Epoxy resin and its manufacturing method
By converting 3,3'-diglycidyl biphenyl-4,4'-diglycidyl ether into a solid form with controlled molecular weight distribution, the resin achieves enhanced elastic modulus and shear adhesion, addressing handling difficulties and improving industrial applicability.
Patent Information
- Application Number
- JP2021508953
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-03-25
- Filing Date
- 2020-03-09
- Publication Date
- 2024-09-26
- Estimated Expiration
- 2040-03-09
AI Technical Summary
The existing epoxy resin containing 3,3'-diglycidyl biphenyl-4,4'-diglycidyl ether is liquid at room temperature, making it difficult to handle industrially and posing a heavy industrial load, while also lacking sufficient elastic modulus and shear adhesion.
The production method involves converting 3,3'-diglycidyl biphenyl-4,4'-diglycidyl ether into a solid form by controlling the molecular weight distribution using Claisen rearrangement and purification techniques, specifically adjusting the content of components with a standard polystyrene equivalent molecular weight between 60.8 and 25% through methods like crystallization and using a basic compound, to enhance elastic modulus and shear adhesion.
The resulting epoxy resin maintains excellent heat resistance and moldability, is easily handled as a solid, and exhibits improved elastic modulus and shear adhesive strength, suitable for industrial applications.
Smart Images

Figure 0007556347000033 
Figure 0007556347000034 
Figure 0007556347000020
Abstract
Description
[Technical field]
[0001] The present invention relates to an epoxy resin and a method for producing the same. [Background technology]
[0002] Epoxy resin is a thermosetting synthetic resin with reactive epoxy groups at the terminals. When epoxy resin reacts with a curing agent, it becomes an infusible, three-dimensional cured product. However, by blending various modifiers such as fillers, flexibility agents, and diluents, it can be used to meet various performance requirements, and is therefore used in a wide range of applications as a high-performance, multifunctional resin.
[0003] There are various methods for producing this type of epoxy resin. For example, Patent Document 1 (JP 2015-166335 A) discloses a method for producing an epoxy compound, which comprises reacting hydrogen peroxide with the carbon-carbon double bond of a compound having a carbon-carbon double bond to epoxidize the compound in the presence of at least one of a tungsten compound and a molybdenum compound, and an onium salt, wherein the onium salt has four or more acyloxy groups having 1 to 4 carbon atoms or one or more benzyloxy groups, and the total number of carbon atoms in the onium salt is 20 or more.
[0004] Meanwhile, polyfunctional epoxide resins obtained by epoxidizing 3,3'-diallylbiphenyl-4,4'-diglycidyl ether (the following formula (4)) are known as epoxy resins. For example, Patent Document 2 (Japanese Patent No. 2539648) discloses 3,3'-diglycidylbiphenyl-4,4'-diglycidyl ether (the following formula (1)) as a polyfunctional epoxide resin obtained by epoxidizing a diallyl diglycidyl ether intermediate. Specifically, as a method for producing 3,3'-diglycidylbiphenyl-4,4'-diglycidyl ether (formula (1) below), a method is disclosed in which 3,3'-diallylbiphenyl-4,4'-diglycidyl ether (formula (4) below) and sodium acetate in chloroform are introduced into a sulfonation flask, peracetic acid is added dropwise at room temperature over about 2 hours, the reaction mixture is stirred after the dropwise addition is completed, chloroform is then added, the organic phase is washed several times with water until it becomes neutral, dried, filtered, and concentrated in a vacuum to obtain 3,3'-diglycidylbiphenyl-4,4'-diglycidyl ether (formula (1) below).
[0005] Formula (1) JPEG0007556347000001.jpg79150
[0006] Formula (4) JPEG0007556347000002.jpg68136 [Prior art documents] [Patent documents]
[0007] [Patent Document 1] JP 2015-166335 A [Patent Document 2] Patent No. 2539648 Summary of the Invention [Problem to be solved by the invention]
[0008] 3,3'-diglycidylbiphenyl-4,4'-diglycidyl ether (the above formula (1)) disclosed in Patent Document 2 has four epoxy groups in one molecule, and is characterized by excellent heat resistance, low viscosity, and excellent moldability, despite being polyfunctionalized. However, the epoxy resin obtained by the production method disclosed in Patent Document 2 is liquid at room temperature, and therefore is difficult to handle industrially, and there is a problem that the industrial load is too large.
[0009] Therefore, an object of the present invention is to provide a new epoxy resin containing 3,3'-diglycidylbiphenyl-4,4'-diglycidyl ether (formula (1)), which can be handled as a solid and has excellent elastic modulus and shear adhesive strength, and a method for producing the same. [Means for solving the problem]
[0010] The present invention proposes an epoxy resin containing 3,3'-diglycidylbiphenyl-4,4'-diglycidyl ether (also referred to as "compound of formula (1)") represented by the following formula (1), characterized in that the epoxy resin contains 9 area % or more and 25 area % or less of components having a standard polystyrene equivalent molecular weight of 60.8 or more in gel permeation chromatography (referred to as "GPC") using an RI detector.
[0011] The present invention also relates to an epoxy resin containing a compound represented by the following formula (5): The present invention proposes an epoxy resin characterized in that it contains components having a standard polystyrene equivalent molecular weight of 60.8 or more in an amount of 9 area % to 25 area % when measured by gel permeation chromatography (referred to as "GPC") using an RI detector.
[0012] The present invention further proposes that, in the epoxy resin, the component having a standard polystyrene-equivalent molecular weight of 60.8 or more as measured by GPC is a compound having two or more biphenyl skeletons.
[0013] The present invention also provides an epoxy resin composition comprising the above-mentioned epoxy resin and an epoxy curing agent in a ratio of 0.80 equivalents or more and 1.03 equivalents or less based on the functional group equivalent of the epoxy resin. The present invention further provides a cured product obtained by curing the above epoxy resin composition.
[0014] The present invention also proposes a method for producing an epoxy resin, comprising the steps of converting a compound represented by the following formula (2) (also referred to as "compound of formula (2)") into a compound represented by the following formula (3) (also referred to as "compound of formula (3)"), then converting the compound of formula (3) into a compound represented by the following formula (4) (also referred to as "compound of formula (4)"), and then converting the compound of formula (4) into a compound of formula (1) represented by the following formula (1), to obtain an epoxy resin, characterized in that the content of components having a molecular weight of 60.8 or more in terms of standard polystyrene in GPC is 9 area % or more and 25 area % or less when measured using an RI detector.
[0015] Formula (1) JPEG0007556347000003.jpg61129
[0016] Formula (2) JPEG0007556347000004.jpg62129
[0017] Formula (3) JPEG0007556347000005.jpg59109
[0018] Formula (4) JPEG0007556347000006.jpg68140
[0019] The present invention further proposes a method for producing an epoxy resin, comprising converting the compound of formula (2) into the compound of formula (3) by a Claisen rearrangement reaction in the presence of a basic compound. The present invention further proposes a method for producing an epoxy resin, comprising adding and reacting the basic compound in a ratio of 1.0 mole or more and 100 moles or less with respect to 1.0 mole of the compound of formula (2). The present invention further proposes the method for producing an epoxy resin, wherein the basic compound is an aniline compound.
[0020] The present invention further proposes a method for producing an epoxy resin, characterized in that after the reaction of converting the compound of formula (2) into the compound of formula (3) and before the reaction of converting the compound of formula (3) into the compound of formula (4), a purification step is carried out to separate and remove components other than the compound of formula (3).
[0021] The present invention further proposes a method for producing an epoxy resin, characterized in that after the reaction of converting the compound of formula (3) into the compound of formula (4) and before the reaction of converting the compound of formula (4) into the compound of formula (1), a purification step is carried out to separate and remove components other than the compound of formula (4).
[0022] The present invention further proposes a method for producing an epoxy resin, characterized in that, after the reaction of converting the compound of formula (4) into the compound of formula (1), a purification step is carried out to separate and remove components other than the compound of formula (1).
[0023] The present invention further proposes a method for producing an epoxy resin, characterized in that the purification is carried out by crystallization.
[0024] The present invention also relates to a method for producing an epoxy resin, comprising the steps of converting a compound represented by the following formula (6) (also referred to as a "formula (6) compound") into a compound represented by the following formula (7) (also referred to as a "formula (7) compound"), then converting the formula (7) compound into a compound represented by the following formula (8) (also referred to as a "formula (8) compound"), and then converting the formula (8) compound into a formula (5) compound represented by the following formula (5), thereby obtaining an epoxy resin, The present invention proposes a method for producing an epoxy resin, characterized in that the content in the epoxy resin of components having a standard polystyrene-equivalent molecular weight of 60.8 or more is 9 area % or more and 25 area % or less when measured by GPC using an RI detector.
[0025] [Formula (5)] TIFF0007556347000007.tif73122
[0026] In formula (5), X is a divalent linking group selected from -SO2-, -O-, -CO-, -C(CF3)2-, -S-, or a hydrocarbon group having 1 to 20 carbon atoms.
[0027] [Formula (6)] TIFF0007556347000008.tif77127
[0028] In formula (6), X is a divalent linking group selected from -SO2-, -O-, -CO-, -C(CF3)2-, -S-, or a hydrocarbon group having 1 to 20 carbon atoms.
[0029] [Formula (7)] TIFF0007556347000009.tif77127
[0030] In formula (7), X is a divalent linking group selected from -SO2-, -O-, -CO-, -C(CF3)2-, -S-, or a hydrocarbon group having 1 to 20 carbon atoms.
[0031] [Formula (8)] TIFF0007556347000010.tif77127
[0032] In formula (8), X is a divalent linking group selected from -SO2-, -O-, -CO-, -C(CF3)2-, -S-, or a hydrocarbon group having 1 to 20 carbon atoms.
[0033] The present invention further proposes a method for producing an epoxy resin, comprising converting the compound of formula (6) into the compound of formula (7) by a Claisen rearrangement reaction in the presence of a basic compound.
[0034] The present invention further proposes a method for producing an epoxy resin, comprising adding and reacting the basic compound in a ratio of 1.0 mole or more and 100 moles or less with respect to 1.0 mole of the compound of formula (6).
[0035] The present invention further proposes a method for producing an epoxy resin, wherein the basic compound is an aniline compound.
[0036] The present invention further proposes a method for producing an epoxy resin, characterized in that after the reaction for converting the compound of formula (6) into the compound of formula (7) and before the reaction for converting the compound of formula (7) into the compound of formula (8), a purification step is carried out to separate and remove components other than the compound of formula (7).
[0037] The present invention further proposes a method for producing an epoxy resin, characterized in that after the reaction for converting the compound of formula (7) into the compound of formula (8) and before the reaction for converting the compound of formula (8) into the compound of formula (5), a purification step is carried out to separate and remove components other than the compound of formula (8).
[0038] The present invention further proposes a method for producing an epoxy resin, characterized in that, after the reaction of converting the compound of formula (8) into the compound of formula (5), a purification step is carried out to separate and remove components other than the compound of formula (5).
[0039] The present invention further proposes a method for producing an epoxy resin, characterized in that the purification is carried out by crystallization. Effect of the Invention
[0040] The epoxy resin proposed by the present invention and the epoxy resin obtained by the production method proposed by the present invention are epoxy resins containing 3,3'-diglycidylbiphenyl-4,4'-diglycidyl ether represented by the above formula (1), i.e., the compound of formula (1), and therefore retain the characteristics of excellent heat resistance and moldability. In addition, the epoxy resin proposed by the present invention and the epoxy resin obtained by the production method proposed by the present invention are epoxy resins containing the compound of formula (5), and therefore have the characteristics of excellent heat resistance and moldability. The epoxy resin proposed by the present invention and the epoxy resin obtained by the production method proposed by the present invention can be handled as a solid and have excellent elastic modulus and shear adhesive strength, and therefore are easy to handle industrially and can be suitably used industrially. [Brief description of the drawings]
[0041] [Figure 1] FIG. 1 is a process diagram showing an example of a method for producing an epoxy resin according to an embodiment of the present invention. [Diagram 2] FIG. 2 is a diagram listing the structural formulas of compounds contained in oligomer component X described below. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0042] <This epoxy resin> An epoxy resin according to one embodiment of the present invention (referred to as "the present epoxy resin") is an epoxy resin containing a compound represented by the following formula (1), and is an epoxy resin containing a component having a predetermined molecular weight (referred to as "oligomer component X") in a predetermined ratio. The epoxy resin of the present invention is an epoxy resin containing a compound having a molar molecular weight of 410, and is an epoxy resin in an uncured state that is not substantially crosslinked, that is, is not intentionally crosslinked.
[0043] Formula (1) JPEG0007556347000011.jpg61129
[0044] (Oligomer component X) The epoxy resin preferably contains 9 area % or more, more preferably 10 area % or more, and even more preferably 15 area % or more, of the components having a standard polystyrene equivalent molecular weight of 60.8 or more ("oligomer component X") in GPC measured using an RI detector, while the epoxy resin preferably contains 25 area % or less, more preferably 20 area % or less, and even more preferably 18 area % or less. When the area ratio of the oligomer component X in the present epoxy resin is 9 area % or more, the energy required for melting can be reduced, and when it is 25 area % or less, the present epoxy resin can be made solid at room temperature and further can be made excellent in elastic modulus and shear adhesive strength.
[0045] The oligomer component X is a compound having two or more biphenyl skeletons, and may be composed of two or more kinds of compounds having two or more biphenyl skeletons. The oligomer component X is not particularly limited as long as it is a compound having two or more biphenyl skeletons, but is preferably a component composed of at least one compound having a molar molecular weight of 819, 805, or 765, and more preferably composed of a compound having a molar molecular weight of 833 or 847. The compound with a molar molecular weight of 847 is presumed to be produced when N,N-diethylaniline is used in the Claisen rearrangement step, and the compound with a molar molecular weight of 833 is presumed to be produced when N,N-dimethylaniline is used.
[0046] Examples of compounds contained in the oligomer component X include compounds having a chemical structure shown in Figure 2. Note that some or all of the double bonds in the structural formula shown in Figure 2 may be oxidized and converted to epoxy groups, and it is preferable that all of them are converted to epoxy groups.
[0047] (Melting Point) The melting point of the present epoxy resin obtained from the DSC curve is preferably 50° C. or higher, more preferably 60° C. or higher. The upper limit is about 100° C. If the melting point of the epoxy resin obtained from the DSC curve is 50°C or higher, it will be in a solid state at room temperature, and therefore it will be easy to handle industrially, which is preferable. If the melting point is 100°C or lower, it will be possible to melt the epoxy resin without requiring a large amount of energy, and it will be easy to maintain the epoxy resin in a liquid state during the process of preparing the epoxy resin composition before curing, which is preferable. In order to adjust the melting point of the present epoxy resin obtained from the DSC curve to 50° C. or higher, the area ratio of the oligomer component X in the present epoxy resin may be set to 9 area % or more and 25 area % or less, as described above.
[0048] <This manufacturing method> Next, a preferred example of a method for producing the present epoxy resin (hereinafter referred to as "the present production method") will be described. However, the method for producing the present epoxy resin is not limited to the following present production method.
[0049] The present production method is a method for producing an epoxy resin comprising a series of steps of converting a compound of formula (2) into a compound of formula (3) (this reaction step is referred to as "step A"), then converting the compound of formula (3) into a compound of formula (4) (this reaction step is referred to as "step B"), and then converting the compound of formula (4) into a compound of formula (1) to obtain an epoxy resin (this reaction step is referred to as "step C"). The method is characterized in that the content of oligomer component X in the epoxy resin, for example, the present epoxy resin, is 9 area % or more and 25 area % or less when measured using an RI detector.
[0050] Formula (2) JPEG0007556347000012.jpg62129
[0051] Formula (3) JPEG0007556347000013.jpg59109
[0052] Formula (4) JPEG0007556347000014.jpg68138
[0053] Formula (1) JPEG0007556347000015.jpg61129
[0054] In the present manufacturing method, the steps A, B, and C may be performed in series by devices connected to each other by a transport means, or may be performed at intervals in different devices. Furthermore, as long as the present manufacturing method includes the steps A, B, and C, it is possible to insert other steps or other processes as appropriate.
[0055] (Process A) The step A, that is, the reaction method for converting the compound of formula (2) to the compound of formula (3), can be carried out by a Claisen rearrangement reaction. Although the Claisen rearrangement reaction is influenced by the solvent and additives used, the reaction can generally be advanced by heating to a temperature of 100 to 300° C. From the viewpoint of shortening the reaction time, it is preferable to heat to a temperature of 150° C. or higher, and in order to suppress side reactions under high temperature conditions, it is preferable to heat to a temperature of 250° C. or lower. Among these, it is particularly preferable to heat to a temperature of 170° C. or higher or 220° C. or lower.
[0056] A solvent is not necessarily required in this step, but a solvent can be used. From the viewpoint of process safety, it is preferable to use a solvent since it has the advantage that the heat of reaction of the Claisen rearrangement reaction can be absorbed by the latent heat of vaporization of the solvent, thereby suppressing an increase in the internal temperature. The solvent used in this step is not particularly limited as long as it has a boiling point higher than the reaction temperature, is stable at the reaction temperature, and is inactive against the compound of formula (2) and the compound of formula (3). Specific examples of the solvent include aromatic hydrocarbons such as toluene, xylene, mesitylene, anisole, etc.; aliphatic chain hydrocarbons such as octane, nonane, decane, undecane, dodecane, etc.; aliphatic cyclic hydrocarbons such as cyclooctane, ethylcyclohexane, decalin, etc.; amides such as N,N-dimethylformamide, N,N-dimethylacetamide, etc.; dimethylsulfoxide; and mixtures of these solvents.
[0057] The compound of formula (2) may be obtained in any manner. It may be a commercially available product, or it may be synthesized by reacting biphenol with an allyl halide such as allyl chloride or allyl bromide in the presence of a base.
[0058] (Process B) The step B, that is, the reaction step of converting the compound of formula (3) to the compound of formula (4), can be carried out using a method currently known as a glycidylation technique. For example, it can be carried out by reacting epihalohydrin in the presence of a base, or by adding epihalohydrin in the presence of an acid catalyst, followed by dehydrohalogenation with a base.
[0059] Examples of the epihalohydrin include epichlorohydrin and epibromohydrin, with epichlorohydrin being preferred because it is easily available on an industrial scale. The amount of epihalohydrin used is preferably 1 to 100 equivalents relative to the compound of formula (3). Of these, from the viewpoint of improving reaction selectivity, 5 equivalents or more is preferable, and from the viewpoint of improving productivity per batch, 50 equivalents or less is preferable. Of these, 10 equivalents or more or 40 equivalents or less is more preferable, and 20 equivalents or more or 35 equivalents or less is particularly preferable.
[0060] The reaction can generally proceed by heating to a temperature of -50 to 200°C. From the viewpoint of shortening the reaction time, a temperature of 0°C or higher is preferable, and in order to suppress side reactions under high temperature conditions, a temperature of 150°C or lower is preferable. Among these, heating to a temperature of 40°C or higher or 100°C or lower is particularly preferable.
[0061] Examples of the base include alkali metal hydroxides such as lithium hydroxide, sodium hydroxide, and potassium hydroxide, and alkaline earth metal hydroxides such as magnesium hydroxide, calcium hydroxide, and barium hydroxide. Among these, potassium hydroxide and sodium hydroxide are preferred from the viewpoint of reaction efficiency. The amount of the base used is preferably 1 to 20 equivalents relative to the compound of formula (3). Of these, from the viewpoint of improving the yield, 1.5 equivalents or more is preferable, and in order to avoid complicated removal, 5 equivalents or less is preferable. Of these, 1.8 equivalents or more or 2.5 equivalents or less is particularly preferable. The base may be used as a solid, but is preferably used in the form of a solution from the viewpoint of improving reactivity.
[0062] Examples of the catalyst that can be used include quaternary ammonium salts such as tetramethylammonium chloride and tetraethylammonium bromide; tertiary amines such as benzyldimethylamine and 2,4,6-(trisdimethylaminomethyl)phenol; imidazoles such as 2-ethyl-4-methylimidazole and 2-phenylimidazole; phosphonium salts such as ethyltriphenylphosphonium iodide; and phosphines such as triphenylphosphine.
[0063] As the solvent, epihalohydrin can be used as the solvent, or alcohols such as methanol, ethanol, propanol, isopropanol, n-propanol, isopropanol, n-butanol, isobutanol, sec-butanol, and t-butanol; ketones such as acetone, methyl ethyl ketone, methyl isobutyl ketone, cyclopentanone, cyclohexanone, and 2-pentanone; glycol ethers such as ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monopropyl ether, ethylene glycol monobutyl ether, propylene glycol monomethyl ether, and propylene glycol monoethyl ether; aromatics such as benzene, xylene, and toluene; aromatic alcohols such as benzyl alcohol; glycol ether acetates such as ethylene glycol monomethyl ether acetate and propylene glycol monomethyl ether acetate; ethers such as 1,3-dioxane, 1,4-dioxane, diethyl ether, and tetrahydrofuran; amides such as N,N-dimethylformamide and N,N-dimethylacetamide; dimethyl sulfoxide, water, and the like may be used. These may be used alone or in combination. As described above, from the viewpoint of reaction efficiency, it is preferable to use a solvent in which the base is easily soluble, and therefore alcohols, ketones, glycol ethers, glycol ether acetates, ethers, amides, and water are preferred, and among these, alcohols and water are preferred.
[0064] (Process C) The step C, that is, the reaction step of converting the compound of formula (4) into the compound of formula (1), may be carried out by any method.
[0065] An example of the optional method is a method in which phosphoric acids or phosphonic acids, an onium salt as a phase transfer catalyst, and at least one of a tungsten compound and a molybdenum compound are allowed to coexist as a catalyst composition, and oxidation is performed using hydrogen peroxide as an oxidizing agent. Also included is a method of oxidation using a peracid such as peracetic acid or m-chloroperbenzoic acid. Further, there can be mentioned a method in which hydrogen peroxide is reacted with an organic nitrile compound in the presence of an alkali metal carbonate or hydrogen carbonate.
[0066] Among these, a method in which phosphoric acids or phosphonic acids are allowed to coexist as a catalyst composition with an onium salt as a phase transfer catalyst, and at least one of a tungsten compound and a molybdenum compound, and hydrogen peroxide is used as an oxidizing agent, is preferred, since it does not require the use of an excessive amount of an oxidizing agent and is therefore safe.
[0067] Examples of the phosphoric acids include inorganic phosphoric acids such as phosphoric acid, polyphosphoric acid, and picophosphoric acid; inorganic phosphates such as sodium phosphate, potassium phosphate, ammonium phosphate, sodium hydrogen phosphate, potassium hydrogen phosphate, ammonium hydrogen phosphate, sodium dihydrogen phosphate, potassium dihydrogen phosphate, and calcium dihydrogen phosphate; and phosphoric acid esters such as monomethyl phosphoric acid, dimethyl phosphoric acid, trimethyl phosphoric acid, triethyl phosphoric acid, and triphenyl phosphoric acid. Examples of the phosphonic acids include aminomethylphosphonic acid and phenylphosphonic acid. Phosphoric acids are preferred because they are inexpensive, and among them, inorganic phosphoric acids are preferred from the viewpoint of reaction activity, and phosphoric acid is particularly preferred.
[0068] The onium salts, which are the phase transfer catalysts, are salts of onium ions and anions, and examples of the onium ions include tetraalkylammonium ions, trialkylphenylammonium ions, trialkylbenzylammonium ions, pyridinium ions, and phosphonium ions. In addition, onium salts disclosed in WO2013147092 and JP2015-166335 can also be used. Among them, it is preferable to use an onium ion having 20 or more carbon atoms from the viewpoint of reaction efficiency. Furthermore, the onium salts disclosed in WO2013147092 and JP2015-166335 can be converted into water-soluble substances by simple post-treatment such as hydrolysis after the reaction is completed, and are preferable in that the catalyst composition can be removed more efficiently.
[0069] The anion species is not particularly limited. For example, monovalent anions such as hydrogen sulfate ion, monomethyl sulfate ion, halide ion, nitrate ion, acetate ion, hydrogen carbonate ion, dihydrogen phosphate ion, sulfonate ion, carboxylate ion, hydroxide ion, etc., and divalent anions such as hydrogen phosphate ion and sulfate ion can be mentioned. In terms of availability or ease of preparation, monovalent anions are preferred. In terms of suppressing side reactions, monomethyl sulfate ion, hydrogen sulfate ion, acetate ion, dihydrogen phosphate ion, or hydroxide ion are preferred. The onium ions and anion species may be used alone or in appropriate combination of two or more.
[0070] Examples of the tungsten compound and molybdenum compound include tungstic acid, tungstates such as sodium tungstate, potassium tungstate, calcium tungstate, and ammonium tungstate, hydrates of the tungstates, phosphotungstic acids such as 12-tungstophosphoric acid and 18-tungstophosphoric acid, silicotungstic acids such as 12-tungstosilicic acid, borotungstic acids such as 12-tungstoboric acid, metallic tungsten, molybdic acids such as molybdic acid, molybdates such as sodium molybdate, potassium molybdate, and ammonium molybdate, hydrates of the molybdates, or hydrates thereof.From the viewpoint of improving the activity of the catalyst, tungstic acid and tungstates are preferred, and from the viewpoint of availability, tungstic acid, sodium tungstate, calcium tungstate, or hydrates thereof are preferred.
[0071] The hydrogen peroxide may be used in the form of a commonly available 35% by mass aqueous solution, a 45% by mass aqueous solution, or a 60% by mass aqueous solution, with the 35% by mass aqueous solution being preferred due to its ease of availability. The hydrogen peroxide concentration in the reaction solution is not particularly limited, but is usually in the range of 0.1% by mass to 30% by mass, and is preferably kept at 1% by mass or more from the viewpoint of reaction efficiency, and is preferably kept at 20% by mass or less from the viewpoint of safety, and is more preferably kept at 2% by mass or more or 15% by mass or less.
[0072] As the solvent, any suitable solvent can be used as long as it is inactive against the compound of formula (4) or the compound of formula (1), the active catalyst, and hydrogen peroxide used.Specific examples of the solvent include aromatic hydrocarbons such as benzene, toluene, and xylene; aliphatic hydrocarbons such as hexane, heptane, octane, and dodecane; alcohols such as methanol, ethanol, isopropanol, butanol, hexanol, and cyclohexanol; halogen-based solvents such as chloroform, dichloromethane, and dichloroethane; ethers such as tetrahydrofuran and dioxane; ketones such as methyl ethyl ketone, methyl isobutyl ketone, cyclopentanone, and cyclohexanone; nitriles such as acetonitrile and butyronitrile, ester compounds such as ethyl acetate, butyl acetate, and methyl formate; amides such as N,N-dimethylformamide and N,N-dimethylacetamide; ureas such as N,N'-dimethylimidazolidinone; and mixtures of these solvents. From the viewpoint of reaction efficiency and ease of separation of the target substance and the catalyst component, it is preferable to use a solvent that is not miscible with water and forms a two-phase system. Therefore, aromatic hydrocarbons, aliphatic hydrocarbons, halogenated solvents, water-insoluble ketones, and ester compounds are preferred, and aromatic hydrocarbons that are stable to oxidation reactions and have high solubility of the reaction raw material represented by the formula (4) are more preferred.
[0073] (This manufacturing method) In the present production method, the method for making the content of the oligomer component X in the present epoxy resin 9 area % or more and 25 area % or less when measured using an RI detector is not particularly limited. For example, it can be carried out by the following production method examples 1 to 4. However, it is not limited to these.
[0074] (Manufacturing method example 1) As an example of the method for adjusting the content of the oligomer component X in the epoxy resin to 9 area % or more and 25 area % or less when measured using an RI detector, there can be mentioned a method in which in the step A, the compound of formula (2) is subjected to a Claisen rearrangement reaction in the presence of a basic compound to convert it into a compound of the following formula (3): The Claisen rearrangement proceeds simply by heating, and therefore the reaction proceeds without the addition of a basic compound. However, by carrying out the Claisen rearrangement reaction in the presence of a basic compound to produce the compound of formula (3), the production of compounds other than the compound of formula (3) can be suppressed, and ultimately the content ratio of the oligomer component X in the epoxy resin can be set to the predetermined range.
[0075] The basic compound may be any compound that does not have a polymerizable functional group in the molecule and does not volatilize at the reaction temperature. For example, it may be an aliphatic chain amine such as diethylenetriamine or triethylenetetramine; an aliphatic amine having a benzene ring such as benzylamine, m-xylylenediamine, p-xylylenediamine, N-methylbenzylamine, N-ethylbenzylamine, N-isopropylbenzylamine, 1-phenylethylamine, dibenzylamine, or N,N-dimethylbenzylamine; an aniline such as aniline, N-methylaniline, N-ethylaniline, N-isopropylaniline, N,N-dimethylaniline, N,N-diethylaniline, or N,N-dipropylaniline; an alicyclic amine such as piperidine or morpholine; a heterocyclic amine such as pyridine, pyrrole, indole, quinoline, imidazole, or carbazole. Among these, anilines which are inexpensive and easily separated from the product are preferred, and among these, N,N-dimethylaniline, N,N-diethylaniline, and N,N-dipropylaniline are particularly preferred, which have low reactivity with the allyl group contained in the compound of formula (2) or the compound of formula (3) used and are unlikely to cause side reactions.
[0076] The basic compound is preferably added in a ratio of 0.5 mol to 100 mol, more preferably 0.8 mol or more, and even more preferably 1.0 mol or more, relative to 1.0 mol of the compound of formula (2), while from the viewpoint of cost, the amount is preferably 20 mol or less, and even more preferably 5 mol or less.
[0077] (Manufacturing method example 2) As another example of the method for making the content ratio of the oligomer component X in the epoxy resin 9 area % or more and 25 area % or less when measured using an RI detector, the method includes the steps of: after the reaction of converting the compound of formula (2) into the compound of formula (3) and before the reaction of converting the compound of formula (3) into the compound of formula (4), An example of a method is to carry out purification to separate and remove components other than the compound of formula (3) so that the content ratio of the oligomer component X in the epoxy resin falls within a predetermined numerical range.
[0078] (Manufacturing method example 3) As yet another example of the method for controlling the content ratio of the oligomer component X in the epoxy resin to be 9 area % or more and 25 area % or less when measured using an RI detector, there can be mentioned a method for controlling the content ratio of the oligomer component X in the epoxy resin to be within a predetermined numerical range by performing purification for separating and removing components other than the compound of formula (4) after the compound of formula (3) is converted into the compound of formula (4) and before the compound of formula (4) is converted into the compound of formula (1).
[0079] (Manufacturing method example 4) Furthermore, as yet another example of the method for adjusting the content ratio of the oligomer component X in the epoxy resin to 9 area % or more and 25 area % or less when measured using an RI detector, there can be mentioned a method in which the compound of formula (4) is reacted to convert it into the compound of formula (1), and then purification is performed to separate and remove components other than the compound of formula (1), thereby adjusting the content ratio of the oligomer component X in the epoxy resin to be within a predetermined numerical range.
[0080] (Specific purification method) In the above-mentioned Production Method Examples 2 to 4, a known purification method can be appropriately used as a specific purification method for separating and removing each component. For example, crystallization, suspension washing, liquid separation, adsorption, column chromatography, distillation, etc. can be mentioned. These purification methods may be appropriately combined. Since the load on the production process is small, crystallization, suspension washing, liquid separation, and distillation are preferred, but crystallization is particularly preferred due to its high purification efficiency.
[0081] Crystallization is an example of a chemical separation technique, which utilizes the temperature dependency of solubility to crystallize a target component from a solution by cooling or heating, thereby selectively separating the component. The purification method by crystallization may be any of a method of precipitating while distilling off the solvent under reduced pressure, a method of precipitating while cooling by utilizing the difference in solubility without distilling off, a method of dissolving in a good solvent and then adding a poor solvent to precipitate, etc. The precipitated solid is filtered and collected, and dried to obtain the target product.
[0082] The solvent used for crystallization is preferably selected appropriately depending on the solubility of the compound, and a combination of multiple solvents may be used. Among these, examples of the solvent include aliphatic hydrocarbons such as hexane, heptane, and cyclohexane; aromatic hydrocarbons such as benzene, toluene, and xylene; esters such as methyl acetate, ethyl acetate, and isopropyl acetate; nitriles such as acetonitrile; chain or cyclic ethers such as diisopropyl ether, 1,2-dimethoxyethane, tetrahydrofuran, and dioxane; alcohols such as methanol, ethanol, 2-propanol, and n-butanol; ketones such as acetone, methyl ethyl ketone, and methyl isobutyl; glycol ethers such as ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monopropyl ether, propylene glycol monomethyl ether, and propylene glycol monoethyl ether; aprotic polar solvents such as N,N'-dimethylformamide, N-methylpyrrolidone, and dimethyl sulfoxide; and water.
[0083] In the purification method by suspension washing, it is preferable to use a poor solvent. Preferred poor solvents include highly polar solvents such as methanol, ethylene glycol, and water, and conversely, aliphatic hydrocarbons with low polarity such as hexane, heptane, and cyclohexane. After the suspension washing is completed, the solid matter is collected by filtration and dried to obtain the target product.
[0084] Purification by liquid separation may involve combining water with an organic solvent that is insoluble or poorly soluble in water, or combining multiple organic solvents that are not miscible with each other. Examples of combinations of water with an organic solvent that is insoluble or poorly soluble in water include combinations of water with an organic solvent such as ethyl acetate or toluene.
[0085] Examples of adsorbents used in the adsorption method include activated carbon, activated clay, molecular sieves, activated alumina, zeolite, ion exchange resins, etc. The adsorbent may be added to a solution containing the compound and then removed by filtration, or may be packed in a column for use.
[0086] The above-mentioned Production Method Examples 1 to 4 may be carried out alone, or two or more of Production Method Examples 1 to 4 may be combined and carried out. Among them, it is particularly preferable to carry out production using only Production Method Example 1, since this avoids losses due to crystallization and allows the production of an epoxy resin containing the compound of formula (1) in high yield.
[0087] The crystallization in Production Method Example 2 is preferably carried out by dissolving the compound under heating in a good solvent such as toluene or ethyl acetate, and recovering the crystals precipitated during the cooling process by filtration. In the crystallization in Production Method Example 3 and Production Method Example 4, it is preferable to add an alcohol such as methanol, ethanol, 2-propanol, n-butanol, etc., heat the mixture, allow it to stand, separate the lower layer from the alcohol solution by liquid separation and removal, cool the remaining upper layer, and recover the crystals precipitated during the cooling process by filtration.
[0088] <The Epoxy Resin Composition> Next, the epoxy resin composition containing the present epoxy resin and the epoxy cured product (hereinafter referred to as "the present epoxy resin composition") will be described.
[0089] The present epoxy resin composition is a composition containing the present epoxy resin, an epoxy curing agent and other components, and is an epoxy resin composition in an uncured state that is not substantially crosslinked, i.e., not intentionally crosslinked.
[0090] The present epoxy resin composition preferably contains an epoxy curing agent in a ratio of 0.80 equivalents or more and 1.03 equivalents or less based on the functional group equivalent of the present epoxy resin. In general, when a curing agent is mixed with an epoxy resin, the epoxy curing agent is usually mixed in a ratio of 1:1 functional group equivalent to the functional group equivalent of the epoxy resin. In contrast, in the present epoxy resin composition, the epoxy curing agent is contained in a ratio of 1.03 equivalents or less, particularly 1.00 equivalents or less, relative to the functional group equivalent of the present epoxy resin, thereby lowering the electrical conductivity of the extracted water and making the pH neutral. The present epoxy resin contains the compound of formula (1) as the main component, and since the compound of formula (1) has epoxy groups in one molecule at high density, the curing rate is lower than that of general epoxy resins, and unreacted functional groups tend to remain in the cured product. Therefore, by reducing the equivalent of the curing agent, the unreacted functional groups that are the source of ion components are reduced, the electrical conductivity of the extracted water is lowered, and the pH approaches the neutral range. This makes it possible to obtain an excellent corrosion inhibition effect in applications such as semiconductor encapsulation materials. On the other hand, by containing an epoxy curing agent in an amount of 0.80 equivalents or more relative to the functional group equivalent of the present epoxy resin, it is possible to prevent the occurrence of insufficient curing and suppress the deterioration of various physical properties due to such insufficient curing. From this viewpoint, when a curing agent is blended with the present epoxy resin, it is preferable that the curing agent is contained in an amount of 0.80 or more and 1.03 or less equivalents relative to the functional group equivalent of the present epoxy resin, and more preferably, the amount is 0.85 or more or 1.00 or less, more preferably, 0.87 or more or 0.98 or less, and even more preferably, the amount is 0.90 or more or 0.96 or less.
[0091] The epoxy curing agent may be a known curing agent.Specific examples of the curing agent include phenol-based curing agents, ester-based curing agents, benzoxazine-based curing agents, acid anhydride-based curing agents, primary and secondary amine-based curing agents, mercaptan-based curing agents, amide-based curing agents, blocked isocyanate-based curing agents, tertiary amine-based curing agents, imidazole-based curing agents, and Lewis acid amine complexes.It is also possible to use a phenoxy resin as a curing agent.
[0092] (Other Ingredients) The present epoxy resin composition may contain, in addition to the present epoxy resin and the curing agent, other epoxy resins, curing accelerators, fillers, release agents, other additives, solvents, and the like, as necessary.
[0093] The content of the epoxy resin in the epoxy resin composition is usually 0.1% by mass or more, preferably 1% by mass or more, and particularly preferably 10% by mass or more, and usually 95% by mass or less, preferably 90% by mass or less, more preferably 80% by mass or less, and particularly preferably 70% by mass or less.
[0094] Examples of the "other epoxy resins" include various epoxy resins such as bisphenol A type epoxy resins, bisphenol F type epoxy resins, naphthalene type epoxy resins, phenol novolac type epoxy resins, cresol novolac type epoxy resins, phenol aralkyl type epoxy resins, biphenyl type epoxy resins, triphenylmethane type epoxy resins, and dicyclopentadiene type epoxy resins.
[0095] Examples of the "curing accelerator" include imidazole-based curing accelerators, tertiary amine-based curing accelerators, organic phosphine-based curing accelerators, phosphonium salt-based curing accelerators, tetraphenyl boron salt-based curing accelerators, metal-based curing accelerators, organic acid dihydrazides, and boron halide amine complexes.
[0096] Examples of the "filler" include insulating fillers such as alumina, aluminum nitride, boron nitride, silicon nitride, and silica when it is desired to obtain an insulating composition at low cost.
[0097] The "release agent" includes, for example, stearic acid, palmitic acid, zinc stearate, calcium stearate, and the like.
[0098] The present epoxy resin composition may contain a solvent for the purposes of adjusting the viscosity during processing and improving the handleability during curing. Examples of this type of solvent include ketones such as acetone, methyl ethyl ketone (MEK), methyl isobutyl ketone, cyclohexanone, etc.; esters such as ethyl acetate, etc.; ethers such as ethylene glycol monomethyl ether, etc.; amides such as N,N-dimethylformamide, N,N-dimethylacetamide, etc.; alcohols such as methanol, ethanol, isopropanol, etc.; alkanes such as hexane, cyclohexane, etc.; and aromatics such as toluene, xylene, etc.
[0099] The present epoxy resin composition may further contain, as appropriate, a coupling agent, an ultraviolet protection agent, an antioxidant, a light stabilizer, a plasticizer, a flux, a flame retardant, a colorant, a dispersant, an emulsifier, an elasticity reducing agent, a diluent, an antifoaming agent, an on-trap agent, and the like.
[0100] <Main cured product> The present epoxy resin composition can be cured to obtain a cured product (referred to as a "cured product").
[0101] The curing method and conditions are not particularly limited, but heat curing is preferred because it allows easy molding.
[0102] (glass transition temperature) The glass transition temperature (Tg) of the cured product is usually 150°C or higher, and when used as an encapsulating material for semiconductors that operate under high temperature conditions such as power devices, it is more preferably 180°C or higher, and particularly preferably 200°C or higher.
[0103] (Storage modulus (E')) The storage modulus (E') of the cured product at 250° C. is usually from 10 MPa to 10 GPa, although this varies depending on the type of curing agent used. When the present cured product is used as, for example, a semiconductor encapsulant, it is necessary to prevent cracks from occurring in the semiconductor package and peeling at the interface between the element mounting surface of the substrate and the cured product of the epoxy resin composition from the viewpoint of improving reliability, and for this purpose, it is required to reduce the elastic modulus of the cured product. From this viewpoint, the storage elastic modulus of the present cured product at 250°C is preferably 1 GPa or less, more preferably 500 MPa or less, and even more preferably 300 MPa or less. In addition, when mechanical durability under high temperature conditions is required, it is effective that the elastic modulus of the cured product is high, so the storage elastic modulus of the present cured product at 250°C is preferably 50 MPa or more, more preferably 70 MPa or more, and even more preferably 100 MPa or more. In order to adjust the storage modulus (E') at 250°C and the shear adhesive strength to copper of the cured product to fall within the above ranges, the present epoxy resin composition may be cured using the present epoxy resin containing a predetermined ratio of oligomer component X. Preferable curing conditions for curing include, for example, using a phenolic curing agent, setting the curing temperature to 100 to 200°C, and setting the curing time to 1 to 20 hours.
[0104] <Application> The epoxy resin composition and the cured product can be used as materials in various fields such as adhesives, paints, civil engineering and construction materials, and insulating materials in the electrical and electronic fields. They are particularly useful as insulating casting, lamination materials, and sealing materials in the electrical and electronic fields. Examples of applications include multilayer printed wiring boards, build-up wiring boards, solder resists, adhesives, semiconductor sealing materials, underfill materials, interchip fills for 3D-LSI, insulating sheets, prepregs, and heat dissipation substrates.
[0105] <Other embodiment examples> The same as described above for this epoxy resin can be said for an epoxy resin in which the compound of formula (1) above is replaced with a compound represented by formula (5) below (referred to as "compound of formula (5)"). In addition, the epoxy resin can be similarly produced by replacing the compound of formula (2) with a compound represented by the following formula (6) (hereinafter referred to as "compound of formula (6)"), replacing the compound of formula (3) with a compound represented by formula (7) (hereinafter referred to as "compound of formula (7)"), and replacing the compound of formula (4) with a compound represented by formula (8) (hereinafter referred to as "compound of formula (8)") in the above-mentioned production method.
[0106] [Formula (5)] TIFF0007556347000016.tif73122
[0107] In formula (5), X is a divalent linking group selected from -SO2-, -O-, -CO-, -C(CF3)2-, -S-, or a hydrocarbon group having 1 to 20 carbon atoms.
[0108] [Formula (6)] TIFF0007556347000017.tif77127
[0109] In formula (6), X is a divalent linking group selected from -SO2-, -O-, -CO-, -C(CF3)2-, -S-, or a hydrocarbon group having 1 to 20 carbon atoms.
[0110] [Formula (7)] TIFF0007556347000018.tif77127
[0111] In formula (7), X is a divalent linking group selected from -SO2-, -O-, -CO-, -C(CF3)2-, -S-, or a hydrocarbon group having 1 to 20 carbon atoms.
[0112] [Formula (8)] TIFF0007556347000019.tif77127
[0113] In formula (8), X is a divalent linking group selected from -SO2-, -O-, -CO-, -C(CF3)2-, -S-, or a hydrocarbon group having 1 to 20 carbon atoms.
[0114] In the formulas (5) to (8), examples of the divalent linker selected from hydrocarbon groups having 1 to 20 carbon atoms include a methylene group, an ethylidene group, a propylidene group, an isopropylidene group, a butylidene group, a phenylmethylene group, a phenylethylidene group, a diphenylmethylene group, a cyclohexylidene group, and a 3,3,5-trimethylcyclohexylidene group.
[0115] <Explanation of terms> In this specification, when expressed as "Y to Z" (Y and Z are any numbers), unless otherwise specified, it includes the meaning of "Y or more and Z or less", as well as "preferably larger than Y" or "preferably smaller than Z". In addition, when it is expressed as "Y or more" (Y is any number) or "Z or less" (Z is any number), it also includes the intention that "greater than Y is preferable" or "less than Z is preferable." EXAMPLES
[0116] The present invention will be described in more detail below with reference to examples and comparative examples. However, the present invention is not limited to the following examples as long as the gist of the present invention is not exceeded. The values of various manufacturing conditions and evaluation results in the following examples are meant as preferred upper or lower limit values in the embodiments of the present invention, and a preferred range may be a range defined by a combination of the above-mentioned upper or lower limit value and the values of the following examples or values between the examples. Unless otherwise specified, commercially available reagents were used as materials in the examples. The analytical methods used in the examples and comparative examples are as follows.
[0117] (GPC analysis) Analytical equipment: Tosoh HLC-8120GPC Analysis software: Tosoh GPC-8020 Model II The columns were connected in the following order: TSKgel SuperHM-L (Tosoh, 6.0 × 150 mm, 3 μm) → TSKgel SuperH1000 (Tosoh, 6.0 × 150 mm, 3 μm) → TSKgel SuperH1000 (Tosoh, 6.0 × 150 mm, 3 μm).
[0118] Column temperature: 40℃ Eluent: tetrahydrofuran Flow rate: 0.4mL / min Detector: RI (differential refractive index) detector, set at 40°C Sample volume: 30 μL of 0.3 w / w% eluent solution Calibration material: Monodisperse polystyrene Calibration method: Polystyrene conversion (cubic equation)
[0119] (HPLC analysis) Analytical equipment: Agilent Technologies HPLC 1100 Column temperature: 35℃ Column: GL Science ODS-3V 3μm 4.5×100 mm Detector: UV254nm Eluent: A: 0.1% by volume trifluoroacetic acid aqueous solution B: Acetonitrile Composition: 60% B was maintained from 0 to 6 minutes, a gradient was applied from 60% to 90% B between 6 and 11 minutes, and 90% B was maintained from 11 to 18 minutes. Flow rate: 1.0ml / min
[0120] (epoxy equivalent) Measurements were performed in accordance with JIS K7236:2001.
[0121] (Melting point measurement) Analytical equipment: SII Nano Technology DSC7020 Measurement temperature range: 20℃ to 250℃ Heating rate: 10℃ / min
[0122] (Storage modulus E'(250℃)) The cured material was cut into a test piece 5 cm long, 1 cm wide, and 4 mm thick, and dynamic mechanical analysis (DMA) was performed under the following conditions to measure the storage modulus (E') at 250°C. Analytical equipment: Seiko Instruments EXSTAR6100 Measurement mode: 3-point bending mode Measurement temperature range: 30℃ to 280℃ Temperature increase rate: 5℃ / min, temperature decrease rate: 5℃ / min
[0123] (Shear adhesive strength to copper) The test was carried out in accordance with JIS-K6850. Specifically, the composition prepared in the Examples and Comparative Examples was applied between two sheets of SPCC (cold-rolled steel plate) measuring 25 mm in width, 100 mm in length, and 1.6 mm in thickness, so that the composition had a width of 25 mm and a length of 12.5 mm. After application, the composition was placed in a thermostatic chamber and cured at 120°C for 2 hours and at 175°C for 6 hours to prepare a peel test piece. The prepared peel test pieces were subjected to a tensile shear test at a speed of 5 mm / min (n=3) using a tensile tester "Instron5582" (manufactured by Instron Corporation) to measure the tensile shear strength.
[0124] <Example 1> A 10L autoclave was charged with 840mL of N,N-dimethylformamide, 575g (7.51mol) of allyl chloride, 1245g (9.01mol) of potassium carbonate, and 280g (1.50mol) of biphenol, sealed, heated to 40°C, and then heated to 65°C over 1 hour. After aging at 65°C for 5 hours, the autoclave was cooled to room temperature and opened. 1678g of water and 1600g of methyl isobutyl ketone were added to dissolve inorganic salts and crystals, and the water layer was removed by a separation operation. 1678g of water was added to the remaining methyl isobutyl ketone layer, and the operation of washing with water at 60°C was repeated three times, after which methyl isobutyl ketone was distilled off to obtain the compound of formula (2).
[0125] (Process A) The resulting compound of formula (2) was then heated at 180° C. for 3 hours to obtain 317 g (1.19 mol, two-stage yield 79.3%) of a compound of formula (3).
[0126] (Process B) Next, 105g (394mmol) of the compound of formula (3) synthesized as described above, 1028g (11.1mol) of epichlorohydrin, 400g of isopropanol and 143g of water were charged into a 3L four-neck flask, and after heating to 40°C and dissolving uniformly, 76g (912mmol) of a 48% by mass aqueous sodium hydroxide solution was added dropwise over 90 minutes while heating to 65°C. After the dropwise addition was completed, the mixture was aged at 65°C for 30 minutes, and then 66g of water was added to wash the mixture and remove inorganic salts. Then, epichlorohydrin and isopropanol were distilled off under reduced pressure to obtain a brown oily substance. 191g of methyl isobutyl ketone was added to this mixture to make it uniform, and then 5.8g (69.6mmol) of a 48% by mass aqueous sodium hydroxide solution was added and reacted at 75°C for 2 hours. 223 g of methyl isobutyl ketone was added to the resulting reaction liquid, and the mixture was washed four times with 525 g of water at 70° C. Then, methyl isobutyl ketone was distilled off to obtain 142 g of the compound of formula (4) as a yellow oil.
[0127] (Crystallization purification of compound of formula (4)) 56.1 g of the obtained compound of formula (4) was placed in a 1 L eggplant flask, 224 mL of methanol and 101 mL of 2-methoxyethanol were added, and the mixture was heated to 50°C. The solution was gradually cooled and stirred at 4°C for 1 hour, at which point the precipitated white crystals were collected by filtration. The white crystals were washed with methanol and then dried under reduced pressure at 50°C to obtain 29.8 g (yield 57%) of a purified product of the compound of formula (4).
[0128] (Process C) Next, a mixed solution was prepared containing 40.0 g (106 mmol) of the purified product of the compound of formula (4) synthesized in the same manner as above, 1.74 g (5.30 mmol) of sodium tungstate dihydrate, 3.63 mL (7.42 mmol) of 20% (mass / volume) phosphoric acid aqueous solution, 1.69 g (2.65 mmol) of N-butyl-N,N-di[2-(4-t-butylbenzoyloxy)ethyl]-N-methylammonium monomethyl sulfate, 80 mL of toluene, and 1.10 mL of water. This mixed solution was heated to 60° C. under a nitrogen stream, and then 26.8 mL (318 mmol) of 35% by mass hydrogen peroxide solution was added dropwise over 5 hours, followed by aging for 2 hours. After the reaction was completed, 34 mL of toluene was added, and the separated aqueous layer was extracted. The remaining organic layer was washed with 40 L each of water and 5 mass% aqueous sodium thiosulfate solution, and then 40 mL of methanol and 7.30 g (530 mmol) of potassium carbonate were added to the organic layer and stirred at 40° C. for 1 hour. 40 mL of water was added to dissolve the inorganic salts, and the aqueous phase was discharged. The organic layer was washed once with 40 mL of 1 mol / L aqueous sodium hydroxide solution and three times with 200 mL of warm water at 55° C. The obtained organic layer was concentrated to obtain a compound of formula (1) containing 10 mass% toluene.
[0129] (Crystallization purification of formula (1)) Next, 24 mL of methyl isobutyl ketone and 12 mL of methanol were added to the compound of formula (1) containing 10% by mass of toluene obtained as described above, and the mixture was heated at 50°C to form a homogeneous solution, which was then gradually cooled, at which point precipitation began at 17°C. 24 mL of methanol was added thereto, and the mixture was cooled on ice, and the precipitated light yellow crystals were collected by filtration. The crystals were washed with 20 mL of methanol and dried under reduced pressure at 50°C, yielding 41.6 g (78% yield) of an epoxy resin containing the compound of formula (1) as light yellow crystals. The epoxy equivalent of the refined product of this epoxy resin of the compound of formula (1) was 105, and the melting point was 79°C.
[0130] The compounds of formula (1), (2), (3) and (4) were identified by NMR (the same applies to the examples and comparative examples described later).
[0131] <Example 2> (Basic compound addition method in step A) 165g (620mmol) of the compound of formula (2) obtained in the same manner as in Example 1 and 825mL of N,N-diethylaniline were placed in a 2L four-neck flask, heated at 200°C for 6 hours, and then cooled to room temperature. Next, 495ml of water and 149mL (1.86mol) of a 50% by mass aqueous sodium hydroxide solution were placed in a 2L separable flask and cooled to 10°C, and the N,N-diethylaniline solution was added dropwise over 15 minutes, stirred for 30 minutes, and allowed to stand, and the upper and lower layers were extracted. Next, 495mL of water and 93.1g (1.86mol) of concentrated sulfuric acid were placed in a 2L separable flask and cooled to 10°C, and the lower layer extracted in the previous operation was added dropwise and stirred for 1 hour. The precipitated solid was collected by filtration, washed with water, and then dried under reduced pressure, and 148g (1.19mol, two-stage yield 80.4%) of the compound of formula (3) was obtained as a gray solid.
[0132] (Step B, Step C, Crystallization purification of compound of formula (1)) The procedure was the same as in Example 1, except that the crystallization purification of the compound of formula (4) was not carried out, and a pale yellow powder was obtained as an epoxy resin containing the compound of formula (1). The epoxy equivalent of this epoxy resin was 107 and the melting point was 69°C.
[0133] <Example 3> (Basic compound addition method in step A, step B, step C) The yellow oily product (compound of formula (4)) containing 9% by mass of toluene obtained in the same manner as in Example 2 was further concentrated to completely remove the toluene, to obtain a yellow solid product as an epoxy resin containing the compound of formula (1). The epoxy equivalent of this epoxy resin was 113 and the melting point was 65°C.
[0134] <Comparative Example 1> (Basic compound addition method in step A, step B) The compound of formula (2) was converted to the compound of formula (3) in the same manner as in Example 2, and the compound of formula (3) was converted to the compound of formula (4) in the same manner as in Example 1, to give the compound of formula (4) as a pale yellow solid.
[0135] (Column purification of compound of formula (4), step C) When this compound of formula (4) was purified by a silica gel column, a purified product of the compound of formula (4) was obtained as white crystals with an HPLC purity of 99.7% by area. When the purified product of the compound of formula (4) was used in step C in the same manner as in Example 1, a pale yellow powder was obtained as an epoxy resin containing the compound of formula (1). The epoxy equivalent of this epoxy resin was 109 and the melting point was 79°C.
[0136] <Comparative Example 2> (Process A, Process B) The compound of formula (4) was synthesized according to the method of Japanese Patent No. 2539648.
[0137] (Process C) 50.0 g (132 mmol) of the compound of formula (4) was dissolved in 250 mL of chloroform and heated to 50°C. 97.6 g (396 mmol) of m-chloroperbenzoic acid (containing 30% by mass of water) was added thereto over 1.5 hours, and the mixture was stirred at 50°C for another 30 minutes. After cooling to room temperature, 100 mL of a 5% by mass aqueous solution of sodium thiosulfate was added and stirred for 1 hour, after which the aqueous layer was removed, and the remaining organic layer was washed with 400 mL of a 1 mol / L aqueous solution of sodium hydroxide. The mixture was further washed three times with 250 mL of 75°C warm water, and then concentrated. As a result, 38.2 g of an epoxy resin containing the compound of formula (1) was obtained as a brown oil. The epoxy equivalent of this epoxy resin was 121.
[0138] The epoxy resins containing the compound of formula (1) obtained in Examples 1 to 3 and Comparative Examples 1 and 2 were analyzed by GPC under the above-mentioned conditions, and it was found that the components having a standard polystyrene-equivalent molecular weight of 60.8 or more were contained in the amounts shown in area % in Table 1 below.
[0139] [Table 1]
[0140] <Examples 4 to 6, Comparative Examples 3 to 4> (Epoxy resin hardening) The epoxy resins produced in Examples 1 to 3 and Comparative Examples 1 and 2 were mixed with the curing agent PSM4261 (Gun-ei Chemical Industry Co., Ltd.) in the compounding ratios shown in Table 2 at 100° C. until uniform. Next, triphenyl phosphate (Hokuko Chemical Industry Co., Ltd.) was added as a curing accelerator and stirred until uniform, obtaining liquid epoxy resin compositions. A casting plate adjusted to a thickness of 2 mm was prepared using two glass plates with release PET film on the inside, and the epoxy resin composition (liquid) was poured into the casting plate and heated at 120°C for 2 hours and then at 175°C for 6 hours to obtain a cured product.
[0141] [Table 2]
[0142] It was found that the cured products of Examples 4 to 6 had a higher storage modulus (E') at 250°C than those of Comparative Examples 3 and 4. In addition, it was found that the cured products of Examples 4 and 5 had a higher shear adhesive strength to copper than those of Comparative Examples 3 and 4. Since an epoxy resin containing an epoxy compound represented by formula (1) can originally achieve both moldability and heat resistance of the cured product, it can be suitably used as a material for devices used in high temperature environments. However, since it has a high high temperature modulus and a high shear adhesive strength to copper, it can be suitably used as a matrix resin for composite materials that require particularly high mechanical strength, and for semiconductor encapsulation materials that require adhesion to copper wires.
[0143] <Comparative Example 5, Examples 7 to 8> (Extracted water test) To an epoxy resin (epoxy equivalent: 105) containing an epoxy compound represented by formula (1) produced in the same manner as in Example 2, a curing agent PSM4261 (manufactured by Gun-ei Chemical Industry Co., Ltd., hydroxyl equivalent: 103) and a curing accelerator triphenyl phosphate (manufactured by Hokko Chemical Industry Co., Ltd.) were added in the compounding ratios shown in Table 3 to obtain an epoxy resin composition, and a cured product was produced in the same manner as in Examples 4 to 6. The hardened material was pulverized using a Wonder Blender (Osaka Chemical Co., Ltd.), and 8 g of the resulting 20 mesh pass powder was weighed into a polyethylene bottle. 80 mL of ultrapure water was added to the bottle, which was then capped and placed in a dryer at 95°C for 20 hours. The bottle was then cooled to room temperature, and the supernatant was filtered through No. 5A filter paper to obtain the extract. The pH and electrical conductivity of the resulting extract were as shown in the table below.
[0144] [Table 3]
[0145] The cured products of Examples 7 and 8 have higher pH values in the extraction water and lower electrical conductivity than those of Comparative Example 5, suggesting that the cured products contain fewer ionic components. As a result, the cured products made of the epoxy resin composition of the present invention are expected to have a corrosion inhibitory effect on metals that they come into contact with, and can be suitably used in applications such as semiconductor encapsulation materials.
[0146] In the above examples, the composition is purified by crystallization so that the content ratio of components having a standard polystyrene-equivalent molecular weight of 60.8 or more falls within a predetermined range, or the composition is prepared by carrying out a Claisen rearrangement reaction in the presence of a basic compound so that the content ratio of components having a standard polystyrene-equivalent molecular weight of 60.8 or more falls within a predetermined range. However, from the above examples and the results of tests conducted by the present inventors, it has been confirmed that the desired effect can be obtained if the content ratio of components having a standard polystyrene-equivalent molecular weight of 60.8 or more falls within a predetermined range. Therefore, it is considered that the same effect can be obtained even if the content ratio of components having a standard polystyrene-equivalent molecular weight of 60.8 or more falls within a predetermined range by adopting another method.
[0147] The compound represented by formula (1) has a structure in which two phenyl groups are covalently bonded by a single bond (direct bond). Even if these two phenyl groups are bonded via various bonds, such as -SO2-, -O-, -CO-, -C(CF3)2-, -S-, or a divalent linking group selected from a hydrocarbon group having 1 to 20 carbon atoms, it is considered that the properties of the epoxy resin are not significantly affected. In addition, it can be produced in the same way as in the case of a single bond (direct bond). Therefore, the compound represented by formula (5) can also be produced in the same way as the compound represented by formula (1), and is expected to have the same action and effect.
Claims
1. The epoxy resin contains 3,3'-diglycidylbiphenyl-4,4'-diglycidyl ether (also referred to as "compound of formula (1)") represented by the following formula (1):
1. An epoxy resin comprising: a component having a standard polystyrene-equivalent molecular weight of 60.8 or more in an amount of 9 area % to 25 area % when measured by gel permeation chromatography (hereinafter referred to as "GPC") using an RI detector; and the component having a standard polystyrene-equivalent molecular weight of 60.8 or more is a compound having two or more biphenyl skeletons. [Formula (1)]
2. An epoxy resin containing a compound represented by the following formula (5): An epoxy resin characterized in that it contains 9 area % or more and 25 area % or less of components having a standard polystyrene equivalent molecular weight of 60.8 or more when measured by gel permeation chromatography (also referred to as "GPC") using an RI detector. [Formula (5)] (X in formula (5) is -SO 2 -, -O-, -CO-, -C(CF 3 ) 2 -, -S-, or a divalent linking group selected from a hydrocarbon group having 1 to 20 carbon atoms)
3. A method for producing an epoxy resin, comprising the steps of converting a compound represented by the following formula (2) (also referred to as a "formula (2) compound") into a compound represented by the following formula (3) (also referred to as a "formula (3) compound"), then converting the formula (3) compound into a compound represented by the following formula (4) (also referred to as a "formula (4) compound"), and then converting the formula (4) compound into a formula (1) compound represented by the following formula (1), to obtain an epoxy resin, 1. A method for producing an epoxy resin, comprising the steps of: adjusting a content ratio of a component having a standard polystyrene-equivalent molecular weight of 60.8 or more in the epoxy resin to be 9 area % or more and 25 area % or less when measured using an RI detector in GPC; and the component having a standard polystyrene-equivalent molecular weight of 60.8 or more is a compound having two or more biphenyl skeletons. [Formula (1)] [Formula (2)] [Formula (3)] [Formula (4)]
4. The method for producing an epoxy resin according to claim 3, characterized in that the compound of formula (2) is converted into the compound of formula (3) by a Claisen rearrangement reaction in the presence of a basic compound.
5. The method for producing an epoxy resin according to claim 4, wherein the basic compound is added in a ratio of 1.0 mole or more and 100 moles or less to 1.0 mole of the compound of formula (2) to react with the compound.
6. The method for producing an epoxy resin according to claim 4 or 5, wherein the basic compound is an aniline compound.
7. After the reaction of converting the compound of formula (2) into the compound of formula (3) and before the reaction of converting the compound of formula (3) into the compound of formula (4), The method for producing an epoxy resin according to claim 3, characterized in that a purification step is carried out to separate and remove components other than the compound of formula (3).
8. After the reaction of converting the compound of formula (3) into the compound of formula (4) and before the reaction of converting the compound of formula (4) into the compound of formula (1), The method for producing an epoxy resin according to claim 3 or 7, characterized in that a purification step is carried out to separate and remove components other than the compound of formula (4).
9. After converting the compound of formula (4) into the compound of formula (1), The method for producing an epoxy resin according to claim 3, 7 or 8, characterized in that a purification step is carried out to separate and remove components other than the compound of formula (1).
10. A method for producing an epoxy resin, comprising the steps of converting a compound represented by the following formula (6) (also referred to as a "formula (6) compound") into a compound represented by the following formula (7) (also referred to as a "formula (7) compound"), then converting the formula (7) compound into a compound represented by the following formula (8) (also referred to as a "formula (8) compound"), and then converting the formula (8) compound into a formula (5) compound represented by the following formula (5), to obtain an epoxy resin, 1. A method for producing an epoxy resin, comprising: adjusting a content ratio of a component having a standard polystyrene-equivalent molecular weight of 60.8 or more in the epoxy resin to be 9 area % or more and 25 area % or less when measured by GPC using an RI detector. [Formula (5)] (X in formula (5) is -SO 2 -, -O-, -CO-, -C(CF 3 ) 2 -, -S-, or or a divalent linking group selected from hydrocarbon groups having 1 to 20 carbon atoms). [Formula (6)] (X in formula (6) is -SO 2 -, -O-, -CO-, -C(CF 3 ) 2 -, -S-, or or a divalent linking group selected from hydrocarbon groups having 1 to 20 carbon atoms). [Formula (7)] (X in formula (7) is -SO 2 -, -O-, -CO-, -C(CF 3 ) 2 -, -S-, or or a divalent linking group selected from hydrocarbon groups having 1 to 20 carbon atoms). [Formula (8)] (X in formula (8) is -SO 2 -, -O-, -CO-, -C(CF 3 ) 2 -, -S-, or or a divalent linking group selected from hydrocarbon groups having 1 to 20 carbon atoms).
11. The method for producing an epoxy resin according to claim 10, characterized in that the compound of formula (6) is converted into the compound of formula (7) by a Claisen rearrangement reaction in the presence of a basic compound.
12. The method for producing an epoxy resin according to claim 11, wherein the basic compound is added in a ratio of 1.0 mole or more and 100 moles or less to 1.0 mole of the compound of formula (6) to react with the compound.
13. The method for producing an epoxy resin according to claim 11 or 12, wherein the basic compound is an aniline compound.
14. After the reaction of converting the compound of formula (6) into the compound of formula (7), Before converting the compound of formula (7) into the compound of formula (8), The method for producing an epoxy resin according to claim 10, characterized in that a purification step is carried out to separate and remove components other than the compound of formula (7).
15. After the reaction of converting the compound of formula (7) into the compound of formula (8), Before converting the compound of formula (8) into the compound of formula (5), The method for producing an epoxy resin according to claim 10 or 14, characterized in that a purification step is carried out to separate and remove components other than the compound of formula (8).
16. After converting the compound of formula (8) into the compound of formula (5), The method for producing an epoxy resin according to claim 10, 14 or 15, characterized in that a purification step is carried out to separate and remove components other than the compound of formula (5).
17. The method for producing an epoxy resin according to claim 7, 8, 9, 14, 15 or 16, wherein the purification is carried out by crystallization.
18. 3. An epoxy resin composition comprising the epoxy resin according to claim 1 or 2, and an epoxy curing agent in an amount of 0.80 equivalents or more and 1.03 equivalents or less based on the functional group equivalent of the epoxy resin.
19. A cured product obtained by curing the epoxy resin composition according to claim 18.
Citation Information
Patent Citations
Polyfunctional epoxide resin
JP1988142019A
Curable resin composition
JP2015127397A
Method for producing epoxy compound and catalyst composition for epoxidation reaction
JP2015166335A
Method for producing polyvalent glycidyl compound
JP2016094353A
Polyfunctional epoxy resin and intermediate, epoxy resin composition, and cured product