Two-component room temperature fast curing organopolysiloxane composition and article

A two-component room-temperature fast-curing organopolysiloxane composition with a specific organopolysiloxane structure and β-ketoester compounds addresses slow curing and toxicity issues, achieving rapid and deep curing with safe, non-toxic by-products for diverse applications.

JP7556335B2Active Publication Date: 2024-09-26SHIN ETSU CHEMICAL CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2021132314
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-08-16
Publication Date
2024-09-26
Estimated Expiration
2041-08-16

AI Technical Summary

Technical Problem

Existing room-temperature-curable organopolysiloxane compositions using condensation reactions face issues with slow deep curing, toxicity from harmful by-products like 2-butanone oxime and methanol, and environmental hazards from tin catalysts, which are undesirable for human health and environmental safety.

Method used

A two-component room-temperature fast-curing organopolysiloxane composition using a specific organopolysiloxane structure with hydrolyzable silyl groups and β-ketoester compounds as leaving groups, combined with a curing catalyst, to achieve rapid and deep curing without toxic by-products.

Benefits of technology

The composition exhibits excellent fast and deep curing properties, safety for human health, and minimal environmental impact, with β-ketoester compounds like acetoacetate and malonic acid esters as non-toxic leaving groups, suitable for various applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007556335000003
    Figure 0007556335000003
  • Figure 0007556335000016
    Figure 0007556335000016
  • Figure 0007556335000008
    Figure 0007556335000008
Patent Text Reader

Abstract

To provide a two-component room temperature quick curing organopolysiloxane composition which is a two component type, excellent in quick curability and deep part curability, has no example of report of health hazard and environmental hazard when curing, and uses a hydrolyzable organosilane compound which eliminates / releases a β-ketoester compound having a comparatively high flash point as an elimination group as a curing agent, and a variety of articles having the composition, and an elastomer molded product obtained by curing the composition.SOLUTION: A composition includes: (A) organopolysiloxane of a specific structure having a silanol group or a hydrolyzable silyl group at a molecular chain terminal; (B) hydrolyzable organosilane compound having another specific structure and / or a partial hydrolysate thereof; (C) a first agent containing a curing catalyst by a specific ratio; and (A') a second agent containing organopolysiloxane of a specific structure having a silanol group at a molecular chain terminal by a specific amount.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a two-component, room-temperature fast-curing organopolysiloxane composition of the condensation cure type that crosslinks (cures) through a hydrolysis and condensation reaction in the presence of moisture (water) in the air at room temperature (23°C±15°C), in particular to a two-component, room-temperature fast-curing organopolysiloxane composition that contains a crosslinking agent in which a cleaved compound that is cleaved or generated from the crosslinking agent (curing agent) by a hydrolysis reaction during curing is a β-ketoester compound such as acetoacetate or malonate, and to various articles and the like that contain the composition or a cured product thereof (silicone rubber). [Background technology]

[0002] Room temperature curable organopolysiloxane compositions that cure at room temperature to become silicone rubber have been known for some time and have been widely used in the industrial world. Known mechanisms for curing at room temperature include a mechanism for curing by hydrosilylation addition reaction, a mechanism for radical curing by ultraviolet light, and a mechanism for curing by condensation reaction between hydrolyzable groups bonded to silicon atoms and hydroxyl groups. Among these, room temperature curable organopolysiloxane compositions that cure by condensation reaction have the advantage that they can be easily cured at room temperature and are less susceptible to curing inhibition by impurities that occur in hydrosilylation addition reactions, etc. Therefore, they are widely used in the fields of automotive gaskets and sealing materials, construction sealants, electrical and electronic parts, etc.

[0003] Room temperature curable organopolysiloxane compositions that cure by condensation reactions contain a hydrolyzable organosilane compound having a hydrolyzable group in the molecule as a curing agent (crosslinking agent), and examples of curing agents that are already widely used include deoxime-type hydrolyzable organosilane compounds that release oxime compounds such as 2-butanone oxime upon curing, and dealcohol-type hydrolyzable organosilane compounds that release alcohol compounds such as methanol. The rubber-like cured products obtained by curing compositions containing these curing agents have high heat resistance, chemical resistance, and weather resistance derived from silicone (siloxane structure). On the other hand, oxime compounds such as 2-butanone oxime that are generated during curing of deoxime-type curing agents are suspected to be carcinogenic and are undesirable, and methanol and the like that are generated during curing of alcohol-free curing agents are toxic to the human body and designated as deleterious substances, which are undesirable from the viewpoint of human health. Furthermore, in some cases, these compositions use tin catalysts as curing catalysts, which are subject to stronger regulations as environmentally hazardous substances, which is undesirable from the viewpoint of environmental protection.

[0004] Furthermore, conventional one-component room temperature curable organopolysiloxane compositions that cure by a condensation reaction have the drawback that curing proceeds from the surface exposed to atmospheric moisture (water), but it takes a long time for curing to be completed in deeper areas that are less exposed to moisture. For this reason, a technology is known that significantly improves curability by making a two-component room temperature curable organopolysiloxane composition in which the base polymer, crosslinking agent, catalyst, etc. are appropriately divided.

[0005] In Japanese Patent No. 3916403 (Patent Document 1), a composition is proposed that contains an organic compound having at least one carbonyl group (C=O group) in one molecule and an organic compound having at least one primary amino group (NH2 group) in one molecule, for a diorganopolysiloxane blocked with a hydrolyzable silyl group, with both ends of the molecular chain having an oxime structure as a leaving group. This improves deep curing and fast curing properties by utilizing water produced as a by-product from a ketimine-forming reaction between a carbonyl group and a primary amino group, but has the disadvantage that a large amount of a carbonyl compound must be intentionally added to one of the two components, and a composition containing a carbonyl compound is prone to separation. In addition, since the curing properties of a dealcohol-type organopolysiloxane composition are inferior to those of a dealcohol-type organopolysiloxane composition, a sufficient curing speed cannot be obtained even if the method of Patent Document 1 is used. For this reason, JP 2011-37968 A (Patent Document 2) reports that a silanol-containing organopolysiloxane and a ketene silyl acetal compound are mixed in the presence of an organic compound having a nitrogen atom, and then mixed with a composition containing silanol groups, thereby dramatically improving curability, but this technique is inferior in terms of deep curability to the technique of Patent Document 1, which generates water from the inside. Furthermore, these techniques cannot reduce the toxicity and environmental load of the leaving groups (methanol, 2-butanone oxime) released during curing of the oxime-free and alcohol-free room temperature curable organopolysiloxane compositions as described above. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] Patent No. 3916403 [Patent Document 2] JP 2011-37968 A Summary of the Invention [Problem to be solved by the invention]

[0007] The present invention has been made in view of the above circumstances, and has an object to provide a two-component, room-temperature-curable organopolysiloxane composition which is a two-component type that has excellent fast curing properties and deep curing properties, and which has no reported health hazards, such as carcinogenicity or reproductive toxicity to the human body, or environmental hazards, such as toxicity to aquatic organisms, during curing, and which uses, as a crosslinking agent (curing agent), a hydrolyzable organosilane compound that eliminates and releases a β-ketoester compound, such as an acetoacetate or malonate, which has a relatively high flash point, as a leaving group (leaving compound); various articles containing the composition; and various articles having an elastomer molded product (cured silicone rubber product) obtained by curing the two-component, room-temperature-curable organopolysiloxane composition. [Means for solving the problem]

[0008] As a result of intensive research conducted by the present inventors in order to achieve the above-mentioned object, it has been found that a two-component, room-temperature-curable, fast-curing organopolysiloxane composition comprising a first part containing, in specific proportions, (A) an organopolysiloxane of a specific structure having a silanol group or a hydrolyzable silyl group at the molecular chain terminal, (B) a hydrolyzable organosilane compound represented by the following general formula (4) and / or a partial hydrolysis condensate thereof, and (C) a curing catalyst, and a second part containing a specific amount of (A') an organopolysiloxane of a specific structure having a silanol group at the molecular chain terminal, has superior curing properties to one-component, room-temperature-curing organopolysiloxane compositions and eliminates and releases a β-ketoester compound such as an acetoacetate ester or a malonate ester as a leaving group (leaving compound) during curing, thereby solving the problems of toxicity to the human body and the environment and safety.

[0009] [ka] (In the formula, R 1 and R 3 are each independently a monovalent hydrocarbon group having 1 to 10 carbon atoms; R 2each independently represents a monovalent aliphatic hydrocarbon group having 1 to 10 carbon atoms which may have an ether-bonded oxygen atom, an aryl group having 6 to 10 carbon atoms which may have an ether-bonded oxygen atom, or an aralkyl group having 7 to 10 carbon atoms which may have an ether-bonded oxygen atom; and a is 3 or 4.

[0010] In the two-component room-temperature curable organopolysiloxane composition of the present invention, a first agent containing, as a base polymer, an organopolysiloxane of a specific structure whose molecular chain terminals are blocked with hydrolyzable silyl groups, or an organopolysiloxane whose molecular chain terminals are blocked with hydrolyzable silyl groups derived from the specific hydrolyzable silane compound, which is produced by coexisting an organopolysiloxane whose molecular chain terminals are blocked with silanol groups and a specific hydrolyzable silane compound with a curing catalyst, is mixed with a second agent containing, as a base polymer, an organopolysiloxane whose molecular chain terminals are blocked with silanol groups, whereby the terminal hydrolyzable silyl groups of the base polymer in the first agent and the terminal silanol groups of the base polymer in the second agent undergo a direct crosslinking reaction, resulting in improved curability compared to that of a one-component room-temperature curable organopolysiloxane composition.

[0011] Furthermore, in response to the above-mentioned curability problem, the present inventors have discovered that by using in combination a hydrolyzable organosilane compound (crosslinking agent) which contains a β-ketoester compound such as acetoacetate or malonate as a leaving group (leaving compound) as component (B) of the present invention, which has no reported health hazards such as carcinogenicity or reproductive toxicity to the human body and which has a relatively high flash point, and an organic compound having at least one primary amino group (NH group) in one molecule as component (D), it is possible to obtain a composition which has excellent fast-curing properties while suppressing separation of the organopolysiloxane composition by generating moisture from the inside through a ketimine reaction, without the need to add a ketone compound as in Patent Document 1, and which has led to the completion of the present invention.

[0012] That is, the present invention provides the following two-component room temperature fast-curing organopolysiloxane composition, and various articles containing the composition or a cured product thereof (automobile parts, automobile oil seals, electrical and electronic parts, building structures, civil engineering structures, adhesives, sealing agents, potting agents, coating agents, etc.). [1] (A) an organopolysiloxane represented by the following general formula (1), (2), or (3): 10 to 90 parts by mass (with the proviso that the total of the components (A) and (A') is 100 parts by mass), [ka] (In the formula, R is the same or different, and is an unsubstituted or halogen atom-substituted monovalent hydrocarbon group having 1 to 10 carbon atoms, and n is an integer of 5 or more.) [ka] (In the formula, R is as defined above, n1 is an integer of 3 or more, n2 is an integer of 1 or more, m is an integer of 1 to 10, and n1+m+(m×n2) is an integer of 5 or more.) [ka] (In the formula, R and n are as defined above, X is an oxygen atom or an alkylene group having 2 to 5 carbon atoms, and k is independently 0 or 1 for each silicon atom to which it is bonded.) (B) a hydrolyzable organosilane compound represented by the following general formula (4) and / or a partial hydrolysis condensate thereof: 0.1 to 30 parts by mass per 100 parts by mass of the total of the components (A) and (A'), [ka] (In the formula, R 1 and R 3 are each independently a monovalent hydrocarbon group having 1 to 10 carbon atoms; R 2each independently represents a monovalent aliphatic hydrocarbon group having 1 to 10 carbon atoms which may have an ether-bonded oxygen atom, an aryl group having 6 to 10 carbon atoms which may have an ether-bonded oxygen atom, or an aralkyl group having 7 to 10 carbon atoms which may have an ether-bonded oxygen atom; and a is 3 or 4. And, (C) Curing catalyst: 0.001 to 10 parts by mass per 100 parts by mass of the total of the components (A) and (A') A first agent comprising (A') an organopolysiloxane represented by the following general formula (1) or (2): 10 to 90 parts by mass (provided that the total of components (A) and (A') is 100 parts by mass); [ka] (In the formula, R is the same or different, and is an unsubstituted or halogen atom-substituted monovalent hydrocarbon group having 1 to 10 carbon atoms, and n is an integer of 5 or more.) [ka] (In the formula, R is as defined above, n1 is an integer of 3 or more, n2 is an integer of 1 or more, m is an integer of 1 to 10, and n1+m+(m×n2) is an integer of 5 or more.) A second agent comprising and does not contain silane and / or siloxane having three or more alkenoxysilyl groups in the molecule. The present invention relates to a two-component room temperature fast curing organopolysiloxane composition. [2] The two-component room-temperature fast-curing organopolysiloxane composition according to [1] further contains, as a curing accelerator (D), an amine compound having a primary amino group, in an amount of 0 to 20 parts by mass in each of the first and second agents, relative to 100 parts by mass of the total of the components (A) and (A') (with the proviso that at least one of the first and second agents contains 0.1 part by mass or more). [3] The two-component room-temperature fast-curing organopolysiloxane composition according to [1] or [2], wherein the hydrolyzable organosilane compound and / or partial hydrolysis condensate thereof of component (B) is one that releases a β-ketoester compound upon hydrolysis. [4] The two-component room-temperature fast-curing organopolysiloxane composition according to [3], wherein the β-ketoester compound that is eliminated is methyl acetoacetate, ethyl acetoacetate, propyl acetoacetate, allyl acetoacetate, phenyl acetoacetate, benzyl acetoacetate, dimethyl malonate, diethyl malonate, dipropyl malonate, dipentyl malonate, diallyl malonate, diphenyl malonate, or dibenzyl malonate. [5] The two-component room-temperature fast-curing organopolysiloxane composition according to any one of [1] to [4] further contains 0 to 1,000 parts by mass of an inorganic filler (E) in each of the first agent and the second agent (with the proviso that at least one of the first agent or the second agent contains 0.1 part by mass or more), relative to 100 parts by mass of the total of the components (A) and (A'). [6] The two-component room temperature fast-curing organopolysiloxane composition according to [5], wherein component (E) is one or more inorganic fillers selected from the group consisting of calcium carbonate, fumed silica, precipitated silica, carbon black, and aluminum oxide. [7] The two-component room-temperature fast-curing organopolysiloxane composition according to any one of [1] to [6], further comprising an adhesion promoter (F) in an amount of 0 to 10 parts by mass in each of the first agent and the second agent, relative to 100 parts by mass of the total of the components (A) and (A') (with the proviso that at least one of the first agent or the second agent contains 0.001 part by mass or more). [8] The two-component room-temperature curable organopolysiloxane composition according to any one of [1] to [7], wherein the blending ratio of the first agent to the second agent is 1:1 to 10:1 by mass. [9] R in general formula (4) of component (B) 2 is a monovalent aliphatic hydrocarbon group having 1 to 10 carbon atoms and having an ether-bonded oxygen atom, an aryl group having 6 to 10 carbon atoms and having an ether-bonded oxygen atom, or an aralkyl group having 7 to 10 carbon atoms and having an ether-bonded oxygen atom. [ 10 ] [1]~[ 9 13. An automobile part having a cured product of the two-component room temperature fast curing organopolysiloxane composition according to any one of claims 1 to 12. [ 11 ] [1]~[9 13. An oil seal for automobiles comprising a cured product of the two-component room temperature fast-curing organopolysiloxane composition according to any one of claims 1 to 12. [ 12 ] [1]~[ 9

[0021] An electric / electronic part having a cured product of the two-component room temperature fast curing organopolysiloxane composition described in any one of the above. [ 13 ] [1]~[ 9 13. A building structure comprising a cured product of the two-component room temperature fast curing organopolysiloxane composition according to any one of claims 1 to 12. [ 14 ] [1]~[ 9 13. A civil engineering structure comprising a cured product of the two-component room temperature fast curing organopolysiloxane composition according to any one of claims 1 to 12. [ 15 ] [1]~[ 9 13. An adhesive comprising the two-component room temperature fast curing organopolysiloxane composition according to any one of claims 1 to 12. [ 16 ] [1]~[ 9 13. A sealant comprising the two-component room temperature fast curing organopolysiloxane composition according to any one of claims 1 to 12. [ 17 ] [1]~[ 9 13. A potting agent comprising the two-component room temperature fast curing organopolysiloxane composition according to any one of claims 1 to 12. [ 18 ] [1]~[ 9 13. A coating agent comprising the two-component room temperature fast curing organopolysiloxane composition according to any one of claims 1 to 12. Effect of the Invention

[0013] The two-component room temperature fast-curing organopolysiloxane composition of the present invention is composed of a two-component composition of a first part and a second part, which provides excellent fast curing properties and deep curing properties when the first part and the second part are mixed together.

[0014] The two-component room temperature fast curing organopolysiloxane composition of the present invention is particularly excellent in fast curing in air at room temperature and has good workability. Furthermore, it has storage stability. Therefore, even after long-term storage, for example, 6 months, the two-component room temperature fast curing organopolysiloxane composition of the present invention quickly cures when the first and second components are mixed and exposed to air, and exhibits excellent physical properties. Furthermore, the crosslinking agent used in the present invention has no reported health hazards such as carcinogenicity and reproductive toxicity to the human body, or environmental hazards such as toxicity to aquatic organisms, during curing, and releases β-ketoester compounds such as acetoacetate and malonate, which have relatively high flash points, as leaving groups (leaving substances), and can be suitably used as various adhesives, sealing agents, potting agents, coating agents, etc., taking into consideration human health and safety and environmental protection (load reduction). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] The present invention will now be described in further detail. <Two-component room temperature fast curing organopolysiloxane composition> The two-component room temperature curable organopolysiloxane composition of the present invention comprises a first part containing specific amounts of components (A), (B), and (C) described below, and a second part containing component (A'). Note that the second part does not contain components (B) and (C). Each component will be described in detail below. In the present invention, the viscosity is a value measured at 23°C using a rotational viscometer in accordance with the method specified in JIS Z-8803. Unless otherwise specified, "room temperature" refers to a state where the temperature is 23°C ± 15°C and the humidity is 50% RH ± 5% RH.

[0016] [Component (A) and Component (A'): Organopolysiloxane] Component (A) is an organopolysiloxane represented by general formula (1), (2) or (3) described below, which is blended into the first agent, and component (A') is an organopolysiloxane represented by general formula (1) or (2) described below, which is blended into the second agent. These components (A) and (A') act as the main component (base polymer) in the two-component room-temperature fast-curing organopolysiloxane composition of the present invention.

[0017] Component (A) used in the two-component room temperature curable organopolysiloxane composition of the present invention is an organopolysiloxane represented by the following general formula (1), (2), or (3) and preferably having a viscosity at 23°C of 20 to 1,000,000 mPa s, and component (A') is an organopolysiloxane represented by the following general formula (1) or (2) and preferably having a viscosity at 23°C of 20 to 1,000,000 mPa s. [ka] (In the formula, R is the same or different, and is an unsubstituted or halogen atom-substituted monovalent hydrocarbon group having 1 to 10 carbon atoms, and n is an integer of 5 or more.) [ka] (In the formula, R is as defined above, n1 is an integer of 3 or more, n2 is an integer of 1 or more, m is an integer of 1 to 10, and n1+m+(m×n2) is an integer of 5 or more.) [ka] (In the formula, R and n are as defined above, X is an oxygen atom or an alkylene group having 2 to 5 carbon atoms, and k is independently 0 or 1 for each silicon atom to which it is bonded.)

[0018] In the general formulae (1), (2), and (3), R is a monovalent hydrocarbon group having 1 to 10 carbon atoms that is unsubstituted or substituted with a halogen atom, such as alkyl groups such as methyl, ethyl, and propyl; cycloalkyl groups such as cyclohexyl; alkenyl groups such as vinyl and allyl; aryl groups such as phenyl and tolyl; and groups in which the hydrogen atoms bonded to the carbon atoms of these groups are partially substituted with halogen atoms, such as 3,3,3-trifluoropropyl. Among these, methyl, vinyl, phenyl, and 3,3,3-trifluoropropyl are preferred, and methyl is particularly preferred. The multiple Rs in the general formulae (1), (2), and (3) may be the same or different groups.

[0019] Furthermore, n is an integer of 5 or more, n1 is an integer of 3 or more, and n2 is an integer of 1 or more, and in particular, these integers are such that the viscosity of these diorganopolysiloxanes at 23°C is in the range of 20 to 1,000,000 mPa·s, preferably in the range of 100 to 300,000 mPa·s. The value of n or the value of n1+m+(m×n2) that gives such a viscosity may be, specifically, usually an integer of about 5 to 2,000, preferably 20 to 1,500, and more preferably 50 to 1,000. In the present invention, the degree of polymerization (or molecular weight) can usually be determined as the number average degree of polymerization (number average molecular weight) in terms of polystyrene in gel permeation chromatography (GPC) analysis using toluene or the like as a developing solvent.

[0020] In addition, in the general formula (2), m represents the number of branched chains (the number of branching points in the molecule) and is an integer from 1 to 10, preferably an integer from 1 to 5, and more preferably an integer from 1 to 3. In the formula (2), the respective repeating units may be bonded randomly.

[0021] In addition, in the general formula (3), X is an oxygen atom or an alkylene group having 2 to 5 carbon atoms, and examples of the alkylene group having 2 to 5 carbon atoms include an ethylene group, a propylene group, a butylene group, etc. Among these, an oxygen atom or an ethylene group is preferable as X. k is independently 0 or 1 for each silicon atom to which it is bonded.

[0022] The organopolysiloxanes of components (A) and (A') have a viscosity at 23°C of 20 to 1,000,000 mPa·s, preferably 100 to 300,000 mPa·s, more preferably 1,000 to 200,000 mPa·s, and particularly preferably 10,000 to 100,000 mPa·s. If the viscosity of the organopolysiloxane is less than the lower limit (20 mPa·s), a large amount of component (B), which will be described later, is required, which is economically disadvantageous. On the other hand, if the viscosity of the organopolysiloxane exceeds the upper limit (1,000,000 mPa·s), workability decreases, which is not preferable.

[0023] The organopolysiloxanes of components (A) and (A') may each be used alone or in combination of two or more kinds. Furthermore, the organopolysiloxanes of components (A) and (A') may be the same or different.

[0024] [Component (B): Hydrolyzable organosilane compound and / or partial hydrolysis condensate thereof] The component (B) used in the room-temperature-curable organopolysiloxane composition of the present invention is a hydrolyzable organosilane compound represented by the following general formula (4) and / or a partial hydrolysis condensate thereof, which is used as a crosslinking agent (curing agent) and is characterized in that it releases a β-ketoester compound such as an acetoacetate ester or a malonate ester as a leaving group (leaving substance) upon hydrolysis. In the present invention, the term "partial hydrolysis condensate" refers to an organosiloxane oligomer having 3 or more, preferably 4 or more, residual hydrolyzable groups in the molecule, which is produced by partial hydrolysis and condensation of the hydrolyzable organosilane compound. [ka] (In the formula, R 1 and R 3 are each independently a monovalent hydrocarbon group having 1 to 10 carbon atoms; R 2each independently represents a monovalent aliphatic hydrocarbon group having 1 to 10 carbon atoms which may have an ether-bonded oxygen atom, an aryl group having 6 to 10 carbon atoms which may have an ether-bonded oxygen atom, or an aralkyl group having 7 to 10 carbon atoms which may have an ether-bonded oxygen atom; and a is 3 or 4.

[0025] Here, in the above general formula (4), R 1 is a monovalent hydrocarbon group having 1 to 10 carbon atoms, particularly a monovalent aliphatic hydrocarbon group having 1 to 10 carbon atoms, preferably a monovalent aliphatic hydrocarbon group having 1 to 6 carbon atoms, an aryl group having 6 to 10 carbon atoms, or an aralkyl group having 7 to 10 carbon atoms, and this R 1 Examples of the alkyl group include alkyl groups such as methyl, ethyl, propyl, isopropyl, butyl, isobutyl, sec-butyl, tert-butyl, pentyl, hexyl, octyl, 2-ethylhexyl, nonyl, and decyl, alkenyl groups such as vinyl, allyl, propenyl, isopropenyl, butenyl, and hexenyl, aryl groups such as phenyl and tolyl, and aralkyl groups such as benzyl and phenylethyl. Among these, methyl, ethyl, vinyl, and phenyl groups are preferred, and methyl and vinyl groups are particularly preferred.

[0026] In the above general formula (4), R 2 is a monovalent aliphatic hydrocarbon group having 1 to 10 carbon atoms, preferably 1 to 6 carbon atoms, which may have an ether-bonded oxygen atom, an aryl group having 6 to 10 carbon atoms which may have an ether-bonded oxygen atom, or an aralkyl group having 7 to 10 carbon atoms which may have an ether-bonded oxygen atom, 2Examples of the alkyl group include alkyl groups such as a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, an isobutyl group, a sec-butyl group, a tert-butyl group, a pentyl group, a hexyl group, an octyl group, a 2-ethylhexyl group, a nonyl group, and a decyl group; alkenyl groups such as a vinyl group, an allyl group, a propenyl group, an isopropenyl group, a butenyl group, and a hexenyl group; alkoxy groups such as a methoxy group, an ethoxy group, a propoxy group, an isopropoxy group, a butoxy group, an isobutoxy group, a sec-butoxy group, a tert-butoxy group, a pentyloxy group, and a hexyloxy group; alkenyloxy groups such as a vinyloxy group, an allyloxy group, a propenoxy group, and an isopropenoxy group; aryl groups such as a phenyl group and a tolyl group; aralkyl groups such as a benzyl group and a phenylethyl group; aryloxy groups such as a phenoxy group; and aralkyloxy groups such as a benzyloxy group and a phenylethyloxy group. Of these, methyl, ethyl, methoxy, ethoxy, propoxy, butoxy, pentyloxy, allyloxy, phenoxy and benzyloxy groups are preferred, with methyl and ethoxy groups being particularly preferred.

[0027] In the above general formula (4), R 3 is a monovalent hydrocarbon group having 1 to 10 carbon atoms, particularly a monovalent aliphatic hydrocarbon group having 1 to 10 carbon atoms, preferably a monovalent aliphatic hydrocarbon group having 1 to 6 carbon atoms, an aryl group having 6 to 10 carbon atoms, or an aralkyl group having 7 to 10 carbon atoms, and this R 3 Examples of the alkyl group include alkyl groups such as methyl, ethyl, propyl, isopropyl, butyl, isobutyl, sec-butyl, tert-butyl, pentyl, hexyl, octyl, 2-ethylhexyl, nonyl, and decyl, alkenyl groups such as vinyl, allyl, propenyl, isopropenyl, butenyl, and hexenyl, aryl groups such as phenyl and tolyl, and aralkyl groups such as benzyl and phenylethyl. Among these, methyl, ethyl, propyl, butyl, pentyl, allyl, phenyl, and benzyl groups are preferred, and methyl and ethyl groups are particularly preferred.

[0028] As mentioned above, a is 3 or 4. If this number is less than 3 (i.e., if a is 0, 1 or 2), rubber hardening by crosslinking reaction does not occur, making the compound unsuitable as a crosslinking agent for room temperature curable organopolysiloxane compositions.

[0029] The leaving group (leaving compound) generated by hydrolysis of the hydrolyzable organosilane compound of the above general formula (4) is a β-ketoester compound such as acetoacetate esters such as methyl acetoacetate, ethyl acetoacetate, propyl acetoacetate, allyl acetoacetate, phenyl acetoacetate, and benzyl acetoacetate, and malonate esters such as dimethyl malonate, diethyl malonate, dipropyl malonate, dipentyl malonate, diallyl malonate, diphenyl malonate, and dibenzyl malonate, and is preferably ethyl acetoacetate or diethyl malonate. These compounds are used as food additives and flavorings, and are highly safe compounds.

[0030] The hydrolyzable organosilane compound of component (B) can be produced, for example, by reacting a chlorosilane with a β-ketoester compound such as an acetoacetate or malonate in the presence of a basic substance (for example, a dehydrochlorination reaction). The reaction formula is, for example, represented by the following formula [1].

[0031] [ka] (In the formula, R 1 , R 2 , R 3 , a is as defined above.)

[0032] Here, examples of chlorosilane include those shown below. [ka]

[0033] Examples of the β-ketoester compound include the acetoacetate esters and malonate esters shown below. [ka] [ka]

[0034] The amount of β-ketoester compound such as acetoacetate ester or malonate ester to be reacted with chlorosilane is preferably 0.95 to 2.0 mol, more preferably 0.99 to 1.5 mol, and even more preferably 1.0 to 1.2 mol, per mol of chlorine atoms in chlorosilane. If the amount of β-ketoester compound is too small, the reaction may not be completed, whereas if the amount of β-ketoester compound is too large, purification takes a long time, increasing the production time.

[0035] The basic substance used in the reaction may be a basic substance having low nucleophilicity, such as trimethylamine, triethylamine, tripropylamine, tributylamine, urea, diazabicycloundecene, diazabicyclononene, etc. Among these, trimethylamine, triethylamine, and tributylamine are preferred, and triethylamine is particularly preferred. The amount of the basic substance added is preferably 0.95 to 2.0 mol, more preferably 0.99 to 1.5 mol, and even more preferably 1.0 to 1.2 mol, per mol of chlorine atoms in the chlorosilane. If the amount of the basic substance added is too small, the reaction may not be completed, whereas if the amount of the basic substance added is too large, it is economically disadvantageous.

[0036] In producing the hydrolyzable organosilane compound of component (B), a commonly used solvent may be used, and examples of such organic solvents include aromatic hydrocarbons such as toluene, xylene, benzene, etc.; aliphatic hydrocarbons such as pentane, hexane, heptane, nonane, octane, decane, etc.; ethers such as dimethyl ether, methyl ethyl ether, tetrahydrofuran, dioxane, etc.; halogenated hydrocarbons such as perchloroethane, perchloroethylene, trichloroethane, chloroform, carbon tetrachloride, etc.; amides such as dimethylformamide, etc.; and esters such as ethyl acetate, methyl acetate, butyl acetate, etc. The amount of the solvent used is not particularly limited, but is usually 10 to 500 parts by mass, preferably 30 to 300 parts by mass, and more preferably 50 to 200 parts by mass, per 100 parts by mass of the β-ketoester compound used.

[0037] The reaction conditions of chlorosilane and β-ketoester compound are usually 0 to 80°C, preferably 0 to 60°C, dropwise add β-ketoester compound to chlorosilane, and react at 30 to 80°C, preferably 40 to 60°C, for 1 to 48 hours, preferably 3 to 30 hours. If the temperature during the reaction is too low, the reaction may not be completed, and if the temperature is too high, the coloring of the product may be large. If the reaction time is too short, the reaction may not be completed, and if the reaction time is too long, it is disadvantageous to productivity. In addition, purification after the completion of the reaction can be performed by heating under a reduced pressure environment to distill off unreacted materials and solvents, and the degree of reduction in pressure is preferably 0 to 3,000 Pa, more preferably 0 to 2,000 Pa, and the temperature is preferably 50 to 150°C, more preferably 70 to 120°C. If the degree of reduction in pressure is too high, it may be difficult to distill off unreacted materials and solvents. Furthermore, if the purification temperature is too low, it may be difficult to distill off the unreacted materials and the solvent, whereas if the temperature is too high, the reaction products may become discolored or decompose.

[0038] Specific examples of the hydrolyzable organosilane compound of component (B) include those represented by the following formula: [ka] [ka] [ka] [ka] [ka]

[0039] The hydrolyzable organosilane compound and / or partial hydrolysis condensate thereof as the component (B) may use either a single compound or a combination of two or more different compounds. Component (B) is blended in the first agent in an amount of 0.1 to 30 parts by mass, and preferably 0.5 to 25 parts by mass, per 100 parts by mass of components (A) and (A') combined. If the blending amount of component (B) is too small, sufficient crosslinking is not obtained when the composition is cured, whereas if the blending amount is too large, the mechanical properties (rubber physical properties) of the resulting cured product (silicone rubber) will decrease, which may be economically disadvantageous.

[0040] [Component (C): Curing catalyst] The curing catalyst of component (C) is used to accelerate the hydrolysis and condensation reaction and is generally called a curing catalyst. Any known catalyst that is commonly used in room temperature curable silicone resin compositions that cure in the presence of moisture can be used.

[0041] Of the curing catalysts of component (C), the non-metallic organic catalyst is not particularly limited, but any known curing accelerator for condensation curing organopolysiloxane compositions can be used. Examples include phosphazene-containing compounds such as N,N,N',N',N'',N''-hexamethyl-N'''-(trimethylsilylmethyl)-phosphorimidic triamide; quaternary ammonium salts such as benzyltriethylammonium acetate; dialkylhydroxylamines such as dimethylhydroxylamine and diethylhydroxylamine; silanes and siloxanes containing guanidyl groups such as γ-(N,N,N',N'-tetramethylguanidyl)propyltrimethoxysilane, γ-(N,N,N',N'-tetramethylguanidyl)propylmethyldimethoxysilane, and γ-(N,N,N',N'-tetramethylguanidyl)propyltris(trimethylsiloxy)silane. The non-metallic organic catalysts may be used alone or in combination of two or more.

[0042] Among the curing catalysts of component (C), the metal catalyst is not particularly limited, but those known as curing catalysts for condensation curing organopolysiloxanes can be used. For example, alkyltin ester compounds such as dibutyltin diacetate, dibutyltin dilaurate, dibutyltin dioctoate, dimethyltin dineodecanoate, dioctyltin dineodecanoate, and di-n-butyl-dimethoxytin; titanate esters or titanium chelate compounds such as tetraisopropoxytitanium, tetra-n-butoxytitanium, tetrakis(2-ethylhexoxy)titanium, dipropoxybis(acetylacetonato)titanium, and titanium isopropoxyoctylene glycol; zinc naphthenate, zinc stearate, and zinc-2-ethyloctoate; aluminum isopropylate, aluminum Examples of suitable metal catalysts include alcoholate aluminum compounds such as aluminum alkyl acetate diisopropylate and aluminum bisethylacetoacetate monoacetylacetonate; organometallic compounds such as bismuth neodecanoate (III), bismuth 2-ethylhexanoate (III), bismuth citrate (III), bismuth octylate, iron 2-ethylhexoate, cobalt 2-ethylhexoate, manganese 2-ethylhexoate, and cobalt naphthenate; and lower fatty acid salts of alkali metals such as potassium acetate, sodium acetate, and lithium oxalate. Metal catalysts are not limited to these. Metal catalysts may be used alone or in combination of two or more.

[0043] The (C) component is blended in the first agent, and its blending amount is 0.001 to 10 parts by mass, preferably 0.005 to 8 parts by mass, and more preferably 0.01 to 5 parts by mass, per 100 parts by mass of the total of the (A) and (A') components. If it is less than 0.001 part by mass, good curability cannot be obtained, and the curing speed is slowed down. On the other hand, if the amount exceeds 10 parts by mass, the curing speed of the composition is too fast, shortening the allowable range of the working time after application of the composition and deteriorating the mechanical properties (rubber physical properties) of the obtained cured product (silicone rubber).

[0044] [Component (D): Curing accelerator] Component (D) is an amine compound having a primary amino group (i.e., an amino group having an -NH2 structure, excluding guanidyl groups) and reacts with the β-ketoester compound produced by hydrolysis of component (B) to produce water, thereby significantly improving the deep curing properties of the composition. The component (D) is not particularly limited as long as it has a primary amino group, but specific examples include aliphatic amines such as methylamine, ethylamine, butylamine, pentylamine, hexylamine, heptylamine, octylamine, nonylamine, and dodecylamine; aliphatic polyamines such as ethylenediamine and triethylenetetramine; aromatic amines such as aniline; cyclic aliphatic amines such as cyclopentylamine, cyclohexylamine, and 2-ethylcyclohexylamine; primary amino group-containing silane coupling agents (hydrolyzable organosilane compounds having a primary amino functional group-containing monovalent hydrocarbon group) such as aminosilanes such as γ-aminopropyltrimethoxysilane, γ-aminopropyltriethoxysilane, and 3-2-(aminoethylamino)propyltrimethoxysilane [also known as N-2-(aminoethyl)-3-aminopropyltrimethoxysilane]; and primary amino group-containing organosilicon compounds such as primary amino group-containing polysiloxanes. These may be used alone or in combination of two or more.

[0045] When the (D) component is blended, it may be blended in the first agent, the second agent, or both, and the blending amount is preferably 0 to 20 parts by mass in each of the first agent and the second agent relative to 100 parts by mass of the total of the (A) and (A') components (however, at least 0.1 parts by mass or more is contained in either the first agent or the second agent), and more preferably 0 to 10 parts by mass (however, at least 0.1 parts by mass or more is contained in either the first agent or the second agent). That is, when the (D) component is blended, the total blending amount in the composition is preferably 0.1 to 20 parts by mass, particularly 0.5 to 10 parts by mass, relative to 100 parts by mass of the total of the (A) and (A') components. When the (D) component is added in an amount of less than 0.1 parts by mass, the amount of water generated by reaction with the β-ketoester compound generated by hydrolysis of the (B) component is small, and sufficient deep curing is not expressed, and when it exceeds 20 parts by mass, it is disadvantageous in terms of the characteristics and storage stability of the obtained cured product.

[0046] [Component (E): Inorganic filler] The two-component, room-temperature-curable organopolysiloxane composition of the present invention may optionally contain an inorganic filler (E). The inorganic filler (E) is a reinforcing or non-reinforcing filler that imparts rubber properties to the two-component, room-temperature-curable organopolysiloxane composition of the present invention. Examples of inorganic fillers of component (E) include dry silica such as calcined silica, fused silica, crushed silica, and fumed silica (fumed silica), wet silica such as precipitated silica and sol-gel silica, and silica-based fillers such as crystalline silica (fine powder quartz), diatomaceous earth, carbon black, talc, bentonite, calcium carbonate, zinc carbonate, and magnesium carbonate, calcium oxide, zinc oxide, magnesium oxide, and aluminum hydroxide, which are surface-treated or untreated, and among these, calcium carbonate, fumed silica, precipitated silica, carbon black, and aluminum oxide are preferred, and calcium carbonate, fumed silica, precipitated silica, carbon black, and aluminum oxide, which are surface-treated or untreated, are more preferred.In this case, it is preferred that these inorganic fillers have a low moisture content. There are no particular limitations on the type, amount, treatment method, etc. of the surface treatment agent (hydrophobic treatment agent). Representative examples of the surface treatment agent that can be used include organosilicon compounds such as chlorosilanes, alkoxysilanes, and organosilazanes, fatty acids, paraffins, silane coupling agents, and titanium coupling agents. The inorganic filler of component (E) may use one type alone, or two or more types in combination.

[0047] When the (E) component is blended, it may be blended in the first agent, the second agent, or both, and the blending amount is preferably 0 to 1,000 parts by mass in each of the first agent and the second agent (provided that at least 0.1 parts by mass or more is contained in at least one of the first agent and the second agent) relative to 100 parts by mass of the total of the (A) and (A') components, and more preferably 0 to 500 parts by mass (provided that at least 0.1 parts by mass or more is contained in at least one of the first agent and the second agent). If it is used in an amount of more than 1,000 parts by mass, not only does the viscosity of the composition increase and workability deteriorate, but the rubber strength after curing decreases, making it difficult to obtain rubber elasticity. That is, when the (E) component is blended, the total blending amount in the composition is preferably 0.1 to 1,000 parts by mass, particularly 1 to 500 parts by mass, relative to 100 parts by mass of the total of the (A) and (A') components.

[0048] [Component (F): Adhesion promoter] Component (F) is an adhesion promoter, which is an optional component that can be added as needed, and is used to impart sufficient adhesion to the cured product formed from the two-component room temperature curable organopolysiloxane composition of the present invention. As the adhesion promoter, a known one is suitably used, and examples thereof include silane coupling agents such as functional group-containing hydrolyzable silanes (excluding aminosilanes having a primary amino group described in the above component (B) and curing accelerator (D)), specifically, vinyl silane coupling agents, (meth)acrylic silane coupling agents, epoxy silane coupling agents, mercapto silane coupling agents, isocyanate silane coupling agents, etc., specifically, vinyl tris(β-methoxyethoxy)silane, γ-acryloxypropyl trimethoxysilane, γ-methacryloxypropyl trimethoxysilane, β-(3,4-epoxycyclohexyl)ethyl trimethoxysilane, γ-glycidoxypropyl trimethoxysilane, γ-glycidoxypropyl methyl diethoxysilane, γ-mercaptopropyl trimethoxysilane, 3-isocyanate propyl triethoxysilane, etc. Among these, particularly preferred are (meth)acrylic silanes such as γ-methacryloxypropyltrimethoxysilane and γ-acryloxypropyltrimethoxysilane, epoxy silanes such as γ-glycidoxypropyltrimethoxysilane and β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, and isocyanate silanes such as 3-isocyanatepropyltriethoxysilane.

[0049] When the (F) component is blended, it may be blended in the first agent, the second agent, or both, and the blending amount is preferably 0 to 10 parts by mass in each of the first agent and the second agent (however, at least one of the first agent and the second agent contains 0.001 part by mass or more) relative to 100 parts by mass of the total of the (A) and (A') components, and is particularly preferably 0.1 to 10 parts by mass. When adhesion can be achieved without the use of an adhesion promoter depending on the inorganic filler and the adherend, this need not be used.

[0050] [Other ingredients] The two-component room temperature fast-curing organopolysiloxane composition of the present invention preferably contains components (A), (A'), (B), and (C) as essential components, and further contains components (D), (E), and (F). In addition, known additives such as pigments, dyes, antioxidants, antioxidants, antistatic agents, antimony oxide, and flame retardants such as chlorinated paraffin can be added. Polyethers as thixotropy improvers, fungicides, and antibacterial agents can also be added.

[0051] In addition, the two-component room temperature fast curing organopolysiloxane composition of the present invention may contain an organic solvent as necessary. Examples of the organic solvent include aliphatic hydrocarbon compounds such as n-hexane, n-heptane, isooctane, and isododecane; aromatic hydrocarbon compounds such as toluene and xylene; linear siloxanes such as hexamethyldisiloxane, octamethyltrisiloxane, decamethyltetrasiloxane, dodecamethylpentasiloxane, and 2-(trimethylsiloxy)-1,1,1,2,3,3,3-heptamethyltrisiloxane; and cyclic siloxanes such as octamethylcyclopentasiloxane and decamethylcyclopentasiloxane. The amount of the organic solvent may be appropriately adjusted within a range that does not impede the effects of the present invention.

[0052] [Preparation of two-component room temperature fast curing organopolysiloxane composition] The two-component room temperature fast-curing organopolysiloxane composition of the present invention comprises a first part containing components (A), (B), and (C), and a second part containing component (A') but not components (B) or (C). By forming the composition into a two-component composition consisting of the first part and second part, the composition has excellent fast-curing properties and deep curing properties. This is presumably due to a direct hydrolysis / condensation reaction (crosslinking reaction) occurring when the first and second agents are mixed together. This reaction occurs when the hydrolyzable silyl groups in the organopolysiloxane having a specific structure in which the molecular chain ends of component (A), which is the base polymer in the first agent, are blocked with hydrolyzable silyl groups, or when the organopolysiloxane having a molecular chain end blocked with a silanol group derived from the specific hydrolyzable silane compound in component (B), which is produced by coexisting the organopolysiloxane having a molecular chain end blocked with a silanol group derived from the specific hydrolyzable silane compound in component (B), and the silanol groups in the organopolysiloxane having a molecular chain end blocked with a silanol group in component (A'), which is the base polymer in the second agent, coexist.

[0053] The first agent can be prepared by mixing all of the components (A), (B), and (C) and, if necessary, some or all of the components (D), (E), and (F) and other components in a conventional manner. The second agent can be prepared by mixing all of the component (A') and, if necessary, the remainder or all of the components (D), (E), and (F) and other components in a conventional manner.

[0054] In the base polymers (A) and (A') components, the (A) component is blended in the first agent and the (A') component is blended in the second agent, with the (A) component being blended in the first agent at 10 to 90 parts by mass, particularly 30 to 70 parts by mass, and the (A') component being blended in the second agent at 10 to 90 parts by mass, particularly 30 to 70 parts by mass (wherein the total of the (A) and (A') components is 100 parts by mass). As for this ratio, blending the first agent and the second agent at a mass ratio of 100:10 to 100:100, particularly 100:25 to 100:100 is preferred from the viewpoints of workability and uniformity (ease of mixing) of the composition when the first agent and the second agent are mixed. In addition, the optional components (D), (E), (F) and other components may be blended into either the first agent or the second agent, or into one or both. However, it is particularly preferable to blend the (D), (E), and (F) components into the first agent and the (D) and (E) components into the second agent. When the (D) component is blended into the first and second agents, it is preferable from the viewpoint of the storage stability of the composition to blend the first and second agents in a mass ratio of 1:99 to 99:1, and particularly 30:70 to 70:30. Furthermore, when the (E) component is blended into the first and second agents, the mass ratio of the first and second agents is preferably 80:20 to 20:80, and particularly preferably 60:40 to 40:60, from the viewpoint of uniformity of the composition (ease of mixing) when mixed.

[0055] The two-component room temperature curable organopolysiloxane composition of the present invention can be obtained by uniformly mixing the above-mentioned components and the various additives in the prescribed amounts in a dry atmosphere. Furthermore, because the two-component room temperature curable organopolysiloxane composition of the present invention has storage stability, the first and second parts produced as described above can be stored in an atmosphere free from moisture.

[0056] [Method of curing two-component room temperature fast curing organopolysiloxane composition] The two-component room temperature curable organopolysiloxane composition of the present invention is prepared by mixing these components in an appropriate ratio, specifically, the mass ratio of the first component to the second component is 1:1 to 10:1, and particularly 1:1 to 4:1, and generally cures at room temperature in 10 minutes to 5 days. The two-component room temperature fast-curing organopolysiloxane composition of the present invention has fast curing properties; when molded into a sheet of 2 mm thickness at 23°C and 50% RH, the composition normally cures in 3 to 5 days but cures in a short time of 10 minutes to 3 days. Furthermore, the two-component room temperature fast-curing organopolysiloxane composition of the present invention has deep curing properties; when cured in a glass petri dish having an inner diameter of 10 mm and a depth of 20 mm at 23°C and 50% RH, the composition cures deep within a short period of 30 minutes, whereas a composition that would normally cure deep within (to a measurable thickness) takes two hours.

[0057] The two-component room-temperature curable organopolysiloxane composition of the present invention cures when allowed to stand at room temperature. The molding method, curing conditions, and the like can be any known method and condition suited to a variety of applications and purposes, such as for use in electronic components, on-vehicle applications, and construction applications.

[0058] In the two-component room temperature fast curing organopolysiloxane composition of the present invention, the compounds generated from the crosslinking agent by the hydrolysis reaction during curing are highly safe β-ketoester compounds such as ethyl acetoacetate and diethyl malonate, and are therefore considered to be safe for the human body and the environment. Furthermore, cyclopentanone has a flash point of 35°C, which is higher than that of a dealcohol type that releases an alcohol compound such as methanol when the composition is cured, and is therefore highly safe. Such a two-component room temperature fast curing organopolysiloxane composition of the present invention shows good curability by using various existing catalysts, and the cured product (silicone rubber) also has excellent adhesion.

[0059] Therefore, the two-component room-temperature-curable organopolysiloxane composition of the present invention is useful as an adhesive, sealing agent, potting agent, coating agent, etc. The method for using the two-component room-temperature-curable organopolysiloxane composition of the present invention as an adhesive, sealing agent, potting agent, or coating agent may follow a conventionally known method.

[0060] Examples of target articles include automobile parts, automobile oil seals, electrical and electronic parts, building structures, and civil engineering structures. EXAMPLES

[0061] Synthesis examples, examples and comparative examples are given below to specifically explain the present invention, but the present invention is not limited to the following examples. In the following examples, the viscosity is measured at 23°C using a rotational viscometer in accordance with the method specified in JIS Z 8803.

[0062] [Synthesis Example 1] Synthesis of hydrolyzable organosilane compound 1 In a 2,000mL four-necked separable flask equipped with a mechanical stirrer, a thermometer, and a dropping funnel, 390g (3.0mol) of ethyl acetoacetate, 304g (3.0mol) of triethylamine, and 800ml of hexane were charged, and 160.6g (0.995mol) of vinyltrichlorosilane was dropped over about 2 hours in an ice bath. After stirring for 4 hours at 40°C, the triethylamine hydrochloride formed was removed by filtration, and the filtrate was distilled at 90°C and 300Pa to remove the hexane, excess triethylamine, and ethyl acetoacetate, obtaining hydrolyzable organosilane compound 1 (yield 348g, 78%). This reaction formula is represented by the following formula [2]. [ka]

[0063] [Synthesis Example 2] Synthesis of hydrolyzable organosilane compound 2 In a 2,000mL four-necked separable flask equipped with a mechanical stirrer, a thermometer, and a dropping funnel, 480g (3.0mol) of diethyl malonate, 304g (3.0mol) of triethylamine, and 800ml of hexane were charged, and 148.7g (0.995mol) of methyltrichlorosilane was dropped over about 2 hours in an ice bath. After stirring for 4 hours at 40°C, the triethylamine hydrochloride formed was removed by filtration, and the filtrate was distilled at 120°C and 300Pa to remove hexane, excess triethylamine, and diethyl malonate, obtaining hydrolyzable organosilane compound 2 (yield 280g, 54%). This reaction formula is represented by the following formula [3]. [ka]

[0064] [Example 1] Preparation of first agent a (Component (A)) 50 parts by mass of a dimethylpolysiloxane (a dimethylpolysiloxane in which, in the general formula (1) above, R=methyl group, a=approximately 620) having a viscosity of 20,000 mPa s at 23°C and both molecular chain terminals are blocked with silanol groups (hydroxyl groups bonded to silicon atoms), and (Component (E)) a dimethylpolysiloxane having a BET specific surface area of ​​130 m 2 A first agent a was prepared by uniformly mixing under reduced pressure 5 parts by mass of fumed silica (fumed silica) having a surface treated with dimethyldichlorosilane (1.0 g / g), 3.5 parts by mass of the hydrolyzable organosilane compound 1 obtained in Synthesis Example 1 (component (B)), 0.4 parts by mass of γ-(N,N,N',N'-tetramethylguanidyl)propyltrimethoxysilane (component (C)), and 0.5 parts by mass of γ-aminopropyltrimethoxysilane (component (D)).

[0065] Preparation of second agent a (Component (A')) 50 parts by mass of a dimethylpolysiloxane (a dimethylpolysiloxane in which, in the general formula (1) above, R = methyl group, a = approximately 620) having a viscosity of 20,000 mPa s at 23°C and both molecular chain terminals are blocked with silanol groups (hydroxyl groups bonded to silicon atoms), and (Component (E)) a dimethylpolysiloxane having a BET specific surface area of ​​130 m 2The second agent a was prepared by uniformly mixing 5 parts by mass of fumed silica (fumed silica) having a surface treated with dimethyldichlorosilane (having a molecular weight of 1.0 to 1.2 g) at 200 nm under reduced pressure.

[0066] The first agent a and the second agent a were uniformly mixed at a mixing ratio (mass ratio) of 1:1 to produce composition 1. Composition 1 was left to stand for 1 day and 3 days, respectively, under conditions of 23°C and 50% RH to cure, and these were designated as cured products 1-1 and 1-2.

[0067] [Example 2] Preparation of second agent b (Component (A')) 50 parts by mass of a dimethylpolysiloxane (a dimethylpolysiloxane in which, in the general formula (1) above, R = methyl group, a = approximately 620) having a viscosity of 20,000 mPa s at 23°C and both molecular chain terminals are blocked with silanol groups (hydroxyl groups bonded to silicon atoms), and (Component (E)) a dimethylpolysiloxane having a BET specific surface area of ​​130 m 2 A second agent b was prepared by uniformly mixing 5 parts by mass of fumed silica (fumed silica) having a surface treated with dimethyldichlorosilane (having a molecular weight of 1.0 to 1.2 g) and 2 parts by mass of octylamine (component (D)) under reduced pressure.

[0068] The first agent a prepared in Example 1 and the second agent b described above were uniformly mixed at a mixing ratio (mass ratio) of 1:1 to produce composition 2. Furthermore, composition 2 was left to stand under conditions of 23°C and 50% RH for 1 day and 3 days, respectively, to cure, to give cured products 2-1 and 2-2.

[0069] [Example 3] Preparation of first agent b (Component (A)) 50 parts by mass of a dimethylpolysiloxane (a dimethylpolysiloxane in which, in the general formula (1) above, R=methyl group, a=approximately 620) having a viscosity of 20,000 mPa s at 23°C and both molecular chain terminals are blocked with silanol groups (hydroxyl groups bonded to silicon atoms), and (Component (E)) a dimethylpolysiloxane having a BET specific surface area of ​​130 m 2A first agent b was prepared by uniformly mixing under reduced pressure 5 parts by mass of fumed silica (fumed silica) surface-treated with dimethyldichlorosilane having a molecular weight of 1000 to 1000 g / g, 3.5 parts by mass of the hydrolyzable organosilane compound 1 obtained in Synthesis Example 1 (component (B)), 0.4 parts by mass of γ-(N,N,N',N'-tetramethylguanidyl)propyltrimethoxysilane (component (C)), 0.5 parts by mass of γ-aminopropyltrimethoxysilane (component (D)), and 0.5 parts by mass of γ-glycidoxypropyltrimethoxysilane (component (F)).

[0070] The first agent b and the second agent b prepared in Example 2 were uniformly mixed at a mixing ratio (mass ratio) of 1:1 to produce composition 3. Furthermore, composition 3 was left to stand for 1 day and 3 days, respectively, under conditions of 23°C and 50% RH to cure, and these were designated as cured products 3-1 and 3-2.

[0071] [Example 4] Preparation of first agent c (Component (A)) 50 parts by mass of a dimethylpolysiloxane (a dimethylpolysiloxane in which, in the general formula (1) above, R=methyl group, a=approximately 620) having a viscosity of 20,000 mPa s at 23°C and both molecular chain terminals are blocked with silanol groups (hydroxyl groups bonded to silicon atoms), and (Component (E)) a dimethylpolysiloxane having a BET specific surface area of ​​130 m 2 A first agent c was prepared by uniformly mixing under reduced pressure 5 parts by mass of fumed silica (fumed silica) surface-treated with dimethyldichlorosilane (0.1 g / g), 3.5 parts by mass of the hydrolyzable organosilane compound 2 obtained in Synthesis Example 2 (component (B)), 0.4 parts by mass of γ-(N,N,N',N'-tetramethylguanidyl)propyltrimethoxysilane (component (C)), 0.5 parts by mass of γ-aminopropyltrimethoxysilane (component (D)), and 0.5 parts by mass of γ-glycidoxypropyltrimethoxysilane (component (F)).

[0072] The first agent c and the second agent b prepared in Example 2 were uniformly mixed at a mixing ratio (mass ratio) of 1:1 to produce composition 4. Furthermore, composition 4 was left to stand for 1 day and 3 days, respectively, under conditions of 23°C and 50% RH to cure, and these were designated as cured products 4-1 and 4-2.

[0073] [Comparative Example 1] Preparation of first agent d (Component (A)) 50 parts by mass of a dimethylpolysiloxane (a dimethylpolysiloxane in which, in the general formula (1) above, R=methyl group, a=approximately 620) having a viscosity of 20,000 mPa s at 23°C and both molecular chain terminals are blocked with silanol groups (hydroxyl groups bonded to silicon atoms), and (Component (E)) a dimethylpolysiloxane having a BET specific surface area of ​​130 m 2 A first agent d was prepared by uniformly mixing under reduced pressure 5 parts by mass of fumed silica (fumed silica) surface-treated with dimethyldichlorosilane (1.0 g / g), 2.5 parts by mass of vinyltrimethoxysilane, 0.05 parts by mass of dioctyltin dilaurate (component (C)), 0.5 parts by mass of γ-aminopropyltrimethoxysilane (component (D)), and 0.5 parts by mass of γ-glycidoxypropyltrimethoxysilane (component (F)).

[0074] The first agent d and the second agent b prepared in Example 2 were uniformly mixed at a mixing ratio (mass ratio) of 1:1 to produce composition 5. Furthermore, composition 5 was left to stand for 1 day and 3 days, respectively, under conditions of 23°C and 50% RH to cure, and these were designated as cured products 5-1 and 5-2.

[0075] [Comparative Example 2] Preparation of first agent e (Component (A)) 50 parts by mass of a dimethylpolysiloxane (a dimethylpolysiloxane in which, in the general formula (1) above, R=methyl group, a=approximately 620) having a viscosity of 20,000 mPa s at 23°C and both molecular chain terminals are blocked with silanol groups (hydroxyl groups bonded to silicon atoms), and (Component (E)) a dimethylpolysiloxane having a BET specific surface area of ​​130 m 2 A first agent e was prepared by uniformly mixing under reduced pressure 5 parts by mass of fumed silica (fumed silica) surface-treated with dimethyldichlorosilane (1.0 g / g), 3.5 parts by mass of vinyltris(methylethylketoxime)silane, 0.05 parts by mass of dioctyltin dilaurate (component (C)), 0.5 parts by mass of γ-aminopropyltrimethoxysilane (component (D)), and 0.5 parts by mass of γ-glycidoxypropyltrimethoxysilane (component (F)).

[0076] The first agent e and the second agent b prepared in Example 2 were uniformly mixed at a mixing ratio (mass ratio) of 1:1 to produce composition 6. Furthermore, composition 6 was left to stand for 1 day and 3 days, respectively, under conditions of 23°C and 50% RH to cure, and these were designated as cured products 6-1 and 6-2.

[0077] [Test Method] The compositions prepared in Examples 1 to 4 and Comparative Examples 1 and 2 were used to evaluate the curability, rubber properties, and adhesion by the methods described below.

[0078] [Curability] Tuck Free Time: Using each of the compositions prepared in Examples 1 to 4 and Comparative Examples 1 and 2, the tack-free time (dry time to touch) was measured according to the method specified in JIS A-5758.

[0079] Deep hardening: Each composition prepared in Examples 1 to 4 and Comparative Examples 1 and 2 was filled into a glass petri dish having an inner diameter of 10 mm and a depth of 20 mm, and after 20 minutes at 23°C and 50% RH, the thickness from the surface exposed to air to the cured part was measured to evaluate deep curability.

[0080] Initial sealability: To compare the curing properties, the initial sealability was measured. The initial sealability was tested by using a pressure vessel similar to the flange pressure vessel for pressure test specified in JIS K-6820 as a test device and performing a pressure test. The pressure vessel was composed of an upper vessel having an upper flange with an inner diameter of 58 mm, an outer diameter of 80 mm, and a thickness of 10 mm, and a lower vessel having a lower flange with the same dimensions as the upper flange, and a ring-shaped notch with a width of 3 mm and a depth of 3 mm was provided along the circumference at the inner side edge of the seal surface of the lower flange. The seal surface of this lower flange was washed with toluene. Then, the composition was applied in a bead shape to the center of the lower seal surface in an amount sufficient to fully fill the seal surface. Immediately after application, the upper vessel was placed on the lower vessel so that the seal surfaces of the upper and lower flanges were in contact with each other, and an iron spacer with a height of 21 mm (in the thickness direction of the flange) was installed to define the distance between the seal surfaces of the upper and lower flanges, and four tightening bolts were installed. The spacer creates a gap of 1 mm between the sealing surfaces, which is intended to make the pressure resistance test for the sealant more severe, i.e., to make it an accelerated test. After curing for 30 minutes at 23°C and 50% RH, gas was introduced from the upper pressure port to measure the gas pressure that the sealant, which is the cured product of the composition, could withstand. Those with a pressure of 400 kPa or more were judged to pass.

[0081] [Rubber properties] Immediately after preparation, each composition prepared in Examples 1 to 4 and Comparative Examples 1 and 2 was extruded into a sheet having a thickness of 2 mm and exposed to air at 23°C and 50% RH, and the sheet was then left in the same atmosphere for 1 or 3 days to obtain a cured product, whose rubber properties (hardness, elongation at break, tensile strength) were measured in accordance with JIS K-6249. The hardness was measured using a JIS K-6249 durometer A hardness tester.

[0082] [Adhesiveness] The compositions prepared in Examples 1 to 4 and Comparative Examples 1 and 2 were used to bond aluminum or glass specimens measuring 25 mm in width and 100 mm in length to each other, and the adhesive bonded the specimens to each other with the same adhesive. 2Shear adhesion test specimens were prepared with a bond thickness of 1 mm and aged at 23°C and 50% RH for one or three days. After this, the shear adhesive strength of these test specimens to aluminum or glass was measured in accordance with the method specified in JIS K-6249.

[0083] The test results of Examples 1 to 4 are shown in Table 1, and the test results of Comparative Examples 1 and 2 are shown in Table 2. Tables 1 and 2 also show the compounds that are released from the curing agent during curing, and whether or not the compounds are harmful to health and the environment.

[0084] [Table 1]

[0085] [Table 2]

[0086] From the above results, it can be seen that the two-component, room temperature fast-curing organopolysiloxane compositions of the present invention (the compositions of Examples 1 to 4) exhibit high values ​​for deep curing ability and initial sealability, and there is little difference in the rubber properties and adhesive strength between the one-day and three-day cures, and therefore have high curing ability compared to the conventional dealcohol-free (composition of Comparative Example 1) and oxime-free (composition of Comparative Example 2) cure forms. In addition, the compounds released during the curing of the compositions of the examples are ethyl acetoacetate or diethyl malonate, which are highly safe compounds with no reported health hazards such as carcinogenicity or reproductive toxicity to the human body, or environmental hazards such as toxicity to aquatic organisms. On the other hand, the compounds released during the curing of the compositions of the comparative examples are all designated as hazardous substances and highly harmful to the human body, and are methanol, which is likely to be carcinogenic and toxic to aquatic organisms, and 2-butanone oxime, which is toxic to aquatic organisms, and whose health hazards are indicated in SDS (Safety Data Sheet) or the like. In addition, since methanol has a lower flash point and boiling point than β-ketoester compounds, it can be seen that the two-component room temperature fast curing organopolysiloxane composition of the present invention is superior in terms of human health and environmental protection.

Claims

1. (A) an organopolysiloxane represented by the following general formula (1), (2), or (3): 10 to 90 parts by mass (provided that the total of components (A) and (A′) is 100 parts by mass); 【Chemistry 1】 (In the formula, R may be the same or different and is an unsubstituted or halogen atom-substituted monovalent hydrocarbon group having 1 to 10 carbon atoms, and n is an integer of 5 or more.) 【Chemistry 2】 (In the formula, R is as defined above, n1 is an integer of 3 or more, n2 is an integer of 1 or more, m is an integer from 1 to 10, and n1+m+(m×n2) is an integer of 5 or more.) 【Chemistry 3】 (In the formula, R and n are as defined above, X is an oxygen atom or an alkylene group having 2 to 5 carbon atoms, and k is independently 0 or 1 for each silicon atom to which it is bonded.) (B) a hydrolyzable organosilane compound represented by the following general formula (4) and / or a partial hydrolysis condensate thereof: 0.1 to 30 parts by mass per 100 parts by mass of the total of the components (A) and (A′), 【Chemistry 4】 (In the formula, R 1 and R 3 are each independently a monovalent hydrocarbon group having 1 to 10 carbon atoms; R 2 each independently represents a monovalent aliphatic hydrocarbon group having 1 to 10 carbon atoms which may have an ether-bonded oxygen atom, an aryl group having 6 to 10 carbon atoms which may have an ether-bonded oxygen atom, or an aralkyl group having 7 to 10 carbon atoms which may have an ether-bonded oxygen atom; and a is 3 or 4. And, (C) Curing catalyst: 0.001 to 10 parts by mass per 100 parts by mass of the total of the components (A) and (A'). A first agent comprising (A') an organopolysiloxane represented by the following general formula (1) or (2): 10 to 90 parts by mass (the total of components (A) and (A') is 100 parts by mass); 【Chemistry 5】 (In the formula, R may be the same or different and is an unsubstituted or halogen atom-substituted monovalent hydrocarbon group having 1 to 10 carbon atoms, and n is an integer of 5 or more.) 【Chemistry 6】 (In the formula, R is as defined above, n1 is an integer of 3 or more, n2 is an integer of 1 or more, m is an integer from 1 to 10, and n1+m+(m×n2) is an integer of 5 or more.) and a second agent containing the above formula (1), and the composition does not contain a silane and / or siloxane having three or more alkenoxysilyl groups in the molecule.

2. The two-component room-temperature fast-curing organopolysiloxane composition according to claim 1, further comprising an amine compound having a primary amino group (D) as a curing accelerator, which is contained in each of the first and second agents in an amount of 0 to 20 parts by mass per 100 parts by mass of the total of the components (A) and (A') (with the proviso that at least one of the first and second agents contains 0.1 part by mass or more).

3. 3. The two-component room-temperature fast-curing organopolysiloxane composition according to claim 1, wherein the hydrolyzable organosilane compound and / or partial hydrolysis condensate thereof, component (B), is a compound that releases a β-ketoester compound upon hydrolysis.

4. 4. The two-component room-temperature fast-curing organopolysiloxane composition according to claim 3, wherein the β-ketoester compound that is eliminated is methyl acetoacetate, ethyl acetoacetate, propyl acetoacetate, allyl acetoacetate, phenyl acetoacetate, benzyl acetoacetate, dimethyl malonate, diethyl malonate, dipropyl malonate, dipentyl malonate, diallyl malonate, diphenyl malonate, or dibenzyl malonate.

5. The two-component room-temperature fast-curing organopolysiloxane composition according to any one of claims 1 to 4, further comprising 0 to 1,000 parts by mass of an inorganic filler (E) in each of the first and second agents, relative to 100 parts by mass of the total of the components (A) and (A') (with the proviso that at least 0.1 part by mass or more is contained in at least one of the first and second agents).

6. 6. The two-component room temperature fast-curing organopolysiloxane composition according to claim 5, wherein component (E) is one or more inorganic fillers selected from the group consisting of calcium carbonate, fumed silica, precipitated silica, carbon black, and aluminum oxide.

7. The two-component room-temperature fast-curing organopolysiloxane composition according to any one of claims 1 to 6, further comprising 0 to 10 parts by mass of an adhesion promoter (F) in each of the first and second agents, relative to 100 parts by mass of the total of the components (A) and (A') (with the proviso that at least one of the first and second agents contains 0.001 part by mass or more).

8. 8. The two-component room temperature fast-curing organopolysiloxane composition according to claim 1, wherein the blending ratio of the first agent to the second agent is from 1:1 to 10:1 by mass.

9. A two-component room temperature fast-curing organopolysiloxane composition described in any one of claims 1 to 8, wherein R 2 in general formula (4) of component (B) is a monovalent aliphatic hydrocarbon group having 1 to 10 carbon atoms and having an ether-bonded oxygen atom, an aryl group having 6 to 10 carbon atoms and having an ether-bonded oxygen atom, or an aralkyl group having 7 to 10 carbon atoms and having an ether-bonded oxygen atom.

10. 10. An automobile part comprising a cured product of the two-component room temperature fast curing organopolysiloxane composition according to any one of claims 1 to 9.

11. 10. An oil seal for automobiles comprising a cured product of the two-component room temperature fast curing organopolysiloxane composition according to any one of claims 1 to 9.

12. 10. An electric or electronic part comprising a cured product of the two-component room temperature fast curing organopolysiloxane composition according to any one of claims 1 to 9.

13. 10. A building structure comprising a cured product of the two-component room temperature fast curing organopolysiloxane composition according to any one of claims 1 to 9.

14. 10. A civil engineering structure comprising a cured product of the two-component room temperature fast curing organopolysiloxane composition according to any one of claims 1 to 9.

15. An adhesive comprising the two-component room temperature fast curing organopolysiloxane composition according to any one of claims 1 to 9.

16. A sealant comprising the two-component room temperature fast curing organopolysiloxane composition according to any one of claims 1 to 9.

17. A potting agent comprising the two-component room temperature fast curing organopolysiloxane composition according to any one of claims 1 to 9.

18. A coating agent comprising the two-component room temperature fast curing organopolysiloxane composition according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Novel silicone compound

    JP1985041684A

  • Room temperature-curable organopolysiloxane composition

    JP1990199170A

  • Room temperature fast-curing organopolysiloxane composition and its curing method

    JP2008280525A

  • Two-part mixing type organopolysiloxane composition

    JP2011037968A

  • Method for producing room temperature-curable organopolysiloxane composition, and automobile oil seal, building sealant and electrical and electronic component using cured product of the composition

    JP2015021019A