FLUOROSULFONYL GROUP-CONTAINING FLUOROPOLYMER AND METHOD FOR PRODUCING SAME, SULFONIC ACID GROUP-CONTAINING FLUOROPOLYMER AND METHOD FOR PRODUCING SAME, SOLID POLYMER ELECTROLYTE MEMBRANE, MEMBRANE ELECTRODE ASSEMBLY, AND SOLID POLYMER FUEL CELL
Patent Information
- Application Number
- JP2021553492
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-10-21
- Filing Date
- 2020-10-21
- Publication Date
- 2024-09-26
- Estimated Expiration
- 2040-10-21
AI Technical Summary
【0008】 本発明によれば、導電性および熱水耐性に優れた固体高分子電解質膜を製造できるフルオロスルホニル基含有含フッ素ポリマーおよびその製造方法、酸型スルホン酸基含有含フッ素ポリマーおよびその製造方法、固体高分子電解質膜、膜電極接合体ならびに固体高分子形燃料電池を提供できる。
Smart Images

Figure 0007556359000028 
Figure 0007556359000017 
Figure 0007556359000025
Abstract
Description
[Technical field]
[0001] The present invention relates to a fluoropolymer containing a fluorosulfonyl group and a method for producing the same, an acid-type sulfonic acid group-containing fluoropolymer and a method for producing the same, a solid polymer electrolyte membrane, a membrane electrode assembly and a solid polymer fuel cell. [Background technology]
[0002] A polymer electrolyte fuel cell has a structure in which, for example, a membrane electrode assembly is sandwiched between two separators to form a cell, and a plurality of cells are stacked. The membrane electrode assembly includes an anode and a cathode having a catalyst layer, and a solid polymer electrolyte membrane disposed between the anode and the cathode. The solid polymer electrolyte membrane is obtained by forming a membrane from a fluorine-containing polymer containing an acid type sulfonic acid group. As a method for producing such a polymer having an acid type sulfonic acid group, Patent Document 1 discloses a method for producing a polymer having an acid type sulfonic acid group by using tetrafluoroethylene and CF 2 =CFCF 2 OCF 2 CF 2 SO 2 The monomer represented by F is copolymerized in the presence of a radical polymerization initiator at a temperature of 100 to 200°C, and then -SO 2 A method is disclosed in which the F group is hydrolyzed, converted into an acid form, and converted into a sulfonic acid group. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2010-18674 A Summary of the Invention [Problem to be solved by the invention]
[0004] In recent years, in order to improve the power generation efficiency of solid polymer electrolyte fuel cells, there has been a demand for highly conductive solid polymer electrolyte membranes. In addition, since the solid polymer electrolyte membrane is exposed to high temperature and high humidity conditions during power generation in solid polymer electrolyte fuel cells, the acid-type sulfonic acid group-containing fluoropolymer constituting the solid polymer electrolyte membrane is required to have hot water resistance. When the present inventors evaluated a solid polymer electrolyte membrane obtained using a fluoropolymer containing acid-type sulfonic acid groups obtained by the production method described in Patent Document 1, the electrical conductivity and hot water resistance were insufficient, and there was room for improvement. Specifically, when a solid polymer electrolyte membrane with a high ion exchange capacity is produced in order to obtain a high electrical conductivity of 0.08 S / cm or more, the hot water resistance is significantly reduced, and therefore, the production method described in Patent Document 1 could not obtain a solid polymer electrolyte membrane that combines high electrical conductivity of 0.08 S / cm or more and hot water resistance.
[0005] In view of the above circumstances, an object of the present invention is to provide a fluorosulfonyl group-containing fluorine-containing polymer capable of producing a solid polymer electrolyte membrane excellent in electrical conductivity and hot water resistance and a production method thereof, an acid-type sulfonic acid group-containing fluorine-containing polymer and a production method thereof, a solid polymer electrolyte membrane, a membrane electrode assembly, and a solid polymer electrolyte fuel cell. [Means for solving the problem]
[0006] As a result of intensive investigations into the above-mentioned problems, the present inventors have found that, when a fluorosulfonyl group-containing fluoropolymer is produced by copolymerizing a monomer represented by the formula m1 described below with tetrafluoroethylene in the presence of a radical polymerization initiator (hereinafter also referred to as "initiator"), by setting the copolymerization temperature within a predetermined range and setting the molar ratio of the total amount of monomer represented by formula m1 added to the total amount of tetrafluoroethylene added within a predetermined range so that the concentration of the initiator in the reactor during copolymerization is maintained at 2.5 ppm by mass or less of the mass of the monomer represented by formula m1 charged in the reactor before the start of polymerization, a fluorosulfonyl group-containing fluoropolymer from which a solid polymer electrolyte membrane excellent in electrical conductivity and hot water resistance can be produced can be obtained, thereby completing the present invention.
[0007] That is, the present inventors have found that the above problems can be solved by the following configuration. [1] A method for producing a fluoropolymer containing a fluorosulfonyl group by copolymerizing a monomer represented by the formula m1 described below with tetrafluoroethylene at a temperature of 150 to 200°C in a reactor in the presence of a radical polymerization initiator, characterized in that during the copolymerization, the radical polymerization initiator is added continuously or stepwise to the reactor so that the concentration of the radical polymerization initiator in the reactor is maintained at 2.5 ppm by mass or less of the mass of the monomer represented by the formula m1 charged in the reactor before the start of the copolymerization, and the molar ratio of the total amount of the monomer represented by the formula m1 added to the total amount of the tetrafluoroethylene added is 1.5 to 20. In the formula m1 described below, Q 1 is a single bond or a perfluoroalkylene group which may have an ether-bonded oxygen atom. [2] A method for producing a fluoropolymer having fluorosulfonyl groups, comprising copolymerizing a monomer represented by the formula m1 described below with tetrafluoroethylene at a temperature of 150 to 200°C in the presence of a radical polymerization initiator in a reactor, a ratio of a total amount of the radical polymerization initiator charged into the reactor to a total amount of the monomer represented by the formula m1 charged into the reactor is 0.01 to 4 ppm by mass on average per hour of copolymerization time, A method for producing a fluoropolymer having fluorosulfonyl groups, characterized in that the molar ratio of the total amount of the monomers represented by the formula m1 to the total amount of the tetrafluoroethylene is from 1.5 to 20. In the formula m1 described below, Q 1 is a single bond or a perfluoroalkylene group which may have an ether-bonded oxygen atom. [3] The method for producing a fluoropolymer having fluorosulfonyl groups according to [1] or [2], wherein the monomer represented by the formula m1 is a monomer represented by the formula m11 described below. In the formula m11 described below, x is an integer of 1 to 12. [4] The method for producing a fluoropolymer having a fluorosulfonyl group according to any one of [1] to [3], wherein the radical polymerization initiator is a bis(perfluoroalkyl)peroxide or a dialkylperoxide. [5] A fluoropolymer having a fluorosulfonyl group and a unit represented by the formula f1 described later and a unit based on tetrafluoroethylene, wherein the Q value of the fluorosulfonyl group-containing fluoropolymer is 0.2 to 60.0 mm 3 / sec, and the proportion of the units represented by the above formula f1 to all units in the fluoropolymer containing fluorosulfonyl groups is 21 to 59 mol %. The above Q value was determined by measuring the cross-sectional area of the fluorosulfonyl group-containing fluorine-containing polymer using a flow tester. 2 The mixture is filled into a cylinder of 1 mm in diameter and extruded from a nozzle of 1 mm in length at 260°C under a load of 30 kg and a pressure of 2.94 MPa. 3 / seconds). In the formula f1 described below, Q 1 is a single bond or a perfluoroalkylene group which may have an ether-bonded oxygen atom. [6] The fluorosulfonyl group-containing fluoropolymer according to [5], wherein the ion exchange capacity of the acid-type sulfonic acid group-containing fluoropolymer when the fluorosulfonyl groups in the fluorosulfonyl group-containing fluoropolymer are converted to acid-type sulfonic acid groups is 1.45 to 2.50 milliequivalents / gram of dry resin. [7] The fluoropolymer having fluorosulfonyl groups according to [5] or [6], wherein the unit represented by the formula f1 is a unit represented by the formula f11 described below. In the formula f11 described below, x is an integer of 1 to 12. [8] A method for producing a sulfonic acid group-containing fluoropolymer, comprising converting the fluorosulfonyl groups of a fluorosulfonyl group-containing fluoropolymer produced by the production method according to any one of [1] to [4] into sulfonic acid groups. [9] A sulfonic acid group-containing fluoropolymer having a unit represented by the formula u1 described later and a unit based on tetrafluoroethylene, wherein the Q value of the fluorosulfonyl group-containing fluoropolymer when the sulfonic acid group in the sulfonic acid group-containing fluoropolymer is a fluorosulfonyl group is 0.2 to 60.0 mm 3 / sec, and the ratio of the units represented by the above formula u1 to all units in the sulfonic acid group-containing fluoropolymer is 21 to 59 mol %. The above Q value was determined by measuring the cross-sectional area of the fluorosulfonyl group-containing fluorine-containing polymer using a flow tester. 2 The mixture is filled into a cylinder of 1 mm in diameter and extruded from a nozzle of 1 mm in length at 260°C under a load of 30 kg and a pressure of 2.94 MPa. 3 / seconds). In the formula u1 described below, Q 1 is a single bond or a perfluoroalkylene group which may have an ether-bonded oxygen atom, Z + is H + , a metal ion, or an ammonium ion.
[10] The sulfonic acid group-containing fluoropolymer according to [9], wherein the sulfonic acid groups in the sulfonic acid group-containing fluoropolymer are acid type sulfonic acid groups, and the acid type sulfonic acid group-containing fluoropolymer has an ion exchange capacity of 1.45 to 2.50 milliequivalents / gram of dry resin.
[11] The sulfonic acid group-containing fluorine-containing polymer according to [9] or
[10] , wherein the unit represented by the formula u1 is a unit represented by the formula u11 described below. In the formula u11 described below, x is an integer of 1 to 12, Z + is H + , a metal ion, or an ammonium ion.
[12] A liquid composition comprising the sulfonic acid group-containing fluorine-containing polymer according to any one of [9] to
[11] and a liquid medium.
[13] The liquid composition according to
[12] , wherein the liquid medium comprises a mixture of an alcohol having 1 to 4 carbon atoms and water.
[14] The liquid composition according to
[12] or
[13] , further comprising one or more atoms selected from the group consisting of cerium atoms and manganese atoms.
[15] The sulfonic acid group-containing fluorine-containing polymer according to any one of [9] to
[11] , A solid polymer electrolyte membrane, characterized in that the sulfonic acid groups of the sulfonic acid group-containing fluorine-containing polymer are acid type sulfonic acid groups.
[16] The solid polymer electrolyte membrane according to
[15] , further comprising a reinforcing material.
[17] The solid polymer electrolyte membrane according to
[16] , wherein the reinforcing material is a porous PTFE body.
[18] The solid polymer electrolyte membrane according to any one of
[15] to
[17] , which has a membrane thickness of 5 to 200 μm.
[19] The solid polymer electrolyte membrane according to any one of
[15] to
[18] , further comprising one or more atoms selected from the group consisting of cerium atoms and manganese atoms.
[20] A membrane electrode assembly comprising: an anode having a catalyst layer containing a catalyst and a polymer having an ion exchange group; a cathode having a catalyst layer containing a catalyst and a polymer having an ion exchange group; and a solid polymer electrolyte membrane containing a polymer having an ion exchange group disposed between the anode and the cathode, A membrane / electrode assembly, characterized in that at least one polymer selected from the group consisting of a polymer having an ion exchange group contained in an anode, a polymer having an ion exchange group contained in a cathode, and a polymer having an ion exchange group contained in a solid polymer electrolyte membrane is a fluorine-containing polymer having a sulfonic acid group according to any one of [9] to
[11] .
[21] The membrane electrode assembly according to
[20] , a polymer having an ion exchange group contained in at least one of the catalyst layers of the anode and the cathode is a polymer having a unit containing a cyclic ether structure and having a sulfonic acid type functional group; A membrane / electrode assembly, wherein the polymer having an ion-exchange group contained in the solid polymer electrolyte membrane is the sulfonic acid group-containing fluorine-containing polymer according to any one of [9] to
[11] .
[22] The membrane / electrode assembly according to
[21] , wherein the unit containing a cyclic ether structure includes a unit represented by the formula U12 described below or a unit represented by the formula U22 described below. In the formula u12 below, R 21 is a perfluoroalkylene group having 1 to 6 carbon atoms or a perfluoroalkylene group having 2 to 6 carbon atoms and an ether-bonding oxygen atom between the carbon-carbon bonds, R 22 is a fluorine atom, a perfluoroalkyl group having 1 to 6 carbon atoms, a perfluoroalkyl group having 2 to 6 carbon atoms and an ether-bonded oxygen atom between the carbon-carbon bonds, or -R 21 (SO 2 X(SO 2 R f ) a ) - M + It is a group represented by M + is H + , a monovalent metal cation or an ammonium ion in which one or more hydrogen atoms may be substituted by a hydrocarbon group; R f is a linear or branched perfluoroalkyl group which may have an ether-bonded oxygen atom, X is an oxygen atom, a nitrogen atom or a carbon atom, and when X is an oxygen atom, a=0, when X is a nitrogen atom, a=1, and when X is a carbon atom, a=2. In the formula u22 described below, s is 0 or 1, and R 51 and R 52 are each independently a fluorine atom, a perfluoroalkyl group having 1 to 5 carbon atoms, or a spiro ring formed by linking together (when s is 0), and R 53 and R 54 are each independently a fluorine atom or a perfluoroalkyl group having 1 to 5 carbon atoms, and R 55 is a fluorine atom, a perfluoroalkyl group having 1 to 5 carbon atoms, or a perfluoroalkoxy group having 1 to 5 carbon atoms.
[23] The membrane / electrode assembly according to any one of
[20] to
[22] , wherein the sulfonic acid group of the sulfonic acid group-containing fluorine-containing polymer is an acid type sulfonic acid group.
[24] A polymer electrolyte fuel cell comprising the membrane electrode assembly according to any one of
[20] to
[23] . Effect of the Invention
[0008] According to the present invention, it is possible to provide a fluorosulfonyl group-containing fluoropolymer capable of producing a solid polymer electrolyte membrane excellent in electrical conductivity and hot water resistance and a production method thereof, an acid-type sulfonic acid group-containing fluoropolymer and a production method thereof, a solid polymer electrolyte membrane, a membrane electrode assembly, and a solid polymer fuel cell. [Brief description of the drawings]
[0009] [Figure 1] 1 is a schematic cross-sectional view showing an example of a membrane electrode assembly of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] The following definitions of terms apply throughout the specification and claims, unless otherwise stated. "Salt-type sulfonic acid group" refers to a salt-type sulfonic acid group (-SO 3 - M + However, M + is a metal ion or an ammonium ion. "Acid type sulfonic acid group" refers to an acid type sulfonic acid group (-SO 3 - H + ) The term "sulfonic acid group" is a general term for salt-type sulfonic acid groups and acid-type sulfonic acid groups. In this specification, when the term "sulfonic acid group" is used without specifying whether it is a salt type or an acid type, the general term -SO 3 - Z + (However, Z + is H + , a metal ion, or an ammonium ion. A "unit" in a polymer means an atomic group derived from one molecule of a monomer formed by polymerization of the monomer. The unit may be an atomic group formed directly by a polymerization reaction, or may be an atomic group in which a part of the atomic group is converted into a different structure by processing the polymer obtained by the polymerization reaction. Note that a structural unit derived from an individual monomer may be named by adding "unit" to the name of the monomer. The unit represented by formula u1 is written as unit u1. The units represented by other formulas are written in the same way. The monomer represented by formula m1 is referred to as monomer m1. Units represented by other formulas are also referred to in the same manner. A numerical range expressed using "~" means that the range includes the numerical values before and after "~" as the lower and upper limits. "Total amount of A added" means the total amount of A added to the reactor for use in polymerizing the polymer, and for example, when A is added to the reactor before and during polymerization, it means the total amount of A added to the reactor before polymerization and A added to the reactor during polymerization. "A" is a component used in polymerization, and examples of such components include TFE, monomer m1, or an initiator, which will be described later. "Productivity index (Rp)" refers to the amount of SO charged before and during copolymerization. 2 The amount of polymer (g) produced per 100 g of the total amount of F group-containing monomers and per hour of polymerization time is shown.
[0011] The term "copolymerization time" means the time from the start of copolymerization to the end of copolymerization. Examples of the "time to start copolymerization" include the time when the monomer and the initiator are made to coexist in the reactor under a predetermined pressure after the reactor is heated to a predetermined temperature or higher, and the time when the reactor is heated to a predetermined temperature or higher after the monomer and the initiator are made to coexist in the reactor. The predetermined temperature means a temperature of 80°C or higher and [(10-hour half-life temperature of the initiator)-30]°C or higher. The predetermined pressure means a pressure at which the partial pressure of the monomer, tetrafluoroethylene, is 0.02 MPa or higher. Examples of the "time to terminate the copolymerization" include the time when the temperature inside the reactor is lowered below a predetermined temperature, the time when the monomer tetrafluoroethylene is purged, the time when a polymerization inhibitor is added to the reactor, etc. Purging tetrafluoroethylene means that the partial pressure of tetrafluoroethylene is reduced to 0.01 MPa or less. In addition, when the copolymerization is stopped and then restarted by a reversible operation (for example, by raising the temperature inside the reactor to a predetermined temperature or higher again, or by adding tetrafluoroethylene again), this is included in the polymerization time.
[0012] [Production method of fluoropolymer containing fluorosulfonyl groups according to the first embodiment] The method for producing a fluoropolymer having fluorosulfonyl groups according to the first embodiment of the present invention is a method for producing a fluoropolymer having fluorosulfonyl groups by copolymerizing monomer m1 and tetrafluoroethylene (hereinafter also referred to as "TFE") in the presence of an initiator at a temperature of 150 to 200°C in a reactor. During the copolymerization, the initiator is continuously or sequentially added to the reactor so that the concentration of the initiator in the reactor is maintained at 2.5 mass ppm or less of the mass of the monomer m1 charged in the reactor before the copolymerization is started. The molar ratio of the total amount of the monomer m1 to the total amount of the TFE is 1.5-20. The fluoropolymer having fluorosulfonyl groups obtained by the production method of the first embodiment is also referred to as "polymer Fx" in this specification.
[0013] According to the present production method, it is possible to produce a fluoropolymer having fluorosulfonyl groups, which can be used to produce a solid polymer electrolyte membrane having excellent electrical conductivity and hot water resistance. In the examples of Patent Document 1, the initiator was used at a relatively high concentration. However, the present inventors found that a polymer having high electrical conductivity and good hot water resistance can be obtained by using a low concentration of the initiator. That is, it is considered that by maintaining the concentration of the initiator at a predetermined value or less during the copolymerization of the monomer m1 and TFE, the termination reaction in the copolymerization of TFE and the monomer m1 is less likely to occur. As a result, it is presumed that the molecular weight of the polymer Fx is increased, and therefore the hot water resistance of the solid polymer electrolyte membrane produced from the acid-type sulfonic acid group-containing fluorine-containing polymer (hereinafter also referred to as "polymer HAx") obtained by converting the fluorosulfonyl groups of the polymer Fx to acid forms is improved. Furthermore, normally, when the amount of the initiator used is reduced, the polymerization rate decreases, resulting in a significant drop in productivity. However, surprisingly, according to the method of the present invention, copolymerization can be carried out at a polymerization rate at an industrially feasible level. That is, even when the concentration of the initiator is low as described above, by setting the copolymerization temperature of the monomer m1 and TFE to a high temperature of 150 to 200° C., it is possible to suppress a decrease in the reaction rate during the production of the polymer Fx. In addition, by setting the molar ratio of the total amount of monomer m1 added to the total amount of TFE added to 1.5 to 20, the content of units based on monomer m1 in polymer Fx increases, and the ion exchange capacity of polymer HAx increases. As a result, it is believed that the conductivity of the solid polymer electrolyte membrane produced from polymer HAx is improved. Moreover, it has been surprisingly found that the chemical durability of the polymer is also superior.
[0014] <Monomer m1> The monomer m1 is a monomer represented by the following formula m1. CF 2 =CFCF 2 OQ 1 -SO 2 F (m1) In formula m1, Q 1 is a single bond or a perfluoroalkylene group which may have an ether-bonded oxygen atom. The perfluoroalkylene group may be linear or branched. The number of carbon atoms in the perfluoroalkylene group is preferably 1 to 12, more preferably 1 to 6, and particularly preferably 1 to 4, in that a decrease in the ion exchange capacity of the polymer HAx can be suppressed and a solid polymer electrolyte membrane with superior conductivity can be obtained. When the perfluoroalkylene group has an ether-bonding oxygen atom, the number of oxygen atoms may be 1 or 2 or more, and is preferably 2 or less. In addition, the oxygen atom may be located between the carbon-carbon bonds of the perfluoroalkylene group.
[0015] As the monomer m1, the monomer m11 is preferable, and the monomer m11-1 is particularly preferable, in that the polymer Fx can be easily produced and industrially implemented.
[0016] [ka]
[0017] In formula m11, x is an integer of 1 to 12, preferably an integer of 1 to 6, and particularly preferably an integer of 1 to 4.
[0018] <Other Monomers> In this production method, monomers other than TFE and monomer m1 (hereinafter also referred to as "other monomers") may be used.
[0019] As the other monomer, a perfluoromonomer is preferable from the viewpoint of improving the chemical durability of the polymer, and a perfluoroallyl ether or a perfluorovinyl ether is more preferable because the amount of the monomer introduced into the polymer can be increased, and a perfluoroallyl ether is even more preferable because the physical properties of the polymer can be easily improved. Note that, since perfluorovinyl ether may act as a chain transfer agent by self-chain transfer at 150 to 200°C, it may be used not only for the purpose of improving the physical properties but also for the purpose of adjusting the molecular weight. Specific examples of other monomers are as follows. CF 2 =CFCF 2 O(CF 2 )n1 F, CF 2 =CF(CF 2 ) n2 F, CF 2 =CFCF 2 [OCF 2 CF(CF 3 )] n3 OCF 2 CF 2 CF 3 , CF 2 =CFO(CF 2 ) n4 CF 3 , CF 2 =CFOCF 2 CF(CF 3 )O(CF 2 ) n5 CF 3 , CF 2 =CF[OCF 2 CF(CF 3 )] n6 O(CF 2 ) 3 F,
[0020] TIFF0007556359000002.tif2965
[0021] In the above formula, n1 is an integer of 1 to 4, n2 is an integer of 1 to 11, n3 is 1 or 2, n4 is an integer of 1 to 9, n5 is an integer of 1 to 9, n6 is 2 or 3, and n7 is an integer of 1 to 6.
[0022] <Initiator> Examples of initiators include bis(fluoroacyl)peroxides, bis(perfluoroalkyl)peroxides (e.g., (CF 3 ) 3 COOC(CF 3 ) 3 ), bis(chlorofluoroacyl) peroxides, dialkyl peroxides (e.g., (CH 3 ) 3 COOC(CH 3 )3 ), peroxyesters, azo compounds, and persulfates are preferred, from the viewpoint of enhancing the chemical durability of the solid polymer electrolyte membrane. Dialkyl peroxides are particularly preferred, from the viewpoints of excellent availability of initiators, low cost, and high decomposition onset temperature, allowing polymerization at high temperatures. Among dialkyl peroxides, (CH 3 ) 3 COOC(CH 3 ) 3 is most preferred. The initiator may be used alone or in combination of two or more kinds.
[0023] <Copolymerization> Specific examples of the copolymerization method include bulk polymerization, solution polymerization, suspension polymerization, and emulsion polymerization. Of these, bulk polymerization, which does not substantially use a polymerization solvent, is preferred in that it can avoid a decrease in the molecular weight of polymer Fx due to the chain transfer property of the polymerization solvent. When adopting the solution polymerization method, it is preferable to use a polymerization solvent with a low chain transfer constant. Examples of such polymerization solvents include compounds that do not have atoms other than carbon atoms, fluorine atoms, oxygen atoms, and nitrogen atoms. Specifically, perfluorotributylamine, perfluorotripropylamine, perfluorohexane, perfluorooctane, perfluorodecane, perfluorododecane, perfluoro(2,7-dimethyloctane), perfluorodecalin, perfluorocyclohexane, perfluoro(1,3-dimethylcyclohexane), perfluoro(1,3,5-trimethylcyclohexane), perfluorodimethylcyclobutane (regardless of structural isomerism), perfluoro(2-butyltetrahydrofuran), perfluorobenzene, liquefied carbon dioxide, and supercritical carbon dioxide.
[0024] Furthermore, as the polymerization solvent, a hydrofluorocarbon having a small number of hydrogen atoms, a hydrochlorofluorocarbon having a small number of hydrogen atoms, or a hydrofluoroether having a small number of hydrogen atoms may be used. Specific examples of hydrofluorocarbons having a small number of hydrogen atoms include 1H-perfluorohexane, 1H-perfluorooctane, 1H,4H-perfluorobutane, 2H,3H-perfluoropentane, 3H,4H-perfluoro(2-methylpentane), 1,1,1,3,3-pentafluorobutane, and 1,1,2,2,3,3,4-heptafluorocyclopentane. A specific example of a hydrochlorofluorocarbon having a small number of hydrogen atoms is 1,3-dichloro-1,1,2,2,3-pentafluoropropane. A specific example of a hydrofluoroether with a small number of hydrogen atoms is HCF 2 CF 2 OCH 2 CF 3 , nC 3 F 7 OCH 3 , nC 3 F 7 OCHFCF 3 , nC 3 F 7 OCH 2 CF 3 , nC 4 F 9 OCH 3 , iso-C 4 F 9 OCH 3 , nC 4 F 9 OCH 2 CH 3 , nC 4 F 9 OCH 2 CF 3 , C.F. 3 OCF(CF 3 )CF 2 OCH 3 , nC 3 F 7 OCF(CF 3 )CF 2 OCHFCF 3 Examples include: Also, chlorofluorocarbons having no hydrogen atoms may be used.
[0025] The copolymerization temperature of the monomer m1 and TFE is 150 to 200°C, and is preferably 155°C or higher, and particularly preferably 160°C or higher, in that the reaction rate of the monomers is further improved, and is preferably 190°C or lower, and particularly preferably 180°C or lower, in that the decomposition rate of the initiator is easily suppressed and the copolymerization is easily controlled.
[0026] The polymerization pressure is appropriately set depending on the copolymerization temperature and the ion exchange capacity of the polymer HAx, but from the viewpoint of improving the yield of the polymer Fx and the ion exchange capacity of the polymer HAx, the partial pressure of TFE is preferably 0.02 to 1.2 MPa. The polymerization pressure is preferably 0.1 to 1.9 MPaG.
[0027] In this production method, the monomer m1 is charged in advance into the reactor, and then the copolymerization is started. The initiator may be added to the reactor together with the monomer m1 before the start of the copolymerization, or may be added to the reactor in which the monomer m1 is charged. TFE and other monomers used as necessary may be added to the reactor together with monomer m1 before the copolymerization is started, may be added to the reactor in which monomer m1 is charged, or may be added to the reactor after the copolymerization of monomer m1 is started. The monomers (TFE, monomer m1 and other monomers used as necessary) and the initiator may be added continuously or stepwise to the reactor. In the present invention, "sequential addition" refers to a method of adding an additive (e.g., a monomer, an initiator) to be used in polymerization in portions and intermittently, in which a period in which the additive is added and a period in which the additive is not added are alternately repeated, and the period in which the additive is added is two or more times. In addition, in the present invention, "continuous addition" means a method of adding an additive (e.g., a monomer, an initiator) to be used in polymerization without interruption within a predetermined period, and does not add the additive outside the predetermined period.
[0028] The molar ratio of the total amount of monomer m1 added to the total amount of TFE added is 1.5 to 20. From the viewpoint of further improving the ion exchange capacity of polymer HAx, it is preferably 1.7 or more, more preferably 2.0 or more, and particularly preferably 2.2 or more, and from the viewpoint of improving the mechanical durability of the solid polymer electrolyte membrane and improving the yield of polymer Fx, it is preferably 15 or less, more preferably 10 or less, and particularly preferably 8 or less. When other monomers are added to the reactor, the molar ratio of the total amount of other monomers to the total amount of TFE or the total amount of monomer m1 is preferably 0.01 to 0.5, particularly preferably 0.05 to 0.2, in order to better exhibit the effects of the present invention.
[0029] In the present invention, during the copolymerization of monomer m1 and TFE, an initiator is added continuously or stepwise into the reactor so that the concentration of the initiator in the reactor is maintained at 2.5 mass ppm or less of the mass of monomer m1 charged in the reactor before the start of the copolymerization. If the concentration of the initiator during copolymerization is 2.5 mass ppm or less, the solid polymer electrolyte membrane has excellent hot water resistance. In addition, an unexpected effect was found to be that the solid polymer electrolyte membrane also has excellent chemical durability. Although the reason for the excellent chemical durability has not yet been clarified, it is speculated that the lower initiator concentration in the reactor reduces the proportion of chemical structural parts derived from the initiator that are incorporated into the polymer by chain transfer, thereby reducing the parts of the polymer HAx that are susceptible to deterioration.
[0030] The concentration of the initiator during copolymerization is preferably 2.5 ppm by mass or less, more preferably 2 ppm by mass or less, and particularly preferably 1.5 ppm by mass or less, of the mass of monomer m1 charged in the reactor before the start of the copolymerization, from the viewpoint of further improving the hot water resistance and chemical durability of the solid polymer electrolyte membrane. The concentration of the initiator during copolymerization is preferably 0.01 ppm by mass or more, more preferably 0.05 ppm by mass or more, and particularly preferably 0.1 ppm by mass or more, of the mass of monomer m1 charged in the reactor before the start of the copolymerization, from the viewpoint of further increasing the polymerization rate of the monomers and smoothly proceeding with the polymerization.
[0031] When the initiator is added stepwise or continuously, it is preferable to add the initiator diluted with a monomer (monomer m1 and other monomers used as necessary) or a polymerization solvent from the viewpoint of controllability of the amount added and safety of copolymerization, and it is preferable to dilute with monomer m1 from the viewpoint of avoiding a decrease in the molecular weight of polymer Fx caused by the chain transfer property of the polymerization solvent and reducing a decrease in the polymerization rate caused by a decrease in the concentration of monomer m1 due to the progress of the copolymerization reaction. The concentration of the initiator in the initiator solution used for stepwise or continuous addition is preferably 10 to 10,000 ppm by mass, more preferably 50 to 3,000 ppm by mass, and particularly preferably 100 to 1,000 ppm by mass, from the viewpoint of improving controllability of the amount added and safety of copolymerization.
[0032] According to the theory of radical polymerization reaction, the thermal decomposition of the initiator can be approximated as a first-order reaction. Therefore, the concentration of the initiator in the reactor after a unit time has elapsed since the start of copolymerization [I] relative to the mass of monomer m1 charged in the reactor before the start of copolymerization is calculated by the following formula 1. [I]=[I 0 ]×exp(-K d ·t) Formula 1 [I]: The concentration of the initiator in the reactor after a unit time has elapsed since the start of copolymerization relative to the mass of monomer m1 charged in the reactor before the start of copolymerization [mass ppm] [I 0 ]: Concentration of initiator in the reactor at the start of unit time relative to the mass of monomer m1 charged in the reactor before the start of copolymerization [mass ppm] K d : Decomposition rate coefficient t: unit time Note that exp means exponential function. Here, the start point of the unit time may be, for example, the point at which copolymerization is started or the point immediately after the successive addition of the initiator.
[0033] In the above formula 1, K d (Decomposition rate coefficient) is calculated by the following formula 2. K d =A×exp(-E a / RT) Formula 2 R:8.314[J·K -1 mol -1 ] T: Temperature [K] E a :Activation energy [kJ / mol] A: Frequency factor [h -1 ] K d is a coefficient defined by the type of initiator and the copolymerization temperature. d A and E in Equation 2 used to calculate a It is known that this rate varies depending on the reaction environment, such as the solvent and initiator concentration. In this specification, however, the value used is obtained by measuring the thermal decomposition rate using an initiator solution (initiator concentration: 0.10 [mol / L]) in which the initiator is dissolved in benzene as a solvent. For example, as an initiator, (CH 3 ) 3 COOC(CH 3 ) 3 (hereinafter referred to as "tBPO"), Ea is 155.8 [kJ / mol] and A is 2.23 × 10 19 [h -1 ] and the 10-hour half-life temperature is 123.7°C. If tBPO is used to copolymerize monomer m1 at a copolymerization temperature of 160°C (T = 160 + 273.15 = 433.15 [K]), then by substituting the values of Ea, A, and T into Equation 2, we get K d is 3.62[h -1 ] Other examples of initiators include (CH 3 ) 3 COOC(CH 3 ) 2 -C 6 H 4-C(CH 3 ) 2 OOC(CH 3 ) 3 When using E a is 166.3 [kJ / mol], A is 9.93 × 10 20 [h -1 ] and the 10-hour half-life temperature is 119.2°C. 6 H 5 -C(CH 3 ) 2 OOC(CH 3 ) 2 -C 6 H 5 When using E a is 158.0 [kJ / mol], A is 1.06 × 10 20 [h -1 ] and the 10-hour half-life temperature is 116.4°C. 3 CH 2 CH 2 C(CH 3 ) 2 OOC(CH 3 ) 2 CH 2 CH 2 CH 3 When using E a is 154.5 [kJ / mol], A is 3.71 × 10 19 [h -1 ] and the 10-hour half-life temperature is 116.4°C. (CH 3 ) 3 COOC(CH 3 ) 2 CH 2 CH 2 C(CH 3 ) 2 OOC(CH 3 ) 3 When using E a is 152.0 [kJ / mol], A is 1.39 × 10 19 [h -1 ] and the 10-hour half-life temperature is 117.9°C. (CH 3 ) 3 COOC(CH 3 ) 2 C 6 H 5 When using Ea is 173.1 [kJ / mol], A is 7.59 × 10 21 [h -1 ] and the 10-hour half-life temperature is 119.5°C. (CH 3 ) 3 COOC(CH 3 ) 2 C≡CC(CH 3 ) 2 OOC(CH 3 ) 3 When using E a is 151.3 [kJ / mol], A is 3.36 × 10 18 [h -1 ] and the 10-hour half-life temperature is 128.4°C. (CF 3 ) 3 COOC(CF 3 ) 3 When (PFtBPO) was used, E a is 148.8 [kJ / mol], A is 5.68 × 10 19 [h -1 ] and the 10-hour half-life temperature is 98.5°C.
[0034] Next, an example of a method for setting the amount of the initiator to be added in the sequential addition will be described, taking as an example the case where the initiator is gradually added during copolymerization. tBPO was used as an initiator, the mass of monomer m1 charged in the reactor before the start of copolymerization was 1000 g, and the concentration of the initiator in the reactor at the start of copolymerization was 2.0 ppm by mass (i.e., [I 0 [I] in Equation 1) is 0.327 ppm by mass relative to the mass of monomer m1 charged in the reactor before the start of copolymerization. Then, if it is desired to make the tBPO concentration immediately after each addition the same as the tBPO concentration in the reactor at the start of copolymerization (2.0 ppm by mass) relative to the mass of monomer m1 charged in the reactor before the start of copolymerization, 1.67 mg of tBPO should be added. In other words, the tBPO concentration recovers to 2.0 ppm by mass every 0.5 hours.
[0035] Next, an example of a method for setting the addition rate [mg / h] of the initiator in continuous addition, that is, the amount of initiator added per hour, will be shown, taking the case of continuous addition as an example. By differentiating Equation 1, the rate of reduction of the initiator can be determined. Initiator reduction rate = -[Io] x K d [Mass ppm / h] For example, tBPO is used as an initiator, the mass of monomer m1 charged in the reactor before the start of copolymerization is 1000 g, and the concentration of the initiator in the reactor at the start of copolymerization is 2.0 ppm by mass (i.e., [I 0 When copolymerization is performed under these conditions at 160°C, the initiator reduction rate is -7.24 ppm by mass / h, which is converted to 7.24 mg by mass / h. In other words, if tBPO is continuously added at a rate of 7.24 mg / h, the initiator concentration during copolymerization relative to the mass of monomer m1 charged in the reactor before the start of copolymerization will be maintained at 2.0 ppm by mass.
[0036] In addition, when the initiator is added stepwise or continuously according to the above-mentioned method for setting the amount of the initiator to be added, the concentration of the initiator relative to the total amount of all monomers, solvents, and polymers produced in the reactor decreases as the copolymerization proceeds due to the increase in the amount of components such as monomers or solvents added to the reactor as the copolymerization proceeds and the dilution of the initiator described below. Even in this case, the effect of the invention can be achieved by continuously or stepwise adding the initiator to the reactor so that the concentration of the initiator in the reactor is maintained at 2.5 mass ppm or less of the mass of monomer m1 charged in the reactor before the copolymerization is started, as defined in the present invention.
[0037] The ratio of the total amount of initiators added into the reactor to the total amount of monomers m1 added into the reactor is preferably 0.01 to 4 ppm by mass, more preferably 0.1 to 3 ppm by mass, and particularly preferably 0.5 to 2.5 ppm by mass, on average per hour of copolymerization time, in order to better exhibit the effects of the present invention.
[0038] In the production method of the present invention, the productivity index (Rp) is preferably 0.5 or more, more preferably 0.6 or more, and particularly preferably 0.7 or more, from the viewpoint of increasing productivity. Also, from the viewpoint of suppressing non-uniformity during copolymerization, the Rp value is preferably 5.0 or less, more preferably 4.0 or less, and particularly preferably 3.0 or less.
[0039] After the production of polymer Fx, polymer Fx may be brought into contact with fluorine gas to fluorinate the unstable terminal groups of polymer Fx, which further suppresses the decomposition of polymer HAx obtained using polymer Fx, thereby further improving the chemical durability of the solid polymer electrolyte membrane. Here, the unstable terminal group is a group formed by a chain transfer reaction, a group derived from an initiator, etc., specifically, -COOH, -CF=CF 2 , -COF, -CF 2 Examples include H. The fluorine gas is preferably diluted with an inert gas (nitrogen, helium, carbon dioxide, etc.). The temperature when the polymer Fx is contacted with the fluorine gas is preferably 150 to 200° C., particularly preferably 170 to 190° C. The contact time between the polymer Fx and the fluorine gas is preferably 1 minute to 1 week, particularly preferably 1 to 50 hours.
[0040] [Method for producing a fluoropolymer containing fluorosulfonyl groups according to the second embodiment] The process for producing a fluoropolymer containing fluorosulfonyl groups according to the second embodiment of the present invention is a process for producing a fluoropolymer containing fluorosulfonyl groups by copolymerizing a monomer m1 and TFE in the presence of an initiator in a reactor at a temperature of 150 to 200°C. The ratio of the total amount of the initiator added in the reactor to the total amount of the monomer m1 added in the reactor is 0.01 to 4 mass ppm on average per hour of copolymerization time. The molar ratio of the total amount of the monomer m1 to the total amount of the TFE is 1.5-20. The fluoropolymer having fluorosulfonyl groups obtained by the production method of the second embodiment is also referred to as "polymer Fy" in this specification.
[0041] According to the present production method, a solid polymer electrolyte membrane having excellent electrical conductivity and hot water resistance can be produced. In the examples of Patent Document 1, the initiator was used at a relatively high concentration. However, the present inventors found that a polymer having high electrical conductivity and good hot water resistance can be obtained by using a low concentration of the initiator. That is, it is considered that by controlling the ratio of the total amount of the initiator added to the reactor to the total amount of the monomer m1 added to the reactor within a predetermined range, the termination reaction in the copolymerization of TFE and monomer m1 is less likely to occur. As a result, it is presumed that the molecular weight of polymer Fy is increased, and therefore the hot water resistance of the solid polymer electrolyte membrane produced from the acid-type sulfonic acid group-containing fluorine-containing polymer (hereinafter also referred to as "polymer HAy") obtained by converting the fluorosulfonyl group of polymer Fy to an acid type is improved. Furthermore, normally, when the amount of the initiator used is reduced, the polymerization rate decreases, resulting in a significant drop in productivity. However, surprisingly, according to the method of the present invention, copolymerization can be carried out at a polymerization rate at an industrially feasible level. That is, even when the concentration of the initiator is low as described above, by setting the copolymerization temperature of the monomer m1 and TFE to a high temperature of 150 to 200° C., a decrease in the reaction rate during the production of the polymer Fy can be suppressed. In addition, by setting the molar ratio of the total amount of monomer m1 added to the total amount of TFE added to 1.5 to 20, the content of units based on monomer m1 in polymer Fy increases, and the ion exchange capacity of polymer HAy increases. As a result, it is believed that the conductivity of the solid polymer electrolyte membrane produced by polymer HAy is improved. Moreover, it has been surprisingly found that the chemical durability of the polymer is also superior.
[0042] The production method in the second embodiment is similar to the production method in the first embodiment, except that the essential configuration is that "the ratio of the total amount of the initiator charged in the reactor to the total amount of the monomer m1 charged in the reactor is 0.01 to 4 ppm by mass on average per hour of copolymerization time" instead of "the initiator is continuously or sequentially added into the reactor so that the concentration of the initiator in the reactor during the copolymerization is maintained at 2.5 ppm by mass or less of the mass of the monomer m1 charged in the reactor before the start of the copolymerization." Moreover, the components used in the production method of the second embodiment and preferred embodiments thereof are similar to the components used in the production method of the first embodiment.
[0043] The ratio of the total amount of initiators added to the reactor to the total amount of monomer m1 added to the reactor is 0.01 to 4 mass ppm on average per hour of copolymerization time, and from the viewpoint of further exerting the effects of the present invention, the ratio is preferably 0.1 to 3 mass ppm, and particularly preferably 0.5 to 2.5 mass ppm.
[0044] In the production method of the second embodiment, in order to more effectively exhibit the effects of the present invention, similarly to the production method of the first embodiment, the initiator may be continuously or sequentially added into the reactor during the copolymerization so that the concentration of the initiator in the reactor is maintained at 2.5 ppm by mass or less of the mass of the monomer m1 charged in the reactor before the start of the copolymerization.
[0045] [Fluorosulfonyl group-containing fluoropolymer] Polymers Fx and Fy are preferably fluoropolymers containing fluorosulfonyl groups (hereinafter also referred to as "polymer F1") having the following characteristics. In the following, polymers Fx and Fy may be collectively referred to as "polymer F". That is, the polymer F1 is a polymer having a unit f1 and a TFE unit, and the Q value of the polymer F1 is 0.2 to 60.0 mm 3 / sec, and the ratio of units f1 to all units in polymer F1 is 21 to 59 mol %. By using an acid-type sulfonic acid group-containing fluorine-containing polymer (hereinafter also referred to as "polymer HA1") in which the fluorosulfonyl groups of polymer F1 are replaced with acid-type sulfonic acid groups, a solid polymer electrolyte membrane excellent in electrical conductivity and hot water resistance can be produced.
[0046] [ka] Q in formula f1 1 The definition of is Q in the above formula m1 1 is synonymous with.
[0047] As the unit f1, the unit f11 is preferable, and the unit f11-1 is particularly preferable, in that the polymer F1 can be easily produced and industrially implemented.
[0048] [ka]
[0049] The x in formula f11 has the same meaning as the x in formula m11 described above.
[0050] Polymer F1 may have units based on the other monomers described above (other monomer units).
[0051] The content of the TFE unit is preferably 41 to 79 mol%, more preferably 63 to 78 mol%, and particularly preferably 66 to 76 mol%, based on the total units in the polymer F1. If it is equal to or more than the lower limit, the water content of the solid polymer electrolyte membrane is reduced and the mechanical durability is further improved. If it is equal to or less than the upper limit, the electrical conductivity of the solid polymer electrolyte membrane is further improved. The content of the unit f1 is 21 to 59 mol %, preferably 22 to 37 mol %, and particularly preferably 24 to 34 mol %, based on the total units in the polymer F1. If the content is equal to or more than the lower limit, the electrical conductivity of the solid polymer electrolyte membrane is superior, and if the content is equal to or less than the upper limit, the water content of the solid polymer electrolyte membrane is reduced and the mechanical durability is improved. When polymer F1 has other monomer units, the content of the other monomer units is preferably 0.01 to 10 mol %, more preferably 0.1 to 8 mol %, and particularly preferably 0.5 to 5 mol %, based on the total units in polymer F1, in order to better exert the effects of the present invention.
[0052] The Q value of polymer F1 was measured by passing polymer F1 through a flow tester with a cross-sectional area of 1 cm 2 The mixture is filled into a cylinder of 1 mm in diameter and extruded from a nozzle of 1 mm in length at 260°C under a load of 30 kg and a pressure of 2.94 MPa. 3 / seconds). The Q value is an index similar to MFR (melt flow rate) and is a value correlated with molecular weight. The lower the Q value of polymer F1, the higher the molecular weight of polymer F1, and the higher the Q value of polymer F1, the lower the molecular weight of polymer F1. The Q value of polymer F1 is 0.2 to 60.0 mm. 3 / sec is preferable, 0.5 to 55 mm 3 / sec is more preferable, 0.8 to 50 mm 3 / sec is more preferable, and 3.0 to 45 mm 3 When the Q value of the polymer F1 is within the above range, the molecular weight of the polymer F1 is sufficiently high, so that the solid polymer electrolyte membrane has better hot water resistance.
[0053] The ion exchange capacity of the polymer HA1 is preferably 1.45 to 2.50 milliequivalents / gram, more preferably 1.50 to 2.00 milliequivalents / gram, and particularly preferably 1.55 to 1.90 milliequivalents / gram. If it is equal to or greater than the lower limit, the electrical conductivity of the polymer HA1 is higher, so that sufficient cell output can be obtained when it is used as a solid polymer electrolyte membrane for a solid polymer electrolyte fuel cell. If it is equal to or less than the upper limit, the mechanical strength is excellent when it is used as a solid polymer electrolyte membrane. The ion exchange capacity of the polymer HA1 can be determined by the method described in the Examples section below.
[0054] [Method of producing sulfonic acid group-containing fluoropolymer] The method for producing the sulfonic acid group-containing fluorine-containing polymer of the present invention includes a method for converting the fluorosulfonyl groups of the above-mentioned polymer F into sulfonic acid groups. One example of a method for converting the fluorosulfonyl group of polymer F into a sulfonic acid group is a method in which the fluorosulfonyl group of polymer F described above is hydrolyzed to form a salt-type sulfonic acid group, or a method in which the fluorosulfonyl group of polymer F produced by the above-mentioned production method of polymer F is hydrolyzed to form a salt-type sulfonic acid group, and the salt-type sulfonic acid group is converted to an acid form to form an acid-type sulfonic acid group. The sulfonic acid group-containing fluoropolymer obtained by this production method is also referred to as "Polymer H" in this specification. According to the former method, a fluoropolymer containing a salt-type sulfonic acid group (hereinafter also referred to as "polymer HB") is obtained in which the sulfonic acid group in polymer H is a salt-type sulfonic acid group, and according to the latter method, a fluoropolymer containing an acid-type sulfonic acid group (i.e., polymer HAx or polymer HAy; hereinafter, polymer HAx and polymer HAy may be collectively referred to as polymer HA) is obtained in which the sulfonic acid group in polymer H is an acid-type sulfonic acid group. Polymer H is a polymer obtained by using the above-mentioned Polymer F. Therefore, by using Polymer H, a solid polymer electrolyte membrane having excellent electrical conductivity and hot water resistance as well as excellent chemical durability can be produced.
[0055] The hydrolysis is carried out, for example, by contacting the polymer F with a basic compound in a solvent. Specific examples of the basic compound include sodium hydroxide, potassium hydroxide, and triethylamine. Specific examples of the solvent include water and a mixed solvent of water and a polar solvent. Specific examples of the polar solvent include alcohol (e.g., methanol, ethanol, etc.) and dimethyl sulfoxide. The conversion to an acid form is carried out, for example, by contacting a polymer having salt-form sulfonic acid groups with an aqueous solution of hydrochloric acid, sulfuric acid, nitric acid or the like. The treatment temperature in the hydrolysis and conversion to an acid form is preferably 0 to 120° C. After the hydrolysis or conversion to an acid form, the polymer is preferably washed with water.
[0056] In order to remove organic matter that may be contained as an impurity in polymer H, the organic matter may be decomposed by a treatment such as immersing the polymer in a hydrogen peroxide solution while it is in the salt form after hydrolysis or after conversion to an acid form. The concentration of hydrogen peroxide in the hydrogen peroxide solution is preferably 0.1 to 30% by mass, and particularly preferably 1% by mass or more and less than 10% by mass. If the concentration of hydrogen peroxide in the hydrogen peroxide solution is equal to or more than the lower limit of the above range, the effect of decomposing organic matter is sufficient. If the concentration of hydrogen peroxide in the hydrogen peroxide solution is equal to or less than the upper limit of the above range, polymer H is less likely to decompose. The temperature of the hydrogen peroxide solution is preferably 15 to 90° C., and particularly preferably 40° C. or higher and lower than 80° C. If the temperature of the hydrogen peroxide solution is equal to or higher than the lower limit of the above range, the effect of decomposing organic matter is sufficient. If the temperature of the hydrogen peroxide solution is equal to or lower than the upper limit of the above range, hydrogen peroxide is less likely to decompose. The time for immersing the polymer H in the hydrogen peroxide solution depends on the thickness of the polymer H and the amount of organic matter contained therein, but for example, when the polymer H is a film having a thickness of 50 μm, it is preferably 0.5 to 100 hours. If the immersion time is 0.5 hours or more, the decomposition of the organic matter inside the film is likely to proceed. If the immersion time is 100 hours or less, it is preferable from the viewpoint of productivity. After immersion in hydrogen peroxide, it is preferable to wash the polymer H with water. The water used for washing is preferably ultrapure water. Before washing with water, an acidification treatment may be performed. The final form of the polymer H after the above treatment may be in the form of a powder, pellets, or film.
[0057] [Fluoropolymer containing sulfonic acid groups] Polymer H is preferably a sulfonic acid group-containing fluorine-containing polymer (hereinafter also referred to as "polymer H1") having the following characteristics. That is, polymer H1 is a polymer having unit u1 and TFE unit. When the sulfonic acid group in polymer H1 is replaced with a fluorosulfonyl group, the Q value of the fluoropolymer having a fluorosulfonyl group (that is, polymer F1) is 0.2 to 60.0 mm 3 / sec. The ratio of the units u1 to all the units in the polymer H1 is 21 to 59 mol %. Polymer H1 may be an acid-type sulfonic acid group-containing fluoropolymer in which the sulfonic acid groups in polymer H1 are acid-type sulfonic acid groups (i.e., polymer HA1), or may be a salt-type sulfonic acid group-containing fluoropolymer in which the sulfonic acid groups in polymer H1 are salt-type sulfonic acid groups (hereinafter also referred to as "polymer HB1"). By using polymer H1, it is possible to produce a solid polymer electrolyte membrane which is excellent not only in electrical conductivity and hot water resistance, but also in chemical durability.
[0058] [ka] Q in equation u1 1 is Q in the above formula m1 1is synonymous with Z + is H + , a metal ion, or an ammonium ion. The metal ion is preferably an alkali metal ion.
[0059] Of the units u1, the units u11 are preferred, and the units u11-1 are particularly preferred, in that the polymer H1 can be easily produced, industrially implemented, and a solid polymer electrolyte membrane having superior electrical conductivity and hot water resistance can be produced.
[0060] [ka]
[0061] In formula u11, x has the same meaning as in formula m11. In addition, Z in formula u11 and formula u11-1 + is Z in the above formula u1 + is synonymous with.
[0062] Polymer H1 may have units based on the other monomers mentioned above (other monomer units). The content of each unit in polymer H1 is preferably the same as the content of each unit in polymer F1.
[0063] The definition and preferred embodiments of the Q value in polymer H1 are the same as those in polymer F1. More specifically, the Q value of the fluorosulfonyl group-containing fluorine-containing polymer in the case where the sulfonic acid group in polymer H1 is replaced with a fluorosulfonyl group is the same as that of polymer F1.
[0064] The method and preferred embodiment for measuring the ion exchange capacity of polymer H1 are the same as those for polymer HA1. When the salt type sulfonic acid groups of polymer HB1 are replaced with acid type sulfonic acid groups, the resulting fluoropolymer containing acid type sulfonic acid groups is polymer HA1.
[0065] [Solid molecular electrolyte membrane] The solid polymer electrolyte membrane of the present invention comprises the above-mentioned polymer HA1. Since the solid polymer electrolyte membrane of the present invention contains the polymer HA1, it has excellent electrical conductivity and hot water resistance as well as excellent chemical durability.
[0066] The thickness of the solid polymer electrolyte membrane is preferably 5 to 200 μm, particularly preferably 10 to 130 μm. If it is equal to or greater than the lower limit of the above range, sufficient hydrogen gas barrier properties can be ensured. If it is equal to or less than the upper limit of the above range, the membrane resistance can be sufficiently reduced.
[0067] The electrical conductivity of the solid polymer electrolyte membrane is preferably 0.08 S / cm or more, more preferably 0.09 S / cm or more, and particularly preferably 0.1 S / cm or more. If it is equal to or more than the above value, the solid polymer electrolyte membrane has a sufficiently low membrane resistance, and a fuel cell with excellent power generation performance can be obtained. The upper limit is not particularly limited, but is usually 0.5 S / cm.
[0068] The mass loss rate, which is an index of hot water resistance of the solid polymer electrolyte membrane, is preferably 10% or less, more preferably 7% or less, and particularly preferably 6% or less. If the mass loss rate is equal to or less than the above value, the amount of the membrane eluted into high-temperature water generated during the operation of the fuel cell can be sufficiently suppressed, and a long-life fuel cell with less performance degradation can be obtained.
[0069] The solid polymer electrolyte membrane may further include a reinforcing material, specific examples of which include a porous body, a fiber, a woven fabric, and a nonwoven fabric. The reinforcing material is preferably made of a material selected from the group consisting of polytetrafluoroethylene (hereinafter also referred to as "PTFE"), tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer (hereinafter also referred to as "PFA"), polyether ether ketone (hereinafter also referred to as "PEEK"), and polyphenylene sulfide (hereinafter also referred to as "PPS"), and is more preferably a porous PTFE body.
[0070] In order to further improve durability, the solid polymer electrolyte membrane may contain one or more metals, metal compounds, or metal ions selected from the group consisting of cerium atoms and manganese atoms. It is believed that the cerium atoms and manganese atoms decompose hydrogen peroxide, hydroxyl radicals, and hydroperoxyl radicals, which are causative substances that cause deterioration of the solid polymer electrolyte membrane. The solid polymer electrolyte membrane may contain silica or a heteropolyacid (e.g., zirconium phosphate, phosphomolybdic acid, phosphotungstic acid) as a water retention agent to prevent drying. Methods for incorporating the water retention agent into the solid polymer electrolyte membrane include a method of contacting the solid polymer electrolyte membrane with a solution containing the water retention agent, and a method of incorporating the water retention agent into a liquid composition described below.
[0071] When a solid polymer electrolyte membrane is obtained from a liquid composition by a casting method described later, it is preferable to perform a heat treatment after the production of the solid polymer electrolyte membrane in order to stabilize the solid polymer electrolyte membrane. The temperature of the heat treatment depends on the type of polymer HA1, but is preferably 130 to 200°C. If the heat treatment temperature is 130°C or higher, the water content of the polymer HA1 becomes appropriate. If the heat treatment temperature is 200°C or lower, the thermal decomposition of the sulfonic acid group is suppressed, and the excellent electrical conductivity of the solid polymer electrolyte membrane can be maintained. The solid polymer electrolyte membrane may be treated with hydrogen peroxide water as necessary, by the same method as that for treating polymer H1 described above.
[0072] An example of a method for producing a solid polymer electrolyte membrane is a method (casting method) in which a liquid composition containing the polymer HA1 is applied to the surface of a substrate film or a catalyst layer and dried. An example of a production method when the solid polymer electrolyte membrane contains a reinforcing material is a method in which the reinforcing material is impregnated with a liquid composition containing the polymer HA1 and dried. [Liquid composition]
[0073] The liquid composition preferably contains the polymer HA1 and a liquid medium. The polymer HA1 in the liquid composition may be dispersed in the liquid medium or may be dissolved in the liquid medium. Specific examples of the liquid medium include water and an organic solvent. As the liquid medium, only water may be used, only an organic solvent may be used, or a mixed solvent of water and an organic solvent may be used, but it is preferable to use a mixed solvent of water and an organic solvent. When the liquid medium contains water, the dispersibility or solubility of the polymer HA1 in the liquid medium is likely to be improved, and when the liquid medium contains an organic solvent, an electrolyte membrane that is less likely to crack is likely to be obtained.
[0074] As the organic solvent, alcohol is preferable since it is easy to obtain an electrolyte membrane that is not easily cracked, and alcohol having 1 to 4 carbon atoms is more preferable from the viewpoint of facilitating evaporation of the organic solvent. Examples of alcohols having 1 to 4 carbon atoms include methanol, ethanol, 1-propanol, 2-propanol, 1-butanol, 2,2,2-trifluoroethanol, 2,2,3,3,3-pentafluoro-1-propanol, 2,2,3,3-tetrafluoro-1-propanol, 1,1,1,3,3,3-hexafluoro-2-propanol, and 3,3,3-trifluoro-1-propanol. The organic solvent may be used alone or in combination of two or more kinds.
[0075] When the liquid medium is a mixed solvent of water and an organic solvent, the content of water is preferably from 10 to 99 mass %, particularly preferably from 20 to 99 mass %, based on the total mass of the liquid medium. When the liquid medium is a mixed solvent of water and an organic solvent, the content of the organic solvent is preferably from 1 to 90% by mass, particularly preferably from 1 to 80% by mass. When the contents of water and organic solvent are within the above ranges, it is easy to obtain a solid polymer electrolyte membrane that has excellent dispersibility or solubility of the polymer HA1 in the liquid medium and is not easily cracked.
[0076] The content of polymer HA1 is preferably 1 to 50 mass %, particularly preferably 3 to 30 mass %, based on the total mass of the liquid composition. If it is equal to or more than the lower limit of the above range, a thick film can be stably obtained during film formation. If it is equal to or less than the upper limit of the above range, the viscosity of the liquid composition becomes appropriate.
[0077] The liquid composition is obtained by mixing the polymer H1 with a liquid medium. The mixing method may be, for example, a method in which shearing, such as stirring, is applied to the polymer H1 in a liquid medium under atmospheric pressure or in a sealed state such as an autoclave. The temperature during stirring is preferably 0 to 250° C., more preferably 20 to 150° C. If necessary, shearing force such as ultrasonic waves may be applied.
[0078] The liquid composition may contain one or more metals, metal compounds, or metal ions selected from the group consisting of cerium atoms and manganese atoms in order to further improve the durability of a solid polymer electrolyte membrane produced from the liquid composition.
[0079] [Membrane electrode assembly] The membrane electrode assembly of the present invention includes an anode having a catalyst layer containing a catalyst and a polymer having an ion exchange group, a cathode having a catalyst layer containing a catalyst and a polymer having an ion exchange group, and a solid polymer electrolyte membrane containing a polymer having an ion exchange group disposed between the anode and the cathode. Hereinafter, an example of the membrane electrode assembly of the present invention will be described with reference to the drawings.
[0080] 1 is a cross-sectional view showing an example of a membrane electrode assembly of the present invention. The membrane electrode assembly 10 includes an anode 13 having a catalyst layer 11 and a gas diffusion layer 12, a cathode 14 having the catalyst layer 11 and the gas diffusion layer 12, and a solid polymer electrolyte membrane 15 disposed between the anode 13 and the cathode 14 in contact with the catalyst layer 11.
[0081] Specific examples of the catalyst contained in the catalyst layer 11 include a supported catalyst in which a catalyst containing platinum, a platinum alloy, or a platinum having a core-shell structure is supported on a carbon support or a support made of a metal oxide, an iridium oxide catalyst, an alloy containing iridium oxide, and a catalyst containing iridium oxide having a core-shell structure. An example of the carbon support is carbon black powder. An example of the support made of a metal oxide is an oxide of a simple substance or a complex of a metal such as aluminum, tin, zinc, nickel, cobalt, iron, titanium, cerium, zirconium, palladium, lanthanum, niobium, tantalum, or antimony. A nonmetal catalyst having electrocatalytic activity, such as a carbon alloy catalyst, may also be used. Examples of the polymer having an ion-exchange group contained in the catalyst layer 11 include fluorine-containing polymers having an ion-exchange group, and it is also preferable to use the above-mentioned polymer HA1. When the above-mentioned polymer HA1 is used as the polymer having an ion exchange group contained in the catalyst layer 11, at least one of the polymer having an ion exchange group contained in the anode catalyst layer and the polymer having an ion exchange group contained in the cathode catalyst layer should be polymer HA1. The preferred range of the ion exchange capacity of the polymer HA1 is the same as the above-mentioned value. If it is equal to or higher than the lower limit, the electrical conductivity of the polymer HA1 becomes higher, so that sufficient battery output can be obtained when it is used as a catalyst layer. If it is equal to or lower than the upper limit, the occurrence of flooding during power generation can be suppressed when it is used as a catalyst layer. The preferred range of the Q value of the polymer F1, which is the precursor of the polymer HA1, is also the same as the above-mentioned value. If the Q value of the polymer F1 is within the above-mentioned range, the molecular weight of the polymer F1 is sufficiently high, so that the hot water resistance of the catalyst layer is superior, and the elution of the polymer out of the system due to dissolution in high-temperature water generated during power generation and the associated deterioration of power generation performance over time can be suppressed.
[0082] As the polymer having an ion exchange group contained in the catalyst layer 11, it is also preferable to use a polymer having a cyclic ether structural unit and a sulfonic acid type functional group. The cyclic ether structural unit preferably contains at least one unit selected from the group consisting of units u11, u12, u13, u22 and u24, more preferably units u12 and u22, and particularly preferably units u22, in order to obtain a catalyst layer having superior oxygen permeability.
[0083] [ka]
[0084] R 11 and R 14 each independently represents a monovalent perfluoro organic group which may have an ether-bonded oxygen atom, a fluorine atom, or -R 17 SO 2 X(SO 2 R f ) a - M + It is a group represented by the following formula: The monovalent perfluoro organic group is preferably a perfluoroalkyl group. When the perfluoroalkyl group has an ether bond oxygen atom, the number of oxygen atoms may be one or more. In addition, the oxygen atom may be located between the carbon-carbon bonds of the perfluoroalkyl group, or may be located at the carbon atom bond end. The perfluoroalkyl group may be linear or branched, but is preferably linear. R 17 is a divalent perfluoro organic group which may have an ether bond oxygen atom. The organic group is a group having one or more carbon atoms. The divalent perfluoro organic group is preferably a perfluoroalkylene group. When the perfluoroalkylene group has an ether bond oxygen atom, the number of oxygen atoms may be one or more. In addition, the oxygen atom may be located between the carbon-carbon bonds of the perfluoroalkylene group, or may be located at the carbon atom bond end. The perfluoroalkylene group may be linear or branched, but is preferably linear. M + is H +, a monovalent metal cation (e.g., potassium ion, sodium ion) or an ammonium ion in which one or more hydrogen atoms may be substituted with a hydrocarbon group (e.g., methyl group, ethyl group). From the viewpoint of high conductivity, H + is preferred. R f is a straight-chain or branched perfluoroalkyl group which may have an ether-bonded oxygen atom. The number of carbon atoms in the perfluoroalkyl group is preferably 1 to 8, and more preferably 1 to 6. Two or more R f If there are two or more R f may be the same or different from each other. X is an oxygen atom, a nitrogen atom, or a carbon atom, and when X is an oxygen atom, a=0; when X is a nitrogen atom, a=1; and when X is a carbon atom, a=2. -(SO 2 X(SO 2 R f ) a ) - M + Specific examples of the group include a sulfonic acid group (-SO 3 - M + group), sulfonimide group (-SO 2 N(SO 2 R f ) - M + group), or a sulfonmethide group (-SO 2 C(SO 2 R f ) 2 ) - M + Groups such as R 12 , R 13 , R 15 and R 16 are each independently a monovalent perfluoro organic group which may have an ether-bonded oxygen atom or a fluorine atom. As the monovalent perfluoro organic group, a perfluoroalkyl group is preferable. 15 and R 16 From the viewpoint of high polymerization reactivity, it is preferable that at least one of them is a fluorine atom, and it is particularly preferable that both of them are fluorine atoms. In formula u11, two R 17 If it contains two R 17 may be the same or different from each other.
[0085] The unit u11 is preferably a unit u11-1 or a unit u11-2.
[0086] [ka]
[0087] [ka]
[0088] In formula u12, R 21 is a perfluoroalkylene group having 1 to 6 carbon atoms or a perfluoroalkylene group having 2 to 6 carbon atoms and having an ether-bonding oxygen atom between the carbon-carbon bonds. When the perfluoroalkylene group has an ether-bonding oxygen atom, the number of oxygen atoms may be 1 or 2 or more. The perfluoroalkylene group may be linear or branched, but is preferably linear. R 22 is a fluorine atom, a perfluoroalkyl group having 1 to 6 carbon atoms, a perfluoroalkyl group having 2 to 6 carbon atoms and an ether-bonded oxygen atom between the carbon-carbon bonds, or -R 21 (SO 2 X(SO 2 R f ) a ) - M + In the case where the perfluoroalkyl group has an ether-bonded oxygen atom, the number of oxygen atoms may be one or more. The perfluoroalkyl group may be linear or branched, but is preferably linear. In the formula (u12), two R 21 If it contains two R 21 may be the same or different from each other. M + , R f, X and a are the M + , R f , X and a.
[0089] Specific examples of the unit u12 include the unit u12-1 and the unit u12-2. + is M in formula u11 + is synonymous with.
[0090] [ka]
[0091] [ka]
[0092] In formula u13, R 31 represents a fluorine atom, a perfluoroalkyl group having 1 to 6 carbon atoms, a perfluoroalkyl group having 2 to 6 carbon atoms and an ether-bonded oxygen atom between the carbon-carbon bonds, -R 37 SO 2 X(SO 2 R f ) a - M + It is a group represented by the following formula: When the perfluoroalkyl group has an ether-bonded oxygen atom, the number of oxygen atoms may be 1 or 2 or more. The perfluoroalkyl group may be linear or branched, but is preferably linear. R 37 is a perfluoroalkylene group having 1 to 6 carbon atoms or a perfluoroalkylene group having 2 to 6 carbon atoms and having an ether-bonding oxygen atom between the carbon-carbon bonds. When the perfluoroalkylene group has an ether-bonding oxygen atom, the number of oxygen atoms may be 1 or 2 or more. The perfluoroalkylene group may be linear or branched, but is preferably linear. R 32 ~R 35are each independently a fluorine atom, a perfluoroalkyl group having 1 to 6 carbon atoms, or a perfluoroalkyl group having 2 to 6 carbon atoms and having an ether-bonding oxygen atom between the carbon-carbon bond. When the perfluoroalkyl group has an ether-bonding oxygen atom, the number of oxygen atoms may be 1 or 2 or more. The perfluoroalkyl group may be linear or branched, but is preferably linear. R 36 is a single bond, a perfluoroalkylene group having 1 to 6 carbon atoms, or a perfluoroalkylene group having 2 to 6 carbon atoms and having an ether-bonding oxygen atom between the carbon-carbon bond. When the perfluoroalkylene group has an ether-bonding oxygen atom, the number of oxygen atoms may be 1 or 2 or more. The perfluoroalkylene group may be linear or branched, but is preferably linear. M + , R f , X and a are the M + , R f , X and a.
[0093] [ka]
[0094] In formula u22, s is 0 or 1, with 0 being preferred. R 51 and R 52 each independently represents a fluorine atom, a perfluoroalkyl group having 1 to 5 carbon atoms, or a spiro ring formed by linking together (with the proviso that s is 0). R 53 and R 54 each independently represents a fluorine atom or a perfluoroalkyl group having 1 to 5 carbon atoms. R 55 R is a fluorine atom, a perfluoroalkyl group having 1 to 5 carbon atoms, or a perfluoroalkoxy group having 1 to 5 carbon atoms. 55 is preferably a fluorine atom because of its high polymerization reactivity. The perfluoroalkyl group and the perfluoroalkoxy group may be linear or branched, but are preferably linear.
[0095] The unit u22 is preferably the unit u22-1.
[0096] [ka]
[0097] [ka]
[0098] In formula u24, R 71 ~R 76 are each independently a monovalent perfluoro organic group which may have an ether-bonding oxygen atom or a fluorine atom. The monovalent perfluoro organic group is preferably a perfluoroalkyl group. When the perfluoroalkyl group has an ether-bonding oxygen atom, the number of oxygen atoms may be one or more. In addition, the oxygen atom may be inserted between the carbon-carbon bond of the perfluoroalkyl group, or may be inserted at the carbon atom bond end. The perfluoroalkyl group may be linear or branched, but is preferably linear. R 71 ~R 74 is preferably a fluorine atom because of its high polymerization reactivity.
[0099] The content of the cyclic ether structural unit relative to all units contained in the polymer having a cyclic ether structural unit and a sulfonic acid functional group is preferably 30 mol % or more, more preferably 40 mol % or more, even more preferably 50 mol % or more, and particularly preferably 70 mol % or more, from the viewpoint of achieving better power generation efficiency of the fuel cell. The upper limit of the content of the cyclic ether structural unit is preferably 100 mol %, particularly preferably 80 mol %, based on all units contained in the polymer having a cyclic ether structural unit and a sulfonic acid functional group. The polymer having a cyclic ether structural unit and a sulfonic acid functional group may contain only one type of unit containing a cyclic ether structure, or may contain two or more types. When two or more types are contained, the above content means the total amount of these.
[0100] The gas diffusion layer 12 has a function of diffusing gas uniformly in the catalyst layer and a function as a current collector. Specific examples of the gas diffusion layer include carbon paper, carbon cloth, carbon felt, and titanium porous bodies (specifically, sintered bodies of titanium particles or fibers, etc.). In order to prevent adhesion of the generated gas to the gas diffusion layer, the gas diffusion layer may be treated with PTFE or the like to be water repellent or hydrophilic, or may be hydrophilized with a polymer having an ion exchange group or the like. Although the membrane electrode assembly in FIG. 1 includes a gas diffusion layer 12, the gas diffusion layer is an optional component and does not necessarily have to be included in the membrane electrode assembly.
[0101] The polymer having an ion exchange group contained in the solid polymer electrolyte membrane 15 is preferably the above-mentioned polymer HA1. That is, the solid polymer electrolyte membrane 15 is preferably the above-mentioned solid polymer electrolyte membrane of the present invention.
[0102] The anode 13 and the cathode 14 may include other components in addition to those described above. A specific example of the other member is a carbon layer (not shown) provided between the catalyst layer 11 and the gas diffusion layer 12. By providing the carbon layer, the gas diffusion property of the surface of the catalyst layer 11 is improved, and the power generation performance of the fuel cell can be further improved. The carbon layer contains, for example, carbon and a non-ionic fluorine-containing polymer. A specific example of the carbon is preferably a carbon nanofiber having a fiber diameter of 1 to 1000 nm and a fiber length of 1000 μm or less. A specific example of the non-ionic fluorine-containing polymer is PTFE.
[0103] Examples of methods for producing a membrane electrode assembly include a method in which a catalyst layer is formed on a solid polymer electrolyte membrane and the resulting assembly is further sandwiched between gas diffusion layers, and a method in which a catalyst layer is formed on a gas diffusion layer to form electrodes (anode, cathode), and the solid polymer electrolyte membrane is sandwiched between the electrodes. The catalyst layer can be produced by applying a coating liquid for forming a catalyst layer to a predetermined position and drying it as necessary. The coating liquid for forming a catalyst layer is a liquid in which a polymer having an ion exchange group and a catalyst are dispersed in a dispersion medium. The coating liquid for forming a catalyst layer can be prepared, for example, by mixing a liquid composition containing a polymer having an ion exchange group and a dispersion liquid of a catalyst. The coating liquid for forming a catalyst layer may contain one or more metals, metal compounds, or metal ions selected from the group consisting of cerium and manganese in order to further improve the durability of the catalyst layer 11.
[0104] [Polymer electrolyte fuel cell] The polymer electrolyte fuel cell of the present invention includes the above-mentioned membrane electrode assembly. The polymer electrolyte fuel cell of the present invention includes the above-mentioned membrane electrode assembly, and therefore has excellent power generation performance and durability. The polymer electrolyte fuel cell of the present invention may have separators on both sides of the membrane electrode assembly, in which grooves serving as gas flow paths are formed. Specific examples of the separator include a metal separator, a carbon separator, a separator made of a mixture of graphite and resin, and separators made of various conductive materials. In a polymer electrolyte fuel cell, power is generated by supplying a gas containing oxygen to the cathode and a gas containing hydrogen to the anode. The above-mentioned membrane electrode assembly can also be applied to a methanol fuel cell in which methanol is supplied to the anode to generate electricity. EXAMPLES
[0105] The present invention will be described in detail below with reference to examples. Examples 1-1 to 1-6, 2-1 to 2-6, 3-1 to 3-6, 4-1 to 4-6, 5-1, 6-1 to 6-3, and 8-2 to 8-10 are working examples, and Examples 1-7 to 1-11, 2-7 to 2-11, 3-7 to 3-11, 4-7 to 4-11, 5-2, 6-4, 8-1, and 8-11 are comparative examples. The sulfonic acid group-containing fluorine-containing polymer according to the working examples is referred to as "polymer H", and the sulfonic acid group-containing fluorine-containing polymer according to the comparative examples is referred to as "polymer H'". The fluorosulfonyl group-containing fluorine-containing polymer according to the working examples is referred to as "polymer F", and the fluorosulfonyl group-containing fluorine-containing polymer according to the comparative examples is referred to as "polymer F'". However, the present invention is not limited to these examples. The blending amount of each component in the tables described below is based on mass unless otherwise specified.
[0106] [Ion exchange capacity] The acid-type sulfonic acid group-containing fluoropolymer was vacuum-dried at 120°C for 12 hours, and then immersed in a 0.85 mol / g sodium hydroxide solution (solvent: water / methanol = 10 / 90 (mass ratio)) to neutralize the ion-exchange groups. The sodium hydroxide solution after neutralizing the ion-exchange groups was back-titrated with 0.1 mol / L hydrochloric acid to determine the ion-exchange capacity of the acid-type sulfonic acid group-containing fluoropolymer.
[0107] [Proportion of each component unit] The proportion of each structural unit such as TFE unit, PSAE unit, etc. in the fluoropolymer containing fluorosulfonyl groups is as follows for each polymer: 19 It was determined from the results of F-NMR measurements. 19 F-NMR: 282.7MHz, solvent: hexafluorobenzene, chemical shift reference: CFCl 3 The measurements were performed under the following conditions. The ratio of each constituent unit in the sulfonic acid group-containing fluoropolymer was the same as that in the fluoropolymer containing fluorosulfonyl groups.
[0108] [Q value, TQ value] A flow tester equipped with a nozzle with an inner diameter of 1 mm and a length of 1 mm (Shimadzu Corporation, Capillary Type Rheometer Flow Tester, CFT-500D) was used to measure the cross-sectional area of 1 cm 2 Polymer F or polymer F' filled in a cylinder was extruded from a nozzle at 260°C under a load of 30 kg and a pressure of 2.94 MPa. At that time, the volume flow rate (mm 3 The Q value was defined as the number of times the polymer reacts with the polymer and the number of times the polymer reacts with the polymer. In addition, the Q value is 100 mm 3 The temperature at which the TQ value was reached was defined as the TQ value.
[0109] [conductivity] A substrate with four terminal electrodes arranged at 5 mm intervals was attached to a 5 mm wide solid polymer electrolyte membrane (film thickness 25 μm), and the resistance of the solid polymer electrolyte membrane was measured by a known four-terminal method under constant temperature and humidity conditions of temperature: 80° C., relative humidity: 50%, AC: 10 kHz, voltage: 1 V, and the conductivity was calculated. The reference dimensions and film thickness of the membrane used in the calculation were measured under conditions of temperature: 23° C., relative humidity: 50% RH.
[0110] [Moisture content] A solid polymer electrolyte membrane (thickness 25 μm) was immersed in 80°C hot water for 16 hours, and then cooled until the water temperature was 25°C or less. The membrane was taken out, the water adhering to the membrane surface was wiped off with filter paper, and the mass W1 of the membrane was measured. The water-containing membrane was placed in a glove box in which dry nitrogen (dew point -70°C or less) was circulated, and dried at room temperature (about 15 to 25°C) for 40 hours or more, and then the mass W2 of the membrane was measured in the glove box. The moisture content was calculated from the following formula. Moisture content = {(W1-W2) / W2}×100
[0111] [Hot water resistance] The solid polymer electrolyte membrane (thickness 25 μm) was placed in a glove box with dry nitrogen (dew point -70 ° C or less) circulating, and dried at room temperature (about 15 to 25 ° C) for 40 hours or more, and then the mass (W1) was measured in the glove box. The membrane and ultrapure water were placed in a 120 mL pressure-resistant container in an amount sufficient to fully immerse the membrane, and the pressure-resistant container was placed in an oven at 120 ° C. After 24 hours, the heating was stopped and the membrane was cooled with water, and then the membrane was removed from the pressure-resistant container and the moisture on the surface was wiped off with filter paper (Advantec, No. 2). The water-containing membrane was placed in a glove box with dry nitrogen (dew point -70 ° C or less) circulating, and dried at room temperature (about 15 to 25 ° C) for 40 hours or more, and then the mass (W2) was measured in the glove box. The mass reduction rate (mass%) was calculated from the following formula. Mass reduction rate={(W1-W2) / W1}×100
[0112] [Chemical durability] A membrane electrode assembly including a solid polymer electrolyte membrane was prepared, and the membrane electrode assembly was incorporated into a power generation cell, and the following open circuit test (OCV test) was carried out as an accelerated test. Current density 0.2A / cm 2 Hydrogen (utilization rate 50%) and air (utilization rate 50%) equivalent to 10000 kcal / kg were supplied to the anode and cathode at normal pressure, respectively. The cell temperature was 90°C, the anode gas dew point was 61°C, and the cathode gas dew point was 61°C. The cell was operated in an open circuit state without power generation. The exhaust gas was bubbled through a 0.1 mol / L potassium hydroxide aqueous solution for 24 hours to capture the exhausted fluoride ions. The fluoride ion concentration was then quantified using an ion chromatograph, and the cumulative amount of fluoride ions emitted was calculated. The durability was evaluated according to the following criteria based on the value obtained by dividing the cumulative amount of fluoride ions discharged 200 hours after the start of the open circuit test by the electrode area. ○: Cumulative emission of fluoride ions is 150 μg / cm 2 The following is the result. △: Cumulative emission of fluoride ions is 150μg / cm 2 Super 300μg / cm 2 The following is the result. ×: Cumulative emission of fluoride ions is 300 μg / cm 2 It's super. In Table 6 described later, durability was evaluated according to the following criteria. "--": Inferior "-": Inferior "+":Good 「++」:Excellent "+++": Better.
[0113] [Power generation characteristics] The membrane electrode assembly was assembled into a power generation cell, and the temperature of the membrane electrode assembly was maintained at 95°C. Hydrogen gas (utilization rate 70%) was supplied to the anode, and air (utilization rate 50%) was supplied to the cathode, each pressurized to 151 kPa (absolute pressure). The gases were humidified to a relative humidity of 20% RH for both hydrogen and air, and the current density was 2 A / cm. 2 The cell voltage at this time was recorded. The higher the cell voltage, the better the power generation characteristics of the polymer electrolyte fuel cell.
[0114] [Wet-dry cycle durability (wet-dry cycle durability)] A wet-dry cycle test was carried out by the following method in accordance with the method described in Yeh-Hung Lai, Cortney K. Mittelsteadt, Craig S. Gittleman, David A. Dillard, “VISCOELASTIC STRESS MODEL AND MECHANICAL CHARACTERIZATION OF PERFLUOROSULFONIC ACID (PFSA) POLYMER ELECTROLYTE MEMBRANES”, Proceedings of FUELCELL2005, Third International Conference on Fuel Cell Science, Engineering and Technology, FUELCELL2005, (2005), 74120. The membrane electrode assemblies obtained in each example were used as power generation cells (electrode area 25 cm 2) and the cell temperature was 80°C, and nitrogen gas was supplied to the anode and cathode at 1 L / min. A process of supplying nitrogen gas at a humidity of 150% RH for 2 minutes and then supplying nitrogen gas at a humidity of 0% RH for 2 minutes was repeated as one cycle. The supply of nitrogen gas was stopped every 1000 cycles, hydrogen was supplied to the anode to pressurize it, a pressure difference was generated between the anode and the cathode, and the amount of hydrogen gas leaking from the anode to the cathode through the membrane electrode assembly was measured. The number of cycles was measured until hydrogen gas leakage occurred and the crossover speed, which is expressed as the amount of hydrogen gas leaked per unit area and unit time, became 5 times the initial value. The more cycles at that time, the better the wet-dry cycle durability of the polymer electrolyte fuel cell.
[0115] [Abbreviation] The following abbreviations are used for monomers, initiators, and solvents: TFE: Tetrafluoroethylene PSAE:CF 2 =CFCF 2 OCF 2 CF 2 SO 2 F tBPO:(CH 3 ) 3 COOC(CH 3 ) 3 PFtBPO:(CF 3 ) 3 COOC(CF 3 ) 3 HFE-347pc-f:CF 3 CH 2 OCF 2 CF 2 H HFC-52-13p:CF 3 (CF 2 ) 5 H
[0116] [Preparation of Polymer F and Polymer F'] Polymers F-1 to F-4 and polymers F'-1 to F'-5 were produced as follows.
[0117] <Example 1-1> 525.0 g of PSAE (monomer) was placed in an autoclave equipped with an air-cooled condenser (hereafter abbreviated as A / C, internal volume 500 mL, made of Hastelloy) and cooled with liquid nitrogen to degas. Nitrogen was introduced into the gas phase, and the mixture was heated in an oil bath until the internal temperature reached 160°C. The pressure at this time was 0.445 MPa (gauge pressure). Next, 10.67 g of TFE was introduced into the autoclave. The pressure at this time was 0.89 MPa (gauge pressure), and the TFE partial pressure at the polymerization temperature was 0.445 MPa. Copolymerization was started by adding 0.79 g of an initiator solution in which tBPO, an initiator, was dissolved in PSAE at a concentration of 667 ppm by mass. The amount of tBPO added at this time was 0.53 mg, and the concentration of tBPO in the autoclave was 1.0 ppm by mass of the mass of PSAE charged in the autoclave before the start of copolymerization. TFE was continuously added while maintaining the pressure at 0.89 MPa (gauge pressure), and polymerization was continued for 10 hours. During this time, 0.66 g (0.44 mg by mass of tBPO) of the above initiator solution was added 19 times every 30 minutes, and a total of 8.34 mg of tBPO was introduced into the autoclave. In other words, tBPO was added so that the tBPO concentration was 1.0 ppm by mass immediately after addition relative to the mass of PSAE charged in the autoclave before the start of copolymerization. Through the above operation, the total amount of PSAE introduced into the autoclave was 537.5 g, and the total amount of tBPO introduced into the autoclave was 8.87 mg. Therefore, the ratio of the total amount of tBPO added to the total amount of PSAE added was 1.6 mass ppm on average per hour of polymerization time (referred to as "hourly average initiator ratio" in the table). The additional amount of TFE added was 20.5 g. Stirring during copolymerization was performed with an anchor blade, and the stirring speed was 250 rpm. After cooling until the internal temperature was 30°C or less, the gas in the autoclave was purged. 550g of HFE-347pc-f, which was the same amount (mass) as PSAE, was added to the reaction liquid, and the polymer was coagulated and filtered. Then, the polymer was stirred in the same amount of HFE-347pc-f and washed with HFE-347pc-f, and this operation was repeated twice. The polymer was dried in a vacuum at 120°C to obtain 42.7g of polymer F-1, which is a copolymer of TFE and PSAE monomer. The Q value was 15.5mm 3 / sec, and the TQ value was 300° C. or more. The results are shown in Table 1-1.
[0118] <Example 1-2> Polymer F-2 was obtained in the same manner as in Example 1-1, except that the conditions in Example 1-1 were changed as shown in Table 1-1. The results are shown in Table 1-1.
[0119] <Example 1-3> The autoclave (volume 2500 mL, stainless steel) was depressurized, and 2625.0 g of PSAE (monomer) was sucked and charged into the autoclave. The autoclave was pressurized to 0.3 MPa (gauge pressure) with nitrogen gas and released to 0.05 MPa, and this operation was repeated five times to remove dissolved oxygen. Nitrogen was introduced into the gas phase, and the autoclave was heated in an oil bath until the internal temperature reached 160°C. The pressure at this time was 1.02 MPa (gauge pressure). Next, 46.9 g of TFE was introduced into the autoclave. The pressure at this time was 1.36 MPa (gauge pressure), and the TFE partial pressure at the polymerization temperature was 0.34 MPa. Copolymerization was started by adding 4.38 g of an initiator solution in which tBPO, an initiator, was dissolved in PSAE at a concentration of 300 ppm by mass. The amount of tBPO added at this time was 1.31 mg, and the concentration of tBPO in the autoclave was 0.5 ppm by mass of the mass of PSAE charged in the autoclave before the start of copolymerization. TFE was continuously added while maintaining the pressure at 1.36 MPa (gauge pressure), and polymerization was continued for 8 hours. During this time, in order to maintain the concentration of tBPO relative to the mass of PSAE charged in the autoclave before the start of copolymerization at 0.5 ppm by mass, the above initiator solution was continuously added at a rate of 15.8 g / h (4.75 mg / h in terms of tBPO mass), and was stopped after 7 hours. Through the above operation, the total amount of PSAE introduced into the autoclave was 2735.9 g, and the total amount of tBPO introduced into the autoclave was 34.6 mg. Therefore, the ratio of the total amount of tBPO added to the total amount of PSAE added was 1.6 mass ppm on average per hour of polymerization time. The additional amount of TFE added was 63.1 g. Stirring during copolymerization was performed with a double helical ribbon impeller, and the stirring speed was 150 rpm. After cooling until the internal temperature was 30°C or less, the gas in the autoclave was purged. 5288g of HFE-347pc-f, which was 1.9 times the amount (mass) of PSAE, was added to the reaction liquid, and the polymer was coagulated and filtered. Then, the polymer was stirred in the same amount of HFE-347pc-f and washed with HFE-347pc-f, and this operation was repeated twice. The polymer was dried in a vacuum at 120°C to obtain 171.0g of polymer F-3, which is a copolymer of TFE and PSAE monomer. The Q value was 15.8mm 3 / sec, and the TQ value was 300° C. or more. The results are shown in Table 1-1.
[0120] <Examples 1-4 to 1-6> Except for changing the conditions of Example 1-3 as shown in Table 1-1, the same procedure as in Example 1-3 was used to obtain polymer F-4 in Example 1-4, polymer F-5 in Example 1-5, and polymer F-6 in Example 1-6. However, in Example 1-5, PFtBPO was used as a polymerization initiator. The results are shown in Table 1-1.
[0121] <Example 1-7> Polymer F'-1 was prepared by the method described in Example 1 of Japanese Patent No. 5,217,708. Specifically, 87.96 g of PSAE (monomer) and 1.8 mg of tBPO as an initiator were charged into a stainless steel autoclave with an internal volume of 125 mL, and the autoclave was thoroughly degassed while being cooled with liquid nitrogen. The concentration of tBPO in the autoclave was 20 mass ppm of the mass of PSAE charged in the autoclave before the start of copolymerization. The temperature was then raised to 100°C, TFE was introduced into the autoclave, and the pressure was maintained at 0.39 MPaG. Nitrogen gas was added thereto to make it 0.72 MPaG. The temperature was then raised to 145°C to make it 0.95 MPaG. A 5.2 mass% initiator solution in which tBPO was dissolved in the following compound s-1 was added successively every 30 minutes. The amount of tBPO added each time was set to 0.67 mg of solids, and 12 additions were made in total (0.67 mg corresponds to a tBPO concentration of 7.6 ppm by mass relative to the mass of PSAE charged in the autoclave before the start of copolymerization, but since the residual rate of tBPO after 30 minutes at 145°C was about 68%, the tBPO concentration immediately after addition was 7.6 ppm by mass or more). After 30 minutes had elapsed since the 12th addition, the gas in the autoclave was purged and the autoclave was cooled to terminate the reaction. The stirring time at 145°C was 6.5 hours. The total amount of tBPO added was 9.84 mg. The product was diluted with compound s-1, and then compound s-2 described below was added thereto to flocculate polymer F'-1, which was then filtered. Then, polymer F'-1 was stirred in compound s-1, re-flocculated with compound s-2, and dried under reduced pressure at 80°C overnight. The yield was 10.8g. The Q value was 423mm 3 / sec and the TQ value was 217° C. The results are shown in Table 1-2. CClF 2 CF 2 CHClF(s-1) CH 3 CCl 2 F(s-2)
[0122] <Example 1-8> Polymer F'-2 was prepared by the method described in Example 4 of Japanese Patent No. 5,217,708. In a stainless steel autoclave with an internal volume of 125 mL, 87.96 g of PSAE (monomer) and 0.9 mg of tBPO as an initiator were charged, and the autoclave was thoroughly degassed while being cooled with liquid nitrogen. The concentration of tBPO in the autoclave was 10 mass ppm of the mass of PSAE charged in the autoclave before the start of copolymerization. The temperature was then raised to 100°C, TFE was introduced into the autoclave, and the pressure was maintained at 0.35 MPaG. Nitrogen gas was added thereto to make it 0.65 MPaG. The temperature was then raised to 170°C to make it 1.59 MPaG. A 5.2 mass% initiator solution in which tBPO was dissolved in compound s-1 was added successively every 30 minutes. The amount of tBPO added each time was set to 0.33 mg of solids, and 12 additions were made in total (0.33 mg corresponds to 3.8 ppm by mass of tBPO concentration relative to the mass of PSAE charged in the autoclave before the start of copolymerization, but since the residual rate of tBPO after 30 minutes at 170°C was about 1%, the concentration of tBPO immediately after addition was 3.8 ppm by mass or more). After 30 minutes had elapsed since the 12th addition, the gas in the autoclave was purged and the autoclave was cooled to terminate the reaction. The stirring time at 170°C was 6.5 hours. The total amount of tBPO added was 4.86 mg. The product was diluted with compound s-1, and then compound s-2 was added thereto to flocculate polymer F'-2, which was then filtered. Then, polymer F'-2 was stirred in compound s-1, re-flocculated with compound s-2, and dried under reduced pressure at 80°C overnight. The yield was 3.5g. The Q value was 232mm 3 / sec and the TQ value was 240° C. The results are shown in Table 1-2.
[0123] <Example 1-9> Polymer F'-3 was prepared by the method described in Example 1 of Japanese Patent No. 5,862,372. A stainless steel autoclave with an internal volume of 2575 mL was depressurized, and then pressure purging with nitrogen gas was repeated three times. The pressure was then reduced again and 1959 g of PSAE (monomer) was charged. The temperature was then raised to 120°C, and nitrogen gas was introduced into the autoclave to set the pressure to 0.38 MPaG. TFE was then added at 0.46 MPa to set the total pressure to 0.84 MPaG. Copolymerization was started by adding 3.91 g of an initiator solution in which PFtBPO, an initiator, was dissolved in PSAE at 5 mass%. The amount of PFtBPO added at this time was 195.50 mg, and the concentration of PFtBPO in the autoclave was 100.0 mass ppm of the mass of PSAE charged in the autoclave before the start of copolymerization. While maintaining the pressure at 0.84 MPG, 2.41 g of the initiator solution was added successively four times every hour, and the reaction was continued for 5 hours (the amount added successively was an amount that resulted in a tBPO solid content of 120.5 mg. This amount corresponds to a PFtBPO concentration of 61.5 mass ppm relative to the mass of PSAE charged in the autoclave before the start of copolymerization, but since the residual rate of tBPO after 1 hour at 120°C was about 38%, the concentration of PFtBPO immediately after addition was 61.5 mass ppm or more). After the fourth addition, one hour later, the autoclave was cooled and the gas in the autoclave was purged to terminate the reaction. The total amount of PFtBPO added was 677.50 mg. The product was diluted with HFC-52-13p, and then HFE-347pc-f was added thereto to flocculate the polymer F'-3, which was then filtered. The polymer F'-3 was then stirred in HFC-52-13p, re-flocculated with HFE-347pc-f, and dried under reduced pressure at 80°C overnight. The yield was 323g. The Q value was 55.6mm 3 / sec and the TQ value was 295° C. The results are shown in Table 1-2.
[0124] <Example 1-10 and Example 1-11> Polymer F'-4 in Example 1-10 and Polymer F'-5 in Example 1-11 were obtained in the same manner as in Example 1-1, except that the conditions in Example 1-1 were changed as shown in Table 1-2 and stirring during copolymerization was performed at 250 rpm using a double helical ribbon impeller. The results are shown in Table 1-2.
[0125] [Preparation of Polymer H and Polymer H'] Polymers H-1 to H-6 and polymers H'-1 to H'-5 were produced as follows.
[0126] [Table 1-1]
[0127] [Table 1-2]
[0128] Table 2 shows the maximum initiator concentration [ppm by mass] relative to the mass of PSAE charged before the start of copolymerization.
[0129] [Table 2]
[0130] <Example 2-1> The polymer F-1 obtained as described above was subjected to press molding at a temperature 10°C higher than the TQ value or 260°C, whichever was lower, and at 4 MPa (gauge pressure) to obtain a film of polymer F-1. The film of polymer F-1 was immersed in an alkaline aqueous solution (aqueous solution A: potassium hydroxide / water = 20 / 80 (mass ratio)) at 80°C for 16 hours to obtain the -SO 2 F is hydrolyzed to -SO 3The polymer film was then immersed in a 3 mol / L aqueous hydrochloric acid solution at 50°C for 30 minutes, then in ultrapure water at 80°C for 30 minutes, and then in a 10 mass% aqueous hydrogen peroxide solution at 80°C for 16 hours. The above cycle of immersion in an aqueous hydrochloric acid solution and ultrapure water was then repeated five times in total to convert the -SO 3 K-SO 3 The polymer film was converted to H. The polymer film was repeatedly washed with ultrapure water until the pH of the water in which it was immersed reached 7. The polymer film was sandwiched between filter paper and air-dried to obtain a film of polymer H-1 in Example 1. The results are shown in Table 3.
[0131] <Example 2-2 to Example 2-11> Polymers H-2 to H-6 in Examples 2-2 to 2-6 and Polymers H'-1 to H'-5 in Examples 2-7 to 2-11 were obtained in the same manner as in Example 2-1, except that Polymer F-1 was changed to Polymers F-2 to F-6 and F'-1 to F'-5 and the type of alkaline aqueous solution was changed as shown in Table 3. The results are shown in Table 3. In Table 3, aqueous solution A has a potassium hydroxide / water ratio of 20 / 80, aqueous solution B has a potassium hydroxide / dimethyl sulfoxide / water ratio of 15 / 30 / 55, and aqueous solution C has a potassium hydroxide / methanol / water ratio of 15 / 20 / 65.
[0132] [Table 3]
[0133] [Production of Liquid Composition S and Liquid Composition S'] Liquid compositions S-1 to S-6 and liquid compositions S'-1 to S'-5 were produced as follows.
[0134] <Example 3-1> 37 g of finely cut polymer H-1 membrane and 147.9 g of ethanol / water mixed solvent (50 / 50 (mass ratio)) were added to an autoclave (capacity 200 mL, made of glass), and the autoclave was heated with stirring. After stirring at 110°C for 4 hours, the mixture was allowed to cool and filtered using a pressure filter (filter paper: Advantec Toyo Co., Ltd., PF040) to obtain 164.0 g of liquid composition S-1 in which polymer H-1 was dispersed in the mixed solvent. The solid content was 20.0%. The results are shown in Table 4.
[0135] <Example 3-2> 37.5 g of finely cut polymer H-2 membrane and 120.0 g of ethanol / water mixed solvent (50 / 50 (mass ratio)) were added to an autoclave (capacity 200 mL, made of glass), and the autoclave was heated with stirring. After stirring at 110°C for 3 hours, 15.0 g of dilution water was added, heated for 2 hours, cooled, and filtered using a pressure filter (filter paper: Advantec Toyo Co., Ltd., PF040) to obtain 161.3 g of liquid composition S-2 in which polymer H-2 was dispersed in the mixed solvent. The solid content was 22.1%. The viscosity was 285.2 mPas. The results are shown in Table 4.
[0136] <Example 3-3> 126.9 g of finely cut polymer H-3 membrane and 394.0 g of ethanol / water mixed solvent (50 / 50 (mass ratio)) were added to an autoclave (capacity 1 L, made of glass), and the autoclave was heated with stirring. After stirring at 105°C for 6.5 hours, 5.0 g of ethanol for dilution and 106.0 g of water were added, heated for 0.5 hours, allowed to cool, and filtered using a pressure filter (filter paper: Advantec Toyo Co., Ltd., PF040) to obtain 602.7 g of liquid composition S-3 in which polymer H-3 was dispersed in the mixed solvent. The solid content was 19.8%. The viscosity was 210.6 mPas. The results are shown in Table 4.
[0137] <Example 3-4> The same procedure as in Example 3-2 was repeated except that 24.7 g of polymer H-4, 80.1 g of a mixed solvent of ethanol / water (50 / 50 (mass ratio)), and 22.5 g of dilution water were used to obtain 122.9 g of liquid composition S-4. The solid content was 19.2%. The results are shown in Table 4.
[0138] <Example 3-5> The same procedure as in Example 3-3 was repeated except that 20.1 g of polymer H-5, 57.2 g of a mixed solvent of ethanol / water (40 / 60 (mass ratio)), 12.0 g of dilution ethanol, and 16.9 g of dilution water were used to obtain 112.2 g of liquid composition S-5. The solid content was 17.9%. The results are shown in Table 4.
[0139] <Example 3-6> The same procedure as in Example 3-3 was repeated except that 23.0 g of polymer H-6, 77.0 g of a mixed solvent of ethanol / water (50 / 50 (mass ratio)), 17.6 g of dilution ethanol, and 17.6 g of dilution water were used to obtain 135.2 g of liquid composition S-6. The solid content was 17.0%. The results are shown in Table 4.
[0140] <Example 3-7 to Example 3-11> Liquid compositions S'-1 to S'-5 were obtained in the same manner as in Example 3-1, except that polymers H'-1 to H'-5 were used instead of polymer H-1. The results are shown in Table 4.
[0141] [Table 4]
[0142] [Production of solid polymer electrolyte membrane] The solid polymer electrolyte membranes E-1 to E-6 and the solid polymer electrolyte membranes E-1' to E-5' were produced as follows.
[0143] <Example 4-1> The liquid composition S-1 was applied to a 100 μm ethylene-tetrafluoroethylene copolymer (ETFE) sheet using a die coater to form a film, which was then dried at 80° C. for 15 minutes and then heat-treated at 160° C. for 30 minutes to obtain a solid polymer electrolyte membrane E-1 made of a film of polymer H-1 (thickness 25 μm). The results are shown in Table 5.
[0144] <Example 4-2 to Example 4-11> Solid polymer electrolyte membranes E-2 to E-6 and solid polymer electrolyte membranes E'-1 to E'-5 were obtained in the same manner as in Example 4-1, except that liquid compositions S-2 to S-6 or liquid compositions S'-1 to S'-5 were used instead of liquid composition S-1. The results are shown in Table 5.
[0145] A liquid composition (solid content concentration = 26.0 mass%, ethanol / water = 60 / 40 (mass ratio)) in which an acid-type sulfonic acid group-containing fluoropolymer having an ion exchange capacity of 1.1 milliequivalents / gram is dispersed was obtained by the method described in Example 4 of JP 2018-55877 A. 117 g of water was added to 20.0 g of a supported catalyst (manufactured by Tanaka Kikinzoku Kogyo Co., Ltd., product name: TEC10E50E) in which 46 mass% of platinum is supported on carbon powder, and ultrasonic waves were used for 10 minutes to uniformly disperse the catalyst. 30.8 g of the above liquid composition was added thereto, and 112 g of ethanol was further added to obtain a coating liquid for forming a catalyst layer having a solid content of 10 mass%. The coating liquid for forming a catalyst layer was applied on an ETFE sheet, dried at 80°C, and further heat-treated at 160°C for 30 minutes, and the platinum amount was reduced to 0.4 mg / cm. 2 A catalyst layer (C-1) was prepared. The solid polymer electrolyte membrane obtained above was sandwiched between two sheets of the above catalyst layer from both sides, and the pressing conditions were: 130°C, 5 minutes, and 1.5 MPa. The catalyst layers were bonded to both sides of the solid polymer electrolyte membrane, and the ETFE sheets were peeled off to obtain an electrode with an area of 25 cm. 2 Thus, a membrane catalyst layer assembly was obtained. The membrane / electrode assembly was obtained by sandwiching the membrane / catalyst layer assembly between two gas diffusion substrates (manufactured by NOK, product name: X0086 IX92 CX320). The gas diffusion substrate had a carbon layer made of carbon and PTFE on one surface, and was arranged so that the carbon layer was in contact with the catalyst layer of the membrane / catalyst layer assembly. The prepared membrane / electrode assembly was incorporated into a power generation cell and evaluated by the above-mentioned open circuit test. The results are shown in Table 5. Note that "impossible to measure" means that the membrane was excessively swollen, dissolved or damaged during evaluation, and a numerical value could not be calculated.
[0146] [Table 5]
[0147] As shown in Table 2, the maximum initiator concentration relative to the mass of PSAE charged before the start of copolymerization was 2.5 mass ppm or less in Examples 1-1 to 1-6, while it was 3.0 mass ppm or more in Comparative Examples 1-7 to 1-11. As shown in Table 5, it was confirmed that when the polymer F obtained by the above-mentioned production method was used, a solid polymer electrolyte membrane excellent in electrical conductivity and hot water resistance could be produced compared to when the polymer F' was used. It was also confirmed that a solid polymer electrolyte membrane excellent in chemical durability could be produced. In addition, the Q value of Polymer F is 0.2 to 60.0 mm. 3 / sec and the ratio of PSAE units to all units in polymer F is 21 to 59 mol %, a solid polymer electrolyte membrane containing polymer H obtained by converting the fluorosulfonyl groups of polymer F to acid-type sulfonic acid groups was confirmed to have excellent electrical conductivity and hot water resistance. In addition, it was confirmed that the solid polymer electrolyte membrane has excellent chemical durability.
[0148] [Performance evaluation as a polymer for catalyst layers] Catalyst layers C-2 and C-3 containing polymer H and polymer H' as the catalyst layer polymer were produced as follows, and the power generation characteristics of the catalyst layers were evaluated.
[0149] <Example 5-1> 19.2 g of water was added to 3.00 g of a supported catalyst (manufactured by Tanaka Kikinzoku Kogyo Co., Ltd., product name: TEC10E50E) in which platinum was supported at 46 mass% on carbon powder, and ultrasonic waves were used for 10 minutes to uniformly disperse the catalyst. 6.14 g of liquid composition (S-5) was added thereto, and 12.8 g of ethanol was further added to obtain a coating liquid for forming a catalyst layer with a solid content of 10 mass%. The coating liquid for forming a catalyst layer was applied on an ETFE sheet, dried at 80°C, and further heat-treated at 160°C for 30 minutes, resulting in a platinum content of 0.4 mg / cm. 2 A catalyst layer (C-2) was prepared.
[0150] <Example 5-2> The same procedure as in Example 5-1 was repeated except that 20.0 g of water was used to disperse the platinum-supported catalyst, and 5.56 g of the liquid composition (S'-4) and 12.6 g of ethanol were added, and a coating solution for forming a catalyst layer and a platinum amount of 0.4 mg / cm were prepared. 2 A catalyst layer (C-3) is obtained.
[0151] A 25 μm thick solid polymer electrolyte membrane was obtained in the same manner as in Example 4-1, except that a liquid composition in which an acid-type sulfonic acid group-containing fluoropolymer having an ion exchange capacity of 1.1 milliequivalents / gram obtained by the method described in Example 4 of JP 2018-55877 A was dispersed was used instead of the liquid composition S-1. This solid polymer electrolyte membrane was sandwiched between two of the above catalyst layers (catalyst layer (C-2) or catalyst layer (C-3)) from both sides, and hot-pressed under pressing conditions of 130°C, 5 minutes, and 1.5 MPa to bond the catalyst layers to both sides of the solid polymer electrolyte membrane, and the ETFE sheets were peeled off to obtain an electrode with an area of 25 cm. 2 A membrane catalyst layer assembly is obtained. The membrane / electrode assembly is obtained by sandwiching the membrane / catalyst layer assembly between two gas diffusion substrates (manufactured by NOK, product name: X0086 IX92 CX320). The gas diffusion substrate has a carbon layer made of carbon and PTFE on one surface, and is arranged so that the carbon layer is in contact with the catalyst layer of the membrane / catalyst layer assembly. The membrane / electrode assembly thus produced is incorporated into a power generation cell, and the above-mentioned power generation characteristic evaluation test is carried out. The membrane electrode assembly made of catalyst layer (C-2) is capable of stable power generation even after 100 hours. On the other hand, in the membrane electrode assembly made of catalyst layer (C-3), the polymer for the catalyst layer dissolves into the hot water generated by power generation, and the generated voltage decreases over time. In addition, flooding occurs due to excessive swelling of the polymer for the catalyst layer, and the generated voltage is 1.0 A / cm lower than that of the membrane electrode assembly made of catalyst layer (C-2). 2 In a region of higher current density, the generated voltage relatively decreases.
[0152] [Best embodiment of the invention] <Example 6-1> Cerium carbonate hydrate (Ce) was added to the liquid composition S-1 so that the ratio of the total number of moles of cerium atoms to the total number of moles of sulfonic acid groups in the polymer H-1 was 0.0067. 2 (CO 3 ) 3 8H 2 O) was added and stirred at 50° C. for 24 hours to obtain a liquid composition L-1. The liquid composition L-1 was applied to a 100 μm ETFE sheet using a die coater to form a film, which was then dried at 80° C. for 15 minutes and further heat-treated at 185° C. for 30 minutes to obtain a 25 μm thick solid polymer electrolyte membrane E-10.
[0153] <Example 6-2> Cerium oxide is added to the liquid composition S-1 so that the ratio of the total number of moles of cerium atoms to the total number of moles of sulfonic acid groups in the polymer H-1 is 0.033, and zirconia beads with a diameter of 5 mm are added, and then the mixture is mixed and dispersed for 30 minutes at a rotation speed of 300 rpm using a planetary beads mill. The mixture is filtered through a 53 μm stainless steel mesh to obtain the liquid composition L-2. A solid polymer electrolyte membrane E-11 having a thickness of 25 μm is obtained in the same manner as in Example 6-1, except that the liquid composition is changed.
[0154] <Example 6-3> The liquid composition L-1 is applied to an ETFE sheet by a die coater method, and then an expanded porous PTFE film (thickness 10 μm, porosity 80%) is immediately placed on the coating layer to impregnate the expanded porous PTFE film with the liquid, and the film is dried in an oven at 80° C. for 15 minutes, and then heat-treated in an oven at 185° C. for 30 minutes to obtain a solid polymer electrolyte membrane E-12 having a thickness of 15 μm. Similarly, a solid polymer electrolyte membrane E-13 having a thickness of 15 μm is obtained from the liquid composition L-2.
[0155] <Example 6-4> A liquid composition L'-1 is obtained in the same manner as in Example 6-1, except that the liquid composition S-1 is replaced by the liquid composition S'-1. A solid polymer electrolyte membrane E'-10 having a thickness of 15 μm is obtained in the same manner as in Example 6-3, except that the liquid composition is changed to L'-1.
[0156] <Example 7-1> A liquid composition (solid content concentration = 26.0 mass%, ethanol / water = 60 / 40 (mass ratio)) in which an acid-type sulfonic acid group-containing fluoropolymer having an ion exchange capacity of 1.1 milliequivalents / gram was dispersed was obtained by the method described in Example 4 of JP2018-55877A. 217.8g of water and 178.2g of ethanol were added to 44g of a supported catalyst (Tanaka Kikinzoku Kogyo Co., Ltd., TEC10E50E) in which 46% by mass of platinum was supported on carbon powder, and mixed and ground using an ultrasonic homogenizer to obtain a catalyst dispersion. 117.4g of a mixture of 80.16g of the above dispersion, 44.4g of ethanol, and 25.32g of Zeorola-H (Zeon Corporation) mixed and kneaded in advance was added to the catalyst dispersion, and 163.42g of water and 139.12g of ethanol were further added and mixed using an ultrasonic homogenizer to make the solid content concentration 7% by mass, obtaining a coating liquid for forming a catalyst layer. The catalyst layer forming coating liquid was applied onto an ETFE sheet, dried at 80°C, and further heat-treated at 160°C for 30 minutes to obtain a platinum content of 0.1 mg / cm. 2 A catalyst layer (C-4) was prepared.
[0157] <Example 7-2> Into a 230 mL stainless steel autoclave, 133.16 g of compound (m32-1), 32.67 g of compound (m22-1), and 14.1 g of a solvent (ASAHIKLIN (registered trademark) AC-2000, manufactured by AGC Corporation) were charged, and the mixture was thoroughly degassed under cooling with liquid nitrogen. 3.94 g of TFE (tetrafluoroethylene) was charged, and the temperature was raised to 24° C. to obtain a radical polymerization initiator ((C 3 F 7 COO) 2 The reaction was started by washing the feed line with 1.1 g of AC-2000. After stirring for 8 hours, the autoclave was cooled to stop the reaction. The product was diluted with AC-2000, then mixed with a mixture of AC-2000:methanol = 8:2 (mass ratio) to flocculate the polymer and filter it. The polymer was washed in a mixture of AC-2000:methanol = 7:3 (mass ratio) and separated by filtration. The solid was dried under reduced pressure at 80°C overnight to obtain polymer (p-1). The obtained polymer (p-1) was immersed in an aqueous solution containing 20% by mass of methanol and 15% by mass of potassium hydroxide at 50° C. for 40 hours to measure the amount of -SO 2 Hydrolysis of the F group to -SO 3 The polymer was then immersed in a 3 mol / L aqueous hydrochloric acid solution at room temperature for 2 hours. The aqueous hydrochloric acid solution was replaced, and the same treatment was repeated four more times to convert the -SO 3 A polymer (P-1) in which the K group was converted to a sulfonic acid group was obtained. The composition of the structural units constituting the polymer (P-1) was as follows: 19 F-NMR analysis revealed that, relative to the total units contained in polymer (P-1), the content of units based on monomer (m22-1) was 67 mol%, the content of units based on monomer (m32-1) was 18 mol%, and the content of units based on TFE was 15 mol%. The TQ value of polymer (p-1) was 275°C. The ion exchange capacity of polymer (P-1) was determined to be 1.23 meq / g dry resin. Polymer (P-1) and a mixed solvent of water and 1-propanol (water / 1-propanol = 50 / 50 mass ratio) were stirred in a Hastelloy autoclave at 115°C for 8 hours at a rotation speed of 150 rpm to prepare a dispersion with a polymer (P-1) concentration of 18 mass%. 49.5g of ultrapure water and 40.5g of ethanol were added to 10g of a catalyst (Tanaka Kikinzoku Kogyo Co., Ltd., TEC10E50E) in which platinum was supported on carbon powder to a content of 46% by mass, and ultrasonic waves were applied for 10 minutes to prepare a catalyst dispersion. 20.4g of the dispersion of the polymer (P-1) was added to this, and the mass ratio of the polymer (P-1) to the catalyst carbon (polymer (P-1) mass / catalyst carbon mass) was set to 0.8, and 20.8g of ultrapure water and 29.8g of ethanol were further added to adjust the solid content concentration to 8% by mass, to obtain a coating solution for forming a cathode catalyst layer. The catalyst layer forming coating liquid was applied onto an ETFE sheet, dried at 80°C, and further heat-treated at 160°C for 30 minutes to obtain a platinum content of 0.1 mg / cm. 2 A catalyst layer (C-5) was prepared.
[0158] [ka]
[0159] [ka]
[0160] <Example 7-3> In a 125 mL stainless steel autoclave, 16.33 g of compound (m22-1), 72.84 g of compound (m32-1), 2.0 g of TFE (tetrafluoroethylene), and a radical polymerization initiator ((C 3 F 7 COO) 2 The autoclave was then cooled and thoroughly degassed with liquid nitrogen, after which the temperature was raised to 24°C and the autoclave was kept at that temperature for 24 hours, after which the reaction was stopped by cooling the autoclave. In the same manner as in Example 7-2, 26.0 g of polymer (p-2) was obtained. The steps after hydrolysis were also performed in the same manner as in Example 7-2 to obtain polymer (P-2) and a platinum content of 0.1 mg / cm2 in polymer (P-2). 2 A catalyst layer (C-6) was prepared.
[0161] <Performance evaluation of membrane electrode assemblies (Examples 8-1 to 8-11)> The solid polymer electrolyte membranes E-1, E-10 to E-13, E'-1 and E'-10 and the catalyst layers C-4 to C-6 were combined, sandwiched between two of the above catalyst layers from both sides of the solid polymer electrolyte membrane, and pressed under the following conditions: 130°C, 5 minutes, 1.5 MPa to bond the catalyst layers to both sides of the solid polymer electrolyte membrane. The ETFE sheet was peeled off to obtain an electrode with an area of 25 cm. 2 A membrane catalyst layer assembly is obtained. The membrane / electrode assembly is sandwiched between two gas diffusion substrates (manufactured by NOK, product name: X0086 IX92 CX320) to obtain a membrane / electrode assembly. The gas diffusion substrate has a carbon layer made of carbon and PTFE on one surface, and is arranged so that the carbon layer is in contact with the catalyst layer of the membrane / electrode assembly. The membrane / electrode assembly thus fabricated is incorporated into a power generation cell, and the above-mentioned power generation characteristics, chemical durability, and wet-dry cycle durability are evaluated. A list of the membrane / electrode assemblies to be evaluated is shown in Table 6.
[0162] [Table 6]
[0163] In Examples 8-1 to 8-11, the permutations for evaluating the power generation characteristics were as follows. Example 8-1<(Example 8-2~8-4)<Example 8-11<(Example 8-5, Example 8-6)<(Example 8-7, Example 8-8)<(Example 8-9, Example 8-10) In Examples 8-1 to 8-11, the permutations for the chemical durability evaluation were as follows. Example 8-1<Example 8-2<Example 8-11<(Example 8-3~8-10) In Examples 8-1 to 8-11, the permutations for wet-dry cycle durability evaluation were as follows. Example 8-1<(Example 8-2~8-4)<Example 8-11<(Example 8-5~8-10) The examples in parentheses above show the same effect. From the above, it can be seen that the performance of the membrane electrode assembly made of the solid polymer electrolyte membrane of the present invention is further improved by adding cerium atoms, reinforcing and thinning the solid polymer electrolyte membrane by combining with a reinforcing material, and combining with a catalyst layer made of a polymer with high oxygen permeability. On the other hand, the solid polymer electrolyte membrane of the conventional technology has poor proton conductivity. It is possible to improve the initial characteristics of power generation by designing the solid polymer electrolyte membrane to be reinforced and thinned by combining with a reinforcing material to reduce the membrane resistance, but since the electrolyte material itself has poor hot water resistance, polymer elution is unavoidable during long-term operation, and the rate of deterioration of the power generation characteristics is greater than that of the membrane electrode assembly made of the solid polymer electrolyte membrane of the present invention. Also, for the same reason, it can be seen that the membrane electrode assembly made of the solid polymer electrolyte membrane has relatively poor wet-dry cycle durability. The entire contents of the specification, claims, drawings and abstract of Japanese Patent Application No. 2019-192095, filed on October 21, 2019, are hereby incorporated by reference as the disclosure of the specification of the present invention. [Explanation of symbols]
[0164] 10 Membrane electrode assembly 11 Catalyst layer 12 Gas diffusion layer 13 Anode 14 Cathode 15 Solid polymer electrolyte membrane
Claims
1. A method for producing a fluoropolymer containing fluorosulfonyl groups, comprising copolymerizing a monomer represented by the following formula m1 with tetrafluoroethylene at a temperature of 150 to 200° C. in the presence of a radical polymerization initiator in a reactor, the method comprising the steps of: During the copolymerization, the radical polymerization initiator is continuously or sequentially added into the reactor so that the concentration of the radical polymerization initiator in the reactor is maintained at 2.5 mass ppm or less of the mass of the monomer represented by formula m1 charged in the reactor before the start of the copolymerization, A method for producing a fluoropolymer having a fluorosulfonyl group, characterized in that the molar ratio of the total amount of the monomers represented by the formula m1 to the total amount of the tetrafluoroethylene is from 1.5 to 20. CF 2 =CFCF 2 O-Q 1 -SO 2 F (m1) In formula m1, Q 1 is a single bond or a perfluoroalkylene group which may have an ether-bonded oxygen atom.
2. A method for producing a fluoropolymer containing fluorosulfonyl groups, comprising copolymerizing a monomer represented by the following formula m1 with tetrafluoroethylene at a temperature of 150 to 200° C. in the presence of a radical polymerization initiator in a reactor, the method comprising the steps of: a ratio of a total amount of the radical polymerization initiator charged into the reactor to a total amount of the monomer represented by the formula m1 charged into the reactor is 0.01 to 4 ppm by mass on average per hour of copolymerization time, A method for producing a fluoropolymer having a fluorosulfonyl group, characterized in that the molar ratio of the total amount of the monomers represented by the formula m1 to the total amount of the tetrafluoroethylene is from 1.5 to 20. CF 2 =CFCF 2 O-Q 1 -SO 2 F (m1) In formula m1, Q 1 is a single bond or a perfluoroalkylene group which may have an ether-bonded oxygen atom.
3. The process for producing a fluoropolymer having fluorosulfonyl groups according to claim 1 or 2, wherein the monomer represented by the formula m1 is a monomer represented by the following formula m11: CF 2 =CFCF 2 O (CF 2 ) x SO 2 F (m11) In formula m11, x is an integer from 1 to 12.
4. The method for producing a fluoropolymer having a fluorosulfonyl group according to any one of claims 1 to 3, wherein the radical polymerization initiator is a bis(perfluoroalkyl)peroxide or a dialkylperoxide.
5. A fluoropolymer having a fluorosulfonyl group and a unit represented by the following formula f1 and a unit based on tetrafluoroethylene, The Q value of the fluorosulfonyl group-containing fluoropolymer is 0.2 to 60.0 mm 3 / sec, A fluoropolymer containing fluorosulfonyl groups, characterized in that the ratio of the units represented by the formula f1 to all units in the fluorosulfonyl group-containing fluoropolymer is 21 to 59 mol %. The Q value was measured by measuring the cross-sectional area of the fluorosulfonyl group-containing fluorine-containing polymer using a flow tester. 2 The mixture was filled into a cylinder of 1.0 mm in diameter and extruded from a nozzle of 1 mm in length at 260° C. under a load of 30 kg and a pressure of 2.94 MPa. The volume extruded per unit time (mm 3 / sec). [Formula 1] In formula f1, Q 1 is a single bond or a perfluoroalkylene group which may have an ether-bonded oxygen atom.
6. Fluorosulfonyl group-containing fluoropolymer according to claim 5, wherein the ion exchange capacity of the acid-type sulfonic acid group-containing fluoropolymer when the fluorosulfonyl group in the fluorosulfonyl group-containing fluoropolymer is converted to an acid-type sulfonic acid group is 1.45 to 2.50 milliequivalents / gram dry resin.
7. The fluoropolymer having fluorosulfonyl groups according to claim 5 or 6, wherein the unit represented by the formula f1 is a unit represented by the following formula f11: [Case 2] In formula f11, x is an integer from 1 to 12.
8. A method for producing a sulfonic acid group-containing fluoropolymer, comprising converting the fluorosulfonyl groups of the fluorosulfonyl group-containing fluoropolymer produced by the production method according to any one of claims 1 to 4 into sulfonic acid groups.
9. A sulfonic acid group-containing fluorine-containing polymer having a unit represented by the following formula u1 and a unit based on tetrafluoroethylene, When the sulfonic acid group in the sulfonic acid group-containing fluoropolymer is a fluorosulfonyl group, the Q value of the fluorosulfonyl group-containing fluoropolymer is 0.2 to 60.0 mm 3 / sec, A sulfonic acid group-containing fluoropolymer, characterized in that the ratio of the units represented by the formula u1 to all units in the sulfonic acid group-containing fluoropolymer is 21 to 59 mol %. The Q value was measured by measuring the cross-sectional area of the fluorosulfonyl group-containing fluorine-containing polymer using a flow tester. 2 The mixture was filled into a cylinder of 1.0 mm in diameter and extruded from a nozzle of 1 mm in length at 260° C. under a load of 30 kg and a pressure of 2.94 MPa. The volume extruded per unit time (mm 3 / sec). [C3] In formula u1, Q 1is a single bond or a perfluoroalkylene group which may have an ether-bonded oxygen atom; Z + H + , a metal ion, or an ammonium ion.
10. The sulfonic acid group-containing fluoropolymer according to claim 9, wherein the sulfonic acid group in the sulfonic acid group-containing fluoropolymer is an acid type sulfonic acid group, and the ion exchange capacity of the acid type sulfonic acid group-containing fluoropolymer is 1.45 to 2.50 milliequivalents / gram dry resin.
11. The sulfonic acid group-containing fluorine-containing polymer according to claim 9 or 10, wherein the unit represented by the formula u1 is a unit represented by the following formula u11: [C4] In formula u11, x is an integer from 1 to 12; Z + H + , a metal ion, or an ammonium ion.
12. A liquid composition comprising the sulfonic acid group-containing fluorine-containing polymer according to any one of claims 9 to 11 and a liquid medium.
13. The liquid composition according to claim 12, further comprising one or more atoms selected from the group consisting of cerium atoms and manganese atoms.
14. The present invention comprises a sulfonic acid group-containing fluorine-containing polymer according to any one of claims 9 to 11, A solid polymer electrolyte membrane, characterized in that the sulfonic acid group of the sulfonic acid group-containing fluorine-containing polymer is an acid type sulfonic acid group.
15. 15. The solid polymer electrolyte membrane of claim 14, further comprising a reinforcing material.
16. The solid polymer electrolyte membrane according to claim 14 or 15, having a membrane thickness of 5 to 200 μm.
17. The solid polymer electrolyte membrane according to any one of claims 14 to 16, further comprising at least one selected from the group consisting of cerium atoms and manganese atoms.
18. A membrane electrode assembly comprising: an anode having a catalyst layer containing a catalyst and a polymer having an ion exchange group; a cathode having a catalyst layer containing a catalyst and a polymer having an ion exchange group; and a solid polymer electrolyte membrane containing a polymer having an ion exchange group and disposed between the anode and the cathode, 12. A membrane / electrode assembly, characterized in that at least one polymer selected from the group consisting of the polymer having an ion exchange group contained in the anode, the polymer having an ion exchange group contained in the cathode, and the polymer having an ion exchange group contained in the solid polymer electrolyte membrane is the sulfonic acid group-containing fluorine-containing polymer according to any one of claims 9 to 11.
19. A polymer electrolyte fuel cell comprising the membrane electrode assembly according to claim 18.
Citation Information
Patent Citations
Polymer, method for producing the same, electrolyte membrane for solid polymer type fuel cell, and membrane electrode assembly
JP2010018674A
Method for manufacturing polymer, electrolyte membrane for solid polymer type fuel cell, and membrane electrode assembly
JP2013181128A