based on these solubility / insolubility characteristics, dimethyl carbonate and dichloromethane solvents are selected in one example for a process to purify crude LiFSI produced using the aqueous neutralization process described above. In this example, crude LiFSI containing the impurities reported in Table II above was mixed in dimethyl carbonate at a concentration of 50% to 75% at about 25° C. (room temperature here) and stirred at room temperature, followed by the addition of about 2 wt % to about 10 wt % dichloromethane to precipitate the impurities. The impurities were removed by filtration, and the filtrate was concentrated to dryness. The resulting dry solid was treated with anhydrous dichloromethane to remove the HF impurity, which is soluble in dichloromethane while LiFSI is insoluble in dichloromethane.

[0146] The ultra-pure LiFSI salt product was collected by filtration and finally dried under reduced pressure (e.g., less than about 0.1 Torr) and at a temperature less than about 40° C. to yield a white, free-flowing powder, which can optionally be stored in a dry polytetrafluoroethylene (PTFE) container.

[0147] In view of the above, in some embodiments, the present disclosure describes a process for producing ultra-high purity lithium bis(fluorosulfonyl)imide (LiFSI) for lithium metal anode battery applications. The process involves neutralizing purified hydrogen bis(fluorosulfonyl)imide (HFSI) with a lithium base, such as lithium carbonate (Li2CO3) or lithium hydroxide (LiOH), in less than about 40% deionized water at less than about 25°C. Insoluble impurities, such as Li2SO4, LiCl, LiF, and LiFSO3, can be removed by filtration. Water can be removed in vacuum (e.g., less than about 0.1 Torr) at an appropriate temperature, such as less than about 35°C.

[0148] The resulting crude LiFSI can be mixed with a minimal amount (e.g., 50% to 70% by weight) of an anhydrous organic solvent in which LiFSI is soluble (e.g., dimethyl carbonate (DMC) or ethyl methyl carbonate (EMC) etc.) to further insolubilize impurities such as LiCl, LiF, Li2SO4 and / or LiFSO3. In some embodiments, the temperature of the solution is maintained below about 25 °C. The solution can then be filtered in an inert atmosphere to remove impurities.

[0149] The process may further include removing the organic solvent from the filtrate to obtain a solid mass, and treating the solid with an organic solvent in which lithium bis(fluorosulfonyl)imide is insoluble (e.g., dichloromethane). The insoluble LiFSI may be isolated by filtering in an inert atmosphere and flushing traces of organic solvent with dry argon and / or nitrogen gas. The resulting LiFSI may be pumped (e.g., below about 0.1 Torr) at an appropriate temperature (e.g., below about 35° C.) for an appropriate period of time (e.g., at least 24 hours) to obtain the ultra-high purity anhydrous LiFSI salt product as a white, free-flowing powder, which may be optionally stored in a dry polytetrafluoroethylene (PTFE) container.

[0150] In some embodiments, the LiFSI salt product synthesized by the disclosed aqueous neutralization method, purified to remove non-reactive solvent impurities, and purified to remove / replace reactive solvent(s), can be produced in electrolyte solution and used in lithium metal batteries, i.e., batteries having lithium metal anodes. As shown in Example 8 in Section III.C.8 below, this "ultra-pure" LiFSI salt product and electrolytes produced therewith exhibited much better cycle life compared to LiFSI from commercial sources such as Nippon Shokubai Co., Ltd. (Japan), Shenzhen Capchem Co., Ltd. (China), Shang Hai Shengzhan Chemifish Co., Ltd. (China), and Oakwood Products, Inc. (USA).

[0151] In the present disclosure, the process for producing ultra-high purity LiFSI may be a continuous process from the start of neutralization to the end of producing the ultra-high purity LiFSI product.

[0152] III.C. Example

[0153] Aspects of the present disclosure are further illustrated by the following examples, which are included for illustrative purposes only and are understood to be in no way intended to limit the scope of the present disclosure. Unless otherwise specified, all chemicals used were of high purity and obtained from commercial sources. Strict precautions were taken to exclude moisture during the process and reactions were carried out in a well-ventilated hood.

[0154] III.C.1. Example 1

[0155] Neutralization of purified HFSI with lithium carbonate in deionized water: In a 1000 mL flask, 1 mole of lithium carbonate (Li2CO3) was mixed with 40 g of deionized water. The suspension was cooled in an ice-water bath below 20°C. 2 moles of hydrogen bis(fluorosulfonyl)imide (HFSI) were taken in a dropping funnel and dropped into the stirred lithium carbonate suspension slurry. After the addition of HFSI was complete, the water bath was removed and the solution was stirred at room temperature for 0.5 hours. Insoluble impurities were removed by filtration. The resulting clear filtrate was concentrated in vacuum below 0.1 Torr and below 35°C to obtain crude LiFSI in quantitative yield, which was used in Example 2 below.

[0156] III.C.2. Example 2

[0157] Treatment of crude LiFSI with dimethyl carbonate: The crude LiFSI obtained in Example 1 above was used in this Example 2. The flask was placed under nitrogen and cooled to 10°C using a water bath. Anhydrous dimethyl carbonate (DMC) (300 g) was added portionwise with stirring, followed by 50 g of anhydrous dichloromethane. The mixture was stirred at room temperature for 1 hour. Insoluble impurities were removed by filtration. The filtrate was concentrated under reduced pressure to give a solid, which was treated with anhydrous dichloromethane (200 g) under argon. The mixture was stirred at room temperature for 1 hour and the desired insoluble LiFSI product was isolated by filtration and finally dried in vacuum (<0.1 Torr) at <35°C to give LiFSI in 95% yield. The LiFSI product obtained was 0.01% pure with impurity FSO3 - = 100 ppm, Cl - = 1 ppm, F - =40ppm, SO4 2- = 40 ppm, and water = 50 ppm.

[0158] III.C.3.Example 3

[0159] Treatment of LiFSI with Dimethyl Carbonate: LiFSI obtained in Example 2 was used in this Example 3. 200 g of LiFSI obtained in Example 2 above was placed in a glove box with a moisture reading of less than 1 ppm and transferred to a 1 L dry flask. The flask was removed and cooled in a water bath at less than 15° C. The LiFSI was mixed with 100 g of anhydrous dimethyl carbonate containing less than 5 ppm water. Insoluble impurities were removed by filtration under argon and the filtrate was collected in a 1 L flask. The filtrate was concentrated under reduced pressure of less than 0.1 Torr to obtain a solid. The solid was treated with anhydrous dichloromethane (150 g) under argon and the solution was stirred at room temperature for 1 hour. The desired insoluble LiFSI product was isolated by filtration and dried in vacuum (less than 0.1 Torr) at 30° C. to obtain a white free-flowing powder LiFSI in 95% yield. The resulting LiFSI product was analyzed by ion chromatography and showed impurities F-=1.3 ppm, Cl - =0.18ppm, SO4 2-= 4.4 ppm. Analysis by Karl Fischer gave a water content of 1.3 ppm. Based on proton NMR it has 0.2% dimethyl carbonate. Dimethyl carbonate was used in the test electrolyte formulation because it is non-reactive with lithium metal in electrochemical devices. This salt electrolyte formulation was used for lithium metal battery testing.

[0160] III.C.3.i. Comparative example

[0161] Comparative Example of LiFSI salt obtained from Capchem (China): By visual inspection, the color of Capchem LiFSI salt was less white than the LiFSI obtained in this Example 3. Capchem LiFSI salt was free of the following impurities: Water=15 ppm, F - = 1 ppm, Cl - = 1 ppm, and SO4 2- = 5.98 ppm. Based on proton NMR, the Capchem LiFSI salt contains 0.3% ethanol, which is incompatible with lithium metal due to its reactivity. Ethanol reacts with lithium metal to form undesirable by-products according to the following reaction: 2Li+2CH3CH2OH=2CH3CH2OLi+H2

[0162] III.C.4 Example 4

[0163] Neutralization of purified HFSI with Lithium Hydroxide in Dionized Water: In a 1 L flask, Lithium Hydroxide (LiOH) (2 moles) was dissolved in 40 g of deionized water. The suspension was cooled in an ice-water bath below 20° C. HFSI, 2 moles, was taken in a dropping funnel and added dropwise into the stirred lithium carbonate suspension slurry. After the addition of HFSI was complete, the water bath was removed and the solution was stirred at room temperature for 0.5 hours. Insoluble impurities were removed by filtration. The resulting clear filtrate was concentrated under vacuum below 0.1 Torr and at a temperature below 35° C. to obtain crude LiFSI in quantitative yield, which was used in Example 5 below.

[0164] III.C.5 Example 5

[0165] Treatment of crude LiFSI with dimethyl carbonate (DMC): Crude LiFSI obtained in Example 4 above was used in this Example 5. The flask was placed under nitrogen and cooled to 10°C using a water bath. Anhydrous dimethyl carbonate (DMC) (300 g) was added portionwise with stirring, followed by 50 g of anhydrous dichloromethane. The solution was stirred at room temperature for 1 hour. Insoluble impurities were removed by filtration. The filtrate was concentrated under reduced pressure to give a solid, which was treated with anhydrous dichloromethane (200 g) under argon. The mixture was stirred at room temperature for 1 hour and the desired insoluble LiFSI product was isolated by filtration and finally dried in vacuum (<0.1 Torr) at <35°C to give LiFSI in 92% yield. The resulting purified LiFSI was free of impurity FSO3 - = 100 ppm, Cl - = 1 ppm, F - =45ppm, SO4 2- = 35 ppm, water = 60 ppm.

[0166] III.C.6. Example 6

[0167] Neutralization of Purified HFSI with Lithium Carbonate in Dionized Water: In a 1 L flask, 0.5 moles of Lithium Carbonate (Li2CO3) was mixed with 20 g of deionized water. The suspension was cooled in an ice-water bath below 20°C. HFSI, 1 mole, was taken in an addition funnel and added dropwise into the stirred lithium carbonate suspension slurry. After the addition of HFSI was complete, the water bath was removed and the solution was stirred at room temperature for 0.5 hours. Insoluble impurities were removed by filtration. The resulting clear filtrate was concentrated under vacuum below 0.1 Torr and at a temperature below 35°C to obtain crude LiFSI in quantitative yield, which was used in Example 7 below.

[0168] III.C.7. Example 7

[0169] Treatment of crude LiFSI with ethyl methyl carbonate: The crude LiFSI obtained in Example 6 was used in this Example 7. The flask was cooled under nitrogen atmosphere and cooled to 10°C using a water bath. Anhydrous ethyl methyl carbonate (EMC) (100 g) was added portionwise with stirring, followed by 50 g of anhydrous dichloromethane. The solution was stirred at room temperature for 1 hour. Insoluble impurities were removed by filtration. The filtrate was concentrated under reduced pressure to give a solid, which was treated with anhydrous dichloromethane (200 g) under argon. It was stirred at room temperature for 1 hour and the desired insoluble LiFSI product was isolated by filtration and finally dried in vacuum (<0.1 Torr) at 35°C to give LiFSI in 90% yield. The purified LiFSI product was 0.01% pure with no impurity FSO3 - = 100 ppm, Cl - = 0.5 ppm, F - =20ppm, SO4 2- = 20 ppm, water = 46 ppm.

[0170] III.C.8. Example 8

[0171] Use of ultra-high purity LiFSI from Example 7 above in lithium metal anode batteries and comparison of results with commercially available LiFSI: Battery grade electrochemically stable organic solvents (dimethyl carbonate, ethyl methyl carbonate, dimethoxymethane, diethoxyethane, etc.) were used to generate electrolytes for the resulting LiFSI of this disclosure, and comparative studies were performed using various commercially available LiFSI salts and corresponding electrolytes under similar conditions.

[0172] The ultra-high purity LiFSI product produced according to the present disclosure provided the greatest number of cycles in lithium metal anode batteries when compared to commercially available LiFSI from Capchem, Nippon Shokubai, Chemfish, and Oakwood. An example of the better performance of the ultra-high purity LiFSI product of the present disclosure is seen in Figures 4A and 4B, which respectively show the discharge capacity versus cycle number and capacity retention versus cycle number for two non-aqueous electrolytes with the same concentration and identical chemistry, except that one electrolyte was produced using the ultra-high purity LiFSI salt product produced using the aqueous neutralization synthesis method of Section III of the present disclosure (the upper line of each of Figures 4A and 4B, "SES LiFSI") and the other electrolyte was produced using LiFSI salt sourced from Capchem (the lower line of each of Figures 4A and 4B, "CapChem LiFSI").

[0173] The batteries used in the experiments from which the graphs in Figures 4A and 4B were obtained were pouch cells with three layers of cathode and four layers of anode. The electrolytes were each composed of 2.0 moles of LiFSI in 1 liter of solvent mixture. All other battery design factors and test conditions were the same, except for the source of LiFSI salt. The batteries were cycled under 0.2C rate charge and 1.0C rate discharge. As Figures 4A and 4B show, the batteries with LiFSI from both sources delivered the same capacity in the initial cycles. However, the battery with electrolyte produced using the disclosed ultra-high purity LiFSI salt showed better capacity retention after about 100 cycles than the battery with Capchem LiFSI salt. This data shows the stability advantage of ultra-high purity LiFSI salt over Capchem LiSFI salt under extended cycling conditions with lithium metal anode rechargeable batteries.

[0174] III.D. Exemplary Uses of Ultra-High Purity LiFSI

[0175] As mentioned above, the ultra-high purity LiFSI salt product produced by the above process may be particularly beneficial for lithium metal batteries having lithium metal anodes. In this regard, it is important to select a suitable anhydrous organic solvent for processing, since at least some of the solvent may remain in the ultra-high purity LiFSI product and, if reactive with lithium metal, may interfere with the performance of the lithium metal battery in which the ultra-high purity LiFSI product is used as the electrolyte. Indeed, residual solvent in the Capchem LiFSI salt, such as ethanol reported in Example 3 above, may be the reason why the performance of that Capchem LiFSI salt was inferior to that of the ultra-high purity LiFSI salt product, as evidenced in Example 8 above (Section III.C.8). As noted in Example 3 above (Section III.C.3), ethanol is reactive with the lithium metal present on / in the anode of the lithium metal battery.

[0176] Thus, when producing an ultra-high purity LiFSI salt product for lithium metal batteries according to the present disclosure, the solvent selected should be one known to be non-reactive with lithium metal. In this way, any solvent that may remain in the final dry solid ultra-high purity LiFSI salt product (e.g., by coordination with LiFSI or by other methods) is non-reactive with lithium metal and is therefore unlikely to adversely affect the performance of the lithium metal battery in which the ultra-high purity LiFSI salt product is used. As used herein and in the appended claims, unless otherwise indicated, the term "non-reactive," when used to modify a "solvent" or "solvents," shall mean that the solvent(s) are non-reactive with lithium metal. Conversely, unless otherwise indicated, the term "reactive," as used herein and in the appended claims to modify a "solvent" or "solvents," shall mean that the solvent(s) are reactive with lithium metal. As one skilled in the art would understand, "reactivity" in this context refers to the magnitude of the reduction potential of lithium metal relative to the solvent(s). Reactive solvents are also ineffective at passivating lithium metal, while non-reactive solvents are either non-reactive toward lithium metal or effectively passivate lithium metal, i.e., are kinetically stable.

[0177] In some embodiments particularly suitable for use in lithium metal batteries, the amount of reactive solvent remaining in the final ultra-high purity LiFSI salt product (i.e., after complete processing of the processes and / or purification disclosed herein) is preferably less than about 500 ppm, more preferably less than about 100 ppm, and most preferably less than about 50 ppm. In some embodiments, depending on the overall cathode-electrolyte-anode system utilized, the non-reactive solvent remaining in the final LiFSI salt product may have less adverse effect on battery performance than the reactive solvent that was removed. In such embodiments, the amount of non-reactive solvent(s) remaining in the final LiFSI salt product is preferably less than about 3000 ppm, more preferably less than about 2000 ppm, and most preferably less than about 500 ppm. In some embodiments, and depending on the overall cathode-electrolyte-anode system utilized, residual non-reactive solvent in the final LiFSI salt product may be beneficial to cell performance, such as when the non-reactive solvent(s) used are purposefully selected to provide one or more benefits to the cathode-electrolyte-anode system, such as improved SEI formation and / or improved ion availability in the electrolyte. In some embodiments, additional amounts of non-reactive solvent(s) used during purification and / or reactive solvent removal / replacement may be added to produce the final electrolyte, if necessary. In embodiments where the non-reactive solvent(s) used to process LiFSI are beneficial to cell performance, the amount of residual non-reactive solvent may be greater than 2000 ppm or greater than 3000 ppm. When purification is performed using only non-reactive solvents for all purification steps, the final LiFSI salt product typically has at least about 100 ppm of non-reactive solvent(s), but typically has about 100 ppm or less of reactive solvent(s). Examples of non-reactive solvents that may be suitable to remain in the LiFSI salt after removal / replacement of the reactive solvent(s) according to the present disclosure include hexane, hydrocarbons, toluene, xylene, aromatic solvents, esters and nitriles.

[0178] As discussed above in section ID2, FIG. 2 illustrates an electrochemical device 200 made according to an embodiment of the present disclosure. In this example, the ultra-high purity LiFSI-based electrolyte 216B produced according to section III may be used in place of the reactive solvent-reduced LiFSI-based electrolyte 216 described above. As discussed above, an advantage of using the ultra-high purity LiFSI-based electrolyte of the present disclosure for the purified LiFSI-based electrolyte 216B is that impurities that may be present in the LiFSI-based electrolyte, such as synthetic impurities and reactive solvent(s), can be reduced to levels acceptable for use in the electrochemical device 200 (e.g., meeting one or more impurity level specifications). Examples of ultra-high purity LiFSI products (salts) that can be used to produce the purified LiFSI-based electrolyte 216B and low levels of their various impurities are described above. This ultra-high purity LiFSI product can then be used to produce the ultra-high purity LiFSI-based electrolyte 216B, for example, by adding one or more solvents, one or more diluents, and / or one or more additives that improve the performance of the electrochemical device 200. An ultra-high purity LiFSI based electrolyte 216B can then be added to the electrochemical device 200, after which the container 220 can be sealed.

[0179] In view of the desire to remove many reactive solvent(s) from the final ultra-high purity LiFSI salt product in lithium metal battery applications, the purification methods disclosed herein may be enhanced by the selection of one or more solvents known to be non-reactive towards lithium metal for the appropriate step(s) of the method used to carry out the purification.

[0180] In some embodiments, the present disclosure relates to a method for producing a reactive solvent reduced lithium bis(fluorosulfonyl)imide (LiFSI) product, the method comprising: providing a first crude LiFSI containing LiFSI and one or more reactive solvents; contacting the first crude LiFSI with at least one first anhydrous organic solvent under inert conditions to produce a solution containing the first crude LiFSI and the one or more reactive solvents, wherein the solubility of LiFSI in the at least one first anhydrous organic solvent is at least about 35% at less than 25° C.; the at least one anhydrous first organic solvent and the one or more reactive solvents to obtain a solid mass; treating the solid mass with at least one anhydrous second organic solvent in which LiFSI is insoluble to produce a combination having an insoluble portion; isolating the insoluble portion in an inert atmosphere; flushing the insoluble portion with at least one dry inert gas to remove traces of the at least one anhydrous second organic solvent; and subjecting the flushed insoluble portion to a pressure of less than about 100 Torr to obtain a reactive solvent reduced LiFSI product.

[0181] In one or more embodiments of the method, providing a first crude LiFSI includes providing a second crude LiFSI containing LiFSI and one or more target impurities; contacting the second crude LiFSI with at least one third anhydrous organic solvent under inert conditions to produce a solution containing LiFSI and one or more target impurities, wherein LiFSI is soluble and each of the one or more target impurities is substantially insoluble in the at least one third anhydrous organic solvent at room temperature; the at least one anhydrous organic solvent, wherein each of the LiFSI and the one or more target impurities is substantially insoluble in the at least one fourth anhydrous organic solvent; filtering the insoluble portion of each of the one or more target impurities from the solution to produce a filtrate; removing the solvent from the filtrate to obtain a solid mass; contacting the solid mass with at least one fifth anhydrous organic solvent in which the LiFSI is substantially insoluble; and isolating the LiFSI from the at least one fifth anhydrous organic solvent to obtain a first crude LiFSI.

[0182] In one or more embodiments of the method, the second crude LiFSI has a solubility of at least about 50% in the at least one third anhydrous organic solvent at room temperature, and each of the one or more target impurities has a solubility of about 20 parts per million (ppm) or less in the at least one third anhydrous organic solvent at room temperature.

[0183] In one or more embodiments of the method, contacting the second crude LiFSI with at least one third anhydrous organic solvent comprises contacting the second crude LiFSI with a minimal amount of the at least one third anhydrous organic solvent.

[0184] In one or more embodiments of the method, the minimum amount of the at least one third anhydrous organic solvent is about 40% to about 75% by weight of the solution.

[0185] In one or more embodiments of the method, adding at least one fourth anhydrous organic solvent to the solution comprises adding the at least one fourth anhydrous organic solvent in an amount of about 10% or less by weight of the solution.

[0186] In one or more embodiments of the method, contacting the second crude LiFSI with the at least one third anhydrous organic solvent occurs at a temperature of less than about 25°C.

[0187] In one or more embodiments of the method, the method includes controlling the temperature of the solution during contacting of the second crude LiFSI with the at least one third anhydrous organic solvent to maintain the temperature within about 2° C. of the target temperature.

[0188] In one or more embodiments of the method, the filtration is performed in an inert atmosphere.

[0189] In one or more embodiments of the method, the inert atmosphere comprises argon gas.

[0190] In one or more embodiments of the method, removing the solvent is performed in vacuum.

[0191] In one or more embodiments of the method, removing the solvent is performed at a pressure of about 0.1 Torr or less.

[0192] In one or more embodiments of the method, removing the solvent is carried out at a temperature of less than about 40°C.

[0193] In one or more embodiments of the method, isolating the LiFSI comprises filtering the solid form of LiFSI from the at least one anhydrous fifth organic solvent.

[0194] In one or more embodiments of the method, isolating the LiFSI includes drying the solid LiFSI in vacuum.

[0195] In one or more embodiments of the method, drying the solid LiFSI in vacuum includes drying the solid LiFSI at a pressure of about 0.1 Torr or less.

[0196] In one or more embodiments of the method, the one or more target impurities include one or more target impurities from the group consisting of lithium chloride (LiCl), lithium fluoride (LiF), lithium sulfate (LiSO), lithium fluorosulfate (LiSO), hydrogen fluoride (HF), and fluorosulfonic acid (FSOH).

[0197] In one or more embodiments of the method, the one or more target impurities include lithium sulfate (Li2SO4), and filtering the insoluble portion of each of the one or more target impurities includes simultaneously filtering the insoluble portion of Li2SO4.

[0198] In one or more embodiments of the method, the at least one third anhydrous organic solvent comprises at least one solvent selected from the group consisting of dimethyl carbonate (DMC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), propyl methyl carbonate (PMC), ethylene carbonate (EC), fluoroethylene carbonate (FEC), transbutylene carbonate, acetonitrile, malononitrile, adiponitrile, methyl acetate, ethyl acetate, propyl acetate, butyl acetate, methyl propionate (MP), ethyl propionate (EP), methanol, ethanol, propanol, and isopropanol.

[0199] In one or more embodiments of the method, contacting the second crude LiFSI with at least one third anhydrous organic solvent comprises contacting the second crude LiFSI with the at least one third anhydrous organic solvent in an amount between about 50% and about 75% by weight of the solution.

[0200] In one or more embodiments of the method, adding at least one fourth anhydrous organic solvent to the solution comprises adding the at least one fourth anhydrous organic solvent in an amount of about 10% or less by weight of the solution.

[0201] In one or more embodiments of the method, the at least one fourth anhydrous organic solvent comprises at least one solvent selected from the group consisting of dichloromethane, dichloroethane, chloroform, pentane, hexane, heptane, octane, nonane, decane, undecane, dodecane.

[0202] In one or more embodiments of the method, adding at least one fourth anhydrous organic solvent to the solution comprises adding the at least one fourth anhydrous organic solvent in an amount of about 10% or less by weight of the solution.

[0203] In one or more embodiments of the method, the at least one fifth anhydrous organic solvent comprises at least one solvent selected from the group consisting of dichloromethane, dichloroethane, chloroform, pentane, hexane, heptane, octane, nonane, decane, undecane, dodecane.

[0204] In one or more embodiments of the method, the at least one fourth anhydrous organic solvent comprises at least one solvent selected from the group consisting of dichloromethane, dichloroethane, chloroform, pentane, hexane, heptane, octane, nonane, decane, undecane, dodecane.

[0205] In one or more embodiments of the method, the at least one fifth anhydrous organic solvent comprises at least one solvent selected from the group consisting of dichloromethane, dichloroethane, chloroform, pentane, hexane, heptane, octane, nonane, decane, undecane, dodecane.

[0206] In one or more embodiments of the method, the method further includes placing the first crude LiFSI in a dry atmosphere in a container that does not substantially react with free fluorine, and storing the container at a temperature below about 25° C.

[0207] In one or more embodiments of the method, the one or more target impurities are by-products of a process for synthesizing LiFSI in the second crude LiFSI.

[0208] In one or more embodiments of the method, the first crude LiFSI contains less than or equal to 10 parts per million (ppm) LiCl.

[0209] In one or more embodiments of the method, the first crude LiFSI contains less than 1 ppm LiCl.

[0210] In one or more embodiments of the method, the first crude LiFSI contains less than or equal to about 500 parts per million (ppm) FSO3Li, less than or equal to about 100 ppm LiCl, and less than or equal to about 150 ppm LiF.

[0211] In one or more embodiments of the method, providing the second crude LiFSI includes synthesizing the second crude LiFSI using an aqueous neutralization process.

[0212] In one or more embodiments of the method, providing the first crude LiFSI includes synthesizing the first crude LiFSI using an aqueous neutralization process.

[0213] In one or more embodiments of the method, the reactive solvent reduced LiFSI product is a salt of an electrolyte for a lithium metal battery, and the method further includes selecting each of the at least one first anhydrous organic solvent to improve the performance of a lithium ion battery.

[0214] In one or more embodiments of the method, the method further includes selecting each of the at least one second anhydrous organic solvent to improve the performance of the lithium ion battery.

[0215] In one or more embodiments of the method, the reactive solvent reduced LiFSI product is a salt of an electrolyte containing an additive solvent, and at least one of the at least one first anhydrous solvent is the same as the additive solvent.

[0216] In some aspects, the disclosure relates to a method of making an electrochemical device, the method including treating lithium bis(fluorosulfonyl)imide (LiFSI) salt using any of the methods enumerated herein to produce a purified LiFSI salt, formulating an electrolyte using the purified LiFSI salt, providing an electrochemical device structure including a positive electrode, a negative electrode spaced apart from the positive electrode, and a volume extending between the positive electrode and the negative electrode, and allowing ions in the electrolyte to move between the positive electrode and the negative electrode, if electrolyte is present, and adding the electrolyte to the volume.

[0217] In one or more embodiments of the method, the electrochemical device is an electrochemical battery and the electrochemical device structure further includes a separator disposed within the volume.

[0218] In one or more embodiments of the method, the electrochemical cell is a lithium ion battery.

[0219] In one or more embodiments of the method, the electrochemical cell is a lithium metal battery.

[0220] In one or more embodiments of the method, the electrochemical device is a supercapacitor.

[0221] In some embodiments, the present disclosure relates to an electrochemical device that includes a positive electrode, a negative electrode spaced apart from the positive electrode, a porous dielectric separator located between the positive electrode and the negative electrode, and an electrolyte contained within at least the porous dielectric separator, wherein the electrolyte is produced using a LiFSI salt produced using any one of the methods described herein.

[0222] In one or more embodiments of the electrochemical device, the electrochemical device is a lithium battery.

[0223] In one or more embodiments of the electrochemical device, the electrochemical device is a lithium metal secondary battery.

[0224] In one or more embodiments of the electrochemical device, the electrochemical device is a supercapacitor.

[0225] The above is a detailed description of an exemplary embodiment of the present invention. Please note that in this specification and the claims appended hereto, unless otherwise stated or indicated otherwise, conjunctions such as those used in the phrases "at least one of X, Y, and Z" and "one or more of X, Y, and Z" are interpreted to mean that each item in the conjunction list can be present in any number of times except for all other items in the list, or in any number of times in combination with any or all other items in the conjunction list, each of which may be present in any number of times. Applying this general rule, the conjunction phrase in the above example where the conjunction list is composed of X, Y, and Z shall include one or more of X, one or more of Y, one or more of Z, one or more of X and one or more of Y, one or more of Y and one or more of Z, one or more of X, one or more of Y, and one or more of Z, respectively.

[0226] Various modifications and additions can be made without departing from the spirit and scope of the present invention. The features of each of the various embodiments described above can be combined with the features of other described embodiments as necessary to provide multiple combinations of features in related new embodiments. Moreover, while the above describes several separate embodiments, what is described herein is merely illustrative of the application of the principles of the present invention. Moreover, although certain methods herein may be illustrated and / or described as being performed in a particular order, the order may be highly variable within the skill of the art to achieve aspects of the present disclosure. Thus, this description is intended to be taken only as an example, and not as limiting the scope of the present invention.

[0227] Exemplary embodiments have been disclosed above and are illustrated in the accompanying drawings. Those skilled in the art will appreciate that various modifications, omissions, and additions can be made to what is specifically disclosed herein without departing from the spirit and scope of the present invention.

[0228] The inventions according to claims 1 to 30 as originally filed are set forth below. [Claim 1] 1. A method for producing a reactive solvent reduced lithium bis(fluorosulfonyl)imide (LiFSI) product, comprising: providing a first crude LiFSI containing LiFSI and one or more reactive solvents; contacting the first crude LiFSI with at least one first anhydrous organic solvent under inert conditions to produce a solution containing the first crude LiFSI and the one or more reactive solvents, wherein the solubility of the LiFSI in the at least one first anhydrous organic solvent is at least about 35% at less than 25° C.; subjecting said solution to a vacuum to remove said at least one first anhydrous organic solvent and said one or more reactive solvents to obtain a solid mass; treating said solid mass with at least one second anhydrous organic solvent in which said LiFSI is insoluble to produce a combination having an insoluble portion; isolating the insoluble portion in an inert atmosphere; flushing the insoluble portion with at least one dry inert gas to remove traces of the at least one second anhydrous organic solvent; and subjecting the flashed insoluble portion to a pressure of less than about 100 Torr to obtain the reactive solvent reduced LiFSI product. [Claim 2] The method of claim 1, wherein contacting the first crude LiFSI with at least one first anhydrous organic solvent comprises contacting the first crude LiFSI with the at least one first anhydrous organic solvent in an amount ranging from about 30% by weight to about 50% by weight of the solution. [Claim 3] The method of claim 2, wherein the at least one first anhydrous organic solvent is selected from the group consisting of organic carbonates, nitriles, alkyl acetates, and alkyl propionates. [Claim 4] 3. The method of claim 2, wherein the at least one first anhydrous organic solvent is selected from the group consisting of dimethyl carbonate (DMC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), propyl methyl carbonate (PMC), ethylene carbonate (EC), fluoroethylene carbonate (FEC), trans-butylene carbonate, acetonitrile, malononitrile, adiponitrile, methyl acetate, ethyl acetate, propyl acetate, butyl acetate, methyl propionate (MP), and ethyl propionate (EP). [Claim 5] The method of claim 4, wherein the at least one first anhydrous organic solvent comprises DMC. [Claim 6] The method of claim 1, wherein the at least one first anhydrous organic solvent is selected from the group consisting of organic carbonates, nitriles, alkyl acetates, and alkyl propionates. [Claim 7] 2. The method of claim 1, wherein treating the solid mass with at least one second anhydrous organic solvent comprises treating the solid mass with at least one second anhydrous organic solvent selected from the group consisting of dichloromethane, dichloroethane, chloroform, pentane, hexane, heptane, octane, nonane, decane, undecane, and dodecane. [Claim 8] The method of claim 7, wherein the at least one second anhydrous organic solvent comprises dichloromethane. [Claim 9] 2. The method of claim 1, wherein the at least one first anhydrous organic solvent is selected from the group consisting of dimethyl carbonate (DMC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), propyl methyl carbonate (PMC), ethylene carbonate (EC), fluoroethylene carbonate (FEC), trans-butylene carbonate, acetonitrile, malononitrile, adiponitrile, methyl acetate, ethyl acetate, propyl acetate, butyl acetate, methyl propionate (MP), and ethyl propionate (EP). [Claim 10] The method of claim 9, wherein the at least one first anhydrous organic solvent comprises DMC. [Claim 11] The method of claim 9, wherein treating the solid mass with at least one second anhydrous organic solvent comprises treating the solid mass with at least one second anhydrous organic solvent selected from the group consisting of dichloromethane, dichloroethane, chloroform, pentane, hexane, heptane, octane, nonane, decane, undecane, and dodecane. [Claim 12] The method of claim 11, wherein the at least one second anhydrous organic solvent comprises dichloromethane. [Claim 13] The method of claim 12, wherein the at least one first anhydrous organic solvent comprises DMC. [Claim 14] The method of claim 9, wherein the dry inert gas comprises at least one of argon and nitrogen. [Claim 15] The method of claim 9, wherein subjecting the solution to a vacuum comprises subjecting the solution to a vacuum of less than about 1 Torr. [Claim 16] The method of claim 15, wherein subjecting the solution to a vacuum comprises subjecting the solution to a vacuum of less than about 0.01 Torr. [Claim 17] The method according to claim 11, wherein the temperature in the vacuum is less than 35°C. [Claim 18] 2. The method of claim 1, wherein treating the solid mass with at least one second anhydrous organic solvent comprises treating the solid mass with at least one second anhydrous organic solvent selected from the group consisting of dichloromethane, dichloroethane, chloroform, pentane, hexane, heptane, octane, nonane, decane, undecane, and dodecane. [Claim 19] The method of claim 1, wherein isolating the insoluble portion in an inert atmosphere comprises filtering the insoluble portion from the combination. [Claim 20] The method of claim 15, wherein the inert atmosphere comprises a dry inert gas. [Claim 21] The method of claim 1, wherein flushing the insoluble portion with at least one dry inert gas comprises flushing the insoluble portion with at least one of argon gas and nitrogen gas. [Claim 22] The method of claim 1, wherein subjecting the flushed insoluble portion to a pressure of less than about 100 Torr comprises subjecting the flushed insoluble portion to a pressure of less than about 1 Torr. [Claim 23] The method of claim 18, wherein the pressure is less than about 0.01 Torr. [Claim 24] The method of claim 1, wherein contacting the first crude LiFSI with at least one first anhydrous organic solvent comprises contacting the first crude LiFSI with the at least one first anhydrous organic solvent in an amount ranging from about 30% by weight to about 50% by weight of the solution. [Claim 25] The method of claim 24, wherein subjecting the solution to a vacuum comprises subjecting the solution to a vacuum of less than about 0.01 Torr at a temperature of less than about 35° C. [Claim 26] The method of claim 1, wherein subjecting the flashed insoluble portion to a pressure of less than about 100 Torr comprises subjecting the flashed insoluble portion to a pressure of less than about 0.01 Torr at a temperature of less than about 40° C. [Claim 27] The method of claim 1, wherein the one or more reactive solvents in the first crude LiFSI contain alcohol at a concentration of at least 2000 parts per million (ppm), and the alcohol in the reactive solvent-reduced LiFSI product is less than about 50 ppm. [Claim 28] The method of claim 26, wherein the alcohol is at a concentration of at least about 3000 ppm. [Claim 29] The method of claim 1, wherein the one or more reactive solvents in the first crude LiFSI contain an initial concentration of water, and the water in the reactive solvent-reduced LiFSI product is about 35% or less of the initial amount. [Claim 30] The method of claim 29, wherein the water in the reactive solvent reduced LiFSI product is about 20% or less of the initial concentration.

Claims

1. 1. A method for producing a reactive solvent reduced lithium bis(fluorosulfonyl)imide (LiFSI) product, comprising: providing a first crude LiFSI containing LiFSI and one or more reactive solvents; contacting said first crude LiFSI with at least one first anhydrous organic solvent under inert conditions to produce a solution containing said first crude LiFSI and said one or more reactive solvents, said at least one first anhydrous organic solvent dissolves said LiFSI, said LiFSI having a solubility of at least 35% in said at least one first anhydrous organic solvent below 25°C; subjecting said solution to a vacuum to remove said at least one first anhydrous organic solvent and said one or more reactive solvents to obtain a solid mass; treating said solid mass with at least one second anhydrous organic solvent in which said LiFSI is insoluble to produce an insoluble portion; isolating the insoluble portion in an inert atmosphere; flushing the insoluble portion with at least one dry inert gas to remove traces of the at least one second anhydrous organic solvent; and subjecting said flashed insoluble portion to a pressure of less than 100 Torr to obtain said reactive solvent reduced LiFSI product. the one or more reactive solvents are protic solvents; method.

2. 2. The method of claim 1, wherein contacting the first crude LiFSI with at least one first anhydrous organic solvent comprises contacting the first crude LiFSI with the at least one first anhydrous organic solvent in an amount ranging from 30% to 50% by weight of the solution.

3. 3. The method of claim 2, wherein the at least one first anhydrous organic solvent is selected from the group consisting of organic carbonates, nitriles, alkyl acetates and alkyl propionates.

4. 3. The method of claim 2, wherein the at least one first anhydrous organic solvent is selected from the group consisting of dimethyl carbonate (DMC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), propyl methyl carbonate (PMC), ethylene carbonate (EC), fluoroethylene carbonate (FEC), transbutylene carbonate, acetonitrile, malononitrile, adiponitrile, methyl acetate, ethyl acetate, propyl acetate, butyl acetate, methyl propionate (MP) and ethyl propionate (EP).

5. 5. The method of claim 4, wherein the at least one first anhydrous organic solvent comprises DMC.

6. 2. The method of claim 1, wherein the at least one first anhydrous organic solvent is selected from the group consisting of organic carbonates, nitriles, alkyl acetates and alkyl propionates.

7. 2. The method of claim 1, wherein treating the solid mass with at least one second anhydrous organic solvent comprises treating the solid mass with at least one second anhydrous organic solvent selected from the group consisting of dichloromethane, dichloroethane, chloroform, pentane, hexane, heptane, octane, nonane, decane, undecane, and dodecane.

8. 8. The method of claim 7, wherein the at least one second anhydrous organic solvent comprises dichloromethane.

9. 2. The method of claim 1, wherein the at least one first anhydrous organic solvent is selected from the group consisting of dimethyl carbonate (DMC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), propyl methyl carbonate (PMC), ethylene carbonate (EC), fluoroethylene carbonate (FEC), transbutylene carbonate, acetonitrile, malononitrile, adiponitrile, methyl acetate, ethyl acetate, propyl acetate, butyl acetate, methyl propionate (MP) and ethyl propionate (EP).

10. 10. The method of claim 9, wherein the at least one first anhydrous organic solvent comprises DMC.

11. 10. The method of claim 9, wherein treating the solid mass with at least one second anhydrous organic solvent comprises treating the solid mass with at least one second anhydrous organic solvent selected from the group consisting of dichloromethane, dichloroethane, chloroform, pentane, hexane, heptane, octane, nonane, decane, undecane, and dodecane.

12. 12. The method of claim 11, wherein the at least one second anhydrous organic solvent comprises dichloromethane.

13. 13. The method of claim 12, wherein the at least one first anhydrous organic solvent comprises DMC.

14. The method of claim 9 , wherein the dry inert gas comprises at least one of argon and nitrogen.

15. 10. The method of claim 9, wherein subjecting the solution to a vacuum comprises subjecting the solution to a vacuum of less than 1 Torr.

16. 16. The method of claim 15, wherein subjecting the solution to a vacuum comprises subjecting the solution to a vacuum of less than 0.01 Torr.

17. 12. The method of claim 11, wherein the temperature in the vacuum is less than 35°C.

18. 2. The method of claim 1, wherein treating the solid mass with at least one second anhydrous organic solvent comprises treating the solid mass with at least one second anhydrous organic solvent selected from the group consisting of dichloromethane, dichloroethane, chloroform, pentane, hexane, heptane, octane, nonane, decane, undecane, and dodecane.

19. The method of claim 1 , wherein isolating the insoluble portion in an inert atmosphere comprises filtering the insoluble portion.

20. The method of claim 15 , wherein the inert atmosphere comprises a dry inert gas.

21. 10. The method of claim 1, wherein flushing the insoluble portion with at least one dry, inert gas comprises flushing the insoluble portion with at least one of argon gas and nitrogen gas.

22. 10. The method of claim 1, wherein subjecting the flushed insoluble portion to a pressure of less than 100 Torr comprises subjecting the flushed insoluble portion to a pressure of less than 1 Torr.

23. 20. The method of claim 18, wherein the pressure is less than 0.01 Torr.

24. 2. The method of claim 1, wherein contacting the first crude LiFSI with at least one first anhydrous organic solvent comprises contacting the first crude LiFSI with the at least one first anhydrous organic solvent in an amount ranging from 30% to 50% by weight of the solution.

25. 25. The method of claim 24, wherein subjecting the solution to a vacuum comprises subjecting the solution to a vacuum of less than 0.01 Torr at a temperature of less than 35°C.

26. 10. The method of claim 1, wherein subjecting the flushed insoluble portion to a pressure of less than 100 Torr comprises subjecting the flushed insoluble portion to a pressure of less than 0.01 Torr at a temperature of less than 40°C.

27. 2. The method of claim 1, wherein the one or more reactive solvents in the first crude LiFSI comprise alcohols at a concentration of at least 2000 parts per million (ppm) and the alcohols in the reactive solvent reduced LiFSI product are less than 50 ppm.

28. The method of claim 27, wherein the alcohol contained in the one or more reactive solvents in the first crude LiFSI is at a concentration of at least 3000 ppm.

29. The method of claim 29, wherein the at least one first anhydrous organic solvent is selected from the group consisting of dimethyl carbonate (DMC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), propyl methyl carbonate (PMC), ethylene carbonate (EC), fluoroethylene carbonate (FEC), transbutylene carbonate, acetonitrile, malononitrile, adiponitrile, methyl acetate, ethyl acetate, propyl acetate, butyl acetate, methyl propionate (MP) and ethyl propionate (EP); the at least one second anhydrous organic solvent is selected from the group consisting of dichloromethane, dichloroethane, chloroform, pentane, hexane, heptane, octane, nonane, decane, undecane, and dodecane; The method of claim 1.

30. The method of claim 29, wherein the one or more reactive solvents are water or an alcohol.

Citation Information

Patent Citations

  • Method for preparing bis(fluorosulfonyl)lithium imine

    CN105523970A

  • Preparation method of difluoro-sulfonyl imide lithium

    CN105731399A

  • Preparation method of lithium bis(fluorosulfonyl)imide

    CN106241757A

  • Purification method of lithium bis(fluorosulfonyl)imide

    CN106976849A

  • Preparation method of high-purity imidodisulfuryl fluoride lithium

    CN108373142A